Method for preparing an anode active material, the material, and a sodium-ion electrochemical cell thereof
Patent Information
- Application Number
- IN202641046299
- Authority / Receiving Office
- IN · IN
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2026-04-10
- Publication Date
- 2026-10-26
- Estimated Expiration
- 2046-04-10
AI Technical Summary
Current anode materials for sodium-ion batteries suffer from low capacity, poor rate capability, structural degradation, and high irreversible capacity loss, limiting their performance and scalability, especially at high current densities.
A method involving a molten salt synthesis of potassium dithioferrate (KFeS₂) with in-situ incorporation of multi-walled carbon nanotubes (MWCNTs) to form a composite anode material, enhancing electronic conductivity and structural stability without additional processing steps.
The KFeS₂-MWCNT composite anode achieves high capacity, high-rate capability, and long cyclic stability, supporting fast-charging applications with improved coulombic efficiency and scalability.
Abstract
Description
TECHNICAL FIELD
[001] The present invention relates generally to the field of electrochemicalenergy storage systems, and more particularly to a method for preparing highcapacity and high rate anode active material for sodium-ion batteries.BACKGROUND
[002] Background description includes information that may be useful inunderstanding the present subject matter. It is not an admission that any of theinformation provided herein is prior art or relevant to the presently claimedinvention, or that any publication specifically or implicitly referenced is prior art.
[003] The skyrocketing demand for electrochemical energy storage devices andrapid progress in a "low carbon economy" urge the identification of potentialalternatives to state-of-the-art Lithium-ion batteries (LIBs). Sodium-ion batteries(SIBs) have emerged as a potential alternative to Lithium-ion batteries owing to theabundance of sodium in the earth's crust (2.36 wt%), low cost of raw materials, anduniform geographical distribution. The similar chemical properties of lithium andsodium make it comparatively easy to switch over from lithium-based technologyto sodium-based technology. SIBs are particularly attractive for large grid-scaleenergy storage applications and exhibit the ability to operate over a wider range oftemperature. In SIB systems, the cathode acts as a sodium (Na) host, and the anodeacts as a sodium (Na) sink.
[004] Extensive and unremitting research on cathode materials has achievedsignificant progress, including developments in Prussian blue analogues, layeredoxides, and polyanionic cathodes. In contrast, currently available anodes for SIBsare predominantly carbon-based materials, which suffer from several limitationssuch as low capacity and poor rate capability, thereby restricting the overallperformance of SIBs. Accordingly, the development of high-performance anodesis necessary to improve SIB performance to levels comparable with LIBs.
[005] Graphite, a successful and widely commercialized anode material for LIBs,has remained unsuitable for SIBs due to the thermodynamic instability of binarygraphite intercalation compounds (b-GICs). Recent developments involving the useof ether-based electrolytes and solvent co-intercalation phenomena have enabledthe use of graphite in SIBs; however, the achievable capacity is limited toapproximately 120 mAh g⁻¹. Commercial hard carbon anodes deliver highercapacities of approximately 300 mAh g⁻¹ but require high-temperature synthesisand suffer from sluggish Na⁺ storage kinetics, limited sodium storage sites, sodiumplating at higher current densities, and very high first-cycle irreversible capacityloss. These drawbacks restrict their application as fast-charging anodes in SIBs.Consequently, the search for high-capacity and high-rate anodes has shifted towardconversion-based anode materials.
[006] Among conversion-based anodes, transition metal sulfides (TMSs) haveemerged as an attractive candidate due to their high theoretical capacity, higherelectrical conductivity, and longer metal-sulphur (M-S) bond length compared totransition metal oxides (TMOs). However, the practical application of TMS anodesin SIBs remains challenging due to structural degradation arising from large volumeexpansion during sodium ion intercalation and de-intercalation, leading to severecapacity fading upon cycling. This represents a major bottleneck restrictingperformance, particularly at high current densities.
[007] Fast-charging capability is a critical factor for the commercialization of SIBtechnology, as it reduces charging time while improving user convenience andenergy efficiency. The adoption of fast-charging SIB systems has potentialapplications in electric vehicles, power electronic devices, and uninterrupted powersupply (UPS) systems. However, achieving a high-rate metal sulfide anode withhigh initial coulombic efficiency (ICE), high capacity, and long cyclic life remainsa significant challenge.
