METHOD FOR INCREASING THE SURFACE ROUGHNESS OF A METAL LAYER
Patent Information
- Application Number
- DE602021020599
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-11-27
- Filing Date
- 2021-11-26
- Publication Date
- 2024-10-23
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for increasing the surface roughness of metal layers are limited, as they require specific plasma etching recipes for each metal and are not applicable to all metals, particularly noble metals and their alloys, which cannot be etched by reactive ion etching.
A method involving the deposition of a sacrificial nitrogen-containing dielectric layer, exposure to an etching plasma to create asperities, and subsequent etching of the metal layer to transfer the roughness, allowing for increased surface roughness applicable to all metals using various etching techniques.
This method effectively increases the surface roughness of metal layers without the need for specific plasma etching recipes for each metal, making it applicable to all metals, including noble metals, and allows for the reduction of forming voltage in resistive memory cells, improving their performance.
Description
TECHNICAL FIELD
[0001] The present invention relates to a method for increasing the surface roughness of a metal layer and its application when manufacturing a resistive memory cell or when forming a via between two metal lines. STATE OF THE ART
[0002] In a metal-insulator-metal (MIM) electronic device such as a capacitor or resistive memory cell, the surface roughness of the metal layers forming the electrodes can have a significant impact on the electrical properties of the device.
[0003] Documents WO 00 / 49651, US 2015 / 236136, WO 2015 / 186064, WO 2016 / 062613 and FR 3 000 602 describe modifying the surface roughness of metal layers.
[0004] For example, in an oxide-based resistive memory (OxRAM) cell comprising a lower electrode, an upper electrode and an active material of variable electrical resistance arranged between the electrodes, the roughness of the lower electrode influences the so-called forming voltage of the memory cell. The forming voltage of an OxRAM cell is the voltage value at which the memory cell switches from a blank state, characterized by a very high (so-called initial) resistance, to a low resistive state. The forming voltage is higher than the nominal operating voltage of the memory cell, which allows the memory cell to be erased or written (transition from the low resistive state to a high resistive state, or vice versa).
[0005] In the article [“Impact of roughness of TiN bottom electrode on the forming voltage of HfO2 based resistive memories”, Microelectronic Engineering, 2020, vol. 221, p. 111194], C. Charpin-Nicolle et al. show that increasing the roughness of the titanium nitride (TiN) bottom electrode has the effect of reducing the forming voltage of the memory cell. A lower forming voltage is advantageous because it allows for a smaller memory circuit (selection transistors, voltage generator circuit) and improves the endurance of the memory cells.
[0006] The TiN bottom electrode is roughened by exposure to a reactive ion etching (RIE) plasma. Different plasma chemistries, each associated with specific etching conditions, allowed the surface roughness to vary in root mean square value from 0.4 nm to 14 nm.
[0007] Increasing roughness by RIE, however, requires developing a specific recipe for each electrode material, by adjusting the numerous process parameters (reactive gas mixture and concentrations, pressure, RF powers, temperatures, etc.). However, for some metals, it is impossible to generate roughness by RIE, as no set of parameters can activate a random and non-uniform etching mechanism. Finally, other metals cannot be etched by RIE (because they do not produce volatile subspecies), but only by ion beam etching (or IBE). However, by nature, ion beam etching is not a technique for increasing roughness. SUMMARY OF THE INVENTION
[0008] There is therefore a need to provide a method for increasing the surface roughness of a metal layer, which is applicable to all metals.
[0009] According to a first aspect of the invention, this need is tended to be satisfied by providing a so-called “roughening” process comprising the following steps: depositing on the metal layer a sacrificial layer of a dielectric material comprising nitrogen; exposing a surface of the sacrificial layer to an etching plasma so as to create asperities; etching the metal layer through the sacrificial layer, so as to transfer the asperities of the sacrificial layer into at least part of the metal layer.
[0010] This roughening process makes it possible to increase the roughness of a metal layer, regardless of the material it is made of, without the need to develop a plasma etching recipe specific to each metal, because the roughness is generated in the sacrificial layer of dielectric material. It is applicable to all metals, because all metal etching techniques (IBE, RIE, etc.) can be used to transfer the asperities of the sacrificial layer into the metal layer. In particular, the roughening process according to the invention is applicable to noble metals and their alloys (which can only be etched by an ion beam), unlike the roughening process of the prior art.
