Hydroconversion in a driven bed of a heavy hydrocarbon feed comprising a mixture of said feed with a catalyst precursor containing an organic additive
The integration of a molybdenum-based catalyst precursor with organic additives in the hydrocarbon feedstock forms colloidal or molecular catalysts in situ, addressing fouling and enhancing conversion efficiency in hydrocarbon reactors by reducing coke precursors and sediments.
Patent Information
- Application Number
- FR2021007378
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-07-08
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2041-07-08
AI Technical Summary
Entrained bed hydroconversion processes face fouling issues in upstream installations due to the accumulation of metals and carbon on the walls, limiting the usability of equipment and not adequately addressing coke precursor and sediment formation, which can occur even with existing catalysts.
A process involving a heavy hydrocarbon feed mixed with a catalyst precursor formulation containing molybdenum and an organic additive with carboxylic acid, ester, or acid anhydride functions, forming a colloidal or molecular catalyst in situ, which reduces fouling by promoting hydrogenation of free radicals and minimizing coke precursor and sediment formation.
The process effectively reduces fouling in upstream installations, enhances conversion rates, and increases the throughput of heavy hydrocarbon feedstocks by inhibiting coke precursor and sediment formation, leading to more efficient and prolonged operation of hydroconversion reactors.
Smart Images

Figure 00000048_0000 
Figure 00000048_0001 
Figure 00000048_0002
Abstract
Description
Title of the invention: Entrained bed hydroconversion of a heavy hydrocarbon feedstock comprising a mixture of said feedstock with a catalyst precursor containing an organic additive. Technical field
[0001] The present invention relates to a process for the conversion of heavy hydrocarbon feedstocks in the presence of hydrogen, a colloidal or molecular catalyst, and an organic additive.
[0002] In particular, the present invention involves a process for the hydroconversion of heavy hydrocarbon feedstocks containing a fraction of at least 50% by weight having a boiling point of at least 300°C, and in particular heavy hydrocarbon feedstocks comprising a significant amount of asphaltenes and / or fractions with a boiling point above 500°C, such as crude oils or heavy hydrocarbon fractions resulting from the atmospheric and / or vacuum distillation of a crude oil, to give higher quality, lower boiling point materials.
[0003] The process specifically comprises mixing said heavy hydrocarbon feedstock with a catalyst precursor formulation comprising an organic additive, before being sent to one or more entrained bed reactors, in order to enable the upgrading of this low quality feedstock while minimizing fouling of the installations by inhibiting the formation of coke precursors and sediments before hydroconversion in the entrained bed reactor(s). Prior art
[0004] Converting heavy hydrocarbon feedstocks into useful end products requires extensive processing, including reducing the boiling point of the heavy hydrocarbon feedstock, increasing the hydrogen-to-carbon ratio, and removing impurities such as metals, sulfur, nitrogen, and high-carbon compounds.
[0005] Catalytic hydroconversion is commonly used for hydro feedstocks heavy carbonaceous and is generally implemented using three-phase reactors in which the feedstock is brought into contact with hydrogen and a catalyst. In the reactor, the catalyst can be used in the form of a fixed bed, a moving bed, an ebullated bed or an entrained bed, as described for example in Chapter 18 "Catalytic Hydrotreatment and Hydroconversion: Fixed Bed, Moving Bed, Ebullated Bed and Entrained Bed" from the book "Heavy Crude Oils: From Geology to Upgrading, An OverView", published by Technip in 2011. In the case of an ebullated bed or an entrained bed, the reactor includes an upward flow of liquid and gas.
[0006] The choice of technology generally depends on the nature of the load to be treated and in particular its metal content, its tolerance to impurities and the conversion sought.
[0007] Entrained bed hydroconversion processes use entrained bed technologies also called slurry technologies.
[0008] In such processes, a dispersed catalyst or catalyst precursor is injected on a continuous basis into the heavy hydrocarbon feedstock in the entrained bed reactor, promoting the hydrogenation of radicals formed by thermal cracking reactions, and limiting coke formation.
[0009] The catalyst provides the catalytic activity but also a surface for the deposition of metals and asphaltenes from the feedstock.
[0010] The very small catalyst, dispersed in the feedstock, is carried out of the reactor with the effluents, since the catalyst and the heavy hydrocarbon feedstock behave as a homogeneous phase.
[0011] Entrained bed hydroconversion processes are known to generally aim to completely convert the heavy hydrocarbon feedstock into lighter fractions, using very severe operating conditions (temperature, hydrogen partial pressure, residence time).
[0012] The theoretical advantages of entrained bed processes lie in much better hydrogenation, especially of heavier products, due to better accessibility of active sites, resulting in higher conversion, improved product quality and higher product stability.
[0013] In addition, due to the lower catalyst residence time, catalyst deactivation is greatly reduced.
[0014] Regarding product stability, it is known that during operation of an entrained bed reactor for upgrading a heavy hydrocarbon feedstock, the heavy feedstock is heated to a temperature at which high boiling fractions of the heavy hydrocarbon feedstock typically having a high molecular weight and / or a low hydrogen / carbon ratio, an example of which is a family of complex compounds grouped together under the name "asphaltenes", tend to undergo thermal cracking to form free radicals of reduced chain length. These free radicals may react with other free radicals, or with other molecules, to produce coke precursors and sediments. A ca The entrained bed flow through the reactor reacts with free radicals in these areas, forming stable molecules of reduced molecular weight and boiling point, and thus helps to control and reduce the formation of sediment and coke precursors. Since coke and sediment formation is the main cause of fouling in hydroconversion plants, such an entrained bed process helps prevent fouling of downstream plants, such as separation tanks, distillation columns, heat exchangers, etc.
[0015] Entrained catalysts for the hydroconversion of a heavy hydrocarbon feedstock, and in particular colloidal or molecular catalysts formed by the use of soluble catalytic precursors, are well known in the art. It is in particular known that certain metallic compounds, such as organo-soluble compounds (e.g. molybdenum naphthenate or molybdenum octoate as cited in US4244839, US2005 / 0241991, US2014 / 0027344) or water-soluble compounds (e.g. phosphomolybdic acid cited in patents US3231488, US4637870 and US4637871; ammonium heptamolybdate cited in patent US6043182, salts of a heteropolyanion as cited in FR3074699), can be used as dispersed catalyst precursors and form catalysts. In the case of water-soluble compounds, the dispersed catalyst precursor is generally mixed with the feedstock to form an emulsion.The dissolution of the dispersed catalyst precursor (generally molybdenum), optionally activated by cobalt or nickel in an acidic medium (in the presence of H3PO4) or in a basic medium (in the presence of NH4 OH), has been the subject of numerous studies and patents.
[0016] Patent document US8431016 describes a hydroconversion process for heavy hydrocarbon feedstocks using a colloidal or molecular catalyst in an entrained bed hydrocracking reactor. The addition of a dispersed organically soluble catalyst precursor, which is pre-diluted in vacuum gas oil (VGO), is carried out in an intimate mixing step with the feedstock for the preparation of a conditioned feedstock prior to its introduction into the entrained bed reactor. The catalyst precursor, typically molybdenum 2-ethylhexanoate, forms a colloidal or molecular catalyst (e.g. dispersed molybdenum sulfide) when heated, by reaction with H2S from the hydrodesulfurization of the feedstock.
[0017] Such a process inhibits the formation of coke precursors and sediments that could otherwise foul the ebullated bed reactor and downstream facilities, while providing conversion of the asphaltene fraction at essentially the same rate as the overall residue conversion rate, even at a very high overall residue conversion rate, unlike hydroconversion processes using conventional supported catalysts.
[0018] In addition to fouling due to coke precursors and sediments which can appear in the entrained bed reactor and in downstream installations, the inventors observed that fouling can also appear in upstream installations, as soon as the heavy hydrocarbon feedstock containing the catalyst precursor is heated before its introduction into the hydroconversion reactor.
[0019] Such fouling in installations upstream of the hydroconversion reactor, in particular in the installation for heating the heavy hydrocarbon feedstock mixed with the catalyst precursor of the particulate molecular or colloidal catalyst, appears to be mainly linked to the accumulation of metals and carbon on the wall, and may limit the operability of the installations.
[0020] Thus, although entrained catalyst in known entrained bed processes, such as described in US8431016, is known to reduce fouling due to coke precursors and sediments in the hydroconversion reactor and in downstream facilities, fouling observed in downstream facilities containing the heavy hydrocarbon feedstock mixed with the catalyst precursor, such as in a preheater, is another operational problem not solved so far. Furthermore, it has been observed that fouling due to coke precursors and sediments can still occur in downstream facilities in some cases, showing that the performance of adding an entrained catalyst can be further improved. Objectives and summary of the invention
[0021] In the context described above, an objective of the present invention is to provide an entrained bed hydroconversion process using a colloidal or molecular catalyst formed by the use of a soluble catalytic precursor, solving the fouling problem, in particular in installations upstream of the hydroconversion reactor, in particular in a device for preheating the feedstock before its conversion in the entrained bed hydroconversion reactor(s).
[0022] More generally, the present invention aims to provide an entrained bed hydroconversion process for the upgrading of heavy hydrocarbon feedstocks allowing one or more of the following effects: reduced fouling of equipment, more efficient treatment of asphaltene molecules, reduced formation of coke precursors and sediments, increased conversion rate, possibility for the reactor to treat a wider range of lower quality hydrocarbon feedstocks, elimination of catalyst-free zones in downstream processing facilities, longer operation between maintenance shutdowns, and increased throughput of heavy hydrocarbon feedstock, and increased production rate of converted products. A reduction in the frequency of shutdown and start-up of process equipment implies a reduction in pressure and temperature cycles of the process facilities, and this significantly increases the safety of the process and extends the useful life of expensive installations.
[0023] Thus, in order to achieve at least one of the objectives set out above, among others, the present invention provides, according to a first aspect, a process for the hydroconversion of a heavy hydrocarbon feedstock containing a fraction of at least 50% by weight having a boiling point of at least 300°C, and containing metals and asphaltenes, comprising the following steps: (a) preparing a conditioned heavy hydrocarbon feedstock, by mixing said heavy hydrocarbon feedstock with a catalyst precursor formulation such that a colloidal or molecular catalyst is formed when it reacts with sulfur, said catalyst precursor formulation comprising: - a catalyst precursor composition comprising molybdenum, and - an organic chemical compound comprising at least one carboxylic acid function and / or at least one ester function and / or one acid anhydride function, and - a molar ratio between said organic chemical compound and molybdenum in said catalyst precursor formulation being between 0.1:1 and 20:1; (b) heating said conditioned heavy hydrocarbon feedstock of step (a) in at least one preheating device; (c) introducing said heated conditioned heavy hydrocarbon feedstock of step (b) into at least one entrained bed reactor and operating said entrained bed reactor in the presence of hydrogen and under hydroconversion conditions to produce an upgraded material; and wherein the colloidal or molecular catalyst is formed in situ in the heavy hydrocarbon feedstock conditioned in step (b) and / or in step (c).
[0024] According to one or more embodiments, step (a) comprises simultaneously mixing said organic chemical compound with said catalyst precursor composition, preferably previously diluted with a hydrocarbon oil diluent, and with said heavy hydrocarbon feedstock, preferably at a temperature below a temperature at which a substantial portion of the catalyst precursor composition begins to thermally decompose, such as at a temperature between room temperature and 300°C, and for a period of time from 1 second to 30 minutes.
[0025] According to one or more embodiments, step (a) comprises (a1) pre-mixing said organic chemical compound with said catalyst precursor composition to produce said catalyst precursor formulation and (a2) mixing said catalyst precursor formulation with said heavy hydrocarbon feedstock.
[0026] According to one or more embodiments, in step (a1) said catalyst precursor composition is mixed at a temperature lower than a temperature at wherein a substantial portion of the catalyst precursor composition begins to thermally decompose, preferably at a temperature between room temperature and 300°C.
[0027] According to one or more embodiments, a hydrocarbon oil diluent is used to form the catalyst precursor formulation, said hydrocarbon oil diluent preferably being selected from the group consisting of vacuum gas oil, decanter oil or recycle oil, light gas oil, vacuum residues, deasphalted oils and resins.
