METHOD FOR MANUFACTURING A FUEL CELL SYSTEM COMPLETING A COMPONENT MADE OF STEEL WITH A NITROGEN-CONTAINING PROTECTIVE LAYER

DE502019012111D1Active Publication Date: 2024-10-02ROBERT BOSCH GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502019012111
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-07-20
Filing Date
2019-07-08
Publication Date
2024-10-02
Estimated Expiration
2039-07-08

AI Technical Summary

Technical Problem

Steel components used in fuel cell systems, particularly those made of martensites or ferrites, suffer from hydrogen embrittlement due to hydrogen diffusion, leading to mechanical property degradation and potential failure.

Method used

A method involving high-temperature nitriding in a nitrogen-containing atmosphere to form a nitrogen-enriched austenitic surface layer, followed by quenching and tempering, which reduces hydrogen diffusion and enhances the component's mechanical properties.

Benefits of technology

The nitrogen-containing protective layer significantly reduces hydrogen embrittlement, allowing steel components to maintain their mechanical properties and be used in hydrogen-containing environments without failure, while adjusting hardness and maintaining desired elastic deformability.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to the use of a component made of steel with a nitrogen-containing protective layer in a fuel cell system and a method for producing such a component. State of the art

[0002] Steel-containing components, particularly in the form of martensites or ferrites, are used for applications in hydrogen atmospheres, for example, in fuel cells. The diffusion of hydrogen into the component can lead to a degradation of the component's mechanical properties, also known as hydrogen embrittlement, and thus to component failure.

[0003] By applying high-temperature nitriding to the component, nitrogen can be dissolved in the edge region of a martensite and a ferrite, allowing an austenitic surface layer to form. The austenitic surface layer and the nitrogen introduced into the component material significantly limit the diffusion of hydrogen into the component. Steel treated in this way offers significant advantages when used in hydrogen environments.

[0004] Document DE 10 2012 216 117 A1 relates to a method for producing a self-tapping screw, wherein a blank made of martensitic hardenable steel is provided, a screw shape is manufactured from the blank, and the screw shape is subsequently hardened at a temperature > 900°C in a nitrogen-containing gas atmosphere. The hardening temperature in the nitrogen-containing gas atmosphere is preferably between 1000°C and 1200°C. The thermochemical process leads to nitriding of the edge zone and thus to increased hardness compared to the base material. The steel of the blank preferably has a chromium content > 12% and / or a nickel content > 2.5%. Following hardening and, if appropriate, quenching, the screw shape is tempered at a temperature between 150°C and 450°C.

[0005] Document WO 2012 / 146254 A1 relates to a method for forming an austenite and / or a martensite, wherein at least nitrogen is dissolved in a workpiece at a temperature T1. Preferably, a nitrogen-containing gas such as N2 is used, wherein the pressure of the gas can be several bar, but also less than 1 bar, such as 0.1 bar. The temperature T1 is preferably more than 1000°C and less than 1350°C, and the high-temperature treatment at temperature T1 is carried out, for example, for more than 20 minutes or even for more than 15 hours. Furthermore, an intermediate cooling step can be carried out. A cooling gas can be nitrogen at a pressure of 6 to 10 bar. The cooling gas is preferably a noble gas such as helium, neon, argon, krypton, xenon, or radon.

[0006] Document DE 10 2008 050 458 A1 discloses jewelry made of a ferritic chromium steel formed from a ferritic core with a substantially martensitic outer layer. Embodiments are also included in which the outer layer still contains a small proportion of residual austenite, depending on the incorporated C and N content of the steel material. The formation of the martensitic outer layer preferably occurs through a heat treatment such as nitriding, wherein the steel material is treated at a temperature between 1000°C and 1200°C in a nitrogen-containing gas atmosphere, followed by cooling. According to one example, the steel grade 1.4016 is nitrided with nitrogen at temperatures above 1050°C, quenched or deep-cooled, and tempered. The inclusion of nitrogen results in a transformation into austenite, with martensite forming during the subsequent quenching.JP 2007 073443 discloses a method for producing a fuel cell system with nitriding. Disclosure of the invention

[0007] A method for producing a steel component with a nitrogen-containing protective layer is proposed. The component produced according to the invention can be used, for example, in a fuel cell system. The method comprises at least the following steps: First, the steel component is annealed in a nitrogen-containing atmosphere to a temperature between 900°C and 1300°C, at which it is held isothermally for a period of between one minute and twelve hours.