[0011] The dielectric material comprising nitrogen may be selected from silicon nitrides (Si x N y ), silicon carbonitride (SiCN) and silicon boron carbonitride (SiBCN).
[0012] Preferably, the etching plasma is formed from a mixture of reactive gases comprising a gas containing oxygen, a gas containing silicon and fluorine or silicon and chlorine and a fluorocarbon gas (C x F y ), optionally hydrogenated (C x H y F z ).
[0013] For example, the gas containing oxygen is O 2 , the gas containing silicon and fluorine or silicon and chlorine is SiCl 4 or SiF 4 and the hydrogenated fluorocarbon gas is CH 3 F.
[0014] In a particular embodiment of the roughening process, the dielectric material is a silicon nitride (Si x N y ) and the etching plasma is generated in a chamber of a reactive ion etching reactor under the following conditions: a flow rate of SiCl 4 or SiF 4 entering the reactor chamber of between 2 sccm and 5 sccm; a flow rate of O 2 entering the reactor chamber of between 40 sccm and 250 sccm; a flow rate of CH 3 F entering the reactor chamber of between 40 sccm and 250 sccm; a power emitted by a reactor source of between 100 W and 1000 W; a bias voltage of between -200 V and -500 V; a pressure in the reactor chamber of between 6.666 Pa and 19.998 Pa; a substrate holder temperature of between 20 °C and 100 °C; and a temperature of the walls of the reactor chamber of between 50 °C and 80 °C.
[0015] The roughening method may further comprise, after the step of etching the metal layer, a step of selectively removing the sacrificial layer. Alternatively, the sacrificial layer may be entirely consumed during the step of etching the metal layer.
[0016] The method according to the first aspect of the invention may also have one or more of the following characteristics, considered individually or in all technically possible combinations: the sacrificial layer has, after the step of exposure to the etching plasma, a surface roughness, expressed as a quadratic mean value, greater than or equal to 10 nm, and preferably between 10 nm and 30 nm; the metal layer initially has a surface roughness, expressed as a quadratic mean value, strictly less than 1 nm; the metal layer is etched by means of an etching process having a selectivity with respect to the sacrificial layer of between 1 and 2 or strictly greater than 2.
[0017] A second aspect of the invention relates to a method of manufacturing a resistive memory cell comprising a first electrode, a second electrode and a resistive layer disposed between the first and second electrodes, the method comprising the following steps: depositing a first metal layer on a substrate; increasing the roughness of the first metal layer by means of a method according to the first aspect of the invention; depositing a layer of material with variable electrical resistance on the first metal layer and a second metal layer on the layer of material with variable electrical resistance; etching the first metal layer, the layer of material with variable electrical resistance and the second metal layer, so as to delimit respectively the first electrode, the resistive layer and the second electrode of the resistive memory cell.
[0018] A third aspect of the invention relates to a method of forming a via extending to a metal barrier layer, the method comprising the following steps: depositing a first dielectric layer on the metal barrier layer, the first dielectric layer being made of a material comprising nitrogen; depositing a second dielectric layer on the first dielectric layer; forming in the second dielectric layer a cavity opening onto the first dielectric layer; exposing at the bottom of the cavity a surface of the first dielectric layer to an etching plasma so as to create asperities; etching the metal barrier layer through the first dielectric layer, so as to transfer the asperities of the first dielectric layer into at least a portion of the metal barrier layer; and filling the cavity with at least one metal.
[0019] A fourth aspect of the invention relates to a method for increasing the surface roughness of a dielectric layer made of a silicon nitride (Si x N y ), the method comprising a step of exposing the sacrificial layer to an etching plasma, the etching plasma being formed from a mixture of reactive gases comprising a gas containing oxygen, a gas containing silicon and fluorine or silicon and chlorine and a fluorocarbon gas (C x F y ), optionally hydrogenated (C x H y F z ). BRIEF DESCRIPTION OF THE FIGURES
[0020] Other characteristics and advantages of the invention will emerge clearly from the description given below, for information purposes only and in no way limiting, with reference to the following figures. [ Fig. 1A], [Fig. 1B], [Fig. 1C] and [Fig. 1D ] represent steps of a method for increasing the surface roughness of a metal layer; [ Fig. 2A], [Fig. 2B] and [Fig. 2C] represent steps of a method of manufacturing a resistive memory cell, in which the method of Figures 1A-1D is implemented; [ Fig. 3A], [Fig. 3B] and [Fig. 3C ] represent steps of a method of forming a via, in which the method of Figures 1A-1D is implemented.
