Method for manufacturing an acoustically insulating glazed assembly comprising a viscoelastic damping layer

A viscoelastic damping layer composed of acrylic polymer, tackifying agent, and plasticizing agent between glass sheets addresses high noise transmission in tempered glass glazing, improving acoustic attenuation and manufacturing efficiency.

FR3141692B1Active Publication Date: 2024-10-18SAINT GOBAIN VITRAGE SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FR2022011461
Authority / Receiving Office
FR · FR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-11-03
Publication Date
2024-10-18
Estimated Expiration
2042-11-03

AI Technical Summary

Technical Problem

Existing tempered glass glazing in vehicles suffers from high airborne noise transmission due to air turbulence and has complex manufacturing processes, including adhesion issues with PVB layers and reduced mechanical rigidity.

Method used

A method involving a viscoelastic damping layer formed by depositing a latex mixture of acrylic polymer, tackifying agent, and plasticizing agent between two glass sheets, with controlled drying and debubbling steps under specific pressure and temperature conditions to create a glazed assembly with improved acoustic attenuation.

Benefits of technology

The method enhances acoustic insulation by maximizing the loss factor of the viscoelastic damping layer, maintaining transparency and mechanical rigidity while simplifying the manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000024_0000
    Figure 00000024_0000
  • Figure 00000024_0001
    Figure 00000024_0001
  • Figure 00000025_0000
    Figure 00000025_0000
Patent Text Reader

Abstract

The present invention relates to a method for manufacturing a glazed assembly comprising a first sheet of glass, a second sheet of glass, and a viscoelastic damping layer for acoustic attenuation of a vehicle. The viscoelastic damping layer is arranged between the first and second sheets of glass and is in direct contact with the first sheet of glass. The method comprises a first step of depositing a layer of latex onto a first face of the first sheet of glass. The deposition is carried out by gravity-fed latex flow onto the first face from a latex dispenser. The latex comprises an acrylic polymer, a tackifying agent, and a plasticizing agent. Fig 2
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: Method for manufacturing an acoustically insulating glazed assembly comprising a viscoelastic damping layer Field of invention

[0001] The present invention relates to a method for manufacturing a glazed element comprising a viscoelastic damping layer for the acoustic attenuation of a motor vehicle, as well as a glazed element obtained by such a method. In particular, the glazed element may be an opening side glazing of a motor vehicle. State of the art

[0002] It is known to use tempered glass glazing as the opening side glazing of a motor vehicle. However, such glazing has a high transmission of airborne noise caused by the turbulence of an air flow over the glazing when the vehicle is moving.

[0003] For this purpose, document EP2608958 describes a side glazing unit comprising a laminated glass assembly. The laminated glass assembly comprises two superimposed glass sheets and an interlayer. The interlayer comprises two superimposed outer PVB layers, and an inner PVB layer arranged between the two outer layers. The inner layer has higher acoustic damping properties than the two outer layers. Such a glazed element has higher acoustic attenuation properties than those of a glazing unit formed by monolithic tempered glass.

[0004] However, the manufacture of glazing comprising one or more layers of PVB can be complex. For example, the adhesion of a layer of PVB to a sheet of glass requires treatment in an autoclave. In addition, a glazed assembly comprising one or more layers of PVB may have a thickness that is too great for the glazed element to be inserted into a rebate of a vehicle door. Finally, laminated glazing may have less mechanical rigidity than toughened glazing. Statement of the invention

[0005] An aim of the invention is to propose a solution for increasing the acoustic attenuation of a glazed assembly of a vehicle, in particular of a side glazing of a vehicle, while limiting the complexity of its manufacture.

[0006] This aim is achieved within the framework of the present invention thanks to a method of manufacturing a glazed assembly comprising a first sheet of glass, a second glass sheet and a viscoelastic damping layer for sound reduction of a vehicle, the viscoelastic damping layer being arranged between the first glass sheet and the second glass sheet and being in direct contact with the first glass sheet, the viscoelastic damping layer being formed by a material comprising: - at least one acrylic polymer, - at least one tackifying agent, and - at least one plasticizing agent, the process comprising: - a first step of depositing a layer of latex on a first face of the first glass sheet, the deposition being carried out by a flow of a latex by gravity onto the first face by a latex dispenser, the latex comprising the acrylic polymer, the tackifying agent, and the plasticizing agent, so as to form the layer of latex after the flow has stopped, the layer of latex having an average thickness of between 15 μm and 500 μm, - a second stage of drying the latex layer deposited during the first stage, - a third step of superimposing the second sheet of glass on the layer of latex dried during the second step, the second sheet of glass and the layer of dried latex being in direct contact, - a fourth debubbling step, during which the assembly formed by the first glass sheet, by the dried latex layer and by the second glass sheet brought into contact during the third step with the dried latex layer is placed in an enclosure in which the pressure is less than 100 mbar, in particular less than 50 mbar and preferably less than 10 mbar and in which the temperature is between 70°C and 120°C, in particular between 80°C and 100°C and preferably between 85°C and 95°C, the dried latex layer forming, after the fourth step, the viscoelastic damping layer.

[0007] The present invention is advantageously supplemented by the following characteristics, taken individually or in any of their technically possible combinations:

[0008] - a mass fraction of the acrylic polymer(s) in the dry matter of the latex is between 0.21 and 0.62, in particular between 0.21 and 0.51, and preferably between 0.21 and 0.35,

[0009] - a mass fraction of the tackifying agent(s) in the dry matter of the latex is between 0.17 and 0.60, in particular between 0.22 and 0.35, and preferably between 0.22 and 0.26,

[0010] - a mass fraction of the plasticizing agent(s) in the dry matter of the latex is between 0.07 and 0.43, in particular between 0.12 and 0.31, and preferably between 0.16 and 0.26,

[0011] - a mass fraction of the acrylic polymer(s) in the latex is included between 0.20 and 0.60, in particular between 0.20 and 0.50, and preferably between 0.20 and 0.30,

[0012] - a mass fraction of the tackifying agent(s) in the latex is included between 0.20 and 0.70, in particular between 0.25 and 0.40, and preferably between 0.25 and 0.30,

