REFLECTIVE GLAZING INCLUDING A LAYER OF CHROME.

A layer stack of silicon oxide, chromium, and silicon nitride with a thin metal layer addresses corrosion and color issues in reflective glazings, ensuring high reflection and low transmission post-thermal treatment.

FR3135456B1Active Publication Date: 2024-10-18SAINT GOBAIN VITRAGE SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FR2022004559
Authority / Receiving Office
FR · FR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-05-13
Publication Date
2024-10-18
Estimated Expiration
2042-05-13

AI Technical Summary

Technical Problem

Existing reflective glazings with high metallic reflection and low light transmission suffer from corrosion and color changes during thermal treatments like quenching, leading to unsightly pinholes and undesirable color shifts.

Method used

A stack of layers comprising silicon oxide, chromium, silicon nitride, and a thin layer of titanium, zirconium, or silicon, deposited via magnetron-assisted cathode sputtering, provides high corrosion resistance and maintains neutral color after thermal treatments.

Benefits of technology

The solution ensures high reflection and low transmission while preventing corrosion and maintaining color neutrality, suitable for architectural applications.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Reflective glazing suitable for withstanding heat treatment, in particular annealing, bending and / or tempering, said glazing comprising a glass substrate and a stack of layers including a layer comprising silicon oxide of thickness between 15 and 35 nm, a metallic layer based on chromium Cr of thickness between 45 and 65 nm, a layer comprising silicon nitride of thickness greater than 20 nm and less than 30 nm and a layer consisting essentially of a metal selected from titanium, zirconium, silicon or mixtures thereof, of thickness greater than 1 nm and less than 3 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: REFLECTIVE GLAZING COMPRISING A CHROMIUM LAYER.

[0001] The present invention relates to a glazing comprising a stack of layers of metallic appearance reflecting visible light and capable of withstanding heat treatments of the annealing, bending and thermal toughening type.

[0002] Such glazing comprises on a glass substrate a coating comprising an essentially metallic layer reflecting a major part of the visible light, most often made of silver or alternatively another metal such as chromium. Most often this reflective layer is encapsulated in the stack by dielectric materials to protect it from corrosion.

[0003] Glazings coated with such a stack of layers having this basic structure are known in various embodiments. In other cases of use, for example for the cladding of walls or facades, for aesthetic reasons, the emphasis is placed here more on the reflective properties of the stack of layers. In many cases, a metallic-looking reflection is desired, but a reduced reflection with very reduced light transmission is often preferred.

[0004] Glazings with a high metallic reflection and a relatively low light transmission are thus very decorative. In architecture, they are often used for cladding walls, facades (as glazing or facade paving) as mirror elements, as semi-transparent mirrors or as decorative glass plates. They can also be provided with an additional decorative print and are most often used in toughened and / or curved (bent) form. If they are used as monolithic glass panes, the surface layer is exposed to the atmosphere without any protection, so that it must have a particularly high resistance capacity to atmospheric influences but also sufficient scratch resistance, which is essential in particular for cleaning operations.For safety reasons and / or to increase their bending and impact resistance, coated glass substrates intended for these applications are conventionally prestressed by thermal toughening, i.e. heated to a temperature above 500°C, 550°C or even 600°C and then very quickly cooled. The reflective thin-film stack described above must be able to overcome this thermal stress without damage. In particular, the aesthetic, optical, and even thermal or energy properties of coated glass glazing must not be affected by this. In particular, it is important that these glazings retain relatively neutral colors after such tempering, on the side of the uncoated glass face (called the glass-side face) but also on the side of the stack of layers (called the stack-side face), that the chemical and physical resistance is sufficient to withstand external aggressions. Importantly, it is also essential that the tempering operations do not result in the appearance of corrosion points (often called pinholes in the field).

[0005] The applicant company has already described, in publication EP 0 962 429 A1, a semi-transparent glazing with a light transmission of between 2 and 4% having a high thermal resistance. In the case of this known stack of layers, the dielectric base layer is composed of a material based on SiO2, Al2O3, SiON, Si3N4 or AIN or a mixture of at least two of these materials. Among all these materials, it is indicated in paragraph

[0028] that the use of a silicon nitride base layer is to be preferred because it protects the chromium layer better than another layer such as silicon oxide.