[008] To mitigate these issues, systematic material design has been identified as apotent strategy. From a general perspective, fast-charging anode performance relieson effective structural design enabling rapid sodium-ion diffusion and electronicconductivity, while maintaining structural stability during cycling. Additionally,simple and scalable synthesis protocols are essential for commercialization beyondlaboratory-scale research.
[009] Although high-capacity TMS anodes demonstrate potential for fastcharging applications, their development is constrained by factors such as high cost,multistep synthesis processes, drastic volume fluctuations, and limited ionic andelectronic conductivity.
[010] Recent literature reports have demonstrated the potential of ternarychalcogenide-based anodes. For example, Wei Ai et al. (Advanced EnergyMaterials, 14 (2024) 2401221) disclosed a two-dimensional metallic ternarychalcogenide, KCu₄S₃, exhibiting an electrical conductivity of 4 x 10³ S cm⁻¹ anddelivering a capacity of 355 mAh g⁻¹ at 20 A g⁻¹ (124 s) with 100% capacityretention after 3000 cycles. Similarly, Shaobo Cheng et al. (Advanced FunctionalMaterials, (2025) 2510286) reported a tunnel-structured KCu₇S₄ anode, whichexhibited first-cycle discharge and charge capacities of 560 and 450 mAh g⁻¹,respectively, at 0.02 A g⁻¹, with an irreversible capacity loss of 19.6%, and acapacity of 337 mAh g⁻¹ at 10 A g⁻¹.
[011] While these studies highlight the potential of ternary chalcogenide-basedanodes, challenges such as irreversible capacity loss, structural instability, andlimited scalability persist.
[012] Hence, there remains a need for an anode material for sodium-ion batteriesthat delivers high capacity, high-rate capability, improved initial coulombicefficiency, and long cyclic stability through a simple and scalable synthesis route.OBJECTS OF THE INVENTION
[013] The objectives are provided to introduce a selection of concepts in asimplified form that are further described below in the detailed description. Theseobjectives are not intended to identify key features or essential features of theclaimed subject matter, nor is it intended to be used as an aid in determining thescope of the claimed subject matter.
[014] It is a principal object of the present invention to provide a high-capacityand high-rate anode material for sodium-ion batteries, thereby improvingelectrochemical performance and enabling fast-charging capability.
[015] It is another object of the present invention to provide a simple, sustainable,cost-effective, and scalable synthesis route for the development of anode activematerial for sodium-ion batteries.
[016] It is another object of the present invention to provide a single-step moltensalt synthesis route for preparing a ternary chalcogenide anode material comprisingKFeS₂, exhibiting inherent high Na⁺ conductivity and improved electrochemicalperformance.
[017] It is another object of the present invention to provide an in-situ compositingapproach wherein multi-walled carbon nanotubes (MWCNTs) are incorporatedwith the anode material during the molten salt synthesis process, thereby improvingelectronic conductivity without requiring additional processing steps.
[018] It is another object of the present invention to provide a method forfabricating an anode electrode based on the said anode active material for sodiumion batteries.
[019] It is another object of the present invention to provide a method forfabricating a sodium half-cell utilizing the anode electrode as a working electrode.
[020] It is another object of the present invention to provide a sodium half-cellbased on an anode electrode as the working electrode, fabricated using the saidanode active material.
[021] These and other objects and advantages of the present subject matter will beapparent to a person skilled in art after consideration of the following detaileddescription taking into consideration with accompanied drawings in whichpreferred embodiments of the present subject matter are illustrated.SUMMARY
[022] Solution to one or more drawbacks of existing technology and additionaladvantages are provided through the present disclosure. Additional features andadvantages are realized through the technicalities of the present disclosure. Otherembodiments and aspects of the disclosure are described in detail herein and areconsidered to be a part of the claimed disclosure.