[0013] - a mass fraction of the plasticizing agent(s) in the latex is included between 0.05 and 0.25, in particular between 0.07 and 0.18, and preferably between 0.09 and 0.15,

[0014] - during the first step, the deposition is implemented by a flow of the latex through gravity from a high part of the first face,

[0015] - the tackifying agent comprises a hydrogenated resin and preferably a resin hydrogenated rosin,

[0016] - the acrylic polymer(s) are formed from monomers chosen from the group formed by methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, propyl acrylate, propyl methacrylate, isopropyl acrylate, isopropyl methacrylate, butyl acrylate, butyl methacrylate, isobutyl acrylate, isobutyl methacrylate, tert-butyl acrylate, tert-butyl methacrylate, pentyl acrylate, pentyl methacrylate, isoamyl acrylate, isoamyl methacrylate, hexyl acrylate, hexyl methacrylate, cyclohexyl acrylate, cyclohexyl methacrylate, octyl acrylate, octyl methacrylate, isooctyl acrylate, methacrylate isooctyl, nonyl acrylate, nonyl methacrylate, isononyl acrylate, isononyl methacrylate, isobornyl methacrylate, decyl acrylate, decyl methacrylate, dodecyl acrylate, dodecyl methacrylate, tridecyl acrylate, tridecyl methacrylate,hexadecyl acrylate, hexadecyl methacrylate, octadecyl acrylate, octadecyl methacrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, vinyl formate, vinyl acetate, vinyl propionate, 2-hydroxyethyl acrylate, hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, 2-hydroxypropyl methacrylate, acrylic acid, styrene and acrylonitrile, ,

[0017] - during the first step, the flow is implemented for a duration between 1 minute and 10 minutes, in particular between 3 minutes and 5 minutes,

[0018] - during the first step, the first face is inclined relative to an axis of the gravity at an angle between 5° and 60° and preferably between 10° and 45°,

[0019] - in the second step, the latex layer is dried in an atmosphere having a temperature maintained between 30°C and 60°C, preferably between 35°C and 50°C, for a period of more than 20 minutes, in particular more than 40 minutes and preferably more than one hour,

[0020] - during the second step, a flow of the atmosphere surrounding the latex layer,

[0021] - the second glass sheet is chemically toughened and has a thickness between 0.5 mm and 3 mm,

[0022] - during the third step, the second glass sheet is heated before being contacting with the dried latex layer so that the second glass sheet has a temperature of between 30°C and 45°C at the time of being contacted with the dried latex layer,

[0023] - during the fourth step, the temperature between 70°C and 120°C is maintained for a period of more than 30 minutes and preferably more than 45 minutes,

[0024] - the method comprises a fifth step, in which the glass assembly is dried at a temperature between 70°C and 120°C in an infrared radiation tunnel,

[0025] - during the fifth step, the glass assembly is held in the tunnel at infrared radiation for a duration greater than 10 minutes and preferably greater than 20 minutes,

[0026] - the latex used to form a flow during the first step is reintroduced in a first-stage flow after flowing from the first face.

[0027] Another aspect of the invention is a glazed assembly for a vehicle obtained by a method according to an embodiment of the invention, the glazed assembly comprising a first glass sheet and a second glass sheet superimposed, the glazed assembly comprising a viscoelastic damping layer for acoustic attenuation of the vehicle, the viscoelastic damping layer being formed by a material comprising: - at least one acrylic polymer, - at least one tackifying agent, and - at least one plasticizing agent, the viscoelastic damping layer being arranged between the first glass sheet and the second glass sheet and being in direct contact with the first glass sheet and preferably in direct contact with the second glass sheet.

[0028] Advantageously, the material has a glass transition temperature of between -70°C and 10°C inclusive, in particular between -45°C and 0°C and preferably between -40°C and -20°C.

[0029] Advantageously, the viscoelastic damping layer has a thickness e of between 5 μm and 500 μm, in particular of between 30 μm and 200 μm. Description of figures

[0030] Other characteristics, aims and advantages of the invention will emerge from the following description, which is purely illustrative and non-limiting, and which must be read in conjunction with the appended drawings in which:

[0031] [Fig-1] - [Fig.l] schematically illustrates a method according to one embodiment of the invention,

[0032] [Fig.2] - [Fig.2] schematically illustrates the first step of a method according to an embodiment of the invention,

[0033] [Fig.3] - [Fig.3] illustrates a loss factor of a material of a glazed assembly according to an embodiment of the invention, for different mass fractions of tackifying agent and plasticizing agent of the latex,

[0034] [Fig.4] - [Fig.4] illustrates a real part of a shear modulus G' of a material of a glazed assembly according to an embodiment of the invention, for different mass fractions of tackifying agent and plasticizing agent of the latex,

[0035] [Fig.5] - [Fig.5] schematically illustrates a section of a glazed assembly according to an embodiment of the invention,

[0036] [Fig.6] - [Fig.6] schematically illustrates a glazed assembly according to one embodiment of the invention,

[0037] [Fig.7] - [Fig.7] illustrates a roughness of a first face of a first glass sheet of a glazed assembly are an embodiment of the invention,

[0038] [Fig.8] - [Fig.8] illustrates the acoustic attenuation of three glazed assemblies, including one glazed assembly according to an embodiment of the invention.

[0039] Throughout the figures, similar elements bear identical references. Definitions

[0040] The term "bar" means the unit of absolute pressure, or "absolute bar", for which 0 bar defines absolute vacuum and for which 1 bar is equal to 100,000 pascals.

[0041] The term “latex” means an aqueous colloidal dispersion of polymers, preferably comprising a tackifying agent and / or a plasticizing agent.

[0042] The term "dry matter" of a composition means the elements of the composition obtained when the water is removed from the composition.

[0043] The term "loss factor q" or "tanô loss factor" of a material, the material having a complex Young's modulus, is understood to mean the ratio between the imaginary part E” of the Young's modulus of the material and the real part E' of the Young's modulus of the material. The loss factor q of a material is defined by the international standard ISO 18437-2:2005 (Mechanical vibration and shock — Characterization of the dynamic mechanical properties of visco-elastic materials — Part 2: Resonance method, part 3.2). Preferably, the loss factor q can be defined for a predetermined frequency. In this document, the expression "a material has a first loss factor p greater than a value" means that the material has a first loss factor p greater than the value for at least one frequency chosen from the audible frequency range, i.e. in a frequency range extending between 20 Hz inclusive and 20 kHz inclusive, and preferably between 20 Hz inclusive and 10 kHz inclusive, at 20°C.

