Solid fuel for a combustion chamber of a hybrid rocket engine and molding device for the production of a solid fuel

A solid fuel for hybrid rocket engines, composed of a hydrocarbon fuel and a cold-curing resin carrier, addresses production complexities and air bubbles, ensuring even combustion and high regression rates with cost-effective, flexible manufacturing.

DE202023002826U1Active Publication Date: 2024-11-14DEUTSCHES ZENTRUM FÜR LUFT UND RAUMFAHRT E V
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
DE202023002826
Authority / Receiving Office
DE · DE
Patent Type
Utility models
Current Assignee / Owner
Filing Date
2023-08-22
Publication Date
2024-11-14
Estimated Expiration
2033-08-31

AI Technical Summary

Technical Problem

Existing solid fuels for hybrid rocket engines face issues such as complex production processes, limited structural integrity, high costs, and low regression rates, with known methods leading to air bubbles that disrupt combustion.

Method used

A method involving a solid fuel composed of a hydrocarbon fuel component and a liquid carrier component, where the carrier component is introduced to envelop the fuel, forming a homogeneous mixture without air bubbles, using a cold-curing resin that hardens at ambient temperature, allowing for complex geometries and cost-effective production.

Benefits of technology

The solution ensures even combustion, high regression rates, and improved structural integrity while reducing production costs and avoiding air bubbles, enabling flexible and efficient manufacturing of solid fuels for hybrid rocket engines.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Solid fuel (12) for a combustion chamber (46) of a hybrid rocket engine, obtainable by a method in which the solid fuel is formed into a solid shape suitable for use in a combustion chamber (46), which forms the solid fuel body (10), wherein the solid fuel (12) comprises a fuel component (14) and a carrier component (16), wherein the fuel component (14) with or consisting of hydrocarbons, in particular paraffin, is filled into a molding device (26) and the carrier component (16) is introduced in liquid form at a lower end (36) into the molding device (26) and wherein the carrier component (16) penetrates the fuel component (14), in particular being largely free of bubbles between components of the fuel component (14).
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a solid fuel for a combustion chamber of a hybrid rocket engine and a molding device for producing such a solid fuel.

[0002] Hybrid rocket engines typically use a solid fuel and a liquid oxidizer. The fuel is stored as a solid fuel in the combustion chamber, in the form of at least one solid fuel body or fuel block, right from the engine's manufacture. To achieve high thrust, as much fuel as possible must be burned per unit of time. The regression rate describes the thickness of the fuel block that is converted during combustion per unit of time. A high regression rate is desirable.

[0003] Solid fuels often used are hydrocarbon compounds, such as polyethylene (PE), hydroxyl-terminated polybutadiene (HTPB) or paraffin.

[0004] The known solid fuels each have specific disadvantages. For example, the production of a fuel block from paraffin, usually via casting and curing processes, is complicated or limited to simple geometries. Large fuel blocks exhibit poor structural integrity. Hydroxyl-terminated polybutadiene is expensive, difficult to obtain, and has a comparatively moderate regression rate. Polyethylene also has a low regression rate.

[0005] From DE 10 2022 131 112, a process for producing a solid fuel is known, in which a fuel component and a carrier component are filled into a mold and hardened therein. Furthermore, a solid fuel comprising the fuel component and the carrier component is known.

[0006] A disadvantage of the method according to DE 10 2022 131 112 is that the carrier component typically has air bubbles after hardening, which can lead to an interruption of the combustion of the solid fuel.

[0007] The invention is based on the objective of providing an improved solid fuel for a hybrid rocket engine and a suitable molding device for its production.

[0008] The problem is solved for the solid fuel with the features of claim 1 and for the forming device according to claim 2.

