BITUMINOUS COMPOSITIONS WITH PHOSPHORDER Derivatives

DE602014091099T2Active Publication Date: 2024-10-30TOTALENERGIES ONETECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE602014091099
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2013-11-12
Filing Date
2014-11-06
Publication Date
2024-10-30
Estimated Expiration
2034-11-06

AI Technical Summary

Technical Problem

Conventional bituminous compositions used in road and industrial applications often lack simultaneous improvement in mechanical and dynamic properties, and they emit significant hydrogen sulfide (H2S) during preparation and use, posing safety and environmental concerns.

Method used

A process involving the treatment of bitumen or bituminous compositions with a scavenger H2S, such as copper oxides, and an acidic adjuvant like phosphoric acid, which are added separately or together, to reduce H2S emissions while enhancing mechanical and dynamic properties.

Benefits of technology

The process significantly reduces H2S emissions to less than 10 ppm, preferably less than 1 ppm, and improves the mechanical and dynamic properties of bituminous compositions, such as increased plasticity range and stability, without degrading the effectiveness of the acidic treatment.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present invention belongs to the field of bituminous compositions and their performance additives. More specifically, it relates to bituminous compositions comprising phosphoric derivatives and their preparation process.

[0002] The invention also relates to the use of these bituminous compositions in the fields of road applications, in particular in the manufacture of road binders such as hot mixes, cold mixes, asphalts or surface coatings, and in the fields of industrial applications, for example in the manufacture of interior and exterior coatings. PREVIOUS ART

[0003] The use of bitumen in the manufacture of materials for road and industrial applications has been known for a long time: bitumen is the main hydrocarbon binder used in road construction and civil engineering. To be used as a binder in these different applications, bitumen must have certain mechanical and dynamic properties.

[0004] Conventional bitumens do not generally possess all the required qualities at the same time. Bituminous compositions are used for the preparation of binders for various surface coatings and, in particular, as road surface coatings, provided that these compositions possess a certain number of mechanical and / or dynamic characteristics in combination. The mechanical properties of bituminous compositions are determined by standardized tests of the various mechanical characteristics such as softening point, penetrability and rheological characteristics in determined traction.

[0005] Much work has focused on improving the mechanical, elastic and / or rheological properties of bituminous compositions.

[0006] It has long been known that the addition of various polymers to these conventional bitumens makes it possible to favorably modify the mechanical properties of the latter and to form bitumen / polymer compositions having improved mechanical qualities compared to those of bitumens alone.

[0007] It is further known that the stability of bitumen / polymer compositions can be improved by chemical coupling of the polymer to the bitumen. This chemical coupling, conventionally carried out by crosslinking the polymer, also makes it possible to broaden the field of use of bitumen / polymer compositions. Documents FR2376188, FR2429241, FR2528439, EP0360656 may be cited as examples of a process involving a random or block copolymer of styrene and a conjugated diene crosslinked with sulfur. Document FR2528439 deals in particular with crosslinking with a polysulfide. Document EP0360656 describes the use of a sulfur-donating vulcanization accelerator used alone or in combination with chemically unbound sulfur and / or a polysulfide or a non-sulfur-donating vulcanization accelerator.

[0008] The resulting crosslinked bitumen / polymer compositions are known by the acronym "PmB" for Polymer-modified Bitumen or "PmA" for Polymer-modified Asphalt. For the sake of clarity, we will only use the acronym PmB for crosslinked bitumen / polymer compositions. The crosslinking of bitumen / polymer compositions gives them very good properties in terms of storage stability, cohesiveness, elongation capacity and resistance to aging.

[0009] Phosphoric acid and / or polyphosphoric acid has been used since the 1970s to improve the rheological properties of bitumens or bituminous compositions, in particular to increase their consistency. For example, document US3751278 describes a manufacturing process using phosphoric acid to increase viscosity at high temperature without reducing consistency at room temperature.

[0010] Some acidic admixtures have also been used to obtain bitumen / polymer compositions with a reinforced multigrade character. In patent application EP703949, the authors have, moreover, demonstrated that the mechanical and / or rheological properties could be improved, in particular the plasticity range could be widened by using specific acidic mineral admixtures. The authors cite, in particular, phosphoric acids, sulfonic acids, sulfuric acids and their mixtures.

[0011] In document WO9714753, the authors have shown that the plasticity range of sulfur-crosslinked bitumen / polymer compositions can be widened by incorporating into said compositions a mineral adjuvant of the acid or acid anhydride type after the sulfur crosslinking phase.

[0012] Another issue related to the use of bituminous compositions concerns the release of hydrogen sulfide (hydrogen sulfide), noted H 2 S, during their preparation process or their use. The emission of H 2 S is higher for bitumen / crosslinked polymer compositions due to the use of a sulfur-donating crosslinking agent in their preparation process. Hydrogen sulfide (H 2 S) is a colorless and toxic gas, with a characteristic odor at very low concentrations. For reasons of safety and environmental constraints, the reduction or even elimination of hydrogen sulfide emissions during the production of bituminous compositions, in particular bitumen / crosslinked polymer compositions, is an industrial challenge.

[0013] Solutions have been proposed in the literature to reduce hydrogen sulfide emissions during the manufacture or use of bituminous compositions. In particular, the addition of an agent capable of trapping hydrogen sulfide (H 2 S) during the crosslinking of bituminous compositions has been proposed to overcome this drawback. For example, mention may be made of the organic or inorganic metal salts described in international application WO2005065177 as capable of trapping H 2 S. The method used to reduce H 2 S emissions consists of introducing an organic or inorganic metal salt into a reactor containing a premixed bitumen / polymer composition. The metal salt added in bulk to the reactor is then stirred in the reactor during the crosslinking reaction.

[0014] Document US2006081152 describes a composition comprising a bitumen base, an H2S scavenger selected from zinc, copper, iron or aluminum oxides.

[0015] The applicant was interested in the effectiveness of agents capable of neutralizing and / or trapping H 2 S in processes for preparing bituminous compositions, in particular bitumen / crosslinked polymer compositions using acidic mineral adjuvants.

[0016] The subject of the present invention relates to the improvement of the mechanical and dynamic properties, in particular the plasticity range of bituminous compositions while reducing the risks of H 2 S emissions during the preparation and / or use of such bituminous compositions.

