METHOD FOR THE DEPOLYMERIZATION OF POLYSTYRENE IN THE PRESENCE OF FOREIGN POLYMERS

DE502020009750D1Active Publication Date: 2024-12-05INEOS STYROLUTION GRP GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502020009750
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-01-10
Filing Date
2020-09-17
Publication Date
2024-12-05
Estimated Expiration
2040-09-17

AI Technical Summary

Technical Problem

Current processes for depolymerizing polystyrene in the presence of foreign polymers face challenges in maximizing styrene monomer yield while minimizing the formation of styrene oligomers, which are necessary for high-quality polymerization processes due to the negative impact of foreign polymers on depolymerization conditions.

Method used

A process involving a polymer composition with 60-99.5% polystyrene, 0.1-30% polyolefin, and/or 0.1-4.9% acrylonitrile-based or polyester polymers, thermally split in a pyrolysis reactor at 450-1000°C with controlled residence time (0.01-10 seconds) to produce a product mixture, followed by cooling and separation of styrene monomers from other components.

Benefits of technology

This process achieves a high yield of styrene monomers with minimized oligomer formation, optimizing the purification process and ensuring high product quality for subsequent polymerization.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a process for producing styrene monomers by depolymerization (degradation) of polystyrene in the presence of foreign polymers, a device for carrying out the process, and the use of a device for depolymerization of polystyrene in the presence of foreign polymers.

[0002] Polystyrene is preferably selected from the group consisting of: standard polystyrene (GPPS), high-impact polystyrene (HIPS), and styrene-butadiene copolymers. High-impact polystyrene (HIPS) and / or standard polystyrene are particularly preferred. High-impact polystyrene (HIPS) and standard polystyrene, as well as their production, structure, and properties, are described in detail in the review literature (A. Echte, et al. in Angew. Chem. (Int. Ed. Engl.) 20, 344-361 (1981); and also in the Plastics Handbook, edited by R. Vieweg and G. Daumiller, Volume 4 "Polystyrene", Carl Hanser Verlag Munich (1996).

[0003] The transition from a linear to a circular economy is both ecologically and economically necessary in light of climate change, environmental pollution, population growth, and resource dependence. Intensive efforts were already undertaken in the 1980s and 1990s to develop processes for the raw material recycling of plastic waste, but large-scale applications have not yet been achieved due to unresolved process engineering problems and economic reasons. However, due to growing environmental awareness and an increasing demand for sustainable solutions, interest in chemical recycling is also growing.

[0004] Not all thermoplastic polymers are equally suitable for chemical recycling. The thermal decomposition of polyolefins or polyesters produces mixtures of waxes, light oil, and gases, among other substances. The degradation of polyethylene terephthalate (PET) leads to organic acids, primarily benzoic acid and terephthalic acid, which are corrosive and can also cause reactor clogging (G. Grause et al., Raw material recycling of polymeric waste material, in: Journal of Material Cycles and Waste Management, 13(4), 2011, 265-282). In the case of polystyrene and other styrene-containing polymers, it is possible to depolymerize these polymers into their basic components, particularly styrene monomers, making polystyrene and other styrene monomer-containing polymers an excellent choice for chemical recycling.

[0005] However, the resulting product mixture of a depolymerization process must be purified in order to use the components as raw material for new purposes, such as polymerization processes.

[0006] When polystyrene is sufficiently thermally treated, it decomposes into styrene monomers, but incomplete decomposition also leads to the formation of, for example, styrene dimers, trimers, and other oligomers. If the decomposition conditions are too harsh, byproducts such as benzene, toluene, ethylbenzene, cumene, and alpha-methylstyrene can be formed. The amounts of these reaction products vary and depend on the reaction conditions and the raw materials used (see C. Bouster et al., Study of the pyrolysis of polystyrenes: Kinetics of thermal decomposition, Journal of Analytical and Applied Pyrolysis, 1 (1980) 297-313 and C. Bouster et al., Evolution of the product yield with temperature and molecular weight in the pyrolysis of polystyrene, in: Journal of Analytical and Applied Pyrolysis 15 (1989) 249-259).

[0007] The recovered styrene monomers can be used for a new polymerization process. Styrene oligomers can potentially disrupt the polymerization process, as even small amounts can affect important properties of the polymer. This also applies to other byproducts. Therefore, the styrene monomers must be separated from other components of the product mixture to ensure high product quality.

[0008] In particular, aromatic compounds other than styrene monomers can act as chain transfer agents in radical polymerization processes, lowering the average molecular weight of the polymers produced and contributing to polymers with a lower glass transition temperature (Tg) (DS Achilias et al., Chemical recycling of polystyrene by pyrolysis: Potential use of the liquid product for the reproduction of polymer, in: Macromolecular Materials and Engineering, 292(8) (2007), 923-934). Protons from, for example, carboxylic acids, alcohols, aldehydes, or ketones act as termination agents in anionic polymerization processes of styrene (D. Baskaran et al., Anionic Vinyl Polymerization, in: Controlled and Living Polymerizations: From Mechanisms to Applications, John Wiley & Sons, 2009, 1-56).

[0009] In the present process, polystyrene can preferably be selected from the group consisting of standard polystyrene (GPPS), high-impact polystyrene (HIPS), and styrene-butadiene copolymers. The high-impact polystyrenes used are structurally modified compared to conventional rubbers by the use of special polybutadiene rubbers with, for example, a modified 1,4-cis and / or 1,4-trans fraction or 1,2- and 1,4-bond.

[0010] Furthermore, instead of polybutadiene rubber, other diene rubbers, as well as ethylene-propylene-diene copolymer (EPDM) elastomers, hydrogenated diene rubbers, or silicone rubbers can be used. In the impact-resistant polystyrene used as polystyrene, the diene rubber content, in particular the polybutadiene rubber content, is generally 5 to 12 wt.%, preferably 6 to 10 wt.%, and particularly preferably 7 to 9 wt.%, and the polystyrene content is generally 88 to 95 wt.%, preferably 90 to 94 wt.%, and more preferably 91 to 93 wt.%, wherein the sum of the polystyrene content and the diene rubber content is 100 wt.%.

