Rubber composition
A rubber composition with butyl rubber, fillers, and N,N'-caprolactam disulfide as a sulfur donor addresses the balance between scorch and crosslinking times, enhancing industrial productivity by extending scorch times without degrading crosslinking times.
Patent Information
- Application Number
- FR2023005213
- Authority / Receiving Office
- FR · FR
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-11-29
AI Technical Summary
Manufacturers face the challenge of balancing scorch time and crosslinking time in rubber compositions, as improving scorch time often leads to increased crosslinking time, making it difficult to maintain both properties within industrially acceptable ranges.
A rubber composition comprising butyl rubber, reinforcing and non-reinforcing fillers, and a crosslinking system with N,N'-caprolactam disulfide as the sulfur donor, without soluble or insoluble sulfur, or with limited amounts of soluble sulfur, to achieve longer scorch times while maintaining acceptable crosslinking times.
The composition achieves significantly longer scorch times with minimal impact on crosslinking times, ensuring industrial productivity and efficiency.
Abstract
Description
Title of the invention: Rubber composition technical field
[0001] The field of the invention is that of rubber compositions for rubber products, in particular rubber compositions comprising butyl rubber. Previous technique
[0002] In the field of manufacturing rubber compositions, those skilled in the art know that it is important to allow crosslinking of rubber compositions within industrially acceptable times, while preserving a minimum safety period ("curing time") during which the compositions can be shaped without risk of premature crosslinking ("curing").
[0003] A constant objective of rubber product manufacturers is to ensure sufficient toasting time while maintaining curing time. Finding a good balance between these two properties proves difficult, as improving toasting time often leads to an increase in curing time.
[0004] In this research, patent document JP2004-018682A1 previously proposed combining a diene elastomer with a cobalt salt of an aliphatic or alicyclic carboxylic acid and an aromatic carboxylate. It was thus observed that when a cobalt salt of an aliphatic carboxylic acid and a benzoate are used in combination with a diene elastomer, the roasting time is prolonged while the vulcanization time is shortened.
[0005] Manufacturers of rubber products are constantly seeking solutions to improve the curing properties of their rubber compositions or to shift their equilibrium. Therefore, there is always a need for rubber compositions that exhibit improved curing times while maintaining crosslinking times within an industrially acceptable range. Description of the invention
[0006] Continuing its research, the Applicant found a rubber composition that meets this need. In particular, the Applicant found a rubber composition that exhibits a significantly longer curing time while maintaining a crosslinking time acceptable in terms of industrial productivity compared to a control rubber composition.
[0007] Thus, a first object of the invention is a rubber composition based on at least:
[0008] - an elastomeric matrix comprising at least one butyl rubber;
[0009] - a load comprising at least one reinforcing load and one non-reinforcing load forcing; and
[0010] - a crosslinking system comprising a sulfur donor comprising disulfide of N,N'-caprolactam; and
[0011] wherein the crosslinking system does not comprise soluble sulfur, nor insoluble sulfur, or comprises less than 0.6 pc of soluble sulfur, insoluble sulfur or a mixture of soluble sulfur and insoluble sulfur.
[0012] Another object of the invention is a finished or semi-finished rubber product comprising a rubber composition according to the invention. Summary of the invention
[0013] The invention, described in more detail below, relates to at least one of the embodiments listed in the following points:
[0014] 1. Rubber composition based on at least: - an elastomeric matrix comprising at least one butyl rubber; - a load comprising at least one reinforcing load and one non-reinforcing load; and - a crosslinking system; wherein the crosslinking system comprises from 0.1 part to 8 parts of a sulfur donor comprising N,N'-caprolactam disulfide; and in which the crosslinking system does not comprise soluble sulfur, nor insoluble sulfur, or comprises less than 0.6 pc of soluble sulfur, insoluble sulfur or a mixture of soluble sulfur and insoluble sulfur.
[0015] 2. Rubber composition according to embodiment 1, wherein the matrix elastomer comprises at least 50 pieces of butyl rubber.
[0016] 3. Rubber composition according to embodiment 1 or embodiment 2, in which the elastomeric matrix comprises at least one other diene elastomer selected from the group consisting of polybutadienes (abbreviated "BR"), natural rubber (NR), synthetic polyisoprenes (IR), butadiene copolymers, isoprene copolymers (other than butyl rubber) and mixtures of these elastomers, preferably natural rubber.
[0017] 4. Rubber composition according to any one of the preceding embodiments, in which the elastomer matrix comprises at least one other elastomer in a proportion of less than 50 parts per annum.
[0018] 5. Rubber composition according to any one of the preceding embodiments, in which the reinforcing filler consists mainly of carbon black.
[0019] 6. Rubber composition according to any one of the preceding embodiments, in which the reinforcing filler comprises carbon black in a total proportion of greater than 50% by weight for 100% by weight of the reinforcing load.
[0020] 7. Rubber composition according to any one of the preceding embodiments, in which the reinforcing filler is essentially made of carbon black.
