Composite material for manufacturing interior trim parts for motor vehicles, associated manufacturing method and trim parts comprising this composite material

A composite material with large lignin-containing natural fibers and UV stabilizers enhances the stability and impact resistance of vehicle interior parts, addressing discoloration and shock resistance issues.

FR3109154B1Active Publication Date: 2024-11-08VITIS VALOREM +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FR2020003706
Authority / Receiving Office
FR · FR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-04-14
Publication Date
2024-11-08
Estimated Expiration
2040-04-14

AI Technical Summary

Technical Problem

Biocomposite materials containing plant fibers for vehicle interiors face issues with discoloration due to lignin degradation from ultraviolet radiation and insufficient impact resistance, failing to meet multiaxial shock simulation requirements.

Method used

A composite material is formulated with thermoplastic polypropylene, elastomers, and natural fibers with lignin particles larger than 500 μm, combined with UV stabilizers and absorbers, to enhance stability and resistance.

Benefits of technology

The composite material exhibits improved resistance to ultraviolet radiation and impact, maintaining color stability and meeting shock simulation standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000020_0000
    Figure 00000020_0000
Patent Text Reader

Abstract

The invention relates to a composite material comprising, in particular, natural fiber containing lignin in the form of particles and notable in that at least 15% by mass of the particles relative to the total mass of said particles have a particle size between 500 µm and 2000 µm. The invention also relates to a method for manufacturing said composite material, its use for the production of an interior trim piece for a motor vehicle, and such a piece. Figure to be published with the abstract: Fig. 1
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: Composite material for producing interior trim parts for a motor vehicle, associated manufacturing method and trim parts comprising this composite material

[0001] The invention relates to a composite material for producing interior trim parts for a motor vehicle, as well as a method for manufacturing this composite material. Interior trim parts for a motor vehicle comprising the composite material according to the invention are also described.

[0002] Among the materials available for the design of a motor vehicle, there are thermoplastic or thermosetting materials (polypropylene, polyethylene, polycarbonate, polyamide, etc.). These materials can be reinforced by the use of inorganic fillers, or inorganic or organic fibers such as plant fibers.

[0003] The incorporation of plant fibers into thermoplastic materials offers numerous advantages, such as the possibility of imparting desirable mechanical properties to the resulting biocomposite materials. Such biocomposite materials generally have a lower mass than those containing inorganic fillers or fibers, thereby reducing the overall mass of the vehicle and consequently its CO2 emissions. Furthermore, the incorporation of plant fibers utilizes renewable resources and gives a second life to plant waste.

[0004] For example, document FR 3 017 132 relates to a composite material comprising a plastic matrix into which vine shoot powder is incorporated, thus avoiding the systematic burning of these shoots and enabling the manufacture of certain products such as vine trellising stakes. The process for obtaining this composite material is also described, and includes a step of grinding the shoots to obtain granules, a step of drying the granules, and a step of incorporating the resulting powder into a plastic matrix, for example, a polymer selected from polypropylene or polylactic acid and mixtures thereof.

[0005] The policy for using green waste from agriculture, particularly from vineyards, avoids its waste through open burning and thus meets current environmental requirements. Giving this green waste a second life also contributes to efforts addressing the CO2 emission problem. Furthermore, vine shoots are a particularly abundant and inexhaustible plant-based raw material for countries including vineyards.

[0006] The incorporation of natural fibers into thermoplastic materials also makes it possible to create biodegradable recyclable materials that are not abrasive to tools.

[0007] For example, document EP 0 855 974 describes a trim panel for a motor vehicle comprising a part made of natural fibers, which makes it possible to avoid the use of fiberglass and to reduce skin irritation for vehicle users.

[0008] Document WO 2012 / 093167 describes a composite material comprising, in particular, a propylene-ethylene copolymer matrix in which an elastomer and natural fibers are incorporated. It is described that, for the manufacture of interior automotive parts, the average length of the natural fibers is between 100 µm and 10,000 µm.

[0009] Plant fibers contain lignin, a biopolymer containing chromophoric structures, such as aromatic motifs. Under the action of light, and more specifically ultraviolet radiation, these chromophoric structures degrade, resulting in a progressive discoloration of the fiber. Biocomposite materials containing this lignin will therefore lose their natural color over time, which is unsuitable for use as interior trim in vehicles.

[0010] Furthermore, biocomposite materials based on plant fibers are promising, but still have limitations, particularly in terms of impact resistance. Thus, the requirements of puncture resistance tests (multiaxial impact simulation) are generally not met, meaning that in practice, these biocomposite materials do not withstand minor impacts caused by user interaction.

[0011] The present invention aims to utilize the advantages offered by plant fibers in the manufacture of the appearance parts of a motor vehicle while making these appearance parts more stable with respect to light - in particular ultraviolet radiation - and sufficiently resistant to the various shocks inherent in their location within the vehicle and their interaction with the vehicle users in order to satisfy the simulation of multiaxial shock.

