Fe-BASED ELECTROPLATED STEEL SHEET, ELECTRODEPOSITION COATED STEEL SHEET, AUTOMOBILE COMPONENT, METHOD FOR MANUFACTURING ELECTRODEPOSITION COATED STEEL SHEET, AND METHOD FOR MANUFACTURING Fe-BASED ELECTROPLATED STEEL SHEET

IN607598BActive Publication Date: 2026-10-28JFE STEEL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
IN202317034455
Authority / Receiving Office
IN · IN
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-11-06
Filing Date
2023-05-17
Publication Date
2026-10-28
Estimated Expiration
2041-11-05
Patent Text Reader

Abstract

Provided is a steel sheet having excellent crack-resistance characteristic against resistance welding in a welded portion, even when crystal orientations of a Fe-based electroplating layer and a Si-containing cold-rolled steel sheet are integrated with a high rate at an interface between the Fe-based electroplating layer and the Si-containing cold-rolled steel sheet. This Fe-based electroplated steel sheet has: a Si-containing cold-rolled steel sheet containing 0.1 mass% to 3.0 mass% of Si; and a Fe-based electroplating layer formed on at least one side of the Si-containing cold-rolled steel sheet and having a deposition amount per single side of more than 20.0 g / m2, wherein the rate of crystal orientations of the Fe-based electroplating layer and the Si-containing integrated cold-rolled steel sheet, is more than 50% at an interface between the Fe-based electroplating layer and the Si-containing cold-rolled steel sheet.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] This disclosure relates to an Fe-based electroplated steel sheet withexcellent resistance to cracking in resistance welding, an electrodepositioncoatedsteel sheet, an automotive part, a method of producing anelectrodeposition-coated steel sheet, and a method of producing an Fe-basedelectroplated steel sheet.BACKGROUND

[0002] In recent years, there has been a strong demand to improve the fuelefficiency of automobiles from the viewpoint of protecting the globalenvironment. In addition, there has been a strong demand for improvedautomobile safety from the viewpoint of ensuring occupant safety in the eventof a collision. In order to meet these demands, it is necessary to achievelightweight and high-strength automotive bodies, and the use of high-strengthcold-rolled steel sheets as the material for automotive parts is being activelypromoted to achieve sheet metal thinning. However, since most automotiveparts are manufactured by forming steel sheets, these steel sheets are requiredto have excellent formability in addition to high strength.

[0003] There are various methods to increase the strength of cold-rolled steelsheets. One method that can increase strength without significantlycompromising the formability of cold-rolled steel sheets is solid solutionstrengthening by adding Si. On the other hand, in the manufacture ofautomotive parts, press-formed parts are often combined by resistance welding(spot welding). If the part to be subjected to resistance welding contains ahigh-strength galvanized steel sheet, there is concern that liquid metalembrittlement (LME) may occur during resistance welding when residualstresses are generated in the vicinity of a welded portion and the zinc in thecoated or plated layer melts and diffuses into crystal grain boundaries,resulting in intergranular cracking (or LME cracking) in the steel sheet. Inparticular, if welding is performed with the welding electrode at an angle tothe steel sheet, residual stresses may increase and cracks may form. Residualstresses are expected to increase with higher strength of the steel sheet, andthus there is concern about LME cracking associated with higher strength ofthe steel sheet. The problem is that even if a high-strength steel sheet doesnot have a galvanized layer, if the counterpart steel sheet to be welded is agalvanized steel sheet, the galvanized layer thereof melts and LME crackingcan occur in the steel sheet without a galvanized layer. This problem of LMEcracking is particularly pronounced in steel sheets containing Si.

[0004] Therefore, there is a need for a high-strength steel sheet with excellentresistance to cracking in resistance welding at a welded portion when combinedwith a galvanized steel sheet (hereinafter referred to simply as "resistance tocracking in resistance welding at a welded portion").

[0005] Conventionally, remedial measures for the above issues have beenreported. For example, JP 6388099 B (PTL 1) describes a steel sheet havingan internal oxidation layer in which the crystal grain boundaries are coated atleast partially with oxides from the surface of the base metal to a depth of 5.0μm or more, wherein the grain boundary coverage of the oxides is 60% ormore in the region ranging from the surface of the base metal to a depth of 5.0μm.CITATION LISTPatent Literature

[0006] PTL 1: JP 6388099 BSUMMARY(Technical Problem)

[0007] We have newly found that forming an Fe-based electroplating layer onthe surface of a cold-rolled steel sheet can improve the resistance to crackingin resistance welding. On the other hand, we also have found that, whenannealing is performed after the formation of the Fe-based electroplating layer,the crystal orientations of the Fe-based electroplating layer and the cold-rolledsteel sheet are integrated at a high ratio at the interface between the Fe-basedelectroplating layer and the cold-rolled steel sheet depending on the annealingconditions. We have found that, when such an Fe-based electroplated steelsheet is combined with a galvanized steel sheet, molten zinc easily penetratesinto the crystal grain boundaries in the cold-rolled steel sheet via the crystalgrain boundaries in the Fe-based electroplating layer. This is not describedin PTL 1 at all.

[0008] It could thus be helpful to provide a steel sheet with excellentresistance to cracking in resistance welding at a welded portion, even if thecrystal orientations of an Fe-based electroplating layer and a Si-containingcold-rolled steel sheet are integrated at a high ratio at the interface betweenthe Fe-based electroplating layer and the cold-rolled steel sheet.(Solution to Problem)

[0009] In order to solve the above problem, we have made intensive studiesand found that it is important to form an Fe-based electroplating layer with acoating weight per surface of more than 20.0 g / m2 on a surface of a cold-rolledsteel sheet after subjection to cold rolling and before subjection to continuousannealing to satisfy a high level of resistance to cracking in resistance weldingat a welded portion. We have found that forming a soft Fe-basedelectroplating layer with a coating weight of more than 20.0 g / m2 per surfaceof the cold-rolled steel sheet reduces the stress applied to the steel sheet surfaceduring welding, and, when the cold-rolled steel sheet contains Si, the Fe-basedelectroplating layer can act as a layer deficient in solute Si to suppress thedecrease in toughness due to solid dissolution of Si and improve the resistanceto cracking in resistance welding at a welded portion, thereby completing thepresent disclosure.

[0010] The present disclosure is based on the aforementioned discoveries.Specifically, primary features of the present disclosure are as follows.

[0011] [1] An Fe-based electroplated steel sheet comprising:a Si-containing cold-rolled steel sheet containing Si in an amount of0.1 mass% or more and 3.0 mass% or less; andan Fe-based electroplating layer formed on at least one surface of theSi-containing cold-rolled steel sheet with a coating weight per surface of morethan 20.0 g / m2, whereincrystal orientations of the Fe-based electroplating layer and the Sicontainingcold-rolled steel sheet are integrated at a ratio of more than 50% atan interface between the Fe-based electroplating layer and the Si-containingcold-rolled steel sheet.

[0012] [2] The Fe-based electroplated steel sheet according to aspect [1],wherein the Si-containing cold-rolled steel sheet contains Si in an amount of0.50 mass% or more and 3.0 mass% or less.