[0021] For clarity, identical or similar elements are identified by identical reference signs throughout the figures. DETAILED DESCRIPTION
[0022] THE Figures 1A to 1C schematically represent steps S11 to S13 of a method for increasing the roughness of a metal layer 10. By metal layer is meant a layer formed from a material whose atoms are united by metallic bonds. This material (a metal) can be a simple body, such as titanium (Ti), tantalum (Ta), platinum (Pt), gold (Au) or ruthenium (Ru); an alloy of several metallic elements, for example an aluminum copper alloy (AICu); an alloy of a metallic element with a non-metallic element, such as a metallic silicide (e.g. AISi), a metallic nitride (e.g. TiN, TaN) or a metallic carbide.
[0023] The metal layer 10 may be arranged on a substrate (not shown), for example made of silicon. It is for example formed by physical vapor deposition (or PVD). Its thickness is preferably greater than or equal to 100 nm.
[0024] The metal layer 10 initially (i.e. immediately after its deposition) has a surface roughness strictly less than 1 nm. This roughness value, as well as all those given subsequently, are expressed as a root mean square value. The root mean square roughness (denoted Rq) is determined by a statistical analysis of an atomic force microscope image, taking as a sample a surface of 5x5 µm 2< .
[0025] In reference to the Figure 1A, the roughness increasing method, also called roughening method, comprises a first step S11 of depositing a sacrificial layer 11 on the metal layer 10. The sacrificial layer 11, also called transfer layer or hard mask layer, is formed from a dielectric material comprising nitrogen. Preferably, the dielectric material has a nitrogen content of between 20% and 50%. By way of example, the dielectric material is chosen from silicon nitrides (Si x N y ; all stoichiometries are possible), silicon carbonitride (SiCN) and silicon boron carbonitride (SiBCN).
[0026] The sacrificial layer 11 is for example formed by plasma-enhanced chemical vapor deposition (PECVD).
[0027] The next step S12, represented by the Figure 1B, consists of exposing the surface of the sacrificial layer 11 to an etching plasma so as to generate asperities 12. The asperities 12 are protruding patterns having a random shape and distributed non-uniformly on the surface of the sacrificial layer 11. These patterns are obtained by partially etching the sacrificial layer 11, by a micro-masking effect (deposition of a portion of the plasma ions in the form of a polymer layer of variable thickness and simultaneous etching of the dielectric layer and the polymer layer, the dielectric layer and the polymer layer having different etching speeds).
[0028] The formation of the asperities 12 has the effect of increasing the surface roughness of the sacrificial layer 11, going for example from an initial value of the order of 1 nm to a final value greater than or equal to 10 nm, and preferably between 10 nm and 30 nm (limits included).
[0029] Step S12 of exposing the sacrificial layer 11 is preferably carried out in a reactive ion etching reactor, for example inductively coupled (ICP, "Inductive Coupled Plasma"). The reactor comprises in particular a chamber in which the etching plasma is generated, a radiofrequency (RF) antenna called a "source generator" and a substrate holder called a "bias generator", on which the substrate (covered with the metal layer 10 and the sacrificial layer 11) is arranged. The substrate holder makes it possible to apply an RF bias to the substrate.
[0030] The etching plasma is formed from a mixture of reactive gases introduced into the reactor chamber. The mixture of reactive gases preferably comprises a gas containing oxygen, a gas containing silicon and fluorine or silicon and chlorine and a fluorocarbon gas (C x F y ), which may be hydrogenated (C x H y F z ). A so-called neutral diluting gas, such as argon or helium, may also be introduced into the reactor chamber to make the plasma less reactive, increasing the physical aspect of the etching (bombardment).
[0031] The ratio of the flow rate of oxygen-containing gas to the flow rate of silicon-containing and fluorine- or chlorine-containing gas is preferably between 20 and 50. The ratio of the flow rate of hydrogenated fluorocarbon gas to the flow rate of oxygen-containing gas is preferably between 0.9 and 1.1.
[0032] For example, the reactive gas containing oxygen is dioxygen (O 2 ), the reactive gas containing silicon and fluorine or chlorine is silicon tetrachloride (SiCl 4 ) or silicon tetrafluoride (SiF 4 ) and the hydrogenated fluorocarbon reactive gas is fluoromethane (CH 3 F).
