METHOD FOR PRODUCE A VENEERED SHEET
Patent Information
- Application Number
- DE502020009480
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-01-24
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2040-01-24
AI Technical Summary
Existing veneered panels have complex structures and limited improvements in veneer properties due to the conventional use of binders, which restricts their economic and functional potential.
A method using polyurethane prepolymers as binders, which penetrate and chemically crosslink with the veneer and carrier board, enhancing mechanical properties and waterproofing, while allowing for the addition of additives to adjust specific properties, such as flame retardancy or UV stability, and are processed at elevated temperatures to create a robust and versatile veneered panel.
The method simplifies the production of veneered panels, improves mechanical performance, and expands application possibilities by creating a waterproof and durable surface with enhanced properties, such as increased compressive strength and light stability, while maintaining economic efficiency.
Description
[0001] The invention relates to a method for producing a veneered panel and a veneered panel.
[0002] Veneered panels convey the impression of a real wood surface, but are very economical due to the economical use of thin veneer layers in combination with a carrier board. A typical veneered panel, in which the veneer is fixed to the carrier board using a binder-impregnated paper, is presented in EP 2 902 196 A1 and DE 103 00 347 B4. DE 10 2011 085 996 A1, IT 2018 0000 3227 A1, DE 10 2012 2017 780 A1, US 2017 / 190156 A1, and the utility model DE 20 2013 012 020 U1 also show comparable panels.
[0003] The disadvantage of such a known veneered panel is that the structure of the veneered panel is complex and that the properties of the veneer can only be improved to a very limited extent.
[0004] It is therefore an object of the invention to provide a method for producing a simply constructed, veneered panel which also makes it possible to improve the properties of the veneer in a simple manner.
[0005] This object is achieved by a method according to claim 1.
[0006] The polyurethane prepolymer (PU prepolymer) used as a binder has proven advantageous for fixing veneer to a carrier board. As a prepolymer made from isocyanates, it is easier to process than isocyanate monomers. PU prepolymers are usually made from two diisocyanates and a diol or glycol. This produces a prepolymer with two isocyanate groups. Aliphatic (e.g., isophorone diisocyanate, 1,6-hexamethylene diisocyanate, 1,4-cyclohexyl diisocyanate, dicyclohexyl 4,4'-diisocyanate, etc.) or aromatic (tolylene diisocyanate) diisocyanates can be used to produce the prepolymers. The diols or glycols used are 1,3-propanediol or low-molecular-weight polyethylene glycols. Although it is a prepolymer, the PU prepolymer is capable of bonding the veneer if necessary.to penetrate evenly and completely during pressing, so that the veneer can be well bonded to a carrier board with the binder PU prepolymer. The PU prepolymer cures essentially thermally, i.e. at elevated temperatures of, for example, 100 °C to 240 °C; it is therefore a post-crosslinking polymer. During pressing, the prepolymer penetrates the veneer, and possibly also the carrier board or its surface. The binder therefore not only hardens, but is also mechanically anchored between the veneer and the carrier board during pressing. A particular advantage here is that isocyanates can react with all molecules containing OH groups (e.g.: water, cellulose, hemicellulose, lignin). This means that the prepolymer chemically crosslinks with the wood matrix of the veneer and the carrier material. A polyurethane can therefore be detected as the binder on the finished veneered board.This binder proves to be water-resistant, so that a veneered panel produced with a PU prepolymer has wider application possibilities than a veneered panel produced with a non-water-resistant binder. Furthermore, the binder according to the invention strengthens the veneer, thus improving its mechanical performance properties, particularly its compressive strength. The PU prepolymer is transparent but can also be colored. Where the binder near the surface of the veneer may be exposed to light, the use of aliphatic PU prepolymers is recommended. These do not react or react only slightly when exposed to light, i.e., they remain transparent and do not discolor or yellow. Where light stability or lightfastness is not important, aromatic PU prepolymers can also be used, which react more strongly under the influence of light and tend to discolor.
[0007] Any board that is flat on at least one side and forms a strong bond with the PU prepolymer or with the polyurethane as a cured binder can be used as the carrier board. Wood-based panels are preferred, e.g. medium-density or high-density fiberboard (MDF, HDF), particleboard, OSB (oriented strand board), solid wood panels, plywood and block or strip panels, but also cement-bonded particle or fiberboard, and also bio-composite panels, panels with a high binder content, in particular panels with a binder content of more than 50 wt.% based on the total weight of the panel, panels that contain a mixture of different fibers, e.g. natural fibers and bicomponent fibers. The carrier board has a top side to which the veneer is applied, and a bottom side to which a counterlayer is optionally applied.