[0028] According to one or more embodiments, the organic chemical compound is selected from the group consisting of ethylhexanoic acid, naphthenic acid, caprylic acid, adipic acid, pimelic acid, suberic acid, azelaic acid, and sebacic acid, ethyl octanoate, ethyl 2-ethylhexanoate, 2-ethylhexyl 2-ethylhexanoate, benzyl 2-ethylhexanoate, diethyl adipate, dimethyl adipate, bis(2-ethylhexyl) adipate, dimethyl pimelate, dimethyl suberate, monomethyl suberate, hexanoic anhydride, caprylic anhydride, and mixtures thereof.
[0029] According to one or more embodiments, the organic chemical compound comprises 2-ethylhexanoic acid, and is preferably 2-ethylhexanoic acid.
[0030] According to one or more embodiments, the organic chemical compound comprises ethyl octanoate or 2-ethylhexyl 2-ethylhexanoate, and is preferably ethyl octanoate or 2-ethylhexyl 2-ethylhexanoate.
[0031] According to one or more embodiments, the catalyst precursor composition comprises an oil-soluble organometallic compound or complex selected from the group consisting of molybdenum 2-ethylhexanoate, molybdenum naphthanate, molybdenum hexacarbonyl, and is preferably molybdenum 2-ethylhexanoate.
[0032] According to one or more embodiments, the molar ratio between said organic chemical compound and molybdenum of said catalyst precursor formulation is between 0.75:1 and 7:1, and preferably between 1:1 and 5:1.
[0033] According to one or more embodiments, the colloidal or molecular catalyst comprises molybdenum disulfide.
[0034] According to one or more embodiments, step (b) comprises heating to a temperature between 280°C and 450°C, more preferably between 300°C and 400°C, and even more preferably in a range of 320°C to 365°C.
[0035] According to one or more embodiments, the heavy hydrocarbon feedstock comprises at least one feedstock from the following: crude oil, bitumen from oil sands, bottoms from atmospheric distillation columns, bottoms from vacuum distillation columns, residues, visbreaker bottoms, coal tar, heavy oil from oil shale, liquefied coal, heavy bio-oils, and heavy oils including plastic waste and / or plastic pyrolysis oil.
[0036] According to one or more embodiments, the heavy hydrocarbon feedstock has sulfur at a content greater than 0.5% by weight, a Conradson carbon residue of at least 0.5% by weight, C7 asphaltenes at a content greater than 1% by weight, transition and / or post-transition metals and / or metalloids at a content greater than 2 ppm by weight, and alkali and / or alkaline earth metals at a content greater than 2 ppm by weight.
[0037] According to one or more embodiments, step (c) is carried out under an absolute pressure of between 2 MPa and 38 MPa, at a temperature of between 300°C and 550°C, at an hourly volumetric flow rate WH relative to the volume of each entrained bed reactor of between 0.05 h 1 and 10 h 1 and under a quantity of hydrogen mixed with the feed entering the entrained bed reactor of between 50 and 5,000 Nm3 / m3 of feed.
[0038] According to one or more embodiments, the molybdenum concentration in the conditioned heavy hydrocarbon feedstock is preferably in a range of 10 ppm to 10,000 ppm by weight of the heavy hydrocarbon feedstock.
[0039] Other subjects and advantages of the invention will become apparent from the following description of specific exemplary embodiments of the invention, given by way of non-limiting examples, the description being made with reference to the appended figures described below. List of figures
[0040] [Fig.l]
[0041] [Fig.l] is a functional diagram illustrating the principle of the entrained bed hydroconversion process according to the invention.
[0042] [Fig.2]
[0043] [Fig.2] is a flow diagram illustrating an entrained bed hydroconversion process according to one embodiment of the invention, wherein the catalyst precursor formulation is obtained by pre-mixing the organic additive with the catalyst precursor composition.
[0044] [Fig.3]
[0045] [Fig. 3] is a flow diagram illustrating an example of an entrained bed hydroconversion as illustrated in [Fig. 2], wherein the catalyst precursor formulation is obtained by mixing the catalyst precursor composition with a diluent containing an organic additive.
[0046] [Fig.4]
[0047] [Fig. 4] is a flow diagram illustrating another example of an entrained bed hydroconversion as illustrated in [Fig. 2], wherein the catalyst precursor formulation is obtained by mixing a catalyst precursor composition containing an additive with a hydrocarbon oil diluent.
[0048] [Fig.5]
[0049] [Fig.5] is a flow diagram illustrating another example of an entrained bed hydroconversion as illustrated in [Fig.2], wherein the catalyst precursor formulation is obtained by mixing a dilute catalyst precursor composition with an organic additive.
[0050] [Fig.6]
[0051] [Fig.6] is a functional diagram illustrating an example of an entrained bed hydroconversion process and system according to the invention.
[0052] [Fig.7]
[0053] [Fig. 7] is a graph showing the fouling tendency of examples of conditioned hydrocarbon feedstocks as prepared in the entrained bed hydroconversion process according to the invention and according to the prior art. Description of the embodiments
[0054] The object of the invention is to provide entrained bed hydroconversion processes and systems for improving the quality of a heavy hydrocarbon feedstock.
[0055] Such processes and systems for the hydroconversion of heavy hydrocarbon feedstocks employ an entrained catalyst that is a molecular or colloidal catalyst dispersed in the heavy hydrocarbon feedstock. They also employ an organic additive added in a catalyst precursor formulation that is mixed with the heavy hydrocarbon feedstock, prior to using the entrained catalyst in one or more entrained bed reactors, each of which comprises a liquid phase comprising the heavy hydrocarbon feedstock, the colloidal or molecular catalyst dispersed therein and the organic additive, and a gas phase comprising hydrogen gas.
[0056] The entrained bed hydroconversion processes and systems of the invention reduce fouling of plants, and in particular fouling in plants upstream of the hydroconversion reactor(s), in particular in plants for preheating the feedstock before its conversion in the entrained bed hydroconversion reactor(s), and can efficiently treat asphaltenes, reduce or eliminate the formation of coke precursors and sediments, increase the conversion rate, in particular by allowing the hydroconversion to be carried out at high temperatures, and eliminate catalyst-free zones that would otherwise exist in downstream treatment plants. Terminology
[0057] Some definitions are given below, although more details on the objects defined below are given later in the description.
[0058] The term "hydroconversion" refers to a process whose primary purpose is to reduce the boiling point range of a heavy hydrocarbon feedstock and in which a substantial portion of the feedstock is converted to products with lower boiling point ranges than the original feedstock. Hydroconversion generally involves the fragmentation of larger hydrocarbon molecules into smaller molecular fragments having a smaller number of carbon atoms and a higher hydrogen to carbon ratio. The reactions carried out during hydroconversion reduce the size of hydrocarbon molecules, primarily by cleavage of carbon-carbon bonds, in the presence of hydrogen to saturate the cleaved bonds and aromatic rings.The mechanism by which hydroconversion occurs typically involves the formation of hydrocarbon free radicals during fragmentation primarily by thermal cracking, followed by capping of the free radical ends or fragments with hydrogen in the presence of active catalyst sites. Of course, during a hydroconversion process, other reactions typically associated with "hydrotreating" may occur such as the removal of sulfur and nitrogen from the feedstock as well as olefin saturation.
[0059] The term "hydrocracking" is often used as a synonym for "hydroconversion" according to English terminology, although "hydrocracking" rather refers to a process similar to hydroconversion but in which the cracking of hydrocarbon molecules is mainly catalytic cracking, i.e. cracking occurring in the presence of a hydrocracking catalyst having a phase responsible for the cracking activity, for example acid sites such as those contained in a clay or zeolites.According to French terminology, for example, hydrocracking, which can be translated as "hydrocraquage", generally refers to the latter definition (catalytic cracking), and its use is, for example, rather reserved for the case of vacuum distillates as oil feedstocks to be converted, whereas the French term "hydroconversion" is generally reserved for the conversion of heavy hydrocarbon feedstocks such as atmospheric and vacuum residues (but not only).
[0060] The term "hydrotreating" refers to a milder operation whose primary purpose is to remove impurities such as sulfur, nitrogen, oxygen, halides, and trace metals from the feedstock and to saturate olefins and / or stabilize hydrocarbon free radicals by reacting them with hydrogen rather than allowing them to react with themselves. The primary purpose is not to change the boiling point range of the feedstock. Hydroprocessing is most commonly carried out using a fixed-bed reactor, although other hydroprocessing reactors can also be used for hydroprocessing, for example, an ebullated-bed hydroprocessing reactor.
[0061] The term "hydroprocessing" refers generally to both "hydroconversion" / "hydrocracking" and "hydrotreatment" processes.
[0062] The term "hydroconversion reactor" refers to any vessel in which the hydroconversion of a feedstock is the primary purpose, e.g., cracking the feedstock (i.e., reducing the boiling point range), in the presence of hydrogen and a hydroconversion catalyst. Hydroconversion reactors typically include an inlet through which a heavy hydrocarbon feedstock and hydrogen may be introduced and an outlet from which an upgraded material may be withdrawn. Specifically, hydroconversion reactors are also characterized by possessing sufficient thermal energy to cause the fragmentation of larger hydrocarbon molecules into smaller molecules by thermal decomposition.Examples of hydroconversion reactors, and in particular hydrocracking reactors, include, but are not limited to, entrained bed reactors, also known as slurry reactors (three-phase reactors - liquid, gas, solid, in which the solid and liquid phases can behave as a homogeneous phase), ebullated bed reactors (three-phase fluidized reactors), moving bed reactors (three-phase reactors with downward movement of the solid catalyst and upward or downward flow of liquid and gas), and fixed bed reactors (three-phase reactors with downward flow of liquid feedstock over a fixed bed of supported catalyst with hydrogen typically flowing simultaneously with the liquid, but possibly countercurrently in some cases).
[0063] The terms "hybrid bed" and "hybrid bubbling bed" and "hybrid entrained-bubbling bed" for a hydroconversion reactor refer to an ebullating bed hydroconversion reactor comprising an entrained catalyst in addition to a porous supported catalyst maintained in the ebullating bed reactor. Similarly, for a hydroconversion process, these terms thus refer to a process comprising a hybrid operation of an ebullating bed and an entrained bed in at least one hydroconversion reactor. The hybrid bed is a mixed bed of two types of catalysts of necessarily different particle size and / or density, one type of catalyst - the "porous supported catalyst" - being maintained in the reactor and the other type of catalyst - the "entrained catalyst", also commonly called "slurry catalyst" - being entrained out of the reactor with the effluents (upgraded feedstock).In the present invention, the entrained catalyst. is a colloidal catalyst or a molecular catalyst, as defined below.
[0064] The terms "entrained bed reactor", "entrained phase reactor" and "slurry reactor" generally refer to two-phase, i.e. liquid and gas, or three-phase, i.e. liquid, gas, and solid, entrained bed reactors for the hydroconversion, in particular hydrocracking, of heavy hydrocarbon feedstock.
[0065] In the present invention, this refers to an entrained bed reactor which at least comprises a colloidal or molecular catalyst as defined below.
[0066] In the present invention, the entrained bed reactor contains an entrained catalyst, at least one colloidal catalyst or molecular catalyst as defined below, which is the only hydroconversion catalyst in the entrained bed reactor (no porous supported catalyst maintained in the reactor during operation as in an ebullated or hybrid bed reactor).
[0067] An example of an entrained bed reactor is disclosed in document US6960325 B.
[0068] The liquid phase typically comprises a hydrocarbon feedstock that contains a colloidal catalyst or a molecular-sized catalyst (solid particles).
[0069] The solid catalyst particles, of colloidal or molecular size, together with the liquid hydrocarbon feedstock, can behave as a continuous liquid phase due to the catalyst particle size (colloidal or molecular).
[0070] A solid catalyst in the form of a solid particle of micron size or larger may also be employed as well as liquid and gas.
[0071] The terms "colloidal catalyst" and "colloidally dispersed catalyst" refer to catalyst particles having a particle size that is colloidal, e.g., less than 1 μm in size (diameter), preferably less than 500 nm in size, more preferably less than 250 nm in size, or less than 100 nm in size, or less than 50 nm in size, or less than 25 nm in size, or less than 10 nm in size, or less than 5 nm in size. The term "colloidal catalyst" includes, but is not limited to, molecular or molecularly dispersed catalyst compounds.
[0072] The terms "molecular catalysts" and "molecularly dispersed catalysts" refer to catalyst compounds that are essentially "dissolved" or completely dissociated from other catalyst compounds or molecules in a heavy hydrocarbon feedstock, non-volatile liquid fraction, bottoms fraction, residue, or other feedstock or product in which the catalyst may be found. They also refer to very small catalyst particles or sheets that contain only a few catalyst molecules joined together (e.g., 15 molecules or less).
[0073] The terms "porous supported catalyst", "solid supported catalyst", and "supported catalyst" refer to catalysts that are typically used in conventional ebullated bed and fixed bed hydroconversion systems, including including catalysts designed primarily for hydrocracking or hydrodemetallization and catalysts designed primarily for hydroprocessing. Such catalysts typically comprise (i) a catalyst support having a large surface area and numerous interconnected channels or pores and (ii) fine particles of an active catalyst such as cobalt, nickel, tungsten, and / or molybdenum sulfides dispersed within the pores. Supported catalysts are commonly produced as cylindrical extrudates (“pellets”) or spherical solids, although other shapes are possible.
[0074] The terms "upgrade," "upgrade," and "upgraded," when used to describe a feedstock that is subjected to or has been subjected to hydroconversion, or a resulting material or product, refer to any of the following characteristics: a reduction in the molecular weight of the feedstock, a reduction in the boiling point range of the feedstock, a reduction in the concentration of asphaltenes, a reduction in the concentration of hydrocarbon free radicals, a reduction in the Conradson carbon residue, an increase in the H / C atomic ratio of the feedstock, and a reduction in the amount of impurities, such as sulfur, nitrogen, oxygen, and halides.
[0075] The terms "conditioned feedstock" and "conditioned heavy hydrocarbon feedstock" refer to the heavy hydrocarbon feedstock to be processed in at least one entrained bed hydroconversion reactor, in which feedstock a catalyst precursor formulation comprising a catalyst precursor composition and an organic additive have been combined and mixed sufficiently such that upon formation of the catalyst, such as by reaction with sulfur, the catalyst will comprise a colloidal or molecular catalyst dispersed in the feedstock.
[0076] The term "active mixing device" refers to a mixing device comprising a moving part, e.g. a stirring rod or propeller or a turbine rotor, for actively mixing the components.
[0077] In the following, the term "includes" is synonymous with (means the same as) "comprises" and "contains", and is inclusive or open and does not exclude other unspecified elements. It will be understood that the term "includes" includes the exclusive and closed term "consisting".
[0078] The terms "between ... and..." and "in the range of ... to ..." and "in a range of ... to ..." mean that the values at the boundaries of the interval are included in the range of values described, unless otherwise stated.
[0079] In the detailed description below, numerous specific details are set forth to convey a deeper understanding of the method of the system according to the invention. However, it will be apparent to those skilled in the art that the method and system may be employed without all of these specific details. In other cases, Features that are well known have not been described in detail, so as not to complicate the description unnecessarily.
[0080] [Fig.l] is a functional diagram schematically illustrating the principle of the entrained bed hydroconversion process 100 according to the invention. It differs from a conventional entrained bed process, as described for example in US8431016 in particular, in that the catalyst precursor formulation comprises an organic additive when mixed with the hydrocarbon feedstock, said catalyst precursor formulation also comprising a catalyst precursor composition comprising molybdenum and having a specific molar ratio of the organic additive to the molybdenum.
[0081] The terms "organic chemical compound" and "organic additive" are used interchangeably in the present description to designate the organic chemical compound comprising at least one carboxylic acid function and / or at least one ester function and / or one acid anhydride function added in the catalyst precursor formulation mixed with the heavy hydrocarbon feedstock in step (a), and described in detail below. The organic additive is a compound in addition to any possible organic compound initially present in the catalyst precursor composition.
[0082] According to the invention, a heavy hydrocarbon feedstock 101 containing a fraction of at least 50% by weight having a boiling point of at least 300°C, and containing metals and asphaltenes, is treated in a hydroconversion process 100 comprising the following steps: (a) preparing a conditioned heavy hydrocarbon feedstock 103 by mixing said heavy hydrocarbon feedstock 101 with a catalyst precursor formulation 104 such that a colloidal or molecular catalyst is formed when it reacts with sulfur, said catalyst precursor formulation 104 comprising: - a catalyst precursor composition 105 comprising molybdenum, and - an organic chemical compound 102 comprising at least one carboxylic acid function and / or at least one ester function and / or at least one acid anhydride function, and - a molar ratio between said organic chemical compound 102 and molybdenum of between 0.1:1 and 20:1; (b) heating the conditioned heavy hydrocarbon feedstock 103 from step (a) in at least one preheating device; (c) introducing the heated conditioned heavy hydrocarbon feedstock 106 from step (b) into at least one entrained bed reactor and operating said entrained bed reactor in the presence of hydrogen and under hydroconversion conditions to produce a recovered material 107.
[0083] In the hydroconversion process according to the invention, the colloidal or molecular catalyst is formed in situ in the heavy hydrocarbon feedstock conditioned in step (b) and / or in step (c).
[0084] The recovered material 107 may be further processed in an optional step (d).
[0085] Each step, flow and material involved are now detailed below.
[0086] Some of the reference numerals mentioned below refer to [Fig. 6], which schematically illustrates an example of an entrained bed hydroconversion system 600 according to the invention, said system being described in detail later in the description, after the description of the general method. Heavy hydrocarbon feedstock
[0087] The term "heavy hydrocarbon feedstock" refers to crude oils, tar sands bitumen, barrel bottoms and residues remaining from refinery processes (e.g., visbreaker bottoms), and any other low-grade feedstock that contains a substantial amount of high-boiling hydrocarbon fraction and / or includes a significant amount of asphaltenes that may deactivate a solid supported catalyst and / or cause or result in the formation of coke precursors and sediment.
[0088] The heavy hydrocarbon feedstock 101 may thus comprise at least one of the following feedstocks: crude oil, bituminous sands bitumen, atmospheric distillation column bottoms, vacuum distillation column bottoms, residues, visbreaker bottoms, coal tar, heavy oil from oil shale, liquefied coal, heavy bio-oils, and heavy oils comprising plastic waste and / or plastic pyrolysis oil.
[0089] Plastic pyrolysis oils are oils obtained by the pyrolysis of plastics, preferably plastic waste, and can be obtained by catalytic, thermal pyrolysis treatment or can be prepared by hydropyrolysis (pyrolysis in the presence of a catalyst and hydrogen).
[0090] In particular, the treated heavy hydrocarbon feedstock contains hydrocarbon fractions of which at least 50% by weight, preferably at least 80% by weight, have a boiling point of at least 300°C, preferably at least 350°C or at least 375°C.
[0091] These are crude oils or heavy hydrocarbon fractions resulting from the atmospheric and / or vacuum distillation of a crude oil. They may also be atmospheric and / or vacuum residues, and in particular atmospheric and / or vacuum residues resulting from hydrotreatment, hydrocracking and / or hydroconversion. They may also be vacuum distillates, fractions from a catalytic cracking unit such as fluidized bed catalytic cracking (FCC), a coking or visbreaking unit.
[0092] Preferably, these are vacuum residues. Generally, these residues are fractions in which at least 80% by weight have a boiling temperature of at least 450°C or more, and most often at least 500°C or 540°C.
[0093] Aromatic fractions extracted from a lubricant production unit, deasphalted oils (raffinates from a deasphalting unit), and asphalt (residues from a deasphalting unit) are also suitable as feedstock.
[0094] The feedstock may also be a residual fraction from direct liquefaction of coal (vacuum distillate and / or atmospheric and / or vacuum residue from e.g. an H-Coal process, registered trademark), from pyrolysis of coal or oil shale residue, or from a residual fraction from direct liquefaction of lignocellulosic biomass alone or mixed with coal and / or a petroleum fraction (hereinafter referred to as "heavy bio-oils").
[0095] Examples of heavy hydrocarbon feedstocks include, but are not limited to, Lloydminster crude oil, Cold Lake bitumen, Athabasca bitumen, Urals crude oil, Arabian Heavy crude oil, Arabian Light crude oil, atmospheric distillation column bottoms, vacuum distillation column bottoms, residue (or "tailings"), residue pitch, vacuum residue, solvent deasphalting pitch, and non-volatile liquid fractions that remain after subjecting a crude oil, bitumen from oil sands, liquefied coal, oil shale, or coal tar feedstocks to distillation, hot separation, and the like and that contain high boiling fractions and / or asphaltenes.
[0096] All these fillers can be used alone or in a mixture.
[0097] The heavy hydrocarbon feedstocks treated above in the process and system according to the invention contain metals and asphaltenes, in particular C7 asphaltenes, and other impurities such as sulfur and nitrogen.
[0098] The term "asphaltene" refers to the fraction of a heavy hydrocarbon feedstock that is typically insoluble in paraffinic solvents such as propane, butane, pentane, hexane, and heptane and comprises sheets of fused cyclic compounds held together by heteroatoms such as sulfur, nitrogen, oxygen, and metals. Asphaltenes broadly comprise a wide range of complex compounds having from 80 to 160,000 carbon atoms. Asphaltenes are operationally defined as "C7 asphaltenes," i.e., compounds insoluble in heptane according to ASTM D 6560 (also corresponding to NF T60-115), and any asphaltene content refers to C7 asphaltenes in this specification. The as- C7 phaltenes are compounds known to inhibit the conversion of residual fractions, both by their ability to form heavy hydrocarbon residues, commonly called coke, and by their tendency to produce sediments that greatly limit the operability of hydrotreating and hydroconversion units.
[0099] The heavy hydrocarbon feedstock 101 may typically have sulfur at a content greater than 0.5% by weight, a Conradson carbon residue of at least 3% by weight, C7 asphaltenes at a content greater than 1% by weight, transition and / or post-transition metals and / or metalloids at a content greater than 2 ppm by weight, and alkali and / or alkaline earth metals at a content greater than 2 ppm by weight.
[0100] These types of fillers are in fact generally rich in impurities such as metals, in particular transition metals (eg Ni, V) and / or post-transition metals, and / or metalloids, for which a content may be greater than 2 ppm by weight, or greater than 20 ppm by weight, and even greater than 100 ppm by weight, and also in alkali metals (eg Na) and / or alkaline earth metals whose content may be greater than 2 ppm by weight, even greater than 5 ppm by weight, and even greater than 7 ppm or 10 ppm by weight.
[0101] The sulfur content is in fact generally greater than 0.5% by weight, and even greater than 1% by weight, or even greater than 2% by weight.
[0102] The C7 asphaltene content can in fact be at least 1% by weight, and even greater than 3% by weight.
[0103] The Conradson carbon residue is in fact generally greater than 3% by weight, and even at least 5% by weight. The Conradson carbon residue is defined by the ASTM D 482 standard and represents the quantity of carbon residue produced after pyrolysis under standard temperature and pressure conditions.
[0104] These contents are expressed in % by weight of the total weight of the charge.
[0105] Step (a): preparation of conditioned heavy hydrocarbon feedstock
[0106] Step (a) comprises mixing said heavy hydrocarbon feedstock 101 with a catalyst precursor formulation 104 in a manner such that a colloidal or molecular catalyst is formed when reacted with sulfur. This mixture forms what is referred to herein as the conditioned heavy hydrocarbon feedstock 103.
[0107] The catalyst precursor formulation 104 comprises a catalyst precursor composition 105 comprising molybdenum, and an organic chemical compound 102 comprising at least one carboxylic acid function and / or at least one ester function and / or at least one acid anhydride function.
[0108] The molar ratio between said organic chemical compound 102 and molybdenum is between 0.1:1 and 20:1.
[0109] This step includes complete / intimate mixing with the precursor formulation catalyst which will lead to the formation of a colloidal or molecular catalyst dispersed in the heavy hydrocarbon feedstock.
[0110] According to one or more embodiments, a hydrocarbon oil diluent is used to form the catalyst precursor formulation 104. Preferably, said hydrocarbon oil diluent is selected from the group consisting of vacuum gas oil, decanter oil or recycle oil, light gas oil, vacuum residues, deasphalted oils, and resins, as further detailed below.
[0111] The inventors have shown that this mixing step (a) improves the bubbling-entrained bed hydroconversion process, in particular by reducing fouling of the installations, in particular upstream of the entrained bed hydroconversion reactor in the charge heating installation in step (b).
[0112] Without being bound by any theory, the presence of the organic additive during the mixing of the heavy hydrocarbon feedstock with the catalyst precursor composition, allows for better solubility of the colloidal or molecular catalyst precursor in the feedstock, avoiding or reducing fouling in particular due to deposits in the installations upstream of the entrained bed hydroconversion reactor as in the heating installation, and thus improving the dispersion of the colloidal or molecular catalyst formed in step (b) and / or in a subsequent step, thus generating increased availability of the metallic active sites, promoting the hydrogenation of free radicals which are precursors of coke and sediments, and generating a substantial reduction in fouling of the installations. The organic additive
[0113] The organic additive 102 having at least one carboxylic acid function and / or at least one ester function and / or at least one acid anhydride function preferably comprises at least 6 carbon atoms, and more preferably at least 8 carbon atoms.
[0114] Typically, the organic additive 102 is neither a catalyst precursor nor a catalyst.
[0115] In particular, the organic additive 102 does not contain any metal.
[0116] Examples of organic additive include, but are not limited to, acid 2-ethylhexanoic acid, naphthenic acid, caprylic acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, ethyl octanoate, ethyl 2-ethylhexanoate, 2-ethylhexyl 2-ethylhexanoate, benzyl 2-ethylhexanoate, diethyl adipate, dimethyl adipate, bis(2-ethylhexyl) adipate, dimethyl pimelate, dimethyl suberate, monomethyl suberate, hexanoic anhydride, caprylic anhydride. Advantageously, the organic additive is an organic chemical compound selected from the group consisting of by the list of specific compounds described above, and their mixtures.
[0117] Preferably, the organic additive is an organic chemical compound comprising at least one carboxylic acid function, and more preferably selected from the group consisting of 2-ethylhexanoic acid, naphthenic acid, caprylic acid, adipic acid, pimelic acid, suberic acid, azelaic acid, and sebacic acid.
[0118] More preferably, the organic additive comprises, or consists of, 2-ethylhexanoic acid.
[0119] The organic additive may be an organic chemical compound comprising at least one ester function and / or one acid anhydride function, and for example chosen from the group consisting of ethyl octanoate, ethyl 2-ethylhexanoate, 2-ethylhexyl 2-ethylhexanoate, benzyl 2-ethylhexanoate, diethyl adipate, dimethyl adipate, bis(2-ethylhexyl) adipate, dimethyl pimelate, dimethyl suberate, monomethyl suberate, and / or from the group consisting of hexanoic anhydride and caprylic anhydride.
[0120] More preferably, the organic additive comprising at least one ester function and / or one acid anhydride function comprises, or consists of, ethyl octanoate or 2-ethylhexyl 2-ethylhexanoate or mixtures thereof, and preferably is ethyl octanoate or 2-ethylhexyl 2-ethylhexanoate.
[0121] The organic additive is added such that the molar ratio of organic additive to molybdenum (provided by the catalyst precursor compound, e.g., molybdenum 2-ethylhexanoate) in the catalyst precursor formulation 104 is in a range of about 0.1:1 to about 20:1, preferably in a range of about 0.75:1 to about 7:1, and more preferably in a range of about 1:1 to about 5:1. The term "about" refers to an approximation of ±5%, preferably ±1%. Catalyst precursor formulation
[0122] The catalyst precursor formulation comprises a catalyst precursor composition selected from all molybdenum-containing metal catalyst precursors known to a person skilled in the art, capable of forming a colloidally or molecularly dispersed catalyst (i.e. the entrained catalyst) in the presence of hydrogen and / or H2S and / or any other sulfur source, and allowing the hydroconversion of a heavy hydrocarbon feedstock after injection into said heavy hydrocarbon feedstock.
[0123] The molybdenum-containing catalyst precursor composition is advantageously an oil-soluble catalyst precursor composition containing at least one transition metal.
[0124] The catalyst precursor composition preferably comprises a compound or oil-soluble organometallic complex.
[0125] The oil-soluble catalyst precursor composition preferably has a decomposition temperature (temperature below which the catalyst precursor composition is substantially chemically stable) in a range of 100°C to 350°C, more preferably in a range of 150°C to 300°C, and even more preferably in a range of 175°C to 250°C.
[0126] The oil-soluble organometallic compound or complex is preferably selected from the group consisting of molybdenum 2-ethylhexanoate, molybdenum naphthanate, and molybdenum hexacarbonyl.
[0127] These compounds are non-limiting examples of oil-soluble catalyst precursor compositions.
[0128] A currently preferred catalyst precursor composition is molybdenum 2-ethylhexanoate (also commonly referred to as molybdenum octoate). Typically, molybdenum 2-ethylhexanoate contains 15% by weight of molybdenum and has a decomposition temperature or decomposition temperature range sufficiently high to avoid substantial thermal decomposition when blended with a heavy hydrocarbon feedstock at a temperature below 250°C.
[0129] One skilled in the art may, in following the present invention, select a mixing temperature profile that results in mixing of a selected precursor composition without substantial thermal decomposition prior to formation of the colloidal or molecular catalyst. Incorporation of the organic additive
[0130] The mixing step (a) can be carried out in different ways detailed below, mainly depending on whether the organic additive is mixed simultaneously with the heavy hydrocarbon feedstock and the catalyst precursor composition, or is introduced sequentially, in particular by pre-mixing the catalyst precursor composition with the organic additive to form the catalyst precursor formulation before its mixing with the heavy hydrocarbon feedstock.
[0131] The mixing step (a) advantageously comprises the use of at least one conditioning mixer 610 configured to provide complete / intimate mixing between the feedstock and the catalyst precursor formulation 104 to form the conditioned heavy hydrocarbon feedstock.
[0132] First embodiment: simultaneous mixing of the hydrocarbon feedstock, d e the organic additive and catalyst precursor composition
[0133] According to a first embodiment, step (a) comprises the simultaneous mixing of the organic additive 102 with the catalyst precursor composition 105, preferably previously diluted with a hydrocarbon oil diluent, and with the heavy hydrocarbon charge 101.
[0134] According to this embodiment, the catalyst precursor formulation 104, comprising the catalyst precursor composition 105, preferably previously diluted, and the organic additive 102 is thus formed during mixing with the heavy hydrocarbon feedstock 101.
[0135] The organic additive is added so that the molar ratio of organic additive to molybdenum (provided by the catalyst precursor compound, e.g. molybdenum 2-ethylhexanoate) is in a range of about 0.1:1 to about 20:1, preferably in a range of about 0.75:1 to about 7:1, and more preferably in a range of about 1:1 to about 5:1, as mentioned above.
[0136] Such simultaneous mixing is preferably carried out at a temperature below a temperature at which a substantial portion of the catalyst precursor composition begins to thermally decompose, such as at a temperature between room temperature, eg 15°C and 300°C, more preferably between 50°C and 200°C, and even more preferably between 75°C and 175°C.
[0137] Such simultaneous mixing is carried out for a sufficient time and in a manner to disperse the catalyst precursor formulation throughout the feedstock to provide a packaged heavy hydrocarbon feedstock 103 in which the catalyst precursor composition is thoroughly / intimately mixed into the heavy hydrocarbon feedstock.
[0138] Preferably, the gauge pressure is between 0 MPa and 25 MPa, more preferably between 0.01 MPa and 5 MPa.
[0139] In order to achieve sufficient mixing of the catalyst precursor composition into the heavy hydrocarbon feedstock prior to formation of the colloidal or molecular catalyst, the simultaneous mixing of the heavy hydrocarbon feedstock 101, the organic additive 102, and the catalyst precursor composition 105, advantageously diluted with a hydrocarbon diluent, is preferably carried out for a period of time in the range of 1 second to 30 minutes, more preferably 1 second to 10 minutes, and even more preferably in a range of 2 seconds to 3 minutes. In the present description, a mixing time (or residence time for the mixture) of 1 second includes instantaneous mixing.
[0140] Although it is within the scope of the invention to directly mix the catalyst precursor composition 105 with the heavy hydrocarbon feedstock 101 and the organic additive 102, care must be taken in such cases to mix the components for a sufficient time to completely / intimately mix the catalyst precursor composition into the feedstock prior to catalyst formation. However, a long mixing time, for example 24 hours mixing, may result in some industrial operations have a prohibitive cost.
[0141] Therefore, according to the first embodiment, step (a) preferably comprises a dilution of the catalyst precursor composition 105 before simultaneous mixing with the heavy hydrocarbon feedstock 101 and the organic additive 102: a pre-dilution of the catalyst precursor composition 105 with a hydrocarbon diluent before simultaneous mixing of said diluted catalyst precursor composition with the heavy hydrocarbon feedstock and the organic additive 102 greatly facilitates the complete and intimate mixing of the catalyst precursor composition into the feedstock, particularly in the relatively short period of time required for large-scale industrial operations to be economically viable.
[0142] Such a mixture of a catalyst precursor composition, preferably the oil-soluble catalyst precursor composition, with a diluent hydrocarbon stream is for example described in document US2005 / 0241991 and recalled below.
[0143] The use of a dilute catalyst precursor composition shortens the overall mixing time by (1) reducing or eliminating solubility differences between the more polar catalyst precursor composition and the heavy hydrocarbon feedstock, (2) reducing or eliminating rheology differences between the catalyst precursor composition and the heavy hydrocarbon feedstock, and / or (3) breaking up the catalyst precursor molecules to form a solute in a hydrocarbon oil diluent that is much more readily dispersed in the heavy hydrocarbon feedstock. It is particularly advantageous to first form a dilute catalyst precursor composition in the case where the heavy hydrocarbon feedstock contains water (e.g., condensed water).
[0144] Otherwise, the greater affinity of water for the polar catalyst precursor composition may cause localized agglomeration of the catalyst precursor composition, resulting in poor dispersion and the formation of micron-sized or larger catalyst particles. The hydrocarbon oil diluent is preferably substantially free of water (i.e., contains less than 0.5 wt. % water, preferably less than 0.1 wt. % water, and more preferably less than 750 ppm wt. water) to prevent the formation of substantial amounts of micron-sized or larger catalyst particles.
[0145] Examples of suitable hydrocarbon diluents include, but are not limited to, a vacuum gas oil known as "VGO" (which typically has a boiling range of 360°C to 524°C), a decanter oil or a cycle oil (which typically has a boiling range of 360°C to 550°C), a light gas oil (which typically has a boiling range of 200°C to 360°C), vacuum residues (which typically have a boiling range of 524°C+), deasphalted oils, and resins.
[0146] The mass ratio of catalyst precursor 105 composition to hydrocarbon oil diluent is preferably in a range of 1:500 to 1:1, more preferably in a range of 1:150 to 1:2, and even more preferably in a range of 1:100 to 1:5 (eg 1:100, 1:50, 1:30, or 1:10).
[0147] Said dilution before simultaneous mixing is advantageously carried out for a period of time from 1 second to 30 minutes, preferably in a range from 1 second to 10 minutes, and even more preferably in a range from 2 seconds to 3 minutes. The actual time for this dilution depends, at least in part, on the temperature (i.e. which affects the viscosity of the fluids) and the mixing intensity implemented for the dilution.
[0148] Said dilution is also advantageously carried out at a temperature below a temperature at which a substantial part of the catalyst precursor composition begins to thermally decompose, preferably at a temperature between room temperature, e.g. 15°C, and 300°C, more preferably between room temperature and 200°C, even more preferably between 50°C and 200°C, even more preferably between 75°C and 150°C, and even more preferably between 75°C and 100°C.
[0149] It will be appreciated that the actual temperature at which the dilute catalyst precursor composition 105 is formed typically depends largely on the decomposition temperature of the specific precursor composition that is used.
[0150] The conditioning mixer 610 may comprise an active mixing device, any injection system for lines or any in-line mixer as detailed below.