[0011] Suitable standard polystyrene is produced by anionic or radical polymerization. The molecular weight inconsistency of the polymer, which can be influenced by the polymerization process, is of minor importance. Standard polystyrene and impact-resistant polystyrene are preferred, the toluene-soluble fraction of which has a mean molecular weight (Mw) of 150,000 to 300,000 g / mol, particularly preferably 150,000 to 270,000 g / mol, and which may optionally be further modified with additives such as mineral oil (e.g., white oil), stabilizers, antistatic agents, flame retardants, or waxes.

[0012] Styrene copolymers used as polystyrene according to the invention can also contain methyl(meth)acrylate, α-methylstyrene and / or maleic anhydride, as well as other copolymerizable monomers.

[0013] In JP 2005132802 and JPH 11100875 (Toshiba Plant Systems) methods for recovering styrene from polystyrene waste are described, but no solution for separating light boiling points, styrene and heavy boiling points is provided.

[0014] There is a high demand for a process for the production of styrene monomers by depolymerization of polystyrene in the presence of foreign polymers, which yields styrene in very high yield while minimizing the formation of styrene oligomers to reduce the subsequent purification process. Foreign polymers are defined as (co)polymers that differ from polystyrene structurally and in their properties.

[0015] The fluidized bed process is known to be suitable for the depolymerization of polystyrene. Liu et al. ("Pyrolysis of polystyrene waste in a fluidized-bed reactor to obtain styrene monomer and gasoline fraction", Fuel Processing Technology, 63, 45-55 (2000)) and Williams et al. ("Product composition from the fast pyrolysis of polystyrene", Environmental Technology, 20, 1109-1118 (1999)) investigated the pyrolysis of PS waste using a fluidized bed reactor and observed the depolymerization of polystyrene into styrene monomers and oligomers.

[0016] Guido Grause et al.: "Pyrolysis of Mixed Plastics in a Fluidized Bed of Hard Burnt Lime" (Industrial & Engineering Chemistry Research 2011, 50, 5459-5466), W. Kaminsky et al.: "Pyrolysis of mixed plastics into aromatics" (Journal of Analytical and Applied Pyrolysis 1999, 51, 127-134), W. Kaminsky et al: "Feedstock recycling of polymers by pyrolysis in a fluidised bed" (Polymer Degradation and Stability 2004, 85, 1045-1050), Samih Said et al.: "From complex feedstocks to new processes: The role of the newly developed micro-reactors" (Chemical Engineering and Processing: Process Intensification 2018, 131, 92-105) und WO 2018 / 018153 A1 offenbaren verschiedene Verfahren zur Depolymerisation von Polystyrol-haltigen Kunststoffen in Wirbelschichtreaktoren und anderen Reaktortypen.

[0017] In the presence of foreign polymers, a difficulty arises because these can negatively affect the depolymerization of polystyrene. An object of the invention is therefore to provide a process for the production of styrene monomers by depolymerization of polystyrene in the presence of foreign polymers with optimized process conditions in order to maximize the yield of styrene monomers.

[0018] It was found that certain combinations of depolymerization temperature and residence time in the reactor lead to particularly high styrene monomer yields.

[0019] An object of the invention is a process for the production of styrene monomers by depolymerization of a polystyrene-containing polymer composition, comprising the steps of: a) Incorporating a polymer composition (A) containing: I) 60 to 99.5 wt.%, based on the total weight of the polymer composition (A), of polystyrene (I); and II) 0.1 to 30 wt.%, based on the total weight of the polymer composition (A), of polyolefin (II); and / or III) 0.1 to 4.9 wt.%, based on the total weight of the polymer composition (A), of acrylonitrile-based polymer (III); and / or IV) 0.1 to 4.9 wt.-%, based on the total weight of the polymer composition (A), of polyester (IV), into the reaction zone (R) of a pyrolysis reactor (P); b) thermal cracking of the polystyrene contained in the polymer composition (A) in the reaction zone (R) of the pyrolysis reactor (P) at a temperature of 450 °C to 1000 °C to obtain a product mixture (G) containing styrene monomers and other components; c) removal of the product mixture (G) obtained in step b) from the reaction zone (R) of the pyrolysis reactor (P); d) cooling of the product mixture (G) removed in step c) to obtain a condensed product mixture (K) containing styrene monomers and other components; and e) separation of the styrene monomers from the other components of the condensed product mixture (K) obtained in step d). where the mean residence time (Z) of the polymer composition (A) in the reaction zone (R) of the pyrolysis reactor (P) is from 0.01 s to 10 s.

[0020] Additionally, the polymer composition (A) may contain up to 30 wt.% of additive(s) based on the total weight of the polymer composition (A).

[0021] Any polyolefin (II) can be used, for example, polyethylene or polypropylene derivatives such as LDPE (low-density polyethylene), LLDPE (linear low-density polyethylene), HDPE (high-density polyethylene), metallocene polyethylenes, ethylene copolymers such as poly(ethylene-co-vinyl acetate), ethylene-butene, ethylene-hexene, ethylene-octene copolymers, as well as cycloolefin copolymers, homopolymers or copolymers of propylene, metallocene-catalyzed polypropylenes, and copolymers of propylene with other comonomers known to those skilled in the art, and mixtures thereof. Preferred polyolefins (II) are homopolymers of ethylene, homopolymers of propylene, copolymers of ethylene and propylene, and mixtures thereof.

[0022] Any acrylonitrile-based polymer (III) can be used, for example styrene-acrylonitrile copolymers (SAN), α-methylstyrene-acrylonitrile copolymers (AMSAN), styrene-acrylonitrile-maleic anhydride copolymers, styrene-acrylonitrile-phenylmaleimide copolymers, and their graft copolymers with rubber-like polymers, e.g. acrylonitrile-butadiene-styrene graft copolymers (ABS), acrylonitrile-styrene-alkyl(meth)acrylate graft copolymers (ASA), α-methylstyrene-acrylonitrile-methyl methacrylate copolymers, α-methylstyrene-acrylonitrile-t-butyl methacrylate copolymers and styrene-acrylonitrile-t-butyl methacrylate copolymers.

[0023] Preferred acrylonitrile-based polymers (III) are styrene-acrylonitrile copolymers (SAN), acrylonitrile-styrene-alkyl acrylate graft copolymers (ASA) and acrylonitrile-butadiene-styrene graft copolymers (ABS).

