Positive electrode active material for secondary battery and the lithium secondary battery including it
The NCM-based lithium transition metal composite oxide with specific dopants and controlled crystallite size addresses the stability and gas generation issues in lithium secondary batteries, enhancing their performance and thermal stability.
Patent Information
- Application Number
- DE202019006087
- Authority / Receiving Office
- DE · DE
- Patent Type
- Utility models
- Current Assignee / Owner
- Priority Date
- 2018-10-26
- Filing Date
- 2019-10-21
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2029-10-31
AI Technical Summary
Existing NCM-based lithium transition metal composite oxides used in lithium secondary batteries face issues such as high specific surface area, low particle strength, excessive lithium by-products, and poor thermal and structural stability, particularly with high nickel content, leading to gas generation and increased resistance.
A positive electrode active material is developed using an NCM-based lithium transition metal composite oxide with specific dopants (Zr, Al, V, Co, Mg for first dopants and Ti, Y, Sr, Nb, Ba, Ca for second dopants) and controlled crystallite size (170-300 nm) to reduce surface area, enhance particle strength, and stabilize the structure, thereby reducing gas generation and resistance.
The solution results in improved stability, reduced gas generation, and suppressed resistance in lithium secondary batteries, especially those with high nickel content, ensuring high capacity and thermal stability.
Abstract
Description
TECHNICAL FIELDCROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This application claims priority to Korean Patent Application No. 10-2018-0129161, filed on October 26, 2018, in the Korean Intellectual Property Office, the disclosure of which is incorporated herein by reference in its entirety. TECHNICAL FIELD
[0002] The present invention relates to a positive electrode active material for a secondary battery and a lithium secondary battery including the same. STATE OF THE ART
[0003] Recently, the demand for a small and lightweight secondary battery with a relatively high capacity has increased rapidly due to the rapid proliferation of battery-based electronic devices such as mobile phones, notebook computers, electric vehicles, and the like. In particular, lithium secondary batteries are lightweight and have high energy density, thus attracting attention as a power source for portable devices. Therefore, active research and development efforts have been made to improve the performance of lithium secondary batteries.
[0004] A lithium secondary battery generates electrical energy through an oxidation and reduction reaction when lithium ions are intercalated / deintercalated from a positive electrode and a negative electrode when an organic electrolyte or a polymer electrolyte made of active materials capable of intercalating and deintercalating lithium ions is inserted between the positive electrode and the negative electrode.
[0005] Lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMnO2, LiMn2O4, or the like), lithium iron phosphate compound (LiFePO4), and the like have been used as positive electrode active materials for lithium secondary batteries. Among these, lithium cobalt oxide (LiCoO2) exhibits high drive voltage and excellent capacity characteristics, making it widely used and applied as a high-voltage positive electrode active material. Due to the price increase and supply instability of cobalt (Co), the large-scale use of lithium cobalt oxide (LiCoO2) as a power source in electric vehicles and the like has been limited. Therefore, there has been a need to develop a positive electrode active material that can replace lithium cobalt oxide (LiCoO2).
[0006] As a result, a lithium transition metal composite oxide (hereinafter referred to simply as "NCM-based lithium transition metal composite oxide") was developed in which part of the cobalt (Co) is replaced with nickel (Ni) and manganese (Mn). However, a typical NCM-based lithium transition metal composite oxide that has been developed takes the form of secondary particles in which primary particles are aggregated, and thus exhibits a large specific surface area, low particle strength, and a high content of lithium by-products. This has led to problems such as generating a large amount of gas during cell operation, reducing stability.In particular, in the case of a high-Ni NCM-based lithium transition metal composite oxide in which the nickel (Ni) content is increased to ensure high capacity, the structural and chemical stability is further deteriorated, and ensuring thermal stability is even more difficult. DISCLOSURE OF THE INVENTION TECHNICAL PROBLEM
[0007] One aspect of the present invention provides a positive electrode active material made of an NCM-based lithium transition metal composite oxide, wherein the positive electrode active material has improved stability. Specifically, the present invention is intended to provide a positive electrode active material made of an NCM-based lithium transition metal composite oxide with a high Ni content, which contains 60 mol% or more of nickel (Ni) to ensure high capacity, wherein the positive electrode active material has improved stability.
[0008] Specifically, the present invention aims to provide a positive electrode active material made of an NCM-based lithium transition metal composite oxide, in which the specific surface area is reduced, the particle strength is improved to suppress particle breakage during roll pressing, the content of lithium by-products is reduced to reduce side reactions with an electrolyte, and an increase in resistance is suppressed. Another aspect of the present invention provides a positive electrode active material made of an NCM-based lithium transition metal composite oxide, capable of reducing gas generation during cell operation and having assured thermal stability. TECHNICAL SOLUTION
[0009] According to one aspect of the present invention, there is provided a lithium transition metal composite oxide including nickel (Ni), cobalt (Co), and manganese (Mn), wherein the lithium transition metal composite oxide includes two or more kinds of first dopants selected from the group consisting of Zr, Al, V, Co, and Mg, and two or more kinds of second dopants selected from the group consisting of Ti, Y, Sr, Nb, Ba, and Ca, and particles of the lithium transition metal composite oxide have a crystallite size of 170-300 nm.
[0010] Also described herein is provided a method for producing a positive electrode active material for a secondary battery, the method including mixing a positive electrode active material precursor including nickel (Ni), cobalt (Co), and manganese (Mn) with a lithium raw material and at least two kinds of first dopant raw materials selected from the group consisting of Zr, Al, V, Co, and Mg, and subjecting the mixture to primary firing, and after the primary firing, mixing at least two kinds of second dopant raw materials selected from the group consisting of Ti, Y, Sr, Nb, Ba, and Ca, and subjecting the mixture to secondary firing, wherein particles of a lithium transition metal composite oxide having a crystallite size of 170-300 nm are formed by the primary firing and the secondary firing.
[0011] According to yet another aspect of the present invention, there is provided a positive electrode including the positive electrode active material and a lithium secondary battery including the positive electrode. BENEFICIAL EFFECTS
[0012] According to the present invention, the specific surface area of an NCM-based positive electrode active material is reduced, particle strength is improved, and the content of lithium by-products is reduced, thereby reducing side reactions with an electrolyte. Accordingly, a lithium secondary battery using the NCM-based positive electrode active material of the present invention can exhibit reduced gas generation during cell operation, suppressed increase in resistance, and assured thermal stability. In particular, even in a positive electrode active material of a high-Ni NCM-based lithium transition metal composite oxide containing 60 mol% or more of nickel (Ni) to ensure high capacity, stability can be improved.The NCM-based positive electrode active material of the present invention can ensure excellent stability and thus can be used for a high-voltage lithium secondary battery. EMBODIMENT OF THE INVENTION
[0013] In the following, the present invention will be described in more detail to facilitate understanding of the present invention. In this case, it is understood that words or expressions used in the specification and claims should not be interpreted as having the meaning defined in commonly used dictionaries. It is further understood that the words or expressions should be interpreted as having a meaning consistent with their meaning in the context of the relevant prior art and the technical idea of the invention, based on the principle that an inventor can reasonably define the meaning of the words or expressions to best explain the invention. <positivelektroden-aktivmaterial>
[0014] A positive electrode active material for a secondary battery of the present invention is a lithium transition metal composite oxide including nickel (Ni), cobalt (Co), and manganese (Mn), wherein the lithium transition metal composite oxide includes two or more kinds of first dopants selected from the group consisting of Zr, Al, V, Co, and Mg, and two or more kinds of second dopants selected from the group consisting of Ti, Y, Sr, Nb, Ba, and Ca, and particles of the lithium transition metal composite oxide have a crystallite size of 170-300 nm.