[0151] The simultaneous mixing of step (a) according to the first embodiment can be carried out in a dedicated tank of an active mixing device forming the conditioning mixer 610.
[0152] Such a configuration makes it possible in particular to increase the dispersion of the colloidal or molecular catalyst formed at a later stage. The use of a dedicated tank also allows a long residence time.
[0153] Such simultaneous mixing may comprise, as a variant, the injection of said organic additive 102 and the catalyst precursor composition 105, preferably previously diluted with a hydrocarbon oil diluent, into a conduit conveying the heavy hydrocarbon feedstock 101 to the entrained bed reactor (heating plant in between). The conditioning mixer 610 thus comprises, in such a configuration, the part(s) of the conduit in which the mixing is carried out, and possibly additional systems to facilitate mixing, such as static in-line mixers or high shear in-line mixers as described later. Such a configuration allows in particular to reduce investments in installations and the required space requirement compared to mixing in a dedicated tank.
[0154] The conditioning mixer 610 used for simultaneous mixing may also include a combination of such a dedicated tank, an active mixing device, and in-line injection systems possibly including static and / or high shear in-line mixers.
[0155] Examples of mixing apparatuses that may be used to effect complete simultaneous mixing of the preferably dilute catalyst precursor composition 105 with the heavy hydrocarbon feedstock 101 and the organic additive 102 include, but are not limited to, high shear mixing such as mixing created in a pump with a propeller or turbine rotor; multiple static in-line mixers; multiple static in-line mixers in combination with high shear in-line mixers; multiple static in-line mixers in combination with high shear in-line mixers; multiple static in-line mixers in combination with high shear in-line mixers followed by recirculation pumping into the surge tank; combinations of the above apparatuses followed by one or more multi-stage centrifugal pumps.In one embodiment, continuous rather than batchwise mixing may be carried out using high-energy pumps having multiple compartments in which the preferably diluted catalyst precursor composition 105, heavy hydrocarbon feedstock 101, and organic additive 102 are stirred and mixed as part of the pumping process itself. The mixing apparatus described above may also be used for the dilution step discussed above in which the catalyst precursor composition 105 is mixed with the hydrocarbon oil diluent.
[0156] Increasing the vigor and / or shear energy of the simultaneous mixing process generally reduces the time required to achieve complete mixing.
[0157] Second embodiment: pre-mixing of the precursor composition of catalyst with organic additive
[0158] According to a second embodiment, as schematically illustrated in [Fig.2], the mixing step (a) comprises (a1) pre-mixing the organic additive compound 102 with the catalyst precursor composition 105 to produce the catalyst precursor formulation 104, and (a2) mixing said catalyst precursor formulation 104 with said heavy hydrocarbon feedstock 101.
[0159] The step (al) of pre-mixing the organic additive compound 102 with the catalyst precursor composition 105 to produce the catalyst precursor formulation 104 can be carried out ex-situ (i.e., outside the hydroconversion system).
[0160] In such a second embodiment, the conditioning mixer 610 comprises at least one first mixing apparatus for step (a1) and at least one second mixing apparatus for step (a2).
[0161] In step (a1), the organic additive is added such that the molar ratio of organic additive 102 to molybdenum (provided by the catalyst precursor composition, e.g., molybdenum 2-ethylhexanoate) in the catalyst precursor formulation 104 is in a range of about 0.1:1 to about 20:1, preferably in a range of about 0.75:1 to about 7:1, and more preferably in a range of about 1:1 to about 5:1.
[0162] In step (a1) the catalyst precursor composition 105 is mixed at a temperature below a temperature at which a substantial portion of the catalyst precursor composition begins to thermally decompose, preferably at a temperature between room temperature, e.g. 15°C and 300°C, more preferably between room temperature and 200°C, even more preferably between 50°C and 200°C, and even more preferably between 75°C and 150°C, and even more preferably between 75°C and 100°C.
[0163] Step (al)
[0164] Step (al) can itself be implemented in different ways detailed below.
[0165] Although it is within the scope of the invention to directly mix a catalyst precursor formulation consisting of the catalyst precursor composition 105 and the organic additive 102 with the heavy hydrocarbon feedstock 101 in step (a2), the method according to said second embodiment of the invention preferably comprises in step (a1) the use of a hydrocarbon oil diluent to produce the catalyst precursor formulation 104, in particular to facilitate the complete and intimate mixing of the catalyst precursor composition into the feedstock in step (a2) in the relatively short period of time required for large-scale industrial operations to be economically viable.
[0166] The use of a hydrocarbon oil diluent to produce the catalyst precursor formulation 104 shortens the mixing time in step (a2) for the reasons already mentioned above in connection with the description of the diluted catalyst precursor composition for the first embodiment (reduction or elimination of differences in solubility, rheology etc.).
[0167] Examples of suitable hydrocarbon diluents include, but are not limited to, a vacuum gas oil known as "VGO" (which typically has a boiling range of 360°C to 524°C), a decanter oil or cycle oil (which typically has a boiling range of 360°C to 550°C), and a light gas oil (which typically has a boiling range of 200°C to 360°C).
[0168] The mass ratio of catalyst precursor 105 composition to hydrocarbon oil diluent in the catalyst precursor 104 formulation is preferably in a range of 1:500 to 1:1, more preferably in a range of 1:150 to 1:2, and even more preferably in a range of 1:100 to 1:5 (eg 1:100, 1:50, 1:30, or 1:10).
[0169] According to one or more sub-embodiments, as schematically illustrated in [Fig.3], step (al) of the method 300 according to the second embodiment comprises: - (al) pre-mixing said organic additive 102 with a hydrocarbon oil diluent to form a diluent containing the additive 108'; and - (a2) mixing the diluent containing the additive 108' with said catalyst precursor composition 105 to produce said catalyst precursor formulation 104.
[0170] Step (al) is preferably carried out at a temperature between room temperature, e.g. 15°C and 300°C, preferably between room temperature and 200°C, even more preferably between 50°C and 200°C, even more preferably between 75°C and 150°C, and even more preferably between 75°C and 100°C.
[0171] The pressure for the pre-mixing stage (al) is advantageously the actual pressure of the diluent flow 108. Preferably, the gauge pressure for the pre-mixing stage (al) is between 0 MPa and 25 MPa, more preferably between 0.01 MPa and 5 MPa.
[0172] The residence time may be between 1 second and several days, preferably in a range of 1 second to 30 minutes, more preferably in a range of 1 second to 10 minutes, and even more preferably in a range of 1 second to 30 seconds.
[0173] Step (a2) is preferably carried out at a temperature below a temperature at which a substantial portion of the catalyst precursor composition 105 begins to thermally decompose, preferably at a temperature between room temperature, e.g. 15°C and 300°C, preferably between room temperature and 200°C, even more preferably between 50°C and 200°C, even more preferably between 75°C and 150°C, and even more preferably between 75°C and 100°C.
[0174] The pressure of the mixing step (a2) is advantageously the actual pressure of the diluent flow 108'.
[0175] Preferably, the gauge pressure for the pre-mixing stage (a2) is between 0 MPa and 25 MPa, more preferably between 0.01 MPa and 5 MPa.
[0176] The residence time may be between 1 second and several days, preferably in a range of 1 second to 30 minutes, more preferably in a range of 1 second to 10 minutes, and most preferably in a range of 1 second to 30 seconds.
[0177] It is understood that the actual temperature used in step (a2) typically depends on the decomposition temperature of the particular precursor composition being used.
[0178] According to one or more sub-embodiments, as schematically illustrated in [Fig.4], step (al) of the method 400 according to said second embodiment comprises: - ([31) pre-mixing said organic additive 102 with said catalyst precursor composition 105 to form a catalyst precursor composition containing additive 105'; and - 02) mixing said catalyst precursor composition containing additive 105' with a hydrocarbon oil diluent 108 to produce said catalyst precursor formulation 104.
[0179] Step (|31) is preferably carried out at a temperature below a temperature at which a substantial portion of the catalyst precursor composition 105 begins to thermally decompose, preferably at a temperature between room temperature, e.g. 15°C and 300°C, preferably between room temperature and 200°C, even more preferably between 50°C and 200°C, even more preferably between 75°C and 150°C, and even more preferably between 75°C and 100°C.
[0180] Preferably, the gauge pressure for the mixing stage ([> I ) is between 0 MPa and 25 MPa, more preferably between 0.01 MPa and 5 MPa.
[0181] The residence time may be between 1 second and several days, preferably in a range of 1 second to 30 minutes, more preferably in a range of 1 second to 10 minutes, and even more preferably in a range of 1 second to 30 seconds.
[0182] Step ([32) is preferably carried out at a temperature below a temperature at which a substantial portion of the catalyst precursor composition 105 begins to thermally decompose, preferably at a temperature temperature between room temperature, eg 15°C and 300°C, preferably between room temperature and 200°C, even more preferably between 50°C and 200°C, even more preferably between 75°C and 150°C, and even more preferably between 75°C and 100°C.
[0183] Preferably, the gauge pressure for the mixing stage ([32) is between 0 MPa and 25 MPa, more preferably between 0.01 MPa and 5 MPa.
[0184] The residence time may be between 1 second and several days, preferably in a range of 1 second to 30 minutes, more preferably in a range of 1 second to 10 minutes, and most preferably in a range of 1 second to 30 seconds.
[0185] It is understood that the actual temperature used in steps ([31) and ([32) typically depends largely on the decomposition temperature of the particular precursor composition being used.
[0186] According to one or more sub-embodiments, as schematically illustrated in [Fig.5], step (al) of the method 500 according to said second embodiment comprises: - (yl) pre-mixing said catalyst precursor composition 105 with a hydrocarbon oil diluent 108 to form a dilute catalyst precursor composition 109; and - (y2) mixing said diluted catalyst precursor composition 109 with organic additive 102 to produce said catalyst precursor formulation 104.
[0187] Step (yl) is preferably carried out at a temperature below a temperature at which a substantial portion of the catalyst precursor composition 105 begins to thermally decompose, preferably at a temperature between room temperature, e.g. 15°C and 300°C, preferably between room temperature and 200°C, even more preferably between 50°C and 200°C, even more preferably between 75°C and 150°C, and even more preferably between 75°C and 100°C.
[0188] Preferably, the gauge pressure for the mixing stage (yl) is between 0 MPa and 25 MPa, more preferably between 0.01 MPa and 5 MPa.
[0189] The residence time may be between 1 second and several days, preferably in a range of 1 second to 30 minutes, more preferably in a range of 1 second to 10 minutes, and even more preferably in a range of 1 second to 30 seconds.
[0190] Step (y2) is preferably carried out at a temperature below a temperature at which a substantial portion of the catalyst precursor composition 105 begins to thermally decompose, preferably at a temperature between room temperature, eg 15°C and 300°C, preferably between room temperature and 200°C, even more preferably between 50°C and 200°C, even more preferably between 75°C and 150°C, and even more preferably between 75°C and 100°C.
[0191] Preferably, the gauge pressure for the mixing stage (y2) is between 0 MPa and 25 MPa, more preferably between 0.01 MPa and 5 MPa.
[0192] The residence time may be between 1 second and several days, preferably in a range of 1 second to 30 minutes, more preferably in a range of 1 second to 10 minutes, and even more preferably in a range of 1 second to 30 seconds.
[0193] It is understood that the actual temperature used in steps (yl) and (y2) typically depends largely on the decomposition temperature of the particular precursor composition being used.
[0194] The different mixing sub-steps of step (a1) may be implemented using different mixing apparatus, examples of which include, but are not limited to, high shear mixing such as mixing created in a vessel with a propeller or turbine rotor; multiple static in-line mixers; multiple static in-line mixers in combination with high shear in-line mixers; multiple static in-line mixers in combination with high shear in-line mixers; multiple static in-line mixers in combination with high shear in-line mixers followed by recirculation pumping in the surge vessel; combinations of the above apparatus followed by one or more multi-stage centrifugal pumps.In one embodiment, continuous rather than batchwise mixing may be implemented using high-energy pumps having multiple compartments in which the components to be mixed are stirred and mixed as part of the pumping process itself.
