SINGLE-LAYER OR MULTI-LAYER TUBULAR STRUCTURE BASED ON RECYCLED POLYAMIDE

A composition of recycled polyamide materials, combined with semi-crystalline aliphatic polyamide and additives, addresses the degradation issues of end-of-life vehicle pipes, enabling their reuse and reducing environmental impact and costs.

FR3125052B1Active Publication Date: 2024-09-27ARKEMA FRANCE SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FR2021007457
Authority / Receiving Office
FR · FR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-07-09
Publication Date
2024-09-27
Estimated Expiration
2041-07-09

AI Technical Summary

Technical Problem

End-of-life motor vehicle pipes and tanks made of polyamide are often too degraded for reuse due to stiffening and thermo-oxidative degradation, leading to incineration and environmental impact, which contradicts the goal of 100% recycling by vehicle manufacturers.

Method used

A composition comprising 30% to 99.8% recycled polyamide material from used tubes and tanks, combined with semi-crystalline aliphatic polyamide, impact modifiers, plasticizers, and additives, without recompounding, to create tubes and reservoirs with equivalent mechanical properties to new materials.

Benefits of technology

The solution allows for the production of tubes and reservoirs with mechanical properties comparable to new materials, reducing environmental impact and costs by enabling the reuse of recycled polyamide components in vehicles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000042_0000
    Figure 00000042_0000
Patent Text Reader

Abstract

The present invention relates to a composition comprising: (a) 30% to 99.8% by weight, in particular 50% to 99.8% by weight of recycled material from a used single-layer and / or multi-layer tube and / or tank that originally transported or contained motor vehicle fluids, in particular air, oil, water, a urea solution, a glycol-based coolant, or a fuel such as gasoline, in particular alcoholic gasoline, bio-gasoline, or diesel, in particular bio-diesel, or hydrogen, said tube and / or tank being made of a composition that predominantly comprises at least one polyamide, said used single-layer and / or multi-layer tube and / or tank having been ground into granules and the fluid residues present in said tube and / or tank having been totally or partially extracted, before or after grinding said tube and / or reservoir, (b) up to 70%,in particular up to 50% of a semi-crystalline aliphatic polyamide, (c) up to 0.2% of an additive, said polyamide of said used tube and / or tank having functionalities resulting from oxidation reactions selected from the imide, carboxylic acid, alcohol and mixtures thereof, in a molar ratio greater than that of the same polyamide constituting an unused tube and / or tank which has never before transported or contained motor vehicle fluids.
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: SINGLE-LAYER OR MULTI-LAYER TUBULAR STRUCTURE BASED ON RECYCLED POLYAMIDE Technical field

[0001] The present invention relates to a composition obtained from used polyamide pipes from motor vehicles, single-layer or multi-layer tubular structures comprising at least one layer made of said composition and a method of manufacturing them. Prior art

[0002] Every year, several million motor vehicles become unusable worldwide. An end-of-life motor vehicle (ELV) contains many toxic and polluting products (liquid or solid): used oil, battery, air conditioning fluid, explosive airbag components, etc. If treated in poor conditions, this waste can lead to soil and water pollution, as well as accidents. ELVs are therefore considered hazardous waste.

[0003] A large quantity of vehicle components can be recovered and recycled, in the form of used spare parts or raw materials. Parts intended for reuse (headlights, indicators, engine, radiator, starter, hood, wings, doors, etc.) are dismantled and stored for resale.

[0004] Non-recyclable carcasses and parts (ferrous and non-ferrous metals, plastics, glass, rubber, etc.) are separated and crushed for recovery or disposal.

[0005] European Directive 2000 / 53 / EC on end-of-life vehicles has set a reuse and recovery rate of 95% by weight per vehicle from 2015.

[0006] There should therefore only remain 5% of ultimate waste, that is to say waste which is not capable of being treated under the technical and economic conditions of the moment and which will be incinerated or evacuated to specific storage centers.

[0007] The 95% reused and recovered are the subject of:

[0008] Energy recovery: use of waste (oils, tires, plastics, etc.) as a means of energy production, by direct incineration with or without other waste;

[0009] Material recovery: Reuse or re-employment: new use of a part which retains the same use and is not transformed, or

[0010] Recycling: operation aimed at introducing materials from waste into the production cycle, as a total or partial replacement for virgin material.

[0011] A motor vehicle contains a large number of pipes including pipes intended for the transport of fluids such as air, oil (for example for cooling the automatic gearbox "TOC", Transmission Oil Cooler), water, a urea solution, a glycol-based coolant, a fuel such as gasoline, in particular bio-gasoline or diesel, in particular bio-diesel, or hydrogen.

[0012] It also contains reservoirs which made it possible to store said fluid in the vehicle.

[0013] These pipes can be single-layer and / or multi-layer tubular structures, in particular based on polyamide(s), just as the tanks can be single-layer and / or multi-layer structures, in particular based on polyamide(s).

[0014] When the motor vehicle is out of use, the various pipes present in it are generally very or too degraded to be able to be reused as such, in the form of a tube, without risk or without this leading to excessively degraded usage properties.

[0015] Indeed, the tubes, particularly under the engine hood, are placed in a severe thermo-oxidative environment due to the heat released by the engine which can typically reach 150°C and the presence of air and therefore oxygen. Each increase in temperature of 10°C typically results in a halving of the service life of the tubes as well as the degradation of certain additives of said tubes such as stabilizers.

[0016] Until now, the hose of the motor vehicle out of use or the tank are not reused and are often incinerated but this then contributes to global warming, the reduction of which is becoming one of the major challenges of the 21st century.

[0017] Furthermore, several motor vehicle manufacturers have the more or less long-term objective of recycling 100% of the vehicles they produce in order to achieve an environmental impact equal to zero.

[0018] Consequently, the supply of recycled pipes to these manufacturers becomes essential and then makes it possible to reduce the quantity of pipe to be thrown away or incinerated.

[0019] The reuse, without modification, of tubes taken from end-of-life cars is not envisaged for the following reasons:

[0020] Analysis of the tubes at the end of their life showed that they had stiffened compared to

[0021] a new tube: the tube at the end of its life has a higher threshold stress (loss of additives, and crystallization induced by the working environment). This stiffening is a problem because the tube risks being damaged during disassembly and assembly on a new vehicle (tubes particularly stressed during feathering).

[0022] The end-of-life tubes were also thermoformed when they were installed in the new vehicle to fit exactly into the vehicle model, a model which will not be probably no longer produced 10 to 15 years after the sale of said vehicle.

[0023] A tank has a specific shape adapted to each vehicle model which changes regularly.

[0024] Conventionally, when a used tube has to be recycled, it is first crushed then recompounded and possibly reformulated before being extruded to make a new tube.

[0025] It is necessary to find ways to reuse or recycle these tubes in order to limit the environmental impact of the motor vehicle industry, and also to limit the costs of recycling used pipe in order to provide motor vehicle manufacturers with pipes at a price compatible with the range of vehicles marketed.

[0026] The present invention therefore relates to a composition comprising:

[0027] (a) 30% to 99.8% by weight, in particular 50 to 99.8% by weight of recycled material from a used single-layer and / or multi-layer tube and / or tank having initially transported or contained motor vehicle fluids, in particular air, oil, water, a urea solution, a glycol-based coolant, or a fuel such as gasoline, in particular alcoholic gasoline, bio-gasoline or diesel, in particular bio-diesel, or hydrogen, said tube and / or said tank being made of a composition which predominantly comprises at least one polyamide,

[0028] said single-layer and / or multi-layer tube and / or said used tank(s) having been ground into granules and the fluid residues present in said tube and / or tank having been totally or partially extracted, before or after grinding said tube and / or tank,

[0029] (b) up to 70%, in particular up to 50% of a semi-aliphatic polyamide crystalline,

[0030] (c) up to 45% by weight of at least one impact modifier, in particular from 1 to 45% by weight weight of at least one impact modifier, in particular from 2 to 45% by weight of at least one impact modifier,

[0031] (d) up to 20% by weight of at least one plasticizer,

[0032] (e) up to 0.2% of an additive,

[0033] said polyamide of said tube and / or said used tank having functions resulting from oxidation reactions chosen from imide functions, carboxylic acids, alcohols and their mixtures, in a molar ratio relative to the amide functions greater than that of the same polyamide constituting an unused tube and / or tank which has never before transported or contained fluids for a motor vehicle.

[0034] Advantageously, said single-layer and / or multi-layer tube and / or said used tank(s) is / are only ground into granules, excluding subsequent grinding of a recomposing with or without reformulation.

[0035] The expression “motor vehicle” means any vehicle with a thermal, electric or hybrid engine equipped with wheels or tracks, excluding a flying vehicle.

[0036] The motor vehicle may be two-wheeled, three-wheeled, four-wheeled or tracked.

[0037] It is for example chosen from an electric bicycle, a moped, a motorcycle, a sidecar, a car, a van, a tractor, a truck, a bus, a coach, a snowmobile, a half-track, a bulldozer, a snow groomer and a tank.

[0038] In particular, it is chosen from a car, a van, a truck, a bus and a coach.

[0039] When using tubes or tanks in motor vehicles for the transport or storage of fluids, new species resulting from oxidation mechanisms, in particular amide functions and / or methylene alpha to said amide functions, such as imide functions, carboxylic acids and alcohols, appear in the polyamides constituting said tubes or tanks. Said functions can be detected by infrared spectrometry.

[0040] Thus the absorption band from 1700 to 1740 cm1 corresponds to an imide, that from 1680 to 1720 cm1 to the carbonyl of the carboxylic acid and that from 3580 to 3670 cm-1 corresponds to the alcohol function of the carboxylic acid.

[0041] The absorption band from 3580 to 3670 cm-1 corresponds to the free alcohol function.

[0042] The amide function is characterized on the one hand by a pair of absorption bands from 3100 to 3500 cm-1 and from 15560 to 1640 cm-1 which corresponds to the NH group of the amide and on the other hand by the absorption band from 1650 to 1700 cm-1 which corresponds to the carbonyl group of the amide.

[0043] The inventors have therefore surprisingly found that the use of at least 30% by weight, in particular at least 50% by weight of recycled material based on partially oxidized polyamides and originating from a used and only ground single-layer and / or multi-layer tube and / or tank, the fluid residues present in said tube and / or tank having been extracted totally or partially, before or after grinding said tube and / or tank, with a semi-crystalline aliphatic polyamide, and optionally an additive, allowed the constitution of a composition which can then be transformed into a tube or tank whose mechanical properties are equivalent to those of a tube or tank originating from non-recycled and non-used material, i.e. a new tube or tank.

[0044] Throughout the description, the term "tube" or "pipe" may be used and means the same thing.

[0045] The recycled material therefore corresponds to a single-layer and / or multi-layer tank used and which therefore initially transported or contained motor vehicle fluids.