[0013] [3] The Fe-based electroplated steel sheet according to aspect [1] or[2], wherein the Fe-based electroplating layer is formed with a coating weightper surface of 25.0 g / m2 or more.

[0014] [4] The Fe-based electroplated steel sheet according to any one ofaspects [1] to [3], wherein the Si-containing cold-rolled steel sheet has achemical composition containing, in addition to Si, in mass%,C: 0.8% or less,Mn: 1.0% or more and 12.0% or less,P: 0.1% or less,S: 0.03% or less,N: 0.010% or less, andAl: 1.0% or less, with the balance being Fe and inevitable impurities.

[0015] [5] The Fe-based electroplated steel sheet according to aspect [4],wherein the chemical composition further contains at least one selected fromthe group consisting ofB: 0.005% or less,Ti: 0.2% or less,Cr: 1.0% or less,Cu: 1.0% or less,Ni: 1.0% or less,Mo: 1.0% or less,Nb: 0.20% or less,V: 0.5% or less,Sb: 0.200% or less,Ta: 0.1% or less,W: 0.5% or less,Zr: 0.1% or less,Sn: 0.20% or less,Ca: 0.005% or less,Mg: 0.005% or less, andREM: 0.005% or less.

[0016] [6] The Fe-based electroplated steel sheet according to any one ofaspects [1] to [5], wherein the Fe-based electroplating layer has a chemicalcomposition containing at least one element selected from the group consistingof B, C, P, N, O, Ni, Mn, Mo, Zn, W, Pb, Sn, Cr, V, and Co, in a total amountof 10 mass% or less, with the balance being Fe and inevitable impurities.

[0017] [7] An Fe-based electroplated steel sheet comprising:a cold-rolled steel sheet; andan Fe-based electroplating layer formed on at least one surface of thecold-rolled steel sheet with a coating weight per surface of more than 20.0 g / m2,whereincrystal orientations of the Fe-based electroplating layer and the coldrolledsteel sheet are integrated at a ratio of more than 50% at an interfacebetween the Fe-based electroplating layer and the cold-rolled steel sheet.As used herein, the cold-rolled steel sheet is a cold-rolled steel sheetwhere a test specimen of the cold-rolled steel sheet that is cut to a size of 50mm x 150 mm with a direction orthogonal to a rolling direction as a lengthwisedirection is overlapped with a test galvannealed steel sheet that is cut to thesame size having a hot-dip galvanized layer with a coating weight per surfaceof 50 g / m2 to obtain a sheet combination,next, using a 50-Hz single-phase AC resistance welding machine ofservomotor pressure type, the sheet combination is inclined 5° to a lengthwisedirection side of the sheet combination with respect to a plane perpendicularto a line connecting central axes of an electrode pair with a tip diameter of 6mm of the resistance welding machine, a lower electrode of the electrode pairand the sheet combination are fixed so that a gap of 60 mm in a lengthwisedirection of the sheet combination and 2.0 mm in a thickness direction of thesheet combination is provided between the lower electrode and the testspecimen, an upper electrode of the electrode pair is movable, and resistancewelding is applied to the sheet combination under a set of conditions: appliedpressure: 3.5 kN, hold time: 0.16 seconds, and welding current and weldingtime to produce a nugget diameter of 5.9 mm, to obtain a sheet combinationwith a welded portion, andthe sheet combination with a welded portion is then cut in half along alengthwise direction of the test specimen to include a welded portion, a crosssection of the welded portion is observed under an optical microscopy at amagnification of 200x, and a crack as long as 0.1 mm or more is observed.

[0018] [8] The Fe-based electroplated steel sheet according to aspect [7],wherein the cold-rolled steel sheet is a cold-rolled steel sheet where the sheetcombination with a welded portion is obtained by performing the resistancewelding with the hold time being 0.24 seconds, a cross section of the weldedportion is observed under the optical microscopy at a magnification of 200x,and a crack as long as 0.1 mm or more is observed.

[0019] [9] An electrodeposition-coated steel sheet comprising: a chemicalconversion layer formed on the Fe-based electroplated steel sheet as recited inany one of aspects [1] to [8] so as to contact the Fe-based electroplating layer;and an electrodeposition coating layer formed on the chemical conversion layer.

[0020]

[10] An automotive part at least partially made from theelectrodeposition-coated steel sheet as recited in aspect [9].

[0021]

[11] A method of producing an electrodeposition-coated steel sheet, themethod comprising:subjecting the Fe-based electroplated steel sheet as recited in any oneof aspects [1] to [8] to chemical conversion treatment, without additionalcoating or plating treatment, to obtain a chemical-conversion-treated steelsheet with a chemical conversion layer formed in contact with the Fe-basedelectroplating layer; andsubjecting the chemical-conversion-treated steel sheet toelectrodeposition coating treatment to obtain an electrodeposition-coated steelsheet with an electrodeposition coating layer formed on the chemicalconversion layer.

[0022]

[12] A method of producing an Fe-based electroplated steel sheet, themethod comprising:subjecting a cold-rolled steel sheet containing Si in an amount of 0.1mass% or more and 3.0 mass% or less to Fe-based electroplating to obtain apre-annealing Fe-based electroplated steel sheet with a pre-annealing Fe-basedelectroplating layer formed on at least one surface thereof with a coatingweight per surface of more than 20.0 g / m2; andthen subjecting the pre-annealing Fe-based electroplated steel sheet toannealing in an atmosphere with a dew point of -30 °C or lower to obtain anFe-based electroplated steel sheet.

[0023]

[13] The method of producing an Fe-based electroplated steel sheetaccording to aspect

[12] , wherein the cold-rolled steel sheet contains Si in anamount of 0.5 mass% or more and 3.0 mass% or less.

[0024]

[14] A method of producing an Fe-based electroplated steel sheet, themethod comprising:subjecting a cold-rolled steel sheet to Fe-based electroplating to obtaina pre-annealing Fe-based electroplated steel sheet with a pre-annealing Febasedelectroplating layer formed on at least one surface thereof with a coatingweight per surface of more than 20.0 g / m2; andthen subjecting the pre-annealing Fe-based electroplated steel sheet toannealing to obtain an Fe-based electroplated steel sheet.As used herein, the cold-rolled steel sheet is a cold-rolled steel sheetwhere a test specimen of the cold-rolled steel sheet that is cut to a size of 50mm x 150 mm with a direction orthogonal to a rolling direction as a lengthwisedirection is overlapped with a test galvannealed steel sheet that is cut to thesame size having a hot-dip galvanized layer with a coating weight per surfaceof 50 g / m2 to obtain a sheet combination,next, using a 50-Hz single-phase AC resistance welding machine ofservomotor pressure type, the sheet combination is inclined 5° to a lengthwisedirection side of the sheet combination with respect to a plane perpendicularto a line connecting central axes of an electrode pair with a tip diameter of 6mm of the resistance welding machine, a lower electrode of the electrode pairand the sheet combination are fixed so that a gap of 60 mm in a lengthwisedirection of the sheet combination and 2.0 mm in a thickness direction of thesheet combination is provided between the lower electrode and the testspecimen, an upper electrode of the electrode pair is movable, and resistancewelding is applied to the sheet combination under a set of conditions: appliedpressure: 3.5 kN, hold time: 0.16 seconds, and welding current and weldingtime to produce a nugget diameter of 5.9 mm, to obtain a sheet combinationwith a welded portion, andthe sheet combination with a welded portion is then cut in half along alengthwise direction of the test specimen to include a welded portion, a crosssection of the welded portion is observed under an optical microscopy at amagnification of 200x, and a crack as long as 0.1 mm or more is observed.

