Ultrahigh-strength high-performance maraging stainless steel for medium-thickness plates and preparation method thereof

The method addresses the trade-off in high-strength stainless steels by controlling nano-scale lath martensite and precipitate distribution in maraging stainless steel, enhancing both mechanical properties and corrosion resistance while reducing material costs.

GB2611411BActive Publication Date: 2024-10-30HARBIN ENG UNIV
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
GB2022011427
Authority / Receiving Office
GB · GB
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-04-07
Filing Date
2022-08-05
Publication Date
2024-10-30
Estimated Expiration
2042-08-05

AI Technical Summary

Technical Problem

Current high-strength stainless steels face a trade-off between strength, ductility, and corrosion resistance, making it difficult to achieve excellent comprehensive mechanical and corrosion properties simultaneously, with high Co content exacerbating spinodal decomposition and increasing material costs.

Method used

A method for preparing maraging stainless steel using vacuum induction melting-vacuum arc remelting (VIM-VAR) and thermomechanical treatments to control nano-scale lath martensite and precipitate distribution, reducing Co content and carbon levels to enhance strength, toughness, and corrosion resistance while maintaining low material costs.

Benefits of technology

The method results in a stainless steel with improved mechanical properties and corrosion resistance, achieving ultrahigh strength, good plasticity, and reduced material costs through controlled nano-phase precipitation and reverted austenite formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000001_0000
    Figure 00000001_0000
  • Figure 00000001_0001
    Figure 00000001_0001
  • Figure 00000002_0000
    Figure 00000002_0000
Patent Text Reader

Abstract

An ultrahigh-strength high-performance maraging stainless steel for medium-thickness plates wherein the stainless steel has a composition in as follows: 3.0-5.0 wt% of Co, 7.0-9.0 wt% of Ni, 11.0-15.0 wt% of Cr, 0.3-2.0 wt% of Ti, 4.0-6.0 wt% of Mo, 0.08-1.0 wt% of Mn, 0.08-0.3 wt% of Si, 0-0.02 wt% of C, 0- 0.003 wt% of P, 0- 0.003 wt% of S, and Fe as a balance. Preferably the stainless steel is prepared via the following method 1) Proportioning the alloying elements, 2) vacuum smelting for an electrode in a vacuum induction melting furnace, 3) vacuum arc remelting, 4) high-temperature homogenizing annealing, 5) hot rolling for cogging and 6) heat treating. Preferably step 6 comprises a high-temperature quenching treatment, cryogenic treatment and aging treatment. Preferably the high-temperature quenching treatment is conducted by maintaining a temperature of 1050-1200 °C for 60-120 min then cooling in air or oil to room temperature. Preferably the cryogenic treatment is conducted with liquid nitrogen for 4-10 h. Preferably the aging treatment is conducted at 450-600 °C for 0.5-500 h.
Need to check novelty before this filing date? Find Prior Art

Description

5 TECHNICAL FIELD

[0001] The present disclosure belongs to the technical field of maraging stainless steels, and relates to a method for preparing a maraging stainless steel for medium-thickness plates. 10  BACKGROUND ART

[0002] Precipitation-strengthened martensitic stainless steel, i.e. maraging stainless steel is a type of steel developed in the 1960s, which has both the strength of maraging steel and the corrosion resistance of stainless steel. Due to the excellent comprehensive mechanical properties thereof, the maraging stainless steel is commonly used in the fields of critical 15 and high-end equipment in aviation, aerospace and navigation.

[0003] The main reason for the maraging stainless steel to achieve ultrahigh strength is the superposition of martensitic transformation strengthening and precipitation strengthening, and its corrosion resistance is attributed to a passive film formed on the surface thereof via addition of Cr and Mo. Table 1 shows the compositions and performances of 20 commercially-available high-strength stainless steels at present. It may be seen that the current high-strength stainless steels have the following problems: on the one hand, there is a trade-off between strength and ductility; on the other hand, when the mechanical properties are excellent, the corrosion resistance is relatively poor. As a result, it is difficult to combine the strength, the plasticity, toughness and the corrosion resistance together to 25 obtain excellent comprehensive performances. Thus, it may be seen that it is indeed a researching hotspot and difficulty in the field of stainless steel to improve the strength and toughness of stainless steel on the premise of maintaining corrosion resistance, so as to meet higher requirements in engineering application on the comprehensive performance of the stainless steel. Accordingly, it is urgent to develop a novel ultrahigh-strength maraging stainless steel with independent intellectual property rights.

[0004] Table 1 Composition and performance of commercially-available high-strength 5 stainless steels 14 05 24

[0005] Material designation Cr Ni Mo Co Others RmZMPa Elongation / % Pitting potential / V sce Nb: 0.15-0.45 17-4PH 15.0-17.5 3.0-5.0 Cu: 3.0-5.0 1370 15 -0.060 Cu: 2.5-4.5 15-5PH 14.0-15.5 3.5-5.5 Nb: 0.15-0.45 1380 14 -0.027 PH13-8Mo 12.2-13.2 7.5-8.5 2.0-2.5 Al: 0.9-1.35 1620 10 0.054 PyrometX-23 9.5-10.5 6.5-7.5 5.0-6.0 9.5-11.0 1780 15 Custom475 10.5-11.5 7.5-8.5 4.5-5.5 8.0-9.0 Al: 1.0-1.5 1980 6 D70 11.5-12.5 4.0-5.0 4.0-5.0 12.0-14.0 1650 9.5 FerriumS53 10.0 5.5 2.5 14 W: 1.0, V: 0.3 1960 12

[0006] A higher content of Co makes the high-strength stainless steel a better mechanical property, while the comprehensive mechanical properties are relatively poor as the content of Co is lower. The addition of Co into the high-strength stainless steel is a double-edged 10 sword. Co may decrease the solubility of Ti and Mo in a martensite matrix to thus form a precipitated phase containing Mo or Ti, thereby increasing the strength. Meanwhile, Co may also hinder recovery of dislocations and stabilize the martensite matrix, thereby producing a relatively high secondary hardening to guarantee the desirable mechanical properties such as strength. Therefore, it is inevitable to add a large amount of Co element in order to obtain excellent mechanical properties. However, Co may promote the spinodal decomposition of Cr in the martensitic stainless steel. High content of Co leads to a great possibility of the spinodal decomposition of Cr, which may reduce the pitting corrosion resistance of the matrix. Therefore, Co should be introduced in an appropriate amount. In 5 the present disclosure, an innovation lies in that by means of inventive alloy compositions, vacuum induction melting-vacuum arc remelting (VIM-VAR) and thermomechanical treatments, nano-scale lath martensite with high dislocation density is obtained. Meanwhile the size, distribution and volume fraction of nano-scale precipitates in the martensite matrix and reverted austenite are controlled by promoting the kinetics of nano-scale 10 precipitation and the nucleation and growth of reverted austenite on the lath boundaries. The nano-phases and the dislocations act to control the strengthening and the reverted austenite for toughening, by which the mechanical properties are thus improved significantly. On the one hand, the carbon content is greatly reduced through replacing the carbon strengthening by the nano-phase precipitation strengthening. At the same time, a 15 pitting corrosion resistance of the alloy is guaranteed by the proper design of steel composition and microstructure. Both the extremely low carbon content, high pitting corrosion resistance equivalence and the proper distribution of Cr in the martensite matrix ensure excellent corrosion resistance of the stainless steel in the present disclosure. Therefore, compared with existing stainless steels, the stainless steel of the present 20 disclosure has an obvious improvement in both mechanical properties and corrosion resistance.

[0007] Chinese patent application CN 106906429 A discloses an ultrahigh-strength martensitic stainless steel and a preparation method thereof. The steel comprises the following constituents in percentage by weight (wt%): 0.10-0.25% of C, 11.0-17.0% of Cr, 25   0.5-2.0% of Mn, 1.1-3.0% of Si, 0.1-4.0% of Ni, 0.1-0.3% of Cu, 0.02% or less of P, 0.02% or less of S, and Fe and inevitable impurity elements as a balance. The stainless steel has yield strength of 1,300 MPa, a tensile strength of 1,600 MPa and elongation of 16%. Chinese patent application CN 103695796 A discloses a high-strength and high-toughness stainless steel and a preparation method thereof. The stainless steel 30 comprises the following chemical constituents in percentage by weight (wt%): 0.13-0.19% 10 CXI 15 20 25 30 of C, 0.6% or less of Si, 0.6-1.0% of Mn, 0.01% or less of P, 0.01% or less of S, 15.0-16.0% of Cr, 3.0-4.0% of Ni, 1.4-1.9% of Mo, 1.0-2.0% of Cu, 0.7-1.2% of W, 0.0-0.6% of V, 0.05-0.12% of N, and Fe and inevitable impurities as a balance. The stainless steel has yield strength of 690-1,388 MPa, tensile strength of 1,200-1,670 MPa and elongation greater than 10%. The two technical solutions above may achieve performances of a high-strength stainless steel. However, these technical solutions adopt relatively high carbon content, and this may seriously deteriorate the corrosion resistance. Besides, the size, morphology and distribution of carbides in a matrix are difficult to be controlled, and when the carbides have a relatively large size and exist on a grain boundary, the mechanical properties may be seriously deteriorated.

[0008] Chinese patent application CN 110358983 A discloses precipitation-hardened martensitic stainless steel and a preparation method thereof. The steel comprises the following constituents in percentage by weight (wt%): 0.14-0.20% of C, 13.0-16.0% of Cr, 0.5-2.0% of Ni, 12.0-15.0% of Co, 4.5-5.5% of Mo, 0.4-0.6% of V, 0.1% or less of Si, 0.5% or less of Mn, 0.01% or less of P, 0.01% or less of S, 0.10% or less of N, and Fe as a balance. The stainless steel has a tensile strength of 1,840-1,870 MPa, yield strength of 780-820 MPa and an elongation of 12.5-14.0%. The technical solution above may achieve the precipitation-hardening martensitic stainless steel. However, due to a relatively high Co addition amount, the cost of raw material is high; also, an increase in Co content causes spinodal decomposition of Cr, further resulting in both Cr-depleted and Cr-enriched regions to reduce the corrosion resistance. Moreover, the carbon content is relatively high, and this may seriously deteriorate the corrosion resistance. Besides, the size, morphology and distribution of carbides in a matrix are difficult to be controlled, and when the carbides have a relatively large size and exist on a grain boundary, the mechanical properties may be seriously deteriorated. Furthermore, the producing process requires two aging treatments and two cryogenic treatments, and thus is complicated.

[0009] Chinese patent application CN 101886228 A discloses a low-carbon maraging stainless steel with high strength, toughness and corrosion resistance. The stainless steel comprises the following chemical constituents in percentage by weight (wt.%): 0.08-0.15% of C, 11.0-12.0% of Cr, 4.0-5.0% ofNi, 0.2-1.0% of Ti, 0.5-1.0% of Mo, 2.0-3.0% of Cu, 14 05 24 2.0-3.0% of Co, 0.1-0.5% of Nb, 0.5-1.5% of Mn, 0.5-1.5% of Si, less than 0.01% ofN, less than 0.01% of V, less than 0.01% of Al, and Fe as a balance. The stainless steel has yield strength of 1,000-1,400 MPa, a tensile strength of 1,100-1,500 MPa and an elongation of 11.0-16%. The results of the mechanical properties in Example 2 of the 5 patent application are all shown brittle fracture. It may be seen that in the case of Example 2, the carbon content is relatively high, and the size, morphology and distribution of carbides in a matrix are thus difficult to be controlled; when the carbides have a relatively large size and exist on a grain boundary, the mechanical properties may be seriously deteriorated. Moreover, when the carbon content increases, the corrosion resistance of 10 materials may also be decreased sharply. Furthermore, the technical solution above adopts a relatively high Cu content, which has a great influence on thermal processing properties of materials, resulting in easy occurrence of thermal embrittlement and relatively complicated process control. 15 SUMMARY

[0010] Aiming at the problems of complicated preparation process, according to the present invention, there is provided a method for preparing a maraging stainless steel for medium-thickness plates as defined in more detail hereinbelow.

[0011] According to the present invention there is provided a method for preparing a 20 maraging stainless steel, the method consisting of the steps of: providing pure iron, metal chromium, metal nickel, metal manganese, metal molybdenum, metal cobalt, metal titanium and iron-silicon as raw materials according to a composition: in mass percentage, 4.0% of Co, 12.0% of Cr, 0.5% of Mn, 6.0% of Mo, 7.0% of Ni, 0.2% of Si, 1.0% of Ti, 0.02% or less of C, 0.003% or less of P, 0.003% or less 25 of S, and Fe as a balance; preparing a billet by vacuum melting throughout; homogenizing annealing, which is conducted as follows: heating the billet with a 14 05 24 furnace in air at a heating rate of 180 °C / h to 850 °C and maintaining for 5 h, further heating to 1,200 °C and maintaining for 30 h; and cooling with the furnace to room temperature; hot rolling for cogging, which is conducted under conditions: 5 heating the billet to 1,250 °C, maintaining for 10 h, and rolling, wherein the hot rolling begins at a temperature of 1,200 °C ± 20 °C and ends at a temperature of 950 °C or higher, such that a hot rolled sheet stock has a total rolling reduction of 70% and a molding thickness of 20 mm; and water cooling a sheet stock obtained to room temperature; 10 quenching treatment: subjecting the sheet stock after water cooling to quenching treatment by maintaining at 1,050 °C for 120 min, and then cooling in an ice-water mixture at 0 °C for quenching; cryogenic treatment: subjecting the sheet stock after the quenching treatment to cryogenic treatment with liquid nitrogen for 4 h and returning to room temperature; and 15 aging treatment: subjecting the sheet stock after the cryogenic treatment to aging treatment at 450 °C for 25 h, and then air cooling to room temperature.

[0012] The present disclosure has the following beneficial effects: 1) compared with other high- strength stainless steels, in the present disclosure, the content of precious metals is relatively low and the cost of raw materials is reduced; 2) the stainless steel of the present 20 disclosure contains extremely low carbon; 3) the method as provided in the present disclosure is simple and highly controllable since different high-strength stainless steels may be prepared just by varying the heat treatments, and thus is applicable for industrial production. Accordingly, a stainless steel with desirable corrosion resistance and excellent mechanical properties is obtained. BRIEF DESCRIPTION OF THE DRAWINGS 14 05 24

[0013] FIG. 1 shows a metallographic microscopy image after aging treatment in Example 1;

[0014] FIG. 2 shows an engineering stress-strain graph in Example 2, where the abscissa 5 refers to engineering strain and the ordinate refers to engineering stress;

[0015] FIG. 3 shows an X-ray diffraction (XRD) graph after high-temperature quenching and aging treatment in Example 2, where the abscissa refers to scanning angle and the ordinate refers to diffraction intensity; and

[0016] FIG. 4 shows an image of precipitated phases in reverted austenite in Example 2. 10 DETAILED DESCRIPTION OF THE EMBODIMENTS

[0017] The present disclosure provides a method for preparing a maraging stainless steel, and the maraging stainless steel prepared thereby. The maraging stainless steel prepared for medium-thickness plates is detailed hereinbelow. 15

[0018] The ultrahigh-strength high-performance maraging stainless steel for medium-thickness plates according to the present disclosure has a composition as follows in mass percentage: 3.0- 5.0% of Co, 7.0-9.0% of Ni, 11.0-15.0% of Cr, 0.3-2.0% of Ti, 4.0-6.0% of Mo, 0.08-1.0% of Mn, 0.08-0.3% of Si, 0.02% or less of C, 0.003% or less of P, 0.003% or less of S, and Fe as a balance. 20

[0019] The the composition design basis of the ultrahigh-strength high- performance maraging stainless steel for medium-thickness plates is as follows.

[0020] According to the present disclosure, the carbon strengthening on the stainless steel is not used, and the carbon content is controlled at an extremely low level instead, thereby improving both the toughness and the corrosion resistance of the stainless steel. However, 25 the ultralow carbon content causes a serious problem of low strength. In the present 10 CXI 15 20 25 30 disclosure, by means of optimization of alloying elements, VIM-VAR and corresponding thermomechanical treatments, nano-phases with excellent precipitation-strengthening contributions are developed and controlled, and the reverted austenite is introduced and controlled into the matrix. A stainless steel with excellent properties is successfully developed by controlling the distribution, size and volume fraction of the nano-scale precipitated phases in the matrix and the reverted austenite. Ice-water quenching makes the martensitic laths a tiny size and an increased dislocation density, and these fine martensitic laths provide nucleation sites for the precipitated nano-scale phases and the film-like sub-stable reverted austenite decorating the lath boundaries. Meanwhile, the relatively high dislocation density allows an increase in the element distribution channels for reverted austenite, and the reverted austenite generated in this way is more prone to the TRIP (Transformation Induced Plasticity) effect when under load, significantly increasing the plasticity and toughness.

[0021] According to the present disclosure, the precipitated phases of a Mo-enriched R' phase, an a'-Cr nano-phase and a Ni3(Ti, Mo) nano-phase are formed by adjusting the contents of Ni, Ti, Mo and Si, which achieve improvement in strength through synergistic strengthening. The three strengthening nano-phases substantially show co-precipitation. In an early stage of aging, small Ni-Ti-Mo-Si clusters in dispersed distribution are formed inside the martensitic laths or on the dislocations. With the extension of aging time, Mo and Si are gradually expelled from the clusters, and a nano-scale Ni3(Ti, Mo) strengthening phase is formed. After a heat preservation, Mo and Si are completely expelled out and form on a surface of NisTi a Mo-enriched R' phase, which wraps NisTi in turn to suppress its growth, thus ensuring the nano phases to be fine and dispersed. Meanwhile, a nano-scale a'-Cr phase is also formed inside the martensitic laths. The newly formed Mo-enriched R' phase, NisTi and a'-Cr provide together a high strength for the matrix.

[0022] In addition, with the coherent strain energy at the matrix interfaces, NisTi with a DO24 structure in dispersed distribution is driven to form film-like reverted austenite in dispersed distribution through the climbing of edge dislocations, together with the diffusion of Fe atoms. The relatively high dislocation density and the fine martensitic laths greatly reduce the energy required for nucleation of the reverted austenite, and the relatively high dislocation density may provide diffusion channels for the growth of the reverted austenite. Thus, the reverted austenite generated in this way has a film-like morphology, which is dispersedly distributed in matrix and is prone to the TRIP effect, thereby effectively relieving stress concentration. The reverted austenite in film-like distribution contains Mo-rich nano phases, and thus may greatly improve the work hardening capacity of materials during plastic deformation and reduce effectively the yielding-to-tensile ratio of ultrahigh-strength steels. 10 CXI 15 20 25 30

[0023] In the present disclosure, an important innovation is to significantly reduce the content of expensive alloying element Co, thereby reducing costs while improving corrosion resistance. In the present disclosure, the content of Co is designed at a quite low level, reducing the formation of Ni-Ti clusters. However, via optimization of alloying elements, VIM-VAR and corresponding thermomechanical treatments, control of the precipitation-strengthening nano-phases is achieved, and reverted austenite is introduced into the matrix. The comprehensive properties, including ultra-high strength, good plasticity and toughness are thus successfully obtained by controlling the distribution, size and volume fraction of the nano-scale precipitated phases and the reverted austenite in the matrix. In the present disclosure, based on the innovations in the strengthening mechanism and the corresponding composition and thermomechanical treatment design, a simple and controllable process is realized, cost is reduced, and the mechanical properties and corrosion resistance are effectively improved.

[0024] Composition design basis: Co is one of the important elements to be considered. Co may elevate the Ms point to ensure that the matrix is martensite. Nevertheless, Co is a double-edged sword for a maraging stainless steel. Co may decrease the solubility of Ti and Mo in a martensite matrix to thus form precipitations containing Mo or Ti, thereby increasing the strength. Meanwhile, Co may also hinder recovery of dislocations and stabilize the matrix, thereby producing a relatively high secondary hardening. However, Co may promote the spinodal decomposition of Cr in martensitic stainless steel, and a higher content of Co leads to a great probability of spinodal decomposition of Cr, which may reduce the pitting corrosion resistance of the steel. In view of the corrosion resistance, Co should be introduced in an appropriate amount. Moreover, the element Co is relatively 14 05 24 expensive, and thus a higher content of Co means a higher cost of the raw materials for ultrahigh-strength stainless steel. Based on a comprehensive consideration, the mass percentage of Co is controlled within a range of 3.0-5.0%, for example 3.0%, 3.5%, 4.0%, 4.5% and 5.0%. 5

[0025] Ni is an important element for forming the intermetallic compounds. In an early stage, B2-Ni(Ti, Mn) and r|-Ni3(Ti, Mo) are formed to strengthen the matrix, and p-Nis(Ti, Mo) is also the core for nucleation of a Mo-enriched R' phase. In addition, Ni may strengthen the matrix to provide certain plasticity and toughness for the stainless steel of the present disclosure. Ni may also improve the hardenability of martensite. Moreover, Ni 10 is a main element for the formation of reverted austenite. However, an excessive content of Ni promotes the generation of retained austenite in the matrix, thus affecting the strength of stainless steel. Based on a comprehensive consideration, the mass percentage of Ni is controlled within a range of 7.0-9.0%, for example 7.0%, 7.5%, 8.0%, 8.5% and 9.0%.

[0026] Mo is a very important element for precipitation strengthening. Mo is one of the 15 main elements to form a Mo-enriched R' phase and Nis(Ti, Mo). The Mo-enriched R' phase is formed via long time of aging and wraps NisTi to form fine core-shell structures in dispersed distribution to effectively improve the strength. Mo is also an effective element for corrosion resistance, and may significantly improve the corrosion resistance of materials. Meanwhile, Mo is an element for forming ferrite. An excessive content of Mo 20 may increase the precipitation tendency of high temperature 5 ferrite, increasing the content of 5 ferrite and deteriorating the performances of materials. Based on a comprehensive consideration, the mass percentage of Mo is controlled within a range of 4.0-6.0%, for example 4.0%, 4.5%, 5.0%, 5.5% and 6.0%.

[0027] Cr is a very important element in stainless steel. Cr generally has a mass 25 percentage of greater than 10% to ensure the corrosion resistance of stainless steel. However, Cr is an element for forming ferrite, and an excessive content of Cr may increase the content of 5 ferrite in matrix, thereby reducing the strength and toughness and the corrosion resistance of materials. Therefore, based on a comprehensive consideration, the mass percentage of Cr is controlled within a range of 11.0-15.0%, for example 11.0%, 11.5%, 12.0%, 12.5%, 13.0%, 13.5%, 14.0%, 14.5% and 15.0%. 14 05 24

[0028] Si is an important element for novel stainless steels. Si is one of the main elements for forming a Mo-enriched R' phase, and may effectively promote the formation of the Mo-enriched R' phase. Si may also effectively inhibit the precipitation and growth of 5 carbides in a martensite matrix during tempering, thereby preventing the appearance of Cr-depleted regions that reduce corrosion resistance. However, an excessive content of Si may seriously deteriorate the plasticity of materials. Based on a comprehensive consideration, the mass percentage of Si is controlled within a range of 0.08-0.30%, for example 0.08%, 0.1%, 0.15%, 0.20%, 0.25% and 0.30%. 10

[0029] Ti is a main element for forming strengthening phases, and may form Ni-Ti clusters at an initial stage preparing for the subsequent precipitation of the strengthening phase. An excessive content of Ti may increase the precipitation tendency of the precipitated phases at the boundary of the martensitic laths. An excessive amount of precipitated phases at boundary of martensitic laths are highly prone to evolve into a 15 source of crack, which extends along the boundary of the martensitic laths to cause quasi-cleavage cracking. Based on a comprehensive consideration, the mass percentage of Ti is controlled within a range of 0.3-2.0%, for example 0.3%, 0.5%, 0.8%, 1.0%, 1.5% and 2.0%.

[0030] Mn is substantially involved in the precipitation of nano-phases to form Ni(Mn, Ti, 20 Mo) intermetallic compounds. Therefore, Mn may be used to replace Ti and Mo elements in a small amount to reduce costs. Mn is also a main element for affecting reverted austenite. However, an excessive content of Mn causes serious segregation, increased thermal stress and structural stress and reduced weldability of billets. Based on a comprehensive consideration, the mass percentage of Mn is controlled within a range of 25   0.08-1.0%, for example 0.08%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9% and 1.0%.

[0031] C exists as an impurity element in matrix in the stainless steel of the present disclosure. When the content of C is excessively high, carbides of MX or M23C6 (M=Cr, Ti) may be formed. These carbides seriously retard the formation of reverted austenite and 14 05 24 offset the benefits of high dislocation density brought by cold rolling; moreover, the carbides with an excessive size may seriously deteriorate the toughness and corrosion resistance of the steel. Therefore, the content of C is strictly controlled to be 0.02% or less. P and S are also impurity elements, and an increase in their contents may seriously 5 deteriorate the performances of stainless steel likewise. Therefore, the contents of P and S are strictly controlled.

[0032] The ultrahigh-strength high-performance maraging stainless steel for medium-thickness plates and preparation method thereof according to the present disclosure will be further explained and illustrated below with reference to the drawings and examples, 10 which should not be regarded as an improper limitation to the technical solutions of the present disclosure.

[0033] Example 1

[0034] Pure iron, metal chromium, metal nickel, metal manganese, metal molybdenum, metal cobalt, metal titanium and iron-silicon were taken as raw materials according to a 15 composition of stainless steel in mass percentage as follows: 3.0% of Co, 11.0% of Cr, 0.08% of Mn, 6.0% of Mo, 9.0% of Ni, 0.08% of Si, 0.8 of Ti, 0.02% or less of C, 0.003% or less of P, 0.003% or less of S, and Fe as a balance.

[0035] A billet was prepared by vacuum melting throughout.

[0036] The high-temperature homogenizing annealing was conducted as follows: the billet 20 was heated with a furnace in air at a heating rate of 100°C / h to 600°C and maintained for 4 h, then was heated to l,100°C and maintained for 20 h, and then was cooled with the furnace to room temperature.

[0037] The hot rolling for cogging was conducted under the following conditions: the billet was heated to l,200°C and maintained for 10 h, and then was rolled; the hot rolling 25 began at a temperature of l,200°C ± 20°C and ended at a temperature of 950°C or higher; the hot rolling sheet stock had a total rolling reduction of 60% and a molding thickness of 30 mm, and was water cooled to room temperature. 14 05 24

[0038] The sheet stock above was subjected to a high-temperature quenching treatment by being maintained at l,200°C for 60 min and then cooled in an ice-water mixture at 0°C for quenching; subsequently, the sheet metal was subjected to a cryogenic treatment with liquid nitrogen for 8 h and returned to room temperature; thereafter, the sheet stock was 5 subjected to an aging treatment at 480°C for 20 h, and then air cooled to room temperature.

[0039] The mechanical properties of Example 1 are shown in Table 1. The stainless steel sample has an average hardness of 512.3 HV, yield strength of 1,820 MPa, a tensile strength of 2,006 MPa, an elongation of 14.9% and a pitting potential of 0.22 Vsce. FIG. 1 shows a metallographic microscopy image after aging treatment of Example 1, where a 10 representative martensitic layered structure may be observed.

[0040] Example 2

[0041] Pure iron, metal chromium, metal nickel, metal manganese, metal molybdenum, metal cobalt, metal titanium and iron-silicon were taken as raw materials according to a composition of stainless steel in mass percentage as follows: 4.0% of Co, 12.0% of Cr, 15   0.5% of Mn, 6.0% of Mo, 7.0% ofNi, 0.2% of Si, 1.0% of Ti, 0.02% or less of C, 0.003% or less of P, 0.003% or less of S, and Fe as a balance.

[0042] A billet was prepared by vacuum melting throughout.

[0043] The high-temperature homogenizing annealing was conducted as follows: the billet was heated with a furnace in air at a heating rate of 180°C / h to 850°C and maintained for 5 20 h, then was heated to l,200°C and maintained for 30 h; and then was cooled with the furnace to room temperature.

[0044] The hot rolling for cogging was conducted under the following conditions: the billet was heated to l,250°C and maintained for 10 h, and then was rolled; the hot rolling began at a temperature of l,200°C ± 20°C and ended at a temperature of 950°C or higher; 25 the hot rolled sheet stock had a total rolling reduction of 70% and a molding thickness of 20 mm, and was water cooled to room temperature.

[0045] The sheet stock above was subjected to a high-temperature quenching treatment by 14 05 24 being maintained at l,050°C for 120 min and then cooled in an ice-water mixture at 0°C for quenching; subsequently, the sheet stock was subjected to a cryogenic treatment with liquid nitrogen for 4 h and returned to room temperature; thereafter, the sheet stock was subjected to an aging treatment at 450°C for 25 h, and then air cooled to room temperature. 5

[0046] The mechanical properties of Example 2 are shown in Table 1. The stainless steel sample has an average hardness of 518.1 HV, yield strength of 1,860 MPa, a tensile strength of 2,130 MPa, an elongation of 15.7% and a pitting potential of 0.20 Vsce. FIG. 2 shows an engineering stress-strain graph of Example 2. FIG. 3 shows an XRD graph after high-temperature quenching and aging treatment of Example 2, where the reverted 10 austenite is precipitated after aging. FIG. 4 shows an image of precipitated phases in the reverted austenite in Example 2.

[0047] In the examples above, the testing methods for corrosion resistance, hardness and tensile mechanical properties of the ultrahigh-strength high-performance maraging stainless steel for medium-thickness plates are as follows. 15

[0048] 1) Hardness: a hardness test was conducted on an HVS-50 Vickers hardness tester with a load of 1 Kg; an average value was taken after 5 dotting, and the results were listed in Table 1.

[0049] 2) Tensile mechanical properties: a tensile test was conducted on an electronic universal testing machine; the samples were prepared as rectangular samples with a 20 nominal size of (2-3) mmx4 mm><20.6 mm; for each of the tensile strength, yield strength and elongation, an average value was taken from three samples treated identically, and the results were listed in Table 1.