[0015] The positive electrode active material of the present invention is an NCM-based lithium transition metal composite oxide including nickel (Ni), cobalt (Co), and manganese (Mn). The lithium transition metal composite oxide may be a high-Ni NCM-based lithium transition metal composite oxide having a nickel (Ni) content of 60 mol% or more in the total content of metals excluding lithium (Li). More preferably, the nickel (Ni) content may be 65 mol% or more, and even more preferably, 70 mol% or more. When the nickel (Ni) content in the total content of metals excluding lithium (Li) in the lithium transition metal composite oxide satisfies 60 mol% or more, a larger capacity can be ensured.Alternatively, the lithium transition metal composite oxide may be an NCM-based low-Ni lithium transition metal composite oxide having a nickel (Ni) content of less than 60 mol% in the total content of metals excluding lithium (Li).
[0016] The lithium transition metal composite oxide includes two or more kinds of first dopants selected from the group consisting of Zr, Al, V, Co, and Mg, and two or more kinds of second dopants selected from the group consisting of Ti, Y, Sr, Nb, Ba, and Ca. More preferably, the lithium transition metal composite oxide may include a first dopant including Al and Zr and a second dopant including Sr and Ti.By using the first dopant including two or more elements such as Al and Zr and the second dopant including two or more elements such as Sr and Ti, when synthesizing a positive electrode active material, a reaction occurs with a lithium raw material and residual lithium on the surface of the positive electrode active material to promote the reactivity of a lithium source or the growth of grain boundaries, so that it can be effective in minimizing the interface of the secondary particles and reducing the specific surface area of an NCM-based positive electrode active material and reducing side reactions with the electrolyte, so that the generation of gas when driving a cell can be reduced, the increase in resistance can be suppressed, and the thermal stability can be improved.
[0017] The first dopant can be contained in a total content of 2,000 to 6,000 ppm. More preferably, the first dopant can be contained in 2,500-5,500 ppm, and even more preferably in 3,000-5,000 ppm. When the first dopant is contained in the above content range, there is an effect of ensuring structural stability and improving the service life due to the reduction of lithium diffusion resistance and the stabilization of the internal structure of the positive electrode active material.
[0018] The second dopant can be contained in a total content of 500 to 3,000 ppm. More preferably, the second dopant can be contained in a content of 700-2,700 ppm, and more preferably in a content of 1,000-2,500 ppm. When the second dopant is contained in the above content range, side reactions with an electrolyte are reduced due to the reduction in reactivity caused by the surface phase modification of the positive electrode active material, thus reducing gas generation.
[0019] More specifically, the NCM-based lithium transition metal composite oxide according to an embodiment of the present invention may be a lithium transition metal composite oxide represented by Formula 1 below. Li p Ni 1-(x1+y1+z1+w1) Co x1 Mn y1 M a z1 M b w1 O 2+δ formula 1
[0020] In the above formula, M a at least one element selected from the group consisting of Zr, Al, V, Co and Mg, M b is at least one element selected from the group consisting of Ti, Y, Sr, Nb, Ba and Ca, and 1≤p≤1.5, 0 <x1≤0,5, 0<y1<0,5, 0<z1≤0,025, 0<w1≤0,015 und -0,1≤δ≤1.
[0021] In the lithium transition metal composite oxide according to Formula 1 above, Li may be included in an amount corresponding to p, that is, 1≤p≤1.5. If p is less than 1, the capacity may be deteriorated. If it is greater than 1.3, the strength of the fired positive electrode active material may be increased, making pulverization difficult, and gas generation may be increased due to the increase of Li by-products. Considering the effect of improving the capacity characteristics of the positive electrode active material according to the control of the Li content and sintering balance during the preparation of the active material, Li may be more preferably included in an amount of 1.0≤p≤1.3.
[0022] In the lithium transition metal composite oxide according to Formula 1 above, Ni may be included in an amount corresponding to 1-(x1+y1+z1+w1), for example, 0<1-(x1+y1+z1+wl)≤0.9. When the Ni content in the lithium transition metal composite oxide according to Formula 1 above is 0.6 or more, the amount of Ni sufficient to contribute to charge and discharge can be ensured, so that high capacity can be achieved. More preferably, Ni may be included in an amount of 0.6≤1-(x1+y1+z1+wl)≤0.99.
[0023] In the lithium transition metal composite oxide according to formula 1 above, Co may be included in an amount corresponding to x1, that is, 0 <x1≤0,5. Wenn der Gehalt an Co in dem Lithium-Übergangsmetall-Verbundoxid nach Formel 1 oben mehr als 0,5 beträgt, können die Kosten steigen. Betrachtet man den bemerkenswerten Effekt der Verbesserung der Kapazitätseigenschaften entsprechend dem Einschluss von Co, kann das Co spezifischer in einer Menge von 0,05≤x1≤0,3 eingeschlossen sein.
[0024] In the lithium transition metal composite oxide according to formula 1 above, Mn may be included in an amount corresponding to y1, that is, 0 <y1≤0,5. Mn kann die Stabilität des Positivelektroden-Aktivmaterials verbessern und kann somit die Stabilität einer Batterie verbessern. Mn kann spezifischer in einer Menge von 0,05≤y1≤0,3 eingeschlossen sein.
[0025] In the lithium transition metal composite oxide according to formula 1 above, M a a first doping element included in the crystal structure of the lithium transition metal composite oxide, and M a can be enclosed in a set corresponding to z1, that is, 0 <z1≤0,025.
[0026] In the lithium transition metal composite oxide according to formula 1 above, M b a second doping element included in the crystal structure of the lithium transition metal composite oxide, and M b can be enclosed in a set corresponding to w1, that is, 0 <w1≤0,015.
[0027] Particles of the lithium transition metal composite oxide of the present invention have a crystallite size of 170 nm to 300 nm. More preferably, their crystallite size may be 180 nm to 280 nm, and even more preferably 190 nm to 260 nm. The positive electrode active material satisfying the crystallite size according to one embodiment of the present invention can suppress particle breakage caused by roll pressing, and the durability characteristics and stability can be improved.
[0028] In the present invention, a "particle" refers to a granule of a microunit, and a "primary particle" refers to a granule of the minimal unit in which the boundaries between particles are separated. A "secondary particle" means an aggregate formed by primary particles aggregated with each other. When a "primary particle" is further magnified, it is possible to identify separate regions where atoms form a lattice structure in a specific direction, which is referred to as "crystallite." The size of a particle observed in XRD (Bruker D4 Endeavor) is defined as the size of the crystallite. A crystallite size can be measured by peak broadening of XRD data to assess the crystallite size, or it can be quantitatively calculated using the Scherrer equation.
[0029] To form an NCM-based positive electrode active material that satisfies the crystallite size of 170 nm to 300 nm, overfiring can be performed by increasing a typical firing temperature of an NCM-based lithium transition metal composite oxide by about 100°C. For example, in the case of a high-Ni NCM-based lithium transition metal composite oxide having a nickel (Ni) content of 60 mol% or more, a typical firing temperature is about 800-900°C. However, by performing overfiring at a temperature about 100-150°C higher than this, the crystallite size of an NCM-based positive electrode active material can be increased. In the case of a low-Ni NCM-based lithium transition metal composite oxide having a nickel (Ni) content of less than 60 mol%, a typical firing temperature is about 850-950°C.However, by performing overfiring at a temperature approximately 100-150°C higher than this, the crystallite size of an NCM-based positive electrode active material can be increased. Meanwhile, when some dopants are doped to improve or stabilize the performance of a positive electrode active material, it can act as a factor preventing particle growth compared to a case where a dopant is not present. Therefore, overfiring at an even higher temperature may be necessary.However, when overfiring is performed at a firing temperature about 100-150°C higher than that described above, there are problems regarding volatilization of lithium (Li) and formation of an excessive rock salt phase on the surface of a positive electrode active material, so that the capacity is excessively deteriorated and the surface resistance of the positive electrode active material is also increased.