[0044] By "a value of the real part E' of the Young's modulus of a material is greater than a value" is meant that a value of the real part E' of the Young's modulus of the material is greater than the value of the real part E' of the Young's modulus of the material for at least one frequency chosen from the audible frequency range, i.e. in a frequency range extending between 20 Hz inclusive and 20 kHz inclusive, and preferably between 20 Hz inclusive and 10 kHz inclusive, at 20°C.

[0045] The real part E' and the imaginary part E' ' of the Young's modulus may be defined for a predetermined temperature. Herein, "the real part E' of the Young's modulus of a material is greater than a value" means that the material has a real part E' of the Young's modulus greater than the value at 20°C. Herein, "a material has a first loss factor q greater than a value" means that the material has a first loss factor q greater than the value at 20°C.

[0046] A shear modulus G can be linked, in particular for an isotropic material, to the Young's modulus E by the relation G=E / 2(l+v), where v is the Poisson's ratio of the material.

[0047] A dynamic characterization of a material can be carried out on a viscoanalyzer of the Metravib viscoanalyzer type, under the following measurement conditions. A sinusoidal stress is applied to the material. A measurement sample formed by the material to be measured consists of two rectangular parallelepipeds, each parallelepiped having a thickness of 3.31 mm, a width of 10.38 mm and a height of 6.44 mm. Each parallelepiped formed by the material is also referred to as a shear “specimen”. The excitation is implemented with a dynamic amplitude of 5 μm around the rest position, covering the frequency range between 1 Hz and 700 Hz, and covering a temperature range between -90°C and +60°C.

[0048] The viscoanalyzer makes it possible to subject each test piece (each sample) to deformations under precise temperature and frequency conditions, and to measure the displacements of the test piece, the forces applied to the test piece and their phase shift, which makes it possible to measure rheological quantities characterizing the material of the test piece.

[0049] The use of the measurements makes it possible in particular to calculate the Young's modulus E of the material, and particularly the real part E' of the Young's modulus and the imaginary part E” of the Young's modulus of the material, and thus to calculate the tangent of the loss angle (or loss factor) q (also designated by tanô).

[0050] A value of the real part E' of the Young's modulus and / or a loss factor p of a material are measured without the material being prestressed.

[0051] The term “light transmission factor” means the factor defined in standard NF EN 410.

[0052] The term "haze factor" is understood to mean the ratio between the intensity of all the light diffused by a passage through the glazed element (diffuse fraction or If) of an angle greater than 2.5° and between the intensity of the light transmitted through the glazed element (If). The haze factor can be measured by spectroscopy techniques. The integration of the intensity over the entire visible range (from 380 nm to 780 nm) makes it possible to determine the normal transmission TL and the diffuse transmission Td. Such a measurement can also be obtained by using a Hazemeter. A glazing is considered to be transparent if its haze factor is less than 10%, in particular less than 5% and preferably less than 1%. The Hazemeter can be a "Haze-Gard®" device marketed by the company BYK-Gardner.

[0053] The term “clarity factor” means the ratio defined by the following formula:

[0054] f_U£(l) J e~ Ic+Ic

[0055] where Ic is the intensity of light after passing through a glazing unit that has not been diffused, and lr is the intensity of light after passing through the glazing unit that has been diffused at a small angle, preferably an angle equal to 15°. The clarity factor can be measured by spectroscopy techniques. Integrating the intensity over the entire visible range (from 380 nm to 780 nm) makes it possible to determine the normal transmission TL and the diffuse transmission Td. Such a measurement can also be obtained by using a Hazemeter. A glazing unit is considered transparent if its clarity factor is greater than 90% and preferably greater than 95%.

[0056] A glass transition temperature Tg of a material, preferably of the first damping layer, can be measured by differential scanning calorimetry (DSC). The glass transition temperature can be determined using the midpoint method as described in ASTM-D-3418 for differential scanning calorimetry. The measuring apparatus used by the applicant is the Discovery DSC model from TA Instruments.

[0057] Preferably, a glass transition temperature Tg is determined by dynamic mechanical analysis (DMA) or dynamic mechanical spectrometry (DMA). The value of Tg is determined by plotting an isofrequency curve of the loss factor as a function of the temperature of the material. The temperature at which the value of the loss factor is maximum is equal to the glass transition temperature Tg. The glass transition temperature depends on the excitation frequency of the material. In this document, the term "glass transition temperature" means the glass transition temperature measured at a frequency of 1 Hz by DMA.

[0058] The term "mass fraction" of a first element in a second element means the ratio of the mass of the first element to the mass of the second element. Detailed description of the invention

[0059] General description of the manufacturing process of a glazed element 1

[0060] With reference to [Fig.l] and [Fig.2], one aspect of the invention is a method 100 for manufacturing a glazed assembly 1. The glazed assembly 1 comprises a first glass sheet 2, a second glass sheet 3 and a viscoelastic damping layer 4 for the acoustic attenuation of a vehicle. The viscoelastic damping layer 4 is arranged between the first glass sheet 2 and the second glass sheet 3 and is in direct contact with the first glass sheet 2 and preferably in direct contact with the second glass sheet 3.

[0061] The viscoelastic damping layer 4 is formed by a material comprising at least one acrylic polymer, at least one tackifying agent, and at least one plasticizing agent.

[0062] The method comprises a first step 101 of depositing a layer of latex 5 on a first face 6 of the first glass sheet 2. The deposition is carried out by a flow of a latex 5 by gravity onto the first face 2, by a distributor 7 of latex 5. The latex 5 comprises the acrylic polymer, the tackifying agent, and the plasticizing agent. The flow of latex is carried out so as to form the layer of latex after the flow on the first face 6 has stopped. The layer of latex has an average thickness of between 15 μm and 500 μm. Preferably, the deposition is carried out by a flow of the latex by gravity from an upper part of the first face. By "upper part" is meant a part of the first face 6 arranged at a height greater than another height of the rest of the first face 6.

[0063] The method 100 comprises a second step 102 of drying the latex layer 5 deposited during the first step 101.

[0064] The method 100 comprises a third step 103 of superimposing the second glass sheet 3 on the dried latex layer during the second step 102. The second glass sheet 3 and the dried latex layer are brought into direct contact.

[0065] The method 100 comprises a fourth debubbling step 104. During the debubbling step, the assembly formed by the first glass sheet 2, by the dried latex layer and by the second glass sheet 3 brought into contact during the third step 103 with the dried latex layer is placed in an enclosure 8 in which the pressure is less than 100 mbar, in particular less than 50 mbar and preferably less than 10 mbar and in which the temperature is between 70°C and 120°C, in particular between 80°C and 100°C and preferably between 85°C and 95°C. The dried latex layer forms, after the fourth step 104, the viscoelastic damping layer 4.

[0066] Thus, due to the composition of the latex, due to the thickness of the deposited latex layer and due to the pressure and temperature treatment of the latex layer in the method, it is possible to manufacture a viscoelastic damping layer 4 for the acoustic attenuation of a vehicle having optical properties suitable for vehicle glazing. Preferably, a light transmission factor of the glazed element 1 is greater than 90%. Preferably, a haze factor of the glazed element 1 is less than 1%. Preferably, a clarity factor of the glazed element 1 is greater than 99%. In particular, the third debubbling step is carried out in a temperature range that is on the one hand high enough for the bubbles present in the dried latex layer to be able to be extracted from the dried latex layer and on the other hand small enough for the dried latex layer not to flow from the first glass sheet 2.Furthermore, for the composition of the latex layer previously defined, the thicknesses chosen in the thickness range of the latex layer previously defined are both small enough to maximize the loss factor of the viscoelastic damping layer 4 and allow the transparency of the viscoelastic damping layer 4, and at the same time high enough to overcome the roughness of the first glass sheet 2. Indeed, with reference to [Fig.7], the inventors have discovered that it is necessary to deposit a latex layer having a thickness greater than 15 μm to cover all of the roughnesses presented by the first glass sheet. Preferably, the first face 6 has a first roughness and the thickness of the latex layer is greater than the first roughness.

[0067] First step 101 and latex 5

[0068] The method comprises a first step 101 of depositing a layer of latex 5 on a first face 6 of the first glass sheet 2. The latex 5 comprises an emulsion. The emulsion comprises an aqueous continuous phase and a dispersed phase. The dispersed phase comprises at least one acrylic polymer. The latex comprises also tackifying agent and plasticizing agent. The tackifying agent and plasticizing agent may be in the aqueous phase.

[0069] Acrylic polymer(s)

[0070] The acrylic polymer(s) may be formed from monomers selected from the group consisting of methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, propyl acrylate, propyl methacrylate, isopropyl acrylate, isopropyl methacrylate, butyl acrylate, butyl methacrylate, isobutyl acrylate, isobutyl methacrylate, tert-butyl acrylate, tert-butyl methacrylate, pentyl acrylate, pentyl methacrylate, isoamyl acrylate, isoamyl methacrylate, hexyl acrylate, hexyl methacrylate, cyclohexyl acrylate, cyclohexyl methacrylate, octyl acrylate, octyl methacrylate, isooctyl acrylate, isooctyl methacrylate, nonyl acrylate, nonyl methacrylate, isononyl acrylate, isononyl methacrylate, isobornyl methacrylate, decyl acrylate, decyl methacrylate, dodecyl acrylate,dodecyl methacrylate, tridecyl acrylate, tridecyl methacrylate, hexadecyl acrylate, hexadecyl methacrylate, octadecyl acrylate, octadecyl methacrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, vinyl formate, vinyl acetate, vinyl propionate, 2-hydroxyethyl acrylate, hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, 2-hydroxypropyl methacrylate, acrylic acid, styrene and acrylonitrile.

[0071] The acrylic polymer(s) may be copolymers, formed from at least two monomers chosen from the group formed by the monomers defined above.

[0072] The latex 5 may comprise two different acrylic polymers. One of the two polymers may be 2-ethylhexyl acrylate (2-EHA) and / or butylacrylate (BA). Preferably, one of the two polymers is 2-ethylhexyl acrylate (2-EHA) and the other of the two polymers is butylacrylate (BA). The mass ratio between 2-ethylhexyl acrylate (2-EHA) and butylacrylate (BA) may be between 2 and 4, and is preferably equal to 3.

[0073] A commercial latex comprising an acrylic polymer may be used to form the viscoelastic damping layer 4. For example, it is possible to use Arkema ® Encor 4028, Arkema ® Encor 4517, Alberdingk® AC 75070 or Al-berdingk® AC 75011 latex.

[0074] The latex 5 may comprise another polymer which is not an acrylic polymer. Such another polymer may be formed from at least one monomer selected from styrene and methyl methacrylate.

[0075] The latex 5 may comprise a first acrylic polymer having a first glass transition temperature Tgb and a second polymer, acrylic or non-acrylic, having a second glass transition temperature Tg2, greater than Tgb The difference between the second glass transition temperature Tg2 and between the first glass transition temperature Tgi may be greater than 10°C and preferably greater than 20°C. Thus, it is possible to increase the glass transition temperature of the material forming the viscoelastic damping layer 4 with respect to the glass transition temperature of a material obtained solely with the first acrylic polymer. Indeed, the glass transition temperature obtained solely with the first acrylic polymer may be too small to present maximum damping of the material in an audible frequency range.

[0076] The polymer(s) of the material of the viscoelastic damping layer 4 obtained by the method 100 may form an interpenetrating polymer network (IPN). The latex 5 may comprise polymer particles having a core-shell structure. The core may be formed from an interpenetrating polymer network (IPN) having a glass transition temperature (Tg) of between -50°C and -30°C, preferably between -45°C and -35°C. The shell may be formed from a polymer having a glass transition temperature sufficiently small to allow the coalescence of the particles from the second step 102. The glass transition temperature of the shell may be lower than that of the core, and may preferably be lower than -50°C, and more preferably lower than -60°C. The core formed from an interpenetrating polymer network may be obtained by two sequential polymerizations.The RIP thus comprises a third crosslinked polymer and a fourth polymer, which can be crosslinked or non-crosslinked. If the fourth polymer is non-crosslinked, the RIP is a so-called "semi-interpenetrating polymer network". The fourth polymer can be linear or branched.