[0024] Any polyester(IV) can be used, for example, polycondensation products of dicarboxylic acids containing 4 to 16 carbon atoms with diols containing 2 to 8 carbon atoms, or polycondensation products of hydroxycarboxylic acids containing 2 to 6 carbon atoms. These include, among others, polyalkylene adipates such as polyethylene adipate and polybutylene adipate, polyalkylene terephthalates such as polyethylene terephthalate and polybutylene terephthalate, polylactic acid, polyhydroxybutyrates, polycaprolactones, and polyvalerolactones. Preferred polyester(IV) components are polyethylene terephthalate (PET) and polybutylene terephthalate (PBT), particularly polyethylene terephthalate.

[0025] In a preferred embodiment, the polymer composition (A) contains polyethylene (PE) and / or polypropylene (PP) as polyolefin (II), and / or acrylonitrile butadiene styrene graft copolymer (ABS) as acrylonitrile-based polymer (III), and / or polyethylene terephthalate (PET) as polyester (IV).

[0026] According to the invention, the polymer composition (A) contains I) 60 to 99.5 wt.%, based on the total weight of the polymer composition (A), of polystyrene (I); and II) 0.1 to 30 wt.%, based on the total weight of the polymer composition (A), of polyolefin (II); and / or III) 0.1 to 4.9 wt.%, based on the total weight of the polymer composition (A), of acrylonitrile-based polymer (III); and / or IV) 0.1 to 4.9 wt.%, based on the total weight of the polymer composition (A), of polyester (IV).

[0027] Preferably the polymer composition (A) contains up to 30 wt.%, in particular 0.1 to 20 wt.%, based on the total weight of the polymer composition (A), of additive(s).

[0028] In a preferred embodiment, the polymer composition (A) contains a total of at most 4.9 wt.%, based on the total weight of the polymer composition (A), of acrylonitrile-based polymer (III) and polyester (IV).

[0029] The polymer composition (A) particularly preferably contains I) 85 to 99.5 wt.%, based on the total weight of the polymer composition (A), of polystyrene (I); and II) 0.1 to 15 wt.%, based on the total weight of the polymer composition (A), of polyolefin (II); and / or III) 0.1 to 2 wt.%, based on the total weight of the polymer composition (A), of acrylonitrile-based polymer (III); and / or IV) 0.1 to 2 wt.%, based on the total weight of the polymer composition (A), of polyester (IV).

[0030] Particularly preferably, the polymer composition (A) contains up to 10 wt.%, in particular 0.3 to 8 wt.%, based on the total weight of the polymer composition (A), of additive(s).

[0031] In a particularly preferred embodiment, the polymer composition (A) contains a total of at most 2 wt.%, based on the total weight of the polymer composition (A), of acrylonitrile-based polymer (III) and polyester (IV).

[0032] The polymer composition (A) is particularly preferably contained I) 95 to 99.5 wt.%, based on the total weight of the polymer composition (A), of polystyrene (I); and II) 0.1 to 5 wt.%, based on the total weight of the polymer composition (A), of polyolefin (II); and / or III) 0.1 to 1 wt.%, based on the total weight of the polymer composition (A), of acrylonitrile-based polymer (III); and / or IV) 0.1 to 1 wt.%, based on the total weight of the polymer composition (A), of polyester (IV).

[0033] The polymer composition (A) most preferably contains up to 4 wt.%, in particular 0.3 to 4 wt.%, based on the total weight of the polymer composition (A), additives.

[0034] In a particularly preferred embodiment, the polymer composition (A) contains a total of at most 1 wt.%, based on the total weight of the polymer composition (A), of acrylonitrile-based polymer (III) and polyester (IV). Preferably, the polymer composition (A) contains no other polymeric components than polystyrene (I) and polyolefin (II) and / or acrylonitrile-based polymer (III) and / or polyester (IV).

[0035] The polymer composition (A) may contain common plastic additives and auxiliaries. For example, an additive or auxiliary may be selected from the group consisting of antioxidants, UV stabilizers, peroxide destructors, antistatic agents, lubricants, demolding agents, flame retardants, fillers or reinforcing agents (glass fibers, carbon fibers, etc.), colorants, and combinations of two or more thereof.

[0036] Examples of oxidation retarders and heat stabilizers include halides of group I metals of the periodic table, e.g. sodium, potassium and / or lithium halides, possibly in combination with copper(I) halides, e.g. chlorides, bromides, iodides, sterically hindered phenols, hydroquinones, various substituted representatives of these groups and their mixtures in concentrations up to 1 wt%, based on the total weight of the polymer composition (A).

[0037] Examples of UV stabilizers, which are generally present in amounts up to 2 wt% based on the total weight of the polymer composition (A), include various substituted resorcinols, salicylates, benzotriazoles and benzophenones.

[0038] Furthermore, organic dyes such as nigrosine, pigments such as titanium dioxide, phthalocyanines, ultramarine blue, and carbon black may be included as colorants in the polymer composition (A), as well as fibrous and powdered fillers and reinforcing agents. Examples of the latter are carbon fibers, glass fibers, amorphous silica, calcium silicate (wollastonite), aluminum silicate, magnesium carbonate, kaolin, chalk, powdered quartz, mica, and feldspar.

[0039] Examples of germination agents that may be included are talc, calcium fluoride, sodium phenylphosphinate, aluminum oxide, silicon dioxide and nylon 22.

[0040] Lubricants and demolding agents, which can generally be used in quantities up to 1 wt% based on the total weight of the polymer composition (A), include, for example, long-chain fatty acids such as stearic acid or behenic acid, their salts (e.g., Ca or Zn stearate) or esters (e.g., stearyl stearate or pentaerythritol tetrastearate) as well as amide derivatives (e.g., ethylene bisstearylamide).

[0041] Furthermore, mineral-based antiblocking agents may be present in amounts up to 0.1 wt%, based on the total weight of the polymer composition (A). Examples include amorphous or crystalline silica, calcium carbonate, or aluminum silicate.

[0042] For example, mineral oil, preferably medical white oil, may be included as a processing aid in amounts up to 5 wt.%, preferably up to 2 wt.%, in particular 0.1 to 2 wt.%, based on the total weight of the polymer composition (A).

[0043] Examples of plasticizers include phthalic dioctyl esters, phthalic dibenzyl esters, phthalic butylbenzyl esters, hydrocarbon oils, N-(n-butyl)benzenesulfonamide and o- and p-tolylethylsulfonamide.