[0030] Therefore, in the present invention, manufacturing is carried out such that a first dopant including two or more types of elements such as Al and Zr and a second dopant including two or more types of elements such as Sr and Ti are contained together, so that the overfiring temperature is lowered to enable the crystallite size of an NCM-based positive electrode active material to satisfy 170 nm to 300 nm. Thus, the positive electrode active material according to the present invention satisfies the crystallite size of an NCM-based positive electrode active material, which is 170 nm to 300 nm, and while ensuring stability such as reducing gas generation and suppressing an increase in resistance, problems related to deterioration in capacity and an increase in resistance due to overfiring are solved.
[0031] In addition, according to one embodiment of the present invention, particles of the lithium transition metal composite oxide are etched into a cross section using a focused ion beam (FIB) device, and when 20 or more secondary particle cross sections are observed using a scanning electron microscope (FE-SEM), the average number of primary particles in secondary particles in a cross section is 20 or less. More preferably, the particles of the lithium transition metal composite oxide may have an average number of primary particles in the secondary particles in the cross section of 10 or less, and more preferably from 1 to 5 particles.
[0032] In the present invention, a "primary particle" means a primary structural body of a single particle, and a "secondary particle" means an aggregate in which primary particles are aggregated by physical or chemical bonding between the primary particles without an intentional aggregation or build-up process for primary particles forming a secondary particle, that is, a secondary structural body.
[0033] In the present invention, the average number of primary particles in the secondary particles in the cross section is obtained by etching a pattern of a positive electrode active material into a cross section using the focused ion beam (FIB) device and then quantifying the total number of primary particles based on the total number of the secondary particle when a cross-sectional pattern for 20 or more secondary particle cross sections is observed with a scanning electron microscope (FE-SEM).
[0034] Average number of primary particles = total number of primary particles / total number of secondary particles
[0035] To enable the average number of primary particles in the secondary particles in the cross-section of an NCM-based positive electrode active material to be 20 or less, overfiring may be performed at a temperature approximately 100°C higher than a typical firing temperature of an NCM-based lithium transition metal composite oxide. Meanwhile, when some dopants are doped to improve or stabilize the performance of a positive electrode active material, it may act as a factor that inhibits particle growth compared to a case where a dopant is not present. Therefore, overfiring at an even higher temperature may be necessary.
[0036] However, when overfiring is performed at a firing temperature about 100-150°C higher than that described above, there are problems regarding volatilization of lithium (Li) and formation of an excessive rock salt phase on the surface of a positive electrode active material, so that the capacity is excessively deteriorated and also the surface resistance of the positive electrode active material is increased.
[0037] Therefore, in the present invention, the preparation is carried out such that a first dopant including two or more kinds of elements such as Al and Zr and a second dopant including two or more kinds of elements such as Sr and Ti are contained together so that the overfiring temperature is lowered to enable the average number of primary particles in the secondary particles in the cross section of an NCM-based positive electrode active material to satisfy 20 or less.
[0038] The positive electrode active material according to the present invention satisfies the average number of primary particles in the secondary particles in the cross section of 20 or less, thus minimizing the secondary particle interface, reducing the specific surface area, and improving particle strength to suppress particle breakage during roll pressing. In addition, side reactions with an electrolyte are reduced to reduce gas generation during cell operation, and resistance increases are suppressed and thermal stability can be improved.
[0039] In addition, particles of the lithium transition metal composite oxide can have a specific surface area of 0.2-0.7 m 2 / g. More preferably, their specific surface area can be 0.25 m 2 / g up to 0.7 m 2 / g, more preferably 0.3 m 2 / g up to 0.7 m 2 / g. By satisfying the above specific surface area, the amount of gas generated during cell operation can be reduced, and since excellent stability is ensured even under high voltage, application to a high-voltage lithium secondary battery is possible. <Verfahren zum Herstellen des Positivelektroden-Aktivmaterials>
[0040] Next, a method for producing a positive electrode active material of the present invention will be described.
[0041] The method for producing a positive electrode active material for a secondary battery includes mixing a positive electrode active material precursor including nickel (Ni), cobalt (Co), and manganese (Mn) with a lithium raw material and at least two kinds of first dopant raw materials selected from the group consisting of Zr, Al, V, Co, and Mg, and subjecting the mixture to primary firing, and after the primary firing, mixing at least two kinds of second dopant raw materials selected from the group consisting of Ti, Y, Sr, Nb, Ba, and Ca, and subjecting the mixture to secondary firing, wherein particles of a lithium transition metal composite oxide having a crystallite size of 170-300 nm are formed by the primary firing and the secondary firing.
[0042] The process for preparing a positive electrode active material is described in detail below step by step.
[0043] First, a precursor of a positive electrode active material is prepared, which includes nickel (Ni), cobalt (Co) and manganese (Mn).
[0044] The precursor of the positive electrode active material may be a commercially available precursor of a positive electrode active material that is purchased and used, or it may be prepared according to a method for preparing a precursor of a positive electrode active material that is well known in the art.
[0045] For example, the precursor can be prepared by adding a transition metal solution containing a nickel-containing raw material, a cobalt-containing raw material, a manganese-containing raw material to an ammonium cation-containing complex-forming agent and a basic compound and subjecting the mixture to a coprecipitation reaction.
[0046] The nickel-containing raw material may be, for example, an acetate, a nitrate, a sulfate, a halide, a sulfide, a hydroxide, an oxide or an oxyhydroxide and the like, all of which contain nickel, specifically Ni(OH)2, NiO, NiOOH, NiCO3 · 2Ni (OH) 2 · 4H2O, NiC2O 2 · 2H2O, Ni(NO3)2·6H2O, NiSO4, NiSO4·6H2O, a fatty acid nickel salt, a nickel halide, or a combination thereof, but is not limited thereto.
[0047] The cobalt-containing raw material may be an acetate, a nitrate, a sulfate, a halide, a sulfide, a hydroxide, an oxide or an oxyhydroxide and the like, all containing cobalt, specifically Co(OH)2, CoOOH, Co(OCOCH3)2·4H2O, Co(NO3)2·6H2O, CoSO4, Co(SO4)2·7H2O or a combination thereof, but is not limited thereto.
[0048] The manganese-containing raw material may be an acetate, a nitrate, a sulfate, a halide, a sulfide, a hydroxide, an oxide or an oxyhydroxide and the like, all containing manganese, specifically a manganese oxide such as Mn2O3, MnO2, Mn3O4 and the like, a manganese salt such as MnCO3, Mn(NO3)2, MnSO4, manganese acetate, dicarboxylic acid manganese salt, manganese citrate and fatty acid manganese salt, manganese oxyhydroxide, manganese chloride or a combination thereof, but is not limited to this.
[0049] The transition metal solution can be prepared by adding a nickel-containing raw material, a cobalt-containing raw material, and a manganese-containing raw material to a solvent, specifically water, or a mixed solvent of water and an organic solvent (e.g., alcohol, etc.) that can be uniformly mixed with water. Alternatively, the transition metal solution can be prepared by mixing an aqueous solution of a nickel-containing raw material, an aqueous solution of a cobalt-containing raw material, and an aqueous solution of a manganese-containing raw material.
[0050] The ammonium cation-containing complex-forming agent may be, for example, NH4OH, (NH4)2SO4, NH4NO3, NH4Cl, CH3COONH4, NH4CO3, or a combination thereof, but is not limited thereto. Meanwhile, the ammonium cation-containing complex-forming agent may be used in the form of an aqueous solution. Water or a mixture of an organic solvent that can be uniformly mixed with water (e.g., alcohol, etc.) and water may be used as the solvent.
[0051] The basic compound can be a hydroxide of an alkali metal or an alkaline earth metal, such as NaOH, KOH, or Ca(OH)2, a hydrate thereof, or a combination thereof. The basic compound can also be used in the form of an aqueous solution. Water or a mixture of an organic solvent that can be uniformly mixed with water (e.g., alcohol, etc.) and water can be used as the solvent.
[0052] The basic compound is added to control the pH of a reaction solution and can be added in such an amount that the pH of a metal solution is 11 to 13.
