TEST DEVICE FOR THE LOST-WAX CASTING MANUFACTURE OF A HOLLOW TURBOMACHINE BLADE

A test device with an S-shaped core configuration addresses core positioning issues in lost wax casting by simulating blade manufacturing, reducing defects and scrapping through anchoring system validation.

FR3142108B1Active Publication Date: 2024-10-11SAFRAN SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FR2022012213
Authority / Receiving Office
FR · FR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-11-23
Publication Date
2024-10-11
Estimated Expiration
2042-11-23

AI Technical Summary

Technical Problem

The manufacturing process of hollow turbine blades using lost wax casting faces challenges in maintaining core positioning due to differential expansion between the core and shell mold at high temperatures, leading to defects such as local thickness issues and blade sizing problems.

Method used

A test device comprising a shell mold and a core with a middle part having an S-shaped configuration, featuring opposite concavities, is used to simulate the core's behavior during the manufacturing process, allowing for the validation or invalidation of the anchoring system and enabling adjustments to reduce manufacturing defects.

Benefits of technology

The test device helps in simulating core movement and anchoring system validation, thereby reducing the number of defective blades by limiting manufacturing defects and scrapping.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000013_0000
    Figure 00000013_0000
  • Figure 00000013_0001
    Figure 00000013_0001
  • Figure 00000014_0000
    Figure 00000014_0000
Patent Text Reader

Abstract

The invention relates to a test device (100) for manufacturing a hollow blade (8) by lost-wax casting, comprising: - a shell mold (101) having an internal cavity (108) for receiving molten metal, - a core (102) arranged in the internal cavity (108) and extending longitudinally between a first end (109) and an opposite second end (110), and a middle portion (111) connecting the first and second ends (109, 110), the core (102) being fixed to the shell mold (101) by its second end (110) and a longitudinal gap (J1) being defined in the internal cavity (108) between the upper end (103) of the shell mold (101) and the first end (109) of the core (102), the middle portion (111) of the core (102) having an S-shape having a first concavity (112a) and a second concavity (112b) opposite the first concavity (112a). Abbreviated figure: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: TEST DEVICE FOR THE MANUFACTURE BY LOST WAX CASTING OF A HOLLOW TURBOMACHINE BLADE Technical field of the invention

[0001] The invention relates to the field of test devices, in particular test specimens, for the manufacture by lost wax casting of a hollow turbine blade, in particular a high-pressure turbine blade. Technical background

[0002] An aircraft turbomachine, such as a turbojet, typically comprises, from upstream to downstream in the direction of gas flow, a fan movable in rotation about a longitudinal axis, a low pressure compressor, a high pressure compressor, a combustion chamber, a high pressure turbine, a low pressure turbine and a gas exhaust nozzle.

[0003] The blower allows the suction of an air flow dividing into a primary flow and a secondary flow. The primary flow passes through a primary vein of the turbomachine while the secondary flow is directed towards a secondary vein surrounding the primary vein.

[0004] The primary flow is compressed within the compressors. The compressed air is then mixed with a fuel and burned within the combustion chamber. The gases resulting from the combustion pass through the turbines and then escape through the nozzle, the cross-section of which allows the acceleration of these gases to generate propulsion.

[0005] Turbines are typically equipped with blades regularly distributed around a disk. A blade extends radially from the disk between a root and a tip. It typically comprises a blade connected to the root via a platform. The root is arranged in a cell of the disk to retain the blade on the disk. The blade also has an aerodynamic shape and typically comprises a pressure face and an extrados face connected by a leading edge and a trailing edge.

[0006] Since high-pressure turbine blades are located downstream of the combustion chamber, they are subjected to high temperatures. Thus, these blades are typically made of metallic material. Although metallic materials have the advantage of withstanding high temperatures, such blades may be subjected to temperatures higher than those materials can withstand.

[0007] In this context, it has been proposed to equip the blades with a cooling system. The cooling system comprises a cooling circuit arranged inside the blades and allowing the passage of air from the compressors to the interior of the blades. The cooling circuit includes internal channels formed during blade manufacturing. Each channel typically extends from the tip of the blade to the root.

[0008] Such blades are typically produced by a lost wax casting manufacturing process. Such a manufacturing process comprises a step of manufacturing cores and then a step of manufacturing by molding wax or resin models of the blade around the respective cores. Then, the method comprises a step of manufacturing shell molds of the blade. For this purpose, each model is impregnated with a refractory material, for example chosen from ceramic materials. The models are then removed for example by heat treatment and the shell molds are typically arranged in clusters around a foundry mold to increase the manufacturing rate of the blades. The foundry mold is subsequently placed in a heating chamber for casting a metallic material.