[0195] For example, each of the different mixing sub-steps of step (a1) may be implemented in a dedicated tank of an active mixing device forming part of the first mixing apparatus of the conditioning mixer 610.
[0196] Such a configuration makes it possible in particular to increase the dispersion of the colloidal or molecular catalyst formed at a later stage. The use of a dedicated tank also makes it possible to achieve a high residence time.
[0197] According to another example, each of the different mixing sub-steps of step (a1) may alternatively comprise injecting the component to be mixed into a pipe carrying the other component, herein referred to as the in-pipe injection system. The second mixing apparatus of the conditioning mixer 610 thus comprises in such a configuration the part(s) of the pipe in which the mixing is carried out, and possibly additional systems to facilitate the mixing, such as for example static in-line mixers or high shear in-line mixers as described above. Such a configuration makes it possible in particular to reduce investments in installations and the required space requirement compared to mixing in a dedicated tank.
[0198] According to another example, the first mixing apparatus of the conditioning mixer 610 may comprise a combination of such a dedicated tank of an active mixing device and in-line injection systems possibly comprising static and / or high shear in-line mixers.
[0199] Step (a2)
[0200] Step (a2) of mixing the catalyst precursor formulation 104 already containing the organic additive with said heavy hydrocarbon feedstock 101 is preferably carried out at a temperature below a temperature at which a substantial portion of the catalyst precursor composition begins to thermally decompose, such as at a temperature from room temperature, e.g. 15°C, to 300°C, preferably in a range of 50°C to 200°C, and even more preferably in a range of 75°C to 175°C, to give the conditioned heavy hydrocarbon feedstock 103.
[0201] Preferably, the gauge pressure is between 0 MPa and 25 MPa, more preferably between 0.01 MPa and 5 MPa.
[0202] Step (a2) is carried out for a sufficient time and in a manner to disperse the catalyst precursor formulation throughout the feedstock to provide a conditioned heavy hydrocarbon feedstock 103 in which the catalyst precursor composition is completely / intimately mixed with the heavy hydrocarbon feedstock.
[0203] In order to obtain sufficient mixing of the catalyst precursor formulation 104 into the heavy hydrocarbon feedstock forming the colloidal or molecular catalyst, step (a2) is preferably carried out for a period of time in the range of 1 second to 30 minutes, more preferably 5 seconds to 10 minutes, and even more preferably in a range of 20 seconds to 3 minutes.
[0204] Step (a2) according to the second embodiment can be implemented in a dedicated tank of an active mixing device forming the second mixing apparatus of the conditioning mixer 610.
[0205] Such a configuration makes it possible in particular to increase the dispersion of the colloidal or molecular catalyst formed in a later stage. The use of a dedicated tank also allows to achieve a high residence time.
[0206] Step (a2) may alternatively comprise injecting said catalyst precursor formulation 104 into a pipe conveying the heavy hydrocarbon feedstock 101 to the entrained bed reactor. The second mixing apparatus of the conditioning mixer 610 thus comprises in such a configuration the part(s) of the pipe in which the mixing is carried out, and possibly additional systems to facilitate the mixing, such as for example static in-line mixers or high shear in-line mixers as described above. Such a configuration makes it possible in particular to reduce investments in installations and the required space requirement compared with mixing in a dedicated tank.
[0207] The second mixing apparatus of the conditioning mixer 610 may also comprise a combination of such a dedicated tank of an active mixing device and in-line injection systems possibly comprising static and / or high shear in-line mixers.
[0208] Alternatively, in step (a2), the catalyst precursor formulation 104 may be initially blended with 20% of the heavy hydrocarbon feedstock 101, the resulting blended heavy hydrocarbon feedstock may be blended with another 40% of the heavy hydrocarbon feedstock, and the resulting 60% of the blended heavy hydrocarbon feedstock may be blended with the remaining 40% of heavy hydrocarbon feedstock in accordance with good engineering practices of gradual dilution to fully disperse the catalyst precursor formulation 104 in the heavy hydrocarbon feedstock. The mixing time in the appropriate mixing devices or methods described herein should also be used for the gradual dilution approach.
[0209] The method according to the present invention is preferably carried out according to the second embodiment in which step (a) comprises (a1) premixing the organic additive compound 102 with the catalyst precursor composition 105 to produce the catalyst precursor formulation 104, and (a2) mixing said catalyst precursor formulation 104 with said heavy hydrocarbon feedstock 101.
[0210] In step (a), the mixing of the heavy hydrocarbon feedstock 101 with the catalyst precursor formulation 104 may be done for the heavy hydrocarbon feedstock 101, in part or in whole.
[0211] According to one or more preferred embodiments, the mixing step (a) is carried out between the catalyst precursor formulation 104 and the entire stream of the heavy hydrocarbon feedstock 101 sent to the hydroconversion system. In one or more alternative embodiments, the mixing step (a) is carried out between the catalyst precursor formulation 104 and a portion of the stream of the heavy hydrocarbon feedstock 101 sent to the hydroconversion. Thus, the preparation of the conditioned heavy hydrocarbon feedstock 103 can be carried out by mixing at least a portion of the stream of said heavy hydrocarbon feedstock 101, for example at least 50% by weight of the stream of said heavy hydrocarbon feedstock 101, with the catalyst precursor formulation 104. The additional portion of the stream of said heavy hydrocarbon feedstock 101 can be reincorporated once the catalyst precursor formulation 104 has been added, i.e. mixed with the conditioned heavy hydrocarbon feedstock 103 before its preheating in step (b).
[0212] Step (b): heating the conditioned heavy hydrocarbon feedstock
[0213] The conditioned heavy hydrocarbon feedstock 103 formed in step (a) is then heated in at least one preheating device 630, before being introduced into the entrained bed reactor for hydroconversion.
[0214] The conditioned hydrocarbon feedstock 103 is sent to the at least one preheating device 630, optionally pressurized by a pump.
[0215] The preheating device comprises any heating means capable of heating a heavy hydrocarbon feedstock known to a person skilled in the art. The preheating device may comprise a furnace comprising at least one preheating compartment, and / or tubes into which the hydrocarbon feedstock flows, a mixer of the conditioned hydrocarbon feedstock with H2, any type of suitable heat exchangers, for example tubular or spiral heat exchangers into which the hydrocarbon feedstock flows, etc.
[0216] This preheating of the conditioned heavy hydrocarbon feedstock makes it possible to reach a target temperature in the entrained bed hydroconversion reactor in the subsequent step (d).
[0217] The conditioned hydrocarbon feedstock 103 is more preferably heated in the preheater 630 to a temperature in a range of 280°C to 450°C, even more preferably in a range of 300°C to 400°C, and even more preferably in a range of 320°C to 365°C, in particular in order to later reach a target temperature in the hydroconversion reactor in step (c).
[0218] The skin temperature of the preheater, e.g. the skin temperature of the steel shell of a compartment or tubes of a furnace or heat exchanger(s), can reach from 400°C to 650°C. Mixing the catalyst precursor formulation 104 comprising the catalyst precursor composition 105 and the organic additive 102 with the heavy hydrocarbon feedstock 101 in step (a) avoids or reduces fouling that can occur in the preheater at these high temperatures.
[0219] According to one or more embodiments, the conditioned load is heated to a temperature which is 100°C lower than the hydroconversion temperature in the entrained bed hydroconversion reactor, preferably 50°C lower than the hydroconversion temperature. For example, for a hydroconversion temperature in the range of 410°C to 440°C, the conditioned hydrocarbon feedstock may be heated in step (b) to a temperature in the range of 310°C to 340°C.
[0220] The absolute pressure is between atmospheric pressure (eg 0.101325 MPa) and 38 MPa, preferably between 5 MPa and 25 MPa and preferably between 6 MPa and 20 MPa.
[0221] The heating in step (b) advantageously causes the conditioned hydrocarbon feedstock to release sulfur which can combine with the metal of the catalyst precursor composition.
[0222] According to one or more embodiments, the colloidal or molecular catalyst is formed, or at least begins to form, in situ in the heavy hydrocarbon feedstock conditioned at this heating step (b) in the preheating device 630.
[0223] In order to form the colloidal or molecular catalyst, sulfur must be available (eg as H2S) to combine with the metal of the catalyst precursor composition.
[0224] Formation of the colloidal or molecular catalyst in situ in the conditioned heavy hydrocarbon feedstock
[0225] The general formation of the colloidal or molecular catalyst in situ in the conditioned heavy hydrocarbon feedstock is described in detail below, as well as the conditions required for such formation in step (b) and / or (c).
[0226] In the event that the heavy hydrocarbon feedstock comprises sufficient or excess sulfur, the final activated catalyst may be formed in situ by heating the conditioned heavy hydrocarbon feedstock 103 to a temperature sufficient to release the sulfur therefrom.
[0227] A source of sulfur can thus be H2S dissolved in the heavy hydrocarbon feedstock, or H2S contained in hydrogen recycled to the entrained bed hydroconversion reactor for hydroconversion or H2S originating from sulfur-containing organic molecules present in the feedstock or possibly introduced beforehand into the heavy hydrocarbon feedstock (injection of dimethyl disulfide, thioacetamide, any hydrocarbon feedstock containing sulfur of the mercaptan type, sulfides, petroleum containing sulfur, gas oil containing sulfur, vacuum distillate containing sulfur, residue containing sulfur), such injection being rare and reserved for very atypical heavy hydrocarbon feedstocks.
[0228] Thus, a sulfur source may be sulfur compounds in the feed or a compound of sulfur added to the feed.
[0229] According to one or more embodiments, the formation of the colloidal or molecular dispersed catalyst is carried out at an absolute pressure between atmospheric pressure and 38 MPa, preferably between 5 MPa and 25 MPa, and more preferably between 6 MPa and 20 MPa.
[0230] Due to the complete / intimate mixing in step (a), a molecularly dispersed catalyst may form upon reaction with sulfur to form the metal sulfide compound. Under certain circumstances, slight agglomeration may occur, resulting in colloidal-sized catalyst particles. However, it is believed that taking care to thoroughly mix the precursor formulation throughout the heavy hydrocarbon feedstock in step (a) will result in individual catalyst molecules rather than colloidal particles. Performing simple assembly, while failing to sufficiently mix, typically results in the formation of large, agglomerated metal sulfide compounds that are micron-sized or larger.
[0231] In order to form the metal sulfide catalyst, the conditioned feedstock 103 is preferably heated to a temperature in a range from room temperature, e.g. 15°C, to 500°C, more preferably in the range of 200°C to 500°C, even more preferably in a range of 250°C to 450°C, and even more preferably in a range of 300°C to 435°C.
[0232] The temperature used in step (b) and / or (c) allows the formation of the metal sulfide type catalyst.
[0233] The colloidal or molecular catalyst may thus be formed, at least in part, during this heating step (b), before the heated conditioned feedstock 106 is introduced into the entrained bed hydroconversion reactor in step (c).
[0234] The colloidal or molecular catalyst can also be formed in situ in the entrained bed hydroconversion reactor itself in step (c), in particular either totally or partially in the case where it has started to form in step (b).
[0235] The molybdenum concentration in the conditioned hydrocarbon feedstock is preferably in a range of 10 ppm to 10,000 ppm by weight of the heavy hydrocarbon feedstock 101, more preferably in a range of 50 ppm to 6,000 ppm by weight, more preferably in a range of 100 ppm to 1,000 ppm by weight, even more preferably in a range of 100 ppm to 800 ppm by weight, and even more preferably in a range of 150 ppm to 400 ppm by weight.
[0236] Mo may become more concentrated as volatile fractions are removed from a non-volatile residue fraction.
[0237] Since the colloidal or molecular catalyst tends to be very hydrophilic, individual particles or molecules will tend to migrate towards the fragments or more hydrophilic molecules in the heavy hydrocarbon feedstock, especially asphaltenes. While the highly polar nature of the catalyst compound causes or allows the colloidal or molecular catalyst to associate with asphaltene molecules, it is the general incompatibility between the highly polar catalyst compound and the hydrophobic heavy hydrocarbon feedstock that necessitates the previously mentioned intimate or complete mixing of the oil-soluble catalyst precursor formulation into the heavy hydrocarbon feedstock prior to the formation of the colloidal or molecular catalyst.