[0053] Meanwhile, the coprecipitation reaction can be carried out in an inert atmosphere, for example, in a nitrogen atmosphere or in an argon atmosphere and the like, at a temperature of 40°C to 70°C.
[0054] Through the above process, nickel-cobalt-manganese hydroxide particles are generated and precipitated in a reaction solution. By controlling the concentration of the nickel-containing raw material, the cobalt-containing raw material, and the manganese-containing raw material, a precursor with a nickel (Ni) content of 60 mol% or more in the total metal content can be produced. The precipitated nickel-cobalt-manganese hydroxide particles are separated and dried according to a typical method to obtain a nickel-cobalt-manganese precursor. The precursor may be secondary particles formed by aggregated primary particles.
[0055] Next, the precursor and a lithium raw material and at least two kinds of raw materials of a first dopant selected from the group consisting of Zr, Al, V, Co and Mg are mixed, followed by primary firing.
[0056] The lithium raw material may be a sulfate, nitrate, acetate, carbonate, oxalate, citrate, halide, hydroxide, or oxyhydroxide, and the like, all of which contain lithium, and is not specifically limited as long as it can be dissolved in water. Specifically, the lithium raw material may be Li2CO3, LiNO3, LiNO2, LiOH, LiOH·H2O, LiH, LiF, LiCl, LiBr, LiI, CH3COOLi, Li2O, Li2SO4, CH3COOLi, Li3C6H5O7, or the like, and one of these or a mixture of two or more thereof may be used.
[0057] The raw material of the first dopant may be a sulfate, a nitrate, an acetate, a carbonate, an oxalate, a citrate, a halide, a hydroxide, or an oxyhydroxide, and the like, all of which contain a first dopant element. The raw material of the first dopant may be mixed so that the first dopant is contained in a total content of 2,000-6,000 ppm based on the total weight of the positive electrode active material, more preferably 2,500-5,000 ppm, and even more preferably 3,000-5,000 ppm.
[0058] In the case of a high-Ni NCM-based lithium transition metal composite oxide having a nickel (Ni) content of 60 mol% or more, the primary firing can be performed at 800-1000°C, more preferably 830-980°C, and even more preferably 850-950°C. In the case of a low-Ni NCM-based lithium transition metal composite oxide having a nickel (Ni) content of less than 60 mol%, the primary firing can be performed at 900-1100°C, more preferably 930-1070°C, and even more preferably 950-1050°C.
[0059] The primary firing can be carried out in an air or oxygen atmosphere and can be carried out for 15-35 hours.
[0060] Next, after the primary firing, at least two kinds of raw materials of a second dopant selected from the group consisting of Ti, Y, Sr, Nb, Ba and Ca are mixed, followed by secondary firing.
[0061] The raw material of the second dopant may be a sulfate, a nitrate, an acetate, a carbonate, an oxalate, a citrate, a halide, a hydroxide, or an oxyhydroxide, and the like, all of which contain a second dopant element. The raw material of the second dopant may be mixed so that the second dopant is contained in a total content of 500-3,000 ppm based on the total weight of the positive electrode active material, more preferably 700-2,700 ppm, and even more preferably 1,000-2,500 ppm.
[0062] In the case of a high-Ni NCM-based lithium transition metal composite oxide having a nickel (Ni) content of 60 mol% or more, the secondary firing can be performed at 600-950°C, more preferably at 650-930°C, and even more preferably at 700-900°C. In the case of a low-Ni NCM-based lithium transition metal composite oxide having a nickel (Ni) content of less than 60 mol%, the secondary firing can be performed at 700-1050°C, more preferably at 750-1000°C, and even more preferably at 800-950°C.
[0063] The secondary firing can be done in an air or oxygen atmosphere and can be carried out for 15-35 hours.
[0064] Through primary firing and secondary firing, particles of a lithium transition metal composite oxide are formed to have a crystallite size of 170 nm to 300 nm. Firing can be performed so that the crystallite size is more preferably 180 nm to 280 nm, and even more preferably 190 nm to 260 nm.
[0065] In addition, by the primary firing and secondary firing, a positive electrode active material having an average number of primary particles of 20 or less in secondary particles in a cross-section can be formed. More preferably, a positive electrode active material having an average number of primary particles of 10 or less in secondary particles in a cross-section can be formed, even more preferably 1 to 5.
[0066] In the present invention, a first dopant including two or more kinds of elements such as Al and Zr is doped during primary firing, and a second dopant including two or more kinds of elements such as Sr and Ti is doped during secondary firing, so that the crystallite size of an NCM-based positive electrode active material is 170 nm to 300 nm, and in order to allow the average number of primary particles in secondary particles in a cross section to be 20 or less, the overfiring temperature can be lowered.Accordingly, the positive electrode active material prepared according to the present invention has the crystallite size of the NCM-based positive electrode active material of 170 nm to 300 nm, and further, the average number of primary particles in secondary particles in a cross section satisfies 20 or less, so that stability is ensured, such as reducing gas generation and suppressing increase in resistance, and problems related to deterioration of capacity and increase in surface resistance of the positive electrode active material are solved. Positive electrode and secondary battery
[0067] According to yet another embodiment of the present invention, a positive electrode for a lithium secondary battery including the positive electrode active material and a lithium secondary battery including the positive electrode are provided.
[0068] Specifically, the positive electrode includes a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector and enclosing the positive electrode active material.
[0069] In the positive electrode, the positive electrode current collector is not specifically limited as long as it has conductivity without causing chemical changes in a battery. For example, stainless steel, aluminum, nickel, titanium, burnt carbon, or aluminum or stainless steel surface-treated with one of carbon, nickel, titanium, silver, and the like can be used. Also, the positive electrode current collector can typically have a thickness of 3-500 μm, and microscopic irregularities can be formed on the surface of the positive electrode current collector to improve the adhesion of the positive electrode active material. For example, the positive electrode current collector can be used in various forms, such as a film, sheet, foil, mesh, porous body, foam, and nonwoven body.
[0070] In addition, the positive electrode active material layer may include a conductive material and a binder together with the positive electrode active material described above.
[0071] Here, the conductive material is used to impart conductivity to an electrode, and any conductive material can be used without specific limitation as long as it has electronic conductivity without causing a chemical change in a battery to be formed. Specific examples thereof may include graphite such as natural graphite or artificial graphite; a carbon-based material such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fiber; metal powder or metal fiber of, for example, copper, nickel, aluminum, and silver; a conductive whisker such as a zinc oxide whisker and a potassium titanate whisker; a conductive metal oxide such as titanium oxide; or a conductive polymer such as a polyphenylene derivative, and one of these or a mixture of two or more thereof may be used.Typically, the conductive material may be included in an amount of 1-30 wt% based on the total weight of the positive electrode active material layer.
[0072] Additionally, the binder serves to improve the bonding between particles of the positive electrode active material and the adhesion between the positive electrode active material and the positive electrode current collector. Specific examples thereof may include: polyvinylidene fluoride (PVDF), a polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, an ethylene-propylene-diene monomer (EPDM), a sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one of these or a mixture of two or more thereof may be used. The binder may be included in an amount of 1-30 wt% based on the total weight of the positive electrode active material layer.
[0073] The positive electrode can be produced according to a typical method for producing a positive electrode, except that the above-described positive electrode active material is used. Specifically, the positive electrode can be produced by applying a composition for forming a positive electrode active material layer including the above-described positive electrode active material, and optionally a binder and a conductive material, to the positive electrode current collector, followed by drying and roll pressing. Here, the type and content of the positive electrode active material, the binder, and the conductive material are as described above.
[0074] The solvent may be a solvent conventionally used in the field, and may be dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, water, or the like. One of these or a mixture of two or more thereof may be used. The amount of the solvent to be used is sufficient if the solvent can dissolve and disperse the positive electrode active material, the binder, and the conductive material, taking into account the application thickness of a slurry and the production yield, and thereafter has a viscosity that exhibits excellent thickness uniformity during application to form a positive electrode.
