Method for manufacturing an acoustically insulating glazed assembly comprising a viscoelastic damping layer

A viscoelastic damping layer composed of acrylic polymer, tackifying agent, and plasticizing agent, applied between glass sheets, addresses noise transmission and manufacturing complexity in tempered glass glazing, enhancing acoustic attenuation and maintaining optical clarity and rigidity.

FR3143595B1Inactive Publication Date: 2024-11-22SAINT GOBAIN VITRAGE SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FR2022013664
Authority / Receiving Office
FR · FR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-12-16
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing tempered glass glazing in vehicles suffers from high airborne noise transmission due to air turbulence and has complex manufacturing processes, including adhesion issues with PVB layers and reduced mechanical rigidity.

Method used

A method involving the application of a viscoelastic damping layer between two glass sheets, composed of acrylic polymer, tackifying agent, and plasticizing agent, using a latex deposition and debubbling process to enhance acoustic attenuation while maintaining optical clarity and mechanical rigidity.

Benefits of technology

The method effectively reduces airborne noise transmission and simplifies manufacturing by ensuring the viscoelastic damping layer adheres well to the glass, maintaining high optical properties and mechanical strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000024_0000
    Figure 00000024_0000
  • Figure 00000024_0001
    Figure 00000024_0001
  • Figure 00000024_0002
    Figure 00000024_0002
Patent Text Reader

Abstract

The present invention relates to a method for manufacturing a glazed assembly, the method comprising a first step of depositing a first layer of latex onto a first face of a first sheet of glass, the deposition being carried out by spraying a latex onto the first face, the latex comprising an acrylic polymer, a tackifying agent, and a plasticizing agent. Figure to be published with the abbreviation: Figure 6
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: Method for manufacturing an acoustically insulating glazed assembly comprising a viscoelastic damping layer Field of invention

[0001] The present invention relates to a method for manufacturing a glazed element comprising a viscoelastic damping layer for the acoustic attenuation of a motor vehicle, as well as a glazed element obtained by such a method. In particular, the glazed element may be an opening side glazing of a motor vehicle. State of the art

[0002] It is known to use tempered glass glazing as the opening side glazing of a motor vehicle. However, such glazing has a high transmission of airborne noise caused by the turbulence of an air flow over the glazing when the vehicle is moving.

[0003] For this purpose, document EP2608958 describes a side glazing unit comprising a laminated glass assembly. The laminated glass assembly comprises two superimposed glass sheets and an interlayer. The interlayer comprises two superimposed outer PVB layers, and an inner PVB layer arranged between the two outer layers. The inner layer has higher acoustic damping properties than the two outer layers. Such a glazed element has higher acoustic attenuation properties than those of a glazing unit formed by monolithic tempered glass.

[0004] However, the manufacture of glazing comprising one or more layers of PVB can be complex. For example, the adhesion of a layer of PVB to a sheet of glass requires treatment in an autoclave. In addition, a glazed assembly comprising layers of PVB may have a thickness that is too great for the glazed element to be inserted into a rebate of a vehicle door. Finally, laminated glazing may have less mechanical rigidity than toughened glazing. Statement of the invention

[0005] An aim of the invention is to propose a solution for increasing the acoustic attenuation of a glazed assembly of a vehicle, in particular of a side glazing of a vehicle, while simplifying its manufacture.

[0006] This aim is achieved within the framework of the present invention thanks to a method of manufacturing a glazed assembly comprising a first sheet of glass, a second glass sheet and a viscoelastic damping layer for sound reduction of a vehicle, the viscoelastic damping layer being arranged between the first glass sheet and the second glass sheet and being in direct contact with the first glass sheet, the viscoelastic damping layer being formed by a material comprising: - at least one acrylic polymer, - at least one tackifying agent, and - at least one plasticizing agent, the method comprising: - a first step of depositing a first layer of latex on a first face of the first glass sheet, the deposit being carried out by spraying a latex on the first face, the latex comprising the acrylic polymer, the tackifying agent, and the plasticizing agent, - a second stage of drying the first layer of latex deposited during the first stage, - a third step of superimposing the first sheet of glass on the second sheet of glass so that the first layer of latex dried during the second step is arranged between the first sheet of glass and the second sheet of glass, - a fourth step of debubbling, during which the assembly formed by the first sheet of glass, by the first layer of dried latex and by the second sheet of glass is arranged in an enclosure in which the pressure is less than 100 mbar, the first layer of dried latex forming at least in part the viscoelastic damping layer.

[0007] The present invention is advantageously supplemented by the following characteristics, taken individually or in any of their technically possible combinations:

[0008] - during the first step, a second layer of latex is deposited by spraying de-bubbling the latex on a second face of the second glass sheet, during the second step, the second layer of latex deposited during the first step is dried, during the third step, the second glass sheet is superimposed on the first layer of latex dried during the second step by bringing the first dried latex layer and the second dried latex layer into contact, and during the fourth de-bubbling step, the assembly formed by the first glass sheet, by the first dried latex layer, by the second dried latex layer and by the second glass sheet is placed in the enclosure in which the pressure is less than 100 mbar, the first layer and the second layer forming at least in part, after the fourth step, the viscoelastic damping layer, latex is between 0.21 and 0.62, in particular between 0.21 and 0.51, and preferably between 0.21 and 0.35,

[0010] - a mass fraction of the tackifying agent(s) in the dry matter of the latex is between 0.17 and 0.60, in particular between 0.22 and 0.35, and preferably between 0.22 and 0.26,

[0011] - a mass fraction of the plasticizing agent(s) in the dry matter of the latex is between 0.07 and 0.43, in particular between 0.12 and 0.31, and preferably between 0.16 and 0.26,

[0012] - a mass fraction of the acrylic polymer(s) in the latex is included between 0.20 and 0.60, in particular between 0.20 and 0.50, and preferably between 0.20 and 0.30,

[0013] - a mass fraction of the tackifying agent(s) in the latex is included between 0.20 and 0.70, in particular between 0.25 and 0.40, and preferably between 0.25 and 0.30,