[0025]

[15] The method of producing an Fe-based electroplated steel sheetaccording to aspect

[14] , wherein the cold-rolled steel sheet is a cold-rolledsteel sheet where the sheet combination with a welded portion is obtained byperforming the resistance welding with the hold time being 0.24 seconds, across section of the welded portion is observed under an optical microscopy ata magnification of 200x, and a crack as long as 0.1 mm or more is observed.

[0026]

[16] The method of producing an Fe-based electroplated steel sheetaccording to any one of aspects

[12] to

[15] , wherein the Fe-basedelectroplating is performed in an Fe-based electroplating bath containing atleast one element selected from the group consisting of B, C, P, N, O, Ni, Mn,Mo, Zn, W, Pb, Sn, Cr, V, and Co, so that the at least one element is containedin the pre-annealing Fe-based electroplating layer in a total amount of 10mass% or less.(Advantageous Effect)

[0027] According to this disclosure, it is possible to provide a steel sheet withexcellent resistance to cracking in resistance welding at a welded portion, evenif the crystal orientations of an Fe-based electroplating layer and a Si10containing cold-rolled steel sheet are integrated at a high ratio at the interfacebetween the Fe-based electroplating layer and the cold-rolled steel sheet.BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In the accompanying drawings:FIG. 1 schematically illustrates a cross section of an Fe-basedelectroplated steel sheet;FIG. 2A is an oblique overview of a sample for observation to measurethe ratio of integrated crystal orientations, and FIG. 2B is an A-A cross sectionof the sample for observation;FIGS. 3A to 3C illustrate a method of evaluating the ratio of integratedcrystal orientations, where FIG. 3A illustrates a boundary line at the interfacebetween an Fe-based electroplating layer and a Si-containing cold-rolled steelsheet in a SIM image, FIG. 3B illustrates a boundary line and an area forevaluation in a binarized image, and FIG. 3C is an enlarged view of the areaenclosed by a square in FIG. 3B;FIG. 4 illustrates an image for observing the interface between the Febasedelectroplating layer and the Si-containing cold-rolled steel sheet inExample No. 31;FIG. 5 illustrates an image of the interface between the Fe-basedelectroplating layer and the Si-containing cold-rolled steel sheet in ExampleNo. 31, where a binarized boundary line and a binarized area for evaluation aredepicted;FIG. 6 illustrates an image for observing the interface between the Febasedelectroplating layer and the Si-containing cold-rolled steel sheet inExample No. 34;FIG. 7 illustrates an image of the interface between the Fe-basedelectroplating layer and the Si-containing cold-rolled steel sheet in ExampleNo. 34, where a binarized boundary line and a binarized area for evaluation aredepicted; andFIG. 8A illustrates evaluation of resistance to cracking in resistancewelding at a welded portion, and FIG. 8B illustrates a top view of a sheetcombination after welding in the evaluation in the upper part, and a B-B crosssection in the lower part.DETAILED DESCRIPTION

[0029] The LME cracking described above can be broadly classified intocracking that occurs on the surface in contact with the electrode (hereinafterreferred to as "surface cracking") and cracking that occurs near the coronabond between steel sheets (hereinafter referred to as "internal cracking"). Itis known that surface cracking is likely to occur in resistance welding at highcurrents where spatter is generated, and surface cracking can be suppressed bykeeping the current within an appropriate range where spatter is not generated.On the other hand, internal cracking occurs even when the current duringresistance welding is kept within an appropriate range where spatter is notgenerated. Surface cracking is easily detected by visual inspection during themanufacturing process, whereas internal cracking is difficult to detect byvisual inspection. For these reasons, internal cracking is a particularlysignificant issue among LME cracking. If resistance welding is performedwith the welding electrode at an angle to the steel sheet, residual stresses mayincrease and internal cracks may form. Since residual stresses are expectedto increase as the steel sheet has higher strength, there is concern about internalcracking associated with higher strength of the steel sheet. According to thepresent disclosure, among the resistance to cracking in resistance welding, theproperty of preventing such internal cracking can be improved.

[0030] The following describes embodiments of the present disclosure.In the following, the units for the content of each element in thechemical composition of the Si-containing cold-rolled steel sheet and thecontent of each element in the chemical composition of the coated or platedlayer are all "mass%", and are simply expressed in "%" unless otherwisespecified. As used herein, a numerical range expressed by using "to" meansa range including numerical values described before and after "to", as the lowerlimit value and the upper limit value. As used herein, a steel sheet having"high strength" means that the steel sheet has a tensile strength TS of 590 MPaor higher when measured in accordance with JIS Z 2241 (2011).

[0031] [Embodiment 1]FIG. 1 schematically illustrates a cross section of an Fe-basedelectroplated steel sheet 1 according to this embodiment. As illustrated inFIG. 1, the Fe-based electroplated steel sheet 1 has an Fe-based electroplatinglayer 3 on at least one surface of a Si-containing cold-rolled steel sheet 2.First, the chemical composition of the Si-containing cold-rolled steel sheet willbe explained.

[0032] Si: 0.1% or more and 3.0% or lessSi is an effective element for increasing the strength of a steel sheetbecause it has a large effect of increasing the strength of steel by soliddissolution (i.e., high solid solution strengthening capacity) withoutsignificantly impairing formability. On the other hand, Si is also an elementthat adversely affects the resistance to cracking in resistance welding at awelded portion. When Si is added to increase the strength of a steel sheet,the addition amount needs to be 0.1% or more. When the Si content is lessthan 0.50%, welding at a conventional hold time of about 0.24 seconds willnot cause any problem in terms of resistance to cracking in resistance weldingat a welded portion. However, the tact time during spot welding in theassembly process of automotive parts has become an issue from the viewpointof production cost, and when measures are taken to reduce the hold time, theresistance to cracking in resistance welding at a welded portion may becomeinsufficient even if the Si content is less than 0.50%. On the other hand, ifthe Si content exceeds 3.0%, hot rolling manufacturability and cold rollingmanufacturability are greatly reduced, which may adversely affect productivityand reduce the ductility of the steel sheet itself. Therefore, Si needs to beadded in the range of 0.1% to 3.0%. The Si content is preferably 0.50% ormore, more preferably 0.7% or more, and even more preferably 0.9% or more.Further, the Si content is preferably 2.5% or less, more preferably 2.0% orless, and even more preferably 1.7% or less.

[0033] The Si-containing cold-rolled steel sheet in this embodiment isrequired to contain Si in the above range, yet it may contain other componentswithin a range allowable for ordinary cold-rolled steel sheets. The othercomponents are not restricted in any particular way. However, if the Sicontainingcold-rolled steel sheet in this embodiment is to be made to havehigh strength with a tensile strength (TS) of 590 MPa or higher, the followingchemical composition is preferred.