[0075] In another method, the positive electrode may be formed by casting a composition for forming a positive electrode active material layer on a separate support and then laminating a film obtained by peeling from the support onto a current collector of the positive electrode.
[0076] According to yet another embodiment of the present invention, an electrochemical device including the positive electrode is provided. The electrochemical device may specifically be a battery, a capacitor, or the like, and more specifically, may be a lithium secondary battery.
[0077] The lithium secondary battery includes a positive electrode, a negative electrode disposed opposite the positive electrode, a separator disposed between the positive electrode and the negative electrode, and an electrolyte. The positive electrode is the same as described above. In addition, the lithium secondary battery may further include a battery case for accommodating an electrode assembly composed of the positive electrode, the negative electrode, and the separator, and optionally a sealing member for sealing the battery case.
[0078] In the lithium secondary battery, the negative electrode includes a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector.
[0079] The negative electrode current collector is not specifically limited, as long as it has high conductivity without causing chemical changes in the battery. For example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with one of carbon, nickel, titanium, silver, and the like, an aluminum-cadmium alloy, and the like can be used. Also, the negative electrode current collector can typically have a thickness of 3-500 μm, and as in the case of the positive electrode current collector, microscopic irregularities can be formed on the surface of the negative electrode current collector to improve the adhesion of a negative electrode active material.For example, the negative electrode current collector can be used in various forms such as film, sheet, foil, mesh, porous body, foam, nonwoven body and the like.
[0080] The negative electrode active material layer optionally includes a binder and a conductive material in addition to the negative electrode active material. As an example, the negative electrode active material layer can be prepared by applying a negative electrode forming composition, which includes a negative electrode active material and optionally a binder and a conductive material, to a negative electrode current collector, followed by drying. Alternatively, the negative electrode active material layer can be prepared by casting the composition onto a separate support and then laminating a film obtained by peeling from the support onto a negative electrode current collector.
[0081] As the negative electrode active material, a compound capable of reversibly intercalating and deintercalating lithium can be used. Specific examples of the negative electrode active material may include a carbonaceous material such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; a metallic material that can be alloyed with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, a Si alloy, a Sn alloy, or an Al alloy; a metal oxide that can be doped or undoped with lithium, such as SiOβ (0 < β < 2), SnO2, a vanadium oxide, and a lithium vanadium oxide; or a composite material including the metallic material and the carbonaceous material, such as a Si-C composite material or an Sn-C composite material, and one of them or a mixture of two or more thereof may be used.A metal-lithium thin film can also be used as the negative electrode active material. Furthermore, low-crystalline carbon, high-crystalline carbon, and the like can all be used as the carbon material. Representative examples of low-crystalline carbon include soft carbon and hard carbon, and representative examples of high-crystalline carbon include irregular, planar, plate-shaped, spherical, or fibrous natural or artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, mesocarbon microspheres, mesophase pitches, and high-temperature sintered carbon such as cokes derived from petroleum pitch and coal tar pitch.
[0082] The binder and the conductive material can also be the same as those described above in the description of the positive electrode.
[0083] Meanwhile, in the lithium secondary battery, the separator serves to separate the negative electrode and the positive electrode and provide a movement path for lithium ions. Without any particular limitation, any separator can be used as long as it is typically used as a separator in a lithium secondary battery. In particular, a separator that has high moisture retention capacity for an electrolyte and low resistance to the movement of electrolyte ions is preferred. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminated structure comprising two or more layers thereof, can be used.Likewise, a typical porous nonwoven fabric, for example, a nonwoven fabric formed from high-melting-point glass fiber or polyethylene terephthalate fiber, and the like, can be used as a separator. Furthermore, a coated separator including a ceramic component or a polymer material can be used to ensure heat resistance or mechanical strength, and can be used optionally in a single-layer or multi-layer structure.
[0084] In addition, the electrolyte used in the present invention may be an organic liquid electrolyte, an inorganic liquid electrolyte, a solid polymer electrolyte, a gel-like polymer electrolyte, an inorganic solid electrolyte, an inorganic molten electrolyte, and the like, which can be used in the production of a lithium secondary battery, but is not limited thereto.
[0085] Specifically, the electrolyte may include an organic solvent and a lithium salt.
[0086] Without any particular limitation, any organic solvent can be used as long as it can serve as a medium through which ions involved in an electrochemical reaction of a battery can move. Specifically, the organic solvent can include an ester-based solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; an ether-based solvent such as dibutyl ether or tetrahydrofuran; a ketone-based solvent such as cyclohexanone; an aromatic hydrocarbon-based solvent such as benzene and fluorobenzene; a carbonate-based solvent such as dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); an alcohol-based solvent such as ethyl alcohol and isopropyl alcohol.Nitriles such as R-CN (where R is a linear, branched, or cyclic C2 to C20 hydrocarbon group and may include a doubly bonded aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes may be used. Among the above solvents, a carbonate-based solvent is preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) with high ionic conductivity and high dielectric constant, which can enhance the charge / discharge performance of the battery, and a linear carbonate-based compound with low viscosity (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate) is more preferable. In this case, the performance of the electrolyte can be excellent when the cyclic carbonate and the chain carbonate are mixed in a volume ratio of about 1:1 to about 1:9.
[0087] Without any specific restrictions, any compound can be used as the lithium salt as long as it can provide lithium ions used in a lithium secondary battery. Specifically, LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2 can be used as the lithium salt. The lithium salt can be used in a concentration range of 0.1-2.0 M. When the lithium salt concentration is within the above range, the electrolyte exhibits suitable conductivity and viscosity, thus demonstrating excellent performance, and lithium ions can move efficiently.
[0088] In the electrolyte, in order to improve the cycle life characteristics of a battery, suppress the reduction of battery capacity, and improve the discharge capacity of the battery, in addition to the above components for constituting the electrolyte, one or more types of additives, for example, a halogen alkylene carbonate-based compound such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, n-glyme, hexaphosphoric triamide, a nitrobenzene derivative, sulfur, a quinone imine dye, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, an ammonium salt, pyrrole, 2-methoxyethanol, or aluminum trichloride, and the like, may be included. Here, the additive may be included in an amount of 0.1-5 wt% based on the total weight of the electrolyte.
[0089] The lithium secondary battery including the positive electrode active material according to the present invention as described above stably exhibits excellent discharge capacity, output characteristics, and capacity retention rate, and is thus useful for portable devices such as a mobile phone, a notebook computer, and a digital camera, and in the field of electric cars such as a hybrid electric vehicle (HEV).
[0090] Accordingly, according to another embodiment of the present invention, a battery module including the lithium secondary battery as a unit cell and a battery pack including the same are provided.
[0091] The battery module or battery pack can be used as a power source for one or more medium and large devices, for example, a power tool, an electric car such as an electric vehicle (EV), a hybrid electric vehicle (HEV), and a plug-in hybrid electric vehicle (PHEV), or an electricity storage system.
[0092] Examples of the present invention are described in detail below so that those skilled in the art can easily practice the present invention. However, the present invention may be embodied in many different forms and is not limited to the examples set forth herein. Example 1
[0093] In a 5 L batch-type reactor set at 60°C, NiSO4, CoSO4 and MnSO4 were mixed in water in such an amount that the molar ratio of nickel:cobalt manganese was 60:20:20 to form a precursor solution with a concentration of 2.4 M.
[0094] One liter of deionized water was added to a coprecipitation reactor (5 L capacity), and nitrogen gas was introduced into the reactor at a rate of 2 liters / minute to remove dissolved oxygen in the water and create a non-oxidizing atmosphere in the reactor. Subsequently, 10 ml of a 25% NaOH aqueous solution was added, followed by stirring at 60°C at a stirring rate of 1200 rpm while maintaining a pH of 12.0.