[0046] It does not in any case correspond to a material resulting from a process for manufacturing a tube or a tank and which would correspond either to scrap material or to rejects or to tubes or tanks which do not comply with the specifications and which have never transported a fluid for a motor vehicle, and which would then be reintroduced into said process. Regarding the composition

[0047] The composition comprises:

[0048] (a) 30% to 99.8% by weight, in particular 50 to 99.8% by weight of recycled material originating from a used single-layer and / or multi-layer tube and / or tank, said tube and / or said tank being made of a composition which mainly comprises at least one polyamide,

[0049] said single-layer and / or multi-layer tube and / or said used tank(s) having been solely ground into granules and the fluid residues present in said tube and / or tank having been totally or partially extracted, before or after grinding said tube and / or tank,

[0050] (b) up to 70%, in particular up to 50% of a semi-aliphatic polyamide crystalline,

[0051] (c) up to 45% by weight of at least one impact modifier, in particular from 1 to 45% by weight weight of at least one impact modifier, in particular from 2 to 45% by weight of at least one impact modifier,

[0052] (d) up to 20% by weight of at least one plasticizer,

[0053] (e) up to 0.2% of an additive,

[0054] said polyamide of said tube and / or said used tank having functions resulting from oxidation reactions chosen from imide functions, carboxylic acids, alcohols and their mixtures, in a molar ratio relative to the amide functions greater than that of the same polyamide constituting an unused tube and / or tank which has never before transported or contained fluids for a motor vehicle.

[0055] The term "fluid" means a gas or liquid used in motor vehicles, in particular air, oil, water, a urea solution, a glycol-based coolant, or a fuel such as gasoline, in particular alcohol-based gasoline, bio-gasoline or diesel, in particular bio-diesel, or hydrogen.

[0056] Advantageously, said fluid designates fuels, in particular gasoline, in particular alcoholic gasoline, bio-gasoline or diesel, in particular biodiesel.

[0057] The term "gasoline" designates a mixture of hydrocarbons resulting from the distillation of petroleum to which additives or alcohols such as methanol and ethanol may be added, with alcohols being the major components in some cases.

[0058] The term "alcohol-based gasoline" refers to gasoline to which methanol or ethanol has been added. It also refers to E95-type gasoline that does not contain petroleum distillation products.

[0059] The expression "polyamide-based" means at least 50% by weight of polyamide in the layer.

[0060] The semi-crystalline aliphatic polyamide used in b) may contain impact modifiers, and / or plasticizers and / or additives.

[0061] The oxidation reactions or oxidation mechanisms correspond to an oxidation in particular of the amide functions and / or of methylene in alpha (a) of said amide functions.

[0062] The used tube and / or the used tank to be reused or in other words to be recycled (single-layer and / or multi-layer for both the tube and the tank) is therefore removed from the motor vehicle, in particular from the automobile, and undergoes crushing.

[0063] Advantageously, it undergoes only grinding, excluding grinding followed by recompounding with or without reformulation.

[0064] Such recompounding is conventionally carried out by introducing the ground material at least once into an extruder, in particular of the co-rotating twin-screw type, or of the co-kneader type (Buss), where the ground material is remixed by melting, with or without the addition of at least one compound chosen from a semi-crystalline aliphatic polyamide, of recycled origin or not, at least one impact modifier, a plasticizer, an additive and antistatic fillers. The molten material emerges from the extruder in rods which are cooled and cut into granules which will then be introduced into an extruder for the manufacture of the single-layer or multi-layer tubular structure.

[0065] On the other hand, the fluid residues present in said tube and / or reservoir are extracted totally or partially, before or after crushing said tube and / or reservoir.

[0066] In a first embodiment, said molar ratio of the functions resulting from oxidation reactions is between 1 / 10000 and 1 / 20.

[0067] Concentrations can be measured by proton NMR in dichloromethane-d2, by adding HFIP (hexafluoroisopropanol) to solubilize the polyamide.

[0068] In a first variant, said molar ratio of the imide functions is from 1 / 1000 to 1 / 20, in particular from 1 / 500 to 1 / 20, in particular from 1 / 200 to 1 / 50.

[0069] In a second variant, said molar ratio of carboxylic acid functions is from 1 / 5000 to 1 / 20, in particular from 1 / 3000 to 1 / 50, very advantageously from 1 / 500 to 1 / 25.

[0070] In a third variant, said molar ratio of alcohol functions is comprised of 1 / 1000 to 1 / 20 and advantageously between 1 / 1000 and 1 / 25, very advantageously between 1 / 200 and 1 / 50.

[0071] Since the composition is made up of at most 99.8% recycled material, it is then necessary to add a polyamide (identical or different) of non-recycled origin to the material to be recycled and / or an impact modifier and / or a plasticizer and / or optionally an additive. This can be done by dry mixing (mixture of recycled shred and formulated or unformulated virgin granules and / or optionally the additive) or by compounding, advantageously by dry mixing.

[0072] This dry mixture is then introduced into the extruder during the manufacture of the single-layer or multi-layer tubular structure.

[0073] The nomenclature used to define polyamides is described in ISO 1874-1:2011 "Plastics — Polyamide (PA) materials for molding and extrusion — Part 1: Designation" and is well known to those skilled in the art.

[0074] The term “polyamide” according to the invention designates both a homopolyamide and a copolyamide.

[0075] The expression "semi-crystalline polyamide" within the meaning of the invention throughout the description designates polyamides which have a melting temperature (Tf) and an enthalpy of fusion AH > 25 J / g, in particular > 40 J / g, in particular > 45 J / g, as well as a glass transition temperature (Tg) as determined by DSC according to the standard ISO 11357-1:2016 and ISO 11357-2 and 3:2013, at a heating rate of 20K / min.

[0076] Said at least one aliphatic semi-crystalline polyamide is obtained from the polycondensation of at least one lactam, or from the polycondensation of at least one amino acid, or from the polycondensation of at least one diamine X with at least one dicarboxylic acid Y.

[0077] When said at least one aliphatic semi-crystalline polyamide is obtained from the polycondensation of at least one lactam, said at least one lactam may be chosen from a C6 to C18 lactam, preferably a C10 to C18 lactam, more preferably a C10 to C12 lactam. A C6 to C18 lactam is in particular caprolactam, decanolactam, undecanolactam, and lauryllactam.

[0078] When said at least one aliphatic semi-crystalline polyamide is obtained from the polycondensation of at least one lactam, it can therefore comprise a single lactam or several lactams.

[0079] Advantageously, said at least one aliphatic semi-crystalline polyamide is obtained from the polycondensation of a single lactam and said lactam is chosen from lauryllactam and undecanolactam, advantageously lauryllactam.

[0080] When said at least one aliphatic semi-crystalline polyamide is obtained from the polycondensation of at least one amino acid, said at least one amino acid may be chosen from an amino acid in C6 to C18, preferably in C10 to C18, more preferably in C10 to C12.

[0081] A C6 to C18 amino acid is in particular 6-aminohexanoic acid, 9-aminononanoic acid, 10-aminodecanoic acid, 10-aminoundecanoic acid, 12-aminododecanoic acid and 11-aminoundecanoic acid as well as its derivatives, in particular N-heptyl-11-aminoundecanoic acid.

[0082] When said at least one aliphatic semi-crystalline polyamide is obtained from the polycondensation of at least one amino acid, it can therefore comprise a single amino acid or several amino acids.

[0083] Advantageously, said aliphatic semi-crystalline polyamide is obtained from the polycondensation of a single amino acid and said amino acid is chosen from 10-aminodecanoic acid, 11-aminoundecanoic acid and 12-aminododecanoic acid, advantageously 11-aminoundecanoic acid.

[0084] When said at least one aliphatic semi-crystalline polyamide is obtained from the polycondensation of at least one C4-C36, preferably C5-C18, preferably C5-C12, more preferably C10-C12, diamine X with at least one C4-C36, preferably C6-C18, preferably C6-C12, more preferably C10-C12 diacid Y, then said at least one X diamine is an aliphatic diamine and said at least one Y diacid is an aliphatic diacid.

[0085] The diamine may be linear or branched. Advantageously, it is linear.

[0086] Said at least one C4-C36 diamine X may in particular be chosen from 1,4-butanediamine, 1,5-pentamethylenediamine, 1,6-hexamethylenediamine, 1,7-heptamethylenediamine, 1,8-octamethylenediamine, 1,9-nonamethylenediamine, 1,10-decamethylenediamine, 1,11-undecamethylenediamine, 1,12-dodecamethyldiamine, 1,13-tridecamethylenediamine, 1,14-tetradecamethylenediamine, 1,16-hexadecamethylenediamine and 1,18-octadecamethylenediamine, octadecenediamine, eicosanediamine, docosanediamine and diamines obtained from fatty acids.

[0087] Advantageously, said at least one diamine X is C5-C18 and chosen from 1,5-pentamethylenediamine, 1,6-hexamethylenediamine, 1,7-heptamethylenediamine, 1,8-octamethylenediamine, 1,9-nonamethylenediamine, 1,10-decamethylenediamine, 1,11-undecamethylenediamine, 1,12-dodecamethylenediamine, 1,13-tridecamethylenediamine, 1,14-tetradecamethylenediamine, 1,16-hexadecamethylenediamine and 1,18-octadecamethylenediamine.

[0088] Advantageously, said at least one diamine X in C5 to C12, is in particular chosen from 1,5-pentamethylenediamine, 1,6-hexamethylenediamine 1,7-heptamethylenediamine, 1,8-octamethylenediamine, 1,9-nonamethylenediamine, 1,10-decamethylenediamine, 1,11-undecamethylenediamine, 1,12-dodecamethylenediamine.

[0089] Advantageously, said at least one diamine X in C6 to C12, is in particular chosen from 1,6-hexamethylenediamine, 1,7-heptamethylenediamine, 1,8-octamethylenediamine, 1,9-nonamethylenediamine, 1,10-decamethylenediamine, 1,11-undecamethylenediamine, 1,12-dodecamethylenediamine.

[0090] Advantageously, the diamine X used is C10 to C12, in particular chosen from 1,10-decamethylenediamine, 1,11-undecamethylenediamine, 1,12-dodecamethylenediamine.

[0091] Said at least one C4 to C36 dicarboxylic acid Y may be chosen from succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, brassylic acid, tetradecanedioic acid, pentadecanedioic acid, hexadecanedioic acid, octadecanedioic acid, and diacids obtained from fatty acids.

[0092] The diacid may be linear or branched. Advantageously, it is linear.

[0093] Advantageously, said at least one dicarboxylic acid Y is C6 to C18 and is chosen from adipic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, brassylic acid, tetradecanedioic acid, pentadecanedioic acid, hexadecanedioic acid, octadecanedioic acid.

[0094] Advantageously, said at least one dicarboxylic acid Y is C6 to C12 and is chosen from adipic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid.

[0095] Advantageously, said at least one dicarboxylic acid Y is C10 to C12 and is chosen from sebacic acid, undecanedioic acid, dodecanedioic acid.

[0096] When said aliphatic semi-crystalline polyamide is obtained from the polycondensation of at least one diamine X with at least one dicarboxylic acid Y, it can therefore comprise a single diamine or several diamines and a single dicarboxylic acid or several dicarboxylic acids.

[0097] Advantageously, said aliphatic semi-crystalline polyamide is obtained from the polycondensation of a single diamine X with a single dicarboxylic acid Y.

[0098] The expression “predominantly comprising at least one aliphatic type polyamide” means that said composition of the layer (1) comprises at least 50% by weight of at least one aliphatic polyamide relative to the total weight of said composition.

[0099] Advantageously, said composition of the layer (1) comprises at least 60% in weight, in particular at least 70% by weight, in particular at least 80% by weight, more particularly at least 90% by weight of at least one aliphatic polyamide relative to the total weight of said composition.

[0100] Said composition of the layer (1) consists of at least 30%, in particular at least 50% and at most 99.8%, of recycled material originating from a single-layer and / or multi-layer tube and / or a tank, said tubes and tanks being used and having been intended for the transport or storage of fluids for motor vehicles.

[0101] This means either that the “at least one majority polyamide” of said composition corresponds in its entirety to what is called “at least 50% recycled material” or that at least 50% by weight of all the constituents of the composition are of recycled origin coming from a single-layer tube, or from a multi-layer tube, or from a tank or from a mixture of these.

[0102] The recycled material may come from a single-layer and / or multi-layer tube and / or a single-layer and / or multi-layer tank, said single-layer and / or multi-layer tubes being used and having been intended for the transport of fluid for a motor vehicle and / or the single-layer and / or multi-layer tank being used and having been intended for the storage of fluid for a motor vehicle. Said tube or tank is therefore a used tube or a used tank, that is to say that it has been used for at least one year for the transport or storage of said fluid defined above. Said single-layer tube is made of a composition comprising a semi-crystalline aliphatic polyamide and optionally impact modifiers and / or additives and / or plasticizers and / or antistatic fillers.

[0103] Said multilayer tube comprises at least one layer consisting of a composition comprising a semi-crystalline aliphatic polyamide and optionally impact modifiers and / or additives. It may therefore comprise other layers consisting of a thermoplastic polymer other than a semi-crystalline aliphatic polyamide, such as for example a polyethylene, a polypropylene, a semi-aromatic polyamide or a poly ethylene vinyl alcohol (EVOH).

[0104] Said reservoir may be single-layer and is made of a composition comprising a semi-crystalline aliphatic polyamide and optionally impact modifiers and / or additives and / or plasticizers and / or antistatic fillers.

[0105] Said tank may be multi-layer and comprises at least one layer consisting of a composition comprising a semi-crystalline aliphatic polyamide and optionally impact modifiers and / or additives. It may therefore comprise other layers consisting of a thermoplastic polymer other than a semi-crystalline aliphatic polyamide, such as for example a polyethylene, a polypropylene, a semi-aromatic polyamide or a poly ethylene vinyl alcohol (EVOH).

[0106] It is obvious that the single-layer tube can also be a mixture of mo tube nocouche, i.e. for example two types of single-layer tubes each made of a different semi-crystalline aliphatic polyamide, for example a PA11 and a PA12.

[0107] It is also obvious that the multilayer tube can also be a mixture of different types of multilayer tube, provided that at least one of the layers of one of the types of multilayer tube is made of a semi-crystalline aliphatic polyamide.

[0108] It is also obvious that the single-layer reservoir can also be a mixture of single-layer reservoirs, i.e. for example two types of single-layer tubes each made of a different semi-crystalline aliphatic polyamide, for example a PAU and a PA12.

[0109] It is also obvious that the multi-layer tank can also be a mixture of different types of multi-layer tank, provided that at least one of the layers of one of the types of multi-layer tank is made of a semi-crystalline aliphatic polyamide.

[0110] If the mixed tubes or reservoirs are incompatible with each other, then the addition of a third semi-crystalline aliphatic polyamide noted B having an average number of carbon atoms per nitrogen atom CB is present to make them compatible.

[0111] If we note A the polyamide of the tube and C the polyamide of the reservoir and which are not compatible:

[0112] Then CB is between (CA+Cc) / 2-2 and (CA+Cc) / 2+2, advantageously (CA+Cc) / 2-1 and (Ca+Cc) / 2+1

[0113] Said single-layer and / or multi-layer tube which was intended for the transport of fluid for motor vehicles and which is therefore used undergoes several different treatments in order to be able to be recycled:

[0114] The fluid residues are either first extracted completely or partially and then the single-layer and / or multi-layer tube and / or the reservoir are crushed, or the single-layer and / or multi-layer tube and / or the reservoir are crushed and then the fluid residues are extracted completely or partially from the crushed material obtained.

[0115] In one embodiment, the extraction of said fluid residues is carried out by means of washing or ventilation.

[0116] Washing can be carried out before or after grinding.

[0117] Advantageously, the washing is carried out using a fluid such as supercritical CO2 or solvents such as methanol, ethanol, in particular methanol, or a mixture of supercritical CO2 and solvent.

[0118] This washing makes it possible in particular to remove fluids miscible in methanol, such as fuels, oil, coolants

[0119] Advantageously, the ventilation is carried out by means of an inerted oven or a desiccator.

[0120] In one embodiment, the extraction is carried out after grinding by means of a degassing zone in said extruder or by means of another apparatus allowing degassing to be carried out in the molten state.

[0121] Advantageously, the used pipes before or after crushing are cleaned to remove any residual oligomers possibly present in the used pipes.

[0122] Fluids such as fuels, when stored in a tank or transported in a tube, degrade the polymer of the constituent layer of the tube in contact with the fluid and cause the appearance of oligomers which must therefore be cleaned before recycling the tubes.

[0123] The oligomers are cleaned by washing with water or polar solvents such as methanol or ethanol.

[0124] PA 6 and 66 are for example systematically washed with hot water (approximately 100 to 120°C) to remove a maximum of caprolactam.

[0125] The oligomers can otherwise be distilled.

[0126] In the case of extraction by ventilation, this can be carried out after grinding in an inerted oven or during the extrusion of the tubular structure if the extruder is equipped with a degassing zone.

[0127] The fluid residues may be any fluid originally transported by the single-layer or multi-layer tube or stored in the reservoir.

[0128] Extraction can also be carried out before or after grinding, for example by vacuuming if the fluid residues are volatile.

[0129] According to another aspect, the present invention relates to a single-layer or multi-layer tubular (MLT) structure intended for the transport of fluids for a motor vehicle, in particular air, oil, water, a urea solution, a glycol-based coolant, or a fuel such as gasoline, in particular alcoholic gasoline, bio-gasoline or diesel, in particular bio-diesel, or hydrogen, comprising at least one layer (1) consisting of a composition as defined above.

[0130] In one embodiment, said tubular structure presents during the first storage of gasoline, in particular alcoholic gasoline, at most 0.3 g / m2 of insoluble extract, advantageously at most 0.2 g / m2.

[0131] In one embodiment, said tubular structure has, during the first storage of gasoline, in particular alcoholic gasoline, 30%, in particular 40%, in particular 50% less insoluble extract than the same tubular structure made from non-recycled material.

[0132] The single-layer tubular structure intended for the transport of fluids for motor vehicles of the invention makes it possible to significantly reduce the proportion of extractables as determined by a test which consists of filling a tubular structure with gasoline al cooled type FAM-B and heating the whole thing to 60°C for 96 hours, then emptying it by filtering the fluid into a beaker.

[0133] The insoluble extracts present during filtration on the filter are weighed after drying and represent less than 0.3 g / m2.

[0134] The soluble extracts are quantified by allowing the filtrate of the beaker to evaporate at room temperature and then by weighing this residue. The proportion of soluble extracts is advantageously less than or equal to approximately 15g / m2 of internal tube surface.

[0135] Alcoholic gasoline FAM B is described in DIN 51604-1:1982, DIN 51604-2:1984 and DIN 51604-3:1984.

[0136] Briefly, alcoholic gasoline FAM A is first prepared with a mixture of 50% Toluene, 30% isooctane, 15% di-isobutylene and 5% ethanol then FAM B is prepared by mixing 84.5% FAM A with 15% methanol and 0.5% water.

[0137] In total, FAB consists of 42.3% toluene, 25.4% isooctane, 12.7% di-isobutylene, 4.2% ethanol, 15% methanol and 0.5% water.

[0138] Said tubular structure has a lower extractable content than that of the same tubular structure made from non-recycled material, i.e. virgin or original material during the first storage of gasoline, in particular alcoholic gasoline, and in particular a proportion of insoluble extract lower by 30%, in particular 40%, in particular 50% compared to the proportion present in the same tubular structure but made from non-recycled or virgin material. Regarding layer (1)

[0139] The layer (1) is made up of a composition comprising predominantly at least one semi-crystalline aliphatic polyamide, said composition being made up of at least 30%, in particular at least 50% of recycled material originating from a single-layer and / or multi-layer tube intended for the transport of fluids for a motor vehicle and / or from a single-layer and / or multi-layer tank intended for the storage of fluids for a motor vehicle.

[0140] The composition of the layer (1) being made up of material recycled at most 99.8%, it is then necessary to add a polyamide (identical or different) of non-recycled origin to the material to be recycled and this is then carried out during passage through the extruder during the manufacture of the single-layer or multi-layer tubular structure and / or an additive.

[0141] In one embodiment, said composition of the layer (1) comprises:

[0142] at least 50% by weight, in particular from 50% to 99.8% by weight, of at least one semi-crystalline aliphatic polyamide noted C having an average number of carbon atoms per nitrogen atom noted Cc of from 6 to 18, advantageously from 8 to 12;

[0143] from 0 to 50% by weight of at least one semi-crystalline aliphatic polyamide noted B and having an average number of carbon atoms per nitrogen atom noted CB = Ce - 1, preferably CB = Ce - 2;

[0144] from 0 to 50% by weight of a semi-crystalline aliphatic polyamide noted A having an average number of carbon atoms per nitrogen atom noted CA = CB - 1, preferably CA = CB - 2;

[0145] from 0 to 45% by weight of at least one impact modifier, in particular from 1 to 45% by weight of at least one impact modifier, in particular from 2 to 45% by weight of at least one impact modifier,

[0146] from 0 to 20% by weight of at least one plasticizer,

[0147] from 0 to 0.2% by weight of at least one additive,

[0148] the sum of the constituents being equal to 100%.

[0149] In another embodiment, said composition of the layer (1) consists of:

[0150] at least 50% by weight, in particular from 50% to 99.8% by weight, of at least one semi-crystalline aliphatic polyamide noted C having an average number of carbon atoms per nitrogen atom noted Cc of from 6 to 18, advantageously from 8 to 12;

[0151] from 0 to 25% by weight of at least one semi-crystalline aliphatic polyamide noted B and having an average number of carbon atoms per nitrogen atom noted CB = Cc - 1, preferably CB = Cc - 2;

[0152] from 0 to 25% by weight of a semi-crystalline aliphatic polyamide noted A having an average number of carbon atoms per nitrogen atom noted CA = CB - 1, preferably CA = CB - 2;

[0153] from 0 to 45% by weight of at least one impact modifier, in particular from 1 to 45% by weight of at least one impact modifier, in particular from 2 to 45% by weight of at least one impact modifier,

[0154] from 0 to 20% of at least one plasticizer,

[0155] from 0 to 0.2% by weight of at least one additive,

[0156] the sum of the constituents being equal to 100%.

[0157] The polyamides noted A, B and C can be of recycled or non-recycled origin provided that the composition of the layer (1) is made up of at least 50% recycled material.

[0158] Advantageously, the Tf of the majority aliphatic semi-crystalline polyamide of the layer (1) is <225°C, in particular <200°C, as determined according to ISO 11357-3: 2013, at a heating rate of 20K / min.

[0159] In one embodiment, said composition of the layer (1) is free of plasticizer and / or impact modifier.