[0034] C: 0.8% or less (exclusive of 0%)C improves formability by forming, for example, martensite as a steelmicrostructure. When C is contained, the C content is preferably 0.8% orless, and more preferably 0.3% or less, from the perspective of goodweldability. The lower limit of C is not particularly limited. However, toobtain good formability, the C content is preferably more than 0%, morepreferably 0.03% or more, and even more preferably 0.08% or more.

[0035] Mn: 1.0% or more and 12.0% or lessMn is an element that increases the strength of steel by solid solutionstrengthening, improves quench hardenability, and promotes the formation ofretained austenite, bainite, and martensite. These effects are obtained by theaddition of Mn in an amount of 1.0% or more. On the other hand, if the Mncontent is 12.0% or less, these effects can be obtained without causing anincrease in cost. Therefore, the Mn content is preferably 1.0% or more. TheMn content is preferably 12.0% or less. The Mn content is more preferably1.3% or more, even more preferably 1.5% or more, and most preferably 1.8% or more. The Mn content is more preferably 3.5% or less, and even morepreferably 3.3% or less.

[0036] P: 0.1% or less (exclusive of 0%)Suppressing the P content can contribute to preventing deterioration ofweldability. Suppressing the P content can also prevent P from segregating atgrain boundaries, thus preventing deterioration of ductility, bendability, andtoughness. In addition, adding a large amount of P promotes ferritetransformation, causing an increase in the crystal grain size. Therefore, the Pcontent is preferably 0.1% or less. The lower limit of the P content is notparticularly limited, yet may be greater than 0% or 0.001% or more, in termsof production technology constraints.

[0037] S: 0.03% or less (exclusive of 0%)The S content is preferably 0.03% or less, and more preferably 0.02%or less. Suppressing the S content can prevent deterioration of weldability aswell as deterioration of ductility during hot working, suppress hot cracking,and significantly improve surface characteristics. Furthermore, suppressingthe S content can prevent deterioration of ductility, bendability, and stretchflangeability of the steel sheet due to the formation of coarse sulfides asimpurity elements. These problems become more pronounced when the Scontent exceeds 0.03%, and it is preferable to reduce the S content as much aspossible. The lower limit of the S content is not particularly limited, yet maybe greater than 0% or 0.0001% or more, in terms of production technologyconstraints.

[0038] N: 0.010% or less (exclusive of 0%)The N content is preferably 0.010% or less. By setting the N contentto 0.010% or less, it is possible to prevent the effect of the addition of Ti, Nb,and V in increasing the strength of the steel sheet from being lost as a result ofN forming coarse nitrides with Ti, Nb, and V at high temperatures. Settingthe N content to 0.010% or less can also prevent deterioration of toughness.Furthermore, setting the N content to 0.010% or less can prevent slab crackingand surface defects during hot rolling. The N content is preferably 0.005%or less, more preferably 0.003% or less, and even more preferably 0.002% orless. The lower limit of the N content is not particularly limited, yet may begreater than 0% or 0.0005% or more, in terms of production technologyconstraints.

[0039] Al: 1.0% or less (exclusive of 0%)Since Al is thermodynamically most oxidizable, it oxidizes prior to Siand Mn, suppressing oxidation of Si and Mn at the topmost surface layer of thesteel sheet and promoting oxidation of Si and Mn inside the steel sheet. Thiseffect is obtained with an Al content of 0.01% or more. On the other hand,an Al content exceeding 1.0% increases the cost. Therefore, when added, theAl content is preferably 1.0% or less. The Al content is more preferably 0.1% or less. The lower limit of Al is not particularly limited, yet may be greaterthan 0% or 0.001% or more.

[0040] The chemical composition may further optionally contain at least oneelement selected from the group consisting of B: 0.005% or less, Ti: 0.2% orless, Cr: 1.0% or less, Cu: 1.0% or less, Ni: 1.0% or less, Mo: 1.0% or less,Nb: 0.20% or less, V: 0.5% or less, Sb: 0.200% or less, Ta: 0.1% or less, W:0.5% or less, Zr: 0.1% or less, Sn: 0.20% or less, Ca: 0.005% or less, Mg:0.005% or less, and REM: 0.005% or less.

[0041] B: 0.005% or lessB is an effective element in improving the quench hardenability of steel.To improve the quench hardenability, the B content is preferably 0.0003% ormore, and more preferably 0.0005% or more. However, since excessiveaddition of B reduces formability, the B content is preferably 0.005% or less.

[0042] Ti: 0.2% or lessTi is effective for strengthening of steel by precipitation. The lowerlimit of Ti is not limited, yet is preferably 0.005% or more to obtain thestrength adjustment effect. However, since excessive addition of Ti causesexcessive hard phase and reduces formability, the Ti content, when added, ispreferably 0.2% or less, and more preferably 0.05% or less.

[0043] Cr: 1.0% or lessThe Cr content is preferably 0.005% or more. Setting the Cr contentto 0.005% or more improves the quench hardenability and the balance betweenstrength and ductility. When added, the Cr content is preferably 1.0% or lessfrom the viewpoint of preventing cost increase.

[0044] Cu: 1.0% or lessThe Cu content is preferably 0.005% or more. Setting the Cu contentto 0.005% or more can promote formation of retained γ phase. When added,the Cu content is preferably 1.0% or less from the viewpoint of preventingcost increase.

[0045] Ni: 1.0% or lessThe Ni content is preferably 0.005% or more. Setting the Ni contentto 0.005% or more can promote formation of retained γ phase. When added,the Ni content is preferably 1.0% or less from the viewpoint of preventing costincrease.

[0046] Mo: 1.0% or lessThe Mo content is preferably 0.005% or more. Setting the Mocontent to 0.005% or more can yield a strength adjustment effect. The Mocontent is more preferably 0.05% or more. When added, the Mo content ispreferably 1.0% or less from the viewpoint of preventing cost increase.

[0047] Nb: 0.20% or lessSetting the Nb content to 0.005% or more is effective in increasingstrength. When added, the Nb content is preferably 0.20 % or less from theviewpoint of preventing cost increase.

[0048] V: 0.5% or lessSetting the V content to 0.005% or more is effective in increasingstrength. When added, the V content is preferably 0.5% or less from theviewpoint of preventing cost increase.

[0049] Sb: 0.200% or lessSb can be contained from the viewpoint of suppressing nitriding andoxidation of the steel sheet surface, or decarburization in an area of severaltens of microns on the steel sheet surface caused by oxidation. Sb suppressesnitriding and oxidation of the steel sheet surface, thereby preventing a decreasein the formation of martensite on the steel sheet surface and improving thefatigue resistance and surface quality of the steel sheet. To obtain this effect,the Sb content is preferably 0.001% or more. On the other hand, to obtaingood toughness, the Sb content is preferably 0.200% or less.

[0050] Ta: 0.1% or lessSetting the Ta content to 0.001% or more is effective in increasingstrength. When added, the Ta content is preferably 0.1% or less from theviewpoint of preventing cost increase.

[0051] W: 0.5% or lessSetting the W content to 0.005% or more is effective in increasingstrength. When added, the W content is preferably 0.5% or less from theviewpoint of preventing cost increase.