[0006] The upper layer according to this publication may be based on silicon, silicon nitride or aluminum nitride. It is indicated in this publication that the thickness of this layer is between 2 and 20 nm, so as to limit the color in reflection of the glazing, in particular on the coating side.

[0007] New glazings are now being sought having a light transmission that is significantly lower than that which is the subject of EP 0962 429, and in particular less than 1%, or even less than 0.5%. To obtain such glazings, the applicant company has carried out a thickening of the chromium layer, on the basis of the stacks described in this publication. Such thickening leads to a reduction in light transmission but also to an increase in the visibility of defects such as corrosion points as described later in the examples.

[0008] The invention thus aims to develop a glazing having a light reflection Rl of the glass greater than 45% and preferably greater than 50% and a light transmission TL less than 1%, and preferably less than 0.5%, and comprising a stack of reflective layers of metallic appearance, having high corrosion resistance and high thermal stability, such that it can withstand heat treatment at a temperature greater than 500°C, in particular toughening, bending or the like, without the appearance of corrosion points (pinholes) and whose coloring is substantially neutral in reflection on the glass side (a* and b* less than 5 in absolute value and if possible negative in the Lab system) and very little colored on the stack side (in particular a value of b* less than or equal to 6 to avoid too marked a yellow coloring), after said heat treatment.

[0009] More particularly, the present invention relates to a reflective glazing capable of withstanding heat treatment, in particular of the annealing, bending and / or toughening type, said glazing comprising a glass substrate and a stack of layers deposited on one of the faces of said glass substrate, said stack successively comprising, from the surface of said substrate:

[0010] - a layer comprising silicon oxide with a thickness of between 15 and 35 nm,

[0011] - a metallic layer based on chromium Cr, with a thickness of between 45 and 65 nm,

[0012] - a layer comprising silicon nitride, with a thickness greater than 20 nm and in less than 30 nm,

[0013] - a layer consisting essentially of a metal chosen from titanium, zirconium, silicon or their mixtures, with a thickness greater than 1 nm and less than 3 nm.

[0014] According to preferred but non-limiting embodiments of the present invention, which can of course be combined with each other if necessary:

[0015] - The metallic layer consists essentially of chromium.

[0016] - The metal layer consists of an alloy of chromium with at least one other metallic element, in which chromium represents more than 50% by weight of said alloy, said at least one element preferably being chosen from Al and / or Si.

[0017] - The metal layer is made of a CrAl alloy preferably comprising 20-25 wt% Al, a CrSi alloy with 15-49 wt% Si, or a CrAISi alloy with 70-80 wt% Cr.

[0018] - The layer comprising silicon oxide has a thickness of between 21 and 29 nm.

[0019] - The chromium-based metal layer has a thickness of between 50 and 60 nm.

[0020] - The layer comprising silicon nitride has a thickness of between 21 and 28 nanometers, preferably between 21 and 25 nm.

[0021] - The stack comprises only one chromium-based layer.

[0022] - The stack does not include silver or gold layers.

[0023] - The stack does not include any metal layers other than those based on chromium.

[0024] - The layer comprising silicon oxide is directly in contact with the surface of the glass substrate and directly in contact with the chromium-based layer.

[0025] - The chromium-based layer is directly in contact with the layer comprising silicon nitride.

[0026] - The layer consisting essentially of titanium, zirconium or silicon is di- directly in contact with the layer comprising silicon nitride.

[0027] - The layer consisting essentially of titanium, zirconium or silicon is the last layer of the stack.

[0028] - said stack only comprises the layer comprising silicon oxide, the chromium-based layer, the layer comprising silicon nitride and the layer consisting essentially of a metal chosen from titanium, zirconium, silicon or mixtures thereof.

[0029] - The light transmission of said coated glazing is less than 1%, preferably is less than 0.5%.

[0030] - The light reflection of the uncoated side of the stack is greater than 45%, preference greater than 50%.

[0031] - The stack of layers is in the form of a discontinuous coating, of the decorative type or frame.

[0032] - A layer of opaque color, in particular of the paint or enamel type, covers the areas of the glazing free from stacking.

[0033] - Said glazing is annealed, curved and / or tempered.

[0034] -said glazing is monolithic.

[0035] The layer comprising silicon nitride comprises mainly silicon and nitrogen as main constituents. In particular, silicon and nitrogen together represent more than 50%, more than 60% or even more than 70% or even more than 80% of the atoms present in a layer, or even more than 90% of the atoms present in a layer. Preferably, said layers comprising silicon nitride are essentially composed of silicon and nitrogen and optionally of at least one element chosen from aluminum, boron or zirconium, preferably aluminum, apart from unavoidable impurities. Said layers comprising silicon nitride are in principle free of oxygen apart from unavoidable impurities, for example they comprise less than 5 mol% of elemental oxygen, in particular less than 1 mol% of elemental oxygen.Preferably, said layer has an N / Si ratio greater than 1.25 and are stoichiometric or substantially stoichiometric layers, preferably substantially stoichiometric. By "stoichiometric" is meant that the N / Si ratio is equal to 1.33 for these silicon-based nitride layers, corresponding to the Si3N4 compound. By "substantially stoichiometric" is meant, for example, that the measured value for this Si3N4 compound differs by less than 5% from this theoretical value.

[0036] Indeed, it should be noted that the layers comprising silicon nitride according to the invention are obtained by a magnetron-assisted cathode sputtering process from a metallic silicon target which may comprise a minor quantity of another element such as aluminium and / or zirconium, for example around of 8 atomic% aluminum, in a reactive atmosphere containing nitrogen. In such a case, the N / Si ratio can vary significantly from the theoretical value 1.33 (= 4 / 3) (corresponding to the defined compound Si3N4) taking into account the stoichiometries of the defined compounds AIN and Si3N4. For example, for a layer of silicon nitride comprising a little aluminum, obtained with the target described above (8% aluminum), the N / Si ratio of the stoichiometric layer theoretically corresponds to a formulation: 92% (SiNl,33) / 8% (AIN) or an N / Si ratio of 1.41 (based on a theoretical formula 0.92 SiNl,33 0.08 AIN, or a ratio: N / Si = [(0.92x1.33+0.08x1 ) / (0.92)] = 1.41).

[0037] Similarly, the layer comprising silicon oxide mainly comprises silicon and oxygen as main constituents. In particular, silicon and oxygen together represent more than 50%, more than 60% or even more than 70% or even more than 80% of the atoms present in a layer, or even more than 90% of the atoms present in a layer. Preferably, said layers comprising silicon oxide are essentially made up of silicon and oxygen and optionally of at least one element chosen from aluminum, boron or zirconium, preferably aluminum, apart from unavoidable impurities.The layers comprising silicon oxide according to the invention are obtained by a magnetron-assisted cathode sputtering process from a metallic silicon target which may comprise a minor quantity of another element such as aluminium and / or zirconium, for example around 8 atomic% of aluminium, in a reactive atmosphere containing oxygen. In particular, the silicon target is the same as that used to obtain the silicon nitride layer described above.

[0038] The reflective functional layer is based on chromium. It is preferably composed essentially of chromium, or even consists of chromium, with the exception of unavoidable impurities. It may alternatively be based on an alloy comprising mainly chromium, in particular more than 50% chromium by weight, preferably more than 60% by weight, or even more than 70% by weight or even more than 80% by weight and very preferably more than 90% by weight of chromium. This is in particular a binary chromium-aluminium alloy CrAl, with a mass content of 10% to 40% of aluminium, in particular 20 to 25% by weight of aluminium. It is also a chromium-silicon alloy, Cr-Si, with preferably at least 5 to 10% by weight of silicon, in particular between 5 and 49% by weight of silicon. It may also be a three-component alloy such as the Cr-Al-Si alloy, preferably comprising at least 60% by weight of chromium, in particular between 70 and 80% by weight of chromium.

[0039] The upper layer of metal with a thickness greater than 1 nm and less than 3 nm consists essentially of a metal chosen from Ti, Zr, Si or their mixtures. preferably the thickness of this layer is between 1.5 nm and 2.5 nm. For example, the atomic sum of these three elements can represent more than 90%, or even more than 95% of the atoms in the layer (except oxygen). Preferably the layer consists essentially of Ti. During a heating step such as quenching, bending or annealing, this layer is at least partially oxidized to the corresponding oxide. Thus, a layer of Ti is ultimately present in the stack in the form of TiOx, after quenching.