[0009] In a process by which a solid fuel according to claim 1 is obtainable and which is suitable for producing a solid fuel body for a hybrid rocket engine, the solid fuel is formed into a solid shape suitable for use in a combustion chamber, thus forming the solid fuel body. The solid fuel comprises a fuel component and a carrier component, wherein the fuel component, in particular containing or consisting of hydrocarbons, for example paraffin, is filled into a molding device, and the carrier component, in liquid form, is introduced into the molding device at a lower end. The fuel component and the carrier component can form a mixture of fuel component and carrier component, wherein the components are advantageously movable relative to one another.

[0010] The solid fuel is suitable for combustion in the hybrid rocket engine. When the carrier component is introduced into the mold, it can surround, and in particular enclose, the fuel component. After curing, the fuel component can be permeated by the carrier component, forming a homogeneous solid fuel body. After curing, the carrier component and the fuel component are fixed to each other, forming a single block of material, specifically a fuel block.

[0011] It is advantageous to supply the carrier component at the bottom, as the carrier component is liquid and can rise slowly in the mold due to the material being fed into it. The carrier component can flow into the spaces between the fuel component and gradually fill them. The formation of air bubbles in the carrier component can be avoided, and in particular prevented, because material of the carrier component is constantly flowing in. Any air bubbles can rise to the top and escape the mixture of fuel component and carrier component. The carrier component can thus completely encapsulate the fuel component. The carrier component is advantageously free of air bubbles. This ensures the formation of an air-bubble-free, homogeneous solid fuel body. This is advantageous because air bubbles in the solid fuel can hinder its uniform combustion.

[0012] "Suitable for combustion in the hybrid rocket engine" means that the carrier component is thermally decomposable and / or flammable. Preferably, the carrier component also serves as an energy carrier, which is used as fuel.

[0013] "Permeated" means that the fuel component is present in the carrier component in a type of fuel-carrier component composite, preferably distributed as uniformly as possible. For example, the fuel component is present in the solid fuel body with the most uniform particle distribution possible. This results in specific, and in particular as uniform as possible, combustion properties of the solid fuel throughout its volume. The combustion process cannot be interrupted because there are no air bubbles that could impede combustion.

[0014] Particular advantages arise when the carrier component comprises or is formed from a cold-curing (especially at ambient temperature) material that is castable before curing. Specifically, the carrier component can comprise or be formed from a casting resin, for example, an epoxy resin. Epoxy resin is inexpensive and readily available. The cold-curing material can advantageously be a cold-curing thermoset resin. The cold-curing material is typically liquid at room temperature, thus ensuring castability. In particular, the liquid carrier component made from the cold-curing material can be fed to the mold in liquid form at comparatively low temperatures, preferably at ambient temperature, especially at the lower end of the mold. The cold-curing material can cure without the application of heat and form the solid, homogeneous fuel body.Ideally, the carrier component contains the resin and a hardener. Once the resin and hardener are mixed, a curing process can begin after some time, and the resin and hardener begin to crosslink to form a polymer composite.

[0015] In contrast, in conventional manufacturing processes, especially when using paraffin as a solid fuel, the fuel is melted and poured into the desired shape. The molding device must be heat-resistant, and the cooling process must ensure that precisely one solidification front moves through the block to prevent cracking. This can limit possible geometries.

[0016] With this process variant, the molding device does not need to be heat-resistant, which allows for comparatively low costs. Furthermore, the risk of cracking within the fuel block during the curing process is minimized, even with complex geometries. The molding device can be manufactured cost-effectively and, thus, allowing for a wide range of possible shapes, using an additive manufacturing process.

[0017] In a further embodiment of the process by which the solid fuel is obtained, the carrier component has a foam structure whose pore size is, for example, a maximum of 1 / 4 of the average particle size of the fuel component. In this way, if necessary, the mass ratio can be advantageously shifted toward the fuel component while maintaining the same volume fraction of the fuel component and the carrier component.

[0018] The process for obtaining the solid fuel may advantageously include at least the following steps: S120: Introducing, in particular pouring, the fuel component into the molding device, S 130: Introducing the carrier component, especially a cold one, into the molding device at a lower end, S150: Curing of the carrier component to form the solid fuel with the fuel component.