[0021] 8. Rubber composition according to any one of the preceding embodiments, which includes 10 to 60 pieces of carbon black, preferably 20 to 45 pieces.
[0022] 9. Rubber composition according to any one of the preceding embodiments, in which the non-reinforcing filler mainly comprises kaolin, preferably at a rate greater than 50% by weight for 100% by weight of the non-reinforcing filler.
[0023] 10. Rubber composition according to any one of the preceding embodiments, in which the non-reinforcing filler consists of kaolin.
[0024] 11. Rubber composition according to any one of the preceding embodiments, which comprises 10 to 80 parts per annum of kaolin as a non-reinforcing filler, preferably 10 to 70 parts per annum and more preferably 20 to 70 parts per annum.
[0025] 12. Rubber composition according to any one of the preceding embodiments, in which the total charge rate is greater than or equal to 10%, preferably greater than or equal to 20%, and less than or equal to 110%.
[0026] 13. Rubber composition according to any one of the preceding embodiments, in which the total amount of N,N'-caprolactam disulfide is greater than 50% by weight for 100% by weight of the sulfur donor.
[0027] 14. Rubber composition according to any one of the preceding embodiments, in which the sulfur donor contains N,N'-caprolactam disulfide as the sole sulfur donor.
[0028] 15. Rubber composition according to any one of embodiments 1 to 13, in in which the sulfur donor comprises a sulfur donor other than N,N'-caprolactam disulfide.
[0029] 16. Rubber composition according to the preceding embodiment, in which the sulfur donor other than N,N'-caprolactam disulfide is alkylphenol disulfide, N,N'-dimorpholine disulfide or a combination thereof.
[0030] 17. Rubber composition according to any one of the preceding embodiments, in which the sulfur donor rate comprising N,N'-caprolactam disulfide is greater than or equal to 0.1 pc and less than or equal to 5 pc.
[0031] 18. Rubber composition according to any one of the preceding embodiments, in which the sulfur donor rate comprising N,N'-caprolactam disulfide varies from 0.1 to 4 pc, preferably from 0.2 to 3 pc.
[0032] 19. Rubber composition according to any one of the preceding embodiments, in which the N,N'-caprolactam disulfide content varies from 0.1 to 4.0 pc, preferably from 0.2 to 3 pc, preferably again from 0.2 to 2.
[0033] 20. Rubber composition according to any one of the preceding embodiments, in which the N,N'-caprolactam disulfide level varies from 0.2 to 1 pc.
[0034] 21. Rubber composition according to any one of the preceding embodiments, in which, when present, the total amount by weight of soluble sulfur, insoluble sulfur or mixture of soluble and insoluble sulfur is less than that of the sulfur donor.
[0035] 22. Rubber composition according to any one of the preceding embodiments, in which the crosslinking system includes neither soluble nor insoluble sulfur.
[0036] 23. Rubber composition according to any one of the preceding embodiments, in which the crosslinking system further includes at least one vulcanization accelerator.
[0037] 24. Rubber composition according to any one of the preceding embodiments, in which the crosslinking system further comprises at least one vulcanization accelerator selected from the group consisting of sul-fenamide type accelerators, thiazole type accelerators, thiuram type accelerators, dithiocarbamate type accelerators, dithiophosphate type accelerators, thiourea type accelerators and xanthate type accelerators and mixtures thereof.
[0038] 25. Rubber product comprising a rubber composition according to one any of the achievements 1 to 24.
[0039] 26. Rubber product according to embodiment 25, which product is a tire.
[0040] 27. Rubber product according to embodiment 26, which product is a tire whose inner rubber comprises the rubber composition according to any one of embodiments 1 to 24. Definitions
[0041] The expression "composition based on" means a composition comprising the mixture and / or the in situ reaction product of the different constituents used, some of these constituents being able to react and / or being intended to react with each other, at least partially, during the different phases of manufacturing the composition; the composition can thus be in a totally or partially crosslinked state or in a non-crosslinked state.
[0042] By the expression "part by weight per hundred parts by weight of elastomer" (or pce), it is to be understood in the sense of the present invention, the part, by mass per hundred parts by mass of elastomer.
[0043] In the present, unless expressly stated otherwise, all percentages (%) indicated are percentages (%) by mass.
[0044] On the other hand, any range of values designated by the expression "between a and b" re- presents the domain of values from greater than a to less than b (that is, excluding the bounds a and b), while any interval of values designated by the expression "from a to b" means the domain of values from a to b (that is, including the strict bounds a and b). In this context, when an interval of values is designated by the expression "from a to b", it also and preferably designates the interval represented by the expression "between a and b".
[0045] When referring to a "major" compound, for the purposes of this invention, it is understood that this compound is the majority among the compounds of the same type in the composition; that is, it is the one that represents the largest quantity by mass among the compounds of the same type. Thus, for example, a major elastomer is the elastomer representing the greatest mass relative to the total mass of the elastomers in the composition. Similarly, a so-called major filler is the one representing the greatest mass among the fillers in the composition. By way of example, in a system comprising a single elastomer, this elastomer is the major component for the purposes of this invention; and in a system comprising two elastomers, the major elastomer represents more than half of the mass of the elastomers. Conversely, a "minor" compound is a compound that does not represent the largest mass fraction among the compounds of the same type.Preferably, "majority" means a mass proportion of more than 50%; when the compound represents 100% by mass, it is also described as "majority".