[0052] Zr: 0.1% or lessSetting the Zr content to 0.0005% or more is effective in increasingstrength. When added, the Zr content is preferably 0.1% or less from theviewpoint of preventing cost increase.

[0053] Sn: 0.20% or lessSn is an effective element in suppressing, for example, denitrificationand deboronization, thereby reducing the strength loss of steel. To obtainthese effects, the content is preferably 0.002% or more. On the other hand,to obtain good impact resistance, the Sn content is preferably 0.20% or less.

[0054] Ca: 0.005% or lessSetting the Ca content to 0.0005% or more makes it possible to controlsulfide morphology and improve ductility and toughness. From the viewpointof obtaining good ductility, the Ca content is preferably 0.005% or less.

[0055] Mg: 0.005% or lessSetting the Mg content to 0.0005% or more makes it possible to controlsulfide morphology and improve ductility and toughness. When added, theMg content is preferably 0.005% or less from the viewpoint of preventing costincrease.

[0056] REM: 0.005% or less.Setting the REM content to 0.0005% or more makes it possible tocontrol sulfide morphology and improve ductility and toughness. Whenadded, the REM content is preferably 0.005% or less from the viewpoint ofobtaining good toughness.

[0057] In the Si-containing cold-rolled steel sheet according to thisembodiment, the balance other than the above components is Fe and inevitableimpurities.

[0058] Next, an Fe-based electroplating layer formed on at least one surfaceof the aforementioned Si-containing cold-rolled steel sheet will be described.Fe-based electroplating layer: more than 20.0 g / m2Although the mechanism by which the presence of an Fe-basedelectroplating layer with a coating weight per surface of more than 20.0 g / m2improves the resistance to cracking in resistance welding at a welded portionis unclear, it is considered that the Fe-based electroplating layer functions as asoft layer to relax the stress given to the steel sheet surface during welding andcan reduce the residual stress at a resistance-welded portion to improve theresistance to cracking in resistance welding, especially internal cracking, at awelded portion (hereinafter referred to as the "stress relaxation effect").Further, it is considered that, when there is a large amount of solute Si on thesteel sheet surface, the toughness of a welded portion is decreased, and theresistance to cracking in resistance welding at a welded portion is deteriorated.In contrast, it is considered that, when a certain amount or more of an Fe-basedelectroplating layer is present on the steel sheet surface, the Fe-basedelectroplating layer acts as a layer deficient in solute Si and reduces the amountof solid dissolution of Si in a welded portion, which suppresses the decreasein toughness of a welded portion due to solid dissolution of Si and improvesthe resistance to cracking in resistance welding, especially internal cracking,at a welded portion (hereinafter referred to as the "toughness degradationsuppression effect"). On the other hand, annealing is performed after formingthe Fe-based electroplating layer in this embodiment, which will be describedlater. By performing annealing after forming the Fe-based electroplatinglayer, it is possible to suppress the occurrence of scratches called pick-ups onthe surface of the Fe-based electroplated steel sheet due to surface oxides ofSi and Mn and the like formed during the annealing. On the other hand, thecrystal orientations of the Fe-based electroplating layer and the Si-containingcold-rolled steel sheet are integrated at a ratio of more than 50% at theinterface between the Fe-based electroplating layer and the Si-containing coldrolledsteel sheet in this case. Accordingly, molten zinc easily penetrates intothe crystal grain boundaries in the Si-containing cold-rolled steel sheet via thecrystal grain boundaries in the Fe-based electroplating layer. Therefore, anFe-based electroplating layer with a coating weight of more than 20.0 g / m2 isformed in this embodiment. Forming an Fe-based electroplating layer with acoating weight of more than 20.0 g / m2 is considered to delay the time for thezinc melted during resistance welding to reach the crystal grain boundaries inthe Si-containing cold-rolled steel sheet, which improves the resistance tocracking in resistance welding, especially internal cracking, at a weldedportion (hereinafter referred to as the "effect of suppressing the intergranularpenetration of zinc"). Although the mechanism by which the stress relaxationeffect, the toughness degradation suppression effect, and the effect ofsuppressing the intergranular penetration of zinc obtained by the formation ofthe Fe-based electroplating layer contribute to the improvement of theresistance to cracking in resistance welding is complicated and notquantitatively clear, it is considered that these effects act in combination toimprove the resistance to cracking in resistance welding. In order to obtainthe effect of improving the resistance to cracking in resistance welding at awelded portion, the coating weight per surface of the Fe-based electroplatinglayer needs to be more than 20.0 g / m2. The upper limit of the coating weightper surface of the Fe-based electroplating layer is not particularly limited, yetis preferably 60.0 g / m2 or less from the cost perspective. The coating weightof the Fe-based electroplating layer is preferably 25.0 g / m2 or more, morepreferably 30.0 g / m2 or more, and even more preferably 35.0 g / m2 or more.The Fe-based electroplated steel sheet preferably has Fe-based electroplatinglayers on both front and back surfaces of the Si-containing cold-rolled steelsheet. By setting the coating weight of the Fe-based electroplating layer to25.0 g / m2 or more, particularly good resistance to cracking in resistancewelding at a welded portion can be obtained.

[0059] The thickness of the Fe-based electroplating layer is measured asfollows. A sample of 10 mm x 15 mm in size is taken from an Fe-basedelectroplated steel sheet and embedded in resin to make a cross-sectionalembedded sample. Three arbitrary locations on the same cross section areobserved using a scanning electron microscope (SEM) at an acceleratingvoltage of 15 kV and a magnification of 2,000x to 10,000x depending on thethickness of the Fe-based electroplating layer. Then, the average thickness inthe three fields of view is multiplied by the density of iron to convert the resultof observation to the coating weight per surface of the Fe-based electroplatinglayer.

[0060] The Fe-based electroplating layer may be an Fe (pure Fe) plating layer,or an alloy plating layer such as the one formed from Fe-B alloy, Fe-C alloy,Fe-P alloy, Fe-N alloy, Fe-O alloy, Fe-Ni alloy, Fe-Mn alloy, Fe-Mo alloy, Fe-W alloy, or another alloy. Although the chemical composition of the Fe-basedelectroplating layer is not particularly limited, it is preferable that the chemicalcomposition contain at least one element selected from the group consisting ofB, C, P, N, O, Ni, Mn, Mo, Zn, W, Pb, Sn, Cr, V, and Co, in a total amount of10 mass% or less, with the balance being Fe and inevitable impurities.Setting the total amount of elements other than Fe to 10 mass% or less canprevent a decrease in electrolytic efficiency, making it possible to form an Febasedelectroplating layer at low cost. In the case of Fe-C alloy, the C contentis preferably 0.08 mass% or less.

[0061] Preferably, the Si-containing cold-rolled steel sheet in this embodimenthas no coated or plated layer other than the Fe-based electroplating layer onits surface. The fact that the Si-containing cold-rolled steel sheet has nocoated or plated layer other than the Fe-based electroplating layer on its surfacemakes it possible to provide parts that do not require excessive galvanized steelsheets for corrosion prevention, or parts that are used in mild corrosionenvironments where excessive corrosion prevention is not required, at low cost.

