Electrode design for a primary lithium-type electrochemical element

The spiral electrochemical element design with a lithium-covered internal face optimizes positive electrode efficiency, addressing inefficiencies at high temperatures by maintaining capacity and reducing material usage.

FR3128060B1Active Publication Date: 2024-10-25SAFT GRP SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FR2021010815
Authority / Receiving Office
FR · FR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-10-12
Publication Date
2024-10-25
Estimated Expiration
2041-10-12

AI Technical Summary

Technical Problem

Primary lithium electrochemical elements used at high temperatures face inefficiencies due to the negative electrode capacity being lower than the positive electrode, leading to incomplete discharge and safety issues, necessitating improved spiral constructions to optimize positive electrode efficiency.

Method used

A spiral electrochemical element design where the external face of the spiral is formed by the positive electrode, and an internal face of the container is partially or fully covered by a lithium or lithium-based alloy sheet, distributing lithium in two contributions to enhance positive electrode efficiency.

Benefits of technology

This design increases the discharge efficiency of the positive electrode, maintaining electrochemical capacity while reducing the need for active materials, thus lowering production costs and improving performance at high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000015_0000
    Figure 00000015_0000
  • Figure 00000015_0001
    Figure 00000015_0001
  • Figure 00000016_0000
    Figure 00000016_0000
Patent Text Reader

Abstract

The present invention relates to an electrochemical element comprising a container including an electrochemical beam, said electrochemical beam being in the form of a spiral formed by the winding of the superposition of: a positive electrode comprising an active material selected from SOCl2, SO2, SO2Cl2; CFx with x≤ 1.5; MnO2, FeS2, V2O5, I2, Bi2O3, Bi2Pb2O5, CuCl2, CuF2, CuO, Cu4O(PO4)2, CuS, FeS, MoO3, Ni3S2, AgCl, Ag2CrO4, V2O5, SVO, MO6S8, and a mixture of several of these; a separator; a negative electrode comprising an active material of lithium metal or lithium-based alloy; characterized in that the external face of the spiral, opposite the container, is formed by the positive electrode; and that a sheet of lithium or a lithium-based alloy covers at least partially the inner surface of the container. Figure for the abbreviation: Fig. 1
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: Design of electrodes for a primary lithium-type electrochemical element Technical field of the invention

[0001] The technical field of the present invention is that of primary electrochemical elements comprising an anode made of lithium metal or lithium-based alloy. Prior art

[0002] The terms “element” or “electrochemical element” will be used interchangeably in the following. The term “primary” designates a non-rechargeable electrochemical element, also referred to as a battery, as opposed to the term “secondary” which designates a rechargeable electrochemical element, also called an accumulator.

[0003] The family of primary lithium electrochemical elements also includes primary electrochemical elements with liquid cathode, sometimes also called catholyte, and primary electrochemical elements with solid cathode.

[0004] Primary electrochemical cells with liquid cathodes, of the Li / SO2, Li / SOCl2 and Li / SO2Cl2 type are known. The anode (or negative electrode) is made of lithium metal or lithium alloy. The positive electrode is a porous mass of carbon with a large specific surface area, the pores of which contain SO2, or SOCl2 or SO2Cl2. SO2 being gaseous at room temperature, is present in the cell in a form dissolved in an organic solvent, such as acetonitrile. Since SOCl2 or SO2Cl2 are liquid at room temperature, they constitute both the solvent of the electrolyte and the cathode of the cell. During the discharge of such a cell, the oxidation of the metallic lithium into lithium ions occurs at the anode according to the following reaction:

[0005] 2 Li —> 2 Li+ + 2 e

[0006] At the positive electrode, the reduction of the oxidizing compound occurs in the pores of the carbon mass, the support for the cathodic reaction. In the case where the oxidizing agent is sulfur dioxide SO2, the reduction reaction is as follows:

[0007] 2 SO2 + 2 e S2O42

[0008] In the case where the oxidant is SOC12, the reduction reaction is as follows:

[0009] 2 SOC12 + 4 e S + SO2 + 4 Cl

[0010] Primary electrochemical cells with solid cathodes of the Li / MnO2 and Li / CFx type are known. The anode is made of metallic lithium or lithium alloy. In discharge at the cathode, MnIV02 is transformed into LiMnUI02; CFX is transformed into carbon. During discharge, it occurs at the anode, as for a primary cell with liquid cathode, the oxidation of metallic lithium to lithium ions. The organic solvents used may be propylene carbonate or dimethoxyethane. The salt used may be chosen from lithium perchlorate LiC104, lithium hexafluoroarsenate LiAsF6, or lithium hexafluorophosphate LiPF6.