[0012] To this end, and according to a first aspect, the invention relates to a composite material containing natural fibers comprising: from 20 to 98% by mass relative to the total mass of the composite material of a thermoplastic polypropylene matrix; from 1 to 30% by mass relative to the total mass of the composite material of at least one elastomer; from 1 to 60% by mass relative to the total mass of the composite material of natural fibers comprising lignin, from 0 to 30% by mass relative to the total mass of the composite material of an inorganic filler; the material being notable in that said natural fibers comprising lignin are in the form of particles and at least 15% by mass of the particles relative to the total mass of said particles have a particle size greater than 500 pm, and preferably between 500 and 2000 pm.

[0013] As will be understood from the definition just given, the invention proposes a composite material based on plant fibers that have been modified to eliminate the finest particles. Indeed, without being bound by any theory, the inventors have shown that when a minimum number of plant fiber particles have a particle size exceeding a certain threshold (corresponding to a minimum fiber length), the lignin they contain remains trapped within the particles and does not mix, or mixes less, with the thermoplastic material forming the matrix of the composite material. The fact that the lignin remains within the particles provides it with protection against light, and more particularly against ultraviolet radiation. Thus, the composite material discolors less quickly than composite materials comprising natural fiber particles with lignin exhibiting a smaller particle size.The addition of an elastomer also gives the composite material better impact resistance properties.

[0014] According to a preferred embodiment of the invention, said natural fibers are selected from the group comprising vine shoots, hemp, sisal, miscanthus, cellulose, wood, cork, jute, bamboo, and mixtures thereof. Preferably, said natural fibers are selected from the group comprising wood and / or vine shoots. More preferably, said natural fibers are or comprise vine shoots.

[0015] According to a preferred embodiment, at least 15% by mass of the particles relative to the total mass of said particles, have a particle size greater than 520 pm, preferably greater than 530 pm; preferably greater than 540 pm, preferably greater than 550 pm.

[0016] According to a preferred embodiment, at least 15% by mass of the particles relative to the total mass of said particles, have a particle size of less than 1500 pm, preferably less than 1400 pm; preferably less than 1300 pm, preferably less than 1200 pm; preferably less than 1100 pm.

[0017] Preferably, at least 17% by mass of the particles relative to the total mass of said particles have a particle size greater than 500 pm; preferably greater than 520 pm, preferably greater than 530 pm; preferably greater than 540 pm, preferably greater than 550 pm, preferably at least 20% by mass. mass; more preferably at least 25% by mass; more preferably at least 30% by mass.

[0018] According to a preferred embodiment of the invention, said composite material comprises between 0.1 and 1.0% by mass relative to the total mass of the composite material of at least one hindered amine-type light stabilizer; preferably between 0.2 and 0.9% by mass.

[0019] According to an alternative or complementary embodiment of the invention, said composite material comprises between 0.1 and 10% by mass relative to the total mass of the composite material of at least one ultraviolet absorbing agent; preferably between 1.0 and 5.0% by mass.

[0020] Preferably, at least one ultraviolet absorbing agent is an inorganic agent selected from titanium dioxide (TiO2), zinc oxide (ZnO), cerium dioxide (CeO2) and mixtures thereof; and / or at least one ultraviolet absorbing agent is an organic agent selected from substituted hydroxybenzophenones and benzotriazoles.

[0021] Advantageously, the composite material further comprises between 1% and 10% by mass relative to the total mass of the composite material of at least one coupling agent; preferably, said coupling agent is a maleated polypropylene (MAPP) showing a maleic anhydride content of at least 1.0% by mass relative to the total mass of the maleated polypropylene; preferably between 1.0 and 5.0% by mass relative to the total mass of the maleated polypropylene.

[0022] Complementarily or alternatively, the composite material further comprises between 0.1% and 10% by mass relative to the total mass of the composite material of at least one colored pigment, preferably of at least one inorganic colored pigment.

[0023] According to a preferred embodiment of the invention, the matrix is ​​based on polypropylene and consists of a propylene homopolymer and / or a propylene-alpha-olefin copolymer consisting of at least 70% by mass of propylene relative to the total mass of the matrix, and up to 30% by mass of at least one alpha-olefin relative to the total mass of the matrix, the alpha-olefin of the propylene-alpha-olefin copolymer being chosen from the group of alpha-olefins comprising 2 or 4 to 20 carbon atoms and their mixtures.

[0024] Complementarily or alternatively, the matrix is ​​based on polypropylene and has a melt flow index between 1 and 200 g / 10 min as measured in accordance with ISO 1133 conditions M, at 230°C and under a load of 2.16 kg.

[0025] According to a preferred embodiment, at least one elastomer is an ethylene-alpha-olefin copolymer comprising from 20 to 80% by mass of ethylene relative to the total mass of the ethylene-alpha-olefin copolymer, preferably from 30 to 65% by mass of ethylene. mass; and 80 to 20% by mass of at least one alpha-olefin relative to the total mass of the ethylene-alpha-olefin copolymer, preferably 70 to 35% by mass; the alpha-olefin of the ethylene-alpha-olefin copolymer being selected from the group of alpha-olefins comprising 3 to 20 carbon atoms and mixtures thereof. In such an embodiment, the elastomer may be in the form of a phase dispersed within the matrix and form a heterophasic polypropylene with said matrix.