[0008] Real wood layers with a thickness of up to 10 mm, but preferably between 0.2 mm and 5 mm, in particular between 0.5 mm and 3 mm, are used as veneer. The veneer can be produced in one piece from a log by slicing or peeling. However, it can also be composed of individual sections that are joined together, for example, by a binding agent or a glue thread. It generally has a moisture content of a maximum of 20 wt.%, preferably a maximum of 12 wt.%, in particular a maximum of 8 wt.%. The veneer preferably has the dimensions of the carrier board. The veneer has an underside facing the carrier board and an upper side facing away from the carrier board.
[0009] The use of an additive enables the targeted adjustment of the properties of the veneered carrier board. The additive is applied between the veneer and the binder, whereby the additive is introduced into the veneer by the binder during pressing. This procedure has proven particularly suitable for achieving the desired effect with economical use of the additive. The additive can be applied to the surface of the binder facing the veneer; alternatively, the additive can be applied to the veneer surface facing the binder, usually the underside of the veneer. Various substances or compounds can be applied to the binder as additives, individually, in mixtures, or one after the other. Suitable additives according to the invention are: flame retardants, such as, for example,Ammonium phosphates or water glass, a UV stabilizer, an infrared absorber, conductivity enhancers, antibacterial agents, antifungal agents, antialgaecide agents, hydrophobic agents, bleaching agents, or mordants. Depending on the required or desired properties, any other additives can also be considered. The additive can be in solid form, preferably in particulate form, e.g., as dust or powder, but also as granules. Alternatively, a liquid or pasty additive can be used. However, the additive can also be soluble in the binder; in this case, the additive may not be fully transported to the surface. This depends on the dosage of the additive.
[0010] According to a further development of the invention, the additive is not soluble in the binder or is not homogeneously soluble in the binder. This ensures that the additive does not mix with the binder and thereby lose its effectiveness, but rather remains on the surface of the binder and thus comes into contact with the veneer as completely as possible.
[0011] In a simple embodiment of the invention, the binder is applied to the underside of the veneer or the top side of the carrier board, as explained in more detail below. According to a preferred alternative, the additive is first applied to the underside of the veneer. Advantageously, the underside of the veneer faces upward during application of the additive, so that the additive lies on the underside of the veneer. After applying the additive or applying a mixture of additives or applying several additives sequentially, the additive can optionally be fixed, e.g., by drying or heating. For example, a liquid additive, e.g., ink, can be dried.It has been shown that despite the fixing of the additive, the additive is transported through the veneer by the PU prepolymer during the pressing process, when the binder is more liquefied before curing and penetrates the veneer at least in sections, so that, for example, an aesthetic effect is reliably achieved with little use of additive.
[0012] A binder is then applied to the veneer. The binder is preferably applied in liquid form, e.g. sprayed or poured on. Typical application quantities range from 40 g / m 2 to 400 g / m 2 , preferably between 60 g / m 2 and 250 g / m 2 , in particular between 80 g / m 2 and 200 g / m 2 . If the intention is simply to bond the veneer to the carrier board, an application quantity of up to 100 g / m 2 is generally sufficient, depending on the type and thickness of the veneer. If penetration of the veneer is also desired, an application quantity of 80 g / m 2 to 400 g / m 2 is required, depending on the type and thickness of the veneer. The binder has a high solids content, usually over 80 wt.%, preferably over 90 wt.%, based on the total weight of the prepolymer. The prepolymer applied as a binder can therefore hardly release any liquid; it usually cannot be dried but remains liquid on the surface of the veneer or the carrier board.
[0013] After the binder or additive has been applied, the veneer or core board is preferably processed directly. Once the binder has been applied to the top side of the core board, the underside of the veneer is placed on the top side of the core board, which has already been coated with binder, for further processing. The pressed product stack is thus formed as follows: the binder lies on the top side of the core board, the additive optionally lies on top of the binder, and the veneer is placed on top of this as the outer layer. Alternatively, the veneer, which has a binder and optionally one or more additives on its underside, is placed on the top side of the core board. The core board, binder, optionally the additive, and the veneer are thus layered to form a pressed product stack.
[0014] Optionally, a countersheet can be arranged on the underside of the carrier board. The countersheet is intended to compensate for the tensile forces triggered by the veneer on the upper side of the carrier board. The countersheet is usually a binder-impregnated paper or cardboard, but it could also be a veneer or another flat layer that is flatly bonded to the underside of the carrier board. Paper or cardboard can also be glued to the underside of the carrier board using the binder. Preferably, a countersheet is used that is comparable or similar to the coating on the upper side of the carrier board. Advantageously, a veneer is used that is coated with the binder and also with an additive. The pressed material stack described above is pressed into a veneered board.