[023] According to an embodiment, the present invention discloses a method ofpreparing an anode active material for a sodium-ion battery. The method includesmixing a ferric nitrate nonahydrate precursor with potassium thiocyanate (KSCN)to form a precursor mixture and heating the precursor mixture to form potassiumdithioferrate (KFeS₂) by a molten salt route to obtain a product containing KFeS2and unreacted precursors, wherein the potassium thiocyanate (KSCN) forms amolten salt reaction medium. The method also includes separating the potassiumdithioferrate as the anode active material from the former product by washing withdeionized (DI) water and drying.
[024] In an embodiment, heating the precursor mixture is performed under an inertatmosphere and the precursor mixture is heated at a temperature in a range fromabout 550°C to about 700°C for a dwell time in a range from about 2 hours to about4 hours. In an embodiment, potassium thiocyanate acts as both a potassium sourceand a sulphur source for formation of KFeS₂, and wherein the process is performedin absence of elemental sulphur. In an embodiment, the method also includescombining multi-walled carbon nanotubes (MWCNTs) with the precursor mixtureprior to said heating, thereby forming a KFeS₂-MWCNT composite. In anembodiment, the MWCNTs are added in an amount of about 2 wt.% to about 5wt.% during the synthesis. In an embodiment, washing the product with deionized(DI) water removes residual salts of the molten salt route.
[025] According to another embodiment, the present invention further disclosesan anode active material for a sodium-ion battery. The anode active materialincludes potassium dithioferrate (KFeS₂) having one-dimensional rod-shapedparticles; and conductive carbon including multi-walled carbon nanotubes(MWCNTs), wherein the MWCNTs are added in an amount of about 2 wt.% toabout 5 wt.% during the synthesis.
[026] According to another embodiment, the present invention further disclosessodium-ion electrochemical cell. The sodium-ion electrochemical cell includes anon-aqueous electrolyte containing a 1M NaPF6 in diethylene glycol dimethyl ether(DEGDME) and an anode, wherein the anode includes composite of potassiumdithioferrate (KFeS₂) having one-dimensional rod-shaped particles and conductivecarbon. The conductive carbon includes multi-walled carbon nanotubes(MWCNTs), wherein the MWCNTs are added in an amount of about 2 wt.% toabout 5 wt.% during the synthesis. The sodium-ion electrochemical cell alsoincludes a sodium metal counter electrode and a separator positioned between theanode and the sodium metal counter electrode.BRIEF DESCRIPTION OF THE DRAWINGS
[027] It is to be noted, however, that the appended drawings illustrate only typicalembodiments of the present subject matter and are therefore not to be consideredfor limiting its scope, for the present disclosure may admit to other equally effectiveembodiments. The detailed description is described with reference to theaccompanying figures. In the figures, a reference number identifies the figure inwhich the reference number first appears. The same numbers are used throughoutthe figures to reference features and components. Some embodiments of system ormethod or structure in accordance with embodiments of the present subject matterare now described, by way of example, and with reference to the accompanyingfigures, in which:
[028] Figure 1 illustrates a flow chart of a method of preparing an anode activematerial for a sodium-ion battery, in accordance with an embodiment of the presentinvention;
[029] Figure 2 illustrates the X-ray diffraction pattern of KFS@C, in accordancewith an embodiment of the present invention;
[030] Figure 3a and 3b illustrate the scanning electron micrographs (SEM) ofKFS@C, in accordance with an embodiment of the present invention;
[031] Figure 4a illustrates the galvanostatic charge discharge (GCD) profile ofKFS@C at 0.05 A g-1 current, in accordance with an embodiment of the presentinvention;
[032] Figure 4b illustrates the galvanostatic charge discharge (GCD) profile ofKFS@C at 0.5 A g-1 current, in accordance with an embodiment of the presentinvention
[033] Figure 4c illustrates the electrochemical cycling performance of KFS@Canode in half cell, in accordance with an embodiment of the present invention;
[034] Figure 5a illustrates rate capability of KFS@C, in accordance with anembodiment of the present invention;
[035] Figure 5b illustrates voltage-time profile at 5 A g-1, in accordance with anembodiment of the present invention; and
[036] Figure 5c illustrates voltage-time profile at 15 A g-1, in accordance with anembodiment of the present invention.
