METHOD FOR COATING A SUBSTRATE WITH TETRAGONAL VANADIUM NITRID

The high-power pulsed magnetron cathode sputtering process stabilizes tetragonal vanadium nitride coatings at room temperature, addressing the need for an alternative to hard chrome that meets environmental and performance criteria, offering stable and homogeneous coatings for diverse applications.

FR3148041A1Active Publication Date: 2024-10-25SAFRAN SA +3
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
FR2023003986
Authority / Receiving Office
FR · FR
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-20
Publication Date
2024-10-25
Estimated Expiration
2043-04-20

AI Technical Summary

Technical Problem

There is a need for an alternative coating to hard chrome that offers equivalent physical, chemical, and wear resistance properties, is stable at ambient temperature, and complies with the REACH directive, while being simple, effective, and economically viable.

Method used

A process for coating substrates with tetragonal vanadium nitride using high-power pulsed magnetron cathode sputtering, involving a controlled polarization of the target under specific conditions of pressure, temperature, and gas mixture, stabilizing the tetragonal crystallographic phase of vanadium nitride at room temperature.

Benefits of technology

The process achieves stable, dense, and homogeneous tetragonal vanadium nitride coatings with controlled microstructure, providing equivalent properties to hard chrome, suitable for various environments and applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

The invention relates to a method for coating a substrate with tetragonal vanadium nitride using the high-power pulsed magnetron sputtering technique. It also relates to a substrate coated with at least one layer of tetragonal vanadium nitride. The method of the invention is of particular interest in the fields of electronic components, sensor transducers, optics, mechanics and micromechanics, surface decoration and protection, automotive, aeronautics, and aerospace. Figure 1 (for the abstract)
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: METHOD FOR COATING A SUBSTRATE WITH TETRAGONAL VANADIUM NITRIDE Technical field of the invention

[0001] The present invention relates to the general field of producing thin layers and more particularly to the metallization of various substrates. It relates more particularly to a method of coating a substrate with tetragonal vanadium nitride using the high-power pulsed magnetron sputtering technique as well as a substrate coated with at least one layer of tetragonal vanadium nitride.

[0002] The method and the substrate of the invention are of particular interest in the field of electronic components, transducers for sensors, optics, photonics, mechanics and micromechanics, decoration and protection of surfaces, automobiles, aeronautics and aerospace. Technical background

[0003] To improve the properties of metallic, composite, polymer or other materials, particularly in terms of resistance to corrosion and / or wear, the substrates are covered with a protective layer.

[0004] The coating commonly called hard chrome has numerous physical, chemical and wear resistance properties in various environments, which make it one of the most widely used versatile coatings and whose applications are found in different industrial sectors (machining, land, air or space transport). Hard chrome is obtained by electrolytic chromium deposition involving the presence of hexavalent chromium (Cr6+). However, the latter has carcinogenic, mutagenic and reprotoxic (CMR) properties, which are not compatible with the REACH directive (a European Union regulation adopted to better protect human health and the environment against risks related to chemical substances, while promoting the competitiveness of the EU chemical industry). However, hard chrome has versatile properties that are difficult to match with a single universal solution.

[0005] The family of transition metal nitrides has different similar structural and functional properties which, for certain applications, can position them as an alternative solution to the use of hard chromium.

[0006] The ban by the REACH directive on the use of hexavalent chromium (Cd,+) present during the production of electrolytic chromium or hard chromium deposits led the inventors of the present invention to study metal nitrides of transition, including vanadium nitride, in order to approach the structural and functional properties of hard chromium. Vanadium nitride was therefore explored and its tribological properties studied. Hardness, electrical resistivity, thermal conduction, etc. are all interesting properties to develop, in line with the field concerned.

[0007] Vanadium nitrides have already been studied by researchers. Different crystallographic phases of vanadium nitride are predicted by ab initio calculations

[0008] In 1988, F. Kubel et al., Physical Review B, 1988, vol. 38, no. 18, 12908-12912, obtained the tetragonal phase of vanadium nitride at a transition temperature of 205 K (-68°C). This metastable phase was not stabilized at temperatures above 205 K (-68°C). Furthermore, the material was not in the form of a coating but in the form of a powder.

[0009] The study of metastable phases of vanadium nitride not present on the binary VN phase diagram whatever the temperature (> 0°C) and the nitrogen stoichiometry, was carried out from ab initio calculations with the aim of understanding the stabilization of these phases.

[0010] Vanadium nitrides have also been studied as hardening reinforcements for steels.

[0011] AB Mei et al. (Physical Review B, vol. 91, no. 5, 054101) developed thin films of cubic phase vanadium nitride by direct current magnetron sputtering (dcMS). The authors also sought to study, by ab initio molecular dynamics calculations, the transition from the cubic phase to the tetragonal phase occurring at 205 K in order to correlate them with analyses carried out at temperatures below 205 K by X-ray diffraction and transmission electron microscopy.

[0012] There is therefore a real need to have an alternative coating to hard chrome having at least equivalent physical, chemical and wear resistance properties.

[0013] In particular, there is a real need to have an alternative coating to hard chrome having at least equivalent physical, chemical and wear resistance properties, and which is stable at room temperature (20 ± 5°C).

[0014] More particularly, there is a real need to have an alternative coating to hard chrome as described above which is compatible with the REACH directive and whose implementation is simple, effective and economical and therefore industrially interesting. Summary of the invention

[0015] The present invention relates to a method of coating a substrate with nitride of tetragonal vanadium by the high-power pulsed magnetron sputtering technique, characterized in that the coating of the substrate is carried out in a deposition chamber in which the vanadium is in the form of a massive vanadium target, facing which is the substrate to be coated,

[0016] the coating process taking place

[0017] - at a pressure between 0.1 and 20 Pa,

[0018] and

[0019] - at a temperature between room temperature (20 ± 5°C) and 900°C, and

[0020] - under an atmosphere containing a mixture of nitrogen and argon with a content of nitrogen between 5 and 99%,

[0021] the polarization of the target being controlled during the deposition of the coating by imposing on it a superposition of a continuous polarization at a potential (Vc) between 0 and -900V and a pulsed polarization whose pulses have a potential (Vp) between -1200 and -100V.

[0022] The polarization of the target can be maintained for a duration of between 10 and 900 ps.

[0023] The polarization of the target can be carried out at a frequency between 100 and 9000 Hz.

[0024] The device for carrying out deposition by high-power pulsed magnetron cathode sputtering comprising a deposition enclosure or chamber illustrated in [Fig.l] and described in detail in application FR 3 097 237, is entirely suitable for implementing the method of the invention.

[0025] As already indicated, the tetragonal crystallographic phase of vanadium nitride was predicted by calculations as a metastable phase, but could never be stabilized or observed at room temperature (20 ± 5°C). However, the inventors succeeded in obtaining and stabilizing the tetragonal crystallographic phase of vanadium nitride at room temperature (20 ± 5°C) and in characterizing it, thanks to the use and control of the parameters of a high power pulsed magnetron sputtering (HiPIMS) process, which has never been done to date.

[0026] In the high power pulsed magnetron sputtering (HiPIMS) technique, the target is polarized in a particular way to form a tetragonal vanadium nitride coating which constitutes a material satisfactory in terms of its physical, chemical and wear resistance properties in various environments, for the replacement of hard chrome.

[0027] The invention also relates to a substrate coated with at least one thin layer of tetragonal vanadium nitride.

[0028] Indeed, the method of the invention can make it possible to coat the substrate with one or more several thin layer(s) of tetragonal vanadium nitride depending on the operating conditions chosen.

[0029] When the substrate is coated with several layers, said layers can optionally be detected according to their microstructure. In HiPIMS, the layers will be dense and the distinction between two layers can be made, for example, by scanning electron microscopy (SEM). It is also conceivable to coat the substrate with one or more thin layer(s) of tetragonal vanadium nitride and / or one or more layers of different materials and / or vanadium nitride of different phases.

[0030] The high-power pulsed magnetron sputtering (HiPIMS) technology implemented by the method of the invention makes it possible to develop dense, homogeneous and defect-free coatings, whose microstructure and chemical composition are perfectly controlled. The method of the invention adds new modifiable parameters such as, for example, the intensity and duration of the pulse, the frequency, etc. to those usually optimized for magnetron sputtering deposition, which has allowed the stabilization of new metastable crystalline phases.

[0031] Thus, the method of the invention is particularly interesting because it allows the stabilization at room temperature (20 ± 5°C), of the tetragonal vanadium nitride phase thanks to the use of high power pulsed magnetron sputtering (HiPIMS). This phase, not predicted in the phase diagram and observed only once experimentally in powder during a phase change at low temperature (205 K) of the cubic phase, has never been able to be characterized at room temperature (20 ± 5°C). Brief description of the figures

[0032] Other characteristics and advantages of the invention will appear during reading of the detailed description which follows and of the appended figures.

[0033] [Fig. 1] schematically represents a deposition chamber in which a process for coating a substrate with tetragonal vanadium nitride is carried out using the high-power pulsed magnetron cathode sputtering technique according to one embodiment of the invention.

[0034] [Fig.2] represents a PANalytical X'Pert Pro X-ray diffractogram of 316L stainless steel substrates of dimensions 2.5 cm x 2.5 cm and thickness 500 μm, coated with a layer of tetragonal vanadium nitride according to the method of the invention. Starting from the bottom, the first diffractogram is that of the bare substrate, i.e. the part on which the coating is deposited. The two diffractograms in the middle and at the top are the diffractograms of two tetragonal VN deposits carried out one month interval. By comparing the peaks and diffraction angles, we observe the reproducibility of the method of the invention.

[0035] The X-rays penetrate the sample (i.e. substrate + coating) with a depth greater than that of the coating. Therefore, on the diffractogram of the sample (the middle and top diffractograms), peaks corresponding to the coating and peaks corresponding to the substrate are observed. The diffractogram of the uncoated metal substrate makes it possible to recognize on the diffractogram of the sample, the peaks of the substrate and the peaks of the coating. Detailed description of the invention

[0036] The present invention relates to a method for coating a substrate with tetragonal vanadium nitride using the high-power pulsed magnetron sputtering technique, characterized in that the coating of the substrate is carried out in a deposition chamber in which the vanadium is in the form of a massive vanadium target, facing which is the substrate to be coated,

[0037] the coating process taking place

[0038] - at a pressure between 0.1 and 20 Pa,

[0039] and

[0040] - at a temperature between room temperature (20 ± 5°C) and 900°C, and

[0041] - under an atmosphere containing a mixture of nitrogen and argon with a content of nitrogen between 5 and 99%,

[0042] the polarization of the target being controlled during the deposition of the coating by imposing on it a superposition of a continuous polarization at a potential (Vc) between 0 and -900V and a pulsed polarization whose pulses have a potential (Vp) between -1200 and -100V.

[0043] In the context of the present invention, the expression “massive vanadium target” designates a vanadium target whose purity is at least 99.5% by mass of vanadium.

[0044] The polarization of the target can be carried out at a frequency between 100 and 9000 Hz.

[0045] According to one embodiment, the coating process takes place at a pressure of 1 Pa.

[0046] Even if an atmosphere containing a mixture of nitrogen and argon as described above is preferred, it may be envisaged to implement the coating method of the invention under a nitrogen atmosphere mixed with other plasma-forming gases known to those skilled in the art.

[0047] In the context of the invention, the expression "between ... and ..." must be understood as including the limits.