[0009] Each shell mold typically comprises an internal cavity for casting the metallic material and has a blade impression comprising a first root impression and a second blade impression. An intermediate platform impression is located between the first and second impressions. The core is arranged inside the internal cavity to form the internal channel of the blade when casting the metallic material into the shell mold.

[0010] The core is held securely in the internal cavity of the shell mold by two connections, a recess at one end and a sliding connection at the other. For example, the recess can be achieved by a holding rod at an anchoring point of the core previously placed during the manufacture of the model. Opposite the holding rod, a flat area of ​​the core and the shell mold delimit in the internal cavity a longitudinal clearance forming a sliding connection of the core in the shell mold. This clearance must be determined precisely, and must be small enough to preserve the properties of the blade and large enough to ensure the sliding of the core and therefore of the cavity at the platform. It is therefore advisable not to use up all the clearance during the manufacturing process of the blade.

[0011] However, when the foundry mold is placed in the heating chamber where the temperature can reach 1600°C, for example during the casting of the molten metal, there is a differential expansion between the core and the shell mold. This differential expansion combined with the distance between the sliding plane of the core and the anchoring point of the latter can lead to a lack of sliding of the core along the internal cavity. This lack of sliding leads to a displacement of the core towards the intrados of the blade and causes problems in sizing the blade, for example a local thickness of the blade that is too small. Such displacement of the core is therefore one of the main manufacturing defects of a blade by this type of process.

[0012] One of the major technical difficulties of this manufacturing process is therefore to ensure the positioning of the core in the internal cavity throughout the manufacturing process, and therefore over a wide temperature range.

[0013] However, there is no solution for observing the effects of temperature on core movement, so some blades produced by a lost wax casting manufacturing process do not meet specifications and are scrapped.

[0014] In this context, there is a need to provide a solution for monitoring the behavior of the core during a process for manufacturing a hollow blade by lost wax casting in order to limit manufacturing defects in these blades by such a process. Summary of the invention

[0015] To this end, the invention proposes a test device for the manufacture by lost wax casting of a hollow turbomachine blade, this blade comprising a blade and a root connected to the blade by a platform, the test device comprising:

[0016] - a shell mold extending longitudinally between an upper end and a lower end, the shell mold comprising an internal cavity extending longitudinally and intended to receive a molten metal,

[0017] - a core arranged in the internal cavity and extending longitudinally between a first end located on the side of the upper end and a second opposite end, the core further comprising a middle part connecting the first and second ends, the core being fixed to the shell mold by its second end and a longitudinal clearance being delimited in the internal cavity between the upper end of the shell mold and the first end of the core.

[0018] The test device according to the invention is remarkable in that the middle part of the core has an S shape comprising a curve having a first concavity and a second concavity opposite the first concavity.

[0019] The invention therefore proposes a test device, in particular a test piece, which makes it possible to reproduce the shell mold and the core used in a lost wax blade manufacturing process.

[0020] The test device comprises a shell mold and a core arranged in the internal cavity of the shell mold. The core is fixed to the shell mold at its second end while a longitudinal clearance is defined in the internal cavity between the first end of the core and the upper end of the mold. These characteristics therefore make it possible to reproduce the anchoring system of the core in the mold during the blade manufacturing process, and in particular to test the sliding of the core along the internal cavity.

[0021] Furthermore, according to the invention, the core of the test device has a double opposite concavity which allows the anchor point to be offset from the slip plane and induces a displacement of the core in a direction perpendicular to the slip plane of the core. Such a configuration of the core therefore makes it possible to study the link between the offset of the core and the distance from the anchor point to the slip plane.

[0022] Thanks to such a test device, it is therefore possible to simulate the offset of the core during the lost wax manufacturing process of a blade, and to possibly validate or invalidate the anchoring system of the core in the shell mold and to resize the core and / or the shell mold accordingly.

[0023] Thanks to such a test device, it is therefore possible to limit manufacturing defects in the blades and the number of blades scrapped.