[0011] Such electrochemical elements are generally constructed with a spiral arrangement of the electrodes.

[0012] This spiral construction can take different forms.

[0013] Document KR 10-1996543 describes, for example, a primary lithium-type element in which only the cathode is spiraled. Documents CN 109698320, US 2020 / 0266452 and US 9748610 describe constructions in which the cathode, the separator and the anode are superimposed and then the assembly is wound to form a spiral.

[0014] Generally, a primary lithium cell used at room temperature has a negative electrode capacity lower than that of the positive electrode, this is so that all the lithium of the negative electrode is consumed at the end of discharge, for safety reasons. However, when these spiral constructions are used for high temperature applications, in particular for temperatures above 150°C, it is intended to use a larger quantity of lithium in the cell to compensate for the effect of temperature on the self-discharge of the anode because the self-discharge phenomenon increases when the cell is used at a temperature above 150°C. Thus, with a larger quantity of lithium, the ratio between the capacity of the negative electrode and the capacity of the positive electrode is preferably greater than 1.Since the positive electrode is the limiting electrode, it is important that its operating efficiency is optimized. There is therefore a need to develop primary lithium cells of spiral construction for high-temperature applications, allowing the efficiency of the positive electrode to be maximized. Summary of the invention

[0015] The invention has as its first subject an electrochemical element comprising a container comprising an electrochemical bundle, said electrochemical bundle being in the form of a spiral constituted by the winding of the superposition: - of a positive electrode comprising an active material chosen from SOCl2, SO2, SO2C12; CFX with x < 1.5; MnO2, FeS2, V2O5,12, Bi2O3, Bi2Pb2O5, CuCl2, CuF2, CuO, Cu4O(PO4)2, CuS, FeS, MoO3, Ni3S2, AgCl, Ag2CrO4, V2O 5, SVO, MO6S8, and a mixture of several of these; - a separator; - a negative electrode comprising an active material made of lithium metal or lithium-based alloy; characterized in that the external face of the spiral, facing the container, is formed by the positive electrode; and that a sheet of lithium or a lithium-based alloy at least partially covers the internal face of the container.

[0016] According to one embodiment of the electrochemical element, the container is cylindrical and the lithium or lithium-based alloy sheet occupies at least 75%, preferably at least 95%, of the circumference of the container.

[0017] According to one embodiment of the electrochemical element, the active material of the positive electrode is chosen from CFV with x < 1.5; MnO2, SOC12, SO2, FeS2.

[0018] According to one embodiment of the electrochemical element, the active material is of the CFX type with x < 1.5.

[0019] According to one embodiment of the electrochemical element, the active material of the negative electrode is a lithium-based alloy of formula LiM, where M is chosen from the group consisting of Mg, Al, Si, B, Ge, Ga or a mixture of several of these.

[0020] According to one embodiment of the electrochemical element, the active material of the negative electrode is an alloy of the LiMg type.

[0021] According to one embodiment of the electrochemical element, the element is of the LiMg / CFr type with x < 1.5.

[0022] According to one embodiment of the electrochemical element, the active material of the negative electrode of the spiral is arranged on both faces of a current collector.

[0023] According to one embodiment of the electrochemical element, the thickness of said lithium sheet or of a lithium-based alloy covering the internal face of the container represents at most 75% or at most 50% or at most 25% of the thickness of the active material of the negative electrode of the spiral.

[0024] According to one embodiment of the electrochemical element, the ratio between the capacity of the negative electrode and the capacity of the positive electrode is greater than 1.

[0025] According to one embodiment of the electrochemical element, the element has a discharge efficiency greater than or equal to 70%, the efficiency being defined as the ratio between the capacity discharged by the element at a rate less than or equal to C / 120 at a temperature of 200°C and the theoretical capacity of the positive electrode or of the negative electrode having the lowest capacity.

[0026] According to one embodiment of the electrochemical element, the diameter of the spiral is between 10 and 50 mm, preferably between 20 and 35 mm.