[0062] The crystal orientations of the Fe-based electroplating layer and the Sicontainingcold-rolled steel sheet needs to be integrated at a ratio of more than50% at the interface between the Fe-based electroplating layer and the Sicontainingcold-rolled steel sheet. This is because, when the crystalorientations of the Fe-based electroplating layer and the Si-containing coldrolledsteel sheet are integrated at a ratio of more than 50% at the interfacebetween the Fe-based electroplating layer and the Si-containing cold-rolledsteel sheet, molten zinc easily penetrates into the crystal grain boundaries inthe Si-containing cold-rolled steel sheet via the crystal grain boundaries in theFe-based electroplating layer, and the effect of providing an Fe-basedelectroplating layer according to this embodiment becomes more pronounced.For the Fe-based electroplated steel sheet in this embodiment, the crystalorientations of the Fe-based electroplating layer and the Si-containing coldrolledsteel sheet may be integrated at a ratio of 70% or more or even 75% ormore at the interface between the Fe-based electroplating layer and the Sicontainingcold-rolled steel sheet. The crystal orientations of the Fe-basedelectroplating layer and the Si-containing cold-rolled steel sheet may beintegrated at a ratio of 100% at the interface between the Fe-basedelectroplating layer and the Si-containing cold-rolled steel sheet, where theupper limit of the ratio is not particularly limited.

[0063] As described above, when the ratio at which the crystal orientations ofthe Fe-based electroplating layer and the Si-containing cold-rolled steel sheetare integrated at the interface between the Fe-based electroplating layer andthe Si-containing cold-rolled steel sheet increases, it becomes easier for moltenzinc to penetrate into the crystal grain boundaries in the Si-containing coldrolledsteel sheet via the crystal grain boundaries in the Fe-based electroplatinglayer. This tendency is particularly pronounced when the crystal orientationsof the Fe-based electroplating layer and the Si-containing cold-rolled steelsheet are integrated at a ratio of more than 50% at the interface between theFe-based electroplating layer and the Si-containing cold-rolled steel sheet. Inthis embodiment, the crystal orientations of the Fe-based electroplating layerand the Si-containing cold-rolled steel sheet are integrated at a high ratiobecause the Si-containing cold-rolled steel sheet is subjected to Fe-basedelectroplating and then annealing, and it is annealed in a low dew-pointatmosphere as described below. Therefore, forming an Fe-basedelectroplating layer with a coating weight of more than 20.0 g / m2 is expectedto delay the penetration of molten zinc into the crystal grain boundaries in theSi-containing cold-rolled steel sheet via the crystal grain boundaries in the Fe25based electroplating layer, which is expected to further improve the resistanceto cracking in resistance welding, especially internal cracking, at a weldedportion.

[0064] The ratio at which the crystal orientations of the Fe-basedelectroplating layer and the Si-containing cold-rolled steel sheet are integratedat the interface between the Fe-based electroplating layer and the Si-containingcold-rolled steel sheet is measured as follows. A sample of 10 mm x 10 mmin size is taken from a Fe-based electroplated steel sheet. Any part of thesample is processed with a focused ion beam (FIB) device to form, at theprocessed part, a 45° cross section at an angle of 45° relative to the directionof a T-section (i.e., a cross section parallel to a direction orthogonal to therolling direction of the steel sheet and perpendicular to the steel sheet surface)with a width of 30 μm in a direction orthogonal to the rolling direction and alength of 50 μm in a direction 45° relative to the T-section direction. The 45°cross section thus formed is used as a sample for observation. FIGS. 2A and2B schematically illustrate the sample for observation. FIG. 2A is an obliqueview of the sample for observation. FIG. 2B is an A-A cross section of thesample for observation illustrated in FIG. 2A. Then, using a scanning ionmicroscope (SIM), the center of the 45° cross section of the sample forobservation is observed at a magnification of 5000x to capture an 8-bit SIMimage with a width of 1024 pixels and a height of 943 pixels. Using the SIMimages taken at each 45° cross section formed at three parts, the ratio at whichthe crystal orientations of the Fe-based electroplating layer and the Sicontainingcold-rolled steel sheet are integrated at the interface between theFe-based electroplating layer and the Si-containing cold-rolled steel sheet isdetermined based on the following equation (1). The result is rounded up toan integer.(Ratio at which the crystal orientations of the Fe-based electroplating layer andthe Si-containing cold-rolled steel sheet are integrated at the interface betweenthe Fe-based electroplating layer and the Si-containing cold-rolled steel sheet)= (Length of the area where the crystal orientations of the Fe-basedelectroplating layer and the Si-containing cold-rolled steel sheet are integratedon the interface between the Fe-based electroplating layer and the Sicontainingcold-rolled steel sheet) / (Length of the interface in the observationfield of view) x 100 (1)

[0065] Whether the crystal orientations of the Fe-based electroplating layerand the Si-containing cold-rolled steel sheet are integrated at the interfacebetween the Fe-based electroplating layer and the Si-containing cold-rolledsteel sheet or not is determined by image processing. FIGS. 3A to 3C are usedto illustrate a method of evaluating the ratio of integrated crystal orientations.First, as illustrated in FIG. 3A, a boundary line B is drawn on the interfacebetween the Fe-based electroplating layer and the Si-containing cold-rolledsteel sheet in the aforementioned SIM image using a scanning electronmicroscope. Next, an image-processed SIM image is created separately fromthe image in which the boundary line has been drawn. Specifically, the crystalgrain boundaries are first emphasized by the Sobel filter on the captured 8-bitSIM image with a width of 1024 pixels and a height of 943 pixels. The imagein which the crystal grain boundaries have been emphasized is then smoothedby the Gaussian filter (where the radius (R) is 10 pixels). Next, binarization(where the threshold is 17) is performed on the image after smoothing. Next,the boundary line B in the image where the interface has been depicted istransferred to the binarized image. Next, as illustrated in FIG. 3B, in theimage after binarization, an area for evaluation with a width of 40 pixelscentered on the boundary line B (the area enclosed by L1 and L2 in FIG. 3B) isdrawn along the boundary line B in the binarized image. The total lengthwhere the interface between the Fe-based electroplating layer and the Sicontainingcold-rolled steel sheet (the black-and-white boundary on thebinarized image) does not exist in the area for evaluation along the length ofthe boundary line B is regarded as the length of the area where the crystalorientations are integrated. The total length where the interface between theFe-based electroplating layer and the Si-containing cold-rolled steel sheet doesnot exist in the area for evaluation along the length of the boundary line isdetermined as follows. First, locations where the area for evaluation can bedivided into substantially rectangular parts where only one of black and whiteis included by two normal lines of the boundary line B are found out in theentire area for evaluation. Next, the maximum distance between theintersections of the boundary line and the two normal lines in those locationsis summed over the entire area for evaluation, and the result is regarded as thetotal length where the interface between the Fe-based electroplating layer andthe Si-containing cold-rolled steel sheet does not exist in the area forevaluation along the length of the boundary line. The length of the area wherethe crystal orientations are integrated may be determined by subtracting thelength of the area where the crystal orientations are not integrated from thelength of the interface in the observation field of view. For explanation, FIG.3C illustrates an enlarged view of the area enclosed by the square in FIG. 3B.First, as illustrated in FIG. 3C, locations where the area for evaluation can bedivided into substantially rectangular parts where two colors, black and white,are included by the two normal lines of the boundary line B (i.e. l1 and l2, andl3 and l4 in FIG. 3(C)) are found out in the entire area for evaluation. Next,the maximum distance between the intersections of the boundary line and thetwo normal lines in those locations is summed over the entire area forevaluation, and the result is regarded as the total length where the interfacebetween the Fe-based electroplating layer and the Si-containing cold-rolledsteel sheet exists in the area for evaluation along the length of the boundaryline. By subtracting this length, i.e., the length of the area where the crystalorientations are not integrated, from the length of the interface in theobservation field of view, the length of the area where the crystal orientationsare integrated can be determined.