[0024] The invention may comprise one or more of the following features, taken in isolation from one another or in combination with one another:

[0025] - the curve of the middle part has an inflection point located at an equal distance of the first and second ends of the core,

[0026] - the first and second ends of the core are planar,

[0027] - the first concavity has a first radius of curvature and the second concavity has a second radius of curvature equal to the first radius of curvature,

[0028] - the shell mold comprises an internal surface delimiting the internal cavity, the internal surface further defining a first footprint of the blade root located on the upper end side and a second footprint of the blade,

[0029] - the S-shape of the middle part of the core is located in a part of the cavity internal which is delimited by the second imprint,

[0030] - the second imprint has a shape complementary to the S shape of the middle part of the core,

[0031] - the internal surface further defines an intermediate footprint of the platform of the dawn, the intermediate imprint being located between the first and second imprints,

[0032] - the core and the second imprint are separated by a first constant distance less than 10 mm, advantageously less than 5 mm,

[0033] - the core and the intermediate imprint are separated by a second distance su greater than the first distance,

[0034] - the core has a constant thickness, advantageously between 1 mm and 10 mm,

[0035] - the shell mold comprises a ceramic material. Brief description of the figures

[0036] Other characteristics and advantages will emerge from the following description of a non-limiting embodiment of the invention with reference to the appended drawings in which:

[0037] [Fig.l] is a longitudinal schematic representation of a half-aircraft turbomachine according to the invention,

[0038] [Fig.2] is a schematic perspective representation of a blade,

[0039] [Fig.3] is a schematic representation of a foundry mold placed in a heating chamber for the manufacture of the blade of [Fig.2],

[0040] [Fig.4] is a block diagram of a manufacturing process by lost wax casting of the blade of [Fig.2] and using the foundry mold of [Fig.3],

[0041] [Fig.5] is a schematic representation in longitudinal section of a test device according to the invention comprising a shell mold and a core,

[0042] [Fig.6] is a schematic representation in longitudinal section of the core equipping the test device of [Fig.5]. Detailed description of the invention

[0043] An example of an aircraft turbomachine 1 according to the invention is shown in [Fig.l]. The turbomachine 1 extends around and along a longitudinal axis A.

[0044] The turbomachine 1 comprises, from upstream to downstream relative to the direction of circulation of the gases in the turbomachine 1 along the longitudinal axis A, a fan 2, at least one compressor such as a low-pressure compressor 3 and a high-pressure compressor 4, a combustion chamber 5, at least one turbine such as a high-pressure turbine 6 and a low-pressure turbine 7, and a nozzle (not shown).

[0045] The blower 2 allows the suction of an air flow F dividing into a primary flow Fl and a secondary flow F2. The primary flow Fl passes through the engine of the turbomachine 1 while the secondary flow F2 is directed towards a secondary vein.

[0046] The primary flow F1 is compressed within the low pressure compressor 3 then the high pressure compressor 4. The compressed air is then mixed with a fuel and burned within the combustion chamber 5. The gases formed by the combustion pass through the high pressure 6 and low pressure 7 turbines. The gases finally escape through the nozzle, the cross-section of which allows the acceleration of these gases to generate propulsion.

[0047] The fan 2 is for example shrouded. It is surrounded by an annular casing 2b centered on the longitudinal axis A. The casing 2b is for example surrounded by a nacelle (not shown) of the turbomachine 1.

[0048] With reference to [Fig. 2], the high pressure and low pressure turbines 6, 7, and in particular the high pressure turbine 6, comprise blades 8 extending radially relative to the longitudinal axis A, from a disc (not shown) movable or fixed in rotation relative to the longitudinal axis A. Each blade 8 extends between a head 10 and a root 12. The root 12 is connected to a blade 9 by a platform 11.

[0049] The foot 12 is mounted in a corresponding socket of the disc to maintain the blade 8 on the disc. The foot 12 has a fir tree or dovetail shape in cross section relative to the longitudinal axis A.

[0050] The blade 9 has an aerodynamic shape and comprises a lower surface face 9i and an upper surface face 9e connected by a leading edge 9a and a trailing edge 9b.

[0051] The blade 8 is made of metallic material. Advantageously, the metallic material is chosen from monocrystalline nickel-based superalloys. Such materials have the advantage of resisting high temperatures and therefore of allowing the implementation of these blades 8 near the combustion chamber 5, in an environment subjected to high temperatures.

[0052] In order to further improve the temperature resistance of the blades 8, each blade 8 is hollow. Indeed, each blade 8 comprises a cooling system comprising at least one internal channel 13 for the circulation of cooling air inside the blade 8. The internal channel 13 extends in the blade 8 from the head 10 to the root 12 of the blade 8. The cooling air is for example air taken from the low pressure compressor 4.