[0026] Complementarily or alternatively, at least one elastomer is chosen from the group comprising ethylene-propylene-diene monomer (EPDM), styrene isoprene styrene sequenced copolymers (SIS), hydrogenated styrene isoprene styrene sequenced copolymers (SEPS), styrene butadiene styrene sequenced copolymers (SBS), hydrogenated styrene butyrene sequenced copolymers (SEBS), styrene butyrene styrene sequenced copolymers (SBSS) and mixtures thereof.

[0027] According to a second aspect, the invention relates to the use of a composite material containing natural fibers according to the first aspect for the production of an interior trim piece for a motor vehicle. Preferably, the use takes place in the context of the production of interior trim for a motor vehicle by injection molding.

[0028] According to a third aspect, the invention relates to an interior trim piece for a motor vehicle, said piece being produced from a composite material containing natural fibers according to the first aspect. Preferably, the interior trim piece is produced by extrusion, blow molding, injection molding, rotomolding, or injection blow molding; more preferably, the interior trim piece is produced by injection molding.

[0029] According to a fourth aspect, the invention relates to a process for producing a composite material containing natural fibers according to the first aspect, said composite material comprising from 20 to 98% by mass relative to the total mass of the composite material of a propylene-based thermoplastic matrix; from 1 to 30% by mass relative to the total mass of the composite material of at least one elastomer; from 1 to 60% by mass relative to the total mass of the composite material of natural fibers comprising lignin; from 0 to 30% by mass relative to the total mass of the composite material of an inorganic filler; said process being notable in that it comprises the following steps: a) grinding natural fibers comprising lignin to obtain particles; preferably to obtain particles with a particle size of less than 2000 µm;b) sieving said natural fibre particles containing lignin with a sieve so as to obtain a residue comprising at least 15% by mass of the particles relative to the total mass of said particles having a particle size greater than 500 µm, and preferably between 500 and 2000 µm; c) collection of the residue; and d) mixing of said residue; residue obtained in step (c) with the other components to form said composite material.

[0030] According to a fifth aspect, the invention relates to a motor vehicle remarkable in that it has at least one piece of interior trim according to the third aspect.

[0031] It is understood that all the features described in terms of the first aspect of the invention can be found, alone or in combination, within the second, third, fourth and / or fifth aspect of the invention.

[0032] The invention will be well understood and other aspects and advantages will become clear upon reading the following description, given by way of example with reference to the attached drawing on which:

[0033] [fig. 1] Figure 1 presents a flowchart of the process according to the fourth aspect of the invention.

[0034] In the following description, the term "include" is synonymous with "include" and is not limiting in that it permits the presence of other components in the composite material or other steps in the process to which it refers. It is understood that the term "include" includes the terms "consist of".

[0035] The invention relates to a composite material containing natural fibers comprising: from 20 to 98% by mass relative to the total mass of the composite material of a thermoplastic polypropylene matrix; from 1 to 30% by mass relative to the total mass of the composite material of at least one elastomer; from 1 to 60% by mass relative to the total mass of the composite material of natural fibers comprising lignin, from 0 to 30% by mass relative to the total mass of the composite material of an inorganic filler; the material is notable in that said natural fibers comprising lignin are in the form of particles and at least 15% of said particles have a particle size greater than 500 pm, and preferably between 500 and 2000 pm.

[0036] The thermoplastic matrix

[0037] The thermoplastic matrix is ​​made of polypropylene.

[0038] The term "matrix" refers to a continuous phase in which the other components are dispersed. Generally, but not always, the matrix is ​​formed by the component present in the majority proportion.

[0039] In a preferred embodiment, the polypropylene is isotactic. For example, it is characterized by high isotacticity, for which the pentad content (mmmm) is a measure. Preferably, the pentad content (mmmm) is at least 90%, more preferably at least 95%, and most particularly at least 97%. Isotacticity can be determined by 13C NMR analysis. Isotacticity is determined by 13C NMR analysis on the total polymer. In the spectral region of the methyl groups, the Signals corresponding to the pentads mmmm, mmmr, mmrr, and mrrm are assigned using published data, e.g., A. Razavi, Macromol. Symp., Vol. 89, pp. 345–367. Only the pentads mmmm, mmmr, mmrr, and mrrm are considered due to the low intensity of the signals corresponding to the remaining pentads. For the signal related to the pentad mmrr, a correction is made for its overlap with a methyl signal linked to 2,1-insertions. The percentage of mmmm pentads is then calculated using the following formula: % mmmm = 100 x AREA mmmm / (AREA mmmm + AREA mmmr + AREA mmrr + AREA mrrm).