[0160] In another embodiment, said composition of the layer (1) comprises at least one compound chosen from a plasticizer, an impact modifier and an additive, and said recycled material is chosen from a crushed tube.

[0161] Advantageously, in these last two embodiments, said tube is a single-layer tube and / or a multi-layer tube.

[0162] In one embodiment, the fluid transported by said single-layer and / or multi-layer tube or stored in said reservoir is different from that of said multi-layer tubular structure (MLT).

[0163] This means that if the single-layer and / or multi-layer tube has transported a fluid such as air, said multi-layer tubular structure (MLT) may be intended to transport gasoline or, if the single-layer and / or multi-layer tube has transported a fluid such as alcoholic gasoline, said tubular structure (MLT) may be intended to transport diesel.

[0164] The same applies to the tank.

[0165] In another embodiment, the fluid transported by said single-layer and / or multi-layer tube or stored in said reservoir is the same as that of said multi-layer tubular structure (MLT).

[0166] This means that if the single-layer and / or multi-layer tube has transported a fluid such as gasoline, said tubular structure (MLT) may be intended to transport gasoline provided that the gasoline of the single-layer and / or multi-layer tube and of said multi-layer tubular structure (MLT) is the same, for example, alcoholic gasoline.

[0167] The same applies to the tank.

[0168] Advantageously, the recycled material comes from a single-layer tube made up of a composition comprising only a PAU.

[0169] It is quite obvious that said PA11 can be formulated.

[0170] In one embodiment, said composition of the layer (1) comprises at least 60% by weight, in particular at least 70% by weight, in particular at least 80% by weight, in particular at least 90% by weight, more particularly at least 95% of recycled material without however exceeding 99.8%.

[0171] The recycled material can be mixed with virgin polyamide with additives or with a master batch with a large quantity of additives.

[0172] Single-layer or multi-layer tube or recycled used tank

[0173] Said used tube or tank which was intended for the transport or storage of fluid for motor vehicles is crushed with extraction of fluid residues before or after crushing and the composition of the layer (1) resulting from said recycling is made up of a composition comprising:

[0174] at least 50% by weight, in particular from 50% to 99.8% by weight, of at least one semi-crystalline aliphatic polyamide noted C having an average number of carbon atoms per nitrogen atom noted CC of from 6 to 18, advantageously from 8 to 12;

[0175] from 0 to 25% by weight of at least one semi-crystalline aliphatic polyamide noted B and having an average number of carbon atoms per nitrogen atom noted CB = Ce -1, preferably CB = Ce - 2;

[0176] from 0 to 25% by weight of a semi-crystalline aliphatic polyamide noted A having an average number of carbon atoms per nitrogen atom noted CA = CB - 1, preferably CA = CB - 2;

[0177] from 0 to 45% by weight of at least one impact modifier, in particular from 3 to 45% by weight of at least one impact modifier,

[0178] from 0 to 20% by weight of at least one plasticizer,

[0179] from 0 to 0.2% by weight of at least one additive,

[0180] the sum of the constituents being equal to 100%. Advantageously, in this first variant, the semi-crystalline aliphatic polyamide denoted C is chosen from PA612, PA1012, PA1010, PAU and PA12, in particular PAU.

[0181] Advantageously, it is only ground, excluding grinding followed by re-compounding with or without reformulation.

[0182] Advantageously, said used tube or said tank was intended for the transport or storage of fuel such as gasoline, in particular alcoholic gasoline, bio-gasoline or diesel, in particular bio-diesel.

[0183] Advantageously, in this first variant, the semi-crystalline aliphatic polyamide denoted C is chosen from PA612, PA 1012, PA 1010, PAU and PA 12, in particular PA11 and said tube was intended for the transport of fuel such as gasoline, in particular alcoholic gasoline, bio-gasoline or diesel, in particular bio-diesel.

[0184] Advantageously, said tube or said tank which has been intended for the transport or storage of fluid for a motor vehicle is single-layer, advantageously said tube and said tank are mixed in a range of 5 / 95 to 95 / 5 by weight. With regard to layer (2)

[0185] In one embodiment, the structure is multi-layer and comprises at least one layer (2).

[0186] The terms “semi-crystalline polyamide” and “aliphatic” have the same definition as for layer (1).

[0187] Said at least one aliphatic semi-crystalline polyamide is obtained in the same manner as described above for layer (1).

[0188] In a first variant, said layer (2) is made up of a composition comprising mainly at least one semi-crystalline aliphatic polyamide and optionally at least one impact modifier,

[0189] and when the layer (2) is made up of a composition comprising predominantly at least one semi-crystalline aliphatic polyamide which is PA 12 and / or PA610 and / or PA612 and / or PA1010 and / or PA 6, then said composition comprises said impact modifier, and said layer (2) is made of at least 90% non-recycled material.

[0190] In one embodiment of this first variant, said layer (2) is devoid of impact modifier.

[0191] In this case, the semi-crystalline aliphatic polyamide which is PA12 and / or PA610 and / or PA612 and / or PA1010 and / or PA 6, is excluded from the composition which constitutes the layer (2).

[0192] In another embodiment of this first variant of the layer (2), said layer (2) comprises from 3 to 45% by weight of at least one impact modifier, in particular from 5 to 20% by weight of at least one impact modifier.

[0193] In yet another embodiment of this first variant, said layer (2) is made up of a composition comprising:

[0194] at least 50% by weight, in particular from 50% to 99.8% by weight, of at least one semi-crystalline aliphatic polyamide noted D having an average number of carbon atoms per nitrogen atom noted CD of from 6 to 18, advantageously from 9 to 15;

[0195] from 0 to 25% by weight of at least one semi-crystalline aliphatic polyamide noted E and having an average number of carbon atoms per nitrogen atom noted CE = CD -1, preferably CE = CD - 2;

[0196] from 0 to 25% by weight of a semi-crystalline aliphatic polyamide noted F having an average number of carbon atoms per nitrogen atom noted CF = CE - 1, preferably CF = CE - 2;

[0197] from 3 to 45% by weight of at least one impact modifier, in particular from 5 to 20% by weight of at least one impact modifier;

[0198] from 0 to 20% of at least one plasticizer;

[0199] from 0 to 0.2% by weight of at least one additive,

[0200] from 0 to 35% of at least one antistatic filler,

[0201] the sum of the constituents being equal to 100%.

[0202] In another embodiment of this first variant, said layer (2) is made up of a composition consisting of:

[0203] at least 50% by weight, in particular from 50% to 99.8% by weight, by weight, of at least one semi-crystalline aliphatic polyamide noted D having an average number of carbon atoms per nitrogen atom noted CD of from 6 to 18, advantageously from 9 to 15;

[0204] from 0 to 25% by weight of at least one semi-crystalline aliphatic polyamide noted E and having an average number of carbon atoms per nitrogen atom noted CE = CD -1, preferably CE = CD - 2;

[0205] from 0 to 25% by weight of a semi-crystalline aliphatic polyamide noted F having an average number of carbon atoms per nitrogen atom noted CF = CE - 1, preferably tially CF = CE - 2;

[0206] from 3 to 45% by weight of at least one impact modifier, in particular from 5 to 20% by weight of at least one impact modifier;

[0207] from 0 to 20% of at least one plasticizer;

[0208] from 0 to 0.2% by weight of at least one additive,

[0209] from 0 to 35% of at least one antistatic filler,

[0210] the sum of the constituents being equal to 100%.

[0211] Advantageously, the composition of said layer (2) comprises a PAU, a PA12 or a PA612 and from 3 to 45% by weight of an impact modifier, in particular from 5 to 20% by weight of an impact modifier. Regarding layer (2')

[0212] In one embodiment, the multilayer tubular structure comprises at least one layer (2') consisting of a composition comprising predominantly at least one semi-crystalline or semi-aromatic aliphatic polyamide, said layer (2') being made of at least 90% non-recycled material.

[0213] The terms “semi-crystalline polyamide” and “aliphatic” have the same definition as for layer (1) or layer (2).

[0214] Said at least one aliphatic semi-crystalline polyamide is obtained in the same manner as described above for layer (1) and layer (2).

[0215] In a first variant of the layer (2'), said layer (2') is devoid of impact modifier.

[0216] In a second variant of the layer (2'), said layer (2') comprises from 3 to 45% by weight of at least one impact modifier, in particular from 5 to 20% by weight of at least one impact modifier.

[0217] In one embodiment of this second variant, said layer (2') is made up of a composition comprising:

[0218] at least 50% by weight, in particular from 50% to 97% by weight, in particular from 50% to 95% by weight, of at least one semi-crystalline aliphatic polyamide denoted D having an average number of carbon atoms per nitrogen atom denoted CD of from 6 to 18, advantageously from 9 to 15;

[0219] from 0 to 25% by weight of at least one semi-crystalline aliphatic polyamide noted E and having an average number of carbon atoms per nitrogen atom noted CE = CD -1, preferably CE = CD - 2;

[0220] from 0 to 25% by weight of a semi-crystalline aliphatic polyamide noted F having an average number of carbon atoms per nitrogen atom noted CF = CE - 1, preferably CF = CE - 2;

[0221] from 3 to 45% by weight of at least one impact modifier, in particular from 5 to 20% by weight of at least one impact modifier;

[0222] from 0 to 20% of at least one plasticizer;

[0223] from 0 to 2% by weight of at least one additive,

[0224] from 0 to 35% of at least one antistatic filler,

[0225] the sum of the constituents being equal to 100%.

[0226] In another embodiment of this second variant, said layer (2') is made up of a composition consisting of:

[0227] at least 50% by weight, in particular from 50% to 97% by weight, by weight, in particular from 50% to 95% by weight, of at least one semi-crystalline aliphatic polyamide noted D having an average number of carbon atoms per nitrogen atom noted CD of from 6 to 18, advantageously from 9 to 15;

[0228] from 0 to 25% by weight of at least one semi-crystalline aliphatic polyamide noted E and having an average number of carbon atoms per nitrogen atom noted CE = CD -1, preferably CE = CD - 2;

[0229] from 0 to 25% by weight of a semi-crystalline aliphatic polyamide noted F having an average number of carbon atoms per nitrogen atom noted CF = CE - 1, preferably CF = CE - 2;

[0230] from 3 to 45% by weight of at least one impact modifier, in particular from 5 to 20% by weight of at least one impact modifier;

[0231] from 0 to 20% of at least one plasticizer;

[0232] from 0 to 2% by weight of at least one additive,

[0233] from 0 to 35% of at least one antistatic filler,

[0234] the sum of the constituents being equal to 100%.

[0235] Advantageously, the composition of said layer (2') comprises a PAU, a PA12 or a PA612 and from 3 to 45% by weight of at least one impact modifier, in particular from 5 to 20% by weight of at least one impact modifier.

[0236] In a second variant, said layer (2') is made up of a composition comprising mainly at least one semi-aromatic polyamide.

[0237] Said at least one semi-crystalline semi-aromatic polyamide is obtained from the polycondensation of at least one diamine X as defined above, with at least one aromatic dicarboxylic acid or a diamine Xa with a dicarboxylic acid Y as defined above.

[0238] The aromatic dicarboxylic acid is advantageously chosen from terephthalic acid (denoted T), isophthalic acid (denoted I) and 2,6-naphthalene dicarboxylic acid (denoted N) or mixtures thereof, in particular it is chosen from terephthalic acid (denoted T), isophthalic acid (denoted I) or mixtures thereof.