[0048] In the context of the invention, the expression “greater than... or less than...” should be understood as not including the boundaries.

[0049] The coating is in the form of a thin layer.

[0050] The thin layer is produced in a low-pressure deposition chamber, the base vacuum of which is less than 10 4 mbar, preferably less than 106 mbar. The vanadium is present in the deposition chamber in the form of a massive vanadium target, facing which is the substrate to be coated. The target constitutes the cathode. The substrate to be coated constitutes an anode.

[0051] The substrate is maintained at a temperature between room temperature (20 ± 5°C) and 900°C for the entire duration of the deposition.

[0052] During deposition, a mixture of plasma gases as described above is introduced into the deposition chamber. The target is in contact with a cooled cathode coupled to permanent magnets while the substrate is connected to ground or possibly positively polarized or left at floating potential. A potential difference is imposed between the two electrodes, making it possible to reach the breakdown voltage of the gas or gas mixture to initiate a low-pressure plasma, i.e. a pressure between 1.10 4 to 1 mbar, in particular between 103 and 5.10-1 mbar during deposition.

[0053] In addition to the continuous electric field (from 0 to -900V or from -100 to -600V according to another embodiment), the generator transmits a high voltage pulsed current. The voltages used are between -1200 and -100V or -1000 and -500V according to another embodiment. The voltage peaks are maintained for durations between 10 and 900 ps or between 50 and 400 ps according to another embodiment, and frequencies of 100 and 9000 Hz or from 100 to 5000 Hz according to another embodiment.

[0054] As previously indicated, the coating process takes place under an atmosphere containing nitrogen mixed with argon, with a nitrogen content of between 5 and 99%.

[0055] The thickness of each layer of coating / tetragonal vanadium nitride deposited on the substrate may be between 5 nm and 15 pm. When the coating is in the form of a multi-layer, the thickness of the multi-layer may be between 10 nm and 100 pm, for example.

[0056] The diffractograms of 316L stainless steel substrates with dimensions of 2.5 cm x 2.5 cm and thickness of 500 μm, coated with a layer of stabilized tetragonal vanadium nitride and obtained by the process of the invention, carried out using a PANalytical X'Pert Pro X-ray diffractometer, clearly show the characteristic peaks of tetragonal vanadium nitride as shown in [Fig.2], thus confirming that the parameters of the process of the invention described above indeed allow the obtaining of a coating of Ipm thickness by the process of the invention based on the use of the HiPIMS technology to stabilize the tetragonal phase of vanadium nitride.

[0057] The invention also relates to a substrate coated with at least one thin layer of tetragonal vanadium nitride.

[0058] The method of the invention applies to the coating of a wide variety of substrates depending on the intended application, provided that they can withstand a temperature of 40°C.

[0059] The substrate may be metallic, ceramic, composite, elastomer, glass, metallic glass, plastic, fabric.

[0060] In one embodiment, the substrate is a stainless steel, such as 316L stainless steel.

[0061] In one embodiment, the substrate is an aircraft part such as for example an aircraft landing gear part or aircraft engine turbine part.

[0062] In one embodiment, the substrate is a part of gas turbines or marine turbines.

[0063] The method of the invention is of particular interest in the field of electronic components, transducers for sensors, optics, photonics (i.e. lasers, light-emitting diodes, optical fibers, optical modulators, optical amplifiers or even photonic crystals, lenses, prisms, and networks), mechanics and micromechanics, decoration and protection of surfaces, automobiles, aeronautics or even aerospace.

[0064] Another object of the invention is therefore the use of the method of the invention for the manufacture of electronic components, transducers for sensors, optical and photonic components, mechanical and micromechanical components, components for the decoration and protection of surfaces, components for the automobile, aeronautics or even aerospace industries. EXAMPLES

[0065] The coating is deposited on 316L stainless steel substrates. The substrate is previously cleaned by immersion in a beaker of boiling isopropanol. The base vacuum of the enclosure reached before deposition is 3.0E-6 T. The plasma is initiated at 5 Pa in an Argon / Nitrogen mixture. The imposed voltage and current are -1000 V and 200 mA respectively, with a continuous background of -50 V and 10 mA. The frequency and width of the high power pulse (HiPIMS) are 100 Hz and 200 ps respectively. The pressure is then decreased to 1 Pa. The enclosure is preheated to 400°C under an Ar / N2 mixture at 1 Pa, 40 sccm of Argon, 5 sccm of Nitrogen. The Ar / N2 mixture can be described by the percentage of N2 in the total volume of gas [Ar+NJ. It is 5 / (40+5) = 11%. The ratio can, however, be a good way to describe the process (N2 ratio = N2 flow rate / Ar flow rate). The Nitrogen ratio is 12.5. The plasma is stabilized at this point in the process for 15 minutes and then the substrate is brought in front of the Vanadium target (purity greater than or equal to 99.9%). The deposition time is 3 hours.

[0066] The thickness of the coating was determined by Scanning Electron Microscopy (SEM JEOL 6360 A) and the crystal structure was determined by X-ray Diffraction (DRX PANalytical X'Pert Pro).

Claims

Claims

1. A method of coating a substrate with tetragonal vanadium nitride using the high-power pulsed magnetron sputtering technique, characterized in that the coating of the substrate is carried out in a deposition chamber in which the vanadium is in the form of a massive vanadium target, facing which is the substrate to be coated, the coating process taking place - at a pressure between 0.1 and 20 Pa, and - at a temperature between room temperature (20 ± 5°C) and 900°C, and - under an atmosphere containing a mixture of nitrogen and argon with a nitrogen content between 5 and 99%, the polarization of the target being controlled during the deposition of the coating by imposing on it a superposition of a continuous polarization at a potential (Vc) between 0 and -900V and a pulsed polarization whose pulses have a potential (Vp) between -1200 and -100 V.

2. Method according to claim 1, characterized in that it takes place at a pressure of 1 Pa.

3. Method according to one of claims 1 or 2, characterized in that the polarization of the target is carried out at a frequency between 100 and 9000 Hz.

4. Method according to any one of claims 1 to 3, characterized in that the polarization of the target is controlled during the deposition of the coating by imposing on it a superposition of a continuous polarization at a potential (Vc) between -100 and -600V.

5. Method according to any one of claims 1 to 4, characterized in that the polarization of the target is controlled during the deposition of the coating by imposing on it a superposition of a continuous polarization at a potential (Vc) as described in claims 1 and 4, and of a pulsed polarization whose pulses have a potential (Vp) between -1000 and -500 V.

6. Method according to any one of claims 1 to 5, characterized in that the substrate is coated with one or more thin layer(s) of tetragonal vanadium nitride, the thickness of each layer being between 5 nm and 15 pm.

7. Method according to claim 6, characterized in that when the coating is in the form of a multi-layer, the thickness of the multi-layer is between 10 and 100 μm.

8. Method according to any one of claims 1 to 7, characterized in that the vanadium is in the form of a massive vanadium target whose purity is at least 99.5% by mass of vanadium.

9. Use of the method according to any one of claims 1 to 8, for the manufacture of electronic components, transducers for sensors, optical components, mechanical and micromechanical components, components for decoration and for the protection of surfaces, components for the automobile, aeronautics or even aerospace industries.

10. Substrate coated with at least one thin layer of tetragonal vanadium nitride by a method according to any one of claims 1 to 8.

11. Substrate according to claim 10, characterized in that it is - a part of aircraft landing gear, or - a part of aircraft engine turbines, or - a part of gas turbines or turbines of the marine industry.

Citation Information

Patent Citations

  • Sputter device

    EP2325349A1

  • METHOD FOR COATING A SUBSTRATE WITH TANTALUM NITRIDE

    FR3097237A1