[0040] In a preferred embodiment of the invention, the thermoplastic matrix is ​​polypropylene-based and consists of a propylene homopolymer and / or a propylene-alpha-olefin copolymer. The propylene copolymer may be a random copolymer, a heterophasic copolymer, or a mixture thereof.

[0041] The propylene copolymer used in the context of the invention is preferably made up of at least 70% by mass of propylene relative to the total mass of the matrix, and up to 30% by mass of at least one alpha-olefin (or comonomer) relative to the total mass of the matrix, the alpha-olefin of the propylene-alpha-olefin copolymer being chosen from the group of alpha-olefins comprising 2 or 4 to 20 carbon atoms and their mixtures.

[0042] The term "copolymer" refers to a polymer resulting from the copolymerization of at least two chemically different types of monomers. The copolymer is therefore formed by at least two repeating units. The copolymer of the composite material of the present invention is a propylene-based copolymer, that is to say, a copolymer in which at least one of the two repeating units is propylene, the second repeating unit being generally called a comonomer.

[0043] The term "propylene" refers to an olefin comprising three carbon atoms. The term "olefin" refers to a molecule comprising at least one hydrogen atom unsaturation between two carbon atoms. An alpha-olefin is an olefin comprising an unsaturation in the primary position. Preferably, the second repeating unit is selected from an olefin comprising a number of carbon atoms other than 3.

[0044] For example, the comonomer is selected from ethylene and alpha-olefins having from 4 to 20 carbon atoms. Examples of alpha-olefins having from 4 to 20 carbon atoms include 1-butene, 1-pentene, 4-methylpentene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-eicosene. Preferably, the comonomer is selected from ethylene, 1-butene, and 1-hexene; more preferably, the comonomer is ethylene.

[0045] Advantageously, the propylene copolymer according to the invention is a co statistical polymer. The propylene copolymer used in the context of the invention is preferably made up of at least 85% by mass of propylene relative to the total mass of the copolymer, and up to 15% by mass of at least one alpha-olefin (or comonomer) relative to the total mass of the copolymer, the alpha-olefin of the propylene-alpha-olefin copolymer being chosen from the group of alpha-olefins comprising 2 or 4 to 20 carbon atoms and their mixtures.

[0046] The statistical propylene copolymer comprises at least 0.1% by mass relative to the total mass of the polymer of one or more comonomers, preferably at least 1% by mass. The statistical propylene copolymer comprises up to 10% by mass relative to the total mass of the polymer of one or more comonomers, and most preferably up to 6% by mass. Preferably, the statistical copolymer is a propylene-ethylene copolymer.

[0047] The heterophasic propylene copolymer comprises a dispersed phase, generally consisting of an ethylene and propylene elastomeric copolymer, for example ethylene-propylene rubber or EPR (English abbreviation for "ethylene propylene rubber"), distributed within a semi-crystalline polypropylene matrix, said semi-crystalline polypropylene matrix being a homopolymer of propylene or a statistical copolymer of propylene.

[0048] In the case of a heterophasic propylene copolymer, the heterophasic polypropylene preferably comprises at least 60% by mass of polypropylene homopolymer and / or polypropylene statistical copolymer relative to the total mass of the matrix, and up to 40% by mass of a dispersed phase comprising an elastomeric copolymer. Preferably, the elastomeric phase comprises propylene in an amount of at least 25% by weight of the elastomeric copolymer, and at least ethylene and / or another C4 to C10 alpha-olefin in an amount of up to 75% by weight of the elastomeric copolymer. Heterophasic polypropylene preferentially comprises at least 70% by mass of homopolymer polypropylene and / or statistical copolymer polypropylene relative to the total mass of the matrix, and up to 30% by mass of a dispersed phase comprising an elastomeric copolymer and / or at least 5% by mass of a dispersed phase comprising an elastomeric copolymer.

[0049] In one embodiment of the invention, polypropylene is a homopolymer of propylene. A homopolymer according to the present invention comprising less than 0.1% by mass relative to the total mass of the polymer of alpha-olefins other than propylene, preferably less than 0.05% by mass and more preferably less than 0.005% by mass. Preferably, no other alpha-olefins are detectable.

[0050] According to a preferred embodiment of the invention; the matrix is ​​polypropylene-based and has a melt flow index between 1 and 200 g / 10 min as measured in accordance with ISO 1133 conditions M, at 230 °C and under a load of 2.16 kg; preferably between 1 and 100 g / 10 min, preferably still between 5 and 50 g / 10 min; or between 10 and 40 g / 10 min.

[0051] The thermoplastics used in the present invention are commercially available.

[0052] Advantageously, the thermoplastic polypropylene matrix is ​​present in an amount between 50% by mass and 90% by mass relative to the total mass of the composite material, or between 55% and 85% by mass, or between 60% and 80% by mass, or between 65% and 75% by mass.