[0017] Another object of the invention is to obtain bituminous compositions releasing small quantities of H 2 S, preferably quantities less than 10 ppm, more preferably less than or equal to 1 ppm during the preparation and / or use (transport, loading, unloading and storage) of such bituminous compositions, it being understood that the temperatures of preparation and / or use are conventionally between 90°C and 200°C and that the H 2 S content is measured according to a conventional method of titration of H 2 S in the liquid phase.

[0018] The present invention also relates to a process for preparing such bituminous compositions. BRIEF DESCRIPTION

[0019] In the context of the preparation of bituminous compositions, the applicant has discovered that, surprisingly, the use of an acid adjuvant has a negative effect on the effectiveness of certain agents capable of neutralizing and / or trapping hydrogen sulfide (H 2 S).

[0020] In particular, the applicant has demonstrated that the acid adjuvant deactivates said agents capable of neutralizing and / or trapping hydrogen sulfide (H 2 S).

[0021] The applicant has further discovered that the selection of certain specific agents capable of neutralizing and / or trapping hydrogen sulfide (H 2 S) makes it possible to overcome this drawback. The specific combination of an acid adjuvant and an agent capable of neutralizing and / or trapping hydrogen sulfide (H 2 S) makes it possible to obtain a bituminous composition with reduced H 2 S emissions while improving the mechanical and / or dynamic properties of said composition. The use of such a combination is particularly advantageous for bitumen / crosslinked polymer compositions.

[0022] The applicant has also discovered that, to obtain this combined effect, the agent capable of neutralizing and / or trapping hydrogen sulfide (H 2 S) and the acid adjuvant can be used together or successively, the order of introduction having no influence.

[0023] For reasons of simplification, the Anglo-Saxon term “H 2 S scavenger” will be systematically used in the remainder of this application to name an agent capable of neutralizing and / or trapping hydrogen sulfide (H 2 S).

[0024] Bituminous composition means any bitumen composition containing, in addition to bitumen, at least one other constituent, for example an elastomer and / or at least one additive.

[0025] According to the invention, the aim of the invention is achieved by a process for preparing a bituminous composition, this process comprising the treatment of a bitumen or a bituminous composition by: between 0.1% and 1% by mass of a H 2 S scavenger chosen from copper oxides and their mixtures with hydroxides, hydrates, carbonates, hydroxy-carbonates, carboxylates, nitrates and phosphates of copper, and an acid adjuvant chosen from phosphoric acids, polyphosphoric acids and their mixtures, the mass percentages being calculated in relation to the total mass of the bituminous composition, the H 2 S scavenger and the acid adjuvant being used separately.

[0026] According to the invention, the aim of the invention is also achieved by a process for preparing a bituminous composition, this process comprising the treatment of a bitumen or a bituminous composition by: between 0.1% and 1% by mass of a H 2 S scavenger chosen from copper oxides and their mixtures with hydroxides, hydrates, carbonates, hydroxy-carbonates, carboxylates, nitrates and phosphates of copper, and an acid adjuvant chosen from phosphoric acids, polyphosphoric acids and their mixtures, this process comprising the direct addition to the bitumen or to the bituminous composition of an additive composition comprising the H 2 S scavenger and the acid adjuvant, the mass percentages being calculated relative to the total mass of the bituminous composition.

[0027] The H2S scavenger is selected from copper oxides and their mixtures with copper hydroxides, hydrates, carbonates, hydroxycarbonates, carboxylates, nitrates and phosphates.

[0028] According to a particular preferred embodiment, the H 2 S scavenger is chosen from copper oxides and their mixtures.

[0029] According to the invention, the object of the invention is also achieved by the use of an H 2 S scavenger to reduce H 2 S emissions from bitumen or a bituminous composition treated with an acid adjuvant, said H 2 S scavenger and acid adjuvant being as described above.

[0030] According to a particular embodiment, the use of an H 2 S scavenger to reduce H 2 S emissions from bitumen or a bituminous composition treated with an acid adjuvant is such that the acid adjuvant and the H 2 S scavenger are in the form of an additive package as described above.

[0031] According to the invention, the aim of the invention is also achieved by a process for preparing a bituminous composition, in which bitumen, an acid adjuvant and an H 2 S scavenger are brought into contact, operating at temperatures between 90°C and 200°C, preferably between 120°C and 200°C, more preferably between 170°C and 190°C, and with stirring for a period of at least 10 minutes, advantageously at least 2 hours, preferably between 20 minutes and 6 hours, more preferably between 30 minutes and 2 hours, said H 2 S scavenger and acid adjuvant being as defined above.

[0032] According to a particular embodiment, the proportion of acid adjuvant is between 0.05% and 15% by mass, preferably between 0.05% and 5% by mass, more preferably between 0.05% and 2% by mass, the mass percentages being calculated relative to the total mass of the bituminous composition.

[0033] According to one variant, the method comprises heating the bitumen to a temperature between 90°C and 200°C, preferably between 120°C and 200°C, more preferably between 170°C and 190°C, for at least 10 minutes, preferably between 20 minutes and 6 hours, more preferably between 30 minutes and 2 hours with stirring followed by the addition of the acid adjuvant and the H 2 S scavenger, the reaction medium then being maintained at temperature for at least 10 minutes with stirring, preferably between 20 minutes and 6 hours, more preferably between 30 minutes and 2 hours.

[0034] Advantageously, the method further comprises a step of adding 0.5% to 10% by mass, preferably between 1% and 6% by mass, more preferably between 1.5% and 4% by mass of an elastomer, it being understood that the bituminous composition is then a bitumen / polymer composition and that the mass percentages are calculated relative to the total mass of the bitumen / polymer composition.

[0035] According to a particular preferred embodiment, the elastomer is chosen from sulfur-crosslinkable elastomers and the method further comprises a step of crosslinking said elastomer with a sulfur-donating coupling agent added in an amount suitable for providing from 0.1% to 20% by mass, advantageously from 1% to 10% by mass, preferably from 1% to 6% by mass, more preferably from 2% to 5% by mass of free sulfur relative to the mass of sulfur-crosslinkable elastomer in said composition, it being understood that the bituminous composition is then a crosslinked bitumen / polymer composition.

[0036] The sulfur-donating coupling agent is advantageously chosen from the group consisting of elemental sulfur, hydrocarbyl polysulfides, sulfur-donating vulcanization accelerators, mixtures of such products with each other and / or with non-sulfur-donating vulcanization accelerators.