[0019] During the curing process in step S150, the temperature can be kept constant. In process step S110, the mold is prepared. In step S140, the carrier component can exit the channels through an opening at the bottom and rise within the mold. Advantageously, the carrier component can rise upwards and displace any air located between the fuel component pellets. This prevents the formation of air bubbles.

[0020] In one embodiment of the method, the fuel component is in solid, granular form prior to step S120, for example in pellet and / or pastille form. Advantageously, the fuel component is in the form of paraffin pellets. The diameter of the pellets can be between 0.5 mm and 5 mm. Alternatively, particularly for pellets with a diameter of less than 0.5 mm, provision can be made to at least partially mix the fuel component with the carrier component before filling the molding device. This creates a homogeneous mass of fuel component and carrier component, which can then be filled, in particular poured or introduced, into the molding device.

[0021] The maximum size of the individual particles is preferably less than 10 mm, e.g., a maximum of 6 mm. This eliminates the need to heat the fuel component before pouring it into the mold; it can simply be poured in cold. The carrier component, subsequently introduced or poured, can then fill the resulting cavities between the particles. Furthermore, paraffin pastilles, in particular, are readily available and inexpensive.

[0022] Ideally, epoxy resin L with hardener W 300 can be used. The viscosity can be 300 ± 100 mPas. An epoxy resin with a lower viscosity can also be used. When using an epoxy resin with a higher viscosity, the infusion time and / or pouring time may increase. As long as the infusion time and / or pouring time does not exceed the resin's settling time, the process can still be carried out, provided the flowability of the carrier component is maintained and no pasty consistency develops.

[0023] The feed rate can be arbitrary, with the introduction and / or pouring process being completed before resin curing begins. A typical mold size has a height of 170 mm. The pouring process typically takes approximately 45 minutes. The amount of epoxy resin used can be approximately 1900 g. This results in an average feed and / or pouring rate of approximately 40 g / min.

[0024] For example, six channels, in particular supply channels, may be provided. The channels, in particular supply channels, may have a diameter of approximately 4 mm.

[0025] At a density of 1100 kg / m³ 3 With six supply channels with a diameter of 4 mm, the supply speed is 8.5 mm / s.

[0026] The channels can be conveniently located in a corner of a combustion channel recess. The channels can have a nearly square cross-section and an edge length of approximately 7 mm. At the end of the combustion chamber, the channels can terminate and be connected to the fuel block via a round 4 mm opening.

[0027] In a favorable embodiment of the method, the carrier component is introduced into the molding device, particularly between the fuel component, through at least one channel, and in particular several channels, at its lower end. The at least one channel, and in particular the several channels, allows for a targeted and metered supply of the carrier component. Furthermore, the at least one channel, and in particular the several channels, allow for targeted placement at a selected location. The selected location can be defined by the arrangement of outlet openings on the channels. Preferably, the outlet openings are arranged at the lower end of the channels. In particular, the feed rate of the carrier component can be regulated and / or controlled.

[0028] After the carrier component is inserted into the mold at its lower end, it can rise within the mold and slowly penetrate the fuel component. Air bubbles located between the fuel components can be forced upwards and thus escape.

[0029] It may be provided to arrange special vent lines at the upper end of the molding device.

[0030] In a further embodiment of the method, the fuel component is compacted in the molding device during and / or after step S120, before and / or during step S130.

[0031] The mass fraction of the fuel component compared to the carrier component can be increased if the fuel component is compacted in the molding device (compared to the uncompacted input) during and / or after step S120, before and / or during step S130, for example by means of pressure, vibration of the molding device or the like.

[0032] A uniform fuel distribution within the carrier component is achieved by securing the fuel component in the molding device after step S120, before and / or during step S130, in particular by means of a fluid-permeable securing device, e.g., a perforated disk, on an upper side of the fuel component bed. This prevents the fuel component from floating against the direction of gravity during the pouring of the carrier component.

[0033] Advantageous combustion properties can result if the mass fraction of the fuel component compared to the mass fraction of the carrier component within the solid fuel is between 30% and 80%, preferably 50% or more.

[0034] In preferred process variants for obtaining the solid fuel, it may be provided that the solid fuel is removed from the mold, particularly after hardening, or that the mold remains at least partially attached to the solid fuel. In the latter variant, the mold is designed to be thermally decomposable and / or combustible, at least largely without leaving residue, and is inserted into the combustion chamber when the hybrid rocket engine is loaded with the solid fuel.

[0035] According to a further aspect of the invention, a solid fuel body for a hybrid rocket engine is provided, wherein the solid fuel comprises a fuel component and a carrier component, wherein the carrier component surrounds the fuel component and, in particular, can be present largely bubble-free between constituents of the fuel component. Bubble-free means that no gas bubbles, in particular no air bubbles, are present in the cured material of the carrier component.

[0036] The resulting solid fuel combines the advantages of a high regression rate with beneficial manufacturing possibilities through the use of the carrier component. The carrier component advantageously serves to maintain high structural integrity of the solid fuel, even in shapes with complex geometries.

[0037] Another aspect of the invention relates to a molding device for producing a solid fuel body with a solid fuel comprising a fuel component and a carrier component, wherein the molding device has an outer shell enclosing a volume and at least one channel for supplying, in particular several channels, in particular supply channels for supplying the liquid carrier component.

[0038] In one embodiment of the molding device, the at least one channel, in particular the feed channels, has openings at the lower end through which the carrier component can exit into the molding device.

[0039] It is advantageous if the channels, especially feed channels, can be filled at the upper end and each has at least one opening, and preferably several openings, at a lower end. The openings can advantageously be evenly distributed around the circumference of the respective channels. Through the at least one opening, and preferably the several openings, the carrier component can be introduced into the mold at the lower end and slowly rise upwards from there.

[0040] The molding device can be created, in particular, using an additive manufacturing process (3D printing). 3D printing allows even geometrically complex shapes to be flexibly replicated in a cost-effective manner. 3D printing allows the molding device to be manufactured without the need for rework.

[0041] The resulting solid fuel offers an advantageous application in a hybrid rocket, particularly in a combustion chamber, where the solid fuel is produced according to the aforementioned method. The solid fuel advantageously contains no bubbles, especially no air bubbles, and is present as a bubble-free solid fuel. The use of this solid fuel advantageously enables uniform combustion of the solid fuel in the combustion chamber. The detection of bubbles in the solid fuel can be carried out, for example, using a bubble detector. This allows for simple monitoring, particularly non-destructive quality control, of the produced solid fuel.

[0042] The invention will now be explained in more detail using an exemplary embodiment and with reference to the drawings. The drawings show: Fig. 1 a schematic sectional view of a solid fuel body according to the invention with a solid fuel, Fig. 2 a schematic sectional view of the solid fuel according to the invention in a molding device, Fig. 3 a schematic view of a hybrid rocket engine, Fig. 4 a schematic view of a hybrid rocket, Fig. 5 a method for producing the solid fuel body.

[0043] Fig. Figure 1 shows a schematic representation of a solid fuel body 10 containing a solid fuel 12 for a hybrid rocket engine. The solid fuel 12 comprises a fuel component 14 and a carrier component 16. The fuel component 14 has a hydrocarbon as its energy carrier or is formed from one. The solid fuel 12 preferably contains or consists of paraffin. The fuel component 14 is preferably in particulate form prior to the production of the solid fuel, for example, as solid, granular particles, such as pellets and / or pastilles, which are contained within the solid fuel body 10. Fig. Figure 1 is represented as circles. The particle size of the granules is typically between 0.5 mm and 10 mm. An advantageous form available as an inexpensive mass-produced item is, for example, lentil-shaped paraffin pastilles, which can have a diameter of approximately 5 mm and a height of 2 mm to 3 mm.

[0044] The carrier component 16 comprises a cold-curing material that is pourable before hardening. In particular, the carrier component 16, especially the cold-curing material, is in liquid form before hardening. Advantageously, the carrier component 16 comprises or is formed from a casting resin. The casting resin is a synthetic resin that is processed in liquid form into the final product and solidifies as this or as a component thereof. The still-liquid casting resin can be poured or introduced into a reusable mold. After a hardening process, the carrier component 16 encloses the fuel component 14, especially the particles of the fuel component 14, and forms a homogeneous solid fuel body 10. The carrier component 16 is depicted within the solid fuel body 10 as irregular dots, illustrating that the carrier component 16 is arranged between the fuel component 14.Paraffin is a particularly suitable, inexpensive and easily available material due to its high regression rate.

[0045] The carrier component 16 comprises, or is formed from, a thermoset that is liquid at room temperature and before a curing process. For example, the carrier component 16 comprises, or is formed from, an epoxy resin. In particular, the carrier component 16 comprises epoxy resin L with hardener W 300. The supplier specifies a viscosity of 300 ± 100 mPas. However, an epoxy resin with a lower viscosity can also be used. If an epoxy resin with a higher viscosity is used, the casting time is increased. As long as this does not exceed the resin's drip time, the process can still be carried out, provided the carrier component retains its flowability and does not become pasty.

[0046] The carrier component 16 can alternatively be or consist of a polyurethane (PUR), a phenolic resin, a urea and melamine resin, a polyester resin and / or a silicone.

[0047] The carrier component 16 penetrates the fuel component 14 in that the particles of the fuel component 14 are embedded in a kind of matrix composed of the carrier component 16, forming a fuel component-carrier component composite. The particle distribution of the fuel component 14 within the carrier component 16 is as homogeneous as possible to ensure uniform combustion properties. The carrier component 16 is suitable for combustion in the hybrid rocket engine.

[0048] The mass fraction of the fuel component 14 compared to the mass fraction of the carrier component 16 within the solid fuel 12 is, for example, between 30% and 80%, preferably 50% or more.

[0049] The solid fuel body 10 has an outer contour 18 adapted to the geometry of the hybrid rocket engine. Typically, the solid fuel body 10 has a rectangular outer contour 18 with a length 20 and a width 22, and a thickness (not shown). The outer contour 18 can be rectangular or cylindrical. In the case of a cylindrical outer contour, the width 24 and the thickness then correspond to the diameter. The length 20 can, for example, be 5 m. The solid fuel body 10 can be a compact cylinder or have an internal structure, in particular a hollow structure.

[0050] Fig. Figure 2 shows a schematic sectional view in the longitudinal direction of the solid fuel body 10 within a molding device 26. The molding device 26 here has, by way of example, a simple geometric shape 28 into which the solid fuel 12 is to be placed.

[0051] The molding device 26 has a first side 30, or longitudinal side 30, which defines the length 20 of the solid fuel body 10. The second side 32, or bottom side 32, defines the thickness and / or width 22 of the solid fuel body 10. The first side 30 and the second side 32 form a shell 33 of the molding device 26. In the case of a cylindrical molding device 26, the second side 32 is the diameter of the cylindrical molding device 26. A third side 34 can be closed with a lid 35 or open, for example, to fill material into the molding device 26.

[0052] A feed device 38 with channels 38, in particular feed channels 38 for the supply of the carrier component 16, is provided on the forming device 26. In the forming device 26, which in Fig. Figure 2 shows two exemplary feed channels 38. The feed channels 38 for introducing the liquid carrier component typically extend from an upper end 37 of the molding device 26 towards the side 32. For example, the feed channels 38 can have a spiral shape.

[0053] At a lower end 36, marked by arrows 36, the feed channels 38 each have at least one opening 39, and in particular several openings 39, through which the liquid carrier component 16 can exit the channels 38 and distribute itself among the pellets of the fuel component 14. During the manufacturing process of the solid fuel body 10, the carrier component 16 is introduced into the feed channels 38 as a pourable, and in particular liquid, material, especially from above. The carrier component 16 is a cold-curing material. Preferably, several channels 38, for example six feed channels 38, are provided. The multiple channels 38 are arranged on the circumference of the mold 26 and configured so that the pourable material can be introduced into an interior space of the mold 26.

[0054] The channels 38, in particular feed channels 38, can typically have a diameter of approximately 2 mm to 10 mm. The diameter is selectable depending on the size of the molding device 26 and can influence the filling speed of the molding device with the support component 16.

[0055] At a density of 1100 kg / m³ 3 With six channels 38 with a diameter of 4 mm, this results in a feed velocity of 8.5 mm / s.

[0056] The channels 38 can be advantageously arranged in a corner of a combustion chamber bulge. The channels 38 can have an almost square cross-section and an edge length of approximately 7 mm. At the end of the combustion chamber, the channels 38 can terminate and be connected to the fuel block 10 via a round opening 4 mm in diameter.

[0057] For the application, the shaping device 26 may have a complex geometry, for example comprising irregular surfaces and / or angles and / or it may be designed to form structures within the solid fuel body 10 in order to obtain an outer contour 18 and thus shape 18 of the solid fuel body 10 that is optimized for use within a specific combustion chamber.

[0058] The carrier component 16, once cured, retains the shape defined by the mold 26 before curing, even after the mold 26 is removed. After curing, the solid fuel body 10 can be removed from the mold 26, or the mold 26 can remain at least partially attached to the solid fuel 12 (for example, in the area of ​​structures). In the latter case, the mold 26 is designed to be thermally decomposable and / or combustible, at least to a large extent, and is inserted into the combustion chamber when the hybrid rocket engine is loaded with the solid fuel 12.

[0059] Fig. Figure 3 shows a schematic isometric representation of an embodiment of the molding device 26. The molding device 26 has a substantially cylindrical geometry. The casing 33 is cylindrical in shape. The third side 34 shows a circular opening 40 and, inside, a geometric structure 42, e.g., with radially outward-pointing extensions. The geometric structure 42 corresponds to a monoport fuel block 10 whose outer contour rests directly against a supporting GRP structure of the combustion chamber and is realized internally by a 3D-printed structure with six longitudinally twisted protrusions. The channels 38 for supplying the carrier component 16 are visible. The channels 38 extend to the lower region 36 of the molding device 26, where the outlet openings are located.When the carrier component 16 is fed into the channels 38, the carrier component 16 flows into the channels 38 until it exits through the openings 39 and is distributed in the already filled fuel component 14. The carrier component 16, as a liquid, penetrates the individual pellets of the fuel component 14 and forces the air present between the pellets of the fuel component 14 upwards. This continues until a mixture of the pellets of the fuel component 14 and the carrier component 16 is present and the molding device 26 is filled with the mixture.

[0060] Fig. Figure 3 shows a schematic isometric view of a section of a hybrid rocket 44 with the combustion chamber 46. The combustion chamber 46 has channels 38 for supplying the liquid carrier component 16. The space for the solid fuel body 10 is also visible; it is located, or will be located, between a support structure 56 for a GRP (glass fiber reinforced plastic) shell (not shown). A connecting element 58 to a valve section 50 is also shown. An injector plate 60 and a heat shield 62 are arranged between the combustion chamber 46 and the connection 58 to the valve section 50.

[0061] Fig. Figure 4 shows a schematic representation of a prototype of the hybrid rocket 44 with the combustion chamber 46, into which the solid fuel body 10 is installed. The hybrid rocket 44 also has an oxidizer tank 48 and a valve section 50. The oxidizer can be metered from the oxidizer tank 48 into the combustion chamber 46 by means of the valve section 50. A nozzle 52 is located behind the combustion chamber 46. A payload 54 can be positioned in the forward section.

[0062] Fig. 5 shows a method 100 for producing the solid fuel body 10. In the first method step S110, the molding device 26 is provided.

[0063] In the second method step S120, the fuel component 14, which is in the form of pellets or pastilles 15, is filled, in particular poured, into the molding device 26.

[0064] In process step S130, the carrier component 16 is filled into the channels 38 at the upper end 37. It emerges in liquid form at the lower end 36 of the channels 38 and rises, particularly slowly, between the pellets of the fuel component 14. The carrier component 16 is present, in particular, as a cold carrier component 16 (i.e., approximately at ambient temperature, or at least at temperatures below 100 °C, and especially below 50 °C) during step S130.

[0065] Epoxy resin L can be used advantageously with hardener W 300. The mixing ratio of resin to hardener is, for example, 100:35, meaning 100 parts resin and 35 parts hardener are mixed. Hardener W 300 is typically a polyether diamine. The epoxy resin is typically a 2,2'-[(1-methylethylidene)bis(4,1-phenyleneoxymethylene)] bisoxirane hexanediol diglycidyl ether bisphenol F epichlorohydrin resin. The viscosity can be 300±100 mPas. A lower viscosity epoxy resin can also be used. Using a higher viscosity epoxy resin may increase the induction time and / or casting time. As long as the induction time and / or pouring time does not exceed the drip time of the resin, the process can still be carried out, as long as the flowability of the carrier component 16 is maintained and no pasty behavior occurs.

[0066] The feed rate can be arbitrarily selected, with the introduction and / or pouring process being completed before the resin curing begins. A typical mold size has a height of 170 mm. The introduction and / or pouring process typically takes approximately 45 minutes. The amount of epoxy resin can be approximately 1900 g of resin. This can result in an introduction and / or pouring rate of approximately 40 g / min on average.

[0067] In process step S140, the carrier component 16 rises in the molding device 26 until it completely envelops the fuel component 14 and the molding device 26 is filled. The carrier component 16 spreads into the spaces between the pellets of the fuel component 14 to form a composite mixture of fuel component 14 and carrier component 16. Within this composite mixture, the fuel component 14 and the carrier component 16 remain movable relative to each other because the carrier component 16 is still liquid. Any air that was present between the pellets of the fuel component 14 has been almost completely expelled from the spaces after process step S140.

[0068] In process step S150, the curing process begins. Curing process S150 typically occurs through chemical cross-linking of the individual components of the carrier component 16. This curing process is made possible by the fact that the carrier component 16 comprises a mixture of the resin, in particular epoxy resin, and the hardener, for example, W 300. The resin-hardener mixture cures without an increase in temperature. This mixture is referred to as the cold-curing carrier component 16. The carrier component 16 thus comprises, or is formed from, a cold-curing material that is castable before curing, in particular a casting resin.

[0069] The curing of the carrier component 16, in particular the casting resin, occurs spontaneously in the cold-curing resin. Curing can also be accelerated by the application of ultraviolet radiation or moisture. In process step S150, the viscosity initially increases continuously until a so-called gelling point is reached and the resin transitions into the solid state. Within the gelled, solid resin, the chemical reaction continues until the polymer network is fully formed and the final properties are achieved. After step S150, the solid fuel body 10 exists as a solid. The previously liquid carrier component 16 has cured and essentially completely and without air bubbles encapsulates the fuel component 14, in particular the fuel pellets.

[0070] The solid fuel 12 combines the advantage of paraffin in particular as fuel component 14, which has a high regression rate (conversion of a fuel thickness within the solid fuel (fuel block) per unit time), with the simple and diverse manufacturing possibilities with cold-curing casting resins as carrier component 16. In addition to the positive structural properties of the carrier component 16, the chemical energy stored therein can also be used as fuel.

[0071] During or after the introduction of the fuel component 14 in process step S120, the mass fraction of the fuel component 14 can be increased by compacting it in the molding device 26, for example by shaking the molding device and / or applying pressure to the bed of fuel component 14.