[0015] In the press, the PU prepolymer is cured under the influence of elevated temperature, i.e. the viscosity of the binder is further reduced upon heating. The PU prepolymer chemically cures during pressing to form a polyurethane and solidifies upon cooling. The pressing pressure causes the binder, as long as it is not yet cured, to penetrate into the veneer and preferably also into the surface of the carrier board. This lays the foundation for good mechanical anchoring of the binder, which ensures that any restoring forces present in the veneer are dissipated or can be absorbed by the binder before the press is opened. The pressing time is typically between 20 and 60 seconds. The pressing temperature is usually between 100 °C and 240 °C, preferably between 160 °C and 200 °C. The pressing pressure is between 25 N / mm 2 and 50 N / mm 2 .During the pressing process, the liquid binder penetrates the veneer. Unlike the denser surface of the core board, the veneer contains cavities, both cracks and gaps caused by manufacturing processes and typical wood cavities, such as those caused by cut veins. The binder, which easily penetrates the veneer, firmly bonds the veneer to the core board. At least partial penetration of the binder into the surface of the core board supports the bond between the veneer and core board.
[0016] Because the PU prepolymer penetrates the veneer at least partially, and preferably completely, a veneered panel with a water-resistant surface is created, as the binder is water-resistant when cured. The veneer, like all wood surfaces, is not water-resistant; it is impregnated by the PU prepolymer or the polyurethane formed during pressing, which makes the veneered surface water-resistant.
[0017] This description clearly shows that the veneered panel is manufactured from just two components: the veneer coated with a binder and optionally an additive, and the core board, or a core board coated with the binder and optionally an additive, and a veneer. This makes the pressed material stack particularly easy to manufacture. With two layers, a core board and a veneer, each of which is coated with a binder and optionally an additive, there is no risk of the layers slipping or shifting against each other, thus resulting in less waste during production. Nevertheless, all of the veneer's performance properties can be adjusted as required, meaning the veneered panel can be supplied with a wide range of properties.The additive, which is optionally placed on the binder in the stack of pressed material, is conveyed through the veneer during the pressing process essentially without mixing with the binder and can thus exert its effect directly where it is needed without major losses.
[0018] Furthermore, a veneered panel is described, comprising a carrier plate and a veneer arranged above the carrier plate, wherein the veneer is impregnated with a binder at least in sections, and wherein an additive selected from the group consisting of flame retardants, UV stabilizers, infrared absorbers, antibacterial agents, antifungal agents, antialgaecides, hydrophobic agents, bleaching agents, and stains is optionally present on the upper side of the binder in the veneer. The additive, which improves the performance properties of the veneer, is predominantly present in the veneer. The binder, in this case polyurethane, is essentially free of additives.
[0019] According to a further embodiment, the veneered panel has a countersheet on the underside of the carrier board. The countersheet can be a binder-impregnated paper or a binder-impregnated cardboard or paperboard, but is preferably also designed as a veneer. The paper or cardboard can also be glued to the underside of the carrier board by the binder. The countersheet is pressed with the carrier board as part of the pressed material stack and ensures that the veneered panel does not warp because approximately equal forces now act on both sides of the carrier board. If a veneer is used as a countersheet, it can be provided with a binder and optionally with an additive in the same way as described above for the veneer on the top side of the carrier board.
[0020] Any board with a flat surface can be used as the carrier board. The carrier board is preferably a wood-based panel or a biocomposite board, as described above.
[0021] Details of the invention are explained in more detail using exemplary embodiments. They show: Fig. 1a schematic representation of a stack of pressed material provided with the binder. The components of the veneered panel are a carrier plate 1 with a top side 2 and a bottom side 3. Furthermore, the veneered panel includes a veneer 4 with a bottom side 5 and a top side 6. Before layering a stack of pressed material, the carrier plate 1 or the veneer 4 is prepared. This is done either by arranging the veneer with the bottom side 5 facing upwards. Optionally, an additive 7 is first applied to the bottom side of the veneer 4. Alternatively, a mixture of additives can be applied or several additives can be applied in sequence. Once the additive(s) 7 have been applied, a layer of binder 8 is applied. A PU prepolymer is used as the binder here. The binder 8 is used in liquid form. The binder 8 is applied in liquid form using a roller or a casting machine.Alternatively, the binder according to the invention is applied to the upper side 2 of the carrier plate 1.