[0040] The stacks of layers according to the invention make it possible to meet to a large extent all of the above-mentioned requirements, the desired result being produced by the combined action of the different layers of the stack.

[0041] The glazing according to the invention is constituted by a glass substrate on which the layers of the stack are deposited and is said to be “bendable” and / or “toughenable”, that is to say that they can undergo such a heat treatment without significant modification of their appearance (in particular in terms of corrosion and colorimetry).

[0042] The layer stacks according to the invention are advantageously deposited on the glass substrates according to the known reactive cathode sputtering processes assisted by a magnetic field in industrial continuous coating installations. The coated glazings can then be subjected to a usual toughening process, without the layer stack significantly losing its desired optical and aesthetic properties, in particular its colors in reflection.

[0043] After the deposition of the stack of layers according to the invention, an additional layer, for example a continuous color layer, in particular opaque, can be applied to the coated side, possibly for aesthetic purposes or to manufacture opaque glazing of the spandrel type. This layer can also be made of paint or enamel, obtained by firing an enameling composition in a known manner. In this case, the firing operation can advantageously be linked to the operation of annealing, bending or tempering the glass substrate carrying the stack. The two operations can thus be concomitant.

[0044] The invention and its advantages are illustrated by the following examples: Reference example (according to EP0962429)

[0045] The reference example is example 4 of the prior publication EP0962429 A1, which describes the following glazing:

[0046] Glass - 15 nm Si3N4 - 35 nm Cr - 3 nm Si3N4 - 3 nm Ti, where the Ti is, after quenching, at least partially oxidized to titanium oxide TiOx. Example 1 (comparative)

[0047] In this example, a glazing identical to the reference example is synthesized but in which the thickness of the chromium layer is increased to 55 nm.

[0048] The conditions for depositing the stack are as follows:

[0049] On an industrial vacuum coating installation, 4 mm thick Planiclear™ clear float glass substrates are coated using a conventional magnetic field-assisted cathode sputtering process to obtain the following layer stack:

[0050] Glass - 15 nm Si3N4 - 55 nm Cr - 3 nm Si3N4 - 3 nm Ti

[0051] The SiO2 layer is sputtered in DMS mode (Dual-Magnetron-Sputter mode), with two cathodes and an alternating current under a reactive atmosphere from a Si target with a working gas composed of Ar / O2, and the Si3N4 layer under a reactive atmosphere from a Si target with a working gas composed of Ar / N2, according to techniques well known in the field. The Cr layer is obtained by sputtering a target made of Cr in an atmosphere made of argon. The upper Ti layer is obtained by sputtering a target made of Ti in an atmosphere made of argon. Example 2 (comparative)

[0052] In this example, the thickness of the silicon nitride layer deposited above the chromium layer was increased:

[0053] The procedure is the same as for example 1 to obtain the following glazing:

[0054] Glass - 22 nm Si3N4- 55 nm Cr - 23 nm Si3N4- 2 nm Ti Example 3 (according to the invention)

[0055] In this example, the procedure is the same as for example 1 to obtain the following glazing:

[0056] Glass - 22 nm SiO2 - 55 nm Cr - 23 nm Si3N4 - 2 nm Ti Example 4 (comparative)

[0057] In this example, the procedure is the same as for example 1 to obtain the following glazing:

[0058] Glass - 22 nm SiO2 - 55 nm Cr - 23 nm Si3N4 - 3 nm Ti Example 5 (comparative)

[0059] In this example, the procedure is the same as for example 1 to obtain the following glazing:

[0060] Glass - 22 nm SiO2 - 55 nm Cr - 23 nm Si3N4 - 1 nm Ti Example 6 (comparative)

[0061] In this example, the procedure is the same as for example 1 to obtain the following glazing:

[0062] Glass - 22 nm SiO2 - 55 nm Cr - 30 nm Si3N4 - 2 nm Ti Example 7 (comparative)

[0063] In this example, the procedure is the same as for example 1 to obtain the following glazing:

[0064] Glass - 22 nm SiO2 - 55 nm Cr - 23 nm Si3N4

[0065] The glazing thus coated is thermally toughened in an industrial toughening installation, by heating to a temperature of approximately 650°C and rapid cooling by blowing cold air using standard techniques.