[037] The figures depict embodiments of the present subject matter for illustrationonly. A person skilled in art will easily recognize from the following descriptionthat alternative embodiments of the structures and methods illustrated herein maybe employed without departing from the principles of the disclosure describedherein.DETAILED DESCRIPTION
[038] While the embodiments of the disclosure are subject to variousmodifications and alternative forms, a specific embodiment thereof has been shownby way of example in the figures and will be described below. It should beunderstood, however, that it is not intended to limit the disclosure to the particularforms disclosed, but on the contrary, the disclosure is to cover all modifications,equivalents, and alternatives falling within the scope of the disclosure.
[039] The terms "comprises", "comprising", or any other variations thereof usedin the disclosure, are intended to cover a non-exclusive inclusion, such that a device,system, assembly that comprises a list of components does not include only thosecomponents but may include other components not expressly listed or inherent tosuch system, or assembly, or device. In other words, one or more elements in asystem or device proceeded by "comprises… a" does not, without more constraints,preclude the existence of other elements or additional elements in the system ordevice.
[040] The present invention relates to a method of preparing an anode activematerial for a sodium-ion battery, the anode active material includes potassiumdithioferrate (KFeS₂) and, in another embodiment, a potassium dithioferrate(KFeS₂)-multi-walled carbon nanotube (MWCNT) composite (hereinafter referredto as "KFS@C"). The invention further relates to the application of anode activematerial in sodium-ion electrochemical cell. The method employs a molten saltroute wherein potassium thiocyanate (KSCN) serves as a molten salt reactionmedium, enabling efficient formation of potassium dithioferrate (KFeS₂) withoutthe use of elemental sulphur.
[041] According to an embodiment, the present invention discloses a method(100) of preparing an anode active material for a sodium-ion battery as shown infigure 1. The method (100) includes a step (102) of mixing a ferric nitratenonahydrate (Fe (NO₃)₃·9H₂O) precursor with potassium thiocyanate (KSCN) toform a precursor mixture. The mixing may be carried out using conventionaltechniques such as grinding using mortar and pestle.
[042] The method (100) further includes a step (104) of heating the precursormixture to form potassium dithioferrate (KFeS₂) by a molten salt route to obtain aproduct containing KFeS2 and unreacted salt precursors, wherein the potassiumthiocyanate (KSCN) forms a molten salt reaction medium. During heating,potassium thiocyanate acts as both a potassium source and a sulphur source forformation of KFeS₂, and the process is performed in absence of elemental sulphur.The molten salt reaction medium facilitates enhanced reaction kinetics and uniformnucleation of the product.
[043] In an embodiment, heating the precursor mixture is performed under an inertatmosphere. The precursor mixture is heated at a temperature in a range from about550°C to about 700°C for a dwell time in a range from about 2 hours to about 4hours. Upon completion of the heating step, a product containing potassiumdithioferrate (KFeS₂) and residual salts is obtained. The method (100) furtherincludes step (106) of recovering the potassium dithioferrate as the anode activematerial from the product by washing with deionized (DI) water and drying.Washing the product with DI water removes residual salts of the molten salt route,thereby yielding purified potassium dithioferrate. The dried material constitutes theanode active material suitable for sodium-ion battery applications.
[044] In another embodiment, the method further includes combining multiwalled carbon nanotubes (MWCNTs) with the precursor mixture prior to heating,thereby forming a KFeS₂-MWCNT composite. The MWCNTs are uniformlymixed with the precursor mixture before the molten salt synthesis step, resulting inin-situ incorporation of conductive carbon with the KFeS₂ during formation. In apreferred embodiment, the MWCNTs are present in an amount of about 2 wt.% toabout 5 wt.% of the KFeS₂-MWCNT composite. The addition of MWCNTsenhances the electronic conductivity of the anode active material without requiringadditional processing steps.
[045] In another aspect, the present invention provides an anode active materialfor a sodium-ion battery including potassium dithioferrate (KFeS₂) having onedimensional rod-shaped particles and conductive carbon including multi-walledcarbon nanotubes (MWCNTs), wherein the MWCNTs are added in an amount ofabout 2 wt.% to about 5 wt.% during the synthesis. The one-dimensional rod-shapedmorphology of potassium dithioferrate provides shortened ion diffusion pathwaysand improved sodium ion transport, while the MWCNTs form a conductivenetwork that enhances electron transport within the electrode.
[046] According to another embodiment, the present invention provides a sodiumion electrochemical cell including a non-aqueous electrolyte containing a 1MNaPF₆ in diethylene glycol dimethyl ether (DEGDME), an anode in the aboveelectrolyte, wherein the anode includes potassium dithioferrate (KFeS₂) having onedimensional rod-shaped particles and conductive carbon including multi-walledcarbon nanotubes (MWCNTs), wherein the MWCNTs are added in an amount ofabout 2 wt.% to about 5 wt.% during the synthesis, a sodium metal counter electrodein the above electrolyte, and a separator positioned between the anode and thesodium metal counter electrode.
[047] During operation of the sodium-ion electrochemical cell, sodium ionsmigrate through the electrolyte and separator between the anode and the sodiummetal counter electrode. The potassium dithioferrate (KFeS₂) acts as a sodium ionhost, accommodating sodium ions during electrochemical cycling, while theconductive carbon including multi-walled carbon nanotubes facilitates efficientelectron transport. The one-dimensional rod-shaped structure of the potassiumdithioferrate further enables rapid sodium ion diffusion, thereby supporting highrate electrochemical performance.Exemplary Synthesis of KFeS₂-MWCNT Composite
[048] In an exemplary embodiment of the present invention, the KFeS₂-MWCNTcomposite anode active material is prepared by a molten salt route as follows.
[049] Approximately 1 g of ferric nitrate nonahydrate (Fe (NO₃)₃·9H₂O) is mixedwith 10 mg of multi-walled carbon nanotubes (MWCNTs) to form a uniformmixture. Subsequently, 10 g of potassium thiocyanate (KSCN) is added to themixture, and the components are thoroughly ground using a mortar and pestle toobtain a homogeneous dark brown precursor mixture.
[050] The obtained precursor mixture is then transferred to a tube furnace andsubjected to heating at a temperature in the range of about 550°C to about 700°Cfor a duration of about 2 hours to about 4 hours, with a ramping rate of about10°C / min, under an inert nitrogen (N₂) atmosphere. During this process, potassiumthiocyanate (KSCN) forms a molten salt reaction medium and acts as both apotassium source and a sulphur source, resulting in the formation of potassiumdithioferrate (KFeS₂) with in-situ incorporation of MWCNTs to form a KFeS₂-MWCNT composite.
[051] After completion of the heating step, the furnace is allowed to cool naturallyto room temperature. The obtained product is then dissolved in DI water andmaintained for approximately 1 hour to facilitate dissolution of residual saltsformed during the molten salt process. The product is subsequently washed with DIwater through vacuum filtration to remove remaining impurities.
[052] The filtered material is then subjected to vacuum drying at about 70°C toobtain the final KFeS₂-MWCNT composite anode active material. After drying, thematerial is transferred to a glove box for storage and further use in sodium-ionbattery fabrication.Exemplary Fabrication of Anode Electrode
[053] In an exemplary aspect of the present disclosure, a method for fabricatingan anode electrode for a sodium-ion battery (SIB) is provided.
[054] The method includes mixing uniformly the anode active material (KFS@C),conductive carbon additive (Super P C-65), and polyvinylidene fluoride (PVDF)binder in a mass ratio of 70:20:10 in an appropriate solvent, namely N-methyl-2-pyrrolidone (NMP), to form a homogeneous slurry. The mixing is carried out untila uniform dispersion of all components is achieved.
[055] The obtained slurry is then cast onto a carbon-coated copper foil using adoctor-blade technique to obtain the coated electrode. The coated foil issubsequently subjected to drying at about 85°C for an overnight duration to removethe solvent. After drying, the electrode sheet is further processed by calendaring,followed by punching into circular discs of about 10 mm diameter to obtain theanode electrodes suitable for cell assembly.Exemplary Fabrication of Sodium Half-Cell
[056] In another exemplary aspect of the present disclosure, a method forfabricating a sodium-ion half-cell is provided.