[0014] - a mass fraction of the plasticizing agent(s) in the latex is included between 0.05 and 0.25, in particular between 0.07 and 0.18, and preferably between 0.09 and 0.15,

[0015] - during the first stage, the latex has a surface tension of between 32 Nm and 42 Mm, in particular between 34 Nm and 40 Nm and preferably between 36 Nm and 38 Nm,

[0016] - during the first stage, the latex has a mass fraction of water comprised between 0.42 and 0.70,

[0017] - the latex comprises an anionic surfactant,

[0018] - a concentration of the anionic surfactant is between 1 mM and 50 mM, in particular between 3 mM and 10 mM and preferably between 6 mM and 8 mM,

[0019] - the anionic surfactant comprises at least one sulfonate group,

[0020] - the tackifying agent comprises a hydrogenated resin and preferably a resin hydrogenated rosin,

[0021] - the acrylic polymer(s) are formed from monomers chosen from the group formed by methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, propyl acrylate, propyl methacrylate, isopropyl acrylate, isopropyl methacrylate, butyl acrylate, butyl methacrylate, isobutyl acrylate, isobutyl methacrylate, tert-butyl acrylate, tert-butyl methacrylate, pentyl acrylate, pentyl methacrylate, isoamyl acrylate, isoamyl methacrylate, hexyl acrylate, hexyl methacrylate, cyclohexyl acrylate, cyclohexyl methacrylate, octyl acrylate, octyl methacrylate, isooctyl acrylate, methacrylate isooctyl acrylate nonyl, nonyl methacrylate, isononyl acrylate, isononyl methacrylate, isobornyl methacrylate, decyl acrylate, decyl methacrylate, dodecyl acrylate, dodecyl methacrylate, tridecyl acrylate, tridecyl methacrylate, hexadecyl acrylate, hexadecyl methacrylate, octadecyl acrylate, octadecyl methacrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, vinyl formate, vinyl acetate, vinyl propionate, 2-hydroxyethyl acrylate, hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, 2-hydroxypropyl methacrylate, acrylic acid, styrene and acrylonitrile,

[0022] - in the second step, the latex layer is dried in an atmosphere having a temperature maintained between 30°C and 80°C, in particular between 30°C and 50°C and preferably between 30°C and 40°C, for a period of more than 20 minutes.

[0023] Another aspect of the invention is a glazed assembly for a vehicle obtained by a method according to an embodiment of the invention, the glazed assembly comprising a first glass sheet and a second glass sheet superimposed, the glazed assembly comprising a viscoelastic damping layer for acoustic attenuation of the vehicle, the viscoelastic damping layer being formed by a material comprising: - at least one acrylic polymer, - at least one tackifying agent, and - at least one plasticizing agent, the viscoelastic damping layer being arranged between the first glass sheet and the second glass sheet and being in direct contact with the first glass sheet.

[0024] Advantageously, the viscoelastic damping layer has a thickness of between 5 μm and 500 μm. Description of figures

[0025] Other characteristics, aims and advantages of the invention will emerge from the following description, which is purely illustrative and non-limiting, and which must be read in conjunction with the appended drawings in which:

[0026] [Fig-1] - [Fig.l] schematically illustrates a method according to one embodiment of the invention,

[0027] [Fig.2] - [Fig.2] schematically illustrates a glazed element according to a method of rea lization of the invention,

[0028] [Fig.3] - [Fig.3] illustrates a loss factor of a material of a visco layer elastic of a glazed assembly according to an embodiment of the invention, for dif- different mass fractions of tackifying agent and plasticizing agent of the latex,

[0029] [Fig.4] - [Fig.4] illustrates a real part of a shear modulus G' of a material of a glazed assembly according to an embodiment of the invention, for different mass fractions of tackifying agent and plasticizing agent of the latex,

[0030] [Fig.5] - [Fig.5] illustrates a first step of deposition by spraying of a method according to an embodiment of the invention,

[0031] [Fig.6] - [Fig.6] illustrates a second step of a method according to an embodiment of the invention, in which a layer of latex is deposited only on one face of a glass sheet during the first deposition step,

[0032] [Fig.7] - [Fig.7] illustrates a second step of a method according to an embodiment of the invention, in which a layer of latex is deposited on one face of a first glass sheet and on one face of a second glass sheet during the first deposition step,

[0033] [Fig.8] - [Fig.8] illustrates a glazed element according to one embodiment of the invention.

[0034] Throughout the figures, similar elements bear identical references. Definitions

[0035] The term "bar" means the unit of absolute pressure, or "absolute bar", for which 0 bar defines absolute vacuum and for which 1 bar is equal to 100,000 pascals.

[0036] The term “latex” means an aqueous colloidal dispersion of polymers, preferably comprising a tackifying agent and / or a plasticizing agent.

[0037] The term "dry matter" of a composition means the elements of the composition obtained when the water is removed from the composition.

[0038] The term “loss factor rj” of a material is understood to mean the material having a complex Young’s modulus, the ratio between the imaginary part E” of the Young’s modulus of the material and the real part E’ of the Young’s modulus of the material. The loss factor rj of a material is defined by the international standard ISO 18437-2:2005 (Mechanical vibration and shock — Characterization of the dynamic mechanical properties of visco-elastic materials — Part 2: Resonance method, part 3.2). Preferably, the loss factor rj can be defined for a predetermined frequency. In the present document, the term “a material has a first loss factor rj greater than a value” means that the material has a first loss factor rj greater than the value for at least one frequency chosen from the audible frequency range, i.e. in a frequency range extending between 20 Hz inclusive and 20 kHz inclusive, and preferably between 20 Hz inclusive and 10 kHz inclusive, at 20°C.

[0039] By "a value of the real part E' of the Young's modulus of a material is greater than a value" is meant that a value of the real part E' of the Young's modulus of the material is greater than the value of the real part E' of the Young's modulus of the material for at least one frequency chosen from the audible frequency range, that is to say in a frequency range extending between 20 Hz inclusive and 20 kHz inclusive, and preferably between 20 Hz inclusive and 10 kHz inclusive, at 20°C.