[0066] FIG. 4 illustrates a SIM image of the interface between the Fe-basedelectroplating layer and the Si-containing cold-rolled steel sheet for ExampleNo. 31 described below. FIG. 5 illustrates an image after the SIM image hasbeen subjected to image processing and binarization processing as describedabove. In Example No. 31, the crystal orientations of the Fe-basedelectroplating layer and the Si-containing cold-rolled steel sheet wereintegrated at a ratio of 97% at the interface between the Fe-basedelectroplating layer and the Si-containing cold-rolled steel sheet. Further,FIG. 6 illustrates a SIM image of the interface between the Fe-basedelectroplating layer and the Si-containing cold-rolled steel sheet for ExampleNo. 34 described below. FIG. 7 illustrates an image after the SIM image hasbeen subjected to image processing and binarization processing as describedabove. In Example No. 34, the crystal orientations of the Fe-basedelectroplating layer and the Si-containing cold-rolled steel sheet wereintegrated at a ratio of 95% at the interface between the Fe-basedelectroplating layer and the Si-containing cold-rolled steel sheet.

[0067] According to the present disclosure, it is possible to provide a highstrengthFe-based electroplated steel sheet with a tensile strength TS of 590MPa or more when measured in accordance with JIS Z 2241 (2011). Thestrength of the Fe-based electroplating steel sheet is more preferably 800 MPaor more.

[0068] The thickness of the Fe-based electroplated steel sheet in thisembodiment is not particularly limited, yet may usually be 0.5 mm or more and3.2 mm or less.

[0069] <Method of Producing Fe-based Electroplated Steel Sheet>Next, a method of producing an Fe-based electroplated steel sheet willbe described.A method of producing an Fe-based electroplated steel sheet accordingto one embodiment may be a method of producing an Fe-based electroplatedsteel sheet comprising:subjecting a cold-rolled steel sheet containing Si in an amount of 0.1mass% or more and 3.0 mass% or less to Fe-based electroplating to obtain apre-annealing Fe-based electroplated steel sheet with a pre-annealing Fe-basedelectroplating layer formed on at least one surface thereof with a coatingweight per surface of more than 20.0 g / m2; andthen subjecting the pre-annealing Fe-based electroplated steel sheet toannealing in an atmosphere with a dew point of -30 °C or lower to obtain anFe-based electroplated steel sheet.

[0070] First, a cold-rolled steel sheet containing Si in an amount of 0.1 mass%or more and 3.0 mass% or less is produced. The cold-rolled steel sheet maycontain Si in an amount of 0.50 mass% or more and 3.0 mass% or less.Regarding the method of producing a cold-rolled steel sheet, conventionalmethods may be followed. In one example, a cold-rolled steel sheet isproduced by hot rolling a steel slab having the chemical composition describedabove to obtain a hot-rolled sheet, then subjecting the hot-rolled sheet to acidcleaning, and then cold rolling the hot-rolled sheet to obtain a cold-rolled steelsheet.

[0071] Next, the surface of the cold-rolled steel sheet is subjected to Fe-basedelectroplating to obtain a pre-annealing Fe-based electroplated steel sheet.The Fe-based electroplating is not limited to a particular method. Forexample, a sulfuric acid bath, a hydrochloric acid bath, or a mixture of the twocan be used as an Fe-based electroplating bath. The term "pre-annealing Febasedelectroplated steel sheet" means that the Fe-based electroplating layerhas not undergone an annealing process, and does not exclude the cold-rolledsteel sheet having been annealed before subjection to Fe-based electroplating.

[0072] The Fe ion content in the Fe-based electroplating bath before the startof current passage is preferably 0.5 mol / L or more as Fe2+. If the Fe ioncontent in the Fe-based electroplating bath is 0.5 mol / L or more as Fe2+, asufficient Fe coating weight can be obtained. In order to obtain a sufficientFe coating weight, the Fe ion content in the Fe-based electroplating bath beforethe start of current passage is preferably 2.0 mol / L or less.

[0073] The Fe-based electroplating bath may contain Fe ions and at least oneelement selected from the group consisting of B, C, P, N, O, Ni, Mn, Mo, Zn,W, Pb, Sn, Cr, V, and Co. The total content of these elements in the Fe-basedelectroplating bath is preferably adjusted so that the total content of theseelements in the pre-annealing Fe-based electroplating layer is 10 mass% or less.Metallic elements may be contained as metal ions, while non-metallic elementsmay be contained as part of, for example, boric acid, phosphoric acid, nitricacid, or organic acid. The iron sulfate plating solution may also containconductivity aids such as sodium sulfate and potassium sulfate, chelatingagents, or pH buffers.

[0074] Other conditions for the Fe-based electroplating bath are not limited.The temperature of the Fe-based electroplating solution is preferably 30 °C orhigher, and it is preferably 85 °C or lower, for constant temperature retention.Although the pH of the Fe-based electroplating bath is not specified, it ispreferably 1.0 or more from the viewpoint of preventing a decrease in currentefficiency due to hydrogen generation. In addition, it is preferably 3.0 or lessconsidering the electrical conductivity of the Fe-based electroplating bath.The current density is preferably 10 A / dm2 or higher for productivity. It ispreferably 150 A / dm2 or lower for ease of control of coating weight of the Febasedelectroplating layer. The sheet passing speed is preferably 5 mpm orhigher for productivity. It is preferably 150 mpm or lower for stable controlof coating weight.

[0075] Prior to the Fe-based electroplating, degreasing and water washing maybe performed to clean the surface of the cold-rolled steel sheet, and acidcleaning and water washing may also be performed to activate the surface ofthe cold-rolled steel sheet. Following these pretreatments, Fe-basedelectroplating is performed. The methods of degreasing and water washingare not limited, and conventional methods may be followed. Various acidssuch as sulfuric acid, hydrochloric acid, nitric acid, and mixtures of these acidscan be used in the acid cleaning. Among these preferred are sulfuric acid,hydrochloric acid, or a mixture of these. Although the acid concentration isnot specified, approximately 1 mass% to 20 mass% is preferable consideringthe ability to remove oxide coating and the prevention of rough skin (surfacedefects) due to excessive acid cleaning. The acid cleaning solution may alsocontain, for example, a defoamer, an acid cleaning promoter, or an acidcleaning inhibitor.