[0053] Each blade 8 is manufactured in a lost wax casting installation 14 illustrated for example in [Fig.3].

[0054] The installation 14 comprises a foundry mold 15 having a central axis Z. It comprises a central barrel 16 extending along the central axis Z between a funnel 17 and a plate 18 which are centered on the central axis Z.

[0055] The installation 14 further comprises shell molds 19 regularly distributed around the central barrel 16 and connected to the latter by fixing arms 20.

[0056] Each shell mold 19 is made of refractory material, for example ceramic material. Each shell mold 19 extends longitudinally along the central axis Z between an upper end 21 and a lower end 22.

[0057] The upper end 21 is connected to the fixing arm 20 while the opposite lower end is connected to the plate 18 by means of a chicane selector 23.

[0058] Each shell mold 19 further comprises an internal cavity intended to receive a molten metal. The internal cavity is connected to the funnel 17 via a molten metal supply channel 24. The internal cavity extends in the shell mold longitudinally relative to the central axis Z.

[0059] Each shell mold 19 further comprises a core arranged in the internal cavity. The core makes it possible to form the internal channel 13 of the blade 8 during molding. The core extends in the internal cavity longitudinally relative to the central axis Z between a first end located on the side of the upper end 21 of the shell mold 19 and a second opposite end. The core is fixed to the shell mold 19 by its second end by a fixing rod. Furthermore, in the internal cavity, the upper end of the shell mold 19 and the core delimit a longitudinal clearance forming a slip bond.

[0060] Advantageously, the core is made of refractory material, for example ceramic material.

[0061] The installation 14 further comprises a heating chamber 27 in which the foundry mold 15 is placed. The heating chamber 27 is advantageously a furnace, preferably a directed solidification furnace such as a Bridgman furnace.

[0062] A method of manufacturing the blade 8 by lost wax casting will now be described with reference to [Fig.4].

[0063] The manufacturing process comprises the following steps:

[0064] (a) making a core,

[0065] (b) placing the core in a mold of the blade 8,

[0066] (c) injecting a wax or resin into the mold to form a model of the blade 8,

[0067] (d) covering the model with a refractory material, such as a ceramic material, to form the shell mold 19 around the model,

[0068] (e) arranging the shell mold 19 in the foundry mold 15,

[0069] (f) removing the model, for example by heat treating the model at a temperature temperature for example between 70°C and 200°C,

[0070] (g) optionally, heat treating the shell mold 19, for example by cooking, to solidify the shell mold 19,

[0071] (h) pouring the molten metal into the internal cavity of the shell mold 19,

[0072] (i) solidifying the metallic material by cooling the internal cavity through of the chicane selector 22,

[0073] (j) unmold the blade 8,

[0074] (k) removing the core, for example by chemical treatment of the blade 8, and

[0075] (1) optionally machine the blade 8.

[0076] Typically, step (h) is carried out in the heating chamber 27. During this step, a movement of the core in a direction perpendicular to the central axis Z can be observed and impact the characteristics of the blade 8, in particular the thickness of the intrados 9i and / or extrados 9e faces or the section of the internal channel 13.

[0077] For this purpose, the invention proposes a test device 100 for the manufacture by lost wax casting of the blade 8. The test device 100 is illustrated for example in [Fig.5].

[0078] The test device 100 is a test piece which comprises a shell mold 101 and a core 102.

[0079] In the remainder of the description, the terms “longitudinal” and “longitudinally” are understood relative to an elongation axis X of the test device 100. The elongation axis X is parallel to the central axis Z of the foundry mold 15 when the test device 100 is placed in the foundry mold 15.

[0080] The terms “interior”, “internal”, “exterior”, “external”, are understood in relation to the distance from the elongation axis X, along a radial axis Y perpendicular to the elongation axis X.

[0081] The terms “low”, “high”, “lower”, “upper”, are understood in relation to the direction of flow E of a molten metal in the test device 100 along the elongation axis X.

[0082] The shell mold 101 extends longitudinally between an upper end 103 and a lower end 104.

[0083] Advantageously, it has a height H as measured along the elongation axis X of between 50 mm and 200 mm, preferably of between 80 mm and 120 mm, even more preferably of 100 mm.