[0044] Furthermore, all flame retardants known for the respective thermoplastics may be included, especially those based on phosphorus compounds.

[0045] Furthermore, it may still contain moisture and / or other inorganic and / or organic foreign components, such as food residues.

[0046] Preferably, the polystyrene component (I) contained in the polymer composition (A) consists substantially, preferably entirely, of GPPS (general purpose polystyrene). In this context, "substantially" means that the polystyrene component contains no components that alter the properties of the GPPS in any way.

[0047] The polymer composition (A) used according to the invention can optionally be pretreated in a suitable manner to remove, for example, adhering contaminants such as food residues or dirt, moisture and foreign substances such as metals or other substances and composite materials.

[0048] This is advantageously achieved in a pretreatment that may include one or more of the following steps, the order of which is not fixed and which may be repeated several times: manual sorting of contaminants, washing, comminution, automatic sorting in suitable equipment. If necessary, polymer compositions that do not correspond to polymer composition (A) can also be converted into a polymer composition (A) used according to the invention by such a process.

[0049] A preferred embodiment of the inventive method is therefore one in which a polymer composition that does not correspond to polymer composition (A) is subjected to a pretreatment comprising one or more of the following steps, the order of which is not fixed and steps can also be repeated several times: manual sorting of contaminants, washing, comminution, automatic sorting in suitable equipment in order to obtain polymer composition (A).

[0050] The thermal decomposition of polystyrene can take place in any suitable reactor where the temperature required for decomposition can be reached. For example, thermal decomposition can be carried out in a rotary kiln. Rotary kilns are described, for example, in EP-A 1481957. Thermal decomposition can also take place in extruders; these are described, for example, in EP-A 1966291. Such reactors can be operated with or without a gas flow, such as carrier gas or gas as the reaction medium.

[0051] The pyrolysis reactor (P) can therefore be any known type of pyrolysis reactor, provided that the design of the pyrolysis reactor allows for precise temperature control in the reaction zone (R) of the pyrolysis reactor (P) and precise control of the mean residence time (Z) of the polymer composition (A) in the reaction zone (R) of the pyrolysis reactor (P).

[0052] In this context, "precise setting" means that the deviation of the actual temperature in the reaction zone (R) of the pyrolysis reactor (P) from the set temperature is at most 10 °C, preferably at most 5 °C, particularly preferably at most 1 °C, or that the deviation of the actual mean residence time (Z) from the set mean residence time (Z) is at most 0.2 s, preferably at most 0.1 s, particularly preferably at most 0.05 s, most preferably at most 0.01 s.

[0053] The pyrolysis reactor (P) is preferably a fluidized bed reactor, as described, for example, in Schildhauer et al., "Reactors for Fluid-Solid Reactions: Fluidized Bed Reactors" in: Reschetilowski W. (ed.): Handbook of Chemical Reactors, Springer Spektrum, Berlin, Heidelberg (2019). A gas or gas mixture is typically used as the fluidization medium. The gas or gas mixture is usually non-reactive under the conditions prevailing in the pyrolysis reactor (P). Preferably, the gas is selected from water vapor, nitrogen, noble gases (Xe, Ar, Ne, He), or a mixture thereof.

[0054] The gas or gas mixture can be introduced into the pyrolysis reactor (P) as a separate gas stream. The optimal flow rate of the gas or gas mixture depends on the reactor configuration as well as the reaction or process conditions. Process optimization is possible via the parameters temperature, residence time of the reaction mixture in the reaction zone (R) of the pyrolysis reactor (P), and concentration of the reactants. The area of ​​the reactor in which the reaction mixture is subjected to conditions under which depolymerization reactions take place is referred to here as the reaction zone (R).

[0055] The pyrolysis reactor (P) can contain a solid medium, e.g., SiO₂ (quartz sand) or SiC. In a preferred embodiment, the pyrolysis reactor (P) is a fluidized bed reactor comprising a fluidized bed of silicon carbide (SiC) in the reaction zone (R). SiC, in addition to high chemical and mechanical stability, possesses good thermal conductivity and heat capacity. This combination is advantageous for carrying out endothermic processes.

[0056] SiC with a weight-average particle size of 20 to 1000 µm, particularly preferably 40 to 500 µm, is preferably used. At such particle sizes, particularly good fluidization of the fluidized bed is achieved and particularly effective heat transfer to the polymer composition (A) is enabled.

[0057] It has been found that the yield of styrene monomers is particularly high when the residence time of the polystyrene in the depolymerization zone is kept short. This can be achieved in fluidized bed reactors or other reactors that utilize a gas stream to transport the introduced polymer composition (A) through the reactor. The average residence times of the reactant range from 0.1 seconds to 10 seconds. Short residence times can be achieved by using high gas flow velocities. Depolymerization can be carried out at pressures from 0.01 bar to 5 bar or at atmospheric pressure (1 bar). Preferably, the gas stream is preheated before being introduced into the reaction zone (R). Preheating is preferably performed at a temperature that is at most 200 °C lower than the temperature in the reaction zone (R) of the pyrolysis reactor (P).

[0058] In the process according to the invention, the temperature in the reaction zone (R) of the pyrolysis reactor (P) is set to 400 to 1000 °C, preferably to 500 to 800 °C, particularly preferably to 550 to 650 °C, and most preferably to 580 to 630 °C, and the mean residence time of the polymer composition (A) in the reaction zone (R) of the pyrolysis reactor (P) is set to 0.1 to 10 s, preferably to 0.2 to 2 s, particularly preferably to 0.3 to 1 s, and most preferably to 0.4 to 0.6 s. In a preferred embodiment, the temperature in the reaction zone (R) is 500 to 800 °C and the mean residence time of the polymer composition (A) therein is 0.2 to 2 s. In a particularly preferred embodiment, the temperature in the reaction zone (R) is 550 to 650 °C and the mean residence time of the polymer composition (A) therein is 0.3 to 1 s.In a particularly preferred embodiment, the temperature in the reaction zone (R) is 580 to 630 °C and the mean residence time of the polymer composition (A) therein is 0.4 to 0.6 s.

[0059] The temperature can be set in any known way, for example by microwave radiation, with the aid of heat exchangers, gas burners, resistive heating elements (resistance heating), or by introducing superheated gas, in particular steam, each alone or in combination. In one embodiment, the temperature is set with the aid of resistive heating elements that are in contact with the wall of the reaction zone (R) of the pyrolysis reactor (P).