[0022] The further production of a veneered panel takes place in that the veneer 4 is placed with its underside 5 on the top side 2 of a carrier plate, preferably without intermediate drying, whereby a stack of pressed material is layered, in which the binding agent 8 according to the invention is arranged between the carrier plate 1 and veneer 4. The stack of pressed material is pressed in a press to form a veneered panel. Optionally, the stack of pressed material is supplemented by a counter-layer, which is applied to the underside 3 of the carrier plate 1 and which then forms the underside of the veneered panel 1. According to an advantageous embodiment, the counter-layer is designed in the same way as the veneer 4 on the top side of the carrier plate. In principle, however, any coating on the underside of the carrier plate is suitable as a counter-layer that at least partially absorbs the forces exerted by the veneer 4 arranged on the top side 2 of the carrier plate 1. Example 1
[0023] Raw materials: Veneer: Strength: 0.8 mm Type: oak This veneer is inserted on the top side 2 of the carrier plate 1. Binder: aliphatic PU prepolymer in liquid form This binder is inserted between the top surface 2 of the core board 1 and the oak veneer. It is exposed to light after the veneered core board is manufactured. Carrier plate: Strength: 10 mm Type: HDF (high-density fiberboard) Binder: aromatic PU prepolymer 678.05 (manufacturer: Jowat) in liquid form This binding agent is inserted between the underside 3 of the carrier plate 1 and the birch veneer used as a counter-layer. Veneer: Strength: 1.05 mm Type: birch This veneer is inserted on the underside 3 of the carrier plate 1. Production of the veneered base plate:
[0024] 100g / m² of PU prepolymer with the product name 678.05 from Jowat is applied to the carrier board, here an HDF board (high-density fiberboard) measuring 2800 x 2070 x 10 mm (length x width x thickness). This PU prepolymer is based on aromatic isocyanates and alcohol, which were reacted to form a prepolymer. The PU prepolymer is liquid. The solids content is approximately 90% by weight based on the total weight of the PU prepolymer. The viscosity is approximately 65 mPas (20°C, Brookfield). The PU prepolymer is applied using a casting machine.
[0025] The PU prepolymer is then applied to the birch veneer. The birch veneer, which is to be fixed to the underside 3 of the carrier board 1, is placed under the underside 3 of the carrier board, which has been coated with a binder, and thus layered to form a stack of pressed material. The stack of pressed material is pressed in a short-cycle press (KT press). The pressing conditions of the KT press are set as follows: pressing temperature 180°C, pressure 40 kg / cm², and pressing time 60 seconds. The pressing temperature ensures the curing of the binder during the pressing time, and the pressing pressure compresses the veneer while simultaneously penetrating the PU prepolymer.
[0026] The short-cycle press is then opened, and the single-sided coated HDF board cools. The core board 1, coated on one side on the underside 3, is rotated, and 200 g / m² of aliphatic isocyanate-based prepolymer is applied to the top side 2 of the core board 1. The oak veneer is then placed on top, and this stack of pressed material is pressed using the parameters mentioned above. Here, too, the binder hardens under thermal influence, penetrates the binder, and compresses the veneer under the influence of pressure. The board, now veneered on both sides, is cooled. Floorboards with a glueless profile are then milled from the core board 1, which is veneered on both sides. The oak veneer side serves as the usable surface.To apply the oak veneer to the light-exposed surface, an aliphatic PU prepolymer was applied that does not or hardly reacts under the influence of light, in particular it does not change its color or yellow.
[0027] By pressing the veneered core board under high pressure, as described above, the veneer is compressed, while the binding agent simultaneously penetrates the veneer. This creates a veneered core board with a particularly mechanically resilient veneer surface, particularly one with increased compressive strength. Furthermore, the polyurethane created during the pressing process is a waterproof binding agent, so even the inherently non-waterproof veneer is rendered waterproof by the binding agent that has penetrated at least partially into it. Example 2
[0028] Raw materials: Veneer: Strength: 0.8 mm Type: oak This veneer is inserted on the top side 2 of the carrier plate 1. Binder: aliphatic PU prepolymer in liquid form This binder is inserted between the top surface 2 of the core board 1 and the oak veneer. It is exposed to light after the veneered core board is manufactured. Carrier plate: Strength: 10 mm Type: HDF (high-density fiberboard) Countermove: Melamine resin-impregnated paper Production of the veneered base plate:
[0029] A 200g / m² liquid PU prepolymer based on aliphatic isocyanates is sprayed onto the carrier board 1, here an HDF board (format: 2800 x 2070 x 10 mm). Optionally, an additive, e.g., a dye, is applied. The oak veneer is then applied to the polymer with the optionally applied additive. A melamine resin-impregnated paper is placed on the reverse side as a backing. The melamine resin-impregnated paper has a paper weight of 80g / m² and a resin application rate of 120% by weight based on the paper weight. The pressed material stack consisting of the backing on the underside 3 of the carrier board 1, the carrier board 1, and the veneer 4 on the top side 2 of the carrier board 1 is pressed in a short-cycle press. The pressing temperature is 180 °C, the pressing pressure is set to 30 kg / cm², and the pressing time is 60 seconds. The veneered carrier board 1 is then allowed to cool.During the pressing process, the prepolymer is pressed into the veneer and often also into the surface of the core board, mechanically anchoring the curing prepolymer. At the same time, the pressing pressure compresses the veneer, thereby densifying it. Furthermore, restoring forces in the veneer are reduced or eliminated.
