PLASTIC-BASED MATERIALS FOR PROCESSING BY GENERATIVE MANUFACTURING METHODS
Patent Information
- Application Number
- DE502017016528
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2016-06-02
- Filing Date
- 2017-05-23
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2037-05-23
AI Technical Summary
Current SLS process materials, such as semi-crystalline polyamides and polyaryl ether ketones, lack sufficient flame protection for applications in the electrical/electronic sector, preventing their use in this industry.
A powder blend of amorphous polyetherimide (PEI) and polyphenylene sulfide (PPS) is developed for the SLS process, with a specific temperature alignment between the glass transition and crystallization melting points to enhance flame retardancy and tracking resistance.
The blended powder provides components with intrinsic flame protection and resistance to tracking current, suitable for the electrical/electronic sector, by optimizing the temperature-dependent sintering and cooling processes in the SLS method.
Description
[0001] The invention relates to a powder for processing in an SLS process.
[0002] The Selective Laser Sintering process is a powder- and beam-based process in which plastic bodies of virtually any geometry are built up layer by layer without tools or molds. The surface quality and the z-direction dependence of the mechanical properties are improved compared to the FDM (fused deposition modeling) process, in which a workpiece is built up layer by layer from a meltable plastic. Workpieces manufactured using SLS generally exhibit less pronounced anisotropy in their mechanical properties.
[0003] In the Selective Laser Sintering (SLS) process, products are manufactured by locally fusing powdered layers of materials with a wide range of properties, specifically developed for this process, using selective laser radiation. Compared to other additively processed plastics, laser-sintered components not only exhibit very high mechanical and / or chemical resilience, but also very high heat resistance. The SLS process is particularly characterized by the temperature difference between the crystallite melting temperature and the crystallization temperature of semi-crystalline plastics. The temperature window between these two temperatures defines the melting and solidification processes and thus the heating and cooling phases.
[0004] To date, semi-crystalline polyamides, polyaryletherketones, and urethane-based polymers have been processed in the SLS process. These plastics can be used to produce components that do not yet offer sufficient flame retardancy, particularly for applications in the electrical / electronics (E&E) sector. Therefore, the SLS process has not yet been used to manufacture components for the E&E sector.
[0005] US2015 / 0145168A1 discloses a method for printing a 3D part with an additive manufacturing system, the method comprising providing a part material comprising in its composition one or more semi-crystalline polymers and one or more amorphous polymers substantially miscible with the one or more semi-crystalline polymers.
[0006] JPS63312355A discloses a composition containing a polyphenylene sulfide with a certain polyetherimide.
[0007] The object of the present invention is therefore to provide a plastic for processing in the SLS process which, in addition to sufficient tracking resistance for use in the E&E sector, offers flame protection, in particular intrinsic flame protection.
[0008] The solution to the problem and the subject matter of the present invention is therefore a powder according to claim 1 for processing in an SLS process, comprising a blend of at least amorphous PEI and PPS.
[0009] A "blend" or "polyblend" refers to a mixture of two or more different polymers. The properties of the resulting plastics differ from those of the original polymers. Nevertheless, it is predominantly a purely physical mixture without the formation of new chemical bonds, as is required for copolymers, for example.
[0010] According to an advantageous embodiment of the invention, the crystallization melting point of the semi-crystalline components lies in a similar temperature range to the glass transition point of the amorphous components of the blend. For example, the glass transition point of the blend differs from the crystallization melting point of the blend by no more than 25 °C. In particular, it is provided that the two temperatures lie within a temperature difference range of 5 °C to 20 °C.
[0011] According to another embodiment of the invention, the two temperatures—the glass transition temperature of the blend on the one hand and the crystallite melting temperature on the other—are separated by up to 100°C. In individual cases, this can lead to components that are both intrinsically flame-resistant and tracking-resistant.
[0012] According to the invention, the first component, the amorphous thermoplastic, is present in the blend with the second component, the semi-crystalline polymeric material, in a ratio of 0.5 parts amorphous thermoplastic to 1.5 parts semi-crystalline polymeric material to 1.5 parts amorphous thermoplastic to 0.5 parts semi-crystalline polymeric material. For example, the two components are present in the blend in a ratio of 1:1, 0.8:1.2, or 0.9:1.1.
[0013] According to a further advantageous embodiment, it is provided that the powder comprises a blend in which the glass transition temperature of the amorphous thermoplastic and the crystallite melting point of the semi-crystalline polymeric material do not differ by more than 25 °C, in particular in the range from 5 °C to 20 °C.
[0014] The present invention also relates to a component according to claim 3 for use in the electrical / electronics sector with sufficient flame retardancy, which can be produced by the SLS process using a powder with a blend according to the invention. Amorphous PEI (polyetherimide) is generally characterized by a glass transition temperature.