[0008] Annealing the component in a nitrogen-containing atmosphere increases nitrogen solubility. Nitrogen diffuses from the nitrogen-containing atmosphere into the steel, forming a nitrogen-containing diffusion zone. This process is also known as high-temperature nitriding. In steels that are ferritic during annealing, an austenitic surface layer develops with sufficient nitrogen input. In steels that are austenitic during annealing, such as martensitic grades, the austenite in the surface layer is enriched with nitrogen and chemically stabilized by sufficient nitrogen input. With sufficient nitrogen input, an austenitic, nitrogen-containing diffusion zone is created, which reduces the diffusion of hydrogen into the component.

[0009] The steel component is then quenched. During quenching, the component is cooled from the temperature achieved during annealing in a relatively short time. Annealing and quenching may harden the steel component. In particular, the nitrogen that previously diffused into the surface layer remains in said surface layer. In steels that exhibit a completely austenitic structure during annealing, quenching results in a transformation into martensite in the insufficiently nitrogen-enriched core, thus resulting in hardening. Steels that are ferritic during annealing remain ferritic in the core during quenching. However, in both cases, the surface layer remains austenitic if the nitrogen content is sufficiently high.

[0010] The component is then deep-frozen to a temperature below -70 °C. Deep-freezing can occur in a temperature range between -70 °C and -273 °C. Deep-freezing serves to reduce the residual austenite content in the core area of ​​martensitic grades. During the transformation to martensite, untransformed austenite may occur in the core area, which is referred to as retained austenite. This retained austenite is converted into martensite by deep-freezing.

[0011] The steel component is then tempered at a temperature above 150 °C. Tempering can be performed, for example, in a temperature range between 150 °C and 600 °C. Tempering reduces the strength compared to the untempered state. This is desirable because it allows for a controlled adjustment of the appropriate strength. Toughness, elongation at break, and ductility, for example, are also improved.

[0012] According to the invention, the steel component is annealed at a nitrogen partial pressure between 50 mbar and 5 bar. The nitrogen content in the surface layer can be adjusted by adjusting the pressure. Depending on the steel, an optimal nitrogen content can be adjusted by adjusting the pressure.

[0013] According to the invention, the steel component is quenched at a quenching pressure between 1 bar and 40 bar. According to a particularly preferred embodiment of the invention, the steel component is quenched at a quenching pressure between 1.5 bar and 10 bar.

[0014] According to the invention, the steel component is quenched using a quenching medium. The quenching medium is a gas selected from the group consisting of nitrogen, argon, and helium. Argon and helium are noble gases. They have a high heat capacity, which allows for a high cooling effect. Furthermore, noble gases do not react with the steel. Although nitrogen reacts with the steel surface in principle, it is already present in the material due to the process. Compared to argon and helium, nitrogen is generally significantly more advantageous.

[0015] The steel component is quenched to a temperature of less than 50 °C.

[0016] Preferably, the steel component is quenched relatively quickly. Rapid quenching advantageously prevents the formation of chromium nitride in the component. Chromium nitride would reduce the component's corrosion resistance.

[0017] According to the invention, the deep freezing of the steel component is carried out over a period of between 15 minutes and 30 minutes.

[0018] The component is tempered in a nitrogen-containing atmosphere. Tempering in a nitrogen-containing atmosphere prevents nitrogen effusion from the material and surface oxidation. The nitrogen partial pressure can, for example, correspond to atmospheric pressure. The tempering time is preferably between 30 minutes and 8 hours.

[0019] The steel used in the component preferably contains between 10 and 20 wt% chromium. Other components of the steel include: carbon of 0 wt% up to 2% by weight, Nitrogen of 0 wt% up to 2% by weight, nickel of 0 wt% up to 2% by weight, manganese of 0 wt% up to 2% by weight, molybdenum of 0 wt% up to 2% by weight, cobalt of 0 wt% up to 2% by weight, copper of 0 wt% up to 2% by weight, aluminum of 0 wt% up to 2% by weight, iron of 64% by weight up to 90% by weight,

[0020] Other elements, such as silicon, can also be included as components in the steel. The sum of the weight percentages of the components amounts to 100 wt%.