[0027] The second object of the invention is the use of the electrochemical element as defined above, in storage, charging or discharging at a temperature of at least 150°C.

[0028] The third subject of the invention is a method for manufacturing an electrochemical element as defined above, comprising at least the following steps: a. Plating the lithium sheet or the lithium-based alloy against the internal face of the container, so that the entire surface of the lithium sheet faces the last turn of the electrochemical bundle formed by the positive electrode; b. Formation of the electrochemical beam in the form of a spiral; c. Introduction of the electrochemical beam into the container obtained in step a); d. Making the electrical connection between the negative electrode and the negative current output terminal of the cell and making the electrical connection between the positive electrode and the positive current output terminal of the cell; e. Assembling a lid on the container; f. Filling the cell with an electrolyte; g. Closing the cell.

[0029] The applicant has surprisingly discovered that dividing the total quantity of lithium into two contributions, namely a first contribution at the level of the spiral negative electrode and a second contribution at the level of the lithium sheet at least partially covering the internal face of the container, makes it possible to increase the efficiency of the positive electrode, that is to say to increase the ratio between the actual discharge capacity of the element and the theoretical (calculated) discharge capacity of the element, in the situation where it is the positive electrode which limits the capacity of the element. Obtaining a better efficiency makes it possible to increase the electrochemical capacity of the element, with equal quantities of active materials. In other words, it is possible to maintain an electrochemical discharge capacity identical to that of a standard spiral primary lithium element, while using less positive and negative active materials.The invention allows to reduce production costs since a lower quantity of positive and negative active materials is used for an identical restored capacity of the element. Brief description of the figures

[0030] [Fig.l] illustrates a schematic representation of an element (1) according to the invention comprising a positive electrode (a), and a negative electrode (b) wound together in the form of a spiral and a lithium sheet (c) covering the internal face of the container (d). The separator, although present in the element, is not shown here, for the sake of ease of understanding.

[0031] [Fig.2] represents the discharged capacity of the elements AO and AP during a discharge at the respective regime of C / 125 and C / l 16 at 200°C under 135 mA after 48 h of storage at 150°C of these elements.

[0032] [Fig.3] represents the discharged capacity of the elements AO, AR1, AP3 and AQ1 during a discharge at the respective regime of C / 125, C / 125, C / l 16 and C / l 10, at 200°C under 135 mA after 48 h of storage at 150°C of these elements.

[0033] Description of embodiments of the invention

[0034] The invention has as its first subject an electrochemical element comprising a container comprising an electrochemical bundle, said electrochemical bundle being in the form of a spiral constituted by the winding of the superposition: - of a positive electrode comprising an active material chosen from SOCl2, SO2, SO2C12; CFX with x<1.5; MnO2, FeS2, V2O5,12, Bi2O3, Bi2Pb2O5, CuCl2, CuF2, CuO, Cu4O(PO4)2, CuS, FeS, MoO3, Ni3S2, AgCl, Ag2CrO4, V2O 5, SVO, MO6S8, and a mixture of several of these; - a separator; - a negative electrode comprising an active material made of lithium metal or a lithium-based alloy; characterized in that the external face of the spiral, facing the container, is formed by the positive electrode; and that a sheet of lithium or a lithium-based alloy at least partially covers the internal face of the container.

[0035] The electrochemical element according to the invention as well as its various constituents will be described in the following.

[0036] Container and lithium foil pressed against the container wall

[0037] The container of the electrochemical element according to the invention can be in different forms compatible with a spiral electrochemical bundle. Preferably, the container is cylindrical.

[0038] The internal face of the container is covered at least partially by a lithium sheet or a lithium-based alloy.

[0039] According to one embodiment, this lithium or lithium-based alloy sheet occupies at least 75%, preferably at least 95% of the circumference of the container. Preferably, it occupies at least half of the internal height of the container, preferably at least 75%, more preferably at least 95% of the internal height of the container.

[0040] According to one embodiment, the lithium or lithium-based alloy sheet reaches 95% to 105% of the height of the electrochemical beam.

[0041] According to another embodiment, this lithium or lithium-based alloy sheet completely covers the internal face of the container which is in contact with the electrochemical beam.