[0037] According to a preferred variant, the elastomer is chosen from random or block copolymers of a monovinyl aromatic hydrocarbon and a conjugated diene.

[0038] The elastomer advantageously comprises between 5% and 50% by mass, preferably between 15% and 40% by mass of monovinyl aromatic hydrocarbon.

[0039] The elastomer is preferably chosen from random or block copolymers of styrene and a conjugated diene.

[0040] According to a particular development, the mass average molecular mass of the elastomer is between 10,000 and 600,000 daltons, preferably between 30,000 and 400,000 daltons.

[0041] According to the invention, the aim of the invention is also achieved by a bituminous composition capable of being obtained by the preparation process as defined above.

[0042] The invention also relates to a bituminous binder comprising a bituminous composition as defined above.

[0043] The invention also relates to an asphalt comprising a bituminous binder as described above, and mineral and / or synthetic fillers.

[0044] The invention further relates to a bituminous coating comprising a bituminous binder as described above, aggregates, and optionally mineral and / or synthetic fillers. DETAILED DESCRIPTION

[0045] Other advantages and characteristics will emerge more clearly from the description which follows and of which the particular embodiments of the invention are given as non-limiting examples.

[0046] According to a particular embodiment, a performance additive package comprises an acid adjuvant and an H 2 S scavenger.

[0047] An additive package is understood to mean a composition comprising at least two additives. The additive package may contain additives alone or dispersed / solubilized in an inert solvent, in particular of the mineral oil type, according to methods well known in the field of bitumen additives. In the field of additivation, the English term "package" is also commonly used to identify an additive composition. The term "additive concentrate" may also be used to designate the additive package, in particular when it is in the form of a solution.

[0048] Performance additives for bitumen or bituminous composition are understood to mean additives capable of being incorporated into a bituminous composition, for example in relation to their compatibility, solubility or stability in said bitumen or said bituminous composition and giving it improved properties compared to unadditified bitumen or bituminous composition. These properties may be mechanical and / or dynamic, and / or concern environmental and safety issues, for example issues of H 2 S emissions.

[0049] The acid adjuvant is chosen from phosphoric acids, polyphosphoric acids and their mixtures.

[0050] Various grades of phosphoric acid and / or polyphosphoric acid containing varying amounts of orthophosphoric acid are commercially available. Commercial phosphoric acids typically contain 50% to 200% orthophosphoric acid.

[0051] The term polyphosphoric acid refers to concentrated grades of phosphoric acid (H 3 PO 4 ) greater than 95%, typically ranging from 97% to 118%, where the percentage refers to the apparent H 3 PO 4 concentration. Polyphosphoric acid is represented by the formula H n+2 P n O 3n+1 where n ≥ 2. Polyphosphoric acid is typically a mixture of pyrophosphoric (n=2), triphosphoric (n=3), and higher acids (n>3). Phosphoric and polyphosphoric acids may contain other acids such as sulfuric and / or hydrofluoric acid as impurities at concentrations typically up to 2%.

[0052] The H2S scavenger is selected from copper oxides and their mixtures with copper hydroxides, hydrates, carbonates, hydroxycarbonates, carboxylates, nitrates and phosphates.

[0053] The mass ratio of the H 2 S scavenger to the acid adjuvant may advantageously be between 1:300 and 100:1, preferably between 1:10 and 10:1, more preferably between 1:10 and 5:1.

[0054] The performance additive package may consist solely of the H 2 S scavenger and the acid adjuvant, alone or in a mixture in one or more inert solvents, it being understood that said H 2 S scavenger and acid adjuvant may contain up to 2% by mass of impurities respectively, without it being considered that they are not used alone. The solvent must be inert with respect to the acid adjuvant and / or the H 2 S scavenger.

[0055] Generally, the quantity of solvent in the additive package is between 1% and 95%, preferably between 10% and 90%, more preferably between 20% and 80% by mass, even more preferably between 40% and 60%, the mass percentages being calculated relative to the total mass of said additive package.

[0056] The inert solvent(s) should preferably be chosen so as to solubilize both the H2S scavenger and the acid adjuvant. The solvent should be chosen, for example, from mineral oils.

[0057] Preferably, the additive package consists solely of the H 2 S scavenger and the acid admixture, the mass ratio of the H 2 S scavenger to the acid admixture being as described above. Such an additive package is storage stable and can be added directly during the preparation of the crosslinked bitumen / polymer composition.

[0058] The additive package can be used directly for the treatment of bitumen or bituminous compositions. In particular, the additive package can advantageously be used in the process for preparing bituminous compositions, preferably bitumen / polymer compositions, more preferably crosslinked bitumen / polymer compositions using a sulfur-donating coupling agent.

[0059] Alternatively, the H 2 S scavenger and the acid adjuvant as described above may be used separately for the treatment of bitumen or bituminous compositions, in particular for the preparation of bitumen / polymer compositions, preferably crosslinked bitumen / polymer compositions using a sulfur donor coupling agent.

[0060] According to a particular embodiment, a process for preparing a crosslinked bitumen / polymer composition comprises a treatment step with the acid adjuvant and the H 2 S scavenger described above at a temperature between 90°C and 200°C, preferably between 120°C and 200°C, more preferably between 170°C and 190°C, for a duration of at least 10 minutes, preferably between 20 minutes and 6 hours, more preferably between 30 minutes and 2 hours.

[0061] According to a particular embodiment, the process for preparing a crosslinked bitumen / polymer composition comprises, for example, the following steps: a bitumen and a sulfur-crosslinkable elastomer are introduced into a reactor, the mixture is stirred until a homogeneous bitumen / elastomer mixture is obtained and heated to a temperature of between 90°C and 200°C, preferably between 120°C and 200°C, more preferably between 170°C and 190°C, for a period of at least 10 minutes, preferably between 20 minutes and 6 hours, more preferably between 1 hour and 5 hours, said elastomer is crosslinked by adding a sulfur-donating coupling agent to the reaction medium in an amount suitable for providing from 0.1% to 20% by mass, advantageously from 1% to 10% by mass, preferably from 1% to 6% by mass, more preferably from 2% to 5% by mass of free sulfur, relative to the total mass of the elastomer and maintaining the reaction medium with stirring at a temperature between 90°C and 200°C, preferably between 120°C and 200°C, more preferably between 170°C and 190°C,for a period of at least 10 minutes, preferably between 20 minutes and 6 hours, more preferably between 30 minutes and 2 hours, the scavenger H 2 S described above is added, the reaction medium being maintained at a temperature of between 90°C and 200°C, preferably between 120°C and 200°C, more preferably between 170°C and 190°C, for a period of at least 10 minutes, preferably between 20 minutes and 6 hours, more preferably between 30 minutes and 2 hours, the acid adjuvant ... minutes and 6 hours, more preferably between 30 minutes and 2 hours.

[0062] According to another particular embodiment, the process for preparing a crosslinked bitumen / polymer composition comprises, for example, the following steps: a bitumen and a sulfur-crosslinkable elastomer are introduced into a reactor, the mixture is stirred until a homogeneous bitumen / elastomer mixture is obtained and heated to a temperature of between 90°C and 200°C, preferably between 120°C and 200°C, more preferably between 170°C and 190°C, for a period of at least 10 minutes, preferably between 20 minutes and 6 hours, more preferably between 1 hour and 5 hours, said elastomer is crosslinked by adding a sulfur-donating coupling agent to the reaction medium in an amount suitable for providing from 0.1% to 20% by mass, advantageously from 1% to 10% by mass, preferably from 1% to 6% by mass, more preferably from 2% to 5% by mass of free sulfur, relative to the total mass of the elastomer and maintaining the reaction medium with stirring at a temperature between 90°C and 200°C, preferably between 120°C and 200°C, more preferably between 170°C and 190°C,for a duration of at least 10 minutes, preferably between 20 minutes and 6 hours, more preferably between 30 minutes and 2 hours, , the acid adjuvant and the H 2 S scavenger described above are simultaneously added, the reaction medium being maintained at a temperature between 90°C and 200°C, preferably between 120°C and 200°C, more preferably between 170°C and 190°C, for a period of at least 10 minutes, preferably between 20 minutes and 6 hours, more preferably between 30 minutes and 2 hours.

[0063] The simultaneous addition of the H 2 S scavenger and the acid admixture has the advantage of reducing the preparation time of the crosslinked bitumen / polymer composition and improving the plasticity range of said composition. The additive package as described above can advantageously be used for the step of simultaneous addition of the acid admixture and the H 2 S scavenger.

[0064] For each step, the temperatures may or may not be the same.

[0065] The bitumen according to the present invention may comprise one or more bitumen bases. The bitumen bases may come from different sources. First of all, we can cite bitumen bases of natural origin, those contained in deposits of natural bitumen, natural asphalt or oil sands.

[0066] Bitumen bases may advantageously be derived from the refining of crude oil, preferably from atmospheric and / or vacuum distillation of oil. Bitumen bases may optionally be blown, visbroken and / or deasphalted.

[0067] Bitumen bases can be chosen from hard or soft grade bitumens. The different bitumen bases obtained by refining processes can be combined with each other to obtain the best technical compromise.

[0068] The bitumen bases used can also be chosen from bitumens fluxed by the addition of volatile solvents, fluxes of petroleum origin and / or fluxes of vegetable origin.

[0069] The bitumen is advantageously chosen from road bitumens of classes 10 / 20 to 160 / 220 and special bitumens of all classes.

[0070] The bitumen represents between 90% and 99.3% by mass, preferably between 94% and 99% by mass of the bitumen / crosslinked polymer composition.

[0071] The quantity of acid adjuvant added advantageously represents between 0.05% and 15% by mass, preferably between 0.05% and 5% by mass, more preferably between 0.05% and 2% by mass of the total mass of the crosslinked bitumen / polymer composition.

[0072] The amount of added H 2 S scavenger represents between 0.1% and 1% by mass of the total mass of the bitumen / crosslinked polymer composition.

[0073] In the particular embodiment described above, the acid adjuvant can be incorporated into the crosslinked bitumen / polymer mixture before or after the H 2 S scavenger, simultaneous incorporation can also be envisaged, in particular by adding a package of additives as described above in the crosslinked bitumen / polymer mixture.

[0074] The quantity of elastomer introduced into the reactor advantageously represents between 0.5% and 10% by mass, preferably between 1% and 6% by mass, more preferably between 1.5% and 4% by mass of the total mass of the crosslinked bitumen / polymer composition.

[0075] The mass average molecular weight of the elastomer is advantageously between 10,000 and 600,000 daltons, preferably between 30,000 and 400,000 daltons.

[0076] The elastomer is preferably chosen from random or block copolymers of a monovinyl aromatic hydrocarbon and a conjugated diene. In particular, the elastomer advantageously comprises between 5% and 50% by mass, preferably between 15% and 40% by mass of monovinyl aromatic hydrocarbon.

[0077] The elastomer is advantageously chosen from random or block copolymers of styrene and a conjugated diene such as butadiene, isoprene, chloroprene, carboxylated butadiene, carboxylated isoprene. Random or block copolymers of styrene and butadiene will preferably be chosen.

[0078] The elastomer may consist of one or more copolymers chosen from block copolymers, with or without a random hinge, of styrene and butadiene, of styrene and isoprene, of styrene and chloroprene, of styrene and carboxylated butadiene or of styrene and carboxylated isoprene.

[0079] Preferably, the copolymer of styrene and conjugated diene is chosen from di- or triblock copolymers of styrene and butadiene, styrene and isoprene, styrene and carboxylated butadiene or styrene and carboxylated isoprene which have styrene contents and mass-average molecular masses situated in the ranges defined above.

[0080] According to one variant, the elastomer is chosen from random or block copolymers of styrene and butadiene containing from 50% to 95%, more particularly from 60% to 95% by mass of units derived from butadiene. In addition, the proportion of 1,2-double bond units derived from butadiene may, advantageously, be between 12% and 50% by mass of said copolymer. The elastomer may, for example, be a styrene / butadiene copolymer of high vinyl type, i.e. having a content of 1,2-double bonds derived from butadiene greater than 20% by mass of said copolymer.

[0081] The sulfur donor coupling agents that can be used are of a very varied nature and are chosen according to the elastomer to be crosslinked in the crosslinked bitumen / polymer composition.

[0082] The sulfur-donating coupling agent is advantageously chosen from the group consisting of elemental sulfur, hydrocarbyl polysulfides, sulfur-donating vulcanization accelerators, mixtures of such products with each other and / or with non-sulfur-donating vulcanization accelerators.