[0021] A component manufactured using the method according to the invention and having a nitrogen-containing protective layer is also proposed. This component is, for example, a pipeline for transporting hydrogen for use in a fuel cell system.

[0022] A component according to the invention is used in a fuel cell system, in particular in the form of a pipeline for transporting hydrogen. Advantages of the invention

[0023] As already mentioned, the nitrogen-containing protective layer limits the diffusion of hydrogen into the component. This advantageously reduces or completely prevents hydrogen embrittlement of the component. The susceptibility of the component to a hydrogen-containing atmosphere is thus reduced, allowing the component to be used in a hydrogen-containing atmosphere. The protective layer is advantageously and simply created by the diffusion of nitrogen and the associated formation of a stable austenitic surface layer. This advantageously preserves the properties of the component's base material, especially the mechanical properties of the steel. In particular, the hardness of the component can be adjusted as required. This advantageously maintains the desired elastic deformability of the component. Short description of the drawings

[0024] Embodiments of the invention are explained in more detail with reference to the drawings and the following description.

[0025] They show: Figure 1 is a schematic representation of a process for producing a component from a steel with a nitrogen-containing protective layer in the form of a flow diagram, Figure 2 is a schematic representation of a cross section through a tubular component which is produced with the process described in Figure 1 shown method, and Figure 3 is a schematic representation of a fuel cell system. Embodiments of the invention

[0026] In the following description of the embodiments of the invention, identical or similar elements are designated by the same reference numerals, whereby a repeated description of these elements is omitted in individual cases. The figures only schematically illustrate the subject matter of the invention.

[0027] Figure 1shows a schematic representation of a method for producing a component 20 from a steel with a nitrogen-containing protective layer 22 in the form of a flow chart.

[0028] In a starting step 100, a component 20 made of steel is provided. In addition to iron, the steel contains several components, for example, 0.5 wt% carbon and 15 wt% chromium. Component 20 is tubular, for example, with a circular cross-section and enclosing an internal cavity.

[0029] In a subsequent step 101, the component 20 is heated in a nitrogen-containing atmosphere to a temperature between 900 °C and 1300 °C. Annealing is carried out for a period of between one minute and twelve hours. The nitrogen-containing atmosphere used during annealing maintains a nitrogen partial pressure between 50 mbar and 5 bar.

[0030] Annealing and the diffusion of nitrogen from the nitrogen-containing atmosphere into component 20 creates or stabilizes an austenitic surface layer of the steel. This surface layer surrounds component 20. The austenitic surface layer of component 20 now includes a nitrogen-containing diffusion zone, which forms the nitrogen-containing protective layer 22 of component 20.

[0031] In a subsequent step 102, the component 20 is quenched. The component 20 is cooled from the temperature obtained during annealing to a temperature of less than 50°C in a relatively short time. The component 20 is quenched at a quenching pressure between 1.5 bar and 10 bar. The component is quenched using a quenching medium. In this case, the quenching medium is a gas selected from the group consisting of nitrogen, argon, or helium.

[0032] Annealing and quenching harden the component 20. The nitrogen previously diffused into the austenitic surface layer remains in said surface layer. The protective layer 22 of the component 20 is thus preserved after quenching.

[0033] In a subsequent step 103, the component 20 is deep-frozen in a temperature range between -70 °C and -273 °C. The deep-freezing of the component 20 is carried out over a period of between 15 minutes and 30 minutes.

[0034] In a subsequent step 104, the component 20 is tempered in a temperature range between 150 °C and 600 °C. The tempering of the component 20, like the annealing, is also carried out in a nitrogen-containing atmosphere.

[0035] In an optional step 105, further processing of the component 20 can take place. For example, the component 20 can be deformed or machined by milling or turning in order to thereby bring it into a shape required for a later application.

[0036] Figure 2 shows a schematic representation of a cross section through a tubular component 20, which is provided with the Figure 1 The tubular component 20 is, as already mentioned, made of steel.

[0037] The component 20 is tubular, has a circular cross-section, and surrounds an internal cavity. The component 20 comprises a core material 25 made of steel. The core material 25 is formed by the Figure 1 The procedures described have changed only insignificantly.

[0038] The component 20 further comprises two protective layers 22, which are formed by the Figure 1The two protective layers 22 are each formed on the surface of the component 20. The two protective layers 22 particularly reduce the diffusion of hydrogen into the component 20.