[0042] The sheet may be made of pure lithium or a lithium-based alloy of formula LiM wherein M is selected from the group consisting of Mg, Al, Si, B, Ge, Ga or a mixture of several thereof. A person skilled in the art will choose the alloying element depending on the environment in which the element is used, in particular its temperature. Preferably, the lithium foil is made of pure lithium. The inner face of the container can be used as a current collector.

[0043] The thickness of said lithium sheet or lithium-based alloy covering the inner face of the container represents at most 75% or at most 50% or at most 25%, or at most 15% of the thickness of the active material of the negative electrode of the spiral. Preferably, the thickness of the lithium sheet represents from 45% to 55% of the thickness of the active material of the negative electrode of the electrochemical bundle.

[0044] The lithium or lithium-based alloy sheet may have a thickness of between 0.1 and 0.6 mm or between 0.2 and 0.4 mm or between 0.2 and 0.3 mm.

[0045] The theoretical electrochemical capacity of the lithium sheet may represent 5 to 35% or 10 to 30% or 15 to 25% of the theoretical electrochemical capacity of the negative electrode of the electrochemical bundle.

[0046] Positive electrode (cathode)

[0047] The active material of the positive electrode may be selected from CF> with x < 1.5; MnO2, SOCl2, SO2, SO2C12, FeS2, V2O5,12, Bi2O3, Bi2Pb2O5, CuCl2, CuF2, CuO, Cu4 O(PO4)2, CuS, FeS, MoO3, Ni3S2, AgCl, Ag2CrO4, V2O5, SVO, MO6S8, and a mixture of several of these.

[0048] The electrochemical element according to the invention may comprise a liquid cathode or a solid cathode.

[0049] a) The liquid cathodic active material may be chosen from SOCl2, SO2, SO2Cl2 or a mixture thereof. In this case, the positive electrode corresponds to a porous mass of carbon with a large specific surface area impregnated with an electrolyte. It supports the cathodic reaction. The electrolyte may be either SO2 dissolved in an organic solvent to which one or more lithium salts have been added, or SOCl2, or SO2Cl2 to which one or more lithium salts have been added. The porous mass of carbon serves as a current collector and the carbon pores house the liquid cathodic active material.

[0050] b) The solid cathodic active material may be chosen from CFV with x < 1.5; MnO 2, FeS2, V2O5,12, Bi2O3, Bi2Pb2O5, CuCl2, CuF2, CuO, Cu4O(PO4)2, CuS, FeS, MoO3, Ni3S2, AgCl, Ag2CrO4, V2O5, SVO, MO6S8 or a mixture thereof.

[0051] According to one embodiment, the active material is CF> with x < 1.5, preferably with x between 0.2 and 1.1.

[0052] The positive electrode and the negative electrode are impregnated with a liquid organic electrolyte comprising: - one or more organic solvents of cyclic carbonate type (carbonate of propylene (PC), ethylene carbonate (EC)), linear carbonates (dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (EMC), fluorinated or not (mono fluoroethyl carbonate ...), glymes and its derivatives (dimethoxyethane ...), furan (tetrahydro-furan) and its fluorinated derivatives, but also ionic liquids or any other solvent known in Li-ion or primary lithium technologies. - lithium salts known from lithium-ion and primary lithium technologies (LiPF6, LiBF4, lithium trifluoromethanesulfonimide LiN(CF3SO2)2 (LiTSFI), lithium bis(fluorosulfonyl)imide Li(FSO2)2N (LiFSI), lithium bis(oxalatoborate) LiBOB...). ; - Optionally additives commonly used in the field of lithium-ion and primary lithium batteries. These additives are in particular vinylene carbonate (VC), LiPO2F2, or any other additive making it possible to actively participate in the passivation of lithium, or even to allow the capture of water in the element also called in English "water scavengers".

[0053] According to another embodiment, the solid active material of the positive electrode can be arranged on a current collector which can be a perforated or non-perforated metal, a grid, a metal fabric, a ribbon. The current collector can be made of a material chosen from copper, aluminum, stainless steel and nickel, preferably nickel.

[0054] The thickness of the current collector may be between 0.2 and 0.3 mm, preferably the thickness is about 0.25 mm.

[0055] The total thickness of the positive electrode may be 0.8 to 1.5 mm.

[0056] Negative electrode (anode)

[0057] The negative electrode according to the invention comprises an active material made of lithium metal or lithium-based alloy.