[0095] Thereafter, the precursor solution was added at a rate of 180 ml / h, and a coprecipitation reaction was carried out for 18 hours while adding an aqueous NaOH solution and an aqueous NH4OH solution to obtain particles of a nickel-cobalt-manganese-containing hydroxide (Ni 0,60 Co 0,20 Mn 0,20 (OH)2). The hydroxide particles were separated, washed, and dried in an oven at 120°C to prepare a positive electrode active material precursor. The positive electrode active material precursor prepared as described above was in the form of secondary particles in which primary particles were aggregated.
[0096] The positive electrode active material precursor prepared as described above and a lithium raw material LiOH were added to a Henschel mixer (700 L) such that the final molar ratio of Li / M(Ni, Co, Mn) was 1.02. The first dopant raw materials Al(OH)2 and ZrO2 were added such that the final total first dopant content was 3500 ppm, and mixed at 300 rpm for 20 minutes. The mixed powder was placed in a 330 mm x 330 mm alumina crucible and subjected to primary firing at 930°C for 15 hours under an oxygen (O2) atmosphere.
[0097] Subsequently, the raw materials of a second dopant, SrCO3 and TiO2, along with a first calcined product, were added to a 700 L Henschel mixer so that the final total content of the second dopant elements was 2000 ppm and mixed for 20 minutes at 300 rpm. The mixed powder was placed in a 330 mm x 330 mm alumina crucible and subjected to secondary firing at 830°C for 15 hours under an oxygen (O2) atmosphere to form a lithium transition metal composite oxide.
[0098] 300 g of the lithium transition metal composite oxide prepared as described above was added to 300 ml of ultrapure water, stirred for 30 minutes, washed with water, and then filtered for 20 minutes. The filtered lithium transition metal composite oxide was dried in a vacuum oven at 130°C for 10 hours, followed by sieving to prepare a positive electrode active material. Example 2
[0099] In a 5 L batch-type reactor set at 60°C, NiSO4, CoSO4 and MnSO4 were mixed in water in such an amount that the molar ratio of nickel:cobalt manganese was 50:30:20 to prepare a precursor solution with a concentration of 2.4 M.
[0100] One liter of deionized water was added to a coprecipitation reactor (5 L capacity), and nitrogen gas was introduced into the reactor at a rate of 2 liters / minute to remove dissolved oxygen in the water and create a non-oxidizing atmosphere in the reactor. Subsequently, 10 ml of a 25% NaOH aqueous solution was added, followed by stirring at 60°C at a stirring rate of 1200 rpm while maintaining a pH of 12.0.
[0101] Thereafter, the precursor solution was added at a rate of 180 ml / h, and a coprecipitation reaction was carried out for 18 hours while adding an aqueous NaOH solution and an aqueous NH4OH solution to form particles of a nickel-cobalt-manganese-containing hydroxide (Ni 0,50 Co 0,30 Mn 0,20 (OH)2). The hydroxide particles were separated, washed, and dried in an oven at 120°C to prepare a positive electrode active material precursor. The positive electrode active material precursor prepared as described above was in the form of secondary particles in which primary particles were aggregated.
[0102] The positive electrode active material precursor prepared as described above and a lithium raw material LiOH were added to a Henschel mixer (700 L) such that the final molar ratio of Li / M(Ni, Co, Mn) was 1.02. The first dopant raw materials Al(OH)2 and ZrO2 were added such that the final total first dopant content was 3500 ppm, and mixed for 20 minutes at 300 rpm. The mixed powder was placed in a 330 mm x 330 mm alumina crucible and subjected to primary firing at 970°C for 15 hours under an oxygen (O2) atmosphere.
[0103] Subsequently, raw materials of a second dopant, SrCO3 and TiO2, along with a first calcined product, were introduced into a 700-liter Henschel mixer such that the final total content of the second dopant elements was 2000 ppm and mixed for 20 minutes at 300 rpm. The mixed powder was placed in a 330 mm x 330 mm alumina crucible and subjected to secondary firing at 870°C for 15 hours under an oxygen (O2) atmosphere to form a lithium transition metal composite oxide.
[0104] The lithium transition metal composite oxide prepared as described above was dried in a vacuum oven at 130°C for 10 hours, followed by sieving to prepare a positive electrode active material. Example 3
[0105] A positive electrode active material was prepared in the same manner as in Example 1, except that Co(OH)2 and MgO as raw materials of the first dopant were mixed so that the final content of the total first dopant elements was 5000 ppm, and Nb2O5 and Y2O3 as raw materials of the second dopant were mixed so that the final content of the total second dopant elements was 1500 ppm. Example 4
[0106] A positive electrode active material was prepared in the same manner as in Example 2, except that Co(OH)2 and MgO as raw materials of the first dopant were mixed so that the final content of the total first dopant elements was 5000 ppm, and Nb2O5 and Y2O3 as raw materials of the second dopant were mixed so that the final content of the total second dopant elements was 1500 ppm. Example 5
[0107] A positive electrode active material was prepared in the same manner as in Example 1, except that the primary firing temperature was set to 890°C and the secondary firing temperature was set to 800°C. Example 6
[0108] A positive electrode active material was prepared in the same manner as in Example 2, except that the primary firing temperature was set to 930°C and the secondary firing temperature was set to 850°C. Comparison example 1
[0109] A positive electrode active material was prepared in the same manner as in Example 1, except that the raw materials of the first dopant and the raw materials of the second dopant were not mixed. Comparison example 2
[0110] A positive electrode active material was prepared in the same manner as in Example 2, except that the raw materials of the first dopant and the raw materials of the second dopant were not mixed. Comparison example 3
[0111] A positive electrode active material was prepared in the same manner as in Example 1, except that ZrO2 as the raw material of the first dopant was mixed so that the final content of the first dopant element was 3500 ppm, and SrCO3 as the raw material of the second dopant was mixed so that the final content of the second dopant elements was 2000 ppm. Comparison example 4
[0112] A positive electrode active material was prepared in the same manner as in Example 2, except that ZrO2 as the raw material of the first dopant was mixed so that the final content of the first dopant element was 3500 ppm, and SrCO3 as the raw material of the second dopant was mixed so that the final content of the second dopant elements was 2000 ppm. Experimental Example 1: Specific surface area and crystallite size of the positive electrode active material
[0113] The specific surface area and crystallite size of the positive electrode active materials prepared in each of Examples 1 to 6 and Comparative Examples 1 to 4 were measured. The specific surface area was measured using a gas adsorption analyzer (BELSORP mini II), and the crystallite size was calculated by measuring an XRD (Bruker D4 Endeavor).
[00129] Table 1 Specific surface area (m 2 / G) Crystallite size (nm) Example 1 0,45 255 Example 2 0,55 251 Example 3 0, 67 234 Example 4 0, 61 223 Example 5 0,57 210 Example 6 0, 60 190 Comparison example 1 0,15 312 Comparison example 2 0,21 308 Comparison example 3 0, 92 155 Comparison example 4 0,87 167
[0114] Referring to Table 1 above, the specific surface area of the positive electrode active material prepared in each of Examples 1 to 6 is 0.7 m 2 / g or less, which is reduced compared to the positive electrode active material of Comparative Examples 3 to 4. In addition, the positive electrode active material of each of Examples 1 to 6 has a crystallite size of 170 nm to 300 nm, which is increased compared to the positive electrode active material of each of Comparative Examples 3 and 4. Meanwhile, in the case of Comparative Examples 1 and 2 in which the first and second dopants were not doped at all, since no energy consumption was required for the migration of the dopants, compared to Examples 1 and 2 in which a dopant was present, the driving force of crystallite growth was increased, so that the crystallite size was more than 300 nm. Experimental Example 2: Observation of the positive electrode active material
[0115] The positive electrode active material prepared in each of Examples 1 to 6 and Comparative Examples 1 to 4 was etched into a cross section using a focused ion beam (FIB) device, and 20 or more secondary particle cross sections were observed using a scanning electron microscope (FEO-SEM). Here, the total number of primary particles compared to the total number of secondary particles was calculated as follows to confirm the average number of primary particles in the secondary particles in the cross section. The results are shown in Table 2 below.