[0066] The glazing is then subjected to the following tests to determine its resistance to toughening and its potential use:

[0067] - Optical quality: The measurement of the transmission of the layer system in the visible spectral region TL, of the reflection in the visible spectral region RL (according to the illuminant D65) according to the ISO9050 (2003) standard. The coordinates a* and b* are determined in the colorimeter system (L, a*, b*) CIELAB. - Mechanical resistance: the scratch resistance of the coatings was measured using a SCRATCH HARDNESS TESTER 413 device supplied by the company Erichsen according to the following protocol: The sample is mounted on a rotary table (number of revolutions in the standard version: 5 min '). The test tool is attached to a load arm with an adjustable weight that allows the pressure of the tool to be adjusted to the sample (load range from 0 to 10 N). The resistance of the sample to this effect is visually assessed using the scratch track. The sample is considered suitable for sale if there are no visible scratches with a load of 1 N and low visibility of scratches at 3 and 5 N. - Quenching corrosion test: the number of corrosion points is visually observed after quenching. 3 levels of occurrence are defined:

[0068] ++: very numerous corrosion points (pinholes)

[0069] +: some visible corrosion points

[0070] 0: no visible corrosion points

[0071] The results of the tests carried out for the evaluation of the properties of the layers are collected in the following Table I, in which the results of the tests on the coated glazings after the toughening treatment are reported.

[0072] [Tables 1] Test performed Example reference Ex. 1 (comp.) Ex. 2 (comp.) Ex. 3 (inv.) Ex. 4 (comp.) Ex. 5 (comp.) Ex. 6 (comp.) Ex. 7 (comp.) Test Scratch EST NM Pass Pass Pass Pass Pass Scratch s Pass Scratch s Light transmission Glazing 3.5* 0.1 0.1 0.1 0.1 0.1 0.1 0.1 Light reflection Stack side 58* 60 50 52 52 52 45 53 Glass side 45* 50 46 55 55 56 53 54 Color coordinate a* Stack side -0.2* -1.5 -2.0 -1.5 -2.1 -1.9 -1.9 -1.9 Glass side -2.9* -2.0 -2.1 -2.0 -1.9 -1.9 -1.9 -1.8 Color coordinate b* Stack side 2.0* -0.3 8.5 6.0 9.8 5.8 12 5.5 Glass side 0.1* -1.0 0.5 -3.4 -2.4 -2.4 -2.4 -2.4 (corrosion points) pinholes Occurrence NM ++ + 0 0 0 0 0

[0073] *data EP0962429 NM: not measured

[0074] The results of the tests show that the stability of the stack, in particular its level of corrosion and its colorimetry, is not affected by the thermal hardening treatment described previously only for example 3 according to the invention, that is to say in which the thicknesses and the materials used in the stack are selected according to the criteria defined previously, and as reported in the claims which follow.

[0075] In detail, it can be seen in the preceding table that the use of a silicon oxide layer below the chromium layer is much more effective in preventing the appearance of corrosion points of the "pinholes" type. Without linking such an observation to any theory, it is possible that such defects were already present in example 4 of EP0962429 with a chromium thickness of 35 nm as described in the comparative example but were not visually detectable, due to a TL greater than 2%. Thus, comparative examples 1 and 2, which include a silicon nitride-based underlayer, exhibit such defects, unlike the layers whose underlayer is based on silicon oxide. Comparative example 1 shows in particular that the thickening of the chromium layer in the example according to EP 0962429 leads to the visual appearance of a large number of corrosion points, making such a product unsaleable.Comparative example 2 also shows that a thicker undercoat based on silicon nitride leads to a marked and undesirable yellow appearance of the glazing in reflection on the stack side (b* value much higher than 6).

[0076] Examples 3 to 7, by comparison with examples 1 and 2, unexpectedly show that the combination of an underlayer comprising silicon oxide and an overlayer comprising silicon nitride with a thickness greater than 20 nm makes it possible to effectively prevent the formation of said corrosion points.