[0084] Advantageously, it has a first thickness L1 located on the side of the upper end 103 and a second thickness L2 located on the side of the lower end 104. The first and second thicknesses L1, L2 are measured along the radial axis Y. Advantageously, the first thickness L1 is greater than the second thickness L2. The first thickness L1 is for example between 10 mm and 50 mm, in particular between 15 mm and 25 mm. The second thickness L2 is for example between 10 mm and 50 mm, in particular between 15 mm and 25 mm.

[0085] Advantageously, the shell mold 101 is made of ceramic material.

[0086] It comprises a wall 105 having a first external surface 105a and a second external surface 105b connected by longitudinal edges. The wall 105 further has an internal surface 106.

[0087] Preferably, the wall 105 has a thickness p as measured along the radial axis Y of between 1 mm and 10 mm, in particular 5 mm.

[0088] The internal surface 106 has an imprint 107 of the blade 8. More particularly, the internal surface 106 has from top to bottom along the elongation axis X, a first imprint 107a of the root 12 of the blade 8, an intermediate imprint 107b of the platform 11 of the blade 8 and a second imprint 107c of the blade 9 of the blade 8.

[0089] The first imprint 107a is located on the side of the upper end 103 of the shell mold 101. The first imprint 107a preferably has a shape complementary to a dovetail or fir tree shape in accordance with the examples of the root 12 of the blade 8.

[0090] The shell mold 101 further comprises an internal cavity 108. The internal cavity 108 is delimited by the internal surface 106 of the shell mold 101. The internal cavity 108 extends longitudinally in the shell mold 101. Preferably, the internal cavity 108 extends from the upper end 103 to the lower end 104 of the shell mold 101.

[0091] The core 102 is arranged in the internal cavity 108. It extends longitudinally between a first end 109 located on the side of the upper end 103 of the shell mold 101 and a second opposite end 110. The first and second ends 109, 110 are advantageously flat.

[0092] With reference to [Fig.6], the core 102 further comprises a middle portion 111 connecting the first and second ends 109, 110. The middle portion 111 has a first face 11a and a second face 111b extending longitudinally from the first end 109 to the second end 110. The first and second faces 111a, 111b are connected by first and second longitudinal edges. The middle portion 111 has, in a longitudinal direction, an S-shape comprising a curve having a first concavity 112a and a second concavity 112b opposite the first concavity 112a. The first concavity 112a has a first radius of curvature RI and the second concavity 112b has a second radius of curvature R2 preferably equal to the first radius of curvature RL. The first and second radii of curvature RI, R2 are for example between 2 mm and 20 mm, between 2 mm and 10 mm, between 2 mm and 5 mm.

[0093] The curve of the middle part 111 of the core 102 thus has an inflection point P. Preferably, the inflection point P is located at an equal distance from the first and second ends 109, 110 of the core 102.

[0094] Preferably, the S-shaped part of the middle part 111 of the core 102 is located in a part 113 of the cavity 108 which is delimited by the second imprint 107c of the blade 9 of the vane 8. Preferably, this part 113 of the cavity 108 has a shape complementary to the S-shaped shape of the core 102.

[0095] Preferably, the middle part 111 has, in a longitudinal direction, an inverted S shape. By inverted S, it is understood the symmetrical of an S with respect to an axis of symmetry extending longitudinally.

[0096] With reference to [Fig.5], preferably, the core 102 is separated from the second imprint 107c by a first constant distance dl, for example between 1 mm and 5 mm. By constant, it is understood that the first distance dl separating the core 102 from the second imprint 107c is identical throughout the portion 113 of the internal cavity 108 delimited by the second imprint 107c of the blade 9 of the vane 8. Preferably, the core 102 is separated from the intermediate imprint 107b by a second distance d2 greater than the first distance dl. The second distance d2 is for example between 2 mm and 10 mm, between 2 mm and 5 mm.

[0097] Preferably, the core 102 has a constant thickness e. The thickness e of the core 102, as measured along the radial axis Y, is for example between 1 mm and 10 mm, between 1 mm and 5 mm, in particular 2 mm.

[0098] Advantageously, the core 102 is made of ceramic or metallic material. The metallic material is for example molybdenum-based.

[0099] Furthermore, the core 102 is fixed to the shell mold 101 by its second end 110. For example, a fixing rod 114 connects the shell mold 101 to the core 102. The fixing rod 114 passes through, for example, the entire thickness e of the core. The fixing rod 114 is, for example, made of a metallic material such as aluminum oxide.