[0239] Diamine Xa is advantageously an arylamine, which may be chosen from meta-xylylene diamine (MXD, CAS No.: 1477-55-0) or para-xylylene diamine (PXD, CAS No.: 539-48-0).

[0240] When said semi-crystalline semi-aromatic polyamide is obtained from the polycondensation of at least one diamine X with at least one aromatic dicarboxylic acid, or of at least one diamine Xa with at least one dicarboxylic acid Y, it can therefore comprise a single diamine or several diamines and a single dicarboxylic acid or several dicarboxylic acids.

[0241] Advantageously, said semi-crystalline semi-aromatic polyamide is obtained from the polycondensation of a single diamine X with a single aromatic dicarboxylic acid or from the polycondensation of a single diamine Xa with a single dicarboxylic acid Y.

[0242] Advantageously, said semi-aromatic semi-crystalline polyamide is obtained from the polycondensation of at least one diamine X with at least one dicarboxylic acid chosen from terephthalic acid and isophthalic acid, in particular terephthalic acid, or said semi-aromatic semi-crystalline polyamide is obtained from the polycondensation of at least one diamine Xa with at least one dicarboxylic acid Y.

[0243] In particular, said at least one diamine X in C6 to C12 is chosen from 1,6-hexamethylenediamine, 1,7-heptamethylenediamine, 1,8-octamethylenediamine, 1,9-nonamethylenediamine, 1,10-decamethylenediamine, 1,11-undecamethylenediamine, 1,12-dodecamethylenediamine and said at least one dicarboxylic acid is an acid chosen from terephthalic acid and isophthalic acid, in particular terephthalic acid.

[0244] In particular, said at least one diamine Xa is an arylamine chosen from meta-xylylene diamine (MXD, CAS No.: 1477-55-0) or para-xylylene diamine (PXD, CAS No.: 539-48-0) and said at least one dicarboxylic acid Y is C6 to C18 and is chosen from adipic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, brassylic acid, tetradecanedioic acid, pentadecanedioic acid, hexadecanedioic acid, octadecanedioic acid.

[0245] Advantageously, said at least one dicarboxylic acid Y is C6 to C12 and is chosen from adipic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid.

[0246] Each of these semi-aromatic polyamides can be copolymerized with a lactam or an amino acid to result in structures such as PA10 / 10T, PA10 / 9T, PA 10 / 12T, PA11 / 9T, PA11 / 10T, PA11 / 12T, PA12 / 9T, PA12 / 10T and PA12 / 12T or PA11 / MXD6, PA11 / MXD10, PA12 / MXD6, PA12 / MXD10.

[0247] In a third variant, said layer (2') is made up of a composition comprising mainly at least one polyolefin. Regarding the impact modifier and the polyolefin

[0248] The impact modifier is advantageously constituted by a polymer having a flexural modulus of less than 100 MPa measured according to standard ISO 178: 2010, determined at 23°C with a relative humidity: RH50%, and a Tg of less than 0°C (measured according to standard 11357-2: 2013 at the inflection point of the DSC thermogram, at a heating rate of 20K / min), in particular a polyolefin.

[0249] The polyolefin of the impact modifier may be functionalized or non-functionalized or be a mixture of at least one functionalized and / or at least one non-functionalized. For simplicity, the polyolefin has been designated (B) and functionalized polyolefins (B1) and non-functionalized polyolefins (B2) have been described below.

[0250] A non-functionalized polyolefin (B2) is conventionally a homopolymer or copolymer of alpha olefins or diolefins, such as, for example, ethylene, propylene, butene-1, octene-1, butadiene. By way of example, mention may be made of:

[0251] - homopolymers and copolymers of polyethylene, in particular LDPE, HDPE, LLDPE (linear low density polyethylene), VLDPE (very low density polyethylene) and metallocene polyethylene.

[0252] - homopolymers or copolymers of propylene.

[0253] - ethylene / alpha-olefin copolymers such as ethylene / propylene, EPRs (short for ethylene-propylene-rubber) and ethylene / propylene / diene (EPDM).

[0254] - styrene / ethylene-butene / styrene (SEBS) block copolymers, styrene / butadiene / styrene (SBS), styrene / isoprene / styrene (SIS), styrene / ethylene-propylene / styrene (SEPS).

[0255] - copolymers of ethylene with at least one product chosen from salts or esters of unsaturated carboxylic acids such as alkyl (meth)acrylate (e.g. methyl acrylate), or vinyl esters of saturated carboxylic acids such as vinyl acetate (EVA), the proportion of comonomer being up to 40% by weight.

[0256] The functionalized polyolefin (B1) may be a polymer of alpha olefins having reactive units (the functionalities); such reactive units are acid, anhydride, or epoxy functions. By way of example, mention may be made of the preceding polyolefins (B2) grafted or co- or terpolymerized by unsaturated epoxides such as glycidyl (meth)acrylate, or by carboxylic acids or the corresponding salts or esters such as (meth)acrylic acid (the latter being able to be neutralized totally or partially by metals such as Zn, etc.) or even by carboxylic acid anhydrides such as maleic anhydride. A functionalized polyolefin is for example a PE / EPR blend, the weight ratio of which may vary within wide limits, for example between 40 / 60 and 90 / 10, said blend being co-grafted with a anhydride, in particular maleic anhydride, according to a grafting rate for example of 0.01 to 5% by weight.

[0257] The functionalized polyolefin (Bl) can be chosen from the following (co)polymers, grafted with maleic anhydride or glycidyl methacrylate, in which the grafting rate is for example from 0.01 to 5% by weight:

[0258] - PE, PP, copolymers of ethylene with propylene, butene, hexene, or octene containing for example from 35 to 80% by weight of ethylene;

[0259] - ethylene / alpha-olefin copolymers such as ethylene / propylene, EPRs (short for ethylene-propylene-rubber) and ethylene / propylene / diene (EPDM).

[0260] - styrene / ethylene-butene / styrene (SEBS) block copolymers, styrene / butadiene / styrene (SBS), styrene / isoprene / styrene (SIS), styrene / ethylene-propylene / styrene (SEPS).

[0261] - ethylene and vinyl acetate (EVA) copolymers, containing up to 40% in vinyl acetate weight;

[0262] - ethylene and alkyl (meth)acrylate copolymers, containing up to 40% in weight of alkyl (meth)acrylate;

[0263] - ethylene vinyl acetate (EVA) and alkyl (meth)acrylate copolymers, containing up to 40% by weight of comonomers.

[0264] The functionalized polyolefin (Bl) can also be chosen from ethylene / propylene copolymers with a majority of propylene grafted with maleic anhydride then condensed with mono-amine polyamide (or a polyamide oligomer) (products described in EP-A-0342066).

[0265] The functionalized polyolefin (Bl) may also be a co- or terpolymer of at least the following units: (1) ethylene, (2) alkyl (meth)acrylate or saturated carboxylic acid vinyl ester and (3) anhydride such as maleic anhydride or (meth)acrylic acid or epoxy such as glycidyl (meth)acrylate.

[0266] As examples of functionalized polyolefins of the latter type, the following copolymers may be mentioned, where ethylene preferably represents at least 60% by weight and where the ter monomer (the function) represents, for example, from 0.1 to 10% by weight of the copolymer:

[0267] - ethylene / alkyl (meth)acrylate / (meth)acrylic acid copolymers or maleic anhydride or glycidyl methacrylate;

[0268] - ethylene / vinyl acetate / maleic anhydride or methacrylate copolymers glycidyl;

[0269] - ethylene / vinyl acetate or alkyl (meth)acrylate / acid copolymers (meth)acrylic or maleic anhydride or glycidyl methacrylate.

[0270] In the preceding copolymers, the (meth)acrylic acid can be salified with Zn or Li.

[0271] The term "alkyl (meth)acrylate" in (B1) or (B2) denotes C1-C8 alkyl methacrylates and acrylates, and may be selected from methyl acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, 2-ethylhexyl acrylate, cyclohexyl acrylate, methyl methacrylate and ethyl methacrylate.

[0272] Furthermore, the aforementioned polyolefins (B 1) can also be crosslinked by any suitable process or agent (diepoxy, diacid, peroxide, etc.); the term functionalized polyolefin also includes mixtures of the aforementioned polyolefins with a difunctional reagent such as diacid, dianhydride, diepoxy, etc. capable of reacting with them or mixtures of at least two functionalized polyolefins capable of reacting with each other.

[0273] The above-mentioned copolymers, (B1) and (B2), can be copolymerized in a random or block manner and have a linear or branched structure.

[0274] The molecular weight, MFI index, and density of these polyolefins can also vary to a large extent, which will be appreciated by those skilled in the art. MFI, short for Melt Flow Index, is the melt flow index. It is measured according to ASTM 1238.

[0275] Advantageously, the non-functionalized polyolefins (B2) are chosen from homopolymers or copolymers of polypropylene and any homopolymer of ethylene or copolymer of ethylene and a comonomer of higher alpha olefin type such as butene, hexene, octene or 4-methyl 1-pentene. Examples that may be mentioned are PP, high density PE, medium density PE, linear low density PE, low density PE, very low density PE. These polyethylenes are known to those skilled in the art as being produced according to a “radical” process, according to a “Ziegler” type catalysis or, more recently, according to a so-called “metallocene” catalysis.

[0276] Advantageously, the functionalized polyolefins (B1) are chosen from any polymer comprising alpha olefinic units and units carrying polar reactive functions such as epoxy, carboxylic acid or carboxylic acid anhydride functions. Examples of such polymers that may be mentioned are terpolymers of ethylene, alkyl acrylate and maleic anhydride or glycidyl methacrylate such as the Applicant's Lotader® or polyolefins grafted with maleic anhydride such as the Applicant's Orevac® as well as terpolymers of ethylene, alkyl acrylate and (meth)acrylic acid. Mention may also be made of homopolymers or copolymers of polypropylene grafted with a carboxylic acid anhydride and then condensed with polyamides or monoamine oligomers of polyamide. Regarding additives

[0277] The additives optionally used in the compositions of the invention are the conventional additives used in polyamides well known to those skilled in the art and are notably described in EP 2098580.

[0278] For example, they are chosen from a catalyst, an antioxidant, a heat stabilizer, a UV absorber, a light stabilizer, a lubricant, an inorganic filler, a flame retardant, a nucleating agent and a colorant, reinforcing fibers, a wax and mixtures thereof.

[0279] The term "catalyst" means a polycondensation catalyst such as a mineral or organic acid.

[0280] Advantageously, the proportion by weight of catalyst is from approximately 50 ppm to approximately 5000 ppm, in particular from approximately 100 to approximately 3000 ppm relative to the total weight of the composition.

[0281] Advantageously, the catalyst is chosen from phosphoric acid (H3PO4), phosphorous acid (H3PO3), hypophosphorous acid (H3PO2), or a mixture thereof.

[0282] For example, the stabilizer may be a UV stabilizer, an organic stabilizer or more generally a combination of organic stabilizers, such as a phenol-type antioxidant (for example of the type of irganox® 245 or 1098 or 1010 from the company Ciba-BASF), a phosphite-type antioxidant (for example irgafos® 126 and irgafos® 168 from the company Ciba-BASF) and possibly other stabilizers such as a HALS, which means Hindered Amine Light Stabilizer or hindered amine light stabilizer (for example Tinuvin® 770 from the company Ciba-BASF), an anti-UV (for example Tinuvin® 312 from the company Ciba) or a phosphorus-based stabilizer. It is also possible to use amine-type antioxidants such as Naugard® 445 from Crompton or polyfunctional stabilizers such as Nylostab® S-EED from Clariant.