[0046] The compounds mentioned in the description may be of fossil origin or bio-based. In the latter case, they may be partially or totally derived from biomass or obtained from renewable raw materials derived from biomass. Similarly, the compounds mentioned may also come from the recycling of materials already in use, that is to say, they may be partially or totally derived from a recycling process, or obtained from raw materials themselves derived from a recycling process. This includes, in particular, polymers, plasticizers, fillers, etc. Detailed description of the invention 1. Elastomer matrix
[0047] By "elastomer matrix", we mean the set of elastomers in the composition.
[0048] 1.1 Butyl rubber
[0049] According to the invention, the elastomer matrix comprises a butyl rubber.
[0050] In a known manner, butyl rubber is understood to be a C4-C6 isobutylene-diene copolymer, preferably isoprene (abbreviated IIR), as well as halogenated versions, preferably chlorinated or brominated, of this type of copolymer. According to the invention, butyl rubber is also understood to be a mixture of rubbers Butyl. Generally, butyl rubbers contain 1 to 5% by mole of diene units, particularly isoprene.
[0051] Halogenated butyl rubbers are obtained by halogenation, in particular by chlorination or bromination of C4-C6 isobutylene-diene copolymers, especially isoprene. The halogen content in the halogenated butyl rubber is preferably in the range of 1 to 4% by weight relative to the weight of the butyl rubber.
[0052] Preferably, according to the invention, the butyl rubber is a halogenated butyl rubber, preferably chlorinated or brominated, and more preferably a brominated butyl rubber. Even more preferably, the butyl rubber is a copolymer of halogenated isobutylene and isoprene (XIIR), preferably chlorinated (CIIR) or brominated (BIIR). Preferably, the butyl rubber useful for the purposes of the invention is a copolymer of isobutylene and brominated isoprene (BIIR).
[0053] By extension of the definition of butyl rubber, butyl rubber can also be a terpolymer of isobutylene, paramethylstyrene and halogenated paramethylstyrene, preferably brominated, marketed under the names Bromobutyl or Exxpro of Exxon or X BUTYLTM BB 2030 of Arlanxeo.
[0054] Advantageously, butyl rubber is the major elastomer of the elastomer matrix. To this end, preferably, the proportion of butyl rubber in the composition according to the invention is at least 50 parts per cent, preferably varies in a range from 50 parts per cent to 100 parts per cent, preferably from 60 parts per cent to 100 parts per cent, and preferably again from 65 parts per cent to 100 parts per cent.
[0055] 1.2 Other elastomer
[0056] The elastomeric matrix of the composition according to the invention may contain one or more different diene elastomers (hereinafter referred to as "other diene elastomer" for the sake of simplicity of writing) of the butyl rubber used in the context of the present invention.
[0057] Advantageously then, the composition according to the invention contains in a minor quantity one or more other different diene elastomers.
[0058] For example, the other diene elastomer may be chosen from the group of highly unsaturated diene elastomers consisting of polybutadienes (abbreviated "BR"), natural rubber (NR), synthetic polyisoprenes (IR), butadiene copolymers, isoprene copolymers (other than butyl rubber) and mixtures of these elastomers. Such copolymers can, for example, be chosen from the group consisting of butadiene-styrene copolymers (SBR), isoprene-butadiene copolymers (BIR), isoprene-styrene copolymers (SIR), isoprene-butadiene-styrene copolymers (SBIR), butadiene-acrylonitrile copolymers (NBR), butadiene-styrene-acrylonitrile copolymers (NSBR), or a mixture of two or more of these compounds.
[0059] According to one variant of the invention, the other diene elastomer can be a natural rubber.
[0060] The other diene elastomer can be modified, i.e., either coupled and / or star-shaped, or functionalized, or coupled and / or star-shaped and simultaneously functionalized. Thus, the other diene elastomer can be coupled and / or star-shaped, for example by means of a silicon or tin atom that links the elastomer chains together.
[0061] According to one embodiment of the invention, the composition comprises the other diene elastomer with a content of less than 50 pc, preferably within a range of 0 to 40 pc, preferably from 0 to 30 pc, more preferably from 0 to 20 pc.
[0062] The elastomeric matrix may also contain, in small quantities, any type of synthetic elastomer other than diene, or even polymers other than elastomers, for example, thermoplastic polymers. Preferably, the elastomeric matrix does not contain any synthetic elastomer other than diene or any polymer other than elastomers, or contains less than 10 parts per million, preferably less than 5 parts per million. 2. Charges and coupling agents
[0063] By load, we mean here any type of load, whether it is reinforcing or non-reinforcing.
[0064] The rubber composition of the invention is based on a filler comprising at least one reinforcing filler and one non-reinforcing filler. Preferably, the total filler content is greater than 10 parts per million, preferably greater than or equal to 20 parts per million, and less than or equal to 110 parts per million.
[0065] Any type of so-called reinforcing filler, known for its ability to reinforce a rubber composition, can be used, for example an organic filler such as carbon black, an inorganic filler such as silica or a mixture of these two types of fillers.
[0066] All carbon blacks are suitable as carbon blacks, including those conventionally used in tires. Among the latter, particularly the reinforcing carbon blacks of the 100, 200, and 300 series, or the blacks of the 500, 600, or 700 series (ASTM D-1765-2017 grades), such as NI 15, N134, N234, N326, N330, N339, N347, N375, N550, N683, N772, and N774. These carbon blacks can be used in isolation, as commercially available, or in any other form, for example, as a carrier for certain rubber additives used. Carbon blacks could for example already be incorporated into the diene elastomer, in particular isoprene in the form of a masterbatch (see for example applications WO97 / 36724-A2 or WO99 / 16600-A1).
[0067] The term "reinforcing inorganic filler" here refers to any inorganic or mineral filler, regardless of its color or origin (natural or synthetic), also called "white" filler, "light" filler, or even "non-black" filler (as opposed to carbon black), capable of reinforcing, on its own and without any other means than an intermediate coupling agent, a rubber composition intended for the manufacture of tires. As is known, certain reinforcing inorganic fillers can be characterized, in particular, by the presence of hydroxyl groups (-OH) on their surface.
[0068] Suitable inorganic reinforcing fillers include mineral fillers of the siliceous type, preferably silica (SiO2), or of the aluminous type, in particular alumina (Al2O3). The silica used may be any reinforcing silica known to those skilled in the art, in particular any precipitated or pyrogenated silica having a specific surface area BET and a specific surface area CT AB both less than 450 m2 / g, preferably in the range of 30 to 400 m2 / g, in particular 60 to 300 m2 / g.
[0069] Any type of precipitated silica can be used, in particular highly dispersible precipitated silicas (known as "HDS"). Examples include the silicas described in applications WO03 / 016215-A1 and WO03 / 016387-A1. Among commercial HDS silicas, the following can be used: "Ulsil® 5000GR", "Ulsil® 7000GR" from Evonik, and "Zeosil® 1085GR", "Zeosil® 1115 MP", "Zeosil® 1165MP", "Zeosil® Premium 200MP", and "Zeosil® HRS 1200 MP" from Solvay. As non-HDS silica, the following commercial silicas may be used: "Ultrasil ® VN2GR", "Ultrasil ® VN3GR" silicas from Evonik, silica, "Hi-Sil EZ120G(-D)", "Hi-Sil EZ160G(-D)", "Hi-Sil EZ200G(-D)", "Hi-Sil 243LD", "Hi-Sil 210", "Hi-Sil HDP 320G" silicas from PPG.
[0070] As a reinforcing inorganic filler, mineral fillers of the aluminous type, in particular alumina (Al2O3) or aluminum (oxide)hydroxides, or reinforcing titanium oxides, will also be mentioned.
[0071] Those skilled in the art will understand that, in place of the inorganic reinforcing filler described above, a reinforcing filler of another nature could be used, provided that this reinforcing filler of another nature is coated with an inorganic layer such as silica, or has functional sites on its surface, particularly hydroxyl sites, requiring the use of a coupling agent to establish the bond between this reinforcing filler and the diene elastomer. By way of example, carbon blacks partially or fully coated with silica, or carbon blacks modified with silica, such as, but not limited to, "Ecoblack®" fillers of the CRX2000 series or the "CRX4000" series, may be cited. of Cabot Corporation.
[0072] In the present exposition, the specific surface area BET is determined by gas adsorption using the Brunauer-Emmett-Teller method described in "The Journal of the American Chemical Society" (Vol. 60, page 309, February 1938), and more specifically according to a method adapted from the standard NF ISO 5794-1, Annex E of June 2010 [multipoint volumetric method (5 points) - gas: nitrogen - degassing under vacuum: one hour at 160°C - relative pressure range w / in: 0.05 to 0.2].
[0073] For inorganic fillers such as silica for example, the specific surface area values CT AB were determined according to standard NF ISO 5794-1, Annex G of June 2010. The process is based on the adsorption of CTAB (N-hexadecyl-N,N,N-trimethylammonium bromide) on the "external" surface of the reinforcing filler.
[0074] For carbon blacks, the STSA specific surface area is determined according to ASTM D6556-2016.
[0075] To couple the reinforcing inorganic filler to the diene elastomer, a coupling agent (or bonding agent) that is at least bifunctional can be used in a well-known manner to ensure sufficient chemical and / or physical connection between the inorganic filler (surface of its particles) and the diene elastomer. Organosilanes or polyorganosiloxanes that are at least bifunctional are used in particular. "Bifunctional" means a compound having a first functional group capable of interacting with the inorganic filler and a second functional group capable of interacting with the diene elastomer.For example, such a bifunctional compound may comprise a first functional group comprising a silicon atom, said first functional group being capable of interacting with the hydroxyl groups of an inorganic charge, and a second functional group comprising a sulfur atom, said second functional group being capable of interacting with the diene elastomer.
[0076] Preferably, the organosilanes are chosen from the group consisting of polysulfide organosilanes (symmetric or asymmetric) such as bis(3-triethoxysilylpropyl) tetrasulfide, abbreviated TESPT and marketed under the name "Si69" by Evonik, or bis-(3-triethoxysilylpropyl) disulfide, abbreviated TES PD and marketed under the name "Si75" by Evonik, polyorganosiloxanes, mercaptosilanes, and blocked mercaptosilanes, such as "NXT-Silane" marketed by Momentive. More preferably, the organosilane is a polysulfide organosilane.
[0077] Of course, mixtures of the coupling agents described above could also be used.
[0078] The coupling agent content in the composition of the invention is advantageous- The percentage of coupling agent is typically less than or equal to 20 parts per cubic meter, it being understood that it is generally desirable to use as little as possible. Typically, the percentage of coupling agent represents 0.5% to 15% by weight relative to the amount of reinforcing inorganic filler. This percentage is easily adjusted by a person skilled in the art according to the percentage of reinforcing inorganic filler used in the composition.
[0079] According to one embodiment of the invention, carbon black is used as a reinforcing filler in a proportion ranging from 10 to 60 parts per liter. Indeed, beyond this proportion, the reduction in the composition's rigidity is too significant for certain applications. Preferably, the carbon black proportion ranges from 20 to 50 parts per liter, and more preferably from 20 to 45 parts per liter.
[0080] Carbon black can advantageously constitute the sole reinforcing filler or the major reinforcing filler, that is to say, the reinforcing filler preferably comprises more than 50% by weight of carbon black relative to the total weight of the reinforcing filler. Of course, a single carbon black or a blend of several carbon blacks of different ASTM grades can be used.
[0081] Carbon black can also be used in cutting with other reinforcing fillers, and in particular reinforcing inorganic fillers such as those described above, and in particular silica. In this case, the total reinforcing filler content is preferably in the range of 10 parts per 10% to 60 parts per 10%.
[0082] According to one embodiment of the invention, carbon black constitutes the only reinforcing filler in the composition according to the invention.
[0083] The composition according to the invention also includes a non-reinforcing filler. Examples of non-reinforcing fillers include phyllosilicates such as kaolin, talc, mica, graphite, clays or modified clays ("organo clays"), bentonite, and chalk.
[0084] According to the invention, a non-reinforcing load ratio greater than or equal to 10 pc is preferably used, preferably varying from 10 to 80 pc, more preferably from 10 to 70 pc and even more preferably from 20 to 70 pc.
[0085] Kaolin can advantageously constitute the only non-reinforcing filler or the majority non-reinforcing filler, that is to say that the non-reinforcing filler preferably comprises more than 50% by weight of kaolin in relation to the total weight of the non-reinforcing filler.
[0086] According to one embodiment of the invention, the composition comprises kaolin in a proportion greater than or equal to 10 parts per cubic centimeter (ppm), preferably from 10 to 80 ppm, more preferably from 10 to 70 ppm, and even more preferably from 20 to 70 ppm. The composition according to the invention may then comprise a non-reinforcing filler other than kaolin in a proportion preferably from 0 to 50 ppm, preferably from 0 to 40 ppm. Most preferably, according to this embodiment of the invention, the composition does not includes no other non-reinforcing fillers and kaolin constitutes the only non-reinforcing filler in the composition.
[0087] According to a preferred embodiment of the invention, the rubber composition comprises carbon black in a proportion ranging from 10 to 60 parts per million, preferably from 20 to 50 parts per million, more preferably from 20 to 45 parts per million, and kaolin in a proportion ranging from 10 to 80 parts per million, preferably from 10 to 70 parts per million, and even more preferably from 20 to 70 parts per million. Preferably, the filler of the rubber composition consists of carbon black and kaolin, present in the composition in these same proportions, as the sole fillers. 3. Crosslinking system
[0088] The rubber composition according to the invention is based on a crosslinking system.
[0089] The crosslinking system of the rubber composition according to the invention comprises from 0.1 pc to 8 pc of a sulfur donor comprising N,N'-caprolactam disulfide.
[0090] According to variants of the invention, the total sulfur donor rate in the crosslinking system of the rubber composition according to the invention is in a range from 0.1 pc to 5 pc, preferably from 0.1 pc to 4 pc, more preferably from 0.2 pc to 3 pc, more preferably from 0.2 pc to 2 pc.
[0091] According to variants of the invention, N,N'-caprolactam disulfide is the major sulfur donor in the crosslinking system of the composition. Preferably, the total amount of N,N'-caprolactam disulfide (DTDC) is greater than or equal to 50% by weight, preferably greater than or equal to 70% by weight, for 100% by weight of the sulfur donor.
[0092] According to preferred embodiments of the invention, the sulfur donor of the crosslinking system of the rubber composition is essentially N,N'-caprolactam disulfide (DTDC). In other words, according to this embodiment, the sulfur donor of the crosslinking system of the rubber composition does not include any other sulfur donor than N,N'-caprolactam disulfide, or N,N'-caprolactam disulfide is the only sulfur donor of the crosslinking system.
[0093] The crosslinking system of the rubber composition may also include a sulfur donor other than N,N'-caprolactam disulfide, for example an alkylphenol disulfide (abbreviated "APDS", for example para-(tert-butyl)phenol disulfide), N,N'-dimorpholine disulfide or a combination thereof.
[0094] The sulfur donor of the crosslinking system of the rubber composition according to the invention may further comprise at least one elastomeric binder (e.g., EPDM / ethylene-vinyl acetate (EVA, EVM)) and dispersants, preferably the total quantity of the elastomeric binder and dispersants is greater than 0% by weight and less than 50% by weight, in particular less than or equal to 30% by weight for 100% by weight of the sulfur donor.
[0095] According to variants, the N,N'-caprolactam disulfide content in the rubber composition according to the invention is greater than or equal to 0.1 pc, more particularly greater than or equal to 0.2 pc, and less than or equal to 5 pc, preferably less than or equal to 4 pc, preferably still less than or equal to 3 pc, more particularly still less than or equal to 2 pc.
[0096] Thus, according to variants, the level of N,N'-caprolactam disulfide in the rubber composition according to the invention varies, for example, in a range from 0.1 to 5 pc, or even from 0.1 to 4 pc, preferably from 0.2 to 3 pc, more preferably from 0.2 to 2 pc.
[0097] According to preferred embodiments of the invention, the N,N'-caprolactam disulfide content in the rubber composition according to the invention varies, for example, from 0.2 to 1 part per annum. In this area, a significant and unexpected increase in roasting time is observed in some cases, without significantly impacting the curing time and while maintaining it at an industrially acceptable level.
[0098] Furthermore, the crosslinking system for the rubber composition according to the invention does not comprise soluble sulfur or insoluble sulfur, or comprises less than 0.6 parts per million, particularly less than 0.4 parts per million, of soluble sulfur, insoluble sulfur, or a mixture of soluble and insoluble sulfur. Preferably, when present, the total weight of soluble and / or insoluble sulfur is less than that of the sulfur donor.
[0099] According to a preferred embodiment, the crosslinking system of the rubber composition according to the invention does not include soluble sulfur or insoluble sulfur.
[0100] The crosslinking system for the rubber composition according to the invention may, in certain embodiments, comprise a crosslinking agent other than a vulcanizing agent. Such a crosslinking agent is, for example, a peroxide, a bismaleimide, or a mixture thereof.
[0101] The crosslinking system for the rubber composition according to the invention may, in certain embodiments, comprise a vulcanization accelerator, in particular and in a known manner, thiazole-type accelerators and their derivatives, sulfenamide-type accelerators, thiuram-type accelerators, dithiocarbamate-type accelerators, dithiophosphate-type accelerators, thiourea-type accelerators, and xanthate-type accelerators. Optionally, a known vulcanization activator such as zinc oxide, stearic acid, or equivalent compounds such as stearic acid salts and transition metal salts, guanidine derivatives (in particular diphenylguanidine), or known vulcanization retardants may also be used. 4. Miscellaneous additives:
[0102] Rubber compositions according to the invention may also comprise all or some of the usual additives and processing agents known to those skilled in the art and commonly used in rubber compositions, such as, for example, plasticizers like liquid plasticizers (e.g., oils), solid plasticizers (e.g., hydrocarbon resins) or mixtures thereof, tackifying resins, processing agents, pigments, and protective agents such as ozone-suppressing waxes, chemical ozone detoxifiers, and antioxidants. 5. Manufacture of rubber compositions:
[0103] The rubber compositions of the invention are manufactured in suitable mixers, using two successive preparation phases according to a general procedure well known to those skilled in the art: a first thermo-mechanical working or mixing phase (sometimes referred to as the "non-productive" phase) on a suitable mixer (for example, a "Banbury" type mixer) at high temperature, up to a maximum temperature between 110°C and 200°C, preferably between 135°C and 185°C, followed by a second mechanical working phase (sometimes referred to as the "productive" phase) at a lower temperature, typically below 120°C, for example between 40°C and 100°C, a finishing phase during which the crosslinking system comprising N,N'-caprolactam is incorporated.
[0104] The final composition thus obtained is then calendered, for example in the form of a sheet or plate, in particular for characterization in the laboratory, or extruded in the form of a semi-finished (or profile) rubber or a finished rubber product.
[0105] The crosslinking of the composition can be carried out in a manner known to those skilled in the art, for example at a temperature between 130°C and 200°C, under pressure.
[0106] The rubber product, comprising at least in part a rubber composition according to the invention described above, can be used in various applications. For example, a rubber composition according to the invention can be used for the manufacture of tires, shoe soles, rubber tracks (treads or pads), anti-vibration mounts, conveyor belts, timing belts, transmission belts, hoses, floor coverings, seals, and molded mechanical parts.
[0107] When the rubber composition according to the invention is used for manufacturing tires, it can advantageously form the inner rubber of a tire. The inner rubber ("innerliner") of the tire is, as is known, a layer of rubber designed to prevent airflow and maintain pressure. high air pressure of a tire. EXAMPLES OF THE INVENTION'S IMPLEMENTATION
[0108] The following examples illustrate the invention, but the latter cannot be limited to these examples alone.
[0109] To confirm the effect of the invention, rubber compositions (Al to A3, B1, and Cl: examples according to the invention, and TA, TB, and Tc: respective controls) were used. Each of the rubber compositions is based on an elastomeric matrix comprising butyl rubber, optionally combined with natural rubber (abbreviated "NR"), a filler comprising carbon black (as a reinforcing filler) and kaolin (a non-reinforcing filler), and N,N'-caprolactam disulfide or alkylphenol disulfide as a sulfur donor or sulfur in insoluble form. Each of the formulations of the rubber compositions is shown in Table 1 with the quantity of the different products expressed in parts per unit (pc). Compositions Al and B1 are identical. 1. Preparation of rubber compositions
[0110] The tests are carried out as follows: the charge composed of carbon black and kaolin, the plasticizer system (if applicable), butyl rubber and natural rubber, as well as various other ingredients (excluding the crosslinking system), are successively introduced into an internal mixer filled to 70% by volume and with an initial tank temperature of approximately 60°C. A thermomechanical process (non-productive phase) is then carried out in a single step, lasting approximately 3 to 4 minutes in total, until a maximum "drop" temperature of 150°C is reached.
[0111] The mixture thus obtained is recovered, cooled, and then the crosslinking system comprising sulfur, alkylphenol disulfide or N,N'-caprolactam disulfide is incorporated on an external mixer (homo-finisher) at 30°C, mixing everything (productive phase) for an appropriate time (for example between 5 and 12 min).
[0112] The compositions thus obtained are then calendered into plates (thickness of 2 to 3 mm).
[0113] 2. Measurement of the toasting time (fixation time) and the crosslinking time
[0114] The measurements are carried out before curing at 130°C, in accordance with French standard NF T 43-005. The evolution of the consistometric index over time makes it possible to determine - the toasting time of the rubber compositions, assessed in accordance with the aforementioned standard by the parameter t5 (case of a large rotor), expressed in minutes, and defined as the time required to obtain an increase in the consistometric index (expressed in UM) of 5 units at- above the minimum value measured for this index. - the applied crosslinking time, t90, which is the time required for the composition's torque to reach 90% of its maximum torque at the end of the recording of the torque evolution over time. The composition's torques are measured at 130°C with an oscillating chamber rheometer, according to DIN 53529 - part 3 (June 1983). 3. Compositions and results
[0115] [Tables 1] Composition Ta Al Iphr A2 0.5phr A3 2phr Tb B1 Iphr Tc Cl Iphr NR(1) 10.00 10.00 10.00 10.00 10.00 10.00 BIIR (2) 90.00 90.00 90.00 90.00 90.00 90.00 70.00 70.00 BIIR (3) 30.00 30.00 Kaolin (4) 30.00 30.00 30.00 30.00 30.00 30.00 20.00 20.00 Carbon black (5) 30.00 30.00 30.00 30.00 30.00 30.00 40.00 40.00 Implementing agent (6) 3.00 3.00 3.00 3.00 3.00 3.00 2.00 2.00 Resin (7) 2.50 2.50 Sulfur donor (8) 0.40 0.80 Sulfur donor (9) 1.00 0.50 2.00 1.00 1.00 MBTS (10) 1.00 1.00 1.00 1.00 1.00 1.00 1.00 1.00 1.00 Stearic acid (H) 0.75 0.75 0.75 0.75 0.75 0.75 0.75 0.75 ZnO (12) 1.00 1.00 1.00 1.00 1.00 1.00 0.70 0.70 Insoluble sulfur (13) 1.25
[0116] (1] Rubber iiatureh (2) Polyisobutylene bromine (“Bromobutyl 3220” of Exxon Chemical Co.); (3) Polyisobutylene-bromine ("BromobuM 4620" of Exxon Chemical Co.); (4) Kaolin “POLWHITE KL.” dTMERYS; (5) Carbon Black (ASTM grade N772 from QRION RAVENNA); (6) “Struktol® 40MS Fiakes” from STRUCKTOL; (7) Aliphatic tackifying resin ("ESCOREZ® 1102", softening point: 100°C, of ExxonMûbil); (8) Alkylphenol disulfide (APDS) “Vuitac TB7” from Arkema; (9) N,N'-caprolactam disulfide (DTDC): 80%, etastomeric binder and dispersants: 20% ('“Renogrand CLD 80” from Lanxess); (10} Vulcanization accelerator: 2-mercaptobenzothiazyl disulfide C'Nocceier DM-P (DM) [MBTS]” from Ouchi Shinko Chemical Industrial): (11) Stearic acid (“Pristerene 493 i” from Umqema); (12) Zinc oxide (industrial grade from Umicore company); (13) Insoluble sulfur.