[0060] Alternatively, the temperature can be adjusted using steam, which is provided by evaporating water and heated to the desired temperature by a steam superheater. In one embodiment, a combination of resistive heating elements in contact with the wall of the reaction zone (R) of the pyrolysis reactor (P) and steam is used to adjust the temperature in the reaction zone (R) of the pyrolysis reactor (P).

[0061] In a preferred embodiment, the pyrolysis reactor (P) is a fluidized bed reactor, preferably comprising a SiC fluidized bed in its reaction zone (R), wherein the temperature in the reaction zone (R) is adjusted by introducing steam of the desired temperature. In this embodiment, the steam is supplied by an evaporator and heated to the desired temperature by a steam superheater. Also in this embodiment, the steam is used both for adjusting the temperature in the reaction zone (R) and for generating the fluidized bed. Optionally, in this embodiment, the heating energy in the reaction zone (R) can additionally be supplied by resistive heating elements that are in contact with the wall of the reaction zone (R) of the pyrolysis reactor (P).

[0062] The particle size and concentration of the polymer composition (A) in the reaction zone (R) can be adapted to the specific characteristics of the reactor and its configuration, the reaction conditions, and the composition of the polymer composition (A). Typically, the polymer composition (A) has a particle size between 100 µm and 50 mm, preferably between 250 µm and 5 mm, and particularly preferably between 500 µm and 2 mm. The particles can have a spherical or non-spherical shape. In the case of a spherical shape, the particle size is determined by measuring the volume-mean diameter. In the case of non-spherical particles, for example, needle-shaped particles, the longest dimension is used to determine the particle size.

[0063] The concentration of the reactant in the reactor depends on the reactor type, reactor size, and reactor configuration. Typically, the concentration of the polymer composition (A) in the reaction zone (R) of the pyrolysis reactor (P) is between 1 and 50 wt.%, preferably between 1 and 25 wt.%, particularly preferably between 1 and 10 wt.%, and most preferably between 2 and 7 wt.%.

[0064] Preferably, the polymer composition (A) is pneumatically fed into the reaction zone (R) of the pyrolysis reactor (P) in step a), mixed with the silicon carbide fluidized bed, and finally depolymerized in step b). Particularly preferably, the polymer composition (A) is fed continuously in step a).

[0065] During the residence time (Z) in the reaction zone (R) of the pyrolysis reactor (P), the polystyrene component and, if applicable, other polymers of the polymer composition (A) are at least partially depolymerized to yield a product mixture (G) containing styrene monomers and other components.

[0066] The product mixture (G) containing styrene monomers and other components is withdrawn from the reaction zone (R) of the pyrolysis reactor (P) in step c). Preferably, the withdrawal takes place continuously. Particularly preferably, the product mixture (G) is withdrawn continuously in a gaseous state from the upper region of the reaction zone (R) of the pyrolysis reactor (P). In this case, the withdrawal of the product mixture (G) can be carried out automatically, for example, by conveying the product mixture (G) out of the reaction zone (R) due to the reaction-induced increase in pressure in the reaction zone (R).

[0067] The pyrolysis reactor may contain or be connected to a quench. In this context, a quench is understood to be a region of the pyrolysis reactor in which the depolymerization reaction is rapidly stopped, preferably by cooling the hot gas consisting of the product mixture (G) and an inert gas stream, for example, steam. The quench serves, among other things, to stabilize the reaction products and to prevent or reduce unwanted repolymerization.

[0068] Typical quenchers cool the product mixture (G) from a temperature of more than 400 °C to a temperature of less than 350 °C within a very short period of time, preferably within less than 10 seconds, particularly preferably within less than 5 seconds, and most preferably within less than 1 second. Quenchers are described, for example, in EP-A 1966291.

[0069] The product mixture (G) is cooled after being removed from the reaction zone (R) of the pyrolysis reactor (P), causing condensation of the styrene monomers and other components, resulting in a condensed product mixture (K) containing styrene monomers and other components. The product mixture (G) is cooled to a temperature below the condensation point of styrene monomers. Preferably, the product mixture (G) is cooled to a temperature below 70 °C, particularly preferably below 50 °C, and most preferably below 40 °C. In a preferred embodiment, the product mixture (G) is cooled to a temperature between 0 °C and 70 °C. In a particularly preferred embodiment, the product mixture (G) is cooled to a temperature between 0 °C and 50 °C. In a most particularly preferred embodiment, the product mixture (G) is cooled to a temperature between 15 °C and 40 °C.

[0070] Cooling can be carried out in any known manner. For example, cooling is possible on a solid surface cooled by water or air. Cooling is also possible using a water mist that is brought into direct contact with the product mixture (G). Preferably, cooling takes place in a water mist. The condensable components of the product mixture (G) condense according to their vapor pressures and are collected along with the water. Condensation yields a condensed product mixture (K) containing styrene monomers and other components.

[0071] In the case of cooling in a water mist, the condensed product mixture (K) is obtained as a two-phase system with the cooling water. In this case, the condensed product mixture (K) is separated from the aqueous phase as a floating organic phase. The aqueous phase can be cooled again and used as a water mist to cool the product mixture (G).

[0072] The condensed product mixture (K) typically contains more than 50 wt%, based on the total weight of the condensed product mixture (K), styrene monomers and less than 50 wt%, based on the total weight of the condensed product mixture (K), of the other components.

[0073] Preferably, the condensed product mixture (K) contains 50 to 99 wt.%, based on the total weight of the condensed product mixture (K), styrene monomers and 1 to 50 wt.%, based on the total weight of the condensed product mixture (K), of the other components, particularly preferably 60 to 99 wt.%, based on the total weight of the condensed product mixture (K), of styrene monomers and 1 to 40 wt.%, based on the total weight of the condensed product mixture (K), of the other components, most preferably 75 to 99 wt.%, based on the total weight of the condensed product mixture (K), of styrene monomers and 1 to 25 wt.%, based on the total weight of the condensed product mixture (K), of the other components.

[0074] In the further course of the process, the condensed product mixture (K) is separated into styrene monomers and other components. This separation can be carried out by any known method suitable for separating mixtures of liquid products and, optionally, solids into their components. Depending on the other components besides styrene monomers, suitable methods for separating the condensed product mixture (K) into styrene monomers and other components may include, for example, sedimentation, centrifugation, filtration, decantation, distillation, chromatography, crystallization, and sublimation.