[0040] The real part E' and the imaginary part E” of the Young's modulus may be defined for a predetermined temperature. Herein, "the real part E' of the Young's modulus of a material is greater than a value" means that the material has a real part E' of the Young's modulus greater than the value at 20°C. Herein, "a material has a first loss factor rj greater than a value" means that the material has a first loss factor rj greater than the value at 20°C.

[0041] A shear modulus G can be linked, in particular for an isotropic material, to the Young's modulus E by the relation G=E / 2(l+v), where v is the Poisson's ratio of the material.

[0042] A dynamic characterization of a material can be carried out on a viscoanalyzer of the Metravib viscoanalyzer type, under the following measurement conditions. A sinusoidal stress is applied to the material. A measurement sample formed by the material to be measured consists of two rectangular parallelepipeds, each parallelepiped having a thickness of 3.31 mm, a width of 10.38 mm and a height of 6.44 mm. Each parallelepiped formed by the material is also referred to as a shear “specimen”. The excitation is implemented with a dynamic amplitude of 5 μm around the rest position, covering the frequency range between 1 Hz and 700 Hz, and covering a temperature range between -90°C and +60°C.

[0043] The viscoanalyzer makes it possible to subject each test piece (each sample) to deformations under precise temperature and frequency conditions, and to measure the displacements of the test piece, the forces applied to the test piece and their phase shift, which makes it possible to measure rheological quantities characterizing the material of the test piece.

[0044] The use of the measurements makes it possible in particular to calculate the Young's modulus E of the material, and particularly the real part E' of the Young's modulus and the imaginary part E” of the Young's modulus of the material, and thus to calculate the tangent of the loss angle (or loss factor) rj (also designated by tanôf

[0045] A value of the real part E' of the Young's modulus and / or a loss factor rj of a material are measured without the material being prestressed.

[0046] The term “light transmission factor” means the factor defined in standard NF EN 410.

[0047] The term "blur factor" means the ratio between the intensity of all the light diffused by a passage through the glazed element (diffuse fraction or If) of an angle greater than 2.5° and between the intensity of the light transmitted through the glazed element (ZL). The haze factor can be measured by spectroscopy techniques. The integration of the intensity over the entire visible range (from 380 nm to 780 nm) makes it possible to determine the normal transmission TL and the diffuse transmission Td. Such a measurement can also be obtained by using a Hazemeter. A glazing is considered transparent if its haze factor is less than 10%, in particular less than 5% and preferably less than 1%. The Hazemeter can be a “Haze-Gard®” device marketed by the company BYK-Gardner.

[0048] The term “clarity factor” means the ratio defined by the following formula:

[0049] f _ J c~ lc+Ii:

[0050] where Ic is the intensity of light after passing through a glazing unit that has not been diffused, and lr is the intensity of light after passing through the glazing unit that has been diffused at a small angle, preferably an angle equal to 15°. The clarity factor can be measured by spectroscopy techniques. Integrating the intensity over the entire visible range (from 380 nm to 780 nm) makes it possible to determine the normal transmission TL and the diffuse transmission Td. Such a measurement can also be obtained by using a Hazemeter. A glazing unit is considered transparent if its clarity factor is greater than 90% and preferably greater than 95%.

[0051] A glass transition temperature Tg of a material, preferably of the first damping layer, can be measured by differential scanning calorimetry (DSC). The glass transition temperature can be determined using the midpoint method as described in ASTM-D-3418 for differential scanning calorimetry. The measuring device used by the applicant is the Discovery DSC model from TA Instruments.

[0052] Preferably, a glass transition temperature Tg is determined by dynamic mechanical analysis (DMA) or dynamic mechanical spectrometry (DMA). The value of Tg is determined by plotting an isofrequency curve of the loss factor as a function of the temperature of the material. The temperature at which the value of the loss factor is maximum is equal to the glass transition temperature Tg. The glass transition temperature depends on the excitation frequency of the material. In this document, the term "glass transition temperature" means the glass transition temperature measured at a frequency of 1 Hz by DMA.

[0053] “Mass fraction” of a first element in a second is understood to mean element the ratio of the mass of the first element to the mass of the second element. Detailed description of the invention

[0054] General description of the manufacturing process of a glazed element 1

[0055] With reference to [Fig. 1], one aspect of the invention is a method 100 for manufacturing a glazed assembly 1. With reference to [Fig. 2], the glazed assembly 1 comprises a first glass sheet 2, a second glass sheet 3 and a viscoelastic damping layer 4 for the acoustic attenuation of a vehicle. The viscoelastic damping layer 4 is arranged between the first glass sheet 2 and the second glass sheet 3. The viscoelastic damping layer 4 is in direct contact with the first glass sheet 2 and preferably in direct contact with the second glass sheet 3. The viscoelastic damping layer 4 is formed by a material comprising at least one acrylic polymer, at least one tackifying agent, and at least one plasticizing agent. The first glass sheet 2 may have a thickness ei of between 3 mm and 5 mm. The second glass sheet 3 may have a thickness e2 of between 0.5 mm and 3 mm.The viscoelastic damping layer 4 may have a thickness e of between 5 pm and 500 pm, in particular between 30 pm and 100 pm.

[0056] The method 100 comprises a first step 101 of depositing a first layer 9 of latex 5 on a first face 6 of the first glass sheet 2. The deposition is carried out by spraying a latex 5 onto the first face 6. The latex 5 comprises the acrylic polymer, the tackifying agent, and the plasticizing agent.

[0057] The method 100 comprises a second step 102 of drying the first layer of latex deposited during the first step 101.

[0058] The method 100 comprises a third step 103 of superimposing the first glass sheet 2 on the second glass sheet 3 so that the first layer 9 of latex dried during the second step 102 is arranged between the first glass sheet 2 and the second glass sheet 3.