[0076] Then, after the Fe-based electroplating, the pre-annealing Fe-basedelectroplated steel sheet is subjected to an annealing process in which the steelsheet is held in a temperature range of 650 °C to 900 °C for 30 seconds to 600seconds in a reducing atmosphere with a dew point of -30 °C or lower and ahydrogen concentration from 1.0 vol.% to 30.0 vol.%, and then cooled to obtainan Fe-based electroplated steel sheet. The annealing process is performed toincrease the strength of the steel sheet by relieving the stress in the preannealingFe-based electroplated steel sheet caused by the rolling process andrecrystallizing the microstructure of the pre-annealing Fe-based electroplatedsteel sheet.

[0077] Dew Point: -30 °C or lowerIn this embodiment, the dew point of the annealing atmosphere in theannealing process is a low dew point of -30 °C or lower, which is a conditionthat requires no additional equipment such as humidification equipment. It ispreferable to control the dew point to -30 °C or lower in a temperature rangeof 650 °C to 900 °C . According to our original study, we have found thatthere is a correlation between the ratio at which the crystal orientations of theFe-based electroplating layer and the Si-containing cold-rolled steel sheet areintegrated at the interface between the Fe-based electroplating layer and theSi-containing cold-rolled steel sheet and the dew point of the annealingatmosphere in the annealing process after the formation of the Fe-basedelectroplating layer. We found that, when the pre-annealing Fe-basedelectroplated steel sheet is subjected to annealing after the formation of the Febasedelectroplating layer, the ratio at which the crystal orientations of the Febasedelectroplating layer and the Si-containing cold-rolled steel sheet areintegrated of the Fe-based electroplated steel sheet obtained after annealingincreases as the dew point of the annealing atmosphere decreases, and the ratioat which the crystal orientations of the Fe-based electroplating layer and theSi-containing cold-rolled steel sheet are integrated decreases as the dew pointof the annealing atmosphere increases. The reason why there is such acorrelation between the ratio at which the crystal orientations of the Fe-basedelectroplating layer and the Si-containing cold-rolled steel sheet are integratedand the dew point is not clear, but can be inferred as follows. In the case ofa high dew point not lower than a certain temperature, elements that diffusefrom the steel sheet to the Fe-based electroplating layer during annealing formoxides inside the Fe-based electroplating layer, and these oxides inhibit thecrystal growth of the Fe-based electroplating layer and make the grains finer.On the other hand, if annealing is performed in an atmosphere with a low dewpoint after the formation of the Fe-based electroplating layer, theabovementioned oxides are less likely to form, and the crystal grains of the Febasedelectroplating layer are coarsened. Therefore, it is considered that thecrystal orientation of the Fe-based electroplating layer integrates with thecrystal orientation of the Si-containing cold-rolled steel sheet at a high ratiowhen annealing is performed at a low dew point. When the dew point of theannealing atmosphere in the annealing process is set to -30 °C or lowerconsidering, for example, costs of humidification equipment in an annealingfurnace, the ratio at which the crystal orientations of the Fe-basedelectroplating layer and the Si-containing cold-rolled steel sheet are integratedat the interface between the Fe-based electroplating layer and the Si-containingcold-rolled steel sheet increases. Accordingly, when it is combined with agalvanized steel sheet, zinc melted during resistance welding easily penetratesinto the crystal grain boundaries in the Si-containing cold-rolled steel sheet viathe crystal grain boundaries in the Fe-based electroplating layer. In thisembodiment, forming an Fe-based electroplating layer with a certain coatingweight delays the time for the zinc melted during resistance welding to reachthe crystal grain boundaries in the Si-containing cold-rolled steel sheet via thecrystal grain boundaries in the Fe-based electroplating layer when combinedwith a galvanized steel sheet, thereby improving the resistance to cracking inresistance welding at a welded portion. The lower limit of the dew point ofthe annealing atmosphere is not specified, yet it is preferably -80 °C or higherbecause it is industrially difficult to achieve a dew point lower than -80 °C .The dew point of the annealing atmosphere is more preferably -55 °C or higher.

[0078] Hydrogen Concentration: 1.0 vol.% or more and 30.0 vol.% or lessThe annealing process is performed in a reducing atmosphere with ahydrogen concentration of 1.0 vol.% or more and 30.0 vol.% or less.Hydrogen plays a role in suppressing the oxidation of Fe on the surface of thepre-annealing Fe-based electroplated steel sheet during the annealing processand activating the steel sheet surface. If the hydrogen concentration is 1.0vol.% or more, it is possible to avoid the deterioration of the chemicalconvertibility, which would otherwise be caused by the oxidation of Fe on thesteel sheet surface when a chemical conversion layer is formed as describedbelow. Therefore, the annealing process is performed in a reducingatmosphere with a hydrogen concentration of preferably 1.0 vol.% or more,and more preferably 2.0 vol.% or more. Although the upper limit of thehydrogen concentration in the annealing process is not particularly limited,from the cost perspective, the hydrogen concentration is preferably 30.0 vol.%or less, and more preferably 20.0 vol.% or less. The balance of the annealingatmosphere other than hydrogen is preferably nitrogen.

[0079] Holding Time in Temperature Range of 650 °C to 900 °C : 30 Secondsto 600 SecondsIn the annealing process, the holding time in the temperature range of650 °C to 900 °C is preferably from 30 seconds to 600 seconds. By settingthe holding time in this temperature range to 30 seconds or more, the naturaloxide layer of Fe formed on the surface of the pre-annealing Fe-basedelectroplating layer can be suitably removed, and the chemical convertibilitycan be improved when a chemical conversion layer is formed on the surface ofthe Fe-based electroplated steel sheet as described below. Therefore, theholding time in this temperature range is preferably 30 seconds or more. Theupper limit of the holding time in this temperature range is not specified, yetfrom the viewpoint of productivity, the holding time in this temperature rangeis preferably 600 seconds or less.

[0080] Maximum Arrival Temperature of Pre-annealing Fe-basedElectroplated Steel Sheet: 650 °C to 900 °C The maximum arrival temperature of the pre-annealing Fe-basedelectroplated steel sheet is not particularly limited, yet it is preferably from650 °C to 900 °C . By setting the maximum arrival temperature of the preannealingFe-based electroplated steel sheet to 650 °C or higher,recrystallization of the microstructure of the steel sheet can suitably proceedand the desired strength can be obtained. In addition, the natural oxide layerof Fe formed on the surface of the pre-annealing Fe-based electroplating layercan be suitably reduced, improving the chemical convertibility when forminga chemical conversion layer on the surface of the Fe-based electroplated steelsheet as described below. In addition, by setting the maximum arrivaltemperature of the Fe-based electroplated steel sheet to 900 °C or lower, thediffusion rate of Si and Mn in the steel is prevented from increasing too muchand the diffusion of Si and Mn to the steel sheet surface can be prevented,making it possible to improve the chemical convertibility when forming achemical conversion layer on the steel sheet surface as described below. Ifthe maximum arrival temperature is 900 °C or lower, damage to the heattreatment furnace can be prevented and costs can be reduced. Therefore, themaximum arrival temperature of the pre-annealing Fe-based electroplated steelsheet is preferably 900 °C or lower. The maximum arrival temperature isbased on the temperature measured on the surface of the pre-annealing Fe35based electroplated steel sheet.

[0081] <Electrodeposition-coated Steel Sheet>According to this embodiment, it is also possible to provide anelectrodeposition-coated steel sheet comprising: a chemical conