STEEL, PRODUCT MADE FROM STEEL AND METHOD FOR MANUFACTURING IT

DE602016090413T2Active Publication Date: 2024-11-27APERAM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE602016090413
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2015-10-15
Filing Date
2016-10-17
Publication Date
2024-11-27
Estimated Expiration
2036-10-17

AI Technical Summary

Technical Problem

Existing maraging steels are costly due to high content of expensive elements like Co and Mo, while maintaining high mechanical properties and surface treatment benefits for fatigue resistance, necessitating a cost-effective composition that retains superior mechanical and surface properties.

Method used

A new maraging steel composition with reduced Co and Mo content, supplemented by hardening elements like Cu, Nb, Mn, Si, and others, achieving a martensitic structure and controlled inclusion population through precise thermomechanical treatments and production processes to maintain mechanical performance and nitriding benefits.

Benefits of technology

The new composition achieves a balance of low material cost with high mechanical properties and enhanced surface treatment effects, such as improved fatigue resistance and surface hardness, while controlling inclusions to prevent degradation, thus delaying cracking under cyclic stress.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to the field of so-called "maraging" steels, used in particular for applications requiring one or more of the following properties: excellent mechanical properties (very good fatigue resistance, high elastic limit and high breaking strength), simplicity of heat treatment and dimensional stability following these treatments, ease of welding and good formability.

[0002] These maraging steels are characterized by a martensitic structure, which can be aged, so as to obtain, after aging of the steel, a hardening by precipitation of intermetallic phases favorable to obtaining high mechanical properties.

[0003] Maraging steels are conventionally known, of type M 250, with a typical composition (expressed in weight percentages, as will be all the compositions given subsequently) Ni = 18%, Co = 9%, Ti = 0.45% (grade called X2NiCoMo18-9-5), containing Ti as a hardening element, the remainder generally being iron and impurities resulting from the production. They are used to produce, in particular, parts with high properties, suitable for use both as solid parts (engine shafts, centrifuge blades, etc.) and as high-performance precision parts: springs for watchmaking, blades for foils, elements of automatic transmission belts of the CVT (Continuous Variable Transmission) type for, in particular, automobiles or vehicles in general, or machine tools or other rotating machines, etc.In the case of applications where the part is subjected to fatigue stress, it is usual to carry out, in addition to aging, a surface treatment to harden the part by nitriding, carbonitriding, shot blasting, carburizing.

[0004] Also known from document EP-B1-1 339 880 are Ti-free maraging steels whose composition is: Ni = 12 to 24.5%; Mo = 2.5%; Co = 4.17%; Al ≤ 0.15%; Ti ≤ 0.1%; N ≤ 30 ppm; Si ≤ 0.1%; Mn ≤ 0.1%; C ≤ 50 ppm; S ≤ 10 ppm; P ≤ 50 ppm; H ≤ 3 ppm; O ≤ 10 ppm; the remainder being Fe and impurities resulting from the production, with Ni + Mo between 20 and 27%; Co% x Mo% between 50 and 200; Ti% x N% ≤ 2.10 -4< , which are produced by methods including vacuum remelting treatments such as VIM (Vacuum Induction Melting) and / or VAR (Vacuum Arc Remelting), possibly coupled with electroslag remelting treatment ESR (ElectroSlag Remelting). These steels are then hot and cold processed to obtain thin strips (1 mm or less for example).After shaping the part, a precipitation hardening treatment is carried out which gives the part its core mechanical properties; a subsequent surface treatment can give the part increased surface properties concerning fatigue stress, static friction and dynamic friction.

[0005] Documents EP 2 412 836 A1, EP 2 180 073 B1, JP 2007 186 780, JP 2008 088540 A and JP H 01 142021 A also relate to maraging steels.

[0006] Compared to previously known maraging steels containing approximately 18% Ni, 9% Co, 5% Mo, 0.5% Ti, and a little AI, these EP-B1-1 339 880 steels are distinguished by superior fatigue resistance (in the aged nitrided state), associated with controlled inclusion cleanliness and fatigue endurance. In more detail: the mechanical properties on cold rolled product targeted are Ar > 2.5%, Rp 0.2 < 1140 MPa, Rm < 1480 MPa; on aged state, Rp 0.2 > 1770 MPa, Rm > 1800 MPa; finally on nitrided state the targeted properties are Ar > 1%; Rm > 1930 MPa.

[0007] Also known from document EP-B1-2 180 073 are maraging steels with high fatigue strength and tensile strength intended for CVT belts, of composition: C ≤ 100 ppm; Si ≤ 0.1%; Mn ≤ 0.1%; P ≤ 0.01%; S ≤ 50 ppm; Ni = 17 - 22%; Cr = 0.1-4.0%; Mo = 3.0-7.0%; Co = 10.0-20.0%; Ti ≤ 0.1%; Al ≤ 0.05%; N ≤ 300 ppm; O ≤ 50 ppm; 0 < B ≤ 0.01%; an optional presence of up to 0.01% Ca, up to 0.005% Mg, up to 0.01% Zr, the remainder being Fe and impurities, with Co / 3 + Mo + 4AI between 8.0 and 15.0%. Preferably the thermal and thermomechanical treatments undergone give them a very fine grain, of ASTM 10 or more.

[0008] Also known from patent application PCT / IB2015 / 052975 in the name of the applicant are maraging steels combining a low carbon composition and a controlled inclusion population, with a Co content of between 1 and 25% and a Mo content of between 1 and 12%. The sum of Mo + Co to which hardening elements can be added is between 20 and 29%, and the sum of Ni + Co + Mo is at least 29%. The most recommended contents of expensive elements, however, remain relatively high.

[0009] The aim of the invention is to propose a new type of maraging steel which has the lowest possible material cost combined with high mechanical properties. In other words, for an application in which the final product would be particularly stressed in fatigue, the steel should have the best possible compromise between a relatively low material cost and very good intrinsic mechanical characteristics, combined with excellent surface properties, concerning the nitriding behavior for example, such as, in particular, the steels just described. Sufficient tensile strength and / or fatigue resistance for the aforementioned applications would be desirable properties, combined with increased surface properties, in particular the ability to form, during a surface treatment, a nitrided, carbonitrided, case-hardened, shot-peened or other layer.This layer must be capable of introducing residual stresses on the surface to delay cracking under cyclic stress for compression of the surface layers. The effect of surface treatments can also be evaluated, for example, through the hardness imparted to the product on the surface, the relative level of residual stresses and the nature of the phases formed.

[0010] For this purpose, the invention relates to a steel according to claim 1.

[0011] The invention also relates to a steel product according to claim 2 or according to claim 3.

[0012] The invention also relates to a cold-rolled sheet or strip according to claim 4.

[0013] Claims 5 and 6 describe particular characteristics of the cold-rolled sheet or strip.

[0014] The invention also relates to a steel product according to claim 7 or according to claim 8.

[0015] The invention also relates to a turbine shaft according to claim 9 or a transmission part according to claim 10.

[0016] The invention also relates to a transmission belt according to claim 11 or according to claim 12.

[0017] The invention also relates to a steel product according to claim 13.

[0018] As will be understood, the invention consists, in order to achieve the savings sought compared to the known prior art, in lowering the maximum obligatory or preferred contents of certain elements such as Co, or even Mo, compared to what was previously recommended, and in compensating for this reduction by the obligatory presence at defined contents of hardening elements of the type, Cu, Nb, Mn, Si, AI, Ta, V, W and others which are not systematically used usually. These grades allow predominantly martensitic structures typical of maraging steels, or also mixed austenitic-ferritic structures.The invention consists of a compromise between material cost and mechanical performance, conferred by mechanical performance due to the composition of the steel and the thermomechanical or thermal treatments it undergoes, combined with a controlled population of non-metallic inclusions (mainly oxides, sulfides, nitrides), meeting precise criteria of number, distribution, size distribution and composition.

[0019] This population can be obtained after careful preparation of the liquid metal through a combination of different preparation processes and conditions controlled by the operators. In particular, it is advisable to use new or not yet too degraded refractory linings in containers such as the melting furnace and the liquid metal treatment ladles, and, to prevent reoxidation and re-nitriding, to avoid contact between the liquid metal and the atmosphere by using vacuum treatments, and also neutral protective gases (argon) when the metal is exposed to air or risks being exposed.It is also necessary to properly control the agitation of the liquid metal in the production containers where it is carried out (by electromagnetic means or by injection of neutral gas, in particular), so as to accelerate the decantation of the inclusions without, in return, capturing oxidized or other impurities due, in particular, to erosion of the refractories or capture of impurities torn from the slag above the liquid metal. These precautions are known in themselves to those skilled in the art, but it is important that they are applied to the best of the known state of the art, within the framework of the invention, so that the threshold of acceptability of the presence of inclusions of oxides, nitrides or sulfides in the final product, as set according to the invention, is not exceeded.

[0020] It also turns out that the steels according to the invention, in particular when they are rich in Cr or Mn or, above all, in Cr and Mn, lend themselves particularly well to the subsequent production of a nitrided layer whose mechanical behavior (low plastic deformation capacities) provides significant advantages, in particular when these steels are used primarily to manufacture CVT transmission belt elements. Cu and Nb are also favorable from this point of view.

[0021] The invention will be better understood upon reading the following description, given with reference to the following appended figures: There figure 1 illustrates the hardening precipitates obtained on sample Inv 15 after gas nitriding by characterization using a transmission electron microscope on a thin section; figure 2 which shows a characterization of the nitrided layers by their surface micro-hardness levels, carried out on reference samples and on samples of a steel according to the invention; The figure 3 which shows a characterization of the nitrided layers by their residual surface stresses, carried out on reference samples and on samples of a steel according to the invention; The figure 4 which illustrates the elastic behavior of the nitrided layer from the penetration depths and residual depths during scratch tests carried out on two samples according to the invention in the nitrided state; The figure 5 which shows the evolution of the acoustic emission during scratch tests at increasing load carried out on the same samples as those of the figure 4 ; There figure 6 which illustrates the elastic behavior during scratch tests carried out on four samples according to the invention and a reference sample, all in the nitrided state.

[0022] The composition of steel (expressed in weight percentages) is motivated by the following considerations.

[0023] The Ni content is between 10.0 and 24.5%, preferably between 12.0 and 24.5%. This is on condition that: on the one hand, a highly martensitic structure is obtained by the usual heat treatments, i.e. representing at least 30%, better at least 50% on the surface of the structure visible on a micrograph. A Ni content of more than 24.5%, combined with the contents required for the other elements, would not make it possible to obtain such a structure regardless of the heat treatments used; on the other hand, after precipitation hardening, properties of ductility, expansion, elastic limit, K1C toughness are obtained which are particularly favorable for the envisaged applications; a minimum Ni content of 10.0%, associated with defined proportions of Co, Mo and other metallic elements, is suitable for this production. A minimum Ni content of 12.0% is still preferred to obtain this effect satisfactorily.

[0024] The Mo content is between 1.0 and 12.0%. This element allows structural hardening by forming, during aging, fine and dispersed intermetallics Fe 2 Mo, MoNi 3 and others. Optimally, the Mo content is 2.5 to 7.0% to obtain both a very significant effect of Mo and intermetallics of optimal size to ensure homogeneity of mechanical properties. The upper limit in Mo is given by the desire to maintain predominantly martensitic structures, suitable for age hardening.

[0025] Since this element is expensive, it is advisable not to add a quantity that could be superfluous, as its effects on structural hardening can be partly ensured by other, more economical elements.

[0026] Mo also plays a role in the constitution and properties of nitrided layers which contain fine and dispersed precipitates of different natures depending on the nitriding conditions (precipitates of types Mo 2 N, Fe x Mo y N z ...).

[0027] The Co content is between 1.0 and 18.0%. This element stabilizes the martensitic structure, raises the solidus temperatures and indirectly participates in hardening by promoting the precipitation of intermetallics. If the proportions of Co used are higher than 18.0%, the addition becomes very expensive (due to the high price of Co), and the properties of the steel can be significantly modified if, moreover, the contents of the other elements remain within the limits of the invention. Preferably, the Co content is 4.0 to 18.0%, better still 7.0% to 16.0%, even better still 8.0% to 15.0%.

[0028] If Co and Mo are at controlled contents which can be relatively moderate compared to what is usual, it is necessary to supplement their action by the addition of one or more of the hardening elements Si, Mn, Cu, W, V, Nb, Zr, C, Al, B, Y, Ta, Cr, Ti, N, within the limits which are specified elsewhere. This is one of the ways, according to the invention, of reducing the cost of the steel while retaining high properties due to structural hardening, in particular if these substitute hardening elements are chosen from among the least expensive of them. We find the problem mentioned above with regard to Mo.

[0029] The consequence of this requirement on the need to have sufficient quantities of Co is that the sum of the hardening elements Mo + Co + Si + Mn + Cu + W + V + Nb + Zr + Ta + Cr + C + AI + B + Y + Ti + N is between 14.0 and 29.0%, preferably between 15.0 and 27.0%, more preferably between 17.0 and 26.0%. This implies that since the Co content is at least 1%, preferably at least 4%, it will often be necessary to add at least one element chosen from Si, Mn, Cu, W, V, Nb, Zr, Ta, Cr, C, AI, Y and B (within the limits prescribed elsewhere), taking into account the fact that Mo is never higher than 12% (for economic reasons comparable to those leading to limiting the Co content) and preferably not higher than 7.0%.

[0030] The lower limit of 14.0% for this sum is justified by obtaining a sufficient hardening effect. Beyond 29.0%, the magnetic properties and the processing conditions of the material are significantly modified. Preferably, the lower limit is 15.0%, better 17.0%, to obtain the usage values ​​required by the most demanding applications envisaged while maintaining an economical nuance.

[0031] The contents of Ni, Co, Mo are also dependent on each other, in that: Ni improves ductility (especially at low temperatures), and allows control of expansion and the modulus of elasticity; it also has an effect on toughness and the Re / Rm ratio; its contents are limited: at the lower limit to benefit from the favorable properties mentioned above (generally from 5% for alloys), and at the upper limit so as not to hinder the martensitic transformation due to its gammagenic character; to this end, the influences of Co and Mo must also be taken into account; Mo is added for structural hardening purposes by the precipitation of intermetallics; and, in order to target the rupture properties of maraging grades, it is advisable to have a martensitic structure with aging; Mo is involved in this hardening as mentioned above (from 1%) and can participate in the structural hardening in conjunction with the proposed addition elements (such as Nb for example);Mo also participates in the nitriding of surfaces through its affinity with nitrogen (from a few %). Finally, it only finds its limits in the formation of embrittling phases (Laves, σ, µ, θ, δ phases, etc.), which can be associated with local segregations; its upper limit is 12.0%.

[0032] Finally, regarding the formation of an aging martensitic structure, the elements Co and Mo act jointly regarding the precipitation of hardening phases, but in a dissociated manner regarding the stabilization of ferritic structures. In order to unify these trends, a formula is proposed to preferably guarantee an Ms temperature located above room temperature: 21.5% ≤ Ni + Co + Mo ≤ 47.5%, preferably 25.0% ≤ Ni + Co + Mo ≤ 40.0%.

[0033] The Al content is between trace and 2.0%. AI is not necessarily added, but it is one of the elements that can be used to compensate for low Co contents with regard to mechanical performance. Its presence can be reduced to that of a residual element, resulting from the quantity that may have been necessary to add for the initial deoxidation of the liquid metal during production, or a voluntary addition of AI can be made to obtain specific properties. For a moderate cost, it increases resilience and can contribute to structural hardening. It also limits oxidation during the production of the liquid metal and the transformations of the solidified metal. However, it is necessary to avoid forming inclusions of significant sizes during hot processes (such as nitrides and oxides containing aluminum) in order not to degrade fatigue resistance and toughness.Limiting the presence of AI to a content of less than 2.0% limits this risk. In any case, a significant presence of AI must go hand in hand with careful production conditions, which avoid significant reoxidation of the liquid metal and which promote the elimination, by decantation and trapping in a slag, of the clusters of alumina inclusions which may have resulted from deoxidation and reoxidation.

[0034] Like Ti, aluminum promotes nitriding but does not allow easy control of the phases formed. Thus, precipitates of uncontrolled size can form at different stages of the production of liquid steel and the transformation of the solidified semi-finished product, and they can have a dramatic role in fatigue properties.

[0035] The Ti content is therefore between traces and 0.1%. By avoiding a significant presence of Ti (which other maraging steels require, unlike those of the invention), the aim is to prevent the formation of Ti nitrides during the solidification of the liquid metal, which deteriorate the fatigue resistance of the final product. In the invention, the desired structural hardening is obtained by other means.

[0036] The N content, which is at most 0.010%, can be imposed at a low level in the presence of nitridable addition elements (type Al, Ti), to avoid the formation of nitrides in the liquid phase as much as possible. Apart from these cases, or if the most harmful nitrides can be safely removed by decantation during production and casting, the tolerable N content of at most 0.010% is often simply provided in an imposed manner, by the quality of the raw materials and the processes of production and casting of the liquid metal.

[0037] The Si content ranges from trace to 2.0%. It can be used for deoxidation of the liquid metal during smelting, and it is one of the elements that can be used to compensate for the relatively low Co contents. The presence of Si can also contribute, even in the presence of Al, to the capture of some of the dissolved oxygen, which will therefore be less available to form large, harmful alumina clusters. However, care must be taken to avoid the formation of large Si-containing oxides in the final solidified steel, hence the upper limit of 2.0%. Si increases the solubility of certain elements and thus homogenizes the structure. Finally, it improves the yield strength. This relatively high maximum Si content is acceptable provided that the necessary precautions to obtain an inclusion population in accordance with the invention have been taken during smelting and casting.

[0038] The Mn content is between traces and 13.0%, and preferably between traces and 4.0%, better between 0.14% and 4.0%. Mn improves nitriding, as it increases the solubility of nitrogen in the solid phase. It also traps free sulfur, and thus limits brittleness during hot processing. Mn is also an effective deoxidizer, and can act on this point in synergy with Si, and the capture by Mn of a part of the dissolved oxygen, as for Si and also Cr (see below), allows the dissolved oxygen to be distributed between different elements other than Al, and thus limits the risk of forming large clusters of alumina inclusions. However, its content should preferably be limited to 4.0% to avoid forming phases that are harmful to the mechanical properties and to avoid drastically increasing the proportion of austenite.Mn promotes the stabilization of ferrito-austenitic biphasic grades (containing less than 70% martensite) with properties to be adjusted. In this context, its proportions must be finely adjusted, as must the heat treatment conditions and mechanical deformations, in order to precisely control the phase transformations and resulting properties. A content exceeding 13.0% risks leading to the formation of inclusions or phases rich in Mn, of large dimensions, as well as to significant proportions of austenite, which can degrade the mechanical properties.

[0039] A minimum of 0.14% may be preferred to start significantly benefiting from the aforementioned advantages of Mn.

[0040] Independently of the preferred conditions set individually on Si and Mn, the sum Si + Mn is at least 0.13%. In doing so, on the one hand, the presence in significant quantity of at least one deoxidizing element other than the AI ​​possibly present is ensured, this other deoxidizing element (as well as Cr) contributing to limiting the quantity of O trapped by Al with the risk of forming large clusters of alumina; on the other hand, Si and Mn are part of the hardening elements which are preferentially added, according to the invention, in partial substitution of Co and Mo, and as they are inexpensive and do not have troublesome side effects in the specified ranges, they are both (a fortiori in conjunction) an economically very interesting means of achieving the desired structural hardening.

[0041] The C content is between traces and 0.03%. In the grades according to the invention where carburizing elements, such as Nb, have been added, carbon contents less than or equal to 0.007% may be preferred in the absence of the addition of chromium. The aim is thus to form soft martensite, because carbon martensite is brittle and does not allow the shaping necessary for the product. It is also desired to avoid the formation of large carbides which would degrade the mechanical properties, since some of the hardening elements replacing Co tend to promote the precipitation of carbides. A C content controlled within the specified limits is therefore required or preferred.

[0042] The S content is between traces and 0.0020%, preferably between traces and 0.0010%, to avoid forming sulfides which would degrade fatigue resistance if they were present in large numbers and sizes. In addition, S weakens grain boundaries by segregating there, hence the possible formation of cracks when the steel is stressed. The presence of dissolved S must therefore be avoided, thanks to careful selection of raw materials and / or deep desulfurization of the liquid metal. The precise maximum tolerable content must be adjusted according to the intended applications, in a known manner (within the limit of 0.0020% at most, as specified above).

[0043] The P content is between trace and 0.005%, preferably less, to limit the possibility of it segregating at grain boundaries, like S.

[0044] B may be present in trace amounts, but a voluntary addition may also be preferred, up to 0.01%. This element promotes the refinement of structures and reduces grain size. It is good for mechanical properties, but too much should not be added to avoid losing ductility.

[0045] The H content is limited to 5 ppm to avoid hydrogen embrittlement problems. Carrying out one or more vacuum treatments during the production of the liquid metal and avoiding subsequent contamination of the liquid metal by ambient humidity, slag or any added materials generally makes it possible not to exceed this level.

[0046] The tolerable O content would depend, strictly speaking, on the intended applications for the final product, as would the tolerable contents of S, B, N and other residuals or elements that can form precipitates. The maximum content is set at 0.030% (300 ppm), which results from the implementation of the processes normally used during the production of liquid metal. The aim is to avoid having in the final product oxides whose composition, distribution and size cannot be controlled. To this end, the addition of AI or another oxidizable element, within the limits prescribed elsewhere, helps to obtain a low O content (for example 16 ppm or lower) and to avoid the presence of large oxides, provided that the quality of the production is well controlled by avoiding as much as possible reoxidation of the liquid metal by the atmosphere and refractories.

[0047] The Cr content is between traces and 5.0%, preferably between 0.01% and 5.0%, better between 0.1% and 5.0%. Its presence is therefore not absolutely mandatory, but it has the advantage of increasing the resistance to oxidation and the mechanical properties and of helping with nitriding. Cr, on the other hand, like Mn, is a gammagenic element, which extends the temperature stability range of austenite, by spacing the As / Af, Ms / Mf transformation points. The upper limit of 5% is justified by the concern not to accentuate this effect drastically.

[0048] Cr also has a beneficial influence on the properties of the nitrided layer that may have formed on the product made from a steel according to the invention: it reduces its ability to crack. This effect is increased in the presence of a significant quantity of Mn.

[0049] Preferably, the sum Al + Cr is at least 0.1%, better at least 0.17%, so that the oxygen forming the oxides can be distributed between Al and Cr, and thus limits the risk of formation of large inclusions.

[0050] The Cu content ranges from trace to 4%. It is one of the elements that can be added deliberately, and not just as an impurity, to compensate for low Co contents. The addition, if it occurs, must be limited, because Cu is gammagenic, and reduces martensitic aging. If added in controlled proportions, Cu participates in hardening (together with Mo) and improves resistance to oxidation.

[0051] The W content is between trace and 6.0%. It is therefore not mandatory and can be added mainly when one wishes to impose a fairly low Co, or even Mo, content, as seen above, for its contribution to structural hardening.

[0052] The Zr content is between trace and 4.0%. It may be desirable to add this element to contribute to deoxidation, and also to the formation of fine nitrides, so that N does not form too coarse nitrides if elements likely to produce them (Al in particular, since the massive presence of Ti is in any case to be avoided) are very significantly present. Zr is also among the hardening elements that can be substituted for Mo and Co.

[0053] Ca and Mg can be found in the metal due to the wear of refractories and steel products, in the form of oxides or sulfides. It may also be desired to voluntarily add these elements so that they contribute to the deoxidation and control of the composition of oxidized inclusions which will determine their propensity to form, in conjunction with Al and Si in particular, oxides which will be able to coalesce and settle more easily than pure alumina inclusions, and make malleable during shaping any inclusions which may remain, reducing their harmfulness. The final content must be limited to 0.1% for Ca and 0.8% for Mg, in order to avoid the formation of oxides whose size and distribution cannot be controlled.

[0054] Y, Nb, Ta, and V can be added up to 4.0% each. They are among the hardening elements that can be used to compensate for low Co and Mo contents.

[0055] In addition, Ta and Y help to form small oxides, and Nb and V are favorable to the formation of small carbides. These elements are therefore favorable to achieving the characteristics of the invention concerning the control of the size of inclusions. Nb also has a beneficial influence on the elastic return of nitrided layers (under low load).

[0056] Finally, 0.14% ≤ Al + Si + Cu + Nb + Mn + V + Ta + Cr + W + C + B + Y + Zr + Ti + N ≤ 8.0%. By limiting the value of the sum of these contents, we seek to avoid the risk of exaggerating the hardening effects that the substitution of these elements for Co and Mo could have, as well as their secondary effects on the other properties of the steel. The minimum value of at least 0.14% for this sum corresponds to what is necessary when there is a deliberate desire to substitute at least one of these hardening elements for Co and Mo.

[0057] It should be understood that the contents that are described as "preferential" for certain elements, or for the sums of the contents of certain elements, are independent of each other. It is possible, without departing from the invention, to respect one or more of said preferential conditions and not to respect the others.

[0058] Among these preferential conditions, the most recommended is that relating to the sum Al + Cr ≥ 0.17%.

[0059] Meeting at least one of the conditions relating to the sum Al + Cr ≥ 0.17% or Si + Mn ≥ 0.13% proves to be particularly advantageous for optimizing the desired results, in terms of inclusion control, mechanical properties, and also for the suitability for nitriding associated with good behavior of the nitrided layer during uses of the final product.

[0060] The elements not mentioned are, at most, present only as impurities resulting from the production process and are not added voluntarily.

[0061] Concerning the inclusion population, the criterion to be respected, according to the invention, is that this inclusion population, observed by image analysis on a polished surface of 650 mm 2< if the steel is in the form of a part or a hot-transformed sheet, and of 800 mm 2< if the steel is in the form of a cold-rolled sheet, does not contain any non-metallic inclusions with an equivalent diameter greater than 10 µm, preferably no inclusions with a size greater than 8 µm.

[0062] In the case of a hot-transformed part or sheet, it optimally does not contain more than two, and preferably not more than 1.5 non-metallic inclusions with an equivalent diameter greater than 1.5 µm per mm 2< on hot-transformed sheet, the observation being carried out by SEM image analysis covering at least 200 mm 2< , carried out for example on a polished surface of 650 mm 2< .

[0063] The non-metallic inclusions considered are oxides, sulfides and nitrides. The oxide population is controlled mainly by the choice of production methods (extensive deoxidation of the liquid metal, after which care is taken to eliminate large inclusions as much as possible, in particular by using remelting processes for the electrode initially cast from the liquid metal). The sulfide population is controlled by imposing very low S contents, requiring a careful choice of raw materials and / or desulfurization of the liquid metal. The nitride population is controlled by imposing low or very low N contents, for example by using reduced pressures during the production of the liquid metal and the remelting of the electrode, and by limiting the Ti content of the metal.

[0064] The steels according to the invention are prepared, for example and in a non-limiting manner, by the following routes.

[0065] The steel, first produced in the liquid state in an arc furnace, and possibly also in a ladle, to adjust its composition to the essential elements, is then cast in the form of remelting electrodes. These electrodes are: either remelted once under vacuum (VIM process: Vacuum Induction Melting VAR process, Vacuum Arc Remelting known in itself), or under electroconductive slag (ESR process, Electro Slag Remelting, known in itself), to form, after casting and solidification of the liquid steel, ingots, billets or slabs; or remelted several times, under vacuum (VAR) or under electroconductive slag (ESR) to form, after casting and solidification, ingots or slabs.

[0066] After the electrode has been produced and cast, either a simple remelting of the electrode or a multiple remelting of the electrode, for example VAR + VAR or ESR + VAR, is carried out. These remelts purify the metal and improve the quality of solidification by reducing segregations and refining its solidification structure. In particular, ESR remelting effectively reduces the sulfur content, and VAR remelting effectively reduces nitrogen contents.

[0067] The ingots or slabs are then hot rolled, after reheating to between 1050 and 1300°C, typically around 1200°C, to obtain hot rolled sheets or strips a few millimeters thick, for example around 1.5 to 5 mm thick. For grades containing gammagenic elements at contents greater than 10% for example, it may sometimes be advisable to control the cooling of the sheets, to promote the formation of martensite and avoid leaving a quantity of austenite that could prove too high. This is particularly the case for steels containing Mn. Experience will be able to demonstrate to the skilled person whether, in the specific case of the steel he wishes to obtain with the tools at his disposal, such cooling control may be useful.

[0068] Hot-rolled products having this thickness may, in certain cases, be used either in the as-hot-rolled state, or be hot-formed, or be used in a state with controlled recrystallization. Recrystallization may possibly already occur sufficiently after hot rolling and the strip remaining in coil form, which then constitutes a true heat treatment, but if it is insufficient to obtain the desired microstructure and / or mechanical properties, a recrystallization annealing may then be carried out to adjust this structure. In the latter case, the person skilled in the art knows how to adjust the parameters of the recrystallization annealing (temperature, duration, etc.) to adjust the microstructure (in particular the grain size) and the desired mechanical properties.

[0069] Typically, after hot rolling and possible recrystallization (or other types of heat treatment), Vickers hardnesses greater than or equal to 285 Hv10 are targeted. This suggests a tensile strength greater than or equal to 950 MPa, and a distributed elongation greater than or equal to 5%.

[0070] Hardness is assessed in hot sheet section. The structures targeted on pickled hot-rolled product are fine, preferably having an austenitic grain size index greater than or equal to 10 according to the ASTM E112 standard, for which it is recalled that the figure giving the grain size is all the higher as the grain is fine.

[0071] These hot-rolled, and possibly heat-treated, strips may also not be intended for direct use, and it is then necessary to reduce their thickness by cold forming for the intended applications. In this case, they are pickled, then cold-rolled, with one or more intermediate anneals between the different passes of the cold rolling, and possibly one (or more) final anneal(s) for aging, recrystallization, or other types of heat treatments, or appropriate surface treatments depending on the intended application (which will be detailed later), to obtain cold-rolled strips with a thickness of less than 2 mm, preferably less than or equal to 1 mm, and for example 0.4 mm or 0.2 mm thick.

[0072] The recrystallization treatment of the cold-rolled strip is preferably carried out at a thickness such that the cold-rolled strip has, at that time, a work-hardening rate greater than 30%, more preferably greater than 40%. It provides the strip with a grain size which is preferably ASTM 10 (average grain diameter of less than 10 µm) or finer (according to ASTM E112).

[0073] The annealing treatment intended to obtain a fine grain, and / or stress relief and / or normalization of the metal, is carried out in a protective atmosphere by suitably adjusting the temperature and duration parameters. These parameters depend on the particular conditions under which the heat treatment is carried out, and the person skilled in the art knows how to determine these parameters in each particular case.

[0074] The preferential requirements on the grain size of cold-rolled products, possibly heat-treated, are also, preferentially, valid for products intended to be used in the hot-rolled state, possibly after having been heat-treated.

[0075] In order to improve the flatness of the strip, and, if necessary, to perfect the martensitic transformation, the strip can also be subjected to a light final cold rolling (skin-pass or planing) with a reduction rate of between 1 and 20%.

[0076] Typically, hardening (aging) treatments of the cold-rolled strip are preferably carried out at a thickness such that the rolled strip has, at that time, a work hardening rate greater than 30%, better, greater than 40%.

[0077] A piece can then be cut from the strip and shaped, for example by bending, welding, etc., then a hardening treatment can be carried out on it, consisting of maintaining it between 400 and 600°C for 30 min to 5 h. (preferably at 420-550°C for 30 min to 2 h, for example 420°C for 30 min or 480°C for 2 h)

[0078] Hot rolled products are also likely to undergo a hardening treatment, typical of maraging steels, with the benefits classically expected from such treatment on their mechanical properties.

[0079] Products made from martensitic grades containing at least 70%, cold rolled and optionally heat treated, according to the invention can achieve a tensile strength Rm of at least 2030 MPa, a conventional elastic limit Rp 0.2 of at least 2000 MPa, and an elongation A (5.65) of at least 1%. Products made from ferrito-austenitic two-phase grades, on the other hand, have lower mechanical properties after certain thermal cycles but retain increased performance during dynamic stresses in service (reinforced work hardening, phase transformation and nitriding).

[0080] These characteristics can also be optimally achieved on hot-rolled products that have been adequately heat-treated.

[0081] The products can then be surface hardened (by nitriding, carburizing, carbonitriding, shot peening, etc.) in order to increase their fatigue performance. The extreme surface hardness Hv0.1 can typically be at least 950 without the need for nitriding processes and conditions other than operating processes and conditions known to those skilled in the art.

[0082] Experiments were carried out on samples of a steel (denoted Inv) and on reference samples (denoted Ref), whose compositions are summarized in Table 1, expressed in % by weight. The remainder is iron, and also impurities resulting from the production process and which are at a level of no importance for the properties considered. The sign "-" means that the element is present in the sample only in trace amounts or in very small quantities, without metallurgical effects. Ni Co Mo Ti Al Cr V Ta Cu Nb Mn W Si Ni+Co+Mo Ref 1 18,11 16,50 5,30 - 0,02 0,081 - - 0,110 - 0,074 - 0,047 39,91 Ref 2 17,70 9,10 4,99 0,457 0,11 - - - - - - - 0,008 31,79 Inv 1 17,70 12,98 4,95 - - 0,021 0,44 - - - 0,291 - < 0,010 35,63 Inv 2 17,90 12,60 4,98 - - 0,082 2,02 - - - 0,273 - 0,021 35,48 Inv 3 18,20 12,20 5,02 - - 0,157 3,95 - - - 0,250 - 0,042 35,42 Inv 4 18,30 12,20 7,10 - - 0,159 3,99 - - - 0,240 - 0,034 37,60 Inv 5 17,90 13,20 5,00 - - - - 0,12 - - 0,217 - < 0,010 36,10 Inv 6 17,90 13,00 5,00 - - 0,005 - 0,53 - - 0,218 - < 0,010 35,90 Inv 7 18,20 12,60 4,80 - - 0,006 - 2,84 - - 0,213 - 0,014 35,60 Inv 8 18,40 12,70 4,90 - 0,80 0,197 - 2,95 - - 0,216 - 0,014 36,00 Inv 9 17,70 13,10 5,00 0,015 - 0,005 - 0,009 0,190 - 0,288 - 0,020 35,80 Inv 10 17,80 13,10 5,00 0,016 - 0,005 - 0,009 0,800 - 0,278 - 0,016 35,90 Inv 11 17,70 13,00 5,00 0,016 - 0,005 - 0,009 2,060 - 0,274 - 0,020 35,70 Inv 12 17,90 13,10 7,00 0,020 - 0,010 - 0,004 4,060 - 0,263 - 0,013 38,00 Inv 13 18,10 13,01 5,32 - 0,02 0,908 - - 2,010 - 0,167 - 0,033 36,43 Inv 14 17,73 13,00 4,95 0,015 - 0,006 - 0,008 - 0,21 0,291 - 0,012 35,68 Inv 15 17,77 12,90 4,95 0,016 - 0,006 - 0,013 - 0,82 0,278 - 0,010 35,62 Inv 16 18,06 12,80 4,97 0,016 - 0,007 - 0,023 - 1,87 0,270 - 0,014 35,83 Inv 17 18,50 12,60 6,46 0,019 0,01 0,100 - 0,043 - 3,77 0,259 - 0,024 37,56 Inv 18 18,20 12,86 5,31 - 0,02 0,037 - - 0,094 0,793 0,174 - 0,038 36,37 Inv 19 18,22 12,89 5,26 - 0,01 0,883 - - 0,084 0,775 0,144 - 0,033 36,37 Inv 20 17,69 13,00 4,96 0,016 - 0,006 - - - - 0,780 - 0,010 35,65 Inv 21 17,73 13,00 4,96 0,015 - 0,007 - - - - 1,970 - < 0,010 35,69 Inv 22 17,87 13,00 4,95 0,015 - 0,010 - - - - 3,920 - < 0,010 35,82 Ref 23 17,94 12,80 4,84 0,015 0,01 0,012 - - - - 7,830 - 0,014 35,58 Inv 24 18,19 13,00 5,31 - 0,01 0,902 - - 0,095 - 1,930 - 0,309 36,50 Réf 25 10,10 2,26 1,98 - 0,54 0,007 - - - - 13,54 - 0,044 14,34 Réf 26 18,24 5,02 4,99 0,007 0,62 0,011 - - - - 13,57 - 0,047 28,25 Inv 27 17,80 5,20 4,90 0,006 0,25 0,005 - - - - 0,0053 0,20 0,036 27,99 Inv 28 17,90 5,20 4,90 0,006 0,24 0,005 - - - - 0,0065 0,80 0,034 28,01 Inv 29 18,00 5,10 4,80 0,006 0,25 0,005 - - - - - 1,90 0,036 27,90 Inv 30 18,00 4,80 4,50 0,006 0,24 0,005 - - - - - 3,70 0,025 27,23 Inv 31 17,90 7,20 5,00 0,006 0,24 0,007 - - - - 0,0058 0,20 0,029 29,99 Inv 32 17,90 7,10 4,90 0,006 0,24 0,007 - - - - 0,0051 0,70 0,032 29,90 Inv 33 18,10 7,00 4,80 0,006 0,24 0,007 - - - - 0,0055 2,10 0,031 29,90 Inv 34 19,40 6,80 4,70 0,006 0,24 0,006 - - - - - 4,20 0,028 30,90 Inv 35 17,88 10,11 4,94 0,007 0,24 0,006 - - - - - 0,20 0,038 32,93 Inv 36 17,88 10,01 4,91 0,007 0,24 0,005 - - - - - 0,82 0,030 32,80 Inv 37 18,08 9,82 4,81 0,006 0,24 0,006 - - - - - 1,96 0,033 32,71 Inv 38 19,42 9,57 4,70 0,006 0,25 0,006 - - - - - 3,94 0,033 33,69 Inv 39 17,90 5,11 4,93 - 0,20 - - - - - 0,037 - < 0,010 27,94 Inv 40 17,98 2,09 4,97 - 0,57 - - - - - - - < 0,010 25,04 Inv 41 18,01 2,11 4,97 - 0,88 - - - - - - - < 0,010 25,09 Inv 42 17,95 2,11 4,96 - 0,51 0,201 - - - - - - < 0,010 25,02 Inv 43 17,92 2,10 4,97 - 0,52 0,474 - - - - - - 0,016 24,99 Inv 44 17,90 5,30 5,00 0,006 0,66 0,200 - - - - 0,0069 - 0,025 28,17 Inv 45 17,90 5,20 4,99 0,006 0,85 0,200 - - - - 0,0067 - 0,027 28,12 Inv 46 17,90 7,20 4,99 0,006 0,85 0,200 - - - - 0,0055 - 0,030 30,09 Inv 47 18,00 10,20 5,00 - 0,86 0,200 - - - - 0,0052 - 0,028 33,20 Inv 48 17,95 5,24 5,00 0,109 0,86 0,006 - - - - 0,0107 - 0,123 28,19 Inv 49 17,97 7,20 5,00 0,109 0,85 0,007 - - - - 0,0119 - 0,120 30,17 Ref 50 17,89 5,26 4,99 0,006 0,85 0,005 - - - - 0,0068 - 0,124 28,14 Ref 51 17,87 7,24 5,03 0,007 0,84 0,006 - - - - 0,0066 - 0,127 30,14 Réf 3 18,04 9,96 4,87 - 4,48 0,005 - - - - 0,063 - 0,027 32,87 Réf 4 18,04 16,21 4,89 - - - - - - - - - 0,021 39,14 Réf 5 18,04 18,57 4,74 - - - - - - - - - 0,035 41,35 Inv 52 17,96 5,12 4,97 0,01 0,80 0,005 - - - 0,008 - 0,124 28,05 Inv 53 18,05 7,18 4,86 0,008 0,82 0,006 - - - - 0,009 - 0,127 30,09 Inv 54 17,96 16,07 9,89 - 0,01 0,02 - - - - 0,11 - 0,09 43,92 Inv 55 18,05 16,30 11,83 - 0,02 0,01 - - - - 0,10 - 0,08 46,18 Inv 56 18,04 8,14 5,06 - 2,63 0,005 - - - - 0,006 - 0,029 31,24 Inv 57 18,16 9,98 5,06 - 3,63 2,2 - - - - - - 0,008 33,20 Ref 58 18,24 10,14 5,06 - 4,63 4,6 - - - - - - 0,007 33,44 Inv 59 18,04 8,14 5,06 - 2,63 0,005 - - - - 0,006 - 1,97 31,24 Inv 60 18,04 16,03 4,70 - 0,01 0,005 - - - - - - 0,03 38,77 Réf 6 18,04 8,14 5,06 - 2,48 - - - - - - - 2,04 31,24 Inv 61 18,16 9,98 5,06 - 3,48 0,04 - - - - - - 0,21 33,20 Table 1: Composition of the samples tested S Mg Zr Y B C N P H O Ca Ref 1 0,0003 - - - - 0,003 0,0015 0,003 < 0,00002 < 0,0005 < 0,0005 Ref 2 < 0,0005 - - - - 0,002 0,0007 < 0,002 < 0,00002 0,0020 < 0,0005 Inv 1 < 0,0005 - - - 0,0004 0,002 0,0009 < 0,003 < 0,00002 0,0036 < 0,0005 Inv 2 < 0,0005 - - - 0,0004 0,002 0,0043 < 0,003 < 0,00002 0,0088 < 0,0005 Inv 3 0,0008 - - - 0,0005 0,002 0,0068 < 0,003 < 0,00004 0,0073 < 0,0005 Inv 4 0,0007 - - - 0,0007 0,002 0,0057 < 0,003 < 0,00002 0,0073 < 0,0005 Inv 5 < 0,0005 - - - - < 0,001 0,0016 < 0,003 < 0,00002 0,0276 < 0,0005 Inv 6 < 0,0005 - - - - < 0,001 0,0017 < 0,003 < 0,00002 0,0028 < 0,0005 Inv 7 < 0,0005 - - - - < 0,001 0,0015 < 0,003 < 0,00002 0,0023 < 0,0005 Inv 8 < 0,0005 - - - 0,0005 0,001 0,0017 < 0,003 < 0,00002 0,0012 < 0,0005 Inv 9 < 0,0005 - - - - 0,005 0,0008 < 0,003 0,00003 0,0073 < 0,0005 Inv 10 < 0,0005 - - - 0,0003 0,002 0,0009 < 0,003 < 0,00002 0,006 < 0,0005 Inv 11 < 0,0005 - - - 0,0004 0,001 0,0007 < 0,003 < 0,00002 0,0062 < 0,0005 Inv 12 < 0,0005 - - - 0,0008 0,002 0,0006 < 0,003 < 0,00002 0,014 < 0,0005 Inv 13 0,00035 - - - - 0,006 0,0016 0,002 < 0,00002 < 0,0005 < 0,0005 Inv 14 < 0,0005 - - - - 0,001 0,0005 < 0,003 0,00007 0,0103 < 0,0005 Inv 15 < 0,0005 - - - - 0,002 0,0015 < 0,003 < 0,00002 0,0046 < 0,0005 Inv 16 < 0,0005 - - - 0,0003 0,001 0,0046 < 0,003 < 0,00002 0,0042 < 0,0005 Inv 17 < 0,0005 - - - 0,0006 < 0,001 0,0095 < 0,003 < 0,00002 0,0044 < 0,0005 Inv 18 0,0005 - - - - 0,008 0,0012 < 0,002 < 0,00002 < 0,0005 < 0,0005 Inv 19 0,00044 - - - 0,0003 0,007 0,0014 0,002 < 0,00002 0,0014 < 0,0005 Inv 20 < 0,0005 - - - 0,0003 0,006 0,0007 < 0,003 < 0,00002 0,0081 < 0,0005 Inv 21 0,0007 - - - 0,0003 0,006 0,001 < 0,003 < 0,00002 0,0048 < 0,0005 Inv 22 0,0012 - - - 0,0004 0,004 0,0015 < 0,003 0,00004 0,0037 < 0,0005 Ref 23 0,0024 - - - 0,0005 0,004 0,0027 < 0,003 < 0,00002 0,0028 < 0,0005 Inv 24 0,001 - - - - 0,005 0,0013 0,002 < 0,00002 < 0,0005 < 0,0005 Ref 25 < 0,0005 - - - - 0,003 0,0057 < 0,003 < 0,00002 0,0008 < 0,0005 Ref 26 < 0,0005 - - - - 0,004 0,0065 < 0,003 < 0,00002 < 0,0005 < 0,0005 Inv 27 < 0,0005 - - - - < 0,001 0,0006 < 0,003 < 0,00002 0,0088 < 0,0005 Inv 28 < 0,0005 - - - - 0,001 0,0008 < 0,003 < 0,00002 0,0088 < 0,0005 Inv 29 < 0,0005 - - - - 0,001 0,0011 < 0,003 < 0,00002 0,0113 < 0,0005 Inv 30 < 0,0005 - - - - < 0,001 0,0015 < 0,003 < 0,00002 0,0111 < 0,0005 Inv 31 < 0,0005 - - - - 0,001 0,0008 < 0,003 < 0,00002 0,0056 < 0,0005 Inv 32 < 0,0005 - - - - 0,002 0,0012 < 0,003 < 0,00002 0,0069 < 0,0005 Inv 33 < 0,0005 - - - - 0,001 0,0017 < 0,003 < 0,00002 0,0078 < 0,0005 Inv 34 < 0,0005 - - - - 0,003 0,0025 < 0,003 < 0,00002 0,0113 < 0,0005 Inv 35 < 0,0005 - - - - 0,003 0,0007 < 0,003 < 0,00002 0,0037 < 0,0005 Inv 36 < 0,0005 - - - - 0,002 0,001 < 0,003 < 0,00002 0,0045 < 0,0005 Inv 37 < 0,0005 - - - - 0,002 0,0019 < 0,003 < 0,00002 0,0052 < 0,0005 Inv 38 < 0,0005 - - - - 0,001 0,0023 < 0,003 < 0,00002 0,0064 < 0,0005 Inv 39 < 0,005 - - - - 0,006 < 0,0005 < 0,002 < 0,00002 0,0014 < 0,0005 Inv 40 < 0,005 - - - - 0,003 < 0,0005 < 0,002 < 0,00002 0,003 < 0,0005 Inv 41 < 0,005 - - - - 0,003 < 0,0005 < 0,002 < 0,00002 0,0017 < 0,0005 Inv 42 < 0,005 - - - - 0,002 < 0,0005 < 0,002 < 0,00002 0,0008 < 0,0005 Inv 43 < 0,005 - - - - 0,002 < 0,0005 < 0,002 < 0,00002 0,0011 < 0,0005 Inv 44 < 0,0005 - - - - 0,002 0,0006 < 0,003 < 0,00002 0,0016 < 0,0005 Inv 45 < 0,0005 - - - - 0,002 0,0005 < 0,003 < 0,00002 0,0024 < 0,0005 Inv 46 < 0,0005 - - - - 0,003 0,0005 < 0,003 < 0,00002 0,0007 < 0,0005 Inv 47 < 0,0005 - - - - 0,002 0,0006 < 0,003 < 0,00002 < 0,0005 < 0,0005 Inv 48 < 0,0005 - - - - 0,003 0,0013 < 0,003 < 0,00002 0,0020 < 0,0005 Inv 49 < 0,0005 - - - - 0,003 0,0013 < 0,003 < 0,00002 0,0017 < 0,0005 Ref 50 0,004 - - - - 0,003 < 0,0005 < 0,003 < 0,00002 0,0005 < 0,0005 Ref 51 0,0053 - - - - 0,003 0,0006 < 0,003 < 0,00002 < 0,0005 < 0,0005 Réf 3 < 0,0005 - - - - 0,002 0,0060 < 0,003 < 0,00002 0,0054 < 0,0005 Réf 4 0,0027 - - - - 0,0035 < 0,0005 < 0,003 < 0,00002 0,0020 < 0,0005 Réf 5 0,0035 - - - - 0,002 < 0,0005 < 0,003 < 0,00002 0,0014 < 0,0005 Inv 52 0,0009 0,03 - - - 0,003 < 0,0005 < 0,003 < 0,00002 0,0005 < 0,0005 Inv 53 0,0009 0,05 - - - 0,003 < 0,0005 < 0,003 < 0,00002 < 0,0005 < 0,0005 Inv 54 < 0,0005 - - - - 0,006 < 0,0005 < 0,003 < 0,00002 0,0011 < 0,0005 Inv 55 < 0,0005 - - - - 0,007 < 0,0005 < 0,003 < 0,00002 0,0032 < 0,0005 Inv 56 < 0,0005 - 0,02 - - 0,002 < 0,0005 < 0,003 < 0,00002 0,008 < 0,0005 Inv 57 < 0,0005 - 0,015 - - 0,004 0,0020 < 0,003 < 0,00002 0,002 < 0,0005 Ref 58 < 0,0005 - 0,13 - - 0,006 0,0015 < 0,003 < 0,00002 0,0015 < 0,0005 Inv 59 < 0,0005 - - 0,96 - 0,006 < 0,0005 < 0,003 < 0,00002 0,003 < 0,0005 Inv 60 < 0,0005 - - - - 0,002 < 0,0005 < 0,003 < 0,00002 0,0018 0,098 Inv 61 < 0,0005 0,782 0,03 - - 0,002 < 0,0005 < 0,003 < 0,00002 0,003 < 0,0005 Réf 6 < 0,0005 - - 3,46 - 0,005 < 0,0005 < 0,003 < 0,00002 0,002 < 0,0005

[0083] In the table above, except for steels Inv 27 to Inv 47 and Inv 54 to Inv 61, the steels marked Inv have compositions in accordance with the claimed invention.

[0084] The preparation of steels marked Inv and reference steels, from which the samples in Table 1 were taken, was carried out according to the following diagram, so as to obtain strips with a thickness of 0.4 mm.

[0085] The samples marked Inv were produced in the laboratory in a research vacuum induction furnace, in the form of test castings of a few kg (5 to 50 kg), except for samples Inv 13, Inv 18, Inv 19 Inv 24, Inv 54, Inv 55, Inv 60 and Inv 61 which were produced on industrial tools (a few tonnes), first by melting in an arc furnace, then application of the VIM and VAR remelting processes.

[0086] Samples Ref 1, Ref 2 and Ref 4 were prepared using industrial tools. The other reference samples Ref 3, Ref 5, Ref 6, Ref 23, Ref 25, Ref 26, Ref 50, Ref 51, Ref 58 were prepared in the laboratory under the same conditions as the samples marked Inv prepared in the laboratory.

[0087] The structures and inclusion populations evaluated on the laboratory castings are very close to those obtained on industrial tools due to the similar production times used. The difference in the densities and sizes of the finest inclusions does not exceed 20% in favor of the laboratory castings (with regard to the ingot formats used), all other things being equal. However, the study castings are characterized by the absence of remelting, which goes in the direction of compensation for the differences on the previous parameters and makes the laboratory test results reasonably comparable to the industrial test results. Then the ingots were transformed into slabs, by blooming with a reduction in thickness bringing this thickness to between 200 and 100 mm.

[0088] Then the slabs were hot rolled to a thickness of 3.5 mm, after reheating to approximately 1300°C which led to hot rolling taking place from a temperature of 1285°C, taking into account the transfer time between the furnace and the rolling stand. The metal was then pickled, and was cold rolled to a thickness of 0.4 mm or less. Austenitization or solution annealing, then recrystallization, then aging, were carried out, where appropriate, at different stages of manufacture, and were carried out respectively between 800 and 850°C (for a maximum of 1 hour), then between 850°C and 1200°C (for durations of less than 10 min) and finally between 420 and 550°C for 30 min to 4 h.

[0089] Table 2 shows: the size of the largest inclusions in each sample in Table 1, after hot rolling, observed on 650 mm 2< of these samples, taken at mid-width of the sheet; the inclusion densities evaluated on a surface of 650 mm 2< by optical microscopy (OM), for inclusions larger than 4 µm; and the inclusion densities observed by scanning electron microscopy (SEM) by automated image analysis for industrially produced samples, observed on surfaces of 100 to 400 mm 2< , for inclusions larger than 1.5 µm.

[0090] The maximum dimensions of the particles observed were transcribed into equivalent inclusion diameters noted as "D circle". It should be understood that by "diameter" of the inclusions, we mean "equivalent diameter", that is to say that of an inclusion which would be of circular section and would have the same surface area as the inclusion observed, if the latter has a more complex section than that of a simple circle.

[0091] Furthermore, since optical image analysis only distinguishes colored contrasts and does not differentiate the composition of the inclusions, only the absence of TiN (orange colored contrast, according to the experience of the person skilled in the art) could be verified by optical microscopy, as well as the inclusion densities of the various other particles evaluated for inclusions larger than 4µm. Finally, the inclusion populations were more precisely characterized by automated counting and analysis in scanning electron microscopy with a field effect gun (FEG SEM) on surfaces of 200 to 400 mm 2 < (by respective magnifications of x300, x1000, x10,000), and their surface densities evaluated. Thus, the densities and nature of the inclusions of the industrially produced samples were specified on 3.5 mm thick hot-rolled strips. All densities were reduced to surface densities (number of inclusions per mm 2 < ). Table 2: Size of the largest inclusions observed on hot-rolled samples, and inclusion densities (for inclusions larger than 4 µm) of the hot-rolled samples in optical microscopy, and in scanning electron microscopy (for inclusions larger than 1.5 µm) D circle max inclusion (µm) Densité inclusionnaire (nombre par mm 2< ) Mo (inclusions > 4µm) MEB (inclusions > 1,5µm) Ref 1 8 0,09 2,6 Ref 2 8 0,5 15 Inv 1 5 0,33 Inv 2 10 0,21 Inv 3 6 0,27 Inv 4 4 0,53 Inv 5 10 0,29 Inv 6 5 0,15 Inv 7 5 0,11 Inv 8 5 0,10 Inv 9 6 0,31 Inv 10 7 0,24 Inv 11 5 0,35 Inv 12 8 0,81 Inv 13 7 0,31 0,89 Inv 14 8 0,32 Inv 15 5 0,19 Inv 16 10 0,28 Inv 17 10 0,32 Inv 18 10 0,29 1,10 Inv 19 6 0,21 1,39 Inv 20 5 0,48 Inv 21 10 0,30 Inv 22 10 0,32 Ref 23 10 0,42 Inv 24 7 0,45 1,10 Ref 25 10 1,73 Ref 26 10 1,75 Inv 27 7 1,28 Inv 28 9 4,20 Inv 29 8 3,06 Inv 30 10 1,11 Inv 31 5 1,55 Inv 32 7 3,39 Inv 33 6 3,29 Inv 34 10 2,07 Inv 35 5 1,92 Inv 36 5 2,82 Inv 37 10 2,49 Inv 38 5 1,59 Inv 39 7 0,07 Inv 40 10 0,12 Inv 41 10 0,11 Inv 42 7 0,12 Inv 43 7 0,09 Inv 44 2 0,24 Inv 45 10 0,92 Inv 46 4 0,39 Inv 47 6 0,13 Inv 48 10 0,80 Inv 49 5 0,48 Ref 50 10 0,81 Ref 51 5 1,56 Ref 3 14 0,96 Ref 4 11 0,54 1,6 Ref 5 11 0,69 2,1 Inv 52 8 0,94 Inv 53 7 1,02 Inv 54 8 0,18 Inv 55 7 0,21 Inv 56 8 0,98 Inv 57 8 1,24 Ref 58 8 1,47 Inv 59 8 1,01 Inv 60 8 0,97 Ref 6 12 0,53 Inv 61 8 0,86

[0092] These results show that in the case of the samples according to the invention, low inclusion densities and a complete absence of inclusions of relatively large size can be obtained by adjusting the composition of the materials and the production processes, namely no inclusions larger than 10 µm on hot-rolled product, and optimally inclusion densities of the order of or below those of the references. Such inclusions are also absent from reference sample 1, but the number of small oxide inclusions (5 to 10 µm in diameter) is significantly higher than in the case of industrial samples (for example) according to the invention, which is unfavorable to the fatigue properties. As for reference sample 2, it has too high a density of nitrides, including nitrides larger than 10 µm.This characteristic alone is prohibitive for achieving sufficient fatigue resistance (due to the size, nature and morphology of the nitrides) and it was not considered useful to focus on the oxides in this sample.

[0093] The samples according to the invention therefore only contain inclusions of small diameter, and in small numbers (the relatively fine size of the inclusions required inclusion counts by scanning electron microscopy in order to evaluate a representative number of inclusions accessible by the resolution of the equipment and to precisely estimate their dimensions from 1.5 µm). In particular, there is no Ti nitride, which is linked in particular to the absence of Ti and the very low N content. Reference sample 1 is in the same case, although the inclusion density and the diameter of its largest inclusions are a little higher than in the best cases of the invention. As for reference sample 2, it is confirmed that nitrides (mainly Ti) are predominant and present in the form of inclusions that are not very ductile and are often excessive in size so that the objectives of excellent fatigue resistance can be met.

[0094] Similarly, Ref 4 and Ref 5, with increased S content, and Ref 3 and Ref 6 with high Al and Y contents respectively, present large oxide inclusions, greater than 10 µm on hot-rolled products.

[0095] Inclusion counts in optical microscopy were first initiated (for speed and ease of implementation), which however quickly found their limits due to the small size of the inclusions and their small number. In addition, the optical microscopy used in the context of the present invention for inclusions of oxides, sulfides or for other types of particles, can introduce artifacts by confusion of the shades of gray induced by the preparation of the samples, surface pollution, etc. if the images of the counts are not correctly sorted by an experienced observer. Automated inclusion counts and analyses in SEM with EDX are then preferred, in order to give a more reliable representation of the surface density of the inclusions of the industrial samples produced according to the invention.

[0096] It is then noted that if the samples according to the invention may have inclusions smaller in maximum size than reference 1 (free of Ti), most of the samples according to the invention also have inclusion densities evaluated by scanning electron microscopy lower than that of the reference (evaluated under the same conditions). Thus the density of inclusions with a diameter greater than 1.5 µm observed by SEM is low, more than twice lower than that of reference 1, and in addition the sizes of the largest particles observed on industrial castings are smaller (by approximately 1 µm) than what is observed on this reference.

[0097] Table 2 makes it possible to specify the preferred composition areas with regard to the inclusion population of the steels according to the invention.

[0098] The samples according to the invention Inv 9 to 13 suggest that up to 4% Cu (by controlling the production processes and the presence of residual elements according to the invention), the maximum size of the inclusions seems controlled.

[0099] Samples Inv 14 to 19, on the other hand, suggest preferential Nb compositions of less than or equal to 2%, and within this composition range, carbon contents of less than 0.007%, in order to avoid the formation of carbides larger than 10µm, or to favor the addition of other carbide-forming elements, such as Cr (allowing higher carbon levels in the presence of Nb).

[0100] Samples Inv 20 to 24 suggest a manganese content of less than or equal to 4% to avoid the formation of inclusions larger than 10 µm, and beyond these contents, the need to precisely control the proportion of free carbon (preferably below 10 ppm).

[0101] The low Co samples (with addition of aluminum and possibly addition of silicon and / or chromium), Ref 25, Ref 26, Inv 27 to 34, Inv 39 to 49, Inv 52, Inv 53, Inv 56 to 59, Inv 61, Ref 50 and Ref 51 have inclusions less than or equal to 10 µm (or even 8 µm) in diameter, particularly for associated oxygen contents less than 16 ppm.

[0102] The person skilled in the art knows that cold processing will only affect the size of the inclusions downwards, possibly by breaking them up, but cannot in any case increase these dimensions.

[0103] The grades according to the invention have the advantage, due to their intrinsic chemical composition, of not forming nitrides during production, and of allowing the size and nature of residual inclusions, in particular oxides, to be controlled. Thanks to careful control of the raw materials used and the production processes implemented, which provide low contents of residual elements N, S, C and P, and thanks to deoxidation of the liquid metal, the oxide particles formed are of limited size, less than or equal to 10 µm, preferably less than 8 µm, and of suitable compositions obtained by the production ranges described.Depending on the composition of the steel, aluminium-based oxides are then formed, for example mixed oxides of AI and Mg (this element inevitably coming from the slags and refractories of the production vessels) or alumina alone, but also oxides based on Si, Ca, Mg or other mixed oxides; sometimes some fine sulphides or carbides support its inclusion populations.

[0104] The important mechanical properties of the various samples are summarized in Tables 3, 4 and 5, Table 3 concerning samples in the hot-rolled stage, Table 4 concerning all the samples in the hot-rolled state after age-hardening annealing, and Table 5 characterizing all the samples in the cold-rolled and then aged state (for a reference treatment at 480°C for 3 h). The properties were measured in the longitudinal direction relative to the rolling direction of the strip.These properties are Vickers hardness HV 10 (for hot-rolled samples), maximum tensile strength Rm (expressed in MPa) for aged hot-rolled samples, conventional yield strength Rp 0.2 (expressed in MPa), maximum tensile strength Rm (expressed in MPa), distributed elongation Ar (expressed in % and measured from specimens of length L 0 equal to 5.65 times the square root of the initial section S 0 ) for cold-rolled samples, in unaged and aged states. Table 3: Vickers hardnesses Hv 10 of samples produced in the hot-rolled state Hv Average Standard deviation Ref 1 measure 1 308 312 3,32 measure 2 314 measure 3 313 Inv 13 measure 1 307 305 1,86 measure 2 304 measure 3 305 Inv 18 measure 1 332 331 2,10 measure 2 329 measure 3 333 Inv 19 measure 1 335 336 0,79 measure 2 336 measure 3 336 Inv 24 measure 1 292 293 0,55 measure 2 293 measure 3 292 Ref 3 measure 1 325 326 0,81 measure 2 326 measure 3 327 Ref 4 measure 1 324 324 0,70 measure 2 325 measure 3 324 Ref 5 measure 1 388 389 1,22 measure 2 390 measure 3 388 Inv 53 measure 1 301 300 1,93 measure 2 298 measure 3 302 Inv 56 measure 1 314 313 0,80 measure 2 312 measure 3 313 Inv 57 measure 1 343 342 0,59 measure 2 342 measure 3 342 Ref 58 measure 1 331 330 0,91 measure 2 331 measure 3 330 Inv 59 measure 1 301 300 1,25 measure 2 300 measure 3 299 Inv 60 measure 1 312 310 1,53 measure 2 310 measure 3 309 Ref 6 measure 1 297 297 0,36 measure 2 297 measure 3 297 Inv 61 measure 1 341 341 0,50 measure 2 341 measure 3 341 Table 4: Tensile strengths Rm of samples in the hot-rolled, aged state Sample Rm in hot rolled and aged condition (MPa) Ref.1 2078 Ref.2 1860 Inv.1 1925 Inv.2 2097 Inv.3 951 Inv.4 590 Inv.5 1883 Inv.6 1941 Inv.7 2016 Inv.8 2136 Inv.9 1869 Inv.10 1870 Inv.11 1945 Inv.12 990 Inv.13 2067 Inv.14 1927 Inv.15 2026 Inv.16 1981 Inv.17 1479 Inv.18 2109 Inv.19 2198 Inv.20 1917 Inv.21 2068 Inv.22 630 Ref.23 510 Inv.24 886 Ref.25 489 Ref.26 544 Inv.27 1318 Inv.28 1342 Inv.29 1512 Inv.30 1379 Inv.31 1379 Inv.32 1406 Inv.33 1672 Inv.34 1794 Inv.35 1651 Inv.36 1724 Inv.37 1949 Inv.38 1984 Inv.39 1329 Inv.40 1388 Inv.41 1622 Inv.42 1606 Inv.43 1581 Inv.44 1498 Inv.45 1673 Inv.46 1661 Inv.47 1683 Inv.48 1659 Inv.49 1685 Ref.50 1702 Ref.51 1802 Ref 3 2498 Ref 4 2089 Ref 5 2354 Inv 52 1712 Inv 53 1820 Inv 54 2668 Inv 55 2730 Inv 56 2107 Inv 57 2361 Ref 58 2503 Inv 59 2078 Inv 60 2065 Ref 6 2384 Inv 61 2349 Table 5: Mechanical properties of samples in the as-rolled cold-rolled state and in the aged cold-rolled state State Thickness mm Width mm Observed surface mm 2< Rm Mpa Rp0.2 Mpa Ar (%) Hv 1 HV 1 Average rough hardened Ref 1 0,42 7,00 2,92 1198,40 1126,50 5,73 369 372 370 370 aged 0,42 7,00 2,93 2132,45 2101,70 2,63 622 621 618 620 rough hardened Inv 13 0,42 7,00 2,94 1298,33 1274,00 5,50 378 373 375 375 aged 0,42 7,00 2,93 2067,33 2041,00 3,13 595 604 600 600 rough hardened Inv 18 0,416 7,00 2,91 1276,67 1254,67 5,87 371 373 370 371 aged 0,42 7,00 2,92 2109,00 2092,00 1,77 622 624 618 621 rough hardened Inv 19 0,43 7,00 2,98 1087,33 1071,67 9,73 328 330 324 327 aged 0,43 7,00 3,00 2189,33 2172,00 1,97 615 625 617 619 rough hardened Inv 24 0,42 7,00 2,97 1141,33 1109,00 9,80 365 371 369 368 aged 0,42 7,00 2,94 885,67 388,67 42,60 185 177 179 180 rough hardened Ref 3 0,42 7,00 2,96 1736,25 1685,26 6,34 512 514 510 512 aged 0,42 7,00 2,94 2512,54 2483,70 3,75 740 740 739 739 rough hardened Inv 54 0,42 7,00 2,92 1564,70 1532,63 7,56 461 461 460 461 aged 0,42 7,00 2,91 2687,24 2654,23 5,02 791 790 790 790 rough hardened Inv 55 0,42 7,00 2,93 1604,26 1576,35 7,32 329 334 331 331 aged 0,42 7,00 2,94 2736,45 2704,68 4,71 804 805 806 805 rough hardened Inv 56 0,42 7,00 2,92 1529,50 1492,10 5,68 452 452 451 451 aged 0,42 7,00 2,92 2238,76 2204,30 4,12 659 658 658 658 rough hardened Inv 57 0,42 7,00 2,94 1488,46 1445,98 3,84 438 439 438 438 aged 0,42 7,00 2,92 2365,40 2340,28 2,83 696 696 698 697 rough hardened Ref 58 0,42 7,00 2,93 1592,58 1567,36 5,24 468 468 469 468 aged 0,42 7,00 2,91 2546,59 2516,36 3,57 749 748 750 749

[0105] The mechanical characteristics obtained on the samples according to the invention in the hot and / or cold rolled aged state are similar to, or even improved upon, the references. Thus, the grades according to the invention combine economic attractiveness (through lower material costs by reducing the number of Ti, Co, etc. kilns) with high mechanical properties. For each alloy element Nb, Cu, Mn, W, Ta, V, a maximum tensile strength in the aged state of more than 1950 MPa is attainable by adjusting the composition and the processing method.

[0106] Table 4 illustrates Rm > 2000 MPa in the hot rolled state for adjusted contents of addition elements, making it possible to obtain martensitic structures capable of aging (so if for example Nb illustrates interesting hardening properties through samples Inv 14 to 19, Mn on the other hand suggests contents less than or equal to 4% and / or to control the added Cr content to avoid the formation of dominant austenite...). In addition, grades Inv 27 to 49, Inv 52 and Inv 61 according to the invention suggest Co + Mo contents greater than 9%, preferably greater than 15% to achieve mechanical characteristics in the aged state at least equivalent to references Ref 1 and Ref 3.

[0107] The compromise between these mechanical properties combined with a controlled inclusion population thanks to careful production conditions already illustrates the innovative nature of the invention, which is coupled with the improvement of surface properties after nitriding of materials for applications subject to fatigue.

[0108] The aging conditions were tested on hot and cold rolled products with a view to their optimization (after standardization annealing or solution treatment).

[0109] A solution annealing at 850°C for 1 hour in a reducing atmosphere was previously carried out on each grade, allowing access to a homogeneous structure. Then different couples (time-temperature) were tested on these annealed materials in order to specify aging conditions adapted to the targeted applications and grades invested.

[0110] Then, according to the aging conditions tested, under argon between 420°C and 550°C, the optimums in terms of hardness after aging and phases present were specified.

[0111] Grades Inv 1 to 4 containing V have ageing conditions identical to those commonly used for references 1 and 2 (for example between 450° and 500°C for treatments ≤ 3h), and allow to reach Rm in the aged state higher than 1900 MPa for V contents ≤ 4%; grades Inv 5 to 8 containing Ta have increased mechanical characteristics (Rm > 1940MPa) from 0.5% of Ta added under similar ageing conditions. Grades Inv 9 to 13 containing Cu have ageing conditions optimized around 500°C for treatments ≤ 2h (or 480°C-3h) allowing to reach Rm in the aged state higher than 1940 MPa from the addition of 2% of Cu; These aging performances are increased in the presence of Cr (< 2%) and Mn (< 1%) in accompaniment to structural hardening, i.e. for Co + Mo + Cu + Cr + Mn contents < 25%.Grades Inv 14 to 19 containing Nb have superior mechanical characteristics to Ref 2 after aging from low proportions of added Nb, and this in a wide range of aging conditions from 420°C to 550°C for durations of 30 minutes to 5 hours. An optimum treatment between 450° and 500°C for 2 hours is proposed.

[0112] The addition of Cr and Mn in controlled proportions increases age hardening. These grades, however, require controlling the Nb content to avoid the formation of inclusion clusters, or particles larger than the maximum values ​​required by the invention. Thus, an Nb content ≤ 4% is required.

[0113] Grades Inv 20 to 24 and Ref 25 and 26, which contain significant amounts of Mn (more than 0.19%), constitute the grades that can be biphasic, requiring a predominantly martensitic structure to be obtained in order to achieve optimal aging. Thus, grades with relatively limited Mn contents (traces ≤ Mn ≤ 4%) allow access to Rm > 1940 MPa for aging conditions identical to those commonly used for references 1 and 2 (for example, between 450° and 500°C for treatments ≤ 3 hours). In these controlled proportions of Mn, the controlled addition of Al, Si or Cr increases hardening by aging provided that a martensitic structure is maintained prior to aging.

[0114] Grades Ref 25 and 26 are, however, outside the invention, due to their Mn content which exceeds 13.0%. In fact, their inclusion population as described in Table 2 is not optimal, although it is at the limit of what is acceptable for the maximum size of the inclusions: the largest inclusions have an equivalent diameter of 10 µm and their inclusion densities of 1.73 and 1.75 inclusions / mm 2< are among the highest for this size class. And Table 4 shows that their Rm in the hot-rolled and aged state are frankly low (489 and 544 MPa).

[0115] In the steels of the invention as in the reference steels, the basis of the mechanical properties of maraging steels lies in the age hardening caused jointly by Co and Mo (and other addition elements). Thus low contents of Co (typically Co < 5%) and / or Mo (typically Mo < 5%) do not allow Rm of more than 1530 MPa to be reached after ageing. The use of higher proportions of Co (between 5 and 16%) or Mo (between 3 and 9%) then allows access to higher ranges of mechanical properties (tensile strength, fatigue endurance, etc.).These trends are confirmed by the characterizations of samples Inv 39 to 49 (for Co contents of 2 to 7%), which show that the addition of Al, Si or Cr does not allow compensation in terms of Rm in the targeted contents; i.e.: for Co: 1.0 to 10.0% and Mo = approximately 5%, maximum tensile strengths Rm, after aging of 1800 MPa cannot be exceeded, whatever the additions of Al up to 1%, Si up to 0.13%, Ti up to 0.1%, or Cr up to 0.5%.

[0116] The objective of the invention lies in an adjustment of mechanical properties brought to a given base by initial contents of Co, Mo elements chosen according to the targeted performances, without deteriorating the inclusion population and the fatigue behavior of the materials, and at lower cost. In many of the examples according to the invention, tensile strengths Rm greater than 1900 MPa after aging are targeted and obtained, also with inclusions of defined and controlled size, in particular to guarantee good fatigue behavior. Other endurance and mechanical property targets can be targeted and obtained with different variants of the invention by adjusting the contents of elements: Co, Mo, W, Cu, V, Nb, Mn, Si, Al, Cr, in particular.

[0117] Thus, grades Inv 27 to 38 containing relatively large quantities of W and AI can have mechanical characteristics superior to Ref 2 after aging for W contents preferably greater than 0.8% and Co contents greater than 10%. These performances after aging are increased with the addition of AI or Cr in accompaniment to structural hardening. Typically, aging conditions identical to those commonly used for grades Ref 1 and 2 make it possible to achieve Rm in the aged state of more than 1940 MPa for compositions Inv 37 and Inv 38.

[0118] It should be noted that grades Inv 48 and Inv 49 have Ti contents at the limit of what is acceptable (0.109%), which can be considered equal to 0.1% taking into account rounding and the usual precision of the analyses. They are not among the very best on the value of Rm, and Inv 48 has a maximum equivalent diameter of inclusions at the limit of what is acceptable and an inclusion density which is not optimal. These grades show that the limit of 0.1% of Ti must be respected to remain within the scope of the invention.

[0119] Grades Ref 50 and Ref 51 have S contents (0.004 and 0.0053%) exceeding the permissible limit (0.002%). In fact, their inclusion populations are not optimal. Ref 50 has a maximum equivalent diameter of inclusions of 10 µm, therefore at the limit of what is permissible, and an inclusion density of 0.81 inclusions / mm 2< , which is relatively average. Ref 51 has smaller but also more numerous inclusions. Their Rm in the hot-rolled and aged state is 1700 to 1800 MPa, which is not optimal. And the embrittlement of the grain boundaries induced by these slightly too high S contents makes hot transformation more difficult than what is desirable.

[0120] Inv 52 and Inv 53 are comparable to Ref 50 and Ref 51, except that their S contents are lower and in accordance with the invention. Their Rm in the hot-rolled and aged state is therefore slightly improved, and they have better fatigue endurance and a better capacity for hot transformation.

[0121] Inv 54 and Inv 55 are characterized by their high Mo content (approximately 9.9 and 11.8%). Their mechanical properties are high. Slightly higher C, Al or Cr contents than for other examples according to the invention ensure an acceptable quality / price ratio, even if it is not optimal. These examples illustrate the effect of Mo on the mechanical properties, but only partially meet the economic objectives that were set.

[0122] Inv 56 is representative of a grade with a high AI content. Inv 57 adds Cr and Ref 58 adds Cr and Zr in significant quantities. These examples, thanks to the addition of the elements mentioned, present interesting properties that can be optimized from the preferred contents shown previously.

[0123] Inv 59 has high Si and Y contents.

[0124] Ref 3 has too high an AI content, and therefore contains too large inclusions which could not be eliminated, and are unfavorable for the targeted fatigue applications.

[0125] Ref 4 and Ref 5 contain too much S, which therefore forms too many sulfides which, moreover, serve as germination sites for oxides, explaining the presence of too large inclusions on hot-rolled products.

[0126] Ref 6 has an excessive Y content, which forms oxidized inclusions of too large size, which could not be eliminated by decantation of the liquid metal.

[0127] Inv 60 is representative of a high presence of Ca and Inv 61 of a high presence of Mg. They show that within the framework of the invention, these two deoxidizers can be used in significant quantities, while requiring compliance with the rules known to those skilled in the art in terms of properties of refractories and refining.

[0128] It is notable here that the grades according to the invention are compatible with aging conditions which allow increased mechanical characteristics, but that they also present ease of implementation both in terms of processes and associated costs. Indeed, the stability of the properties obtained, in particular the hardness, allows the implementation of short-term annealing (typically 30 minutes) to obtain properties identical or comparable to those obtained by treatments lasting 2 to 5 hours on conventional grades. These qualities of simplicity and economy of heat treatments are particularly advantageous for these economic grades targeted according to the invention.

[0129] The new grades according to the invention have interesting mechanical properties (hardness, elastic limit, breaking strength, etc.) which can be optimized for certain applications, known as "unlimited" endurance, intended to be subjected to high fatigue stress. Thus, these aging conditions and an inclusion population optimized according to the invention allow, thanks to subsequent surface treatments (nitriding, carbonitriding, cementation, shot peening, etc.), access to improved properties during dynamic stresses, for example in fatigue.

[0130] Finally, the improved properties of these grades according to the invention were also tested after a surface compression treatment. In this case, on thin materials subjected to fatigue stress, nitriding treatments were applied before stressing, in order to delay the onset of surface cracking. This compression can also be achieved by shot peening, in a known manner.

[0131] Thus, various nitriding conditions were tested for the grades according to the invention, including treatments between 420 and 480°C for 30 to 90 min in a gaseous atmosphere (under an atmosphere of cracked NH 3).

[0132] The nitrided layers are then formed by the diffusion of nitrogen within the various matrices, constituting characteristic thicknesses of a few tens of µm, evaluated by chemical attack or profile by glow discharge spectrometry (GDS). They sometimes contain uniformly distributed fine precipitates, the chemical nature of which can possibly, if useful, be adjusted by adjusting the composition of the steel and the nitriding conditions.

[0133] There figure 1illustrates the density of hardening phases obtained on sample Inv.15 after nitriding at 420°C for 30 min, by characterization with a transmission electron microscope on a thin section. The hardening precipitates are essentially Mo x Nb y (with x = 2y approximately) uniformly distributed, whose size varies from 80 to 400 nm. There are also some Nb and Mo carbides and nitrides, of smaller dimensions, and with specific stoichiometry and lattice parameters.

[0134] In the temperature and duration ranges explored, the grades according to the invention reveal increased surface properties after nitriding. Table 6 illustrates as an example hardness levels evaluated by micro indentation using identical methods (average of three Hv 0.1 measurements carried out on the surface). The various nitriding conditions were investigated in gas nitriding under cracked NH 3 ; these conditions can also be adapted in ionic nitriding, carbonitriding or others in order to obtain similar properties. Table 6: Average Hv0.1 hardnesses evaluated by micro-indentation at the extreme surface according to different nitriding conditions. 420°C 450°C 480°C 510°C 30 min 60 min 90 min 30 min 60 min 90 min 30 min 60 min 90 min 30 min Ref 1 623 949 613 794 911 943 820 930 890 792 Ref 2 775 730 923 843 900 680 Ref 51 325 320 488 285 355 613 Inv 1 643 643 698 808 790 403 Inv 6 623 735 815 608 623 575 Inv 7 578 370 588 620 940 787 Inv 8 1033 475 778 638 920 747 Inv 9 803 875 623 670 485 762 Inv 10 705 888 530 810 805 475 Inv 11 803 658 665 885 755 777 Inv 13 325 870 910 995 835 1025 1030 900 908 Inv 14 853 1070 730 593 875 743 Inv 15 810 790 568 543 665 713 Inv 16 523 590 580 490 473 598 Inv 18 750 1280 635 1018 885 653 1088 815 890 Inv 21 558 548 405 815 823 837 Inv 24 380 1160 305 1030 320 543 380 908 625 Inv 38 220 215 275 280 Ref 3 748 882 1019 1048

[0135] It should be understood that measurement uncertainties in this type of test are significant when, as is the case here, the tests are carried out on samples with rough surfaces and local indentations. The results in Table 7 should therefore be interpreted in terms of a general trend.

[0136] Thus, in addition to excellent mechanical properties, controlled material costs and a controlled inclusion population, the samples according to the invention have a nitriding capability allowing access to increased surface hardness levels as well as increased resistance to friction, compared to reference samples 1 and 2. Thus, similar extreme surface hardness levels compared to references 1 and 2 can be expected (for example Hv0.1 > 900), or even for certain grades according to the invention gains of more than 50 Hv0.1 in the extreme surface are accessible for reduced nitriding times. It is thus possible to achieve extreme surface hardnesses of more than 1000 Hv0.1 (or even 1050 Hv0.1) on the grades according to the invention, under suitable nitriding conditions which are not particularly demanding.

[0137] However, for certain applications subject to fatigue, it is advisable not to reach excessively high surface hardness levels (Hv0.1 hardness) compared to the aged core of the material (Hv10 hardness) in order to avoid weakening the internal interface or the extreme surfaces. For these purposes, nitrogen diffusion profiles that evolve regularly according to the depth of the material are preferred to abrupt diffusion profiles leading to the presence of significant and heterogeneous precipitation zones on the surface. In steels, these areas are called "combination layers", and are made up, for example, of brittle and extremely hard iron nitrides.In this context, it was verified, for the samples according to the invention, the existence of gas nitriding conditions making it possible to avoid the formation of iron nitrides at the extreme surface, while maintaining sufficient stress levels at the surface to delay the initiation of cracking under dynamic stress in service (in the target surface hardness ranges).

[0138] The minimum and maximum hardness values ​​reached at the extreme surface (hardnesses Hv0.1) according to the different nitriding conditions (temperature, duration) are reported in the figure 2 . We see that extreme surface hardness levels greater than 900 Hv0.1 are accessible for each major family of hardening element present according to the invention. We can thus access surface fatigue properties at least equivalent to those of the previously cited references.

[0139] It is found that Mn or Cu grades produced on industrial tools with a quantified addition of Cr can exhibit increased extreme surface hardnesses after nitriding compared to the grades according to the invention free of Cr, and that a similar effect can be expected by adding defined proportions of AI together with a hardening element (such as Ta, see Inv 8).

[0140] Thus, for levels of Co and Mo sufficient to obtain the targeted mechanical properties detailed above, the invention illustrates the possibility of achieving extreme surface hardnesses greater than 900 HV0.1 for each family of grades according to: values ​​lower than 900 Hv0.1 are observed on vanadium grades for hardening element contents lower than 0.5%; beyond this, increased hardnesses are expected at the extreme surface; for tantalum grades according to the invention (Inv 6 to 8 of table 7) hardness levels higher than 940 Hv 0.1 are reached at the extreme surface from 3% of Ta added (with adjusted nitriding conditions); Cu grades also have increased hardness levels (and residual stresses) at the extreme surface from 2% of hardening element and in the presence of Cr and Mn (Inv 13); these elements promote the solubility of nitrogen at the surface; Grades according to the invention 14 to 18, on the other hand, suggest vanadium levels lower than 2% in order to reach sufficient hardness levels at the extreme surface (free from combination layer).The Mn grades presenting a good compromise between mechanical properties and inclusion population present increased levels of hardness at the extreme surface in the presence of Cr (Inv 24). The W and Al grades tested (Inv 38 and Ref 51) have not yet made it possible to specify the nitriding conditions allowing high levels of hardness to be achieved at the extreme surface.

[0141] Finally, it was verified that these significant hardnesses accessible on the surface are accompanied by controlled residual stresses (evaluated by X-ray diffraction) allowing the surface to be put into compression relative to the matrix and thus delay the onset of surface cracking.

[0142] There figure 3is a qualitative evaluation of the residual compressive stresses on the surface of nitrided rolled sheets, for samples Ref 1, Ref 2, and various samples according to the invention. For each sample, the minimum and maximum values ​​of the compressive stresses evaluated for all the tests carried out by varying the nitriding temperatures and times were recorded. The evaluation of the residual stresses within the nitrided layers was carried out on the surface of the samples by X-ray diffraction with the following parameters: Chi varying from 0 to 51°, measurement interval 1s, sin 2< (psi) from 0 to 0.6 in steps of 0.1. The values ​​obtained under these conditions make it possible to determine, by following the evolution of the position of the Fe line, the level of stresses on the surface of the material. It can be seen that the residual stresses of the samples according to the invention are improved compared to those observed on the reference samples 1.

[0143] Thus, it is easier, by using the invention, to control the properties of the nitrided layer and, therefore, to adapt it to the particular needs of the use envisaged for future products. If this seems preferable, it is thus easy to avoid the presence at the extreme surface of phases commonly called "combination layers" within the nitrided layers. These phases result from the precipitation of iron nitrides of the Fe 4 N, Fe 2 N, Fe 2 N 1-x types in particular.

[0144] The characterizations of the nitrided layers of certain samples (reference Ref 1 and according to the invention Inv 13, Inv 18, Inv 21 and Inv 24) were completed by the execution of tests commonly called “scratch tests”, derived from “scratch tests”, or “sclerometric tests” and distinguished by the notion of low load applied.

[0145] These tests consist of generating supports through the nitrided layer-substrate system, using a sphero-conical tip, such as a diamond tip for Rockwell C hardness tests (angle of 120°, tip radius of curvature 100 µm), by applying a constant substrate running speed and an increasing load to the tip.

[0146] The degradation of a coating under the application of a load is a combination of elastic and / or plastic indentation stresses, frictional stresses as well as residual stresses internal to the material.

[0147] Under low loads, these stresses can cause tension or compression cracking of the coating surface, which, however, continues to adhere to the substrate.

[0148] The scratch test is a comparative test that allows the detection of a sound wave during the propagation of possible microcracks in the material and the penetration depth of the indentation tool during support (compared to the actual surface initially probed), and to evaluate the residual depth of the coating on the test path at the end of the test. This last estimation makes it possible to evaluate the elastic return of the coating-substrate or surface-substrate system after the application of an increasing load, at low loads.

[0149] On each system, three successive measurements are carried out on the surface of the nitrided samples, spaced 1 mm apart, by applying an increasing load of 0.03 to 10 N over 10 mm of the nitrided surface.

[0150] Thus, if, for the various samples according to the invention, the results differ little in terms of evaluation of the normal force, or of the penetration depths, certain characteristics of the nitrided layers according to the invention are distinguished, however.

[0151] So the figure 4 illustrates the elastic return of the nitrided layer-substrate system at the end of the scratch test by relative difference of the penetration depths (significantly decreasing curves) and the residual depths at the end of the scratch test on the nitrided samples Inv. 21 and Inv. 24 (respectively treated at 480 and 450°C for 30 minutes in a gas atmosphere).

[0152] Inv 21 is an example containing Mn (1.970%) and where the Cr content (0.007%) results only from impurities present in the raw materials used. Inv 24 is an example containing 1.930% Mn, therefore a content comparable to that of Inv 21, but associated with a Cr content of 0.902%, therefore corresponding to a very significant addition of Cr. These two samples give comparable results on the penetration depths during the support phase of the scratch test, but the curves are more irregular in the case of Inv 21 than in the case of Inv 24.

[0153] There Figure 5 illustrates the associated acoustic emission results during the scratch test on these two same nitrided Inv 21 and Inv 24 samples. Here, the differences are clearly more significant, these emissions being higher in the case of Inv 21 than in that of Inv 24.

[0154] Thus the addition of Mn associated with an addition of Cr reveals a lower noise on the evaluated depths, which is found in the significant reduction of acoustic emission of Inv. 24 nitrided ( Figure 5 ).

[0155] Such behavior is also observed on other shades according to the invention containing Cr.

[0156] It therefore appears that the significant presence of Cr reduces the potential cracking of the nitrided layers of the grades according to the invention, under the application of low loads (< 10 N), which is the case in particular when using parts subjected to fatigue stress locally subjected to friction, support or friction of parts between them.

[0157] Likewise the figure 6illustrates the elastic behavior of the nitrided layer-substrate assembly at the end of the scratch test on the nitrided samples Inv. 13, Inv. 18, Inv. 21 and Inv. 24, in comparison with the sample Ref 1 (average curves of the three tests carried out per sample, respectively treated under gas atmosphere at 480 - 30 minutes for Inv. 13, Inv 18, Inv 21 and Ref 1, and at 450°C-30 minutes for Inv 24). Thus, the shifts of the curves relative to the abscissa axis of the residual depth curves illustrate the residual plastic deformation at the end of the test.

[0158] There figure 6reveals an increased elastic behavior of the nitrided layers of the samples according to the invention, compared to that of the nitrided layers obtained on Ref 1. Indeed, the elastic return evaluated by the difference between the curves of penetration depths and residual depths is significantly increased for the samples containing Cu (Inv 13 which also contains Cr) or Nb (Inv 18). There is a variation in altitude of approximately 15 µm in thickness for these samples, and of 13 µm on the grades with Mn (Inv. 21) and Mn + Cr (Inv 24 which also contains a little Si), therefore twice as important as for Ref 1 which does not contain these alloying elements and whose Co content (16.50%) is higher than that of the samples according to the invention tested (of the order of 13%). The Mo contents are of the order of 5.0 to 5.30% for all these samples.

[0159] In addition, the residual depths evaluated rd are low for the samples according to the invention Inv 13, Inv 18, Inv 21, Inv 24, and slightly better than for Ref 1.

[0160] This behavior reflects an improved elastic return of the nitrided layers according to the invention, which is of major interest in the context of applications where the parts are subjected to fatigue stress, since it makes it possible to reduce the plastic deformations of the substrate / nitrided layer assembly, and thus to reduce the friction and friction generated in certain applications by the plastic deformations of assemblies requiring precise dimensions.

[0161] Thus, for the application to CVT belts, which are made up of a superposition of cold-rolled maraging steel rings, and which are subjected to bending and tensile fatigue by the torque transmitted from the engine, the gap between each ring ensures the lubrication of the assembly, and does not accept plastic deformation which could damage the rings under cyclic stresses. At the end of each stress cycle, the nitrided materials according to the invention are less plastically deformed, thus not inducing cumulative plastic deformations of the parts over time, which could ultimately alter the fatigue lives of the reference nitrided materials.

[0162] So the figure 6confirms a plastic deformation under low load, 10 N, greater than that obtained on the samples according to the invention. This is shown by the deviation from the horizontal axis a of the different residual penetration curves.

[0163] Thus, Ref 1 seems to deform less than the grades according to the invention during the scratch test (as shown by their relative penetration depths), but the deformation mechanisms implemented are not entirely the same, and the residual stresses at the end of these stresses do not generate the same effects. Thus, if the deformation generated on Ref 1 during the test seems less significant, (by the penetration depth evaluated), its resultant at the end of the test has an increased plastic component compared to the samples according to the invention, which is detrimental for the applications primarily targeted by the invention.

[0164] The penetration depths observed on the samples according to the invention prove to be essentially elastic, unlike Ref 1 which exhibits less elastic return under low load.

[0165] These criteria for the behavior of the nitrided surface, associated with a controlled inclusion population and the mechanical properties inherent in the composition of the steel, were not highlighted by previous studies conducted on maraging steels of the general type to which the invention relates, in particular with a view to use for CVT type transmission belts.

[0166] Generally speaking, the steels according to the invention exhibit, under different nitriding conditions, increased economic performance and usage properties that are at least equal, or even increased, compared to the reference steels of the prior art, insofar as the nitriding layer is more easily controllable: for its composition, in particular concerning the existence or not of combination layers; for its thickness; for the hardness levels accessible under given nitriding conditions; for the distribution in the thickness of the layer of the nitrogen contents, of the precipitated phases, of their nature and their distribution, as well as the hardness levels, of the residual stresses; by a reduced level (almost zero) of plastic deformation induced in these nitrided layers, stressed under low load; for the ease and economy of the conditions of industrial implementation of the nitriding, with equal properties obtained compared to the reference grades, whether the nitriding is carried out by plasma or, above all, by gas.

[0167] Preferred applications of the invention are, in particular: for products made from hot-rolled or hot-formed semi-finished products, turbine shafts or transmission parts in general; but also blades of rotating machines (wind turbines, centrifuges, etc.) for products made from cold-rolled sheets or strips, elements of transmission belts for vehicles or rotating machines such as machine tools, in particular belts for automatic transmissions of CVT-type motor vehicles.

Claims

1. Steel, characterized in that it has the following composition in weight percent: - 10.0 % ≤ Ni ≤ 24.5 %; - 1.0 % ≤ Mo ≤ 12.0 %; - 1.0 % ≤ Co ≤ 18.0 %; - 14.0 % ≤ Mo + Co + Si + Mn + Cu + W + V + Nb + Zr + Y + Ta + Cr + C + Al + B + Ti + N ≤ 29.0 %; - 25.0 % ≤ Ni + Co + Mo ≤ 40.0%; - traces ≤ Al ≤ 2.0 %; - traces ≤ Ti ≤ 0.1 %; - traces ≤ N ≤ 0.010 %; - traces ≤ Si ≤ 2.0 %; - traces ≤ Mn ≤ 13.0 %; - traces ≤ C ≤ 0.03 %; - traces ≤ S ≤ 0.0020 %; - traces ≤ P ≤ 0.005 %; - traces ≤ B ≤ 0.01 %; - traces ≤ H ≤ 0.0005 %; - traces ≤ O ≤ 0.03 %; - traces ≤ Cr ≤ 5.0 %; - traces ≤ Cu ≤ 4 %; - traces ≤ W ≤ 6.0 %; - traces ≤ Zr ≤ 4.0 %; - traces ≤ Ca ≤ 0.1 %; - traces ≤ Mg ≤ 0.8%; - traces ≤ Nb ≤ 4.0 %; - traces ≤ V ≤ 4.0 %; - traces ≤ Ta ≤ 4.0 %; - traces ≤ Y ≤ 4.0 %; - Si + Mn ≥ 0.13% ; - 0.14 % ≤ Al + Si + Cu + Nb + Mn + V + Ta + Cr + W + C + B + Y + Zr + Ti + N ≤ 8.0 %; the remainder being iron and manufacturing impurities; and in that the inclusion population observed under image analysis on a polished surface of 650 mm2 if the steel is in the form of a hot worked part or hot rolled sheet, and 800 mm2 if the steel is in the form of cold rolled sheet, does not contain non-metallic inclusions having an equivalent diameter larger than 10 µm, the metallic inclusions being oxides, sulphides and nitrides.

2. Steel product that is hot worked and optionally heat treated, characterized in that it has the following composition in weight percent: - 10.0 % ≤ Ni ≤ 24.5 %; - 1.0 % ≤ Mo ≤ 12.0 %; - 1.0 % ≤ Co ≤ 18.0 %; - 14.0 % ≤ Mo + Co + Si + Mn + Cu + W + V + Nb + Zr + Y + Ta + Cr + C + Al + B + Ti + N ≤ 29.0 %; - 25.0 % ≤ Ni + Co + Mo ≤ 40.0%; - traces ≤ Al ≤ 2.0 %; - traces ≤ Ti ≤ 0.1 %; - traces ≤ N ≤ 0.010 %; - traces ≤ Si ≤ 2.0 %; - traces ≤ Mn ≤ 13.0 %; - traces ≤ C ≤ 0.03 %; - traces ≤ S ≤ 0.0020 %; - traces ≤ P ≤ 0.005 %; - traces ≤ B ≤ 0.01 %; - traces ≤ H ≤ 0.0005 %; - traces ≤ O ≤ 0.03 %; - traces ≤ Cr ≤ 5.0 %; - traces ≤ Cu ≤ 4 %; - traces ≤ W ≤ 6.0 %; - traces ≤ Zr ≤ 4.0 %; - traces ≤ Ca ≤ 0.1 %; - traces ≤ Mg ≤ 0.8%; - traces ≤ Nb ≤ 4.0 %; - traces ≤ V ≤ 4.0 %; - traces ≤ Ta ≤ 4.0 %; - traces ≤ Y ≤ 4.0 %; - Si + Mn ≥ 0.13% ; - 0.14 % ≤ Al + Si + Cu + Nb + Mn + V + Ta + Cr + W + C + B + Y + Zr + Ti + N ≤ 8.0 %; the remainder being iron and manufacturing impurities; and in that the inclusion population observed under image analysis on a polished surface of 650 mm2 of a hot worked part or of hot rolled sheet does not contain non-metallic inclusions having an equivalent diameter larger than 10 µm, the metallic inclusions being oxides, sulphides and nitrides.

3. The steel product hot worked according to claim 2, optionally heat treated, characterized in that it has an at least 70 % martensitic structure, a tensile strength of 2030 MPa or higher, an offset yield strength of 2000 MPa or higher and a uniform elongation of 1 % or higher, and Vickers hardness of 285 Hv10 or higher, this hardness being evaluated along a cross-section of the hot worked product.

4. Cold rolled sheet or strip made of steel, characterized in that it has the following composition in weight percent: - 10.0 % ≤ Ni ≤ 24.5 %; - 1.0 % ≤ Mo ≤ 12.0 %; - 1.0 % ≤ Co ≤ 18.0 %; - 14.0 % ≤ Mo + Co + Si + Mn + Cu + W + V + Nb + Zr + Y + Ta + Cr + C + Al + B + Ti + N ≤ 29.0 %; - 25.0 % ≤ Ni + Co + Mo ≤ 40.0%; - traces ≤ Al ≤ 2.0 %; - traces ≤ Ti ≤ 0.1 %; - traces ≤ N ≤ 0.010 %; - traces ≤ Si ≤ 2.0 %; - traces ≤ Mn ≤ 13.0 %; - traces ≤ C ≤ 0.03 %; - traces ≤ S ≤ 0.0020 %; - traces ≤ P ≤ 0.005 %; - traces ≤ B ≤ 0.01 %; - traces ≤ H ≤ 0.0005 %; - traces ≤ O ≤ 0.03 %; - traces ≤ Cr ≤ 5.0 %; - traces ≤ Cu ≤ 4 %; - traces ≤ W ≤ 6.0 %; - traces ≤ Zr ≤ 4.0 %; - traces ≤ Ca ≤ 0.1 %; - traces ≤ Mg ≤ 0.8%; - traces ≤ Nb ≤ 4.0 %; - traces ≤ V ≤ 4.0 %; - traces ≤ Ta ≤ 4.0 %; - traces ≤ Y ≤ 4.0 %; - Si + Mn ≥ 0.13% ; - 0.14 % ≤ Al + Si + Cu + Nb + Mn + V + Ta + Cr + W + C + B + Y + Zr + Ti + N ≤ 8.0 %; the remainder being iron and manufacturing impurities; and in that the inclusion population, observed under image analysis on a polished surface of 800 mm2, does not contain non-metallic inclusions having an equivalent diameter larger than 10 µm, the metallic inclusions being oxides, sulphides and nitrides.

5. Cold rolled sheet or strip according to claim 4, characterized in that it has been subjected to at least one heat treatment after cold rolling to harden the material.

6. Hot or cold rolled sheet or strip according to one of claims 2 to 5, characterized in that it has a tensile strength 2030 MPa or higher, an offset yield strength of 2000 MPa or higher, and uniform elongation of 1 % or higher.

7. Steel product, characterized in that it is derived from hot or cold rolled sheet or strip according to one of claims 2 to 6, optionally formed, and in that it has undergone surface treatment to improve the dynamic strength thereof.

8. The product according to claim 7, characterized in that said surface treatment is selected from among carburization, gas nitriding, ionic nitriding, carbonitriding and shot peening.

9. Turbine shaft, characterized in that said shaft comprises at least one element made from a hot worked product according to claim 2 or 3.

10. Hot formed transmission part, characterized in that said part comprises at least one element made from a hot worked product according to claim 2 or 3.

11. Transmission belt, characterized in that it comprises at least one element made from cold rolled sheet or strip according to one of claims 4 to 8, or from a product derived from said sheet or strip.

12. The transmission belt according to claim 11, characterized in that it is an automotive transmission belt of CVT type.

13. Steel product that has been hot worked and optionally heat treated according to one of claims 2 or 3, or sheet or strip that is cold rolled and optionally heat treated according to one of claims 4 to 6, characterized in that the grain size of the product or of the sheet or strip is 5 ASTM or finer.