[0283] This stabilizer may also be a mineral stabilizer, such as a copper-based stabilizer. Examples of such mineral stabilizers include copper halides and acetates. Alternatively, other metals such as silver may be considered, but these are known to be less effective. These copper-based compounds are typically combined with alkali metal halides, particularly potassium.

[0284] Regarding the plasticizer

[0285] The plasticizers are, for example, the plasticizers are chosen from benzene sulfonamide derivatives, such as n-butyl benzene sulfonamide (BBSA); ethyl toluene sulfonamide or N-cyclohexyl toluene sulfonamide; hydroxybenzoic acid esters, such as ethyl-2-hexyl parahydroxybenzoate and decyl-2-hexyl parahydroxybenzoate; tetrahydrofurfuryl alcohol esters or ethers, such as oligoethyleneoxytetrahydrofurfuryl alcohol; and citric acid esters or hydroxymalonic acid, such as oligoethyleneoxy malonate.

[0286] It would not be outside the scope of the invention to use a mixture of plasticizers.

[0287] The additives when present in the composition are advantageously present from 1 to 20% by weight, in particular from 5 to 15% by weight, in particular from 5 to 12% by weight. Regarding antistatic charges

[0288] The antistatic fillers are for example chosen from carbon black, graphite, carbon fibers, carbon nanotubes, in particular carbon black and carbon nanotubes. Regarding the structure

[0289] All embodiments of layer (1) described above in the paragraph "regarding layer (1)" can be used for the structure detailed in this part.

[0290] In one embodiment, said layer (1) is located between a layer (2) and a layer (2').

[0291] Advantageously, said layer (2') is the layer in contact with the transported fluid.

[0292] Advantageously, said layer (2') is as defined for layer (2), and preferably layers (2) and (2') are identical.

[0293] In one embodiment, layers (2) and (2') are different, only layer 2' can contain anti-static charges.

[0294] In this latter embodiment, said layer (2') is as defined for layer (2) meaning that the compositions of layer (2) and layer (2') may be identical or different.

[0295] When they are different, they may differ by the polyamide or the proportion of polyamide or by one of the other constituents of the composition.

[0296] Advantageously, the composition of said layer (2) comprises a PAU, a PA12 or a PA612 and the recycled material comes from a single-layer tube and / or a tank consisting of a composition comprising only a PAU, in particular the composition of the layer (1) consists of at most 99.8% recycled material.

[0297] Advantageously, the composition of said layer (2) comprises a PAU, a PA12 or a PA612, the recycled material comes from a single-layer tube and / or a tank consisting of a composition comprising only a PAU, in particular the composition of the layer (1) consists of at most 99.8% recycled material and the composition of said layer (2') comprises a PAU, a PA12 or a PA612.

[0298] Advantageously, the composition of said layer (2) comprises a PAU, a PA12 or a PA612 and from 3 to 45% by weight of at least one impact modifier, in particular from 5 to 20% by weight of at least one impact modifier and the recycled material comes from a single-layer tube and / or a tank consisting of a composition comprising only a PAU, in particular the composition of layer (1) consists of at most 99.8% recycled material.

[0299] Advantageously, the composition of said layer (2) comprises a PAU, a PA12 or a PA612 and from 3 to 45% by weight of at least one impact modifier, in particular from 5 to 20% by weight of at least one impact modifier and the recycled material comes from a single-layer tube and / or a tank consisting of a composition comprising only a PAU, in particular the composition of the layer (1) consists of at most 99.8% recycled material and the composition of said layer (2') comprises a PAU, a PA12 or a PA612 and from 3 to 45% by weight of at least one impact modifier, in particular from 5 to 20% by weight of at least one impact modifier.

[0300] Advantageously, the compositions of layer (2) and layer (2') are identical and therefore layers (2) and (2') are obviously identical, that is to say that both the polyamide and the other constituents of the composition are identical in nature and proportion and that the thickness of the two layers (2) and (2') is identical. Layer (2') is then a layer (2).

[0301] In a first variant of the multi-layer tubular structure (MLT), it is made up of three layers (2) / / (1) / / (2'),

[0302] Advantageously, this is made up of three layers (2) / / (1) / / (2).

[0303] In one embodiment, at least one binder layer (3) is present, said layer (3) being located between layer (2) and layer (1) and / or between layer (1) and layer (2').

[0304] In a second variant of the multi-layer tubular structure (MLT), this is made up of four layers (2) / / binder (3) / / (l) / / (2'), in particular (2) / / binder (3) / / (1) / / (2).

[0305] In a third variant of the multi-layer tubular structure (MLT), this consists of four layers (2) / / (1) / / binder (3) / / (2'), in particular (2) / / (1) / / binder (3) / / (2).

[0306] In a fourth variant of the multi-layer tubular structure (MLT), this consists of five layers (2) / / binder (3) / / (1) / / binder (3) / / (2'), in particular (2) / / binder (3) / / (1) / / binder (3) / / (2).

[0307] In this fourth variant, the two layers of binder (3) may be identical or different, in particular they are identical.

[0308] In another embodiment, at least one layer of EVOH is present, said layer (3) being located between layer (1) and layer (2').

[0309] The multi-layer tubular structure (MLT) is then made up of four layers

[0310] (2) / / (1) / / EVOH H (2'), in particular (2) / / (1) / / EVOH / / (2).

[0311] In one embodiment, said layer (1) represents at least 10%, in particular at least 30%, in particular at least 50% of the total thickness of said multi-layer tubular structure (MLT).

[0312] Advantageously, said layer (1) represents at least 60%, in particular at least 70% of the total thickness of said multilayer tubular structure (MLT).

[0313] In one embodiment of one of the four variants of the multilayer tubular structure (MLT) or of the four-layer structure with EVOH, said composition of said layer (1) is free of polyamides denoted A and B and said composition of said layer (2) comprises polyamides chosen from those denoted E, F and a mixture thereof.

[0314] In another embodiment of one of the four variants of the multilayer tubular structure (MLT) or of the four-layer structure with EVOH, said composition of said layer (1) comprises polyamides chosen from those noted A, B and a mixture thereof, and said composition of said layer (2) is free of polyamides noted E and F.

[0315] In yet another embodiment of one of the four variants of the multilayer tubular structure (MLT) or of the four-layer structure with EVOH, said composition of said layer (1) comprises polyamides chosen from those denoted A, B and a mixture thereof, and said composition of said layer (2) comprises polyamides chosen from those denoted E, F and a mixture thereof.

[0316] In yet another embodiment of one of the four variants of the multilayer tubular structure (MLT) or of the four-layer structure with EVOH, said composition of said layer (1) is free of polyamides noted A and B and said composition of said layer (2) is free of polyamides noted E and F.

[0317] Advantageously, in these last four embodiments, the layer (1) comes from a single-layer recycled tube or a single-layer recycled tank or a mixture of the two.

[0318] Advantageously, in these last four embodiments, the layer (1) comes from a single-layer recycled tube or a single-layer recycled tank or a mixture of the two and only said composition of said layer (1) comprises at least one impact modifier.

[0319] Advantageously, in these last four embodiments, the layer (1) comes from a single-layer recycled tube or from a single-layer recycled tank or from a mixture of the two and said composition of said layer (1) as well as said compositions of the layer (2) and of the layer (2') comprise at least one impact modifier.

[0320] Advantageously, in these last four embodiments, the layer (1) comes from a multi-layer recycled tube or a multi-layer recycled tank or a mixture of both.

[0321] Advantageously, in these last four embodiments, the layer (1) comes from a multi-layer recycled tube or from a multi-layer recycled tank or from a mixture of the two and only said composition of said layer (1) comprises at least one impact modifier.

[0322] Advantageously, in these last four embodiments, the layer (1) comes from a single-layer recycled tube or from a multi-layer recycled tank or from a mixture of the two.

[0323] Advantageously, in these last four embodiments, the layer (1) comes from a multi-layer recycled tube or from a single-layer recycled tank or from a mixture of the two.

[0324] Advantageously, in these last four embodiments, the layer (1) comes from a recycled multi-layer tube and said composition of said layer (1) as well as said compositions of the layer (2) and of the layer (2') comprise at least one impact modifier.

[0325] In one embodiment, said multi-layer tubular (MLT) is intended for the transport of fluids chosen from a fuel such as gasoline, in particular alcoholic gasoline, bio-gasoline or diesel, in particular bio-diesel. As regards the binder

[0326] The binder is notably described in patents EP1452307 and EPI 162061, EP1216826, EP0428833 and EP3299165.

[0327] It is implied that layers (2) and (1) or (1) and (2') adhere to each other. The binder layer is intended to be inserted between two layers which do not adhere or adhere with difficulty to each other.

[0328] The binder may be, for example, but not limited to, a composition based on 50% copolyamide 6 / 12 (70 / 30 ratio by mass) of Mn 16000, and 50% copolyamide 6 / 12 (30 / 70 ratio by mass) of Mn 16000, a composition based on PP (polypropylene) grafted with maleic anhydride, known under the name Admer QF551A from the company Mitsui, a composition based on PA610 (of Mn 30000, and as defined elsewhere) and 36% PA6 (of Mn 28000) and 1.2% organic stabilizers (consisting of 0.8% Lowinox 44B25 phenol from the company Great Lakes, 0.2% phosphite Irgafos 168 from Ciba, 0.2% anti-UV Tinuvin 312 from Ciba), a composition based on PA612 (of Mn 29000, and as defined elsewhere) and 36% PA6 (of Mn 28000, and as defined elsewhere) and 1.2% organic stabilizers (consisting of 0.8% phenol Lowinox 44B25 from Great Lakes, 0.2% phosphite Irgafos 168 from Ciba, 0.2% of anti-UV Tinuvin 312 from the company Ciba), a composition based on PA610 (Mn 30000, and . as defined elsewhere) and 36% PA12 (of Mn 35000, and as defined elsewhere) and 1.2% organic stabilizers (consisting of 0.8% Lowinox 44B25 phenol from Great Lakes, 0.2% Irgafos 168 phosphite from Ciba, 0.2% Tinuvin 312 UV stabilizer from Ciba), a composition based on 40% PA6 (of Mn 28000, and as defined elsewhere), 40% PA12 (of Mn 35000, and as defined elsewhere) and 20% Exxelor VA1801 functionalized EPR (Exxon company) and 1.2% organic stabilizers (consisting of 0.8% Lowinox phenol 44B25 from Great Lakes, 0.2% phosphite Irgafos 168 from Ciba, 0.2% anti-UV Tinuvin 312 from Ciba) or a composition based on 40% PA6.10 (of Mn 30000, and as defined elsewhere), 40% PA6 (of Mn 28000, and as defined elsewhere) and 20% impact modifier type ethylene / ethyl acrylate / anhydride in mass ratio 68.5 / 30 / 1.5 (MFI 6 at 190°C under 2.16 kg), and 1.2% organic stabilizers (consisting of 0.8% Lowinox 44B25 phenol from Great Lakes, 0.2% Irgafos 168 phosphite from Ciba, 0.2% Tinuvin 312 UV stabilizer from Ciba).

[0329] According to another aspect, the present invention relates to a method for preparing a tubular structure as defined above, characterized in that it comprises the extrusion of at least one layer (1) consisting of at least 50% recycled material as defined above, after taking used pipes from a motor vehicle, in an extruder optionally provided with a degassing zone.

[0330] All embodiments of layer (1) described above in the paragraph “regarding layer (1)” can be used for the method detailed in this part.

[0331] In one embodiment, the used pipes are crushed into granules after collection.

[0332] In another embodiment, the fluid residues were extracted completely or partially from the used pipes before or after crushing.

[0333] In yet another embodiment, the extraction is carried out by means of washing or ventilation.

[0334] Advantageously, the washing is carried out using a solvent, in particular methanol.

[0335] Advantageously, the ventilation is carried out by means of an inerted oven.

[0336] In one embodiment, the extraction is carried out after grinding by means of a degassing zone in said extruder.

[0337] Advantageously, the used pipes before or after crushing are cleaned to remove any residual oligomers possibly present in the used pipes.

[0338] In one embodiment, said method comprises the following steps:

[0339] 1) sampling a used single-layer and / or multi-layer tube and / or a tank used on a motor vehicle,

[0340] 2) optionally cleaning of the oligomers present,

[0341] 3) optionally extraction of fluid residues,

[0342] 4) crushing of said tubes and / or said reservoir,

[0343] 5) extraction of fluid residues if this has not been carried out in step 3),

[0344] 6) extrusion in the form of a single-layer or multi-layer tubular structure of the of said tubes and / or said tank crushed.

[0345] According to another aspect, the present invention relates to the use of a used single-layer and / or multi-layer tube and / or tank having initially transported or contained motor vehicle fluids, as defined above, for the preparation of a single-layer and / or multi-layer tubular structure intended for the transport of motor vehicle fluids, in particular air, oil, water, a urea solution, a glycol-based coolant, or a fuel such as gasoline, in particular alcoholic gasoline, bio-gasoline or diesel, in particular bio-diesel, or hydrogen as defined above, said single-layer and / or multi-layer tube and / or said used tank(s) having been ground into granules and the fluid residues present in said tube and / or tank having been extracted totally or partially,before or after crushing said tube and / or tank and said tubular structure having during the first storage of gasoline, in particular alcoholic gasoline, less than 0.3 g / m2 of insoluble extract.

[0346] All embodiments of layer (1) described above in the paragraph "regarding layer (1)" can be used for the use detailed in this part.

[0347] Advantageously, said single-layer and / or multi-layer tube and / or said used tank(s) is / are ground into granules, excluding grinding followed by recom-pounding with or without reformulation. Brief description of the drawings

[0348] [Fig-1] presents the Fourier Transform Infrared (FTIR) analysis in attenuated total reflectance (ATR) mode of a crushed PA 11 PL gasoline line ELV (solid gray line), and compared to a PA 11 PL gasoline line based on 100% virgin material (solid black line). EXAMPLES Compositions of the invention Single-layer tubes of the invention:

[0349] The tubes are 8*1mm in size

[0350] Preparation of monolayer structures (tubes):

[0351] Single-layer structures are made by extrusion. An in-line is used Maillefer extrusion machine.

[0352] This line includes a single-screw extrusion extruder equipped with a screw with a screw profile adapted to polyamides. In addition, the extrusion line includes:

[0353] a die-punch assembly, located at the end of the extrusion head; the internal diameter of the die and the external diameter of the punch are chosen according to the structure to be produced and the materials which compose it, as well as the dimensions of the tube and the line speed;

[0354] a vacuum tank with an adjustable depression level. In this tank circulates water maintained at 20°C in general, a gauge is inserted in the front of this tank allowing the tube to be shaped in its final dimensions. The diameter of the gauge is adapted to the dimensions of the tube to be produced, typically from 8.1 to 10 mm for a tube with an external diameter of 8 mm and a thickness of 1 mm;

[0355] a cooling tank in which water is maintained at around 20°C, allowing the tube to be cooled along the route from the head to the drawing bench;

[0356] a diameter meter;

[0357] a drawing bench.

[0358] Before the tests, in order to ensure the best tube properties and good extrusion quality, it is checked that the extruded materials have a residual moisture content before extrusion of less than 0.08%. Otherwise, an additional step of drying the material is carried out before the tests, generally in a vacuum dryer, for 1 night at 80°C.

[0359] The tubes, which meet the characteristics described in the present patent application, were taken, after stabilization of the extrusion parameters, the dimensions of the tubes targeted no longer changing over time. The diameter is controlled by a laser diameter meter installed at the end of the line.

[0360] The line speed is typically 20m / min. It generally varies between 5 and 100m / min.

[0361] The screw speed of the extruder depends on the thickness and diameter of the tube as is known to those skilled in the art.

[0362] Generally speaking, the temperatures of the extruders and the tools (head and connector) must be adjusted so as to be sufficiently higher than the melting temperature of the compositions in question, so that they remain in the molten state, thus preventing them from solidifying and blocking the machine.

[0363] The single-layer tubes produced by extrusion above were then evaluated on several criteria:

[0364] Aging (Ageing): This refers to durability, in other words, it refers to the resistance of the tube to oxidative aging in hot air. The tube is aged in air at 150°C, then it is shocked with a shock according to DIN 73378, this shock being carried out at -40°C, the half-life (in hours) is indicated, which corresponds to the time after which 50% of the tubes tested break. A qualitative comment accompanies this value.

[0365] We note a durability that can be described as "very good", which corresponds to >= 200h of half-life.

[0366] We note a durability (resistance to thermo-oxidative aging) that can be described as "good", which corresponds to >= 100h of half-life (and <200h)

[0367] We note a durability (resistance to thermo-oxidative aging) that can be described as "acceptable", which corresponds to >= 50h of half-life (and <100h)

[0368] We note a durability (resistance to thermo-oxidative aging) which can be described as "poor", which corresponds to <50h

[0369] In the case where a half-life figure is given to show nuances, this figure is rounded by 25h increments, to take into account significant figures, linked to the precision of the evaluation.

[0370] Use as is: geometry, mechanical behavior, pollution status suitable for mounting on a new vehicle.

[0371] +: use as is is possible.

[0372] - : use as is is impossible

[0373] Oligomers (insoluble extractables): this test consists of a tube filled with alcoholic essence type FAM B at 60°C, for 96 hours, then emptied and filtered into a beaker. The filter and the residue are dried until a constant mass is obtained, the latter having to be less than or equal to 3g / m2 (internal surface of the tube).

[0374] [Tables 1] Example Structure (mixture weight %) distribution of layer thickness (in % of total thickness) Life 11. Use as is Oligomers (insoluble extractables) (g / m2) CEI Single-layer virgin gasoline line + + >0.3 CE2 Single-layer gasoline line from ELVs - - <0.3 CE3 PA11NX2 / / PA11PL gasoline line crushed ELV + PA11PL tank crushed ELV (50 / 50) / / PA11NX2 15 / 70 / 15% + + <0.3 CE4 Three-layer virgin gasoline line + + >0.3 CE5 Three-layer gasoline line from ELVs - - <0.3 EH Single-layer PA 11 PL gasoline line crushed ELV + PA11 PL tank crushed ELV + PA 11 PL (35 / 35 / 30)% +- + <0.3 EI2 Single-layer PA11PL gasoline line Crushed ELV + PA11PL (50 / 50)% + + <0.3 EI3 PA11NX2 / / Three-layer gasoline line from Crushed ELV (ex 8) / / PA11NX2 15 / 70 / 15% + + <0.3 EI4 PA11NX2 / / Three-layer gasoline line from Crushed ELV + PA610PL (50 / 50) / / PA11NX2 15 / 70 / 15% + + <0.3

[0375] CEI to CE5: counter examples

[0376] EU to EI4: Examples of the invention

[0377] The following compositions were compounded on a Coperion / Wemer 40mm twin-screw extruder, 70kgh, 300rpm, 270°C setpoint, with a degassing of -100mmHg.

[0378] “PA11PL” is a virgin PA 11 containing 7% BBSA and 1% stabilizer.

[0379] “PA 11NX2” is a virgin PA 11 containing 10% PA 610, 5% impact modifier EPR functionalized with maleic anhydride and 1% stabilizer.

[0380] “PA610PL” is a virgin PA610 containing 7% BBSA and 1% stabilizer.

[0381] The following compositions are ground tubes and tanks collected on ELV.

[0382] “PA 11 PL gasoline line VHU crushed” are gasoline line chips collected from ELVs.

[0383] “PA11 PL crushed VHU tank” are fuel tank chips collected on ELVs Multilayer tubes of the invention:

[0384] The layers are described from the outside to the inside, followed by their respective thicknesses indicated in the form of %; the tubes are of dimension 8 * 1mm

[0385] Preparation of multilayer structures (tubes):

[0386] The multilayer tubes are produced by coextrusion. A Maillefer industrial multilayer extrusion line is used, equipped with 5 extruders, connected to a multilayer extrusion head with spiral mandrels.

[0387] The screws used are single-screw extrusion screws with screw profiles adapted to polyamides. In addition to the 5 extruders and the multi-layer extrusion head, the extrusion line includes:

[0388] a die-punch assembly, located at the end of the coextrusion head; the internal diameter of the die and the external diameter of the punch are chosen according to the structure to be produced and the materials which compose it, as well as the dimensions of the tube and the line speed;

[0389] a vacuum tank with an adjustable depression level. In this tank circulates water maintained at 20°C in general, in which a gauge is immersed to conform the tube to its final dimensions. The diameter of the gauge is adapted to the dimensions of the tube to be produced, typically from 8.5 to 10 mm for a tube with an external diameter of 8 mm and a thickness of 1 mm;

[0390] a succession of cooling tanks in which water is maintained at around 20°C, allowing the tube to be cooled along the route from the head to the drawing bench;

[0391] a diameter meter;

[0392] a drawing bench.

[0393] The 5-extruder configuration is used to produce tubes ranging from 2 layers to 5 layers (and also single-layer tubes). In the case of structures with fewer than 5 layers, several extruders are then fed with the same material.

[0394] Before testing, in order to ensure the best tube properties and good extrusion quality, it is checked that the extruded materials have a residual moisture content before extrusion of less than 0.08%. Otherwise, an additional step of drying the material is carried out before testing, generally in a vacuum dryer, for 1 night at 80°C.

[0395] The tubes, which meet the characteristics described in the present patent application, were taken, after stabilization of the extrusion parameters, the dimensions of the tubes targeted no longer changing over time. The diameter is controlled by a laser diameter meter installed at the end of the line.

[0396] The line speed is typically 20m / min. It generally varies between 5 and 100m / min.

[0397] The screw speed of the extruders depends on the layer thickness and the screw diameter as is known to those skilled in the art.

[0398] Generally speaking, the temperatures of the extruders and the tools (head and connector) must be adjusted so as to be sufficiently higher than the melting temperature of the compositions in question, so that they remain in the molten state, thus preventing them from solidifying and blocking the machine.

[0399] “Virgin single-layer gasoline line” is a virgin single-layer gasoline line of dimension 8*1mm made of PA11 PL

[0400] “Single-layer gasoline line from ELVs” is a single-layer gasoline line from dimension 8*1mm composed of PA11 PL collected from an ELV

[0401] “Virgin three-layer gasoline line” is a virgin three-layer gasoline line of dimension 8* 1mm inside>PA1 1NX2 / / PA610 PL / / PA1 lNX2 <extérieur ayant les répartitions d’épaisseur suivante : 15% / 70% / 15%

[0402] “Three-layer gasoline line from ELV” is a three-layer gasoline line from ELV of dimension 8* 1mm interior>PA1 1NX2 / / PA610 PL / / PA1 lNX2

Claims

Claims

1. Composition comprising: (a) 30% to 99.8% by weight, in particular 50 to 99.8% by weight of recycled material from a used single-layer and / or multi-layer tube and / or tank having initially transported or contained motor vehicle fluids, in particular air, oil, water, a urea solution, a glycol-based coolant, or a fuel such as gasoline, in particular alcoholic gasoline, bio-gasoline or diesel, in particular bio-diesel, or hydrogen, said tube and / or said tank being made of a composition which predominantly comprises at least one polyamide, said single-layer and / or multi-layer tube and / or said used tank(s) having been ground into granules and the fluid residues present in said tube and / or tank having been totally or partially extracted, before or after grinding of said tube and / or reservoir, (b) up to 70%,in particular up to 50% of a semi-crystalline aliphatic polyamide, (c) up to 45% by weight of at least one impact modifier, in particular from 1 to 45% by weight of at least one impact modifier, in particular from 2 to 45% by weight of at least one impact modifier, (d) up to 20% by weight of at least one plasticizer, (e) up to 0.2% of an additive, said polyamide of said used tube and / or tank having functions resulting from oxidation reactions chosen from imide functions, carboxylic acids, alcohols and their mixtures, in a molar ratio relative to the amide functions higher than that of the same polyamide constituting an unused tube and / or tank which has never before transported or contained fluids for a motor vehicle.,

2. Composition according to claim 1, characterized in that said molar ratio of the functions resulting from oxidation reactions is from 1 / 10000 to 1 / 20.

3. Composition according to claim 1 or 2, characterized in that said molar ratio of the imide functions is from 1 / 1000 to 1 / 20, in particular from 1 / 500 to 1 / 20, in particular from 1 / 200 to 1 / 50.

4. Composition according to one of claims 1 to 3, characterized in that said molar ratio of the carboxylic acid functions is from 1 / 5000 to 1 / 20, in particular from 1 / 3000 to 1 / 50 very advantageously. from 1 / 500 to 1 / 25.

5. Composition according to one of claims 1 to 4, characterized in that said molar ratio of the alcohol functions is from 1 / 1000 to 1 / 20 and advantageously from 1 / 1000 to 1 / 25, very advantageously from 1 / 200 to 1 / 50.

6. Single- or multi-layer tubular (MLT) structure for transporting fluids for a motor vehicle, in particular air, oil, water, a urea solution, a glycol-based coolant, or a fuel such as gasoline, in particular alcohol-based gasoline, bio-gasoline or diesel, in particular bio-diesel, or hydrogen, comprising at least one layer (1) consisting of a composition as defined in one of claims 1 to 5.

7. Single-layer or multi-layer tubular structure (MLT) according to claim 6, characterized in that it has, during the first storage of gasoline, in particular alcoholic gasoline, a maximum of 0.3 g / m2 of insoluble extract, advantageously a maximum of 0.2 g / m2.

8. Single-layer or multi-layer tubular structure (MLT) according to claim 6 or 7, characterized in that the extraction of said fluid residues is carried out by means of washing or ventilation.

9. Single-layer or multi-layer tubular structure (MLT) according to one of claims 6 to 8, characterized in that the structure is multi-layer and comprises at least one layer (2).

10. Multilayer tubular structure (MLT) according to claim 9, characterized in that said layer (2) is made of a composition comprising predominantly at least one semi-crystalline aliphatic polyamide and optionally at least one impact modifier, and when the layer (2) is made of a composition comprising predominantly at least one semi-crystalline aliphatic polyamide which is PA 12 and / or PA610 and / or PA612 and / or PA 1010, then said composition comprises said impact modifier, and said layer (2) is made of at least 90% non-recycled material.

11. Multi-layer tubular structure (MLT) according to one of claims 9 to 10, characterized in that it comprises at least one layer (2') consisting of a composition comprising predominantly at least one semi-crystalline or semi-aromatic aliphatic polyamide, said layer (2') being made up of at least 90% non-recycled material.

12. A multi-layer tubular (MLT) structure according to claim 11, ca- characterized in that said layer (2') is made up of a composition comprising predominantly at least one semi-aromatic polyamide.

13. Multilayer tubular structure (MLT) according to claim 11, characterized in that said layer (2') is made of a composition mainly comprising at least one polyolefin.

14. Multi-layer tubular structure (MLT) according to one of claims 11 to 13, characterized in that said layer (1) is located between a layer (2) and a layer (2').

15. Multi-layer tubular structure (MLT) according to one of claims 11 or 14, characterized in that the layer (2') is the layer in contact with the fluid.

16. Multi-layer tubular structure (MLT) according to one of claims 11 to 15, characterized in that the layer (2') is as defined for the layer (2), and preferably the layers (2) and (2') are identical.

17. Multi-layer tubular structure (MLT) according to one of claims 11 to 16, characterized in that at least one binder layer (3) is present, said layer (3) being located between the layer (2) and the layer (1) and / or between the layer (1) and the layer (2').

18. Single-layer or multi-layer tubular structure (MLT) according to one of claims 6 to 17, characterized in that said layer (1) represents at least 10%, in particular at least 30%, in particular at least 50% of the total thickness of said single-layer or multi-layer tubular structure (MLT).

19. Single-layer or multi-layer tubular structure (MLT) according to one of claims 6 to 18, characterized in that said layer (1) consists of a composition comprising: at least 50% by weight, in particular from 50% to 99.8% by weight, of at least one semi-crystalline aliphatic polyamide denoted C having an average number of carbon atoms per nitrogen atom denoted Cc of from 6 to 18, advantageously from 8 to 12; from 0 to 25% by weight of at least one semi-crystalline aliphatic polyamide denoted B and having an average number of carbon atoms per nitrogen atom denoted CB = Ce - 1, preferably CB = Ce - 2; from 0 to 25% by weight of a semi-crystalline aliphatic polyamide noted A having an average number of carbon atoms per nitrogen atom noted CA = CB - 1, preferably CA = CB - 2; from 0 to 45% by weight of at least one impact modifier, in particular from 3 to 45% by weight of at least one impact modifier, from 0 to 20% by weight of at least one plasticizer, from 0 to 0.2% by weight of at least one additive, the sum of the constituents being equal to 100%.

20. Single-layer or multi-layer tubular structure (MLT) according to claim 19, characterized in that said composition of the layer (1) is free of plasticizer and / or impact modifier.

21. Single-layer or multi-layer tubular structure (MLT) according to claim 19, characterized in that said composition of the layer (1) comprises at least one compound chosen from a plasticizer, an impact modifier and an additive.

22. Single-layer or multi-layer tubular structure (MLT) according to one of claims 6 to 21, characterized in that the fluid transported by said single-layer and / or multi-layer tube or stored in said reservoir is the same as that of said single-layer or multi-layer tubular structure (MLT).

23. Single-layer or multi-layer tubular structure (MLT) according to one of claims 6 to 21, characterized in that the fluid transported by said single-layer and / or multi-layer tube or stored in said reservoir is different from that of said multi-layer tubular structure.

24. Multilayer tubular structure (MLT) according to one of claims 9 to 23, characterized in that the layer (2) consists of a composition comprising: at least 50% by weight, in particular from 50% to 99.8% by weight, in particular from 50% to 95% by weight, of at least one semi-crystalline aliphatic polyamide denoted D having an average number of carbon atoms per nitrogen atom denoted CD of from 6 to 18, advantageously from 9 to 15 from 0 to 25% by weight of at least one semi-crystalline aliphatic polyamide denoted E and having an average number of carbon atoms per nitrogen atom denoted CE = CD - 1, preferably CE = CD - 2; from 0 to 25% by weight of a semi-crystalline aliphatic polyamide noted F having an average number of carbon atoms per nitrogen atom noted CE = CE - 1, preferably CE = CE - 2;from 3 to 45% by weight of at least one impact modifier, in particular from 5 to 20% by weight of at least one impact modifier, from 0 to 20% by weight of at least one plasticizer, from 0 to 0.2% by weight of at least one additive, from 0 to 35% of at least one antistatic filler; the sum of the constituents being equal to 100%.

25. Multilayer tubular structure (MLT) according to claim 24, characterized in that said composition of said layer (1) is free of polyamides noted A and B and said composition of said layer (2) comprises polyamides chosen from those noted E, F and a mixture thereof.

26. Multilayer tubular structure (MLT) according to claim 24, characterized in that said composition of said layer (1) comprises polyamides chosen from those noted A, B and a mixture thereof, and said composition of said layer (2) is free of polyamides noted E and F.

27. Single-layer or multi-layer tubular structure (MLT) according to one of claims 6 to 26, characterized in that the layer (1) comes from a single-layer recycled tube.

28. Single-layer or multi-layer tubular structure (MLT) according to one of claims 6 to 26, characterized in that the layer (1) comes from a recycled multi-layer tube.

29. Multi-layer tubular structure (MLT) according to one of claims 9 to 22, characterized in that the MLT consists of three layers of the following structure: (2) / / (1) / / (2).

30. Process for preparing a tubular structure as defined in one of claims 6 to 29, characterized in that it comprises the extrusion of a composition as defined in one of claims 1 to 5 to constitute the layer (1), after taking used pipes from a motor vehicle, in an extruder optionally equipped with a degassing zone.

31. Method according to claim 30, characterized in that the used pipes are crushed into granules after collection.

32. A method according to claim 30 or 31, characterized in that the fluid residues have been extracted from the used pipes before or after crushing.

33. A method according to claim 32, characterized in that the extraction is carried out by means of washing or ventilation.

34. Method according to claim 33, characterized in that the washing is carried out using a solvent, in particular methanol.

35. Method according to claim 33, characterized in that the ventilation is carried out by means of an inerted oven.

36. Method according to claim 32, characterized in that the extraction is carried out after grinding by means of a degassing zone in said extruder.

37. Method according to one of claims 30 to 36, characterized in that the used pipes before or after crushing are cleaned to remove any oligomers possibly present in the used pipes.

38. Use of a used single-layer and / or multi-layer tube and / or tank having initially transported or contained motor vehicle fluids, as defined in claim 1, for the preparation of a single-layer tubular structure intended for the transport of motor vehicle fluids, in particular air, oil, water, a urea solution, a glycol-based coolant, or a fuel such as gasoline, in particular alcoholic gasoline, bio-gasoline or diesel, in particular bio-diesel, or hydrogen as defined in claim 1, said single-layer and / or multi-layer tube and / or said used tank(s) having been ground into granules and the fluid residues present in said tube and / or tank having been extracted totally or partially, before or after grinding said tube and / or tank and said said tubular structure having during the first storage of gasoline,in particular alcoholic essence, less than 0.3 g / m2 of insoluble extract.,