[0072] Furthermore, to secure the bed of fuel component 14, particularly after compaction, a fluid-permeable securing device can be placed on top of the bed. The securing device can be, for example, a perforated disc, a grid, or the like, through which the particles cannot pass. The securing device can be in the form shown in Fig. The forming device 26 shown in section 3 is arranged on the pellets of the fuel component 14.

[0073] Floating of the fuel component 14 against the direction of gravity can preferably be prevented by means of the fixing device, so that at least a largely uniform distribution of the fuel component 14 is achieved both over the cross-section and over the height of the forming device 26 within the support component 16.

[0074] After the carrier component 16 has hardened within the molding device 26, the solid fuel body 10 is formed.

[0075] Optionally, in process step S160, the solid fuel body 10 can be removed from the molding device 26. Alternatively, the molding device 26 or parts of the molding device 26 can be burned together with the solid fuel body in the hybrid rocket.

[0076] Due to the preferably cold manufacturing process, without heating any of the components, the molding device 26 does not need to be heat-resistant. This increases cost-effectiveness and / or the possible variety of shapes. The molding device 26 can be manufactured, for example, using an additive manufacturing process (3D printing), thereby increasing the number of possible geometries for an optimized combustion process within the combustion chamber. Furthermore, no cooling process is required, which could lead to cracking, particularly when using paraffin as fuel and especially with more complex geometries, and would limit the possible geometries.

[0077] Thus, by means of the specified method for manufacturing the solid fuel body 10, a fuel block 10 made of solid fuel 12 can be economically provided, even with complex geometries, for optimized combustion within a hybrid rocket engine 44. Reference symbol 10 solid fuel bodies 12 Solid fuel 14 Fuel component 15 pellets, particles, lozenges 16 Carrier component 18 Outer contour 20 Length 22 width 24 Thickness 26 Forming device 28 geometric shapes 30 first page 32 second page 33 coat 34 third page 35 lids 36 lower side of the mold 37 upper end of the molding device 26 38 channels, feed channels 39 Opening, exit opening 40 circular openings 42 geometric structure 44 hybrid rocket 46 Combustion chamber 48 Oxidizer tank 50 valve section 52 nozzle 54 payload 56 Support structure 58 Connecting element to the valve section 60 Injector plate 62 Heat shield 100 methods for producing a solid fuel body S110 Providing the molding device 26 S120 Filling the fuel component S130 Introduction of the carrier component S140 Ascending of the carrier component in the mold S150 Curing of the fuel component / carrier component mixture S160 Removing the solid fuel body from the mold QUOTES CONTAINED IN THE DESCRIPTION

[0000] This list of documents submitted by the applicant was generated automatically and is included solely for the convenience of the reader. This list is not part of the German patent or utility model application. The DPMA assumes no liability for any errors or omissions. Cited patent literature

[0000] DE 10 2022 131 112 [0005, 0006]

Claims

[1] Solid fuel (12) for a combustion chamber (46) of a hybrid rocket engine, obtainable by a process in which the solid fuel is brought into a solid form suitable for use in a combustion chamber (46), which forms the solid fuel body (10), wherein the solid fuel (12) has a fuel component (14) and a carrier component (16), wherein the fuel component (14) with or consisting of hydrocarbons, in particular paraffin, is filled into a molding device (26) and the carrier component (16) is introduced in liquid form at a lower end (36) into the molding device (26), and wherein the carrier component (16) penetrates the fuel component (14), in particular is present largely free of bubbles between components of the fuel component (14). [2] A molding device (26) for producing a solid fuel (12) according to claim 1, comprising a fuel component (14) and a carrier component (16), wherein the molding device (26) has an outer shell (33) enclosing a volume and supply channels (38) for supplying the liquid carrier component (16). [3] Forming device (26) according to claim 2, characterized by that the channels (38), in particular supply channels (38), can be filled at the upper end (37) and each have at least one opening, in particular a plurality of openings (39) at a lower end (36).

Citation Information

Patent Citations

  • Method for producing a solid fuel for a hybrid rocket engine and solid fuel

    DE102022131112A1