METHOD FOR THE PREPARATION OF NON-CYCLICAL ALKOXY FUNCTIONAL POLYSILOXANES

DE502020009483D1Active Publication Date: 2024-10-31EVONIK OPERATIONS GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502020009483
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-05-28
Filing Date
2020-05-14
Publication Date
2024-10-31
Estimated Expiration
2040-05-14

AI Technical Summary

Technical Problem

The existing processes for producing SiOC-based polyether siloxanes, such as defoamers, face challenges with corrosive and toxic chlorosiloxanes, require stoichiometric excess of polyetherols leading to unreacted excess polyethers, and generate ecological and toxicological issues, along with the need for corrosive catalysts and salt formation.

Method used

A process involving the heating of a reaction system comprising cyclic polyorganosiloxanes, silanes, and a catalyst system of metal trifluoromethanesulfonate and Brönsted acids like methanesulfonic acid, which avoids the use of corrosive and heavy metal catalysts, achieving acid-catalyzed ring opening to produce non-cyclic alkoxy-functional polysiloxanes.

Benefits of technology

This process effectively produces non-cyclic alkoxy-functional polysiloxanes without corrosive catalysts, reduces ecological and toxicological concerns, and minimizes unreacted polyethers, enhancing the stability and effectiveness of SiOC-based polyether siloxanes for applications like defoamers and polyurethane foam stabilizers.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a process for producing a reaction product containing a non-cyclic alkoxy functional polysiloxane, and its use for the production of SiOC-based silicon compounds, in particular for the production of SiOC-based polyethersiloxanes.

[0002] SiOC-based polyethersiloxanes are well-known components of defoamers that exhibit exceptional efficacy and stability in defoaming aqueous and non-aqueous media. These properties include foam inhibition, defoaming, excellent long-term stability, and outstanding compatibility in both aqueous and non-aqueous media. All of these characteristics are of great importance for modern coating applications.

[0003] In this context, the term defoamer encompasses both products and formulations that prevent foaming, as well as those that break down foam and facilitate deaeration. In practice, the boundaries between these products are fluid, which is why the collective term defoamer is used here.

[0004] In many technical processes, especially when working in aqueous media, it is necessary to suppress or completely prevent the unwanted formation of foam during manufacturing or processing, since foam or foam crowns that accumulate during stirring and dispersing processes or in the containers during the filling process can extend production times, reduce the effective volume of the system, or even prevent its correct operation (overflow, lack of color transfer).

[0005] This can be achieved by adding defoamers that, even at very low concentrations from approximately 0.001 wt%, are able to prevent or destroy unwanted foams and simultaneously do not cause any surface defects after application. In practice, this latter factor must be considered at least as much as effective defoaming.

[0006] Surface defects are undesirable properties for the user, such as pinholes, craters, loss of gloss, orange peel effect, wrinkling, and loss of adhesion in the coating system. However, the long-term stability of the formulations is also crucial for the user, as products like paints are often not used immediately but only after extended storage. Under extreme climatic conditions (heat and sunlight), the effectiveness of a defoaming formulation can sometimes collapse after only a short time.

[0007] DE 24 13 987 A1 discloses the use of non-cyclic alkoxy functional siloxanes for the production of polyether siloxanes, in particular for the production of polyurethane foam stabilizers.

[0008] To produce the economically important class of SiOC-based polyethersiloxanes, also known as silicone polyethers or siloxane-polyether copolymers, several process variants are used according to the current state of the art.

[0009] Experts know that these SiOC-linked polyethersiloxanes are a class of products that do not tend to resinify. Even though SiOC-linked polyethersiloxanes contain reactive groups, such as hydroxyl groups, they are not used for targeted crosslinking. They are not film-forming, unlike silicone resins.

[0010] Traditionally, SiOC linkages are formed by the reaction of a siloxane with a leaving group (e.g., a halogen) bonded to the silicon atom and an alcohol or polyetherol. The latter is usually obtained beforehand by alkoxylation of monohydroxy functional starting compounds such as butanol with alkylene oxides. Chlorosilicones are particularly common as starting materials for this type of reaction. However, chlorosiloxanes are difficult to handle due to their high reactivity. Their use is further hampered by the disadvantage that the hydrogen chloride formed during the reaction restricts handling to corrosion-resistant equipment and leads to environmental problems. Moreover, in the presence of chlorosiloxanes and alcohols or polyetherols, organochlorine compounds can be formed, which are undesirable for toxicological reasons.Furthermore, achieving quantitative conversion in the reaction of a chlorosiloxane with an alcohol or polyetherol is not straightforward, so the OH-functional component often has to be used in a stoichiometric excess relative to the SiCl functionalities of the siloxane component. In practice, the use of a polyether excess means that the resulting silicone polyethers inevitably contain larger amounts of unreacted excess polyethers, which reduce the concentration of the surfactant-active silicone polyethers and impair the application properties of the target products. Frequently, bases must be used as HCl scavengers in the chlorosiloxane route to achieve good conversions. The use of these bases generates large amounts of salts, the removal of which poses difficulties on an industrial scale.