[0033] Generally speaking, the more nitrogen the dielectric material of the sacrificial layer 11 contains, the more oxygen the mixture of reactive gases can contain (for example by increasing the O 2 flow rate / SiCl 4 or SiF 4 flow rate ratio).
[0034] In a particular embodiment of the roughening process, the dielectric material is a silicon nitride (Si x N y ), such as stoichiometric silicon nitride Si 3 N 4 , and the etching plasma is generated under the following conditions: a flow rate of SiCl 4 or SiF 4 between 2 sccm and 5 sccm (abbreviation for “Standard Cubic Centimeter per Minute” in English, i.e. the number of cm 3< of gas flowing per minute under standard pressure and temperature conditions, i.e. at a temperature of 0°C and a pressure of 1013.25 hPa); an O 2 flow rate of between 40 sccm and 250 sccm; a CH 3 F flow rate of between 40 sccm and 250 sccm; a reactor source power of between 100 W and 1000 W; a substrate bias voltage of between -200 V and -500 V; a reactor chamber pressure of between 6.666 Pa (50 mTorr) and 19.998 Pa (150 mTorr); a substrate holder temperature of between 20 °C and 100 °C; and a reactor chamber wall temperature of between 50 °C and 80 °C.
[0035] For example, the flow rate of SiCl 4 or SiF 4 is 5 sccm, the flow rate of oxygen is 200 sccm, the flow rate of CH 3 F is 200 sccm, the source power is 400 W, the substrate bias voltage is -250 V, the pressure in the reactor chamber is 11.999 Pa (90 mTorr), the substrate temperature is 50 °C and helium is additionally introduced into the reactor (flow rate: 120 sccm).
[0036] The duration of exposure of the sacrificial layer 11 to the etching plasma is determined as a function of the surface roughness that is sought to be obtained at the end of step S12. For the parameter ranges described previously, it is typically between 30 s and 300 s.
[0037] The initial thickness (i.e. before etching) of the sacrificial layer 11 is advantageously greater than or equal to the desired surface roughness (in root mean square value).
[0038] At the end of the exposure step S12, the sacrificial layer 11 can still completely cover the metal layer 10, as illustrated by the Figure 1B . Alternatively, a portion of the metal layer 10 may have been uncovered.
[0039] At step S13 of the Figure 1C , the metal layer 10 is etched through the sacrificial layer 11 so as to transfer the asperities 12 of the sacrificial layer 11 into at least a portion of the metal layer 10. In other words, the sacrificial layer 11 is used as a hard mask for etching the metal layer 10.
[0040] When the sacrificial layer 11 completely covers the metal layer 10, the sacrificial layer 11 is first consumed until it opens onto a portion of the metal layer 10, then portions of the metal layer 10 are etched at the same time as the sacrificial layer 11. The etching of the metal layer 10 therefore does not start at the same time depending on the regions of the surface of the metal layer 10, which leads to the formation of surface asperities. Portions of the metal layer 10 may not be etched if the hard mask formed by the sacrificial layer 11 is sufficiently thick above these portions or if the etching time is limited. These portions are then covered by residues 11' of the sacrificial layer 11 at the end of the transfer step S13, as represented by Figure 1C .
[0041] The etching of the metal layer 10 can be accomplished by means of any technique known to those skilled in the art: reactive ion etching (RIE), ion beam etching (IBE), etc. The metal layer 10 can be etched in the transfer step S13 by means of an etching method that is not very selective with respect to the sacrificial layer 11, i.e. having a selectivity of between 1 and 2 (limits included). In this case, the asperities 12 of the sacrificial layer 11 are transferred into the metal layer 10 substantially identically. Ion beam etching is an example of a non-selective method (selectivity equal to 1) and reactive ion etching with a chlorine-based plasma or fluorine is an example of a not very selective method (selectivity less than or equal to 2).
[0042] Conversely, by using an etching process having a selectivity strictly greater than 2, the size of the asperities 12 is increased during the transfer from the sacrificial layer 11 to the metal layer 10.
[0043] Thus, the final roughness of the metal layer 10 can be modulated by varying the selectivity of the etching process of the metal layer.
[0044] An advantage of the roughening process of Figures 1A-1Cis to be able to use the same dielectric material to form the sacrificial layer 11, regardless of the material of the underlying metal layer 10, and therefore to have only one plasma etching recipe (instead of having as many recipes as there are metals). The roughening process is applicable to all metals, since all etching techniques known to those skilled in the art (for etching a metal layer) can be used to transfer the roughness of the sacrificial layer 11 to the metal layer 10.