[0077] Tackifying agent

[0078] The tackifying agent is adapted to allow bonding by direct contact between the viscoelastic damping layer 4 and the first glass sheet 2 and, preferably, between the viscoelastic damping layer 4 and the second glass sheet 3.

[0079] The tackifying agent may comprise a hydrogenated resin, and preferably a hydrogenated rosin resin. The hydrogenated resin may comprise a glycerol ester of wood resin, preferably abietic acid. The hydrogenated resin may comprise a hydrogenated rosin ester (for example, a resin of the Arakawa ® KE-311 or KE 100 brand).

[0080] Plasticizing agent

[0081] The plasticizing agent is suitable for increasing the plasticity of the viscoelastic damping layer 4. The plasticizing agent may comprise at least one element selected from a citrate, an adipate, a glycol and a triethylene glycol derivative. The citrate may be acetyl tributyl citrate. The adipate may be triethylene glycol bis(2-ethylhexanoate) (e.g. marketed as Celanese® WVC 3800).

[0082] Adjustment of the acoustic properties of the glazed element 1

[0083] A mass fraction of the acrylic polymer(s) in the dry matter of the latex 5 may be between 0.21 and 0.62, in particular between 0.21 and 0.51, and preferably between 0.21 and 0.35. Thus, after drying the latex layer, and in particular after the fourth step 104, the material forming the viscoelastic damping layer 4 may have a mass fraction of the acrylic polymer(s) in the viscoelastic damping layer 4 respectively between 0.21 and 0.62, in particular between 0.21 and 0.51, and preferably between 0.21 and 0.35. Thus, the material forming the viscoelastic damping layer 4 has a tanô loss factor greater than 1. The latex 5 may have a proportion of water such that a mass fraction of the acrylic polymer(s) in the latex 5 is between 0.20 and 0.60, in particular between 0.20 and 0.50, and preferably between 0.20 and 0.30..

[0084] Known materials for sound reduction comprising an acrylic polymer have a frequency y^ for which a value of the loss factor tanô of the material of the viscoelastic damping layer 4 is greater than 50 kHz. This frequency is not included in the audible frequency spectrum, which reduces the sound reduction properties of the glazed element 1.

[0085] A mass fraction of the plasticizing agent(s) in the dry matter of the latex 5 may be between 0.07 and 0.43, in particular between 0.12 and 0.31, and preferably between 0.16 and 0.26. Thus, after drying the latex layer, and in particular after the fourth step 104, the material forming the viscoelastic damping layer 4 may have a mass fraction of the plasticizing agent(s) in the viscoelastic damping layer 4 respectively between 0.07 and 0.43, in particular between 0.12 and 0.31, and preferably between 0.16 and 0.26. Thus, the frequency^, for which the value of the loss factor tanô of the material of the viscoelastic damping layer 4 is maximum is included in the audible frequency spectrum while increasing the value of the loss factor tanô with respect to known materials.The latex 5 may have a proportion of water such that a mass fraction of the plasticizing agent(s) is between 0.05 and 0.25, in particular between 0.07 and 0.18, and preferably between 0.09 and 0.15.

[0086] Indeed, the inventors have discovered that, for a predetermined concentration of acrylic polymer(s), the frequency for which the loss factor is maximum varies in the same direction as the mass fraction of the plasticizing agent in the viscoelastic damping layer 4. The inventors have thus discovered the range of mass fraction of the plasticizing agent in the latex 5 for which the frequency^, is included in the audible frequency spectrum. In addition, the value of the loss factor tanô of the material of the viscoelastic damping layer 4 varies in the same direction as the mass fraction of the plasticizing agent in the latex 5.

[0087] A mass fraction of the tackifying agent(s) in the dry matter of the latex may be between 0.17 and 0.60, in particular between 0.22 and 0.35, and preferably between 0.22 and 0.26. Thus, after drying the latex layer, and in particular after the fourth step 104, the material forming the viscoelastic damping layer 4 may have a mass fraction of the tackifying agent(s) in the first layer respectively between 0.17 and 0.60, in particular between 0.22 and 0.35, and preferably between 0.22 and 0.26. Thus, the frequency^ for which the value of the loss factor tanô of the material of the viscoelastic damping layer 4 is maximum is included in the audible frequency spectrum.Latex 5 may have a proportion of water such that a mass fraction of the tackifying agent(s) is between 0.20 and 0.70, in particular between 0.25 and 0.40, and preferably between 0.25 and 0.30.

[0088] Indeed, the inventors have discovered that, for a predetermined concentration of acrylic polymer(s), the frequency for which the loss factor is maximum varies in the opposite direction to the mass fraction of the tackifying agent in the first layer. The inventors have thus discovered the range of mass fraction of the tackifying agent in the latex 5 for which the frequency^, is included in the audible frequency spectrum. In addition, the value of the loss factor tanô of the material of the viscoelastic damping layer 4 is little dependent on the mass fraction of the tackifying agent in the latex 5.