[0011] Cyclic siloxanes such as hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane and decamethylcyclopentasiloxane can be polymerized to linear, long-chain reactive siloxanes by catalysis with Lewis or Brønsted acids, as described, for example, in W. Noll, Chemie und Technologie der Silicone, Verlag Chemie GmbH, Weinheim, 1968.

[0012] Furthermore, it is known to use a reactive product such as a methoxy-terminated polydiorganosiloxane for the preparation of crosslinkable polyorganopolysiloxanes, which is prepared from hexamethylcyclotrisiloxane (D3) and 1,4,6-trimethyl-2,4,6-trivinylcyclotrisiloxane (V3) with tetramethoxysilane (TMOS) in the presence of trifluoromethanesulfonic acid. ("Cationic Telomerization of Hexamethylcyclotrisiloxane (O3) with Silanes Containing Alkoxy, Aryloxy and Acyloxy functions bound to Silicon", European Polymer Journal, Vol. 17, No. 4, 1981, pages 413-419).

[0013] EP 3 022 248 B1 discloses a process for producing a non-cyclic hydrocarbonoxyfunctional polyorganosiloxane by heating a composition of cyclic polyorganosiloxanes, a silane and a metal triflate, wherein the metal atom is selected from aluminium (Al), bismuth (Bi), iron (Fe), gallium (Ga), indium (In), scandium (Sc), samarium (Sm) and ytterbium (Yb).

[0014] Extensive investigations have shown that the success of the catalysis depends on a specific catalyst system. The object of the invention is therefore to provide a process for producing non-cyclic alkoxy-functional polysiloxanes without using catalysts that are corrosive to metals or contain heavy metals.

[0015] In this context, it was found in a completely surprising manner according to the invention that a process for producing a reaction product containing a non-cyclic alkoxy-functional polysiloxane by heating a reaction system comprising: (A) a cyclic polyorganosiloxane of the formula [(R 1< 2 SiO) 2 / 2 ] n , wherein the subscript n is an integer of at least 4 and each R 1< is an alkyl group or aryl group; (B) a silane of the formula R 2< (4-m) Si(OR 3< ) m , wherein the subscript m is an integer of 1 to 4, each R 2< is independently an alkyl group or aryl group, a hydrocarbyl group or a halogenated hydrocarbyl group and each R 3< is independently an alkyl group; and (C) a catalyst system comprising a metal trifluoromethanesulfonate of the formula [M] +< [CF 3 SO 3 ] -< , wherein M is a metal atom selected from sodium (Na) and potassium (K) and a Brønsted acid, where Brönsted acids with a pKa value ≤ 3.0, preferably with a pKa value ≤ 2.0, particularly preferably with a pKa value ≤ - 0.0 are used, the problem is excellently solved.

[0016] It was completely surprising that the acid-catalyzed ring opening of the cyclic polyorganosiloxane was made possible by the catalyst system according to the invention comprising a metal trifluoromethanesulfonate of the formula [M] +< [CF 3 SO 3 -< ], where M is a metal atom selected from sodium (Na) and potassium (K) and a Brønsted acid.

[0017] Trifluoromethanesulfonate salts, metal trifluoromethanesulfonates, triflates, metal triflates are used synonymously here.

[0018] Preferably, the molar ratio of Brønsted acid to metal trifluoromethanesulfonate used is in the range of 1:10 to 10:1, more preferably from 1:5 to 5:1, and most preferably from 1:2 to 2:1.

[0019] Preferred co-catalysts are Brønsted acids. Examples of suitable Brønsted acids include carboxylic acids, such as trifluoroacetic acid; sulfonic acids, such as methanesulfonic acid, p-toluenesulfonic acid, and dodecylbenzenesulfonic acid; and mineral acids, such as hydrochloric acid, nitric acid, sulfuric acid, and phosphoric acid.