[0045] For example, etching of Ti, Ta, TaN, AlCu and AISi metals is possible by RIE using chlorine or fluorine-based chemistry, while etching of noble metals such as Pt, Au and Ru is accomplished by IBE. Since ion beam etching is inherently non-selective with respect to the dielectric material, asperities are transferred essentially identically into a noble metal layer.
[0046] There Figure 1D represents an additional step S14 of the roughening process, which can be accomplished after step S13 of the Figure 1C . When the sacrificial layer 11 is not completely consumed at the end of the transfer step S13, the sacrificial layer 11 can be removed selectively with respect to the metal layer 10. This selective removal step S14 is advantageously accomplished by wet etching, for example using a hydrofluoric acid (HF) solution.
[0047] Two examples of application of the roughening process will now be described in relation to the Figures 2A-2C and the Figures 3A-3C .
[0048] The first application example concerns a method for manufacturing a resistive memory cell, for example of the OxRAM type. A resistive memory cell typically comprises a first electrode called the lower electrode, a second electrode called the upper electrode, and a resistive layer (also called the active layer) arranged between the lower and upper electrodes. The resistive layer is formed from a material with variable electrical resistance, an oxide in the case of an OxRAM cell.
[0049] THE Figures 2A to 2C schematically represent steps S21 to S23 of this resistive memory cell manufacturing method.
[0050] Stage S21 of the Figure 2A consists of depositing a first metal layer 21 on a substrate 20. For example, the first metal layer 21 is formed from titanium nitride (TiN) and its thickness is between 100 nm and 150 nm.
[0051] The substrate 20 may in particular comprise active components (e.g. transistors), connected to each other by one or more interconnection levels (or metal levels) to form a CMOS logic circuit (typically a reading circuit). Each interconnection level comprises metal vias and / or metal lines 201 coated in one or more dielectric layers 202.
[0052] The first metal layer 21 is deposited on an interconnection level (for example the first metal level M1) so as to be in contact with the metal lines 201 of this level. Thus, in this example, the memory cell is formed within the BEOL (“Back End Of Line” in English) functional block of a CMOS circuit.
[0053] The surface roughness of the first metal layer 21 is then increased by means of the roughening method described in relation to the Figures 1A-1C(and 1D, if applicable). The final surface roughness of the first metal layer 21 is advantageously greater than or equal to 2 nm, preferably between 3 nm and 15 nm, in order to significantly reduce the forming voltage of the memory cell.
[0054] At step S22 of the Figure 2B , a layer of variable electrical resistance material 22 is then deposited on the first metal layer 21, then a second metal layer 23 is deposited on the layer of variable electrical resistance material 22. The variable electrical resistance material may be an oxide, preferably a transition metal oxide such as hafnium oxide (HfO 2 ). The second metal layer 22 is for example formed of titanium nitride (TiN). The thickness of the layer of variable electrical resistance material 22 may be between 5 nm and 20 nm and the thickness of the second metal layer 22 between 100 nm and 150 nm.
[0055] Finally, at step S23 of the Figure 2C , the first metal layer 21, the variable electrical resistance material layer 22 and the second metal layer 23 are etched so as to delimit respectively the lower electrode 210, the resistive layer 220 and the upper electrode 230 of the resistive memory cell. The etching can be carried out by RIE through a hard or resin mask, formed by photolithography and removed after the etching. The etching of the lower electrode (e.g. TiN) by RIE can be selective with respect to the dielectric layer 202 (e.g. SiO 2 ) of the interconnection level, so that there is no transfer of roughness in this dielectric layer 202.
[0056] Several memory cells (each comprising a stack of lower electrode 210 - resistive layer 220 - upper electrode 230) can be formed simultaneously in the etching step S3, as illustrated by the Figure 2CThe lower electrode 210 of each memory cell is in contact with a metal line 201 of the interconnection level.
[0057] A second example of application of the roughening process concerns a process for forming a via with random electrical resistance.
[0058] In reference to the Figure 3C, a via 300 is a metal pad electrically connecting two metal lines 301 belonging to two consecutive interconnection levels (i.e. two metal levels) of an integrated circuit. These two interconnection levels are hereinafter called levels N and N-1. The metal line 301 of the level N-1 (as possibly that of the level N) can be covered with a barrier layer 303, preventing the diffusion of the line metal into the dielectric layer(s) 302a-302b of the higher interconnection levels, in particular those of the level N. This diffusion barrier 303 can be made of metal, for example a cobalt and tungsten alloy doped with phosphorus (CoWP) or boron (CoWB), and self-aligned on the metal line 301 (selective deposition, only localized on the metal line).