[0075] If the condensed product mixture (K) contains solids, it is advantageous to separate the solids before separating the liquid components. In this case, it is preferred to separate the solids from the liquid components by sedimentation, centrifugation, filtration, distillation, sublimation and / or decantation, particularly preferably by filtration, and most preferably by filtration using a solid-liquid filter.

[0076] The further separation of the liquid components into styrene monomers and other components preferably comprises at least one distillation step, such as fractional distillation, at least one chromatography step, such as column chromatography, HPLC, or flash chromatography, and / or at least one crystallization step, such as fractional crystallization. Particularly preferably, the separation of the liquid components comprises at least one distillation step, and most preferably, at least one fractional distillation step. In a particularly preferred embodiment, the separation of the liquid components into styrene monomers and other components comprises at least one fractional distillation step in one or more rectification columns.

[0077] It is often advantageous to return at least some of the other components to the reaction zone (R) of the pyrolysis reactor (P). This is particularly beneficial if some of the other components contain styrene oligomers, such as styrene dimers and styrene trimers. This allows for an overall better yield of styrene monomers, as it also enables the depolymerization of the remaining oligomers.

[0078] For this reason, preferably at least some of the other components of the condensed product mixture (K), which have been separated from styrene monomers, are recycled into the reaction zone (R) of the pyrolysis reactor (P). Continuous recycling of the other components is particularly preferred.

[0079] In a preferred embodiment, the additional components that are recycled to the reaction zone (R) of the pyrolysis reactor (P) consist essentially of styrene oligomers, preferably styrene dimers and styrene trimers. In this context, "essentially" means that, besides styrene oligomers, the additional components recycled to the reaction zone (R) of the pyrolysis reactor (P) do not contain any other components that interfere with the depolymerization process in the reaction zone (R) of the pyrolysis reactor (P).

[0080] A further object of the invention is the use of a fluidized bed reactor for the depolymerization of a polystyrene-containing polymer composition (A), at a temperature in the reaction zone (R) of the reactor of 400 °C to 1000 °C and a mean residence time of the polystyrene-containing polymer composition (A) in the reaction zone (R) of 0.01 s to 10 s, wherein the polymer composition (A) contains upon entry into the reaction zone (R) of the reactor: I) 60 to 99.5 wt.%, based on the total weight of the polymer composition (A), of polystyrene (I); and II) 0.1 to 30 wt.%, based on the total weight of the polymer composition (A), of polyolefin (II); and / or III) 0.1 to 4.9 wt.%, based on the total weight of the polymer composition (A), of acrylonitrile-based polymer (III); and / or IV) 0.1 to 4.9 wt.%, based on the total weight of the polymer composition (A), of polyester (IV).

[0081] Preferably, the fluidized bed reactor in the reaction zone (R) comprises a fluidized bed of silicon carbide (SiC). Particularly preferably, the polymer composition (A), the silicon carbide, the temperature in the reaction zone (R), and the mean residence time of the polystyrene in the reaction zone (R) are selected as described for the process according to the invention.

[0082] A device suitable for carrying out the process according to the invention for the production of styrene monomers by depolymerization of a polystyrene-containing polymer composition (A) as described above is a device for carrying out the process according to the invention for the production of styrene monomers by depolymerization of a polystyrene-containing polymer composition (A) as described above, in which the reaction zone (R) and the pyrolysis reactor (P) are designed in such a way that a gentle depolymerization of polystyrene can take place.

[0083] Preferably, the device comprises, as a pyrolysis reactor (P), a fluidized bed reactor, particularly preferably a fluidized bed reactor comprising a fluidized bed of silicon carbide (SiC) in the reaction zone (R), wherein the silicon carbide preferably has a weight-average particle size of 20 to 1000 µm, particularly preferably 40 to 500 µm, optionally resistive heating conductors on the outer walls of the reaction zone (R), an evaporator for generating steam, a steam superheater for adjusting the desired steam temperature, a line for introducing the steam into the reaction zone (R) and a quench for cooling the product mixture (G).

[0084] Another aspect of the invention is the use of a polymer composition (A) containing I) 60 to 99.5 wt.%, based on the total weight of the polymer composition (A), of polystyrene (I); and II) 0.1 to 30 wt.%, based on the total weight of the polymer composition (A), of polyolefin (II); and / or III) 0.1 to 4.9 wt.%, based on the total weight of the polymer composition (A), of acrylonitrile-based polymer (III); and / or IV) 0.1 to 4.9 wt.%, based on the total weight of the polymer composition (A), of polyester (IV), as a starting material in the production of styrene monomers by depolymerization in a fluidized bed reactor.

[0085] Preferably, the polymer composition (A), the silicon carbide, the temperature in the reaction zone (R) and the mean residence time of the polystyrene in the reaction zone (R) are selected as described for the process according to the invention.

[0086] The invention is illustrated by the following examples, figures and claims. Examples

[0087] From an inerted feed container (B101), the polymer is metered via volumetric dosing into a gas jet, which pneumatically conveys the particles into the reaction zone of a fluidized bed reactor (R101) containing SiC particles. Heating energy is transferred to the reaction zone via resistive heating conductors through the metallic reactor wall.

[0088] The steam for generating the fluidized bed is supplied by an evaporator (D101) and brought to the desired temperature via a steam superheater (E102).

[0089] In the reaction zone, the SiC fluidized bed is created with the steam, and the pneumatically introduced polymer particles are mixed in the fluidized bed and finally depolymerized.

[0090] The product mixture from the depolymerization process (R101) is cooled to below 50 °C in column (K101) using a water mist. Condensable components condense according to their vapor pressures and are collected with the water in the cooled sump. Solid particles are also precipitated by the mist according to their coalescence tendency. Floating, water-insoluble components are transferred to a buffer vessel via a skimmer system. Samples are taken from the concentrated organic fraction of the condensed product mixture and analyzed by gas chromatography.