[0020] The Brønsted acid particularly preferred according to the invention is a methanesulfonic acid, sulfuric acid, phosphoric acid, trifluoroacetic acid, or p-toluenesulfonic acid. The inventors have found that acid-catalyzed ring opening of the cyclic polyorganosiloxane is not successful with sodium triflates or potassium triflates alone, or with methanesulfonic acid alone, but is successful with a mixture of sodium triflates or potassium triflates and methanesulfonic acids. Thus, the advantage lies in the fact that corrosive catalysts such as aluminum triflates or iron triflates can be dispensed with. The use of heavy metal-containing catalysts such as gallium triflates, scandium triflates, or chromium triflates is another advantageous aspect of the invention.

[0021] Preferably, the silanes are dimethyldialkoxysilanes (such as diethoxydimethylsilane and dimethoxydimethylsilane), methyltrialkoxysilanes (such as triethoxymethylsilane and trimethoxymethylsilane) and tetraalkoxysilanes (tetraethoxysilane and tetramethoxysilane).

[0022] If cyclic polyorganosiloxanes are used in the context of the invention, in particular comprising D 4 (octamethylcyclotetrasiloxane), D 5 (decamethylcyclopentasiloxane) and / or D 6 (dodecamethylcyclohexasiloxane), wherein D 4 and / or D 5 are particularly preferred, and D 5 is most preferred, then a further preferred embodiment of the invention is present.

[0023] If, within the scope of the invention, cyclic polyorganosiloxanes, in particular cyclically branched siloxanes of the DT type, are used, preferably i. Mixtures of cyclic branched siloxanes of the D / T type, consisting (preferably exclusively) of siloxanes having D and T units and whose total fraction of the D and T units present in the siloxane matrix, having Si alkoxy and / or SiOH groups, as determined by 29< Si NMR spectroscopy, is ≤ 2 mol percent, preferably less than 1 mol percent, and which preferably contain at least 5 wt percent siloxane cycles, such preferably octamethylcyclotetrasiloxane (D 4 ), decamethylcyclopentasiloxane (D 5 ) and / or mixtures thereof, or ii. Mixtures of cyclic-branched siloxanes (preferably exclusively) containing D and T units, the total fraction of D and T units present in the siloxane matrix, which have Si alkoxy and / or SiOH groups and can be determined by 29< Si NMR spectroscopy, is greater than 2 and less than 10 mol percent. This represents another preferred embodiment of the invention.

[0024] According to a preferred embodiment of the invention, the heating takes place at a temperature of 40 °C to 180 °C, particularly preferably from 80 °C to 150 °C, for a time sufficient to form the non-cyclic alkoxy-functional siloxane.

[0025] Preferably, the components (A) and (B) are present in such quantities that the molar ratio of (A) / (B) is at least 1:1, preferably at least 2:1.

[0026] The process according to the invention is characterized in that the component (C) is preferably present in an amount of 0.1 mol% to 5 mol%, preferably 0.2 mol% to 1 mol% and particularly preferably 0.5 mol% to 1 mol% based on the combined weights of the components (A), (B) and (C).

[0027] From a process engineering and economic perspective, it is not preferred to add higher amounts of metal trifluoromethanesulfonates and Brønsted acids to the reaction system according to the invention, since these must also be removed again, if necessary, during further processing of the obtained alkoxy-functional siloxane.

[0028] In another preferred embodiment, no addition of water is required.

[0029] Another object of the invention is the use of alkoxy-functional siloxanes, produced using a reaction system as described above, for the production of polyether siloxanes, in particular for the production of polyurethane foam stabilizers, defoamers, especially diesel defoamers, aerators, wetting agents, paint, leveling and dispersing additives and / or dismulsifiers, hydrophobing agents.

[0030] It is also conceivable to use polyethersiloxanes produced in this manner, as described above, for the production of polymer dispersions; for the production of adhesives or sealants; for the surface treatment of fibers, particles, or sheet structures, in particular for the finishing or impregnation of textiles, for the production of paper towels, in the coating of fillers; for the production of cleaning and care formulations for household or industrial applications, in particular for the production of fabric softeners; for the production of cosmetic, pharmaceutical, and dermatological compositions, in particular cosmetic cleaning and care formulations, hair treatment products, and hair after-treatment products; for the cleaning and care of hard surfaces; as a process aid in the extrusion of thermoplastics; for the production of thermoplastic molded parts; and as an adjuvant in plant protection.to be used for the production of building material compositions. Examples

[0031] The following examples serve solely to illustrate this invention to those skilled in the art and do not constitute any limitation of the claimed subject matter. The determination of water content is generally carried out using the Karl Fischer method in accordance with DIN 51777, DGF E-III 10 and DGF C-III 13a. 29<Si NMR spectroscopy was used in all examples for reaction monitoring.