[0117] [Tables2] Composition of DTDC rate ta (with APDS) Al Iphr A2 0.5phr A3 2phr Tb (with S) B1 Iphr Tc (with APDS) Cl Iphr Roasting time t5 (minutes) 10 24 25 24 15 24 13 30 Increase in roasting time (minutes) control 14 15 14 control 9 control 17 Crosslinking time t90 (minutes) 19 30 27 31 23 30 21 33 Increase in crosslinking time (minutes) control 11 8 12 control 7 control 12
[0118] The results in Table 2 demonstrate that the compositions according to the invention (Ai, Bi, and Ci) have a significantly longer roasting time (t5) than the roasting time (t5) of the control compositions (TA, TB, and Tc). More specifically, when comparing compositions TA (control with 0.4 part APDS) and A2 (according to the invention with 0.5 part DTDC), the roasting time is significantly and unexpectedly longer given the similar sulfur donor levels.
[0119] Furthermore, Table 2 shows that the examples (Ai, Bi, and Ci) according to the invention have a crosslinking time (t90) that remains acceptable from an industrial productivity standpoint, and whose increase compared to the respective controls (TA, TB, and Tc) remains less than the gain in roasting time. More specifically, comparing compositions TA (control with 0.4 parts APDS) and A2 (according to the invention with 0.5 parts DTDC), the roasting time is significantly lengthened without excessively impacting the crosslinking time, thus maintaining it as industrially viable.
[0120] In conclusion, the rubber composition according to the invention makes it possible to ensure an improved (longer) curing time while maintaining an industrially acceptable curing time or not degrading it beyond what is industrially acceptable.
Claims
Claims
1. Rubber composition based on at least: - an elastomer matrix comprising at least one butyl rubber; - a filler comprising at least one reinforcing filler and one non-reinforcing filler; and - a crosslinking system; wherein the crosslinking system comprises from 0.1 phr to 8 phr of a sulfur donor comprising N,N'-caprolactam disulfide; and wherein the crosslinking system comprises neither soluble sulfur nor insoluble sulfur, or comprises less than 0.6 phr of soluble sulfur, insoluble sulfur or a mixture of soluble sulfur and insoluble sulfur.
2. A rubber composition according to claim 1, wherein the elastomer matrix comprises at least 50 phr of butyl rubber.
3. A rubber composition according to any one of the preceding claims, wherein the reinforcing filler predominantly comprises a carbon black, preferably at a rate greater than 50% by weight per 100% by weight of the reinforcing filler.
4. A rubber composition according to any preceding claim, which comprises from 10 to 60, preferably from 20 to 45 phr of carbon black.
5. A rubber composition according to any one of the preceding claims, wherein the non-reinforcing filler predominantly comprises a kaolin, preferably at a rate greater than 50% by weight per 100% by weight of the non-reinforcing filler.
6. A rubber composition according to any preceding claim, which comprises 10 to 80 phr, preferably 10 to 70 phr, of kaolin as a non-reinforcing filler.
7. A rubber composition according to any preceding claim, wherein the total amount of N,N'-caprolactam disulfide is greater than 50% by weight per 100% by weight of the sulfur donor.
8. A rubber composition according to any preceding claim, wherein the sulfur donor contains N,N'-caprolactam disulfide as the sole sulfur donor.
9. A rubber composition according to any one of embodiments 1 to 7, wherein the sulfur donor comprises a sulfur donor other than N,N'-caprolactam disulfide.
10. A rubber composition according to any preceding claim, wherein the level of sulfur donor comprising N,N'-caprolactam disulfide ranges from 0.1 to 5, preferably from 0.2 to 3 phr.
11. A rubber composition according to any one of the preceding claims, wherein the N,N'-caprolactam disulfide content ranges from 0.1 to 4, preferably from 0.2 to 3 phr, more preferably from 0.2 to 2 phr.
12. A rubber composition according to any preceding claim, wherein the N,N'-caprolactam disulfide content ranges from 0.2 to 1 phr.
13. A rubber composition according to any preceding claim, wherein, when present, the total amount by weight of soluble sulfur, insoluble sulfur and the mixture of soluble sulfur and insoluble sulfur is less than that of the sulfur donor.
14. A rubber product comprising a rubber composition according to any one of claims 1 to 13.
15. A rubber product according to claim 14, which product is a tire whose inner rubber comprises the rubber composition according to any one of claims 1 to 13.
Citation Information
Patent Citations
Rubber composition
JP2004018682A
Novel elastomer composites, method and apparatus
WO1997036724A2
Elastomer composite blends and methods for producing them
WO1999016600A1
Method of preparing silicas, silicas with specific pore-size and / or particle-size distribution and the use thereof, in particular for reinforcing polymers
WO2003016215A1
Diene rubber composition for tyres comprising a specific silicon as a reinforcing filler
WO2003016387A1