[057] The sodium half-cell is assembled using CR2032-type coin cells, whereinthe previously prepared anode electrode of approximately 10 mm diameter is usedas the working electrode. A sodium metal chip of about 12 mm diameter is used asboth the reference and counter electrode.
[058] A glass fiber separator (GF / D) of about 16 mm diameter is positionedbetween the working electrode and the sodium metal counter electrode.Subsequently, approximately 100 μL of a non-aqueous electrolyte having 1MNaPF₆ dissolved in diethylene glycol dimethyl ether (DEGDME) is added to thecell. The assembly of the coin cell is carried out inside an argon-filled glove box toprevent exposure to moisture and oxygen.Experimental results
[059] The high-capacity anode material KFeS₂ (hereinafter referred to as KFS)and its carbon-composited form, were synthesized via a molten salt route. For thesynthesis of KFS, the precursors iron nitrate nonahydrate (Fe(NO₃)₃·9H₂O) andpotassium thiocyanate (KSCN) were mixed in a weight ratio of 1:10. The precursorswere thoroughly ground to obtain a homogeneous dark brown mixture. Thismixture was subsequently subjected to heat treatment in a temperature range of 550-700°C for 2-4 hours with a ramping rate of 10°C min⁻¹ under a nitrogen (N₂)atmosphere. After the heat treatment, the obtained product was washed usingvacuum filtration to remove residual salts and then dried under vacuum at 70°C.
[060] To enhance the electronic conductivity of KFS, 2-5 wt% multi-walledcarbon nanotubes (MWCNTs) were incorporated, resulting in the compositematerial represented as KFS@C. The synthesis procedure for KFS@C followed asimilar route. Initially, Fe(NO₃)₃·9H₂O was mixed with 10 mg of MWCNTs,followed by the addition of KSCN. The mixture was ground thoroughly to form auniform dark brown precursor. This was then calcined at a temperature range from550-700°C for 2-4 hours under a nitrogen atmosphere with a heating rate of 10°Cmin⁻¹. The final product was washed via vacuum filtration to eliminate excess saltsand subsequently dried under vacuum at 70°C.
[061] The structural characteristics of the synthesized KFS@C were examinedusing X-ray diffraction (XRD), as shown in Figure 2. The diffraction patternexhibits sharp and well-defined peaks, indicating high crystallinity. The observedpeaks correspond to a monoclinic crystal structure, which is in good agreement withthe ICSD reference data (98-004-3451), confirming the successful formation of thedesired phase.
[062] The morphology of KFS@C was investigated using scanning electronmicroscopy (SEM), as presented in Figure 3. The micrographs reveal that thematerial predominantly exhibits a one-dimensional rod-like morphology, which isbeneficial for facilitating efficient ion transport.
[063] The electrochemical performance of KFS@C is illustrated in Figures 4(a)and 4(b) show the galvanostatic charge-discharge profiles at current densities of0.05 A g⁻¹ and 0.5 A g⁻¹ within a voltage window of 0.01-3 V. At 0.05 A g⁻¹,KFS@C delivers an initial discharge and charge capacity of 730.52 mAh g⁻¹ and653.51 mAh g⁻¹, respectively, corresponding to an initial coulombic efficiency(ICE) of 89.4%. The irreversible capacity loss is approximately 10.5%. Thedeliverable reversible discharge capacity at 0.05 A g⁻¹ is 669 mAh g⁻¹. At a highercurrent density of 0.5 A g⁻¹, the material delivers a high reversible capacity of 654.3mAh g⁻¹.
[064] Figure 4(c) presents the cycling performance of the KFS@C anode. Afteran initial formation cycle at 0.05 A g⁻¹, the cycling was carried out at 0.5 A g⁻¹. Theelectrode demonstrates excellent cycling stability, delivering a capacity of 659.21mAh g⁻¹ after 150 cycles with nearly 100% capacity retention.
[065] The rate capability of KFS@C was further evaluated over a wide range ofcurrent densities, as shown in Figure 5(a). The current density was progressivelyincreased from 0.05 A g⁻¹ to an ultra-high value of 15 A g⁻¹. The material deliversaverage discharge capacities of 590, 596.7, 573.42, 554.54, 540.13, 531.3, 494.67,345, 140.2, and 97.36 mAh g⁻¹ at current densities of 0.05, 0.1, 0.25, 0.5, 0.75, 1,2, 5, 10, and 15 A g⁻¹, respectively. Notably, when the current density is revertedfrom 15 A g⁻¹ back to 0.05 A g⁻¹, the electrode recovers a high capacity of 602.34mAh g⁻¹, demonstrating excellent structural stability and reversibility.
[066] Furthermore, the rate performance demonstrates that the KFS@C anodedelivers a capacity of 345 mAh g⁻¹ at a current density of 5 A g⁻¹ and 97.36 mAhg⁻¹ at 15 A g⁻¹. The voltage-time profiles shown in Figures 5(b) and 5(c) furtherindicate that the KFS@C electrode completes a full charge-discharge cycle withinapproximately 500 seconds (~8 minutes) at 5 A g⁻¹ and only 47 seconds at 15 A g⁻¹.This outstanding high-rate performance highlights the strong potential of KFS@Cas a fast-charging anode material for sodium-ion batteries (SIBs).
[067] The present invention provides a high-capacity and high-rate KFeS₂-basedanode material through an easy and one-step molten salt synthesis route that isefficient and scalable, wherein potassium thiocyanate acts as both potassium andsulphur source, and the process is performed in absence of elemental sulphur. Thesynthesis route is inexpensive and does not involve the use of toxic organic solvents.The in-situ incorporation of multi-walled carbon nanotubes during synthesiseliminates the need for additional compositing steps and improves the electronicconductivity of KFeS₂, thereby resulting in improved electrochemical performance.Further, washing with DI water effectively removes residual salts to yield a highpurity anode active material.
[068] While the invention has been described with reference to specificembodiments, it will be understood that modifications and variations may be madewithout departing from the scope of the invention as defined in the appended claims.
[069] It will be understood by those within the art that, in general, terms usedherein, and especially in the appended claims (e.g., bodies of the appended claims)are generally intended as "open" terms (e.g., the term "including" should beinterpreted as "including but not limited to," the term "having" should beinterpreted as "having at least," the term "includes" should be interpreted as"includes but is not limited to," etc.). It will be further understood by those withinthe art that if a specific number of an introduced claim recitation is intended, suchan intent will be explicitly recited in the claim, and in the absence of such recitation,no such intent is present. For example, as an aid to understanding, the followingappended claims may contain usage of the introductory phrases "at least one" and"one or more" to introduce claim recitations. However, the use of such phrasesshould not be construed to imply that the introduction of a claim recitation by theindefinite articles "a" or "an" limits any particular claim containing such introducedclaim recitation to disclosures containing only one such recitation, even when thesame claim includes the introductory phrases "one or more" or "at least one" andindefinite articles such as "a" or "an" (e.g., "a" and / or "an" should typically beinterpreted to mean "at least one" or "one or more"); the same holds true for the useof definite articles used to introduce claim recitations. Also, even if a specificnumber of an introduced claim recitation is explicitly recited, those skilled in theart will recognize that such recitation should typically be interpreted to mean at leastthe recited number (e.g., the bare recitation of "two recitations," without othermodifiers, typically means at least two recitations or two or more recitations).Furthermore, in those instances where a convention analogous to "at least one of A,B, and C, etc." is used, in general, such construction is intended in the sense onehaving skill in the art would understand the convention (e.g., "a system having atleast one of A, B, and C" would include but not be limited to systems that have Aalone, B alone, C alone, A and B together, A and C together, B and C together,and / or A, B, and C together, etc.). In those instances, where a convention analogousto "at least one of A, B, or C, etc." is used, in general, such construction is intendedin the sense one having skill in the art would understand the convention (e.g., "asystem having at least one of A, B, or C" would include but not be limited tosystems that have A alone, B alone, C alone, A and B together, A and C together,B and C together, and / or A, B, and C together, etc.). It will be further understoodby those within the art that virtually any disjunctive word and / or phrase presentingtwo or more alternative terms, whether in the description, claims, or drawings,should be understood to contemplate the possibilities of including one of the terms,either of the terms or both terms. For example, the phrase "A or B" will beunderstood to include the possibilities of "A" or "B" or "A and B."
[070] It will be further appreciated that functions or structures of a plurality ofcomponents or steps may be combined into a single component or step, or thefunctions or structures of one-step or component may be split among plural stepsor components. The present disclosure contemplates all of these combinations.Unless stated otherwise, dimensions and geometries of the various structuresdepicted herein are not intended to be restrictive of the disclosure, and otherdimensions or geometries are possible. Also, while a feature of the presentdisclosure may have been described in the context of only one of the illustratedembodiments, such feature may be combined with one or more other features ofother embodiments, for any given application. It will also be appreciated from theabove that the fabrication of the unique structures herein and the operation thereofalso constitute methods in accordance with the present disclosure. The presentdisclosure also encompasses intermediate and end products resulting from thepractice of the methods herein. It will be apparent to one of ordinary skill in the artthat methods, devices, device elements, materials, procedures, and techniques otherthan those specifically described herein may be applied to the practice of theinvention as broadly disclosed herein without resort to undue experimentation. Allart-known functional equivalents of methods, devices, device elements, materials,procedures, and techniques described herein are intended to be encompassed by thisinvention. The use of "comprising" or "including" also contemplates embodimentsthat "consist essentially of" or "consist of" the recited feature.
Claims
1. A method (100) of preparing an anode active material for a sodium-ion battery, the method (100) comprising: - mixing a ferric nitrate nonahydrate precursor with potassium thiocyanate (KSCN) to form a precursor mixture; - heating the precursor mixture to form potassium dithioferrate (KFeS₂) by a molten salt route to obtain a product containing KFeS2 and unreacted precursors, wherein the potassium thiocyanate (KSCN) forms a molten salt reaction medium; and - recovering the potassium dithioferrate as the anode active material from the former product by washing with deionized (DI) water and drying.
2. The method (100) as claimed in claim 1, wherein heating the precursor mixture is performed under an inert atmosphere.
3. The method (100) as claimed in claim 1, wherein the precursor mixture is heated at a temperature in a range from about 550°C to about 700°C for a dwell time in a range from about 2 hours to about 4 hours.
4. The method (100) as claimed in claim 1, wherein potassium thiocyanate acts as both a potassium source and a sulphur source for formation of KFeS₂, and wherein the process is performed in absence of elemental sulphur.
5. The method (100) as claimed in claim 1, further comprising combining multi-walled carbon nanotubes (MWCNTs) with the precursor mixture prior to said heating, thereby forming a KFeS₂-MWCNT composite.
6. The method (100) as claimed in claim 5, wherein the MWCNTs are added in an amount of about 2 wt.% to about 5 wt.% of the KFeS₂-MWCNT composite.
7. The method (100) as claimed in claim 1, wherein washing the product with DI water removes residual salts of the molten salt route.
8. An anode active material for a sodium-ion battery comprising: - potassium dithioferrate (KFeS₂) having one-dimensional rod-shaped particles; and- conductive carbon comprising multi-walled carbon nanotubes (MWCNTs), wherein the MWCNTs are added in an amount of about 2 wt.% to about 5 wt.% of the anode active material.
9. A sodium-ion electrochemical cell, comprising: - a non-aqueous electrolyte containing a 1M NaPF6 in diethylene glycol dimethyl ether (DEGDME); - an anode in the electrolyte, wherein the anode comprises potassium dithioferrate (KFeS₂) having one-dimensional rod-shaped particles and conductive carbon comprising multi-walled carbon nanotubes (MWCNTs), wherein the MWCNTs are added in an amount of about 2 wt.% to about 5 wt.% of the anode active material; - a sodium metal counter electrode in the electrolyte; and - a separator positioned between the anode and the sodium metal counter electrode.