[0039] The core material 25 and the two protective layers 22 are each formed in the shape of a circular ring. The two protective layers 22 concentrically surround the core material 25. One of the protective layers 22 faces radially toward an internal cavity. The other of the protective layers 22 faces radially outward.

[0040] The component 20 can be used, for example, as a pipeline for transporting hydrogen, in particular for use in a fuel cell system 70. The hydrogen required by the fuel cell system 70 flows through the internal cavity in the component 20 along the inner protective layer 22.

[0041] In the present application of component 20 as a pipeline in a fuel cell system 70, the outer protective layer 22 serves no significant function. The outer protective layer 22 can simply remain on the component 20. However, the outer protective layer 22 can also be completely or partially removed from the component 20 by turning or milling.

[0042] Figure 3 shows a schematic representation of a fuel cell system 70. The fuel cell system 70 comprises a fuel cell unit 75, which has a plurality of fuel cells not explicitly shown here. The fuel cell unit 75 has an anode 73 and a cathode 74. The individual fuel cells each have negative electrodes, which together form the anode 73 of the fuel cell unit 75. The individual fuel cells each have positive electrodes, which together form the cathode 74 of the fuel cell unit 75.

[0043] The fuel cell unit 75 has a negative terminal 71, which is electrically connected to the anode 73. The fuel cell unit 75 also has a positive terminal 72, which is electrically connected to the cathode 74. An electrical voltage is present between the negative terminal 71 and the positive terminal 72 of the fuel cell unit 75 during operation of the fuel cell system 70. The negative terminal 71 and the positive terminal 72 of the fuel cell unit 75 are connected, for example, to an on-board electrical system (not shown here) of a motor vehicle, in particular an electric vehicle.

[0044] The fuel cell system 70 comprises a first supply line 56 for supplying a fuel, in particular hydrogen, to the anode 73. For this purpose, the first supply line 56 is connected to a compressed gas reservoir 36 in which hydrogen is stored at a pressure of, for example, 350 bar to 700 bar. During operation of the fuel cell system 70, hydrogen flows in a first flow direction 51 from the compressed gas reservoir 36 to the anode 73 of the fuel cell unit 75. The fuel cell system 70 also comprises a first discharge line 57 for discharging excess fuel, in particular hydrogen, from the anode 73 of the fuel cell unit 75.

[0045] The first supply line 56 for supplying hydrogen and the first discharge line 57 for discharging hydrogen are each made of a component 20, or of several components 20 connected to one another, as in Figure 2 represented, formed.

[0046] The fuel cell system 70 further comprises a second supply line 66 for supplying an oxidizing agent, in particular air with oxygen, to the cathode 74. For this purpose, the second supply line 66 is connected, for example, to a compressor (not shown here). The compressor supplies compressed air in a second flow direction 61 to the cathode 74 of the fuel cell unit 75. The fuel cell system 70 also comprises a second discharge line 67 for discharging excess oxidizing agent from the cathode 74. The second discharge line 67 also serves to discharge product water produced by the electrochemical reaction in the fuel cells of the fuel cell unit 75.

[0047] The invention is not limited to the embodiments described here and the aspects highlighted therein. Rather, numerous modifications are possible within the scope of the appended claims.

Claims

1. Process for producing a fuel cell system (70), comprising a component (20) made of a steel having a nitrogen-containing protective layer (22), comprising the following steps: - annealing the component (20) in a nitrogen-containing atmosphere at a temperature between 900°C and 1300°C; - quenching the component (20); - freezing the component (20) at a temperature of less than -70°C; - tempering the component (20) at a temperature of more than 150°C; - annealing the component (20) for between one minute and twelve hours at a partial nitrogen pressure between 50 mbar and 5 bar, - quenching the component (20) at a quench pressure between 1 bar and 40 bar, where the quenching of the component (20) is conducted with a quench medium selected from a group of nitrogen, argon and helium, - quenching the component (20) to a temperature of less than 50°C, - freezing the component (20) over a period between 15 minutes and 30 minutes, - tempering the component (20) in a nitrogen-containing atmosphere.

2. Process according to Claim 1, wherein the steel of the component (20) contains between 10% by weight and 20% by weight of chromium.