[0058] The active material of the negative electrode may be a lithium-based alloy of formula LiM, where M is selected from the group consisting of Mg, Al, Si, B, Ge, Ga or a mixture of several thereof. Preferably, M is Mg.

[0059] The proportion of lithium in an alloy may be between 70 and 95%, preferably between 75 and 85% relative to the total weight of the alloy. Advantageously, lithium may be present in the alloy at a level of 75% relative to the total weight of the alloy.

[0060] According to one embodiment, the active material of the negative electrode can be arranged on one or two faces of a current collector. Preferably, the active material is deposited on both faces of the current collector.

[0061] According to another embodiment, the current collector is chosen from the group comprising a metal sheet in expanded or perforated form, a metal fabric, a ribbon, a grid. It is made of a material that can be chosen from copper, stainless steel and nickel, preferably nickel.

[0062] According to another embodiment, the active material of the negative electrode is not arranged on a current collector.

[0063] The thickness of the negative electrode may be between 0.1 and 0.8 mm, preferably between 0.2 and 0.3 mm. Advantageously, the thickness of the negative electrode is 0.25 mm.

[0064] Separator

[0065] The separator material may be selected from polyolefins, for example polypropylene, polyethylene, polyesters, glass fibers bonded together by a polymer, polyimides, polyamides, polyaramid, polyamideimide and cellulose. The polyester may be selected from polyethylene terephthalate (PET) and polybutylene terephthalate (PBT). Advantageously, the polyester or polypropylene or polyethylene contains or is coated with a material selected from the group consisting of a metal oxide, a carbide, a nitride, a boride, a silicide and a sulfide. This material may be SiO2 or Al2O3.

[0066] Preferably, at high temperature, the separator may be composed of glass fibers bonded together by a polymer or a porous polymer film whose degradation temperature allows its use at high temperature (200°C to 230°C). The polymers capable of being used for this purpose may be chosen from para-aramid, PEEK (polyetheretherketone), PPS (polyphenylene sulfide) or a mixture of one or more of these polymers with cellulose or PAN (polyacrylonitrile).

[0067] Electrochemical beam

[0068] An electrochemical beam is formed by inserting a separator between at least one positive electrode and at least one negative electrode.

[0069] The electrochemical bundle according to the invention is formed by the spiral winding of at least one positive electrode and at least one negative electrode separated by a separator.

[0070] The electrochemical bundle is wound so that the external face of the spiral, facing the container, is formed by the positive electrode. Thus, the positive electrode is located opposite the lithium sheet covering at least partially the internal face of the container. [Fig.l] is a schematic representation of an element (1) according to the invention comprising a positive electrode (a) and a negative electrode (b) wound together in the form of a spiral and a lithium sheet (c) covering the internal face of the container (d). The separator, although present in the element, is not shown here, for the sake of ease of understanding.

[0071] The diameter of the spiral electrochemical beam can be between 10 and 50 mm, preferably between 20 and 35 mm, or between 25 and 30 mm, advantageously the diameter is 30 mm. The diameter of the electrochemical beam is dependent on the diameter of the container. Thus, it must be adapted according to the format chosen by the person skilled in the art. Formats A to F can be used.

[0072] Generally speaking, “standard” primary lithium type elements used at room temperature are limited by the capacity of the negative electrode, i.e. the ratio between the capacity of the negative electrode and the capacity of the positive electrode is less than 1.

[0073] However, this type of element is not suitable for high temperature applications, for example from 150°C, due to the increased self-discharge of the negative lithium electrode caused by these high temperatures. To compensate for this loss of lithium, it is expected that the lithium is present in excess and consequently that the element is limited by the capacity of the positive electrode.

[0074] Thus, in the context of certain applications of the element according to the invention at a temperature above 150°C, the ratio between the capacity of the negative electrode and the capacity of the positive electrode is reversed and is therefore greater than 1.

[0075] According to one embodiment, the element according to the invention has a discharge efficiency greater than or equal to 70%, or greater than or equal to 72%, or greater than or equal to 73%, or greater than or equal to 74%, or greater than or equal to 75% or greater than or equal to 76%, or greater than or equal to 77%, or greater than or equal to 78%; the efficiency being defined as the ratio between the actual capacity discharged by the element at a rate less than or equal to C / 120 at a temperature of 200°C and the theoretical (calculated) capacity of the positive electrode and of the negative electrode having the lowest capacity, C being the nominal (theoretical) capacity of the element.