[0015] In contrast, semi-crystalline polyphenylene sulfide systems, such as the commercial polyphenylene sulfide-based material primarily used in the SLS process to date, do not offer sufficiently good flame retardancy. The SLS process is characterized in particular by the temperature difference between the crystallite melting temperature and the crystallization temperature of the semi-crystalline plastics. The temperature window between these two temperatures defines the melting and solidification processes and thus the heating and cooling phases.
[0016] By producing plastic blends of amorphous PEI with polyphenylene sulfide, the properties of both plastic components are utilized. Engineering the glass transition temperature and crystallite and / or crystallization temperature enables processing using SLS processes.
[0017] In addition to the locally limited sintering of the plastic particles of the semi-crystalline component, blend production allows the use of an additional process parameter for the heating and cooling process of the SLS process to improve the properties, in particular to increase flame retardancy, by selecting the amorphous component and its glass transition temperature.
[0018] In the following, the invention is explained in more detail using selected exemplary embodiments: 1. Example that is not claimed:
[0019] A plastic blend of PEI and PA was produced in approximately equal proportions. The blend produced the Figure 1 shown characteristics: Figure 1 shows the reaction kinetics of a blend according to Example 1 with a PEI to PA ratio of 1:1. In the graph, the y-axis indicates the heat flow in mW and the x-axis the temperature in °C.
[0020] The melting peak of semi-crystalline PA at 220°C overlaps with the glass transition of PEI at approximately 217°C. The glass transition of PEI is reflected in the pronounced shoulder 1 in this temperature range. During the SLS process, the laser heats the powder of the plastic blend above the melting point of the semi-crystalline component.
[0021] When processing the blend from Example 1 using the SLS process, the glass transition temperature of the PEI overlaps with the crystallite melting temperature of the PA in the range between approximately 217°C and 220°C. The plastic blend particles are fused together and with the previous layer in the temperature range of approximately 230°C to 270°C, for example, at approximately 260°C.
[0022] The unmelted powder supports the melt at temperatures below 217°C. When selecting PA, a component whose recrystallization begins at 190°C is preferred.
[0023] At the recrystallization temperature of PA of 190°C, the PEI is in a solid state. The blend according to Example 1 of PEI and PA in a ratio of 1:1 produces the Figure 2 shown reaction kinetics during recrystallization. An advantage of the blend according to Example 1 is that - as shown in Figure 2shown - a broad transition from the melt to the solid state takes place, which can be used to reduce stresses in the build space with suitable temperature control during SLS processes.
[0024] In a blend prepared according to Example 1, the crystallization kinetics can be influenced compared to pure semi-crystalline plastics. 2. Example:
[0025] A plastic blend of PEI and PPS was produced in approximately equal proportions. The blend produced the Figure 3 shown characteristics: Figure 3 shows the reaction kinetics of a blend according to Example 2 with a PEI to PPS ratio of 1:1. In the graph, the y-axis indicates the heat flow in mW and the x-axis the temperature in °C.
[0026] The melting peak of PPS at 277.5°C does not overlap with the glass transition of PEI at approximately 217°C.
[0027] When processing the two high-temperature-stable plastic systems at temperatures above 300°C, preferably even higher, for example, at 320°C, the two powders fuse together. Appropriate cooling keeps the environment below the crystallization temperature and / or below the glass transition temperature.
[0028] The combination of amorphous and semi-crystalline plastics (amorphous PEI and PPS) proposed in the invention also results in a complementary or combined range of properties. In addition to good dynamic behavior, the amorphous state should improve damping. The semi-crystalline component should reduce abrasion and improve stress formation compared to a pure amorphous plastic. The semi-crystalline component guarantees good flowability, and the amorphous component lowers shrinkage.
[0029] By changing the mixing ratios of the individual components, i.e. the compound composition, the property profile and / or the process parameters can be adapted as required.
[0030] The invention discloses, for the first time, a powder for processing using the SLS process that combines the properties of a semi-crystalline polymer compound with those of an amorphous polymer compound. Thus, for the first time, components are accessible via the SLS process that have sufficient flame resistance for use in the E&E sector.
Claims
1. Powder for processing in a selective laser sintering method, SLS method, comprising a blend of at least amorphous polyether imide, PEI, and semicrystalline polyphenylene sulfide, PPS, wherein the blend exhibits not only the glass transition temperature but also at least one crystallization melting point, so that additive manufacturing by SLS is achievable with the blend, wherein the blend comprises the amorphous PEI and the PPS in a ratio of 0.5 parts amorphous PEI : 1.5 parts PPS to 1.5 parts amorphous PEI : 0.5 parts PPS.
2. Powder according to any of the preceding claims comprising a blend of amorphous PEI and PPS in a ratio of 0.8 : 1.2.
3. Component for use in the electricals / electronics sector having sufficient flame retardancy which is producible in the SLS method using a powder according to either of Claims 1 and 2.