[00133] Table 2 Average number of primary particles in secondary particles in cross section Example 1 4, 3 Example 2 4, 9 Example 3 11 Example 4 14,7 Example 5 7, 9 Example 6 7 Comparison example 1 5, 1 Comparison example 2 3,5 Comparison example 3 28,4 Comparison example 4 27
[0116] Referring to Table 2, the positive electrode active material prepared in each of Examples 1 to 6 of the present invention had an average number of primary particles in the secondary particles in the cross section of 20 or less, but in the case of Comparative Examples 3 and 4 in which only one kind of doping element was doped, the average number of primary particles in the secondary particles in the cross section was more than 20. Regarding the positive electrode active material prepared as in each of Examples 1 to 6, it was confirmed that the average number of primary particles in the secondary particles in the cross section was 20 or less, although the overfiring temperature was lowered by doping two or more specific first and second dopants during the primary firing and the secondary firing, respectively.Meanwhile, in the case of Comparative Examples 1 and 2 in which the first and second dopant were not doped at all, since there was no factor hindering the growth of primary particles, compared with a case where a dopant was added, the average number of primary particles in the secondary particles was 20 or less, which was similar to that of Examples 1 and 2. Experimental Example 3: Evaluation of thermal stability
[0117] To evaluate the thermal stability of the positive electrode active material prepared in each of Examples 1-2 and 5 and Comparative Example 3, the heat flow versus temperature was measured using a differential scanning calorimeter (SETARAM Co., Ltd., SENSYS Evo). Specifically, a lithium secondary battery prepared as in the preparation example using the positive electrode active material of each of Examples 1-2 and 5 and Comparative Example 3 was disassembled at a state of charge (SOC) of 100%, and a positive electrode and a new electrolyte were placed in a DSC measurement cell to proceed with the measurement by raising the temperature from room temperature to 400°C at a rate of 10°C per minute. The results are shown in Table 3 below.
[00137] Table 3 DSC main peak (°C) Maximum heat flow Example 1 320 1,36 Example 2 299 1,5 Example 5 301 1,58 Comparison example 3 288 1,71
[0118] Referring to Table 3, in the case of Examples 1-2 and 5, the main peak at which the heat flux is maximum appeared at a relatively high temperature of 299°C or more, and it can be confirmed that the maximum heat flux was significantly reduced compared to Comparative Example 3. From the above, it can be seen that the examples of the present invention had significantly improved thermal stability. Experimental Example 4: Evaluation of the properties of high-temperature storage
[0119] The positive electrode active material prepared in each of Examples 1 to 6 and Comparative Examples 1 to 3, a conductive carbon black material, and a PVdF binder were mixed in an N-methylpyrrolidone solvent in a weight ratio of 96:2:2 to prepare a positive electrode mixed material (viscosity: 5000 mPa s), and the mixed material was applied to a surface of an aluminum current collector, dried at 130°C, and then roll-pressed to produce a positive electrode. Lithium metal was used as the negative electrode.
[0120] A porous polyethylene separator was placed between the positive electrode and the negative electrode prepared as described above to form an electrode assembly. The electrode assembly was then placed inside a casing. An electrolyte was then injected into the casing to fabricate a lithium secondary battery. The electrolyte was prepared by dissolving lithium hexafluorophosphate (LiPF6) at a concentration of 1.0 M in an organic solvent containing ethylene carbonate / ethyl methyl carbonate / diethylene carbonate (mixing volume ratio of EC / EMC / DEC = 3 / 4 / 3).
[0121] The half-cell of the lithium secondary battery, prepared as described above, was charged (final current 1 / 20 C) to 0.5 C and 4.4 V in CCCV mode. Two positive electrodes charged as described above and two polyethylene separators were alternately laminated to the bottom of a button cell. An electrolyte was then injected into the cell, and the button cell, prepared by covering it with a gasket, was packaged in an aluminum bag and vacuum sealed. Afterward, the gas generated by storing the button cell at 60°C for 2 weeks was measured using a gas chromatograph-mass spectrometer (GC-MS). The results are shown in Table 4 below. Table 4 Gas generation during high-temperature storage µl / g) Example 1 1320 Example 2 1200 Example 3 1580 Example 4 1610 Example 5 1550 Example 6 1480 Comparison example 1 2440 Comparison example 2 2615 Comparison example 3 2430 Comparison example 4 2190
[0122] Referring to Table 4, the positive electrode active material prepared in each of Examples 1 to 6 exhibited a significantly reduced amount of gas generation during high-temperature storage compared with the positive electrode active material prepared in each of Comparative Examples 1 to 4. In the case of Comparative Examples 1 and 2, in which the first and second dopants were not doped at all, the amount of gas generated was significantly higher because there was no dopant to stabilize the surface and structure. In the case of Comparative Examples 3 and 4, in which one type of dopant was doped, since overburning was not sufficiently performed, compared with Examples 1 to 6, the BET was relatively high, and the amount of gas generated was significantly higher due to the resulting increase in the reaction surface area. Experimental Example 5: Evaluation of resistance properties at room temperature
[0123] A lithium secondary battery prepared as in Experimental Example 4 using the positive electrode active material of each of Examples 1 to 6 and Comparative Examples 1 to 4 was subjected to a constant current discharge at 1.0 C for 10 seconds at 25°C and an SOC of 10%. Using a measured voltage drop, the resistance was calculated and compared. The results are shown in Table 5 below.
[00148] Table 5 25°C resistance (Ω) Example 1 22,4 Example 2 23 Example 3 26, 6 Example 4 24, 1 Example 5 20,5 Example 6 21 Comparison example 1 45,7 Comparison example 2 48,5 Comparison example 3 25, 8 Comparison example 4 27,2
[0124] Referring to Table 5, Examples 1 to 6 of the present invention exhibited improved resistance at room temperature compared with Comparative Examples 1 to 4. In particular, Examples 1 to 6 exhibited significantly improved resistance characteristics at room temperature compared with Comparative Examples 1 to 2 in which the first and second dopants were not doped at all, which may be due to the fact that Comparative Examples 1 and 2 could not exhibit any effect of improving the diffusion resistance of lithium ions from the addition of dopant.
[0125] This utility model is branched from EP application No. 19 875 260.2 (PCT / KR2019 / 013805), the entire contents of which are incorporated herein by reference, and a copy of its original claims is repeated below in the form of numbered embodiments. [1] A positive electrode active material for a secondary battery, wherein the material is a lithium transition metal composite oxide including nickel (Ni), cobalt (Co) and manganese (Mn), wherein the lithium transition metal composite oxide includes two or more kinds of first dopants selected from the group consisting of Zr, Al, V, Co and Mg, and two or more kinds of second dopants selected from the group consisting of Ti, Y, Sr, Nb, Ba and Ca, and Particles of the lithium transition metal composite oxide have a crystallite size of 170-300 nm. [2] The positive electrode active material for a secondary battery according to [1], wherein the particles of the lithium transition metal composite oxide are etched into a cross section using a focused ion beam (FIB) device, and when 20 or more secondary particle cross sections are observed using a scanning electron microscope (FE-SEM), the average number of primary particles in secondary particles in a cross section is 20 or less. [3] Positive electrode active material for a secondary battery according to [1], wherein the first dopants are contained in the total content of 2,000 to 6,000 ppm. [4] Positive electrode active material for a secondary battery according to [1], wherein the second dopants are contained in the total content of 500 to 3,000 ppm. [5] Positive electrode active material for a secondary battery according to [1], wherein the particles of the lithium transition metal composite oxide have a specific surface area of 0.2-0.7 m 2 / g. [6] The positive electrode active material for a secondary battery according to [2], wherein the particles of the lithium transition metal composite oxide have an average number of primary particles in secondary particles in a cross section of 10 or less. [7] The positive electrode active material for a secondary battery according to [1], wherein the lithium transition metal composite oxide has a nickel (Ni) content of 60 mol% or more in a total content of metals excluding Li (lithium). [8] The positive electrode active material for a secondary battery according to [1], wherein the lithium transition metal composite oxide has a nickel (Ni) content of less than 60 mol% in the total content of metals excluding Li (lithium). [9] A method for producing a positive electrode active material for a secondary battery, the method comprising: Mixing a precursor of a positive electrode active material including nickel (Ni), cobalt (Co), and manganese (Mn) with a lithium raw material and at least two kinds of first dopant raw materials selected from the group consisting of Zr, Al, V, Co, and Mg, and subjecting the mixture to primary firing; and after the primary firing, mixing at least two kinds of raw materials of second dopants selected from the group consisting of Ti, Y, Sr, Nb, Ba and Ca, and subjecting the mixture to a secondary firing, wherein particles of a lithium transition metal composite oxide having a crystallite size of 170-300 nm are formed by primary firing and secondary firing.