[0050] 3) Corrosion resistance

[0051] A sample was processed into a specification of 10 mm* 10 mmx2 mm, and was 25 exposed to 1 cm2 for experiment after being encapsulated with epoxy resin. The surface of the sample was polished to 2000# with sandpaper, scrubbed with ethyl alcohol to remove oil stains, washed with deionized water and air dried for later use. An experiment was 14 05 24 conducted with a solution of 0.1M Na2SO4+xNaCl (pH=3) at temperature of 25°C. The electrochemical experiment was conducted using a CHI660E electrochemical workstation. The electrochemical experiment was conducted with a common three-electrode system, where the ultrahigh-strength stainless steel sample was used as a working electrode, a Pt 5 sheet was used as an auxiliary electrode and a saturated calomel electrode (SCE) was used as a reference electrode. Before the electrochemical experiment, the sample was applied with a potential of -1.2 Vsec and subjected to potentiostatic polarization for 5 min to remove the oxide membrane formed on a surface of the sample in the air. The system was stabilized for 30 min and recording was started. Potentiodynamic polarization was 10 conducted at a scanning rate of 0.5 mV / S within a scanning potential region of -0.3 V (vs. open circuit potential Eoc) to 1.5 V (vs. reference electrode potential Er), and the experiment was stopped after current changed stably. An average value was taken from three measurements and the results were listed in Table 1.

[0052] Table 1 Composition, hardness, tensile properties and pitting potential of 15 examples Chemical composition / % Average hardness / HV Yield strength / MPa Tensile strength / MPa Elongation / % Pitting potential / VsCE Co Ni Cr Ti Mo Mn Si Fe Example 1 3.0 9.0 11.0 0.8 6.0 0.08 0.08 Bal. 512.3 1820 2006 14.9 0.22 Example 2 4.0 7 12.0 1.0 6.0 0.5 0.2 Bal. 518.1 1860 2130 15.7 0.20

[0053] Note: The contents of components such as C, P and S in examples in Table 1 conform to the elemental composition of the stainless steel according to the present disclosure. The content of C is 0.02% or less, the content of P is 0.003% or less and the content of S is 0.003% or less, all of which are not listed in Table 1. The abbreviation Bal. 20 represents balance.

Claims

14 05 241. A method for preparing a maraging stainless steel consisting of the steps of:providing pure iron, metal chromium, metal nickel, metal manganese, metal molybdenum, metal cobalt, metal titanium and iron-silicon as raw materials according to a 5 composition: in mass percentage, 4.0% of Co, 12.0% of Cr, 0.5% of Mn, 6.0% of Mo, 7.0% of Ni, 0.2% of Si, 1.0% of Ti, 0.02% or less of C, 0.003% or less of P, 0.003% or less of S, and Fe as a balance;preparing a billet by vacuum melting throughout;homogenizing annealing, which is conducted as follows: heating the billet with a 10 furnace in air at a heating rate of 180 °C / h to 850 °C and maintaining for 5 h, further heating to 1,200 °C and maintaining for 30 h; and cooling with the furnace to room temperature;hot rolling for cogging, which is conducted under conditions:heating the billet to 1,250 °C, maintaining for 10 h, and rolling, wherein the hot 15 rolling begins at a temperature of 1,200 °C ± 20 °C and ends at a temperature of 950 °C or higher, such that a hot rolled sheet stock has a total rolling reduction of 70% and a molding thickness of 20 mm; andwater cooling a sheet stock obtained to room temperature;quenching treatment: subjecting the sheet stock after water cooling to quenching 20 treatment by maintaining at 1,050 °C for 120 min, and then cooling in an ice-water mixture at 0 °C for quenching;cryogenic treatment: subjecting the sheet stock after the quenching treatment to cryogenic treatment with liquid nitrogen for 4 h and returning to room temperature; andaging treatment: subjecting the sheet stock after the cryogenic treatment to aging 25 treatment at 450 °C for 25 h, and then air cooling to room temperature.

Citation Information

Patent Citations

  • Stainless steel with low cost, high strength and high corrosion resistance and preparation method thereof

    CN113046642A

  • Ultrahigh-strength and high-performance maraging stainless steel and warm rolling preparation method thereof

    CN113667905A

  • 2400MPa-grade maraging stainless steel with high plasticity, toughness and corrosion resistance and preparation method thereof

    CN113774280A

  • 2000MPa-grade maraging stainless steel with high plasticity, toughness and corrosion resistance and preparation method thereof

    CN113774281A

  • Ultrahigh-strength high-performance medium-thickness plate martensitic stainless steel and preparation method thereof