[0238] Preferably, the colloidal or molecular catalyst comprises molybdenum disulfide.
[0239] Theoretically, a nanoscale crystal of molybdenum disulfide has 7 molybdenum atoms sandwiched between 14 sulfur atoms, and the total number of molybdenum atoms exposed at the edge, thus available for catalytic activity, is greater than in a micron-sized crystal of molybdenum disulfide. In practical terms, the formation of small catalyst particles as in the present invention, i.e., a colloidal or molecular catalyst, with improved dispersion, results in more catalyst particles and catalyst sites distributed more uniformly throughout the hydrocarbon feedstock. In addition, nanoscale or smaller molybdenum disulfide particles are believed to intimately associate with asphaltene molecules.
[0240] Step (c): hydroconversion of the heated conditioned charge
[0241] The heated conditioned feedstock 106 is then introduced, optionally pressurized by a pump, in particular if it has not already been pressurized before step (b), into at least one entrained bed reactor 640 together with hydrogen 601, and is operated under hydroconversion conditions to produce a recovered material 107.
[0242] As mentioned previously, the colloidal or molecular catalyst may form in situ in the entrained bed hydroconversion reactor itself in step (c), if it is not fully formed or not formed at all in step (b).
[0243] When the colloidal or molecular catalyst is formed in situ in the heavy hydrocarbon feedstock conditioned in step (b), the heated conditioned feedstock 106 already contains the colloidal or molecular catalyst, in part or in whole, when it is introduced into at least one entrained bed reactor 640.
[0244] The entrained bed reactor 640 comprises a liquid phase which comprises said heated conditioned feedstock 106 containing the colloidal or molecular catalyst dispersed therein, and a gas phase comprising hydrogen.
[0245] This type of entrained bed reactor is well known to a person skilled in the art.
[0246] The entrained bed reactor preferably comprises an upward flow of liquid and gas.
[0247] The entrained bed reactor for the hydroconversion of heavy hydrocarbon oils may, like most entrained bed reactors, be an empty plug flow type reactor, since the conditioned heavy hydrocarbon feedstock 106 containing the colloidal or molecular catalyst dispersed therein behaves as a homogeneous phase.
[0248] When operating with an upward flow of liquid and gas, the entrained bed reactor preferably includes an inlet port located at or near the bottom of the entrained bed reactor through which the heated conditioned feedstock 106 is introduced together with the hydrogen 201, and an outlet port at or near the top of the reactor through which the upgraded material 107 is withdrawn.
[0249] The colloidal or molecular catalyst is dispersed throughout the feed in the entrained bed reactor and is entrained from the reactor with the effluent comprising the recovered material 107.
[0250] The entrained bed reactor may include at its lower portion an agitator for dispersing the hydrogen more uniformly in the feedstock.
[0251] The entrained bed reactor may comprise a former ebullated bed reactor converted to an entrained phase reactor by removing the porous supported catalyst from the former ebullated bed reactor.
[0252] In some cases, the entrained bed reactor may include at its lower portion an agitator, and alternatively or in addition to such an agitator, the entrained bed reactor may include a recycle conduit, a recycle pump, and a distributor grid plate as in conventional ebullated bed reactors, allowing for the continuous recycling of at least a portion of a liquid fraction drawn from the upper portion of the reactor and reinjected at the lower portion of the reactor and promoting a more uniform dispersion of reactants, catalyst, and heat, and, as for example in US6960325B, also including a riser.
[0253] If an internal recycled feedstock is implemented, such internal recycled feedstock may be mixed with a second fresh heated conditioned feedstock 106 and additional hydrogen gas 201.
[0254] The presence of colloidal or molecular catalyst in the entrained bed reactor provides the catalytic hydrogenation activity. Free radical capping minimizes the formation of sediments and coke precursors, as already explained.
[0255] In the hydroconversion step (c), said heated conditioned feedstock 106 is generally converted under conventional conditions for the hydroconversion of a heavy hydrocarbon feedstock.
[0256] According to one or more embodiments, the hydroconversion step (c) is carried out under an absolute pressure of between 2 and 38 MPa, preferably between 5 and 25 MPa and preferably between 6 and 20 MPa, and at a temperature of between 300°C and 550°C, preferably between 350°C and 500°C, preferably between 370°C and 450°C, and more preferably between 400°C and 440°C, and even more preferably between 410°C and 435°C.
[0257] According to one or more embodiments, the liquid hourly space velocity (LHSV) of the feedstock relative to the volume of each entrained bed reactor is between 0.05 h 1 and 10 h 1, preferably between 0.10 h 1 and 2 h 1 and preferably between 0.10 h 1 and 1 h *. According to another embodiment, the WH is between 0.05 h 1 and 0.09 h 1. The WH is defined as the volumetric flow rate of liquid feedstock at room temperature and atmospheric pressure (typically 15°C and 0.101325 MPa) per reactor volume.
[0258] According to one or more embodiments, the quantity of hydrogen mixed with the heavy hydrocarbon feedstock 106 is preferably between 50 and 5,000 normal cubic meters (Nm3) per cubic meter (m3) of liquid heavy hydrocarbon feedstock, such as between 100 and 2,000 Nm3 / m3 and preferably between 500 and 1,500 Nm3 / m3.
[0259] According to one or more embodiments, the hydroconversion step (c) is carried out in one or more entrained bed hydroconversion reactors, which may be in series and / or in parallel.
[0260] Step (d): further treatment of the recovered material from the hydroconversion step (c)
[0261] The recovered material 107 can be further processed.
[0262] Examples of such further processing include, without limitation, at least one of the following: separation of hydrocarbon fractions from the upgraded material, further hydroconversion in one or more entrained bed reactors or ebullated-entrained hybrid reactors or additional ebullated bed reactors, which may be in series and / or in parallel, to produce further upgraded material, fractionation into hydrocarbon fractions of the further upgraded material, deasphalting of at least a portion of the upgraded material 107 or a heavy liquid fraction resulting from fractionation of the upgraded material or the further upgraded material, guard bed purification of the upgraded or further upgraded material to remove at least a portion of the colloidal or molecular catalyst and metallic impurities.
[0263] The various hydrocarbon fractions that may be produced from the upgraded material 107 may be sent to different processes in the refinery, and details of these post-treatments are not described herein since they are generally known to those skilled in the art and will complicate the description unnecessarily. For example, gaseous fractions, naphtha, middle distillates, VGO, DAO can be sent to hydrotreating, steam cracking, fluidized catalytic cracking (FCC), hydrocracking, lube oil extraction processes, etc., residues (atmospheric or vacuum residues) can also be post-treated, or used for other applications like gasification, bitumen production etc. Heavy fractions, including residues, can also be recycled to the hydroconversion process, for example in the entrained bed reactor.
[0264] According to one or more embodiments, as illustrated in [Fig.6], the method further comprises: - a second hydroconversion step in a second entrained bed reactor 660 in the presence of hydrogen 604 of at least a portion of, or all of, the recovered material resulting from the hydroconversion step (c) or optionally a liquid heavy fraction 603 which boils predominantly at a temperature greater than or equal to 350°C resulting from an optional separation step separating a portion of, or all of, the recovered material resulting from the hydroconversion step (c), said second entrained bed reactor 660 being operated under hydroconversion conditions to produce a hydroconverted liquid effluent 605 having a reduced heavy residue fraction, a reduced Conradson carbon residue, and optionally a reduced amount of sulfur and / or nitrogen; - a step of fractionating a portion of, or all of, said hydroconverted liquid effluent 605 in a fractionation section 670 to produce at least one heavy fraction 607 which boils predominantly at a temperature greater than or equal to 350°C, said heavy fraction containing a residual fraction which boils at a temperature greater than or equal to 540°C; - an optional step of deasphalting part of, or all of, said heavy fraction 607 in a deasphalter 680 with at least one hydrocarbon solvent to produce a deasphalted oil DAO 608 and a residual asphalt 609.
[0265] Said second hydroconversion step is carried out in a manner similar to that described for hydroconversion step (c), and its description is therefore not repeated here. This applies in particular to the operating conditions, to the equipment used, with the exception of the specifications mentioned below.
[0266] As for the hydroconversion step (c), the second hydroconversion step is carried out in a second entrained bed reactor 660 similar to the entrained bed reactor 640.
[0267] In this additional hydroconversion step, the operating conditions may be similar or different from those in hydroconversion step (c), the temperature remaining in the range between 300°C and 550°C, preferably between 350°C and 500°C, more preferably between 370°C and 450°C, still preferably between 400°C and 440°C, and even more preferably between 410°C and 435°C, and the amount of hydrogen introduced into the reactor remaining in the range between 50 and 5,000 NmVm3 of liquid feed, preferably between 100 and 2,000 NmVm3, and even more preferably between 500 and 1,500 Nm3 / m3. The other pressure and WH parameters are in the same ranges as those described for the hydroconversion step (c).
[0268] The optional separation step, separating some or all of the upgraded material 107 to produce at least two fractions including the heavy liquid fraction 603 which boils predominantly at a temperature greater than or equal to 350°C, is carried out in a separation section 650.
[0269] The other fraction(s) 602 are one or more light and intermediate fractions. The light fraction thus separated mainly contains gases (H2, H2S, NH3, and CrC 4), naphtha (fraction which boils at a temperature below 150°C), kerosene (fraction which boils between 150°C and 250°C), and at least part of the diesel (fraction which boils between 250°C and 375°C). The light fraction can then be sent at least partially to a fractionation unit (not shown in [Fig.6]) where the light gases are extracted from said light fraction, for example by passing through an expansion drum. The hydrogen gas thus recovered, which may have been sent to a purification and compression installation, can advantageously be recycled in the hydroconversion step (c). The recovered hydrogen gas can also be used in other installations of the refinery.
[0270] The separation section 650 comprises any separation means known to a person skilled in the art. It may comprise one or more expansion tanks arranged in series, and / or one or more steam and / or hydrogen stripping columns, and / or an atmospheric distillation column, and / or a vacuum distillation column, and preferably consists of a single expansion tank, commonly referred to as a “hot separator”.
[0271] The fractionation step separating a portion of, or all of, the hydroconverted liquid effluent from the second hydroconversion step to produce at least two fractions comprising the at least one heavy liquid fraction 607 which boils predominantly at a temperature above 350°C, preferably above 500°C and preferably above 540°C, is carried out in the fractionation section 670 comprising any separation means known to a person skilled in the art. The other fraction(s) 606 are one or more light and intermediate fractions.
[0272] The heavy liquid fraction 607 contains a fraction that boils at a temperature above 540°C, called vacuum residue (which is the unconverted fraction). It may contain a portion of the diesel fraction that boils between 250°C and 375°C and a fraction that boils between 375°C and 540°C, called vacuum distillate.
[0273] The fractionation section 670 may comprise one or more flash drums arranged in series, and / or one or more steam and / or hydrogen stripping columns, and / or an atmospheric distillation column, and / or a vacuum distillation column, and preferably consists of a set of several flash drums in series and atmospheric and vacuum distillation columns.
[0274] When it is desired to recycle a portion of the heavy residue fraction (e.g., a portion of the heavy liquid fraction 107, and / or a portion of the residual asphalt 609, or a portion of the DAO 608) into the hydroconversion system (e.g., into the entrained bed reactor 640 or upstream), it may be advantageous to leave the colloidal or molecular catalyst in the residues, and / or the residual asphalt fraction. A purge on the recycled stream may be implemented, generally to prevent certain compounds from accumulating at excessive levels.
[0275] The present invention also relates to an entrained bed system 600 configured to hydroconvert the heavy hydrocarbon feedstock 101 as detailed above. The reference numerals mentioned below relate to [Fig. 6], which schematically illustrates an example of an entrained bed hydroconversion system according to the invention. Said system 600 comprises: - the conditioning mixture 610 configured to prepare the conditioned feedstock 103 by mixing said heavy hydrocarbon feedstock 101 with the catalyst precursor formulation 104 which comprises the catalyst precursor composition 105 comprising molybdenum and the organic additive at a molar ratio between said organic chemical compound 102 and molybdenum of between 0.1:1 and 20:1; - the at least one preheating device 630 configured to heat the conditioned load 103; - the at least one entrained bed reactor 640 configured to comprise: — a liquid hydrocarbon phase comprising the heated conditioned feedstock 106 containing the colloidal or molecular catalyst dispersed therein; — and a gaseous phase comprising hydrogen.
[0276] Said at least one entrained bed reactor 640 is configured to operate in the presence of hydrogen and under hydroconversion conditions in order to cause thermal cracking of hydrocarbons in said heated conditioned feedstock to provide an upgraded material 107.
[0277] Said at least one preheater 630 and / or said at least one entrained bed reactor 640 are also configured to form the colloidal or molecular catalyst in said conditioned heavy hydrocarbon feedstock.
[0278] Details of each device / apparatus / section used in the system in driven bed have already been mentioned above in connection with the process and are not repeated. Examples
[0279] The following example illustrates, without limiting the scope of the invention, some of the performances of the method and system according to the invention, in particular the reduced fouling of the installations, by comparison with a method and a system according to the prior art.
[0280] The example is based on a test using an analytical device, called Alcor Hot Liquid Process Simulator, or HLPS, from Alcor, stimulating the fouling effect of atmospheric residues (AR) in heat exchangers. AR is pumped through a heating tube (laminar flow tube-in-shell heat exchanger) under controlled conditions and fouling deposits are formed on the heating tube. The temperature of PAR exiting the heat exchanger is related to the effect of the deposits on the efficiency of the heat exchanger. The decrease in AR liquid outlet temperature from its initial maximum value is called Delta T and is correlated with the amount of deposits. The greater the decrease in Delta T, the greater the amount of fouling and deposits.
[0281] The HLPS test can be used to evaluate the fouling tendency of different ARs by comparing the decreasing slope of the AR liquid outlet temperature obtained under identical test conditions. The effectiveness of an organic additive can also be determined by comparing the test results of a neat sample (without an organic additive) to the sample mixed with the organic additive.
[0282] Two samples are tested: sample 1 is a mixture of a heavy hydrocarbon feedstock and a molecular or colloidal catalyst according to the prior art, and sample 2 is a mixture according to the invention comprising the same heavy hydrocarbon feedstock with the same molecular or colloidal catalyst, in addition to an organic additive.
[0283] The heavy hydrocarbon feedstock used (“Feedstock”) is an atmospheric residue (AR) whose main composition and properties are given in Table 1 below.
[0284] [Tables 1] Standardized Method Unit VGO Charge (CPC Diluent) Density NF EN ISO 12185 0.959 0.8677 IBP at 350°C ASTM DI 160 wt. % 21 2.7 350 to 540°C ASTM DI 160 wt. % 35 95.5 540°C+ ASTM DI 160 wt. % 44 1.8 C ASTM D5291 wt. % 84.5 86.5 H ASTM D5291 wt. % 11.4 13.71 N ASTM D5291 wt. % 0.3 0.0037 S NF ISO 8754 wt. % 3.81 0.074 Ni ASTM D7260 wt. ppm 25 <2 V ASTM D7260 wt. ppm 78 <2 K ASTM D7260 ppm by weight 2 < 1 Na ASTM D7260 ppm by weight 196 < 1 Ca ASTM D7260 ppm by weight < 1 < 1 P ASTM D7260 ppm by weight <5 <5 Si ASTM D7260 ppm by weight < 1 < 1 Fe ASTM D7260 ppm by weight 3 6 Ti ASTM D7260 ppm by weight 79 < 1 C5 asphaltenes UOP99 - 07% by weight 10.6 0.2 C7 asphaltenes NF T60-115% by weight 4.7 0.05 Conradson carbon NF EN ISO 10370% by weight 11.3 0.2
[0285] Sample 1: Sample 1 is a mixture of the Feedstock and a catalyst precursor composition (CPC) which is molybdenum 2-ethylhexanoate diluted in vacuum gas oil (VGO).
[0286] The composition of VGO is given in Table 1 above.
[0287] The CPC solution is obtained by mixing molybdenum 2-ethylhexanoate with VGO, at a temperature of 70°C for a period of 30 minutes. The molybdenum content in the CPC solution containing VGO is 3500 ppm by weight.
[0288] The CPC solution is then mixed with the Charge (AR) at a temperature of 70°C and for a period of time of 30 minutes.
[0289] The Mo content in sample 1 is 283 ppm by weight (see Table 2 below).
[0290] Sample 2: Sample 2 is a mixture of the Charge (AR) with the same CPC solution (molybdenum 2-ethylhexanoate diluted with VGO) as in Sample 1, and with an organic additive which is 2-ethylhexanoic acid (2EHA). The CAS number of 2EHA is 149-57-5.
[0291] The CPC solution, obtained as detailed for sample 1, is first mixed with the 2EHA, for a period of time of 30 min, and at a temperature of 70°C.
[0292] Then, the CPC solution containing the organic additive 2EHA is mixed with the Charge (AR), at a temperature of 70°C and for a period of time of 30 minutes.
[0293] The Mo content in sample 2 is 283 ppm by weight (see Table 2 below).
[0294] The concentration of organic additive 2EHA is 5,761 ppm by weight (see Table 2 below).
[0295] The molar ratio of 2EHA / Mo = 13.6.
[0296] [Tables2] Sample 1: Filler + CPC in VGO Sample 2: Filler + (CPC in VGO + 2EHA) Mo (ppm by weight) 283 283 Acid-type organic additive 2EHA (ppm by weight) - 5761
[0297] The Mo content in the samples was determined according to ASTM D7260. The content of organic additives of acid and ester type was determined by weighing.
[0298] The HLPS test conditions are given in Table 3 below.
[0299] [Tables3] Test Mode Single Pass Load Temperature (°C) 90 Flow Rate (mL / min) 1 Inlet Oil Temperature (°C) 100 Tube Temperature (°C) 450 Tube Material 1018 Steel Gauge Pressure (MPa) 3.4
[0300] The test results for the different samples (Si for sample 1, S2 for sample 2) are shown in the graph of [Fig.7]. The X axis represents the time in hours, and the Y axis represents the temperature difference AT between the temperature of the oil mixture (sample) leaving the tube at time t [THuiieSortie]t and the maximum temperature of the oil mixture (sample) leaving the tube [THuiieSortie]Max: AT [THuiie Sortie]t ” [Tuuile Sortie]Max*
[0301] The results show that sample 1 has a strong tendency to fouling since its Delta T drops rapidly. Sample 2 which contains an organic additive, e.g. 2EHA, according to the invention has a lower Delta T than sample 1, showing that the fouling behavior is significantly reduced under the action of said organic additive.
Claims
Claims
1. Process for the hydroconversion of a heavy hydrocarbon feedstock (101) containing a fraction of at least 50% by weight having a boiling point of at least 300°C, and containing metals and asphaltenes, said heavy hydrocarbon feedstock (101) comprises at least one of the following feedstocks: crude oil, tar sands bitumen, atmospheric distillation column bottoms, vacuum distillation column bottoms, residues, screw coreducer bottoms, coal tar, heavy oil from oil shale, liquefied coal, heavy bio-oils, and heavy oils comprising plastic waste and / or plastic pyrolysis oil, said method comprising the following steps: (a) preparing a conditioned heavy hydrocarbon feedstock (103) by mixing said heavy hydrocarbon feedstock (101) with a catalyst precursor formulation (104) in such a way that a colloidal or molecular catalyst is formed when it reacts with sulfur,said catalyst precursor formulation (104) comprising:, - a catalyst precursor composition (105) comprising molybdenum, and - an organic chemical compound (102) selected from the group consisting of ethylhexanoic acid, naphthenic acid, caprylic acid, adipic acid, pimelic acid, suberic acid, azelaic acid, and sebacic acid, ethyl octanoate, ethyl 2-ethylhexanoate, 2-ethylhexyl 2-ethylhexanoate, benzyl 2-ethylhexanoate, diethyl adipate, dimethyl adipate, bis(2-ethylhexyl) adipate, dimethyl pimelate, dimethyl suberate, monomethyl suberate, hexanoic anhydride, caprylic anhydride, and mixtures thereof, and - a molar ratio between said organic chemical compound (102) and molybdenum in said catalyst precursor formulation (104) being between 0.1:1 and 20:1; (b) heating the conditioned heavy hydrocarbon feedstock (103) from step (a) in at least one preheating device; (c) introducing said heated conditioned heavy hydrocarbon feedstock (106) of step (b) into at least one entrained bed reactor and operating said entrained bed reactor in the presence of hydrogen and in hydroconversion conditions to produce a recovered material (107); and the colloidal or molecular catalyst being formed in situ in the heavy hydrocarbon feedstock conditioned in step (b) and / or in step (c).
2. The method of claim 1, wherein step (a) comprises simultaneously mixing said organic chemical compound (102) with said catalyst precursor composition (105), preferably previously diluted with a hydrocarbon diluent, and with said heavy hydrocarbon feedstock (101), preferably at a temperature below a temperature at which a substantial portion of the catalyst precursor composition begins to thermally decompose, such as at a temperature between room temperature and 300°C, and for a period of time from 1 second to 30 minutes.
3. The method of claim 1, wherein step (a) comprises (a1) pre-mixing said organic chemical compound (102) with said catalyst precursor composition (105) to produce said catalyst precursor formulation (104) and (a2) mixing said catalyst precursor formulation (104) with said heavy hydrocarbon feedstock (101).
4. The method of claim 3, wherein in step (a1) said catalyst precursor composition (105) is mixed at a temperature below a temperature at which a substantial portion of the catalyst precursor composition begins to thermally decompose, preferably at a temperature between room temperature and 300°C.
5. A method according to any preceding claim, wherein a hydrocarbon oil diluent is used to form the catalyst precursor formulation (104), said hydrocarbon oil diluent preferably being selected from the group consisting of vacuum gas oil, decanter oil or recycle oil, light gas oil, vacuum residues, deasphalted oils, and resins.
6. A method according to any preceding claim, wherein the organic chemical compound (102) comprises 2-ethylhexanoic acid, and is preferably 2-ethylhexanoic acid.
7. A method according to any one of claims 1 to 5, wherein the organic chemical compound (102) comprises ethyl octanoate or 2-ethylhexyl 2-ethylhexanoate, and is preferably ethyl octanoate or 2-ethylhexyl 2-ethylhexanoate.
8. A method according to any preceding claim, wherein the catalyst precursor composition comprises an oil-soluble organometallic compound or complex selected from the group consisting of molybdenum 2-ethylhexanoate, molybdenum naphthanate, molybdenum hexacarbonyl, and is preferably molybdenum 2-ethylhexanoate.
9. A method according to any preceding claim, wherein the molar ratio of said organic chemical compound (102) to molybdenum in said catalyst precursor formulation (104) is between 0.75:1 and 7:1, and preferably between 1:1 and 5:
1.
10. A method according to any preceding claim, wherein the colloidal or molecular catalyst comprises molybdenum disulfide.
11. A method according to any preceding claim, wherein step (b) comprises heating to a temperature between 280°C and 450°C, more preferably between 300°C and 400°C, and more preferably in a range of 320°C to 365°C.
12. A method according to any preceding claim, wherein the heavy hydrocarbon feedstock (101) has sulfur in a content greater than 0.5% by weight, a Conradson carbon residue of at least 0.5% by weight, C7 asphaltenes in a content greater than 1% by weight, transition and / or post-transition metals and / or metalloids in a content greater than 2 ppm by weight, and alkali and / or alkaline earth metals in a content greater than 2 ppm by weight.
13. A process according to any preceding claim, wherein said hydroconversion step (c) is carried out under an absolute pressure of between 2 MPa and 38 MPa, at a temperature of between 300°C and 550°C, at an hourly volumetric flow rate WH relative to the volume of each entrained bed reactor of between 0.05 h 1 and 10 h 1 and under an amount of hydrogen mixed with the feed entering the entrained bed reactor of between 50 and 5,000 normal cubic meters (Nm3) per cubic meter (m3) of feed.
14. A method according to any preceding claim, wherein the molybdenum concentration in the conditioned hydrocarbon feedstock is in a range of 10 ppm to 10,000 ppm by weight of the heavy hydrocarbon feedstock.