[0030] After the prepolymer has cured and cooled, floorboards with a glueless profile are milled from it. The oak veneer side serves as the usable surface. The increased use of binder ensures that the veneer is permeated by the binder, making it completely waterproof. The backing can be advantageously pressed with the core board in a single pressing process, because melamine also hardens under the conditions chosen for pressing. In contrast to Example 1, one pressing process is eliminated here.
[0031] Of course, an additive or a mixture of additives can also be added to the prepolymer to create specific properties in the product. These can be, for example, dyes, conductivity-enhancing agents, etc. However, according to a preferred embodiment, the additive can also be applied between veneer 4 and binder 8, allowing the additive to act close to the surface, since additives are usually used to create surface effects.
[0032] The veneered core board according to the invention can be used in all applications where veneered surfaces have previously been used. Furthermore, the boards with the veneer surfaces can, of course, also be used for the production of wall or ceiling paneling in addition to the production of floor panels. They can also be used in the manufacture of furniture. Example 3
[0033] Raw materials: Veneer: Strength: 0.8 mm Type: oak This veneer is inserted on the top side 2 of the carrier plate 1. Binder: aliphatic PU prepolymer This binder is inserted between the top surface 2 of the core board 1 and the oak veneer. It is exposed to light after the veneered core board is manufactured. Carrier plate: Strength: 10 mm Type: Fiberboard comprising 48% by weight of wood fibers and 52% by weight of melamine resin, each based on the total weight of the board. Binder: aromatic PU prepolymer 678.05 Jowat The binding agent is applied between the underside 3 of the carrier plate and the birch veneer used as a counter-layer. Veneer: Strength: 1.05 mm Type: birch Production of the veneered base plate:
[0034] The carrier plate (1) according to embodiment 3 is veneered in the same way as the veneered carrier plate according to embodiment 1.
[0035] Since the carrier plate (1) used in the embodiment 3 and also the binder are waterproof, a waterproof, veneered carrier plate 1 is provided.
Claims
1. A method for producing a veneered board, which comprises a veneer (4) having an upper face (6) and a lower face (5) and a carrier board (1) having an upper face (2) and a lower face (3), comprising the steps of: - providing a veneer (4), - applying an additive (7) between binder (8) and veneer (4), then applying a binder (8) onto the upper face (2) of the carrier board (1) or the lower face (5) of the veneer (4), wherein a PU prepolymer is used as the binder, - producing a stack of materials to be pressed comprising the carrier board (1) and the veneer (4) with the binder (8) arranged between the carrier board (1) and the veneer (4) and with the additive (7) arranged between the binder (8) and the veneer (4), - pressing the stack of materials to be pressed in order to form a veneered board wherein one of the following substances is used as an additive (7), either individually or in a mixture: flame retardant, UV stabilizer, infrared absorber, agent for increasing conductivity, antibacterial agent, antifungal agent, an-tialgal agent, hydrophobizing agent, bleaching agent, stain.
2. The method according to claim 1, characterized in that an aliphatic and / or aromatic PU prepolymer is used as the binder (8).
3. The method according to one of the preceding claims, characterized in that the additive (7) is applied as a particulate solid or in liquid form.
4. The method according to one of the preceding claims, characterized in that the additive (7) is not soluble in the binder (8) or is not homogeneously soluble in the binder (8).
5. The method according to one of the preceding claims, characterized in that the binder (8) is applied as a liquid.
6. The method according to one of the preceding claims, characterized in that the pressing temperature is between 100°C and 240 °C.
7. The method according to one of the preceding claims, characterized in that the pressing time is between 20 seconds and 60 seconds.
8. The method according to one of the preceding claims, characterized in that the pressing pressure is between 25 N / mm2 and 50 N / mm2.