[0076] Manufacturing process

[0077] The method of manufacturing the element according to the invention comprises at least the following steps: a. Plating the lithium or lithium-based alloy sheet against the internal face of the container, so that the entire surface of the lithium sheet faces the last turn of the electrochemical bundle, formed by the positive electrode; b. Formation of the electrochemical beam in the form of a spiral, preferably using a spiralizer; c. Introduction of the electrochemical beam into the container obtained in step a); d. Making the electrical connection between the negative electrode and the negative current output terminal of the element and making the electrical connection between the positive electrode and the positive current output terminal of the element. Generally, the container is at the negative electrode potential and a boss located on the cover of the element is at the positive electrode potential; e. Assembling a lid on the container, for example by laser welding; f. Filling the cell with the electrolyte; g. Closing the element.

[0078] According to one embodiment, in step f), the cover may comprise a filling hole through which the electrolyte is introduced. Once the electrolyte has been introduced, this filling hole is closed in step g) by a stainless steel ball via electrical welding of the ball to the hole.

[0079] EXAMPLES

[0080] 1) Two prototype elements AO and AP were prepared. Each of them comprises a negative electrode made of LiMg alloy with 75% by weight of lithium and a positive electrode of CFV type. The electrochemical bundle is spiraled in an identical manner in both the AO and AP prototype elements, and the capacity of these two elements is limited by the quantity of CF> constituting the positive electrode. The AO prototype differs from the AP prototype according to the invention by the absence of the lithium foil plated on the internal face of the container and by the fact that the length of the negative electrode of the electrochemical bundle is extended by 10% compared to the length of the negative electrode of the electrochemical bundle of the AP element according to the invention. The discharge results at 200°C of these two prototypes are presented in Table 1 below.

[0081] [Tab. 1] AO element Element according to the invention AP Li sheet plated on the internal face of the container no yes Capacity Li electrochemical bundle 18.9 Ah 14 Ah Capacity Li plated - 2.9 Ah Total capacity negative electrode 18.9 Ah 16.9 Ah Capacity CF^ 17.1 Ah 15.7 Ah Theoretical battery capacity 17.1 Ah 15.7 Ah Capacity discharged under 11.5 Ah 11.4 Ah 0.135A at 200°C Efficiency 67% 73% Electrochemical beam diameter 30 mm 29 mm

[0082] [Fig. 2] represents the discharged capacity of the AO and AP elements during a discharge at the C / 125 regime for the AO prototype or C / 1 16 for the AP prototype, at 200°C under 135 mA after 48 h of storage at 150°C. It is observed that although the theoretical capacity of the AP element according to the invention (15.7 Ah) is lower by 9% compared to that of the AO element (17.1 Ah), the discharged capacity under 135 mA at 200°C is almost identical since it is respectively 11.4 Ah and 11.5 Ah. This means that with a smaller quantity of CFV and lithium, the AP element according to the invention makes it possible to obtain a discharged capacity identical to that of the AO element comprising more CF> and lithium.

[0083] Consequently, the discharge efficiency is higher in the case of the element according to the invention (73% vs 67%).

[0084] The lithium foil plated against the inner face of the container allows the outer face of the positive electrode to operate, which forms the last turn of the spiral of the electrochemical beam. Thus, the positive electrode operates more homogeneously.

[0085] Other prototypes (AO, AR1, AQ1, AP3) were designed according to the following characteristics: - Negative electrode in LiMg alloy with 75% lithium by weight; - Positive electrode in CFV; - Separator: either 2 separators of 380 pm thickness (prototypes AR1, AQ1), or 4 separators including 2 of 230 pm thickness and 2 of 102 pm thickness (prototypes AO, AP3).

[0086] [Tab. 2] Element with +10% negative electrode length Element according to the invention Prototype name Proto AO Proto AR1 Proto AQ1 Proto AP3 Separator 4 separators 2 separators 2 separators 4 separators Plated lithium foil No No Yes Yes Discharge temperature (in °C) 200 200 200 200 Total negative electrode capacity (Ah) 18.9 19.5 17.0 16.9 Theoretical cell capacity (Ah) 17.1 17.1 14.9 15.7 Actual discharged capacity (Ah) 11.5 11.3 11.3 11.4 Efficiency 67% 66% 76% 73%

[0087] [Fig.3] represents the discharged capacity of the elements AO, AR1, AP3 and AQ1 during a discharge at 200°C under 135 mA after 48 h of storage at 150°C of these elements.