[0089] With reference to [Fig. 3], curve (a) illustrates a loss factor of a layer different from the viscoelastic damping layer 4, manufactured from an adhesive which does not allow the manufacture of a layer having the optical properties of the viscoelastic damping layer 4, differently from the viscoelastic damping layer 4 obtained by the method 100. Curve (b) illustrates a loss factor of the viscoelastic damping layer 4, the mass fraction of the acrylic polymers being equal to 0.58, the mass fraction of plasticizing agent in the viscoelastic damping layer 4 being equal to 0.08 and the mass fraction of tackifying agent in the viscoelastic damping layer 4 being equal to 0.34. Curve (c) illustrates a loss factor of the viscoelastic damping layer 4, the mass fraction of acrylic polymers being equal to 0.55, the mass fraction in plasticizing agent in the viscoelastic damping layer 4 being equal to 0.12 and the mass fraction of tackifying agent in the viscoelastic damping layer 4 being equal to 0.32. Curve (d) illustrates a loss factor of the viscoelastic damping layer 4, the mass fraction of acrylic polymers being equal to 0.53, the mass fraction of plasticizing agent in the viscoelastic damping layer 4 being equal to 0.16 and the mass fraction of tackifying agent in the viscoelastic damping layer 4 being equal to 0.31. Curve (e) illustrates a loss factor of the viscoelastic damping layer 4, the mass fraction of acrylic polymers being equal to 0.49, the mass fraction of plasticizing agent in the viscoelastic damping layer 4 being equal to 0.09 and the mass fraction of tackifying agent in the viscoelastic damping layer 4 being equal to 0.43.Curve (f) illustrates a loss factor of the viscoelastic damping layer 4, the mass fraction of acrylic polymers being equal to 0.48, the mass fraction of plasticizing agent in the viscoelastic damping layer 4 being equal to 0.10 and the mass fraction of tackifying agent in the viscoelastic damping layer 4 being equal to 0.42. Curve (g) illustrates a loss factor of the viscoelastic damping layer 4, the mass fraction of acrylic polymers being equal to 0.46, the mass fraction of plasticizing agent in the viscoelastic damping layer 4 being equal to 0.14 and the mass fraction of tackifying agent in the viscoelastic damping layer 4 being equal to 0.41.Curve (h) illustrates a loss factor of the viscoelastic damping layer 4, the mass fraction of acrylic polymers being equal to 0.42, the mass fraction of plasticizing agent in the viscoelastic damping layer 4 being equal to 0.09 and the mass fraction of tackifying agent in the viscoelastic damping layer 4 being equal to 0.49.

[0090] With reference to [Fig. 4], curve (i) illustrates a real part G' of the shear modulus of a layer different from the viscoelastic damping layer 4, manufactured from an adhesive which does not allow the manufacture of a layer having the optical properties of the viscoelastic damping layer 4, differently from the interface obtained in the embodiments of the invention. Curve (j) illustrates the real part G' of the shear modulus of the viscoelastic damping layer 4, the mass fraction of the acrylic polymers being equal to 0.58, the mass fraction of plasticizing agent in the viscoelastic damping layer 4 being equal to 0.08 and the mass fraction of tackifying agent in the viscoelastic damping layer 4 being equal to 0.34.Curve (k) illustrates the real part G' of the shear modulus of the viscoelastic damping layer 4, the mass fraction of acrylic polymers being equal to 0.55, the mass fraction of plasticizing agent in the viscoelastic damping layer 4 being equal to 0.12 and the mass fraction . in tackifying agent in the viscoelastic damping layer 4 being equal to 0.32. Curve (1) illustrates the real part G' of the shear modulus of the viscoelastic damping layer 4, the mass fraction of acrylic polymers being equal to 0.53, the mass fraction of plasticizing agent in the viscoelastic damping layer 4 being equal to 0.16 and the mass fraction of tackifying agent in the viscoelastic damping layer 4 being equal to 0.31. Curve (m) illustrates the real part G' of the shear modulus of the viscoelastic damping layer 4, the mass fraction of acrylic polymers being equal to 0.49, the mass fraction of plasticizing agent in the viscoelastic damping layer 4 being equal to 0.09 and the mass fraction of tackifying agent in the viscoelastic damping layer 4 being equal to 0.43.Curve (n) illustrates the real part G' of the shear modulus of the viscoelastic damping layer 4, the mass fraction of acrylic polymers being equal to 0.48, the mass fraction of plasticizing agent in the viscoelastic damping layer 4 being equal to 0.10 and the mass fraction of tackifying agent in the viscoelastic damping layer 4 being equal to 0.42. Curve (o) illustrates the real part G' of the shear modulus of the viscoelastic damping layer 4, the mass fraction of acrylic polymers being equal to 0.46, the mass fraction of plasticizing agent in the viscoelastic damping layer 4 being equal to 0.14 and the mass fraction of tackifying agent in the viscoelastic damping layer 4 being equal to 0.41.Curve (p) illustrates the real part G' of the shear modulus of the viscoelastic damping layer 4, the mass fraction of acrylic polymers being equal to 0.42, the mass fraction of plasticizing agent in the viscoelastic damping layer 4 being equal to 0.09 and the mass fraction of tackifying agent in the viscoelastic damping layer 4 being equal to 0.49.

[0091] The latex 5 may have a mass fraction of the acrylic polymer(s) of between 0.20 and 0.60, a mass fraction of the plasticizing agent(s) of between 0.05 and 0.25 and a mass fraction of the tackifying agent(s) of between 0.20 and 0.70.

[0092] The latex 5 may have a mass fraction of the acrylic polymer(s) of between 0.20 and 0.50, a mass fraction of the plasticizing agent(s) of between 0.07 and 0.18 and a mass fraction of the tackifying agent(s) of between 0.25 and 0.40.

[0093] The latex 5 may have a mass fraction of the acrylic polymer(s) of between 0.20 and 0.30, a mass fraction of the plasticizing agent(s) of between 0.09 and 0.15 and a mass fraction of the tackifying agent(s) of between 0.25 and 0.35.

[0094] Deposit

[0095] With reference to [Fig. 2], the deposition is implemented by a flow of the latex 5 by gravity from the first face 6, by a distributor 7 of latex 5. Thus, it is possible to form a layer of latex on at least a majority of the surface of the first face 6 and preferably on the entirety of the first face 6. The first face 6 can be inclined relative to an axis of gravity 9 at an angle a of between 5° and 60° and preferably of between 10° and 45°. Thus, it is possible to increase the speed of the deposition while avoiding losing a portion of the latex 5 which would not participate in the flow. With reference to [Fig. 7], the first glass sheet 2 can have a thickness of between 3 mm and 5 mm.

[0096] The flow can be carried out for a period of between 1 minute and 10 minutes, in particular between 3 minutes and 5 minutes. The latex 5 can be filtered before the flow by a filter making it possible to eliminate from the flow impurities of a size greater than 90 μm.