[0091] The water from the condensation process is cooled via a heat exchanger and then pumped back into the cooling column (K101). Any solids are removed using a solid-liquid filter. Examples 1.1 and 1.2

[0092] A polymer composition consisting of 99 wt% of an amorphous polystyrene (GPPS) (INEOS Styrolution, Frankfurt) with a melt volume flow rate (Melt Volume Rate 200 / 5 kg load, ISO 1133) of approximately 28 cm³ / 10 min and 1 wt% acrylonitrile butadiene styrene graft polymer (ABS of INEOS Styrolution, Frankfurt) with a melt volume flow rate (Melt Volume Rate 220 / 10 kg load, ISO 1133) of approximately 5.5 cm³ / 10 min was depolymerized in the apparatus described above under various conditions.

[0093] The temperature in the reaction zone of the fluidized bed reactor (R101) was varied between 550 °C and 650 °C. The concentration of the polymer composition in the reaction zone was maintained at 5% of the total reactor filling, consisting of SiC and polymer particles. The yields of styrene monomers as a function of the reaction conditions are shown in Table 1. The compositions of the pyrolysis oil are shown in Table 2. Comparative example 1

[0094] Example 1 was repeated using a polymer composition consisting of 95 wt% of an amorphous polystyrene (GPPS) (INEOS Styrolution, Frankfurt) with a melt volume flow rate (Melt Volume Rate 200 / 5 kg load, ISO 1133) of approximately 28 cm³ / 10 min and 5 wt% of an acrylonitrile butadiene styrene graft polymer (INEOS Styrolution, Frankfurt) with a melt volume flow rate (Melt Volume Rate 220 / 10 kg load, ISO 1133) of approximately 5.5 cm³ / 10 min. The yield of styrene monomers is shown in Table 1. The composition of the pyrolysis oil (condensate oil) is shown in Table 2. Comparison example 2

[0095] Example 1 was repeated using a polymer composition consisting of 100 wt% of an amorphous polystyrene (GPPS) (INEOS Styrolution, Frankfurt) with a melt volume flow rate (Melt Volume Rate 200 / 5 kg load, ISO 1133) of approximately 28 cm³ / 10 min. The yield of styrene monomers is shown in Table 1. The composition of the pyrolysis oil is shown in Table 2. Example 2

[0096] Example 1 was repeated using a polymer composition consisting of 95 wt% amorphous polystyrene (GPPS) (INEOS Styrolution, Frankfurt) with a melt volume flow rate (Melt Volume Rate 200 / 5 kg load, ISO 1133) of approximately 28 cm³ / 10 min and 5 wt% polyethylene (LDPE, type 2102, Sabic). The styrene monomer yield is shown in Table 1. The composition of the pyrolysis oil is shown in Table 2. Example 3

[0097] Example 1 was repeated with a polymer composition consisting of 90 wt% of an amorphous polystyrene (GPPS) (INEOS Styrolution, Frankfurt) with a melt volume flow rate (Melt Volume Rate 200 / 5 kg load, ISO 1133) of approximately 28 cm 3< / 10 min and 10 wt% polyethylene (LDPE, type 2102, Sabic).

[0098] The yield of styrene monomers is shown in Table 1. The composition of the pyrolysis oil is shown in Table 2. Example 4

[0099] Example 1 was repeated using a polymer composition consisting of 95 wt% of an amorphous polystyrene (GPPS) (INEOS Styrolution, Frankfurt) with a melt volume flow rate (Melt Volume Rate 200 / 5 kg load, ISO 1133) of approximately 28 cm³ / 10 min and 5 wt% polypropylene (Type 579s, Sabic). The yield of styrene monomers is shown in Table 1. The composition of the pyrolysis oil is shown in Table 2. Example 5

[0100] Example 1 was repeated using a polymer composition consisting of 90 wt% of an amorphous polystyrene (GPPS) (INEOS Styrolution, Frankfurt) with a melt volume flow rate (Melt Volume Rate 200 / 5 kg load, ISO 1133) of approximately 28 cm³ / 10 min and 10 wt% polypropylene (Type 579s, Sabic). The yield of styrene monomers is shown in Table 1. The composition of the pyrolysis oil is shown in Table 2. Example 6

[0101] Example 1 was repeated using a polymer composition consisting of 95 wt% of an amorphous polystyrene (GPPS) (INEOS Styrolution, Frankfurt) with a melt volume flow rate (Melt Volume Rate 200 / 5 kg load, ISO 1133) of approximately 28 cm³ / 10 min and 5 wt% titanium dioxide. The yield of styrene monomers is shown in Table 1. The composition of the pyrolysis oil is shown in Table 2. Example 7

[0102] Example 1 was repeated with a polymer composition consisting of 98 wt% of an amorphous polystyrene (GPPS) (INEOS Styrolution, Frankfurt) with a melt volume flow rate (Melt Volume Rate 200 / 5 kg load, ISO 1133) of approximately 28 cm 3< / 10 min and 2 wt% carbon black.

[0103] The yield of styrene monomers is shown in Table 1. The composition of the pyrolysis oil is shown in Table 2. Table 1: Results of the pyrolysis of the polymer compositions Example polymer Temperature in the reaction zone [°C] Average residence time in the reaction zone [s] Mass fraction of condensate oil relative to the mass used [wt.%] Styrene concentration in condensate oil [wt%] 1.1 99% GPPS / 1% ABS 550 0,51 55,6 69,8 1.2 99% GPPS / 1% ABS 600 0,51 56,7 71,6 2 95% GPPS / 5% LDPE 600 0,51 56,4 73,9 3 90% GPPS / 10% LDPE 600 0,51 66,8 72,8 4 95% GPPS / 5% PP 600 0,51 85,9 71,9 5 90% GPPS / 10% PP 600 0,51 85,1 73,6 6 95% GPPS / 5% TiO2 600 0,51 41,6 77,5 7 98% GPPS / 2% soot 600 0,51 76,5 72,8 Comparative example 1 95% GPPS / 5% ABS 600 0,51 0,0 not applicable Comparison example 2 100% GPPS 600 0,51 65,9 83,2 Table 2: Composition of the obtained pyrolysis oil Example Styrene concentration in condensate oil [wt%] Dimer concentration in condensate oil [wt%] Trimer concentration in condensate oil [wt%] Concentration of other compounds in the condensate oil [wt.%] 1.1 69,8 7,3 9,7 13,2 1.2 71,6 9,2 0,6 18,6 2 73,9 8,7 0,7 16,8 3 72,8 8,1 0,6 18,5 4 71,9 8,1 0,6 19,4 5 73,6 7,3 0,5 18,7 6 77,5 8,0 0,4 14,1 7 72,8 8,7 0,6 17,8 Comparison 1 No pyrolysis oil was produced No pyrolysis oil was produced No pyrolysis oil was produced No pyrolysis oil was produced Comparison 2 83,2 6,0 0,6 10,3 Explanation of the characters