[0088] Comparing AP3 and AO on the one hand and AQ1 and AR1 on the other hand allows us to conclude that a significantly higher efficiency is obtained with the element according to the invention (76% vs 66% and 73% vs 67%). This significant increase in efficiency is due to the presence of the lithium sheet plated against the internal face of the container.

[0089] Consequently, the alternative solution consisting of extending the length of the negative electrode by 10% to compensate for the fact that the outer turn constituted by the positive electrode is only opposite a single anode turn does not make it possible to solve the technical problem of the invention which is to optimize the work of the positive electrode.

Claims

Claims

1. Electrochemical element comprising a cylindrical container comprising an electrochemical bundle, said electrochemical bundle being in the form of a spiral formed by the winding of the superposition: - of a positive electrode comprising an active material chosen from SOCl2, SO2, SO2C12; CF^with x<1.5; MnO2, FeS2, V2O5,12, Bi2O3, Bi2Pb2O5, CuCl2, CuF2, CuO, Cu4O(PO4)2, CuS, FeS, MoO3, Ni3S2, AgCl, Ag2CrO4, V2O5, SVO, MO6S8, and a mixture of several of these; - of a separator; - of a negative electrode comprising an active material made of lithium metal or of a lithium-based alloy; characterized in that the external face of the spiral, facing the container, is formed by the positive electrode; and that a lithium or lithium-based alloy sheet occupies at least 75% of the circumference of the container.

2. An electrochemical element according to claim 1, wherein the lithium or lithium-based alloy sheet occupies at least 95% of the circumference of the container.

3. Electrochemical element according to any one of the preceding claims, in which the active material of the positive electrode is chosen from CFV with x < 1.5; MnO2, SOCl2, SO2, FeS2.

4. Electrochemical element according to any one of the preceding claims, in which the active material is of CFV type with x < 1.

5.

5. An electrochemical element according to any preceding claim, wherein the active material of the negative electrode is a lithium-based alloy of formula LiM, where M is selected from the group consisting of Mg, Al, Si, B, Ge, Ga or a mixture of several thereof.

6. Cl. An electrochemical element according to any preceding claim, wherein the active material of the negative electrode is a LiMg type alloy.

7. An electrochemical element according to any preceding claim, wherein the element is of the LiMg / CFv type with x < 1.

5.

8. An electrochemical element according to any preceding claim, wherein the active material of the negative electrode of the spiral is arranged on both sides of a current collector.

9. An electrochemical element according to any one of the preceding claims, wherein the thickness of said lithium or lithium-based alloy sheet covering the inner face of the container represents at most 75% or at most 50% or at most 25% of the thickness of the active material of the negative electrode of the spiral.

10. An electrochemical element according to any preceding claim, wherein the ratio of the capacity of the negative electrode to the capacity of the positive electrode is greater than 1.

11. An electrochemical element according to any one of the preceding claims, having a discharge efficiency greater than or equal to 70%, the efficiency being defined as the ratio between the capacity discharged by the element at a rate less than or equal to C / 120 at a temperature of 200°C and the theoretical capacity of the positive electrode or the negative electrode having the lowest capacity.

12. Electrochemical element according to any one of the preceding claims, in which the diameter of the spiral is between 10 and 50 mm, preferably between 20 and 35 mm.

13. Use of the electrochemical element as defined according to any one of claims 1 to 12, in storage, charging or discharging at a temperature of at least 150°C.

14. A method of manufacturing an electrochemical element as defined according to one of claims 1 to 12, comprising at least the following steps: a. Plating the lithium foil or lithium-based alloy against the inner face of the container, so that the entire surface of the lithium foil faces the last turn of the electrochemical bundle formed by the positive electrode; b. Forming the electrochemical bundle in the form of a spiral; c. Introducing the electrochemical bundle into the container obtained in step a); d. Making the electrical connection between the negative electrode and the negative current output terminal of the element and making the electrical connection between the positive electrode and the positive current output terminal of the element; e. Assembling a cover on the container; f. Filling the element with an electrolyte; g. Closing the element.