[0059] The method 100 comprises a fourth step 104 of debubbling, during which the assembly formed by the first glass sheet 2, by the first dried latex layer 9 and by the second glass sheet 3 is placed in an enclosure in which the pressure is less than 100 mbar, in particular less than 10 mbar, and preferably less than 1 mbar. After debubbling, the first dried latex layer 9 at least partly forms the viscoelastic damping layer 4.

[0060] Thus, due to the composition of the latex 5 and the deposition of the latex 5 by spraying, it is possible to manufacture a viscoelastic damping layer 4 for the acoustic attenuation of a vehicle having optical properties suitable for vehicle glazing. Preferably, a light transmission factor of the glazed element 1 is greater than 90%. Preferably, a haze factor of the glazed element 1 is less than 1%. Preferably, a clarity factor of the glazed element 1 is greater than 99%. Indeed, for the composition of the latex layer previously defined, the thicknesses chosen in the range of thicknesses of the latex layer previously defined are both small enough to maximize the loss factor of the viscoelastic damping layer 4 and to allow the glazed element 1 to exhibit the predefined optical properties.

[0061] With reference to [Fig.8], the glazed element 1 obtained by the method may be a side glazing of a vehicle, in particular a motor vehicle.

[0062] First step 101 and latex 5

[0063] The method comprises a first step 101 of depositing a layer of latex 5 on a first face 6 of the first glass sheet 2. The latex 5 comprises an emulsion. The emulsion comprises an aqueous continuous phase and a dispersed phase. The dispersed phase comprises at least one acrylic polymer. The latex also comprises tackifying agent and plasticizing agent. The tackifying agent and the plasticizing agent may be in the aqueous phase.

[0064] Acrylic polymer(s)

[0065] The acrylic polymer(s) may be formed from monomers selected from the group consisting of methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, propyl acrylate, propyl methacrylate, isopropyl acrylate, isopropyl methacrylate, butyl acrylate, butyl methacrylate, isobutyl acrylate, isobutyl methacrylate, tert-butyl acrylate, tert-butyl methacrylate, pentyl acrylate, pentyl methacrylate, isoamyl acrylate, isoamyl methacrylate, hexyl acrylate, hexyl methacrylate, cyclohexyl acrylate, cyclohexyl methacrylate, octyl acrylate, octyl methacrylate, isooctyl acrylate, isooctyl methacrylate, nonyl acrylate, nonyl methacrylate, isononyl acrylate, isononyl methacrylate, isobornyl methacrylate, decyl acrylate, decyl methacrylate, dodecyl acrylate,dodecyl methacrylate, tridecyl acrylate, tridecyl methacrylate, hexadecyl acrylate, hexadecyl methacrylate, octadecyl acrylate, octadecyl methacrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, vinyl formate, vinyl acetate, vinyl propionate, 2-hydroxyethyl acrylate, hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, 2-hydroxypropyl methacrylate, acrylic acid, styrene and acrylonitrile.

[0066] The acrylic polymer(s) may be copolymers, formed from at least two monomers chosen from the group formed by the monomers defined above.

[0067] The latex 5 may comprise two different acrylic polymers. One of the two polymers may be 2-ethylhexyl acrylate (2-EHA) and / or butylacrylate (BA). Preferably, one of the two polymers is 2-ethylhexyl acrylate (2-EHA) and the other of the two polymers is butylacrylate (BA). The mass ratio between 2-ethylhexyl acrylate (2-EHA) and butylacrylate (BA) may be between 2 and 4, and is preferably equal to 3.

[0068] A commercial latex comprising an acrylic polymer may be used to form the viscoelastic damping layer 4. For example, it is possible to use Arkema ® Encor 4028, Arkema ® Encor 4517, Alberdingk® AC 75070 or Al-berdingk® AC 75011 latex.

[0069] The latex 5 may comprise another polymer which is not an acrylic polymer. Such another polymer may be formed from at least one monomer selected from styrene and methyl methacrylate.

[0070] The latex 5 may comprise a first acrylic polymer having a first glass transition temperature Tgb and a second polymer, acrylic or non-acrylic, having a second glass transition temperature Tg2, greater than Tgp. The difference between the second glass transition temperature Tg2 and between the first glass transition temperature Tgi may be greater than 10°C and preferably greater than 20°C. Thus, it is possible to increase the glass transition temperature of the material forming the viscoelastic damping layer 4 with respect to the glass transition temperature of a material obtained solely with the first acrylic polymer. Indeed, the glass transition temperature obtained solely with the first acrylic polymer may be too small to present maximum damping of the material in a range of audible frequencies.

[0071] The polymer(s) of the material of the viscoelastic damping layer 4 obtained by the method 100 may form an interpenetrating polymer network (IPN). The latex 5 may comprise polymer particles having a core-shell structure. The core may be formed from an interpenetrating polymer network (IPN) having a glass transition temperature (Tg) of between -50°C and -30°C, preferably between -45°C and -35°C. The shell may be formed from a polymer having a glass transition temperature sufficiently small to allow the coalescence of the particles from the second step 102. The glass transition temperature of the shell may be lower than that of the core, and may preferably be lower than -50°C, and more preferably lower than -60°C. The core formed from an interpenetrating polymer network may be obtained by two sequential polymerizations.The RIP thus comprises a third crosslinked polymer and a fourth polymer, which can be crosslinked or non-crosslinked. If the fourth polymer is non-crosslinked, the RIP is a so-called "semi-interpenetrating" network. polymers”. The fourth polymer can be linear or branched.

[0072] Tackifying agent

[0073] The tackifying agent is adapted to allow bonding by direct contact between the viscoelastic damping layer 4 and the first glass sheet 2 and, preferably, between the viscoelastic damping layer 4 and the second glass sheet 3.

[0074] The tackifying agent may comprise a hydrogenated resin, and preferably a hydrogenated rosin resin. The hydrogenated resin may comprise a glycerol ester of wood resin, preferably abietic acid. The hydrogenated resin may comprise a hydrogenated rosin ester (for example, a resin of the Arakawa ® KE-311 or KE 100 brand).

[0075] Plasticizing agent

[0076] The plasticizing agent is suitable for increasing the plasticity of the viscoelastic damping layer 4. The plasticizing agent may comprise at least one element selected from a citrate, an adipate, a glycol and a triethylene glycol derivative. The citrate may be acetyl tributyl citrate. The adipate may be triethylene glycol bis(2-ethylhexanoate) (for example marketed under the name WVC 3800 from Celanese®).

[0077] Adjustment of the acoustic properties of the glazed element 1

[0078] A mass fraction of the acrylic polymer(s) in the dry matter of the latex 5 may be between 0.21 and 0.62, in particular between 0.21 and 0.51, and preferably between 0.21 and 0.35. Thus, after drying the latex layer, and in particular after the fourth step 104, the material forming the viscoelastic damping layer 4 may have a mass fraction of the acrylic polymer(s) in the viscoelastic damping layer 4 respectively between 0.21 and 0.62, in particular between 0.21 and 0.51, and preferably between 0.21 and 0.35. Thus, the material forming the viscoelastic damping layer 4 has a tanô loss factor greater than 1. The latex 5 may have a proportion of water such that a mass fraction of the acrylic polymer(s) in the latex 5 is between 0.20 and 0.60, in particular between 0.20 and 0.50, and preferably between 0.20 and 0.30..

[0079] Known materials for sound reduction comprising an acrylic polymer have a frequency y^ for which a value of the loss factor tanô of the material of the viscoelastic damping layer 4 is greater than 50 kHz. This frequency is not included in the audible frequency spectrum, which reduces the sound reduction properties of the glazed element 1.

[0080] A mass fraction of the plasticizing agent(s) in the dry matter of the latex 5 may be between 0.07 and 0.43, in particular between 0.12 and 0.31, and preferably potentially between 0.16 and 0.26. Thus, after drying the latex layer, and in particular after the fourth step 104, the material forming the viscoelastic damping layer 4 may have a mass fraction of the plasticizing agent(s) in the viscoelastic damping layer 4 respectively between 0.07 and 0.43, in particular between 0.12 and 0.31, and preferably between 0.16 and 0.26. Thus, the frequency^, for which the value of the loss factor tanô of the material of the viscoelastic damping layer 4 is maximum is included in the audible frequency spectrum while increasing the value of the loss factor tanô with respect to known materials. The latex 5 may have a proportion of water such that a mass fraction of the plasticizing agent(s) is between 0.05 and 0.25, in particular between 0.07 and 0.18, and preferably between 0.09 and 0.15.

[0081] Indeed, the inventors have discovered that, for a predetermined concentration of acrylic polymer(s), the frequency for which the loss factor is maximum varies in the same direction as the mass fraction of the plasticizing agent in the viscoelastic damping layer 4. The inventors have thus discovered the range of mass fraction of the plasticizing agent in the latex 5 for which the frequency^ is included in the audible frequency spectrum. In addition, the value of the loss factor tanô of the material of the viscoelastic damping layer 4 varies in the same direction as the mass fraction of the plasticizing agent in the latex 5.

[0082] A mass fraction of the tackifying agent(s) in the dry matter of the latex may be between 0.17 and 0.60, in particular between 0.22 and 0.35, and preferably between 0.22 and 0.26. Thus, after drying the latex layer, and in particular after the fourth step 104, the material forming the viscoelastic damping layer 4 may have a mass fraction of the tackifying agent(s) in the first layer respectively between 0.17 and 0.60, in particular between 0.22 and 0.35, and preferably between 0.22 and 0.26. Thus, the frequency^, for which the value of the loss factor tanô of the material of the viscoelastic damping layer 4 is maximum is included in the audible frequency spectrum.Latex 5 may have a proportion of water such that a mass fraction of the tackifying agent(s) is between 0.20 and 0.70, in particular between 0.25 and 0.40, and preferably between 0.25 and 0.30.

[0083] Indeed, the inventors have discovered that, for a predetermined concentration of acrylic polymer(s), the frequency for which the loss factor is maximum varies in the opposite direction to the mass fraction of the tackifying agent in the first layer. The inventors have thus discovered the range of mass fraction of the tackifying agent in the latex 5 for which the frequency^ is included in the audible frequency spectrum. Moreover, the value of the loss factor tanô of the material of the viscoelastic damping layer 4 is little dependent on the mass fraction of the tackifying agent in the latex 5.

[0084] With reference to [Fig. 3], curve (a) illustrates a loss factor of a layer different from the viscoelastic damping layer 4, manufactured from an adhesive which does not allow the manufacture of a layer having the optical properties of the viscoelastic damping layer 4, differently from the viscoelastic damping layer 4 obtained by the method 100. Curve (b) illustrates a loss factor of the viscoelastic damping layer 4, the mass fraction of the acrylic polymers being equal to 0.58, the mass fraction of plasticizing agent in the viscoelastic damping layer 4 being equal to 0.08 and the mass fraction of tackifying agent in the viscoelastic damping layer 4 being equal to 0.34.Curve (c) illustrates a loss factor of the viscoelastic damping layer 4, the mass fraction of acrylic polymers being equal to 0.55, the mass fraction of plasticizing agent in the viscoelastic damping layer 4 being equal to 0.12 and the mass fraction of tackifying agent in the viscoelastic damping layer 4 being equal to 0.32. Curve (d) illustrates a loss factor of the viscoelastic damping layer 4, the mass fraction of acrylic polymers being equal to 0.53, the mass fraction of plasticizing agent in the viscoelastic damping layer 4 being equal to 0.16 and the mass fraction of tackifying agent in the viscoelastic damping layer 4 being equal to 0.31.Curve (e) illustrates a loss factor of the viscoelastic damping layer 4, the mass fraction of acrylic polymers being equal to 0.49, the mass fraction of plasticizing agent in the viscoelastic damping layer 4 being equal to 0.09 and the mass fraction of tackifying agent in the viscoelastic damping layer 4 being equal to 0.43. Curve (f) illustrates a loss factor of the viscoelastic damping layer 4, the mass fraction of acrylic polymers being equal to 0.48, the mass fraction of plasticizing agent in the viscoelastic damping layer 4 being equal to 0.10 and the mass fraction of tackifying agent in the viscoelastic damping layer 4 being equal to 0.42.Curve (g) illustrates a loss factor of the viscoelastic damping layer 4, the mass fraction of acrylic polymers being equal to 0.46, the mass fraction of plasticizing agent in the viscoelastic damping layer 4 being equal to 0.14 and the mass fraction of tackifying agent in the viscoelastic damping layer 4 being equal to 0.41. Curve (h) illustrates a loss factor of the viscoelastic damping layer 4, the mass fraction of acrylic polymers being equal to 0.42, the mass fraction of plasticizing agent in the viscoelastic damping layer 4 being equal to 0.09 and the mass fraction of tackifying agent in the damping layer . viscoelastic 4 being equal to 0.49.

[0085] With reference to [Fig. 4], curve (i) illustrates a real part G' of the shear modulus of a layer different from the viscoelastic damping layer 4, manufactured from an adhesive which does not allow the manufacture of a layer having the optical properties of the viscoelastic damping layer 4, differently from the interface obtained in the embodiments of the invention. Curve (j) illustrates the real part G' of the shear modulus of the viscoelastic damping layer 4, the mass fraction of the acrylic polymers being equal to 0.58, the mass fraction of plasticizing agent in the viscoelastic damping layer 4 being equal to 0.08 and the mass fraction of tackifying agent in the viscoelastic damping layer 4 being equal to 0.34.Curve (k) illustrates the real part G' of the shear modulus of the viscoelastic damping layer 4, the mass fraction of acrylic polymers being equal to 0.55, the mass fraction of plasticizing agent in the viscoelastic damping layer 4 being equal to 0.12 and the mass fraction of tackifying agent in the viscoelastic damping layer 4 being equal to 0.32. Curve (1) illustrates the real part G' of the shear modulus of the viscoelastic damping layer 4, the mass fraction of acrylic polymers being equal to 0.53, the mass fraction of plasticizing agent in the viscoelastic damping layer 4 being equal to 0.16 and the mass fraction of tackifying agent in the viscoelastic damping layer 4 being equal to 0.31.Curve (m) illustrates the real part G' of the shear modulus of the viscoelastic damping layer 4, the mass fraction of acrylic polymers being equal to 0.49, the mass fraction of plasticizing agent in the viscoelastic damping layer 4 being equal to 0.09 and the mass fraction of tackifying agent in the viscoelastic damping layer 4 being equal to 0.43. Curve (n) illustrates the real part G' of the shear modulus of the viscoelastic damping layer 4, the mass fraction of acrylic polymers being equal to 0.48, the mass fraction of plasticizing agent in the viscoelastic damping layer 4 being equal to 0.10 and the mass fraction of tackifying agent in the viscoelastic damping layer 4 being equal to 0.42.Curve (o) illustrates the real part G' of the shear modulus of the viscoelastic damping layer 4, the mass fraction of acrylic polymers being equal to 0.46, the mass fraction of plasticizing agent in the viscoelastic damping layer 4 being equal to 0.14 and the mass fraction of tackifying agent in the viscoelastic damping layer 4 being equal to 0.41. Curve (p) illustrates the real part G' of the shear modulus of the viscoelastic damping layer 4, the mass fraction of acrylic polymers being equal to 0.42, the mass fraction of plasticizing agent in the viscoelastic damping layer 4 being equal to 0.09 and the mass fraction of tackifying agent in the damping layer . viscoelastic 4 being equal to 0.49.

[0086] The latex 5 may have a mass fraction of the acrylic polymer(s) of between 0.20 and 0.60, a mass fraction of the plasticizing agent(s) of between 0.05 and 0.25 and a mass fraction of the tackifying agent(s) of between 0.20 and 0.70.

[0087] The latex 5 may have a mass fraction of the acrylic polymer(s) of between 0.20 and 0.50, a mass fraction of the plasticizing agent(s) of between 0.07 and 0.18 and a mass fraction of the tackifying agent(s) of between 0.25 and 0.40.

[0088] The latex 5 may have a mass fraction of the acrylic polymer(s) of between 0.20 and 0.30, a mass fraction of the plasticizing agent(s) of between 0.09 and 0.15 and a mass fraction of the tackifying agent(s) of between 0.25 and 0.35.

[0089] Deposition of latex 5

[0090] With reference to [Fig. 5], during the first step 101, the deposition is carried out by spraying the latex 5 onto the first face 6. A nozzle 11 may be supplied with both the latex 5 and a spray gas, in particular air. The latex 5 may be sprayed towards the first face 6, at the outlet of the nozzle 11 by hydrodynamic instability. A spray gun may comprise the nozzle 11. The nozzle 11 may have an outlet orifice having a diameter equal to 1.5 mm. The spray gun may be configured to envelop the flow of sprayed latex with an air flow so as to flatten the section of the flow of sprayed latex. In this configuration, the gun comprises an auxiliary air cap. The nozzle 11 can be moved so as to sweep a surface opposite the first face 6 to allow the latex 5 to be sprayed homogeneously onto the first face 6.The inventors have discovered that the deposition of the latex 5 by spraying allows the glazed assembly 1 to have optical properties, in particular to have a transmission factor, a haze factor and a clarity factor, sufficient for the glazed element 1 to be used in a vehicle. Preferably, the glazed element 1 has the optical properties previously defined.