[0104] Fig. 1 shows the flow diagram of the pilot plant for the production of styrene monomers by depolymerization of polystyrene-containing polymer compositions. Fig. 2 shows an overview of the styrene concentration in the condensate oil. Fig. 3shows the dependence of the pyrolysis oil composition on the temperature for a polymer composition of 99 wt% GPPS and 1 wt% ABS. Fig. 4 shows the dependence of the pyrolysis oil composition on the polymer composition for an ABS content of 0, 1 and 5 wt.%. Fig. 5 shows the dependence of the pyrolysis oil composition on the polymer composition at 0, 5 and 10 wt% LDPE and / or PP. Fig. 6 shows the dependence of the pyrolysis oil composition on the polymer composition upon addition of TiOz or soot.

Claims

1. A process for the production of styrene monomers by depolymerization of a polystyrene-containing polymer composition, comprising the steps of: a) introducing a polymer composition (A) containing: I) 60% to 99.5% by weight of polystyrene (I), based on the total weight of the polymer composition (A); and II) 0.1% to 30% by weight of polyolefin (II), based on the total weight of the polymer composition (A); and / or III) 0.1% to 4.9% by weight of acrylonitrile-based polymer (III), based on the total weight of the polymer composition (A); and / or IV) 0.1% to 4.9% by weight of polyester (IV), based on the total weight of the polymer composition (A), into the reaction zone (R) of a pyrolysis reactor (P); b) thermally cleaving the polystyrene present in the polymer composition (A) in the reaction zone (R) of the pyrolysis reactor (P) at a temperature of from 400°C to 1000°C, in order to obtain a product mixture (G) containing styrene monomers and further components; c) withdrawing the product mixture (G) obtained in step b) from the reaction zone (R) of the pyrolysis reactor (P); d) cooling the product mixture (G) withdrawn in step c), in order to obtain a condensed product mixture (K) containing styrene monomers and further components; and e) separating the styrene monomers from the further components of the condensed product mixture (K) obtained in step d), wherein the average residence time (Z) of the polymer composition (A) in the reaction zone (R) of the pyrolysis reactor (P) is from 0.01 s to 10 s.

2. The process according to claim 1, wherein the polyolefin (II) is polyethylene (PE) and / or polypropylene (PP), and / or the acrylonitrile-based polymer (III) is acrylonitrile-butadiene-styrene graft copolymer (ABS) and / or the polyester (IV) is polyethylene terephthalate (PET).

3. The process according to claim 1 or 2, wherein the polymer composition (A) contains the polystyrene (I) in an amount of from 85% to 99.5% by weight, based on the total weight of the polymer composition (A), and the polyolefin (II) in an amount of from 0.1% to 15% by weight, based on the total weight of the polymer composition (A), and / or the acrylonitrile-based polymer (III) in an amount of from 0.1% to 2% by weight, based on the total weight of the polymer composition (A), and / or the polyester (IV) in an amount of from 0.1% to 2% by weight, based on the total weight of the polymer composition (A).

4. The process according to any one of claims 1 to 3, wherein the temperature in the reaction zone (R) of the pyrolysis reactor (P) is 580°C to 630°C and the average residence time (Z) of the polymer composition (A) in the reaction zone of the pyrolysis reactor is 0.4 s to 0.6 s.

5. The process according to any one of claims 1 to 4, wherein the condensed product mixture (K) obtained in step d) contains from 75% to 99% by weight of styrene and 1% to 25% by weight of the further components, based in each case on the total weight of the product mixture (K).

6. The process according to any one of claims 1 to 5, wherein the pyrolysis reactor (P) is a fluidized bed reactor, preferably comprising a silicon carbide fluidized bed in the reaction zone (R).

7. The process according to any one of claims 1 to 6, wherein at least a portion of the further components obtained in step e) is recycled into the reaction zone (R) of the pyrolysis reactor (P).

8. The process according to claim 7, in which the further components obtained in step e) which are recycled, preferably continuously, into the reaction zone (R) of the pyrolysis reactor (P) essentially consist of styrene oligomers.

9. The process according to any one of claims 1 to 8, in which the polystyrene component in the polymer composition (A), which in step a) is recycled into the reaction zone (R) of the pyrolysis reactor (R), essentially consists of GPPS (general purpose polystyrene).

10. The process according to any one of claims 1 to 9, in which, in step d), the product mixture (G) withdrawn in step c) is cooled to a temperature of from 0°C to 50°C.

11. The process according to any one of claims 1 to 10, in which the separation of the styrene monomers in step e) comprises a step of fractional distillation.

12. The use of a fluidized bed reactor for the depolymerization of a polystyrene-containing polymer composition (A), at a temperature in the reaction zone (R) of the reactor of from 400°C to 1000°C and with an average residence time of the polystyrene-containing polymer composition (A) in the reaction zone (R) of from 0.01 s to 10 s, wherein the polymer composition (A) on entry into the reaction zone (R) of the reactor contains: I) 60% to 99.5% by weight of polystyrene (I), based on the total weight of the polymer composition (A); and II) 0.1% to 30% by weight of polyolefin (II), based on the total weight of the polymer composition (A); and / or III) 0.1% to 4.9% by weight of acrylonitrile-based polymer (III), based on the total weight of the polymer composition (A); and / or IV) 0.1% to 4.9% by weight of polyester (IV), based on the total weight of the polymer composition (A).

13. The use according to claim 12, wherein the fluidized bed reactor comprises a silicon carbide fluidized bed.

14. The use of a polymer composition (A) containing I) 60% to 99.5% by weight of polystyrene (I), based on the total weight of the polymer composition (A); and II) 0.1% to 30% by weight of polyolefin (II), based on the total weight of the polymer composition (A); and / or III) 0.1% to 4.9% by weight of acrylonitrile-based polymer (III), based on the total weight of the polymer composition (A); and / or IV) 0.1% to 4.9% by weight of polyester (IV), based on the total weight of the polymer composition (A), as a feedstock for the production of styrene monomers by depolymerization in a fluidized bed reactor.