[0077] Comparative examples 3 and 5 show the importance of selecting the thickness of the layer between 1 and 3 nm: thus a thickness of 3 nm leads to an undesirable marked yellow appearance of the glazing in reflection on the stack side while a layer of 1 nm does not provide sufficient mechanical strength for the stack.

[0078] Comparison of comparative example 7 with example 3 according to the invention also shows that an additional metallic layer of Ti above the silicon nitride layer in the stack only very slightly modifies the b* value in reflection on the stack side, but only if its thickness does not reach 3 nanometers (comparative example 4).

[0079] Comparative example 6 shows that too great a thickness of the silicon nitride layer above the reflective chromium layer also leads to an undesirable marked yellow appearance of the glazing in reflection on the stack side (b* much higher than 6).

[0080] The substrate provided with the stack of layers is preferably made of glass, and can be used as monolithic glazing or incorporated into a laminated glazing or insulating multiple glazing structure. It can remain transparent or be opacified, and be continuous or have patterns.

Claims

Claims

1. Reflective glazing capable of withstanding heat treatment, in particular of the annealing, bending and / or tempering type, said glazing comprising a glass substrate and a stack of layers deposited on one of the faces of said glass substrate, said stack successively comprising, from the surface of said substrate: - a layer comprising silicon oxide with a thickness of between 15 and 35 nm, - a metal layer based on chromium Cr, with a thickness of between 45 and 65 nm, - a layer comprising silicon nitride, with a thickness greater than 20 nm and less than 30 nm, - a layer consisting essentially of a metal chosen from titanium, zirconium, silicon or their mixtures, with a thickness greater than 1 nm and less than 3 nm.

2. Glazing according to claim 1, in which the metallic layer consists essentially of chromium.

3. Glazing according to claim 1, in which the metallic layer consists of an alloy of chromium with at least one other metallic element, in which the chromium represents more than 50% by weight of said alloy, said at least one element preferably being chosen from Al and / or Si.

4. Glazing according to claim 1, in which the metallic layer consists of a CrAl alloy preferably comprising 20-25% by weight of Al, a CrSi alloy comprising 15 to 49% by weight of Si, or a CrAISi alloy comprising 70-80% by weight of Cr.

5. Glazing according to one of the preceding claims, in which the layer comprising silicon oxide has a thickness of between 21 and 29 nm.

6. Glazing according to one of the preceding claims, in which the chromium-based metal layer has a thickness of between 50 and 60 nm.

7. Glazing according to one of the preceding claims in which the layer comprising silicon nitride has a thickness of between 21 and 28 nanometers, preferably of between 21 and 25 nm.

8. Glazing according to one of the preceding claims in which the stack consists of only one chromium-based layer.

9. Glazing according to one of the preceding claims in which the layer comprising silicon oxide is directly in contact with the surface of the glass substrate and directly in contact with the chromium-based layer.

10. Glazing according to one of the preceding claims in which the chromium-based layer is directly in contact with the layer comprising silicon nitride.

11. Glazing according to one of the preceding claims in which the layer consisting essentially of titanium, zirconium or silicon is directly in contact with the layer comprising silicon nitride.

12. Glazing according to one of the preceding claims in which the layer consisting essentially of titanium, zirconium or silicon is the last layer of the stack.

13. 13. Glazing according to one of the preceding claims in which said stack comprises only the layer comprising silicon oxide, the chromium-based layer, the layer comprising silicon nitride and the layer consisting essentially of a metal chosen from titanium, zirconium, silicon or their mixtures.

14. 14. Glazing according to one of the preceding claims in which the light transmission is less than 1%, preferably less than 0.5%.

15. 15. Glazing according to one of the preceding claims in which the light reflection of the uncoated side of the stack is greater than 45%, preferably greater than 50%.

16. 16. Glazing according to one of the preceding claims, in which the stack of layers is in the form of a discontinuous coating, of the decorative or frame type.

17. 17. Glazing according to the preceding claim, in which an opaque colored layer covers the areas of the glazing free from the stack.

18. 18. Glazing according to one of the preceding claims, characterized in that it is annealed, curved and / or tempered.

19. 19. Glazing according to one of the preceding claims, characterized in that it is monolithic.