[0100] Opposite the second end 110, the core 102 is connected to the shell mold 101 by a sliding connection. For this purpose, according to the invention, a longitudinal clearance J1 is delimited in the internal cavity 108 between the upper end 103 of the shell mold 101 and the first end 109 of the core 102. This longitudinal clearance J1 makes it possible to ensure the sliding of the core 102 in a sliding plane G parallel to the elongation axis X.

[0101] The test device 100 further comprises a chicane selector 115 connected to the lower part 104 of the shell mold 101. The selector 115 is advantageously made of ceramic material. For example, it forms a single piece with the shell mold 101.

[0102] The test device 100 can be arranged in the foundry mold 15. The assembly can then be arranged in a furnace for casting a metal into the internal cavity 108.

[0103] The thicknesses of the raw casting formed in the internal cavity 108 may be determined by tomography for example. Depending on the different thicknesses, the configurations of the core 102 and the shell mold 101 may be validated and / or adapted.

[0104] The double curvature of the core 102 therefore makes it possible to study the link between the offset of the core and the distance from the anchoring point to the sliding plane during the temperature rise of the test device 100, in particular during the casting of the metal. Thanks to such a double curvature, it is possible to simulate this offset and to validate or invalidate the anchoring system of the core 102 in the shell mold 101. It is therefore possible to size the core and / or the shell mold to limit this offset and thus limit manufacturing defects of the blade.

[0105] The number of blades discarded is therefore limited.

Claims

Claims

1. Test device (100) for the manufacture by lost wax casting of a hollow blade (8) of a turbomachine (1), this blade (8) comprising a blade (9) and a root (12) connected to the blade (9) by a platform (11), the test device (100) comprising: - a shell mold (101) extending longitudinally between an upper end (103) and a lower end (104), the shell mold (101) comprising an internal cavity (108) extending longitudinally and intended to receive a molten metal, - a core (102) arranged in the internal cavity (108) and extending longitudinally between a first end (109) located on the side of the upper end (103) and a second opposite end (110), the core (102) further comprising a middle portion (111) connecting the first and second ends (109, 110),the core (102) being fixed to the shell mold (101) by its second end (110) and a longitudinal clearance (Jl) being delimited in the internal cavity (108) between the upper end (103) of the shell mold (101) and the first end (109) of the core (102), characterized in that the middle part (111) of the core (102) has an S shape comprising a curve having a first concavity (112a) and a second concavity (112b) opposite the first concavity (112a).,

2. Device according to the preceding claim, characterized in that the curve of the middle part (111) has an inflection point (P) located at an equal distance from the first and second ends (109, 110) of the core (102).

3. Device according to any one of the preceding claims, characterized in that the first and second ends (109, 110) of the core (102) are planar.

4. Device according to any one of the preceding claims, characterized in that the first concavity (112a) has a first radius of curvature (RI) and in that the second concavity (112b) has a second radius of curvature (R2) equal to the first radius of curvature (RI).

5. Device according to any one of the preceding claims, characterized in that the shell mold (101) comprises an internal surface (106) delimiting the internal cavity (108), and defining a first imprint (107a) of the foot (12) of the blade (8) located on the side of the upper end (103) and a second imprint (107c) of the blade (9) of the blade (8).

6. Device according to the preceding claim, characterized in that the S-shape of the middle part (111) of the core (102) is located in a part (113) of the internal cavity (108) which is delimited by the second imprint (107c).

7. Device according to the preceding claim, characterized in that the second imprint (107c) has a shape complementary to the S shape of the middle part (111) of the core (102).

8. Device according to any one of claims 5 to 7, characterized in that the internal surface (106) further defines an intermediate imprint (107b) of the platform (11) of the blade (8), the intermediate imprint (107b) being located between the first and second imprints (107a, 107c).

9. Device according to any one of claims 5 to 8, characterized in that the core (102) and the second imprint (107c) are separated by a first constant distance (dl) less than 10 mm, advantageously less than 5 mm.

10. Device according to claims 8 and 9, characterized in that the core (102) and the intermediate imprint (107b) are separated by a second distance (d2) greater than the first distance (dl).

11. Device according to any one of the preceding claims, characterized in that the core (102) has a constant thickness (e), advantageously between 1 mm and 10 mm.

12. Device according to any one of the preceding claims, characterized in that the shell mold (101) comprises a ceramic material.