[0053] The elastomer

[0054] The term "elastomer" or "impact modifier" refers to a component added to a material to improve its impact resistance properties. Elastomers are polymers or molecules that form multiphase systems with the matrix or react chemically with the matrix to enhance its resilience. This makes the composite material more ductile, which is advantageous when molded into aesthetically pleasing parts for the interior of motor vehicles, as these parts can then fit perfectly into the confined spaces of the vehicle's passenger compartment and withstand potential impacts from vehicle occupants.

[0055] According to a preferred embodiment, at least one elastomer is an ethylene-alpha-olefin copolymer comprising from 20 to 80% by mass of ethylene relative to the total mass of the ethylene-alpha-olefin copolymer, and from 80 to 20% by mass of at least one alpha-olefin relative to the total mass of the ethylene-alpha-olefin copolymer; the alpha-olefin of the ethylene-alpha-olefin copolymer being selected from the group of alpha-olefins comprising 3 to 20 carbon atoms and mixtures thereof. In such an embodiment, the elastomer may be in the form of a phase dispersed in the matrix and form with said matrix a heterophasic polypropylene.Preferably at least one elastomer is an ethylene-alpha-olefin copolymer comprising 30 to 65% by mass of ethylene relative to the total mass of the ethylene-alpha-olefin copolymer, and 70 to 35% by mass of at least one alpha-olefin relative to the total mass of the ethylene-alpha-olefin copolymer.

[0056] Complementarily or alternatively, at least one elastomer is chosen from the group comprising ethylene-propylene-diene monomer (EPDM), styrene isoprene styrene sequenced copolymers (SIS), hydrogenated styrene isoprene styrene sequenced copolymers (SEPS), styrene butadiene styrene sequenced copolymers (SBS), hydrogenated styrene butyrene sequenced copolymers (SEBS), styrene butyrene styrene sequenced copolymers (SBSS) and mixtures thereof.

[0057] According to a preferred embodiment, the composite material comprises ethylene-propylene-diene monomer (EPDM).

[0058] Advantageously, said elastomer is present in an amount between 2% and 30% by mass relative to the total mass of the composite material, or between 2% and 28%, or between 5% and 25% by mass, or between 7% and 23% by mass, or between 9% and 20% by mass.

[0059] The elastomers used in the context of the invention are commercially available.

[0060] Natural fibers comprising lignin

[0061] The incorporation of natural fibers serves to modulate the properties of composite materials. The plant fibers have a lignin content of between 1% and 40% by mass of lignin relative to the total mass of the natural fiber, preferably between 3% and 35% by mass, or between 5% and 20% by mass or between 10% and 15% by mass.

[0062] In a preferred embodiment of the invention, said natural fibers are selected from the group comprising vine shoots, hemp, sisal, miscanthus, cellulose, wood, cork, jute, bamboo, and mixtures thereof. Preferably, said natural fibers are selected from the group comprising wood and / or vine shoots. More preferably, said natural fibers are or comprise vine shoots.

[0063] The choice of vine shoots as a plant fiber is preferred in countries with developed viticulture because this product is available in large quantities each year. For example, approximately 3 tonnes of vine shoots can be produced per hectare of vineyard.

[0064] According to the invention, in order to reduce lignin leaching within the thermoplastic matrix and thus prevent its degradation under the action of ultraviolet radiation, a given proportion of the natural fibers incorporated into the composite material according to the present invention must have a minimum length, expressed in the context of the invention as a minimum particle size of the particles obtained by grinding the starting material. In the context of the invention, particle size refers to the diameter of the particles.

[0065] Thus, according to the invention, at least 15% by mass of the particles relative to the total mass of said particles has a particle size of at least 500 pm; preferably at least 510 pm, preferably at least 520 pm, more preferably at least 525 pm, even more preferably at least 530 pm or at least 540 pm, most preferably at least 550 pm or at least 560 pm. This measurement can be determined using a calibrated laboratory sieve.

[0066] Preferably at least 15% by mass of the particles relative to the mass The total particle size of said particles is less than 2000 µm; preferably less than 1500 µm, preferably less than 1400 µm; preferably less than 1300 µm, preferably less than 1200 µm; preferably even less than 1100 µm. This measurement can be determined using a calibrated laboratory sieve.

[0067] Advantageously, at least 15% by mass of the particles relative to the total mass of said natural fiber particles comprising lignin have a particle size between 500 µm and 2000 µm, or at least 16% by mass, or at least 17% by mass, or at least 18% by mass, or at least 20% by mass, or at less than 25% by mass, or at least 30% by mass, or at least 35% by mass, or at less than 40% by mass, or at least 45% by mass, or at least 50% by mass, or at less than 55% by mass, or at least 60% by mass.

[0068] Without being bound by any theory, it would appear that natural fiber particles release their lignin more readily when they have a particle size of less than 500 µm. In order to ensure good photostability of the composite material, it is advantageous that at least 15% by mass of the natural fiber particles have a particle size between 500 µm and 2000 µm, and more preferably at least 30% by mass.

[0069] Thus, in a preferred embodiment, at least 60% by mass of said particles have a particle size between 530 pm and 2000 pm.

[0070] The hindered amine-type light stabilizer and / or the absorbing agent ultraviolet

[0071] In order to improve resistance to ultraviolet radiation, said composite material comprises between 0.1 and 5.0% by mass relative to the total mass of the composite material of at least one hindered amine-type light stabilizer; preferably between 0.2 and 2.0% by mass, more preferably between 0.3 and 1.0% by mass or between 0.4 and 0.8% by mass. For example, said composite material comprises between 0.1 and 1.0% by mass relative to the total mass of the composite material of at least one hindered amine-type light stabilizer. More preferably, said composite material comprises between 0.2 and 0.9% by mass relative to the total mass of the composite material of at least one hindered amine-type light stabilizer, even more preferably between 0.3 and 0.8% by mass.Hindered amine light stabilizers are known to those skilled in the art by the acronym "HALS", which stands for "Hindered Amine Light Stabilizers", and are commercially available.

[0072] An example of a hindered amine type light stabilizer that can be used in the context of the invention is bis(l,2,2,6,6-pentamethyl-4-piperidyl sebacate) also known as PEDA.

[0073] According to an alternative or complementary embodiment, said composite material comprises between 0.1% and 10% by mass relative to the total mass of the composite material of at least one ultraviolet absorber; preferably, between 0.5% and 5.0% by mass or between 1.0% and 4.5% by mass.

[0074] Preferably, at least one ultraviolet absorbing agent is an inorganic agent selected from titanium dioxide (TiO2), zinc oxide (ZnO), cerium dioxide (CeO2) and mixtures thereof; and / or at least one ultraviolet absorbing agent is an organic agent selected from substituted hydroxybenzophenones and benzotriazoles.

[0075] The synergy between the elimination of fine fiber particles and the presence of a hindered amine type light stabilizer and / or ultraviolet absorber makes it possible to considerably slow down the discoloration of the composite material over time, which makes it practical to use this material for the manufacture of appearance parts for the interior of a motor vehicle.

[0076] Other components

[0077] Various components can be added to the composite material according to the invention in order to improve its properties. Thus, since it is intended to be used as an aesthetic component for the interior of a motor vehicle, the composite material may comprise between 0.1% and 20% by mass of the total mass of the composite material of at least one pigment, preferably at least one inorganic pigment, for example, iron oxide. The composite material may advantageously comprise between 0.5% and 19% by mass of the total mass of the composite material of at least one pigment, or between 1% and 18% by mass, or between 5% and 15% by mass, or between 7% and 13% by mass, or between 0.1% and 10% by mass. This makes it possible to provide a color that matches the interior of the vehicle.

[0078] In order to ensure good affinity between the plant fibers and the polypropylene-based copolymer matrix with a view to obtaining a homogeneous mixture, the composite material may advantageously comprise between 1% and 10% by mass relative to the total mass of the composite material of at least one coupling agent; preferably, said coupling agent is a maleated polypropylene (MAPP) showing a maleic anhydride content of at least 1.0% by mass relative to the total mass of the maleated polypropylene; preferably between 1.0 and 5.0% by mass relative to the total mass of the maleated polypropylene.

[0079] The coupling agent is also called a compatibilizing agent. The coupling agent can preferably be selected from polyolefins grafted with polar groups, such as maleate polypropylene. The composite material can thus comprise between 2% and 8% by mass relative to the total mass of the composite material of at least one coupling agent, or between 3% and 7% by mass, or between 4% and 6% by mass.

[0080] In order to control the tendency of the composite material to resist bending, an inorganic filler may be added to the composite material. The inorganic filler is preferably selected from compounds such as talc, hydrotalcite, calcium carbonate, calcium hydroxide, barium sulfate, mica, calcium silicate, clay, kaolin, silica, alumina, wollastonite, magnesium carbonate, magnesium hydroxide, zinc sulfate, and mixtures thereof. Most preferably, the inorganic filler is talc. When the inorganic filler is present, it is incorporated in an amount of between 1% and 30% by mass relative to the total mass of the composite material, more preferably between 5% and 25% by mass, or between 10% and 20% by mass.

[0081] The interior trim piece

[0082] The composite material according to the invention can be used to manufacture an interior trim piece for a motor vehicle. This piece is designed to be installed inside the passenger compartment, for example as a trim panel or the bottom of a storage compartment. Preferably, the interior trim piece is produced by extrusion, blow molding, injection molding, rotomolding, or injection blow molding; more preferably, the interior trim piece is produced by injection molding.

[0083] The process for producing the composite material (see figure 1)

[0084] The invention proposes a process for producing a composite material containing natural fibers as described above, said composite material comprising from 20 to 98% by mass relative to the total mass of the composite material of a propylene-based matrix; from 1 to 30% by mass relative to the total mass of the composite material of at least one elastomer; from 1 to 60% by mass relative to the total mass of the composite material of natural fibers comprising lignin; from 0 to 30% by mass relative to the total mass of the composite material of an inorganic filler; said process being notable in that it comprises the following steps: a) grinding 100% of natural fibers comprising lignin to obtain particles; preferably to obtain particles with a particle size of less than 2000 µm;b) sieving 200 of said natural fibre particles comprising lignin carried out with a sieve so as to obtain a residue comprising at least 15% by mass of the particles relative to the total mass of said particles having a particle size greater than 500 µm, and preferably between 500 and 2000 µm; c) collection 300 of the residue; and d) mixing 400 of said residue obtained in step (c) with the other components in order to form said composite material.

[0085] This process makes it possible to manufacture the composite material according to the invention, while at least partially removing the finest particles of natural fibers so as to increase the proportion of diameter or particle size greater than 500 pm, of so that more lignin remains within the natural fiber once it is incorporated into said composite material.

[0086] Advantageously, the mesh size of the sieve is selected so that the residue obtained after the sieving step comprises at least 15% of particles having a particle size between 500 pm and 2000 pm. Advantageously, the particles have a particle size of at least 510 pm and / or at most 2000 pm, more preferably at least 520 pm, even more preferably at least 525 pm, most preferably at least 530 pm, even more preferably at least 560 pm.

[0087] Optionally, the residue is dried before mixing 400 with the other components, in particular the polypropylene composition serving as a matrix for said composite material and at least one elastomer, preferably the residue is dried at a temperature below 100°C.

[0088] Advantageously, step 400 of mixing said residue with the other components, in particular a polypropylene composition serving as a matrix for said composite material and at least one elastomer, is carried out in an extruder.

[0089] Advantageously, the polypropylene matrix composition of said composite material and at least one elastomer further comprises: at least one hindered amine light stabilizer; and / or at least one ultraviolet absorber, for example an inorganic material such as zinc oxide and / or titanium dioxide; and / or at least one pigment, for example at least one inorganic pigment such as iron oxide; and / or at least one coupling agent, for example maleic acid and / or maleic acid anhydride; and / or at least one inorganic filler, for example talc.

[0090] The following examples are given for illustrative purposes.

[0091] Example 1 (comparative)

[0092] A composite material was prepared comprising a matrix made of a propylene copolymer, EPDM (ethylene-propylene-diene monomer) as the elastomer, and vine shoot powder as a natural fiber containing lignin. The average particle size of all the natural fibers in the composite material is equivalent to 160 µm. After 200 hours of ultraviolet radiation (with a wavelength ranging from 100 nm to 400 nm), the areas exposed to ultraviolet radiation became lighter, while the areas in shaded locations, and therefore exposed to less ultraviolet radiation, remained a dark red.

[0093] Example 2

[0094] A composite material has been prepared comprising a matrix made of a propylene copolymer, EPDM (ethylene-propylene-diene monomer) as The material consists of an elastomer and vine shoot powder as a natural fiber containing lignin. Unlike the material in Example 1, the vine shoot powder underwent a sieving step to remove at least some of the finest particles. A particle size analysis of the sieved powder was performed before the particles were added to the mixture using calibrated sieves. The powder added to form the composition exhibits the following particle size distribution: 1% by mass of fibers with a length greater than 1000 µm; 17% by mass of fibers with a length between 530 µm and 1000 µm; and 82% by mass of fibers are fine particles with a length less than 530 µm.

[0095] After 200 hours of ultraviolet radiation, no discoloration was observed, which is a surprising result compared to the comparative example, where the colored areas faded, becoming lighter. It was only after 300 hours of ultraviolet radiation that the red color faded to green. In the less exposed areas, i.e., the shaded areas, the red color also underwent a loss of color and became more yellow. The discoloration effect is less pronounced in this case because the shaded areas receive less ultraviolet radiation.

[0096] Example 3

[0097] A composite material was prepared comprising a matrix made of a propylene copolymer, EPDM (ethylene-propylene-diene monomer) as the elastomer, and vine shoot powder as a natural fiber containing lignin. Unlike the material in Example 1, a sieving step was performed on the vine shoot powder to at least partially remove the finest particles. A particle size analysis of the sieved powder was carried out before the particles were added to the mixture using calibrated sieves. The powder added to form the composition shows the following particle size distribution: 2% fibers with a length greater than 1000 µm; 58.2% fibers with a length between 530 µm and 1000 µm; and 39.8% fibers with a length less than 530 µm.

[0098] After 200 hours of ultraviolet radiation, similarly to the previous example, no discoloration was observed. After 300 hours of ultraviolet radiation, the red color directly exposed to the ultraviolet radiation faded to green. However, in the least exposed areas, i.e., in the shaded areas, the red color remained red, demonstrating greater photostability of this composite material containing 60.2% particles with a particle size between 530 µm and 2000 µm.

[0099] These examples therefore show that the exclusion of fine particles of natural fibers containing lignin, and more particularly vine shoot powder, This makes the composite material more stable to light by delaying its discoloration. This new property is advantageous for manufacturing aesthetic parts for the interior of a motor vehicle.

Claims

Claims

1. Composite material containing natural fibers comprising: from 20 to 98% by mass relative to the total mass of the composite material of a polypropylene matrix; from 1 to 30% by mass relative to the total mass of the composite material of at least one elastomer; from 1 to 60% by mass relative to the total mass of the composite material of natural fibers comprising lignin, from 0 to 30% by mass relative to the total mass of the composite material of an inorganic filler; the material being characterized in that said natural fibers comprising lignin are in the form of particles and at least 15% by mass of the particles relative to the total mass of said particles have a particle size greater than 500 μm, and preferably between 500 and 2000 μm.

2. Composite material according to claim 1, characterized in that said natural fibers are selected from the group comprising vine shoot, hemp, sisal, miscanthus, cellulose, wood, cork, jute, bamboo and mixtures thereof; preferably, said natural fibers are or comprise vine shoot.

3. Composite material according to claim 1 or 2, characterized in that at least 15% by mass of the particles relative to the total mass of said particles have a particle size greater than 520 pm, preferably greater than 550 pm; and / or at least 15% by mass of the particles relative to the total mass of said particles have a particle size less than 1500 pm; preferably less than 1100 pm.

4. Composite material according to one of claims 1 to 3, characterized in that said composite material comprises between 0.1 and 1% by mass relative to the total mass of the composite material of at least one hindered amine type light stabilizer and / or between 0.1 and 10% by mass relative to the total mass of the composite material of at least one ultraviolet absorbing agent.

5. Composite material according to one of claims 1 to 4, characterized in that the composite material further comprises between 0.1% and 10% by mass relative to the total mass of the composite material of at least one colored pigment; and / or in that the composite material further comprises between 1% and 10% by mass relative to the total mass of the composite material of at least one coupling agent; preferably, said coupling agent is a maleated polypropylene showing a maleic anhydride content of at least 1.0% by mass relative to the total mass of the maleated polypropylene.

6. Composite material according to one of claims 1 to 5, characterized in that the matrix is ​​based on polypropylene and has a melt flow index of between 1 and 200 g / 10 min as measured in accordance with ISO 1133 conditions M, at 230°C and under a load of 2.16 kg; and / or in that the matrix is ​​based on polypropylene and consists of a propylene homopolymer and / or a propylene-alpha-olefin copolymer consisting of at least 70% by mass of propylene relative to the total mass of the matrix, and up to 30% by mass of at least one alpha-olefin relative to the total mass of the matrix, the alpha-olefin of the propylene-alpha-olefin copolymer being chosen from the group of alpha-olefins comprising 2 or 4 to 20 carbon atoms and mixtures thereof.

7. Composite material according to one of claims 1 to 6, characterized in that at least one elastomer is an ethylene-alpha-olefin copolymer comprising from 20 to 80% by mass of ethylene relative to the total mass of the ethylene-alpha-olefin copolymer, and from 80 to 20% by mass of at least one alpha-olefin relative to the total mass of the ethylene-alpha-olefin copolymer; the alpha-olefin of the ethylene-alpha-olefin copolymer being chosen from the group of alpha-olefins comprising 3 to 20 carbon atoms and mixtures thereof; and / or in that at least one elastomer is selected from the group comprising ethylene-propylene-diene monomer (EPDM), styrene isoprene styrene block copolymers (SIS), hydrogenated styrene isoprene styrene block copolymers (SEPS), styrene butadiene styrene block copolymers (SBS), hydrogenated styrene butyrene block copolymers (SEBS), styrene butyrene styrene block copolymers (SBSS) and mixtures thereof.

8. Use of a composite material containing natural fibers according to one of claims 1 to 7 for the production of an interior trim part of a motor vehicle; preferably this use takes place in the context of the production of an interior trim of a motor vehicle by injection.

9. Interior trim part of a motor vehicle, said part being produced from a composite material containing natural fibers according to one of claims 1 to 7; preferably, the interior trim part is produced by extrusion, blow molding, injection, rotational molding or injection blow molding; more preferably, the interior trim part is produced by injection.

10. A method of producing a composite material containing natural fibers according to one of claims 1 to 7, said composite material comprising from 20 to 98% by mass relative to the total mass of the composite material of a propylene-based matrix; from 1 to 30% by mass relative to the total mass of the composite material of at least one elastomer; from 1 to 60% by mass relative to the total mass of the composite material of natural fibers comprising lignin; from 0 to 30% by mass relative to the total mass of the composite material of an inorganic filler; said method being characterized in that it comprises the following steps: a) grinding (100) natural fibers comprising lignin to obtain particles; preferably to obtain particles with a particle size of less than 2000 μm;b) sieving (200) said particles of natural fibers comprising lignin carried out with a sieve so as to obtain a residue comprising at least 15% by mass of the particles relative to the total mass of said particles having a particle size greater than 500 pm; and preferably between 500 and 2000 pm; c) collecting (300) the residue; and d) mixing (400) said residue obtained in step (c) with the other components in order to form said composite material.;