[0083] The elemental sulfur that may be used to constitute, in part or in whole, the crosslinking agent is, advantageously, flower sulfur and, preferably, crystallized sulfur in the orthorhombic form and known as alpha sulfur.

[0084] The vulcanization accelerators are either hydrocarbyl polysulfides, or sulfur-donating vulcanization accelerators, or non-sulfur-donating vulcanization accelerators. The hydrocarbyl polysulfides may be chosen from those defined in patent FR2528439 cited as an example and / or incorporated by reference in the present application. The sulfur-donating vulcanization accelerators may be chosen from thiuram polysulfides, such as, for example, tetrabutylthiuram disulfides, tetraethylthiuram disulfides and tetramethylthiuram disulfides. The non-sulfur-donating vulcanization accelerators that can be used may be sulfur compounds chosen in particular from mercaptobenzothiazole and its derivatives, dithiocarbamates and its derivatives, and thiuram monosulfides and its derivatives.

[0085] Examples that may be mentioned include zinc-2-mercaptobenzothiazole, zinc dibutyldithiocarbamate, tetramethylthiuram monosulfide. For further details on the sulfur-donating and non-sulfur-donating vulcanization accelerators that can be used according to the invention, reference may be made to patents EP0360656, EP0409683 and FR2528439 cited as examples and / or incorporated by reference in the present application.

[0086] Adhesive dopes and / or surfactants may also be added to the crosslinked bitumen / polymer composition according to any known method. They are generally chosen from alkylamine derivatives, alkylpolyamine derivatives, alkylamidopolyamine derivatives, alkyl amidopolyamine derivatives and quaternary ammonium salt derivatives, taken alone or as a mixture. The amount of adhesive dopes and / or surfactants in the crosslinked bitumen / polymer composition is, for example, between 0.2% and 2% by mass, preferably between 0.5% and 1% by mass relative to the total mass of the crosslinked bitumen / polymer composition.

[0087] The order of introduction of the different constituents does not appear to have any influence on the mechanical and / or dynamic properties of the bitumen / crosslinked polymer composition thus obtained. However, it is preferable to add the elastomer before or at the same time as the sulfur-donating coupling agent for better homogeneity of the composition.

[0088] According to one variant, the elastomer and the sulfur-donating coupling agent may be introduced simultaneously in the form of a mother solution, according to any known method, during the process for preparing the crosslinked bitumen / polymer composition. The mother solution generally comprises a hydrocarbon oil serving as a fluidizer, from 5% to 40% by mass of elastomer and from 0.02% to 15% by mass of coupling agent, preferably from 10% to 35% by mass of elastomer and from 0.1% to 5% by mass of coupling agent.

[0089] The crosslinked bitumen / polymer compositions can be used as they are or diluted, according to any known process, with variable proportions of bitumen or of a composition according to the invention having different characteristics to constitute bitumen / polymer binders having a chosen content of crosslinked elastomer, which can be either equal (undiluted composition) or lower (diluted composition) than the content of crosslinked elastomer of the corresponding initial bitumen / polymer compositions.

[0090] Generally, the dilution of the crosslinked bitumen / polymer compositions can be carried out either directly after obtaining said compositions, when almost immediate use of the resulting bitumen / polymer binders is required, or even after a more or less prolonged storage period of the crosslinked bitumen / polymer compositions, when deferred use of the resulting bitumen / polymer binders is envisaged. The bitumen for the dilution of a crosslinked bitumen / polymer composition according to the invention can be chosen from the bitumens described above. Where appropriate, the bitumen used for the dilution may itself have been previously treated with an acid adjuvant and / or an H 2 S scavenger according to the invention.

[0091] The crosslinked bitumen / polymer compositions obtained by the preparation process described above have improved mechanical and dynamic properties, in particular a reinforced multigrade character. Reinforced multigrade character means that these crosslinked bitumen / polymer compositions have a wide plasticity range. Said range is defined as the difference between the ring and ball softening temperature, which indicates the hot properties of the binder or bitumen / polymer composition, and the Fraass brittleness point, which indicates the cold properties of the crosslinked bitumen / polymer composition. The bituminous binder consisting of / or based on the crosslinked bitumen / polymer composition will be more resistant to hot and cold stresses as the plasticity range is wider.

[0092] More generally, the bituminous compositions obtained by the preparation process according to the present invention have improved mechanical and dynamic properties, in particular a better consistency, with lower needle penetrability at 25°C and / or a higher ring-ball temperature.

[0093] Furthermore, at preparation and / or use temperatures (transport, loading, unloading and storage) conventionally between 90°C and 200°C, H 2 S emissions from bituminous compositions, in particular from the bitumen / crosslinked polymer compositions according to the invention, are greatly reduced. The H 2 S level emitted is, in particular, less than 10 ppm, more preferably less than or equal to 1 ppm, the H 2 S level being measured according to a conventional method of titrating H 2 S in the liquid phase.

[0094] Various uses of the bituminous compositions obtained according to the invention are envisaged. In particular, the bituminous compositions, in particular the bitumen / polymer compositions and the crosslinked bitumen / polymer compositions according to the invention can be used for the preparation of bituminous binders.

[0095] According to a particular embodiment, a bituminous binder comprises a bituminous composition as described above.

[0096] The bituminous binder according to the invention can in turn be used to prepare an association with aggregates, particularly road aggregates.

[0097] With regard to road applications, the invention relates in particular to bituminous coatings as materials for the construction and maintenance of road surfaces and their surfacing, as well as for carrying out all road works.

[0098] Bituminous coating means a mixture of a bituminous binder with aggregates and, possibly, mineral and / or synthetic fillers.

[0099] The bituminous mix comprises a bituminous binder as described above, and optionally mineral and / or synthetic fillers, preferably chosen from fines, sand, gravel and recycled millings. The aggregates are mineral and / or synthetic aggregates, in particular recycled millings, with dimensions greater than 2 mm, preferably between 2 mm and 20 mm.

[0100] The bituminous binder described above can advantageously be used to prepare a surface dressing, a hot mix, a cold mix, a cold-poured mix or an emulsion gravel.

[0101] With regard to road applications, the invention also relates to asphalts as materials for manufacturing and covering sidewalks.

[0102] Asphalt means a mixture of bituminous binder with mineral and / or synthetic fillers.

[0103] An asphalt comprises a bituminous binder as described above and mineral fillers such as fines, sand or gravel and / or synthetic fillers. The mineral fillers consist of fines (particles with dimensions less than 0.063 mm), sand (particles with dimensions between 0.063 mm and 2 mm) and possibly gravel (particles with dimensions greater than 2 mm, preferably between 2 mm and 4 mm).

[0104] Asphalts have 100% compaction and are primarily used to make and cover pavements, while asphalts have a compaction of less than 100% and are used to make roads. Unlike asphalts, asphalts are not compacted with a roller during installation.

[0105] Another aspect of the invention is the use of a bituminous composition, preferably a crosslinked bitumen / polymer composition in various industrial applications, in particular for preparing a waterproofing coating, a membrane or an impregnation layer.

[0106] Industrial applications of bituminous compositions include the preparation of waterproofing membranes, noise-reducing membranes, insulation membranes, surface coatings, carpet tiles, and impregnation layers. EXAMPLES

[0107] The invention is illustrated by the following examples given without limitation.

[0108] In these examples, quantities and percentages are expressed by mass unless otherwise indicated.

[0109] For the record, throughout this application, the following properties of bitumens are measured as shown in Table 1 below: Table 1 Property Abbreviation Unit Measurement standard Needle penetration at 25°C P25 1 / 10mm IN 1426 Ring and ball softening temperature TBA °C IN 1427 FRAASS Fragility Point Fraass °C EN 12593 Bitumen

[0110] The bitumen used is derived from vacuum residues from the direct distillation of crude oil. The bitumen has a P25 of 43 1 / 10 mm. Elastomer

[0111] Styrene / butadiene / styrene block copolymer, with 30.5% by weight of styrene and 69.5% by weight of butadiene. The 1,2-vinyl group content is 27.8% by weight relative to the total weight of copolymer. The copolymer has a molecular weight (Mw) of 142,500 Daltons and a polydispersity index I p of 1.09. Acid adjuvant

[0112] Polyphosphoric acid 115%, noted PPA; CAS No. 8017-16-1. Sulfur-donating coupling agent

[0113] Flowering sulfur; CAS No. 7704-34-9. Scavenger

[0114] The characteristics of the different S x scavengers tested are listed in the following table 2: Table 2 Scavenger SX Reference Product Trade Name / Supplier CAS No. S 1 Zinc carboxylate Nalco S 2 Copper (II) hydroxycarbonate Merck 12069-69-1 S 3 Magnesium hydroxycarbonate VWR International 12125-28-9 S 4 Calcium carbonate Sigma-Aldrich 471-34-1 S 5 Zinc oxide VWR International 1314-13-2 S 6 Calcium oxide Aldrich 1305-78-8 S 7 Magnesium oxide VWR International 1309-48-4 S 8 Copper (II) oxide VWR International 1317-38-0 Bitumen / crosslinked polymer compositions C 1 à C 8

[0115] The bitumen / crosslinked polymer compositions C 1 to C 8 are prepared according to a preparation process involving the following three steps: First step: preparation of bitumen compositions / crosslinked polymer without PPA: C° 1 à C° 9

[0116] The following are introduced into the reactor: 97.71% by mass of bitumen, 2.22% by mass of elastomer,

[0117] The mixture is stirred at high density, i.e. at high shear rate, to obtain a homogeneous mixture at the micron scale and heated to 185°C for approximately 4 hours.

[0118] Then 0.07% by mass of the sulfur donor coupling agent is added.

[0119] The mixture is stirred at low intensity and heated to 185°C for 2 hours.

[0120] The percentages of each of the constituents are calculated in relation to the mass of the crosslinked bitumen / polymer composition resulting from the first stage. Second step : treatment of H emissions 2 S to obtain bitumen compositions / PPA-free crosslinked polymer with scavenger : C s < 1 à C s < 9

[0121] The second step consists of adding 0.2% by mass of the scavenger S x . The scavenger S x is introduced into the reactor and then the mixture is stirred while maintaining the temperature at 185°C for 20 minutes. The percentage of scavenger S x is calculated relative to the mass of the bitumen / crosslinked polymer composition from the second step.

[0122] For compositions C s < 1 to C s < 8 , the scavenger S x was added directly into the reactor, without prior dissolution.

[0123] For composition C s < 9, scavenger S 2 was added in solution at 20% by mass in a mineral oil. Third step : acid treatment with PPA to obtain bitumen compositions / crosslinked polymer with PPA and scavenger : C 1 à C 8

[0124] The third step consists of adding 0.8% by mass of PPA to the reaction medium. The PPA is introduced into the reactor and then the mixture is stirred while maintaining the temperature at 185°C for 30 minutes. The percentage of PPA is calculated relative to the mass of the bitumen / crosslinked polymer composition resulting from the third step.

[0125] The quantities used are as follows: 967.3 g of bitumen, 22 g of elastomer, 0.7 g of sulfur, 2 g of scavenger S x and 8 g of PPA. Measurement of H emissions 2 S

[0126] The measurement of H 2 S emissions is carried out using a conventional H 2 S titration method. The measurement of H 2 S emissions consists of bubbling nitrogen gas through the bitumen / crosslinked polymer composition to be tested, maintained at 185°C, followed by measurement of the rate of H 2 S trapped in the nitrogen gas using a H 2 S gas detector. The calculation of the H 2 S concentration in the liquid phase is based on the initial mass of the bitumen / crosslinked polymer composition being tested.

[0127] This measurement is not intended to be representative of the rate of H 2 S present in the gaseous sky in real time but aims to compare the efficiency of scavengers used in identical conditions, by determining the presence or absence of H 2 S release. Thus, we have set a limit threshold for H 2 S release above which we consider that the efficiency of the scavenger is not sufficient. This method also makes it possible to highlight the phenomenon of deactivation of certain scavengers in the presence of an acid adjuvant.

[0128] H2S emissions are measured after each of the three steps described above. The results are listed in Table 3 below. Table 3 PmB PmB + SX PmB + SX + PPA C° X H2S (ppm) CS< x H2S (ppm) C x H2S (ppm) C° 1 >100 CS< 1 <1* C 1 >100 C° 2 >100 CS< 2 <1* C 2 <1* C° 3 >100 CS< 3 >100 C 3 >100 C° 4 >100 CS< 4 >100 C 4 >100 C° 5 >100 CS< 5 >100 C 5 >100 C° 6 >100 CS< 6 >100 C 6 >100 C° 7 >100 CS< 7 >100 C 7 >100 C° 8 >100 CS< 8 <1* C 8 (°) <1* C° 9 >100 CS< 9 <1* C 9 <1* * detection limit of the H 2 S gas detector (°) according to the invention

[0129] In view of the results collected in Table 3, we can make the following remarks: In the first step of the process for preparing the bitumen / polymer composition C° x , the sulfur crosslinking of the elastomer is accompanied by the release of H 2 S. The measured H 2 S levels exceed the limit threshold of 100 ppm. In the second step treatment, scavengers S 1 to S 8 can be differentiated according to their effectiveness in trapping and / or neutralizing H 2 S. For the crosslinked bitumen / polymer composition C s < 3 , C s < 4 , C s < 5 , C s < 6 or C s < 7 , the addition of 0.2% by mass of the scavenger S 3 , S 4 , S 5 , S 6 or S 7 respectively is not sufficient to reduce the release of H 2 S to a level below 100 ppm. Scavengers S 3 , S 4 , S 5 , S 6 and S 7 are therefore found to be ineffective scavengers for reducing H 2 S emissions in bitumen / crosslinked polymer compositions. On the other hand, scavengers S 1 , S 2 and S 8 are particularly effective.H 2 S emissions from bitumen / crosslinked polymer compositions C s < 1 , C s < 2 and C s < 8 can be reduced to a level below the detection limit of the H 2 S gas detector (1 ppm).

[0130] Furthermore, it is noted that the addition of the scavenger S 2 in solution in a mineral oil does not degrade the effectiveness of said scavenger in reducing the H 2 S emissions of the bitumen / crosslinked polymer composition C s < 9 . During the acid treatment of the third stage, the measured level of H 2 S in the bitumen / crosslinked polymer composition C 1 is, surprisingly, significantly higher than the limit threshold of 100 ppm whereas the measurement carried out after the second stage on the bitumen / crosslinked polymer composition C s < 1 had revealed almost no presence of H 2 S (<1 ppm). This increase in the level of H 2 S before and after the third stage (20 min after the introduction of the PPA) reflects a phenomenon of release of H 2 S responsible for the deactivation of the scavenger S 1 .

[0131] Furthermore, this H 2 S release phenomenon is also observed for the bitumen / crosslinked polymer compositions C s < 3 , C s < 5 and C s < 6 comprising respectively the scavengers S 3 , S 5 and S 6 . Indeed, a significant increase in the H 2 S rate (ΔH 2 S ≥ 100 ppm) is observed, before and after the third stage (30 min after the introduction of the PPA).

[0132] Thus, the results highlight that the addition of PPA deactivates the scavengers S 1 , S 3 , S 5 , S 6 and produces a phenomenon of release of H 2 S in the bitumen / crosslinked polymer composition C 1 , C 3 , C 5 , and C 6 .

[0133] For the bitumen / crosslinked polymer compositions C s < 4 and C s < 7 comprising, respectively, the scavengers S 4 and S 7 , it is not possible to rely on these measurements to decide on the presence of a phenomenon of deactivation of the scavenger by the PPA since the scavengers S 4 and S 7 are not sufficiently effective as H 2 S scavengers. The effectiveness of the S 2 and S 8 scavengers is particularly remarkable in the presence of PPA since it is possible to eliminate almost all H 2 S emissions in the C 2 and C 8 bitumen / crosslinked polymer compositions.

[0134] Furthermore, the presence of PPA does not degrade the effectiveness of the S 2 and S 8 scavengers because no H 2 S release phenomenon is observed in the C 2 and C 8 bitumen / crosslinked polymer compositions. The S 2 and S 8 scavengers are therefore compatible with an acid treatment of a bitumen / crosslinked polymer composition, in particular, a treatment with PPA.

[0135] Furthermore, the effectiveness of the scavenger S 2 is maintained after treatment with PPA when said scavenger is added in solution in a mineral oil (bitumen / crosslinked polymer composition C 9 ).

[0136] In conclusion, inorganic or organic copper salts are particularly effective compared to other inorganic or organic metallic salts as H 2 S scavengers from bitumen / crosslinked polymer compositions using acid treatment, in particular, treatment with PPA. Properties of crosslinked bitumen / polymer compositions

[0137] The characteristics of the different bitumen / crosslinked polymer compositions measured according to the standards cited above are recorded in the following table 4: Table 4 Composition Bitumen / crosslinked polymer CS< 1 C 1 C 2 C 8 (°)< Scavenger H 2 S S 1 S 1 S 2 S 8 PPA presence yes / no No Yes Yes Yes P25 (1 / 10mm) 34 31 27 28 TBA (°C) 62 65,4 68,4 66,8 Fraass (°C) -8 -12 -10 -9 Plasticity interval (ΔTBA- Fraass) 70 77,4 78,4 75,8 (°) according to the invention

[0138] Comparison of TBA and Fraass results of bitumen / crosslinked polymer compositions CS<1 and C confirms the increase in the plasticity range due to acid treatment with PPA described in the prior art.

[0139] The use of scavenger S 2 on the one hand, and the use of scavenger S 8 according to the present invention on the other hand, does not affect the effect of the acid treatment on the mechanical and dynamic properties of the crosslinked bitumen / polymer composition, in particular on the plasticity range. On the contrary, the crosslinked bitumen / polymer composition C 2 has a widened plasticity range compared to that of the crosslinked bitumen / polymer composition C 1 . As for the plasticity range of the composition C 8 , it remains comparable to that of the composition C 1 . Using an additive package scavenger H 2 S / acid adjuvant: effect on H emissions 2 S and on the properties of bitumen / crosslinked polymer compositions Preparation of P additive packages 2 and P 8 :

[0140] Two additive packages P 2 and P 8 are prepared by mixing 20% ​​by mass of scavenger S 2 (package P 2 ) or S 8 (package P 8 ) and 80% by mass of PPA. Scavengers S 2 and S 8 are soluble in PPA and additive packages P 2 and P 8 are in the form of a homogeneous solution. Preparation of crosslinked bitumen / polymer compositions C' 2 etc' 8 :

[0141] Crosslinked bitumen / polymer compositions C' 2 and C' 8 were prepared by adding respectively the additive package P 2 (composition C' 2 ) or P 8 (composition C' 8 ) to the crosslinked bitumen / polymer composition C° 2 or C° 8 obtained at the end of the first step as described previously. Measurement of H emissions 2 S :

[0142] The measurement of H 2 S emissions is carried out after the preparation of the crosslinked bitumen / polymer composition (first step) and after the addition of the additive package. The results are listed in Table 5 below. Table 5 PmB PmB + Additive Pack C° x H2S (ppm) C x H2S (ppm) C° 2 >100 C' 2 <1* C° 8 >100 C' 8 (°) <1* (°) according to the invention

[0143] In view of the previous results, it is noted that the addition of the additive package P 2 or P 8 at the end of the first step of the process for preparing the bitumen / crosslinked polymer composition C° 2 or C° 8 does not degrade the effectiveness of the scavenger in trapping H 2 S emissions. Indeed, no H 2 S release phenomenon is observed in the bitumen / crosslinked polymer compositions C' 2 and C' 8 . The scavengers S 2 and S 8 and the PPA can therefore be introduced at once in the form of an additive package, which makes it possible to shorten the preparation time of a bitumen / crosslinked polymer composition while reducing H 2 S emissions. Properties of crosslinked bitumen / polymer compositions :

[0144] The characteristics of the different bitumen / crosslinked polymer compositions measured according to the standards cited above are listed in Table 6 below: Table 6 Composition Bitumen / crosslinked polymer C 1 C 2 C 8 (°) C' 2 C' 8 (°) Scavenger H 2 S S 1 S 2 S 8 S 2 S 8 PPA presence yes / no Yes Yes Yes Yes Yes P25 (1 / 10mm) 31 27 28 23 22 TBA (°C) 65,4 68,4 66,8 71 70,4 Fraass (°C) -12 -10 -9 -10 -10 Plasticity interval (ΔTBA- Fraass) 77,4 78,4 75,8 81 80,4 (°) according to the invention

[0145] The addition of the additive package P 2 or P 8 does not affect the effect of acid treatment on the mechanical and dynamic properties of the crosslinked bitumen / polymer composition, in particular on the plasticity range. On the contrary, the crosslinked bitumen / polymer compositions C' 2 and C' 8 have a widened plasticity range compared to that of the crosslinked bitumen / polymer composition C 1 .

[0146] In conclusion, the process for preparing the crosslinked bitumen / polymer compositions according to the invention makes it possible to substantially reduce the release of hydrogen sulfide (H 2 S) in the presence of an acidic adjuvant, while having mechanical and dynamic properties comparable to those of the crosslinked bitumen / polymer compositions of the prior art.

Claims

1. A method for preparing a bituminous composition, this method comprising treatment of bitumen or of a bituminous composition with: - between 0.1 and 1 weight % of H2S scavenger chosen from among copper oxides and mixtures thereof with copper hydroxides, hydrates, carbonates, hydroxycarbonates, carboxylates, nitrates, and phosphates; and - an acid additive chosen from among phosphoric acids, polyphosphoric acids and mixtures thereof, the weight percentages being calculated relative to the total weight of the bituminous composition, the H2S scavenger and acid additive being used separately.

2. A method for preparing a bituminous composition, this method comprising treatment of bitumen or of a bituminous composition with: - between 0.1 and 1 weight % of H2S scavenger chosen from among copper oxides and mixtures thereof with copper hydroxides, hydrates, carbonates, hydroxycarbonates, carboxylates, nitrates, and phosphates, and - an acid additive chosen from among phosphoric acids, polyphosphoric acids and mixtures thereof; this method comprising the direct addition to the bitumen or bituminous composition of a composition of additives comprising the H2S scavenger and acid additive, the weight percentages being calculated relative to the total weight of the bituminous composition.

3. The method according to either of claims 1 and 2 for preparing a polymer / bitumen composition.

4. The method according to claim 3, for preparing a Polymer-modified Bitumen composition using a sulfur-donor coupling agent.

5. The method for preparing a bituminous composition according to any of claims 1 to 4, characterized in that the bitumen, acid additive and H2S scavenger are placed in contact, operating at temperatures of between 90 °C and 200 °C and under agitation for a time of at least 10 minutes.

6. The method according to any of claims 1 to 5, characterized in that the proportion of acid additive is between 0.05 and 15 weight %, the weight percentages being calculated relative to the total weight of the bituminous composition.

7. The method according to any of claims 1 to 6, characterized in that the H2S scavenger is chosen from among copper oxides.

8. The method according to any of claims 4 to 7, characterized in that it comprises heating the bitumen to a temperature of between 90°C and 200°C for a time of at least 10 minutes under agitation, followed by addition of the acid additive and H2S scavenger, the temperature of the reaction medium then being held for a time of at least 10 minutes under agitation, and in that said method further comprises a step to add from 0.5 to 10 weight % of an elastomer, on the understanding that the bituminous composition is then a polymer / bitumen composition and the weight percentages being calculated relative to the total weight of the polymer / bitumen composition:

9. The method according to claim 8, characterized in that the elastomer is chosen from among sulfur-crosslinkable elastomers, and in that the method further comprises a step to crosslink said elastomer with a sulfur-donor coupling agent added in an amount suitable for providing from 0.1 to 20 weight % of free sulfur relative to the weight of sulfur-crosslinkable elastomer in said composition, on the understanding that the bituminous composition is then a crosslinked Polymer-modified Bitumen composition.

10. The method according to any of claims 4 to 9, characterized in that the sulfur-donor coupling agent is chosen from the group formed by elementary sulfur, hydrocarbyl polysulfides, sulfur-donor vulcanization accelerators, mixtures of said products with each other and / or with non-sulfur-donor vulcanization accelerators.

11. The method according to any of claims 8 to 10, characterized in that the elastomer is chosen from among statistical or block copolymers of an aromatic monovinyl hydrocarbon and a conjugated diene, preferably from among statistical or block copolymers of styrene and a conjugated diene.

12. A bituminous composition able to be obtained with the preparation method as defined in any of claims 1 to 11.

13. An asphalt, characterized in that it comprises a bituminous composition according to claim 12 and mineral and / or synthetic fillers.

14. An asphalt mix characterized in that it comprises a bituminous composition according to claim 12 and aggregates, and optionally mineral and / or synthetic fillers.