[0032] Within the scope of this invention, the 29< Si NMR samples are measured at a measurement frequency of 79.49 MHz in a Bruker Avance III spectrometer equipped with a 287430 probe head with a 10 mm slit width, dissolved in CDCl3 at 22°C and against tetramethylsilane (TMS) as an external standard [δ( 29< Si) ​​= 0.0 ppm].

[0033] The GPCs (gel permeation chromatography) are recorded using THF as the mobile phase on a column combination SDV 1000 / 10000A, length 65 cm, ID 0.80 at a temperature of 30°C on a SECcurity 2< GPC System 1260 (PSS Polymer Standards Service GmbH).

[0034] The gas chromatograms were recorded on an Agilent Technologies GC 7890B GC instrument equipped with an HP-1 column; 30m × 0.32mm ID × 0.25µm dF (Agilent Technologies No. 19091Z-413E) and hydrogen as the carrier gas with the following parameters: Detector: FID; 310°C Injector: Split; 290°C Mode: constant flow 2 mL / min Temperature program: 60°C with 8°C / min -150°C with 40°C / min - 300°C 10 min.

[0035] Unless otherwise stated, all figures are to be understood as weight percent. Examples: I. Inventive process for the production of a non-cyclic alkoxy-functional polysiloxane Example 1A.

[0036] In a 500 mL four-necked round-bottom flask equipped with a KPG stirrer, internal thermometer, and reflux condenser, 327.2 g (4.4 mol of D units) of a cycle mixture D4 / D5, available from Dow, are mixed with 72.8 g (0.5 mol) of diethoxydimethylsilane (Dynasylan 9811, Evonik) with stirring at 23°C. In a second step, 0.8 g of potassium triflate and 0.8 g of methanesulfonic acid are sequentially added to the reaction mixture. The mixture is then heated to 140°C and maintained at reaction temperature for 6 hours. After the reaction time, the mixture is cooled to 23°C. Upon cooling, a clear orange α-ω diethoxypolysiloxane is obtained.

[0037] This yields a clear terminal α-ω diethoxypolysiloxane, the target structure of which is confirmed by the accompanying 293Si NMR spectroscopy. The 293Si NMR spectroscopy also confirms that no SiOH groups are present within the limits of measurement accuracy. Example 1B.

[0038] In a 500 mL four-necked round-bottom flask equipped with a KPG stirrer, internal thermometer, and reflux condenser, 327.2 g (4.4 mol of D units) of a cycle mixture D4 / D5, available from Dow, are mixed with 72.8 g (0.5 mol) of diethoxydimethylsilane (Dynasylan 9811, Evonik) with stirring at 23°C. In a second step, 0.8 g of potassium triflate, 0.8 g of methanesulfonic acid, and 0.2 g of water are sequentially added to the reaction mixture. The mixture is then heated to 140°C and maintained at reaction temperature for 6 hours. After the reaction time, the mixture is cooled to 23°C. Upon cooling, a clear yellow α-ω diethoxypolysiloxane is obtained.

[0039] This yields a clear terminal α-ω diethoxypolysiloxane, the target structure of which is confirmed by the accompanying 293Si NMR spectroscopy. The 293Si NMR spectroscopy also confirms that no SiOH groups are present within the limits of measurement accuracy. Example 1C.

[0040] In a 500 mL four-necked round-bottom flask equipped with a KPG stirrer, internal thermometer, and reflux condenser, 327.2 g (4.4 mol of D units) of a cycle mixture D4 / D5, available from Dow, are mixed with 72.8 g (0.5 mol) of diethoxydimethylsilane (Dynasylan 9811, Evonik) with stirring at 23°C. In a second step, 0.8 g of sodium triflate and 0.8 g of methanesulfonic acid are sequentially added to the reaction mixture. The mixture is then heated to 140°C and maintained at reaction temperature for 6 hours. After the reaction time, the mixture is cooled to 23°C. Upon cooling, a clear, colorless α-ω diethoxypolysiloxane is obtained.