[0097] The latex dispenser 7 is adapted to generate a flow of the latex 5 from an outlet of the dispenser 7. The outlet may be point-like. The dispenser 7 may be a pipette, which may be moved along an upper portion of the first face 6 during the first step 101. The outlet may be linear. A linear outlet of the latex dispenser 7 may be arranged to extend along an upper portion of the first face 6.

[0098] The latex 5 used to form a flow during the first step 101 can be reintroduced into a flow of a subsequent first step 101 after having flowed over the first face 6. Indeed, only a portion of the latex 5 of the flow participates in the formation of the latex layer on the first face 6. The remainder of the latex 5 can be reused for the formation of another latex layer.

[0099] Second step 102

[0100] The method comprises a second step 102 of drying the latex layer 5 deposited during the first step 101. The second step 102 allows the extraction of water and any solvents from the latex layer deposited during the first step 101 by evaporation.

[0101] The latex layer can be dried in an atmosphere having a temperature maintained between 30°C and 60°C, preferably between 35°C and 50°C. This temperature range makes it possible to avoid the appearance of bubbles in the latex layer while avoiding the appearance of a crust on the surface of the latex layer, which would prevent the water from evaporating.

[0102] During the second step 102, a flow of the atmosphere surrounding the latex layer can be actuated. The second drying step 102 can be carried out in a ventilated oven. Thus, it is possible to avoid sudden evaporation of the water from the latex layer and thus avoid the formation of a layer 4 cracked viscoelastic damping.

[0103] The latex layer may be dried for a period of more than 20 minutes, in particular more than 40 minutes and preferably more than one hour. Thus, it is possible to evaporate all of the water contained in the latex layer at the end of the first step 101 in the temperature range previously defined for the drying of the second step 102. The temperature range and the drying duration previously defined for the second step 102 make it possible to avoid the formation of a cracked viscoelastic damping layer 4.

[0104] Third step 103

[0105] The method comprises a third step 103 of superimposing the second glass sheet 3 on the dried latex layer during the second step 102. The second glass sheet 3 and the dried latex layer are in direct contact. The second glass sheet 3 may be chemically toughened and have a thickness e2 of between 0.5 mm and 3 mm. Thus, it is possible to flex the second glass sheet 3 when bringing the second glass sheet 3 into contact with the dried latex layer so as to avoid the formation of air bubbles when superimposing the second glass sheet 3 on the dried latex layer.

[0106] During the third step 103, the second glass sheet 3 may be heated before being brought into contact with the dried latex layer so that the second glass sheet 3 has a temperature of between 30°C and 45°C at the time of being brought into contact with the dried latex layer. Thus, it is possible to avoid the cooling of the dried latex layer by the second glass sheet 3 during contacting, which makes it easier to position the second glass sheet 3 on the dried latex layer.

[0107] Fourth step 104

[0108] The method 100 comprises a fourth debubbling step 104. During the fourth step 104, the assembly formed by the first glass sheet 2, by the dried latex layer and by the second glass sheet 3 brought into contact during the third step 103 with the dried latex layer is placed in an enclosure 8 in which the pressure is less than 100 mbar, in particular less than 50 mbar and preferably less than 10 mbar. The temperature in the enclosure 8 is between 70°C and 120°C, in particular between 80°C and 100°C and preferably between 85°C and 95°C. The dried latex layer forms, after the fourth step 104, the viscoelastic damping layer 4. The glazed assembly 1 is formed by the first glass sheet 2, the viscoelastic damping layer 4 and the second glass sheet 3.

[0109] The enclosure 8 may be a flexible pocket formed around the first glass sheet 2, the dried latex layer and the second glass sheet 3.

[0110] During the fourth step 104, the temperature between 70°C and 120°C can be maintained for a period of more than 30 minutes and preferably more than 45 minutes.

[0111] For example, during the fourth step 104, a pressure of less than 10 mbar may first be controlled in the pocket, for a duration greater than 15 minutes. Then, a temperature rise may be controlled between ambient temperature and 90°C for a duration of between 10 minutes and 15 minutes. The temperature of 90°C in the pocket may be maintained for a duration equal to 30 minutes. A temperature drop from 90°C to ambient temperature may be controlled for a duration equal to 30 minutes. The pressure inside the pocket may then be increased so as to reach ambient pressure.

[0112] Fifth step 105

[0113] The method may comprise a fifth step 105 of additional debubbling. During the fifth step 105, the glazed assembly 1 is dried at a temperature of between 70°C and 120°C in an infrared radiation tunnel. The temperature of the glazed assembly 1 in the infrared radiation tunnel is in particular between 80°C and 120°C and preferably between 85°C and 95°C. This step makes it possible to eliminate residual air bubbles in the dried latex layer, which makes it possible to increase the optical quality of the viscoelastic damping layer 4. The glazed assembly 1 may be kept in the infrared radiation tunnel for a period of more than 10 minutes and preferably more than 20 minutes.

[0114] With reference to [Fig.5], another aspect of the invention is a glazed assembly 1 obtained by a method according to an embodiment of the invention. With reference to [Fig.6], the glazed assembly may be a vehicle side glazing. The glazed assembly 1 comprises a first glass sheet 2 and a second glass sheet 3 superimposed. The glazed assembly 1 comprises a viscoelastic damping layer 4 for acoustic attenuation of the vehicle formed by a material comprising at least one acrylic polymer, at least one tackifying agent, and at least one plasticizing agent. The viscoelastic damping layer 4 is arranged between the first glass sheet 2 and the second glass sheet 3 and is in direct contact with the first glass sheet 2, and preferably with the second glass sheet 3. The viscoelastic damping layer 4 has a thickness e of between 5 μm and 500 μm and preferably between 30 μm and 200 μm.