[10] The method for producing a positive electrode active material for a secondary battery according to [9], wherein, when the precursor of the positive electrode active material has a nickel (Ni) content of 60 mol% or more in the total content of metals, the primary firing is carried out at 800-1,000°C.
[11] The method for producing a positive electrode active material for a secondary battery according to [9], wherein, when the precursor of the positive electrode active material has a nickel (Ni) content of less than 60 mol% in the total content of metals, the primary firing is carried out at 900-1,100°C.
[12] The method for producing a positive electrode active material for a secondary battery according to [9], wherein, when the precursor of the positive electrode active material has a nickel (Ni) content of 60 mol% or more in the total content of metals, the secondary firing is carried out at 600-950°C.
[13] The method for producing a positive electrode active material for a secondary battery according to [9], wherein, when the precursor of the positive electrode active material has a nickel (Ni) content of less than 60 mol% in the total content of metals, the secondary firing is carried out at 700-1,050°C.
[14] The method for producing a positive electrode active material for a secondary battery according to [9], wherein the particles of the lithium transition metal composite oxide formed by the primary firing and the secondary firing are etched into the cross section using a focused ion beam (FIB) device, and when 20 or more secondary particle cross sections are observed using a scanning electron microscope (FE-SEM), the average number of primary particles in the secondary particles in the cross section is 20 or less.
[15] The method for producing a positive electrode active material for a secondary battery according to [9], wherein the raw materials of the first dopant are mixed so that a total content of the first dopants based on the total weight of the positive electrode active material is 2,000-6,000 ppm.
[16] The method for producing a positive electrode active material for a secondary battery according to [9], wherein the raw materials of the second dopant are mixed so that the total content of the second dopants is 500-3,000 ppm based on the total weight of the positive electrode active material.
[17] A positive electrode for a secondary battery comprising the positive electrode active material according to any one of [1] to [8].
[18] Lithium secondary battery comprising the positive electrode according to
[17] . QUOTES CONTAINED IN THE DESCRIPTION
[0000] This list of documents submitted by the applicant was generated automatically and is included solely for the convenience of the reader. This list is not part of the German patent or utility model application. The DPMA assumes no liability for any errors or omissions. Cited patent literature
[0000] Korean Patent Application No. 10-2018-0129161
[0001] EP application No. 19 875 260.2
[0125] KR2019 / 013805
[0125]
Claims
[1] A positive electrode active material for a secondary battery, wherein the material is a lithium transition metal composite oxide including nickel (Ni), cobalt (Co) and manganese (Mn), wherein the lithium transition metal composite oxide includes two or more kinds of first dopants selected from the group consisting of Zr, Al, V, Co and Mg, and two or more kinds of second dopants selected from the group consisting of Ti, Y, Sr, Nb, Ba and Ca, and Particles of the lithium transition metal composite oxide have a crystallite size of 170-300 nm. [2] The positive electrode active material for a secondary battery according to claim 1, wherein the particles of the lithium transition metal composite oxide are etched into a cross section using a focused ion beam (FIB) device, and when 20 or more secondary particle cross sections are observed using a scanning electron microscope (FE-SEM), the average number of primary particles in secondary particles in a cross section is 20 or less. [3] A positive electrode active material for a secondary battery according to claim 1 or claim 2, wherein the first dopants are contained in the total content of 2,000 to 6,000 ppm. [4] The positive electrode active material for a secondary battery according to any one of claims 1 to 3, wherein the first dopants are contained in the total content of 2,500 to 5,500 ppm. [5] The positive electrode active material for a secondary battery according to any one of claims 1 to 4, wherein the first dopants are contained in the total content of 3,000 to 5,000 ppm. [6] The positive electrode active material for a secondary battery according to any one of claims 1 to 5, wherein the second dopants are contained in the total content of 500 to 3,000 ppm. [7] The positive electrode active material for a secondary battery according to any one of claims 1 to 6, wherein the second dopants are contained in the total content of 700 to 2,700 ppm. [8] The positive electrode active material for a secondary battery according to any one of claims 1 to 7, wherein the second dopants are contained in the total content of 1000 to 2500 ppm. [9] A positive electrode active material for a secondary battery according to any one of claims 1 to 8, wherein the particles of the lithium transition metal composite oxide have a specific surface area of 0.2-0.7 m 2 / g. [10] A positive electrode active material for a secondary battery according to any one of claims 1 to 9, wherein the particles of the lithium transition metal composite oxide have a specific surface area of 0.25-0.7 m 2 / g. [11] A positive electrode active material for a secondary battery according to any one of claims 1 to 10, wherein the particles of the lithium transition metal composite oxide have a specific surface area of 0.3-0.7 m 2 / g. [12] The positive electrode active material for a secondary battery according to claim 2, wherein the particles of the lithium transition metal composite oxide have an average number of primary particles in secondary particles in a cross section of 10 or less. [13] The positive electrode active material for a secondary battery according to any one of claims 1 to 12, wherein the lithium transition metal composite oxide has a nickel (Ni) content of 60 mol% or more in a total content of metals excluding Li (lithium). [14] The positive electrode active material for a secondary battery according to any one of claims 1 to 13, wherein the lithium transition metal composite oxide has a nickel (Ni) content of 65 mol% or more in a total content of metals excluding Li (lithium). [15] The positive electrode active material for a secondary battery according to any one of claims 1 to 13, wherein the lithium transition metal composite oxide has a nickel (Ni) content of 70 mol% or more in a total content of metals excluding Li (lithium). [16] The positive electrode active material for a secondary battery according to any one of claims 1 to 12, wherein the lithium transition metal composite oxide has a nickel (Ni) content of less than 60 mol% in the total content of metals excluding Li (lithium). [17] The positive electrode active material for a secondary battery according to any one of claims 1 to 16, wherein the lithium transition metal composite oxide includes the first dopants Al and Mg and the second dopants Ti and Y. [18] The positive electrode active material for a secondary battery according to any one of claims 1 to 17, wherein the lithium transition metal composite oxide includes two first dopants selected from the group consisting of Al and Mg, and two second dopants selected from the group consisting of Ti and Y. [19] A positive electrode active material for a secondary battery, wherein the material is a lithium transition metal composite oxide including nickel (Ni), cobalt (Co) and manganese (Mn), wherein the lithium transition metal composite oxide includes two first dopants selected from the group consisting of Al and Mg, and two second dopants selected from the group consisting of Ti and Y, and Particles of the lithium transition metal composite oxide have a crystallite size of 170-300 nm. [20] A positive electrode for a secondary battery comprising the positive electrode active material according to any one of claims 1 to 19. [21] A lithium secondary battery comprising the positive electrode according to claim 20.
Citation Information
Patent Citations
Cathode active material for secondary battery, manufacturing method therefor, and lithium secondary battery comprising same
EP3843181A1
Electrochromism element
KR1020180129161A
Modular system for magnetic generation
KR102095357B1