[0041] A clear terminal α-ω diethoxypolysiloxane is thus obtained, the target structure of which is confirmed by the accompanying 29<Si NMR spectroscopy. Likewise, the 29<Si NMR spectroscopy ensures that no SiOH groups are present within the limits of measurement accuracy. Fig. 1 )

[0042] Fig. 1 In the 29<Si NMR spectrum, the signal at -13 ppm can be attributed to the ethoxy groups. At -22 ppm, the polysiloxane chain is identified. Example 1.D.

[0043] In a 500 mL four-necked round-bottom flask equipped with a KPG stirrer, internal thermometer, and reflux condenser, 327.2 g (4.4 mol of D units) of a cycle mixture D4 / D5, available from Dow, are mixed with 72.8 g (0.5 mol) of diethoxydimethylsilane (Dynasylan 9811, Evonik) with stirring at 23°C. In a second step, 0.8 g of sodium triflate, 0.8 g of methanesulfonic acid, and 0.2 g of water are sequentially added to the reaction mixture. The mixture is then heated to 140°C and maintained at reaction temperature for 6 hours. After the reaction time, the mixture is cooled to 23°C. Upon cooling, a clear yellow α-ω diethoxypolysiloxane is obtained.

[0044] This yields a clear terminal α-ω diethoxypolysiloxane, the target structure of which is confirmed by the accompanying 293Si NMR spectroscopy. The 293Si NMR spectroscopy also confirms that no SiOH groups are present within the limits of measurement accuracy. II. Process for the preparation of a non-cyclic alkoxy-functional siloxane using Na triflates or K triflates Example 2A

[0045] In a 500 mL four-necked round-bottom flask equipped with a KPG stirrer, internal thermometer, and reflux condenser, 327.2 g (4.4 mol of D units) of a cycle mixture D4 / D5 available from Dow are mixed with 72.8 g (0.5 mol) of diethoxydimethylsilane (Dynasylan 9811, Evonik) while stirring at 23°C. In a second step, 0.8 g of potassium triflate is added to the reaction mixture. The mixture is then heated to 140°C and held at reaction temperature for 6 hours. After the reaction time, the mixture is cooled to 23°C. Upon cooling, a clear yellow mixture of D4 / D5 and diethoxydimethylsilane is obtained.

[0046] No terminal α-ω diethoxypolysiloxane is obtained, as evidenced by the accompanying 29< Si NMR spectroscopy. Example 2B

[0047] In a 500 mL four-necked round-bottom flask equipped with a KPG stirrer, internal thermometer, and reflux condenser, 327.2 g (4.4 mol of D units) of a cycle mixture D4 / D5 available from Dow are mixed with 72.8 g (0.5 mol) of diethoxydimethylsilane (Dynasylan 9811, Evonik) with stirring at 23°C. In a second step, 0.8 g of sodium triflate is added to the reaction mixture. The mixture is then heated to 140°C and held at reaction temperature for 6 hours. After the reaction time, the mixture is cooled to 23°C. Upon cooling, a clear yellow mixture of D4 / D5 and diethoxydimethylsilane is obtained.

[0048] No terminal α-ω diethoxypolysiloxane is obtained, as evidenced by the accompanying 29< Si NMR spectroscopy. III. Process for the production of a non-cyclic alkoxy-functional siloxane using MSS Example 3A

[0049] In a 500 mL four-necked round-bottom flask equipped with a KPG stirrer, internal thermometer, and reflux condenser, 327.2 g (4.4 mol of D units) of a cycle mixture D4 / D5, available from Dow, are mixed with 72.8 g (0.5 mol) of diethoxydimethylsilane (Dynasylan 9811, Evonik) with stirring at 23°C. In a second step, 0.8 g of methanesulfonic acid is added to the reaction mixture. The mixture is then heated to 140°C and held at reaction temperature for 6 hours. After the reaction time, the mixture is cooled to 23°C. Upon cooling, a clear yellow mixture of D4 / D5 and diethoxydimethylsilane is obtained.

[0050] No terminal α-ω diethoxypolysiloxane is obtained, as evidenced by the accompanying 29< Si NMR spectroscopy. Example 3B

[0051] In a 500 mL four-necked round-bottom flask equipped with a KPG stirrer, internal thermometer, and reflux condenser, 327.2 g (4.4 mol of D units) of a cycle mixture D4 / D5, available from Dow, are mixed with 72.8 g (0.5 mol) of diethoxydimethylsilane (Dynasylan 9811, Evonik) with stirring at 23°C. In a second step, 0.8 g of methanesulfonic acid and 0.2 g of water are sequentially added to the reaction mixture. The mixture is then heated to 140°C and maintained at reaction temperature for 6 hours. After the reaction time, the mixture is cooled to 23°C. Upon cooling, a clear yellow mixture of D4 / D5 and diethoxydimethylsilane is obtained.