[0115] With reference to [Fig.8], a glazed assembly 1 according to an embodiment of the invention provides a reduction in acoustic attenuation compared to known side glazings, in particular for frequencies between 6500 Hz and 9000 Hz. The curve (p) illustrates the acoustic attenuation of a side glazing formed by a tempered glass sheet having a thickness equal to 3.85 mm. Curve (q) illustrates the acoustic attenuation of a side glazing formed by a laminate comprising two glass sheets, each having a thickness equal to 1.6 mm, separated by an acoustic PVB interlayer film (model RZN-12 of the Sekisui Chemical Co. Ltd brand). Curve (q) illustrates the acoustic attenuation of a glazing formed by a glazed element according to an embodiment of the invention, comprising two glass sheets separated by a viscoelastic damping layer 4. The first glass sheet 2 has a thickness ej equal to 1.6 mm. The second glass sheet 3 has a thickness e2 equal to 1.6 mm. The viscoelastic damping layer 4 has a thickness equal to 100 μm.The material forming the viscoelastic damping layer is formed from a latex 5 comprising 2-ethylhexyl acrylate and butyl acrylate respectively in a mass proportion equal to 3:1.

Claims

Claims

1. A method (100) of manufacturing a glazed assembly (1) comprising a first glass sheet (2), a second glass sheet (3) and a viscoelastic damping layer (4) for sound reduction of a vehicle, the viscoelastic damping layer (4) being arranged between the first glass sheet (2) and the second glass sheet (3) and being in direct contact with the first glass sheet (2), the viscoelastic damping layer (4) being formed by a material comprising: - at least one acrylic polymer, - at least one tackifying agent, and - at least one plasticizing agent, the method comprising: - a first step (101) of depositing a layer of latex (5) on a first face (6) of the first glass sheet (2), the deposition being carried out by a flow of a latex (5) by gravity onto the first face (6) by a latex (5) distributor (7), the latex (5) comprising the acrylic polymer, the tackifying agent, and the plasticizing agent, so as to form the latex layer after the flow has stopped, the latex layer having an average thickness of between 15 μm and 500 μm, - a second step (102) of drying the latex layer (5) deposited during the first step (101), - a third step (103) of superimposing the second glass sheet (3) on the latex layer dried during the second step (102), the second glass sheet (3) and the dried latex layer being in direct contact, - a fourth step (104) of debubbling, during which the assembly formed by the first glass sheet (2), by the dried latex layer and by the second glass sheet (3) brought into contact during the third step (103) with the dried latex layer is placed in an enclosure (8) in which the pressure is less than 100 mbar, and in which the temperature is between 70°C and 120°C, the dried latex layer forming, after the fourth step, the viscoelastic damping layer (4).

2. Method according to the preceding claim, in which a mass fraction of the acrylic polymer(s) in the dry matter of the

3.

4.

5.

6.

7.

8. latex (5) is between 0.21 and 0.

62. Method according to one of the preceding claims, in which a mass fraction of the tackifying agent(s) in the dry matter of the latex (5) is between 0.17 and 0.

60. Method according to one of the preceding claims, in which a mass fraction of the plasticizing agent(s) in the dry matter of the latex (5) is between 0.07 and 0.

43. A method according to any preceding claim, wherein the tackifying agent comprises a hydrogenated resin. A method according to any preceding claim, wherein the acrylic polymer(s) are formed from monomers selected from the group consisting of methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, propyl acrylate, propyl methacrylate, isopropyl acrylate, isopropyl methacrylate, butyl acrylate, butyl methacrylate, isobutyl acrylate, isobutyl methacrylate, tert-butyl acrylate, tert-butyl methacrylate, pentyl acrylate, pentyl methacrylate, isoamyl acrylate, isoamyl methacrylate, hexyl acrylate, hexyl methacrylate, cyclohexyl acrylate, cyclohexyl methacrylate, acrylate octyl, octyl methacrylate, isooctyl acrylate, isooctyl methacrylate, nonyl acrylate, nonyl methacrylate, isononyl acrylate, isononyl methacrylate, isobutyl methacrylate, decyl acrylate,decyl methacrylate, dodecyl acrylate, dodecyl methacrylate, tridecyl acrylate, tridecyl methacrylate, hexadecyl acrylate, hexadecyl methacrylate, octadecyl acrylate, octadecyl methacrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, vinyl formate, vinyl acetate, vinyl propionate, 2-hydroxyethyl acrylate, hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, 2-hydroxypropyl methacrylate, acrylic acid, styrene and acrylonitrile., Method according to one of the preceding claims, in which, during the first step (101), the flow is carried out for a duration of between 1 minute and 10 minutes. Method according to one of the preceding claims, in which, during the first step (101), the first face (6) is inclined relative to an axis of gravity (9) at an angle of between 5° and 60°.

9. Method according to one of the preceding claims, in which, during the second step (102), the latex layer is dried in an atmosphere having a temperature maintained between 30°C and 60°C, for a period greater than 20 minutes.

10. Method according to the preceding claim, in which, during the second step (102), a flow of the atmosphere surrounding the latex layer is actuated.

11. Method according to one of the preceding claims, in which the second glass sheet (3) is chemically toughened and has a thickness of between 0.5 mm and 3 mm.

12. Method according to one of the preceding claims, in which, during the third step (103), the second glass sheet (3) is heated before being brought into contact with the dried latex layer so that the second glass sheet (3) has a temperature of between 30°C and 45°C at the time of being brought into contact with the dried latex layer.

13. Method according to one of the preceding claims, in which, during the fourth step (104), the temperature between 70°C and 120°C is maintained for a period greater than 30 minutes.

14. Method according to one of the preceding claims, comprising a fifth step (105), in which the glazed assembly (1) is dried at a temperature between 70°C and 120°C in an infrared radiation tunnel.

15. Method according to the preceding claim, in which, during the fifth step (105), the glazed assembly (1) is kept in the infrared radiation tunnel for a period greater than 10 minutes.

16. Glazed assembly (1) for a vehicle obtained by a method according to one of claims 1 to 15, the glazed assembly (1) comprising a first glass sheet (2) and a second glass sheet (3) superimposed, the glazed assembly (1) comprising a viscoelastic damping layer for acoustically reducing the vehicle, the viscoelastic damping layer (4) being formed by a material comprising: - at least one acrylic polymer, - at least one tackifying agent, and - at least one plasticizing agent, the viscoelastic damping layer (4) being arranged between the first glass sheet (2) and the second glass sheet (3) and being in direct contact with the first sheet of glass (2).