[0059] The via 300 extends from the metal line 301 of the level N to the metal barrier layer 303 covering the metal line 301 of the level N-1. Its electrical resistance depends in particular on the surface state of the metal barrier layer 303.
[0060] The roughening process is applied in this context to increase the roughness of the metal barrier layer 303, in order to give the via 300 a random electrical resistance. Vias with random electrical resistance make it possible to construct an integrated circuit with a physical unclonable function (or PUF). A physical unclonable function is a unique and unforgeable digital signature or fingerprint that is used to identify the integrated circuit. Such an integrated circuit finds numerous applications in cryptography.
[0061] THE Figures 3A to 3Cschematically represent steps S31 to S33 of the method of forming a via 300 having a random electrical resistance.
[0062] At step S31 of the Figure 3A , a first dielectric layer 302a is deposited on the metal barrier layer 303, then a second dielectric layer 302b is deposited on the first dielectric layer 302a.
[0063] The first dielectric layer 302a is intended to serve as a sacrificial layer (or hard mask layer) during the roughening process of the metal barrier layer 303. It is therefore made of a dielectric material comprising nitrogen, for example Si 3 N 4 or SiCN.
[0064] The second dielectric layer 302b is preferably formed from a dielectric material having a low dielectric constant (also called dielectric material low-k ) . For example, the second dielectric layer 302b is made of SiOC.
[0065] Then, the second dielectric layer 302b is etched so as to form a cavity 304, the first dielectric layer 302a advantageously serving as a stop layer for the etching of the second dielectric layer 302b. The cavity 304 opens onto the first dielectric layer 302a (in other words, the bottom of the cavity 304 is formed by the first dielectric layer 302a). The cavity 304 can be shaped so as to simultaneously produce the via and the metal line of the N level, in accordance with a conventional “Double Damascene” integration method.
[0066] Stage S32 of the Figure 3B comprises steps S12, S13 and optionally S14 of the roughening process. These are accomplished in the manner described in relation to the Figures 1B, 1C and 1D .
[0067] A surface of the first dielectric layer 302a, located at the bottom of the cavity 304, is exposed to an etching plasma (for example CH 3 F / SiCl 4 / O 2 ) so as to create asperities (step S12).
[0068] Then, the metal barrier layer 303 is etched through the first dielectric layer 302a, so as to transfer the asperities of the first dielectric layer 202a into the metal barrier layer 303 (step S13). The etching of the metal barrier layer 303 may partially open onto the metal line 301 of the N-1 level. An etching method having a selectivity (with respect to the first dielectric layer 302a) of between 1 and 2 may be preferred to have better control, and in particular to avoid etching the metal line 301 too deeply.
[0069] Any residues of the first dielectric layer 302a are then selectively etched relative to the underlying metal layers (step S14).
[0070] Finally, at step S33 of the Figure 3C , the cavity 304 is filled with one or more metals in order to form the via 300 and, preferably simultaneously, the metal layer 301 of the N level. Step S33 may successively comprise the deposition of a metal diffusion barrier (for example in Ta / TaN) on the walls of the cavity 304, the deposition of a seed layer (typically in copper) on the metal diffusion barrier and the filling of the rest of the cavity with a metal (typically copper) by electrochemical deposition.
[0071] The random roughness of the metal barrier layer 303 at the level of the via 300, as well as its more or less pronounced opening on the metal line 301 of the level N-1, gives the via 300 a random electrical resistance which can be measured by a reading circuit.
[0072] The roughening process of Figures 1A-1Dis here integrated into a process for the simultaneous formation of a via and a metal line (double damascene process). However, it can just as easily be integrated into a process for the formation of a via alone (single damascene process).
Claims
1. Method for increasing the surface roughness of a metal layer (10), comprising the following steps: - depositing (S11) on the metal layer (10) a sacrificial layer (11) made of a dielectric material comprising nitrogen; - exposing (S12) a surface of the sacrificial layer (11) to an etching plasma so as to create asperities (12), the etching plasma being formed from a mixture of reactive gases comprising a gas containing oxygen, a gas containing silicon and fluorine or silicon and chlorine and a fluorocarbon gas (CxFy); - etching (S13) the metal layer (10) through the sacrificial layer (11), so as to transfer the asperities (12) of the sacrificial layer into a part at least of the metal layer.
2. Method according to claim 1, wherein the asperities (12) are projecting patterns having a random shape and distributed in a non-uniform manner on the surface of the sacrificial layer (11).
3. Method according to one of claims 1 and 2, wherein the dielectric material comprising nitrogen is selected from among silicon nitrides (SixNy), silicon carbonitride (SiCN) and silicon boron carbonitride (SiBCN).
4. Method according to any of claims 1 to 3, wherein the gas containing oxygen is O2, the gas containing silicon and fluorine or silicon and chlorine is SiCl4 or SiF4 and the hydrogenated fluorocarbon gas is CH3F.
5. Method according to any of claims 1 to 4, wherein the dielectric material is a silicon nitride (SixNy) and wherein the etching plasma is generated in a chamber of a reactive ion etching reactor in the following conditions: - a flow rate of SiCl4 or SiF4 entering into the chamber of the reactor comprised between 2 sccm and 5 sccm; - a flow rate of O2 entering into the chamber of the reactor comprised between 40 sccm and 250 sccm; - a flow rate of CH3F entering into the chamber of the reactor comprised between 40 sccm and 250 sccm; - a power emitted by a source of the reactor comprised between 100 W and 1000 W; - a bias voltage comprised between -200 V and -500 V; - a pressure in the chamber of the reactor comprised between 6.666 Pa and 19.998 Pa; and - a temperature of substrate holder comprised between 20 °C and 100 °C; - a temperature of the walls of the chamber of the reactor comprised between 50 °C and 80 °C.
6. Method according to any of claims 1 to 5, further comprising, after step (S13) of etching of the metal layer (10), a step (S14) of selective removal of the sacrificial layer (11).
7. Method according to any of claims 1 to 5, wherein the sacrificial layer (11) is entirely consumed during the step of etching of the metal layer (10).
8. Method according to any of claims 1 to 7, wherein the sacrificial layer (11) has, after the step (S2) of exposure to the etching plasma, a surface roughness, expressed in root mean square value, greater than or equal to 10 nm, and preferably comprised between 10 nm and 30 nm.
9. Method according to any of claims 1 to 8, wherein the metal layer (10) initially has a surface roughness, expressed in root mean square value, strictly less than 1 nm.
10. Method according to any of claims 1 to 9, wherein the metal layer (10) is etched by means of an etching method having a selectivity with respect to the sacrificial layer (11) comprised between 1 and 2.
11. Method according to any of claims 1 to 9, wherein the metal layer (10) is etched by means of an etching method having a selectivity with respect to the sacrificial layer (11) strictly greater than 2.
12. Method for manufacturing a resistive random access memory cell comprising a first electrode (210), a second electrode (230) and a resistive layer (220) arranged between the first and second electrodes, the method comprising the following steps: - depositing (S21) a first metal layer (21) on a substrate; - increasing the roughness of the first metal layer (21) by means of a method according to any of claims 1 to 11; - depositing (S22) a layer of material with variable electrical resistance (22) on the first metal layer (21) and a second metal layer (23) on the layer of material with variable electrical resistance; - etching (S23) the first metal layer (21), the layer of material with variable electrical resistance (22) and the second metal layer (23), so as to delimit respectively the first electrode (210), the resistive layer (220) and the second electrode of the resistive random access memory cell (230).
13. Method for forming a via (300) extending up to a metal barrier layer (303), the method comprising the following steps: - depositing (S31) a first dielectric layer (302a) on the metal barrier layer (303), the first dielectric layer being comprised of a material comprising nitrogen; - depositing (S31) a second dielectric layer (302b) on the first dielectric layer (302a); - forming (S31) in the second dielectric layer (302b) a cavity (304) leading into the first dielectric layer (302a); - exposing (S32) at the bottom of the cavity (304) a surface of the first dielectric layer (302a) to an etching plasma so as to create asperities (12), the etching plasma being formed from a mixture of reactive gases comprising a gas containing oxygen, a gas containing silicon and fluorine or silicon and chlorine and a fluorocarbon gas (CxFy); - etching (S32) the metal barrier layer (303) through the first dielectric layer (302a), so as to transfer the asperities (12) of the first dielectric layer into a part at least of the metal barrier layer; and - filling (S33) the cavity with at least one metal.