[0091] With reference to [Fig. 6], the deposition of latex 5 can be carried out only on the first face 6 during the first step 101. With reference to [Fig. 7], during the first step 101, a second layer 10 of latex 5 can be deposited by spraying the latex 5 onto a second face 7 of the second glass sheet 3, so that the deposition of the latex 5 is carried out both on the first face 6 and on the second face 7. In this embodiment of the invention, during the second step 102, the second layer 10 of latex 5 deposited during the first step 101 is dried. During the third step 103, the second glass sheet 3 is superimposed on the first layer 9 of dried latex during the second step by bringing the first layer 9 of dried latex into contact with the second layer 10 of dried latex. During the fourth debubbling step 104, the assembly formed by the first glass sheet 2, by the first layer 9 of dried latex, by the second layer 10 of dried latex and by the second glass sheet 3 is placed in the enclosure 8 in which the pressure is less than 100 mbar, the first layer 9 and the second layer 10 forming at least in part, after the fourth step 104, the viscoelastic damping layer 4. Thus, it is possible to improve the optical properties of the glazed assembly 1. Indeed, the inventors have discovered that the interface between the glass and the dried latex is a significant source of optical defects.Since the latex 5 is deposited in the liquid state on both the first face 6 and the second face 7, the formation of optical defects at the interface between the glass and the latex is minimized. In addition, the inventors have discovered that the thicker a latex layer is at the time of deposition, the more its drying can lead to optical defects. Indeed, an increased thickness of the deposited latex layer leads to increased cracking of the layer during its drying during the evaporation of the water it contains. Thus, by depositing a latex layer on the first face 6 and a latex layer on the second face 7, it is possible to reduce the thickness of the layers to be dried for a predetermined viscoelastic layer thickness 4 and thus to reduce the quantity of optical defects.

[0092] Dilution of latex 5

[0093] [Tables 1] type of acrylic polymer presence of plasticizer and tackifier Anionic surfactant Other type of surfactant mass fraction of water in latex transmission factor haze factor clarity factor AC 75011 no no no 0.41 92.5 4.9 46.7 AC 75011 no no no 0.61 91.2 0.34 99.7 AC 75011 no no no 0.61 90.5 2.9 97.3 AC 75011 yes no no 0.44 91.1 0.72 99.7 AC 75011 yes yes no 0.44 91.2 0.78 99.7 AC 75011 yes no yes 0.56 89.2 7 97

[0094] During the first step 101, the latex 5 may have a mass fraction of water of between 0.42 and 0.70 inclusive, in particular of between 0.42 and 0.65 inclusive and preferably of between 0.42 and 0.50. Thus, the dilution of the latex 5 is high enough for the latex 5 to be sprayed, and small enough not to degrade the optical properties of the glazed element 1. Indeed, bubbles and / or an increase in the haze factor may be caused by excessive dilution. In addition, the evaporation of too much water from the latex layer 5 during drying of the latex layer may reduce the optical properties of the glazed element 1.

[0095] Surface tension

[0096] During the first step 101, the latex 5 may have a surface tension of between 32 Nm and 42 Nm, in particular between 34 Nm and 40 Nm and preferably between 36 Nm and 38 Nm. Thus, it is possible to manufacture a glazed assembly 1 having optical properties of light transmission factor, haze factor and clarity factor comparable to a glazed assembly manufactured from a latex 5 having a surface tension outside the ranges defined above, while reducing the formation of bubbles and dendrites during the manufacture of the glass assembly 1.

[0097] The latex 5 may comprise an anionic surfactant. Thus, it is possible to manufacture a glazed assembly 1 having optical properties of light transmission factor, haze factor and clarity factor comparable to a glazed assembly manufactured from a latex 5 not comprising an anionic surfactant, while reducing the formation of bubbles and dendrites during the manufacture of the glazed assembly 1. The concentration of anionic surfactant in the latex 5 may be between 1 mM and 50 mM, in particular between 3 mM and 10 mM and preferably between 6 mM and 8 mM. The anionic surfactant may comprise at least one sulfonate group and preferably at least two sulfonate groups. In particular, the anionic surfactant may comprise a pair of sulfonate groups on a diphenyl oxide backbone, in particular comprising a linear or branched alkyl group, itself comprising from six to sixteen carbon atoms.Dow brand (registered trademark) "dowfax" anionic surfactant may be used.

[0098] Second step 102

[0099] The method comprises a second step 102 of drying the latex layer 5 deposited during the first step 101. The second step 102 allows the extraction by evaporation of the water and any solvents from the latex layer(s) deposited during the first step 101.

[0100] The latex layer may be dried in an atmosphere having a temperature maintained between 30°C and 80°C, in particular between 30°C and 50°C and preferably between 30°C and 40°C. This temperature range makes it possible to avoid the appearance of bubbles in the latex layer while avoiding the appearance of a crust and cracks on the surface of the latex layer during drying, which would prevent the water from evaporating.

[0101] The latex layer may be dried for a period of more than 20 minutes, in particular more than 40 minutes and preferably more than one hour. Thus, it is possible to evaporate all of the water contained in the latex layer at the end of the first step 101 in the temperature range previously defined for the drying of the second step 102. The temperature range and the drying duration previously defined for the second step 102 make it possible to avoid the formation of a cracked viscoelastic damping layer 4.

[0102] Third step 103

[0103] The method comprises a third step 103 of superimposing the second glass sheet 3 on the latex layer dried during the second step 102. The second glass sheet 3 can be chemically toughened and have a thickness e2 of between 0.5 mm and 3 mm. Thus, it is possible to bend the second glass sheet 3 when bringing the second glass sheet 3 into contact with the first layer 9 of dried latex, so as to avoid the formation of air bubbles when superimposing the second sheet of glass 3 on the first layer 9 of dried latex.

[0104] Fourth step 104

[0105] The method 100 comprises a fourth step 104 of debubbling. During the fourth step 104, the assembly formed by the first glass sheet 2, by the first layer 9 of dried latex, by the second glass sheet 3 and possibly by the second layer 10 of dried latex, is placed in an enclosure 8 in which the pressure is less than 100 mbar, in particular less than 50 mbar and preferably less than 10 mbar. The temperature in the enclosure 8 is between 70°C and 120°C, in particular between 80°C and 100°C and preferably between 85°C and 95°C. The dried latex layer(s) form(s), after the fourth step 104, the viscoelastic damping layer 4. The assembly formed by the first glass sheet 2, the viscoelastic damping layer 4 and the second glass sheet 3 forms the glazed assembly 1.

[0106] The enclosure 8 may be a flexible pocket formed around the first glass sheet 2, the dried latex layer and the second glass sheet 3.

[0107] During the fourth step 104, the temperature between 70°C and 120°C can be maintained for a period of more than 30 minutes and preferably more than 45 minutes.

Claims

Claims

1. A method of manufacturing a glazed assembly (1) comprising a first glass sheet (2), a second glass sheet (3) and a viscoelastic damping layer (4) for the acoustic attenuation of a vehicle, the viscoelastic damping layer (4) being arranged between the first glass sheet (2) and the second glass sheet (3) and being in direct contact with the first glass sheet (2), the viscoelastic damping layer (4) being formed by a material comprising: - at least one acrylic polymer, - at least one tackifying agent, and - at least one plasticizing agent, the method comprising: - a first step (101) of depositing a first layer (9) of latex (5) on a first face (6) of the first glass sheet (2), the deposition being carried out by spraying a latex (5) on the first face (6), the latex (5) comprising the acrylic polymer, the tackifying agent, and the plasticizing agent, - a second step (102) of drying the first layer (9) of latex (5) deposited during the first step (101), - a third step (103) of superimposing the first glass sheet (2) on the second glass sheet (3) so that the first layer (9) of latex dried during the second step is arranged between the first glass sheet (2) and the second glass sheet (3), - a fourth step (104) of debubbling, during which the assembly formed by the first glass sheet (2), by the first layer (9) of dried latex and by the second glass sheet (3) is arranged in an enclosure (8) in which the pressure is less than 100 mbar, the first layer (9) of dried latex forming at least in part the viscoelastic damping layer (4).

2. Method according to the preceding claim, in which: - during the first step (101), a second layer (10) of latex (5) is deposited by spraying the latex (5) onto a second face (7) of the second sheet of glass (3), - during the second step (102), the second layer (10) of latex deposited during the first step (101) is dried, - during the third step (103), the second glass sheet (3) is su- perposed to the first layer (9) of dried latex during the second step by bringing the first layer (9) of dried latex into contact with the second layer (9) of dried latex, - during the fourth step (104) of debubbling, the assembly formed by the first glass sheet (2), by the first layer (9) of dried latex, by the second layer (9) of dried latex and by the second glass sheet (3) is arranged in the enclosure (8) in which the pressure is less than 100 mbar, the first layer (9) and the second layer (10) forming at least in part, after the fourth step, the viscoelastic damping layer (4).

3. Method according to one of the preceding claims, in which a mass fraction of the acrylic polymer(s) in the dry matter of the latex (5) is between 0.21 and 0.

62.

4. Method according to one of the preceding claims, in which a mass fraction of the tackifying agent(s) in the dry matter of the latex (5) is between 0.17 and 0.

60.

5. Method according to one of the preceding claims, in which a mass fraction of the plasticizing agent(s) in the dry matter of the latex (5) is between 0.07 and 0.

43.

6. Method according to one of the preceding claims, in which, during the first step (101), the latex (5) has a surface tension of between 32 Nm and 42 Nm, in particular between 34 Nm and 40 Nm and preferably between 36 Nm and 38 Nm.

7. Method according to one of the preceding claims, in which, during the first step (101), the latex (5) has a mass fraction of water of between 0.42 and 0.

70.

8. Method according to one of the preceding claims, in which the latex (5) comprises an anionic surfactant.

9. Method according to the preceding claim, in which a concentration of the anionic surfactant is between 1 mM and 50 mM, in particular between 3 mM and 10 mM and preferably between 6 mM and 8 mM.

10. The method of claim 8 or 9, wherein the anionic surfactant comprises at least one sulfonate group.

11. Method according to one of the preceding claims, in which the tackifying agent comprises a hydrogenated resin and preferably a hydrogenated rosin resin.

12. A method according to any preceding claim, wherein the or

13.

14. the acrylic polymer(s) are formed from monomers selected from the group consisting of methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, propyl acrylate, propyl methacrylate, isopropyl acrylate, isopropyl methacrylate, butyl acrylate, butyl methacrylate, isobutyl acrylate, isobutyl methacrylate, tert-butyl acrylate, tert-butyl methacrylate, pentyl acrylate, pentyl methacrylate, isoamyl acrylate, isoamyl methacrylate, hexyl acrylate, hexyl methacrylate, cyclohexyl acrylate, cyclohexyl methacrylate, octyl acrylate, methacrylate octyl, isooctyl acrylate, isooctyl methacrylate, nonyl acrylate, nonyl methacrylate, isononyl acrylate, isononyl methacrylate, isobutyl methacrylate, decyl acrylate, decyl methacrylate, dodecyl acrylate, dodecyl methacrylate,tridecyl acrylate, tridecyl methacrylate, hexadecyl acrylate, hexadecyl methacrylate, octadecyl acrylate, octadecyl methacrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, vinyl formate, vinyl acetate, vinyl propionate, 2-hydroxyethyl acrylate, hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, 2-hydroxypropyl methacrylate, acrylic acid, styrene and acrylonitrile., Method according to one of the preceding claims, in which, during the second step (102), the latex layer is dried in an atmosphere having a temperature maintained between 30°C and 80°C, for a period greater than 20 minutes. Glazed assembly (1) for a vehicle obtained by a method according to one of claims 1 to 13, the glazed assembly (1) comprising a first glass sheet (2) and a second glass sheet (3) superimposed, the glazed assembly (1) comprising a viscoelastic damping layer (4) for acoustic attenuation of the vehicle, the viscoelastic damping layer (4) being formed by a material comprising: - at least one acrylic polymer, - at least one tackifying agent, and - at least one plasticizing agent, the viscoelastic damping layer (4) being arranged between the first glass sheet (2) and the second glass sheet (3) and being in direct contact with the first sheet of glass (2).

15. Glazed assembly (1) according to the preceding claim, in which the viscoelastic damping layer (4) has a thickness of between 5 μm and 500 μm.