[0052] No terminal α-ω diethoxypolysiloxane is obtained, as evidenced by the accompanying 29< Si NMR spectroscopy.

Claims

1. Process for producing a reaction product containing a non-cyclic alkoxy-functional polysiloxane by means of heating a reaction system comprising: (A) a cyclic polyorganosiloxane of the formula [(R12SiO)2 / 2]n, where the subscript n is an integer of at least 4 and each R1 is an alkyl group or aryl group; (B) a silane of the formula R2(4-m)Si(OR3)m, where the subscript m is an integer from 1 to 4, each R2 independently is an alkyl group or aryl group, a hydrocarbyl group or a halogenated hydrocarbyl group and each R3 independently is an alkyl group; and (C) a catalyst system comprising a metal trifluoromethanesulfonate of the formula [M]+[CF3SO3]-, where M is a metal atom selected from sodium (Na) and potassium (K), and a Bronsted acid, wherein Bronsted acids having a pKa ≤ 3.0, preferably having a pKa ≤ 2.0, particularly preferably having a pKa ≤ - 0.0 are used.

2. Process according to Claim 1, characterized in that the molar ratio of Bronsted acid used to metal trifluoromethanesulfonate in the range from 1:10 to 10:1, preferably from 1:5 to 5:1, particularly preferably from 1:2 to 2:1.

3. Process according to Claim 1 or 2, characterized in that the Bronsted acid is carboxylic acids such as for example trifluoroacetic acid, sulfonic acids such as for example methanesulfonic acid, p-toluenesulfonic acid and dodecylbenzenesulfonic acid, mineral acids such as for example hydrochloric acid, nitric acid, sulfuric acid and phosphoric acid.

4. Process according to any of the preceding claims, characterized in that the silanes are dimethyldialkoxysilanes selected from diethoxydimethylsilane and dimethoxydimethylsilane, methyltrialkoxysilanes selected from triethoxymethylsilane and trimethoxymethylsilane, and tetraalkoxysilanes selected from tetraethoxysilane and tetramethoxysilane.

5. Process according to any of the preceding claims, characterized in that the cyclic polyorganosiloxanes is selected from D4 (octamethylcyclotetrasiloxane), D5 (decamethylcyclopentasiloxane) and / or D6 (dodecamethylcyclohexasiloxane), where D4 and / or D5 are particularly preferred, and D5 is most preferred, are used.

6. Process according to any of the preceding claims, characterized in that the cyclic polyorganosiloxanes are cyclic branched polyorganosiloxanes of the DT type, preferably i) mixtures of cyclic branched siloxanes of the D / T type which consist of siloxanes having D and T units and whose cumulative proportion of D and T units present in the siloxane matrix and having Si-alkoxy and / or SiOH groups, determinable by 29Si NMR spectroscopy, is ≤ 2 mole per cent, preferably less than 1 mole per cent, and which preferably contain at least 5 per cent by weight of siloxane cycles, such as preferably octamethylcyclotetrasiloxane (D4), decamethylcyclopentasiloxane (D5) and / or mixtures of these or else ii) mixtures of cyclic branched siloxanes having D and T units whose cumulative proportion of D and T units present in the siloxane matrix and having Si-alkoxy and / or SiOH groups, determinable by 29Si NMR spectroscopy, is greater than 2 and less than 10 mole per cent.

7. Process according to any of the preceding claims, wherein the heating takes place at a temperature of 40°C to 180°C, particularly preferably of 80°C to 150°C, for a time which suffices for the formation of the non-cyclic alkoxy-functional siloxane.

8. Process according to any of the preceding claims, wherein the constituents (A) and (B) are present in amounts such that the molar ratio of (A) / (B) is at least 1:1, preferably at least 2:1.

9. Process according to any of the preceding claims, wherein the constituent (C) is present in an amount of 0.1 mol% to 5 mol%, preferably 0.2 mol% to 1 mol% and particularly preferably 0.5 mol% to 1 mol%, based on the combined weights of the constituents (A), (B) and (C).

10. Process according to any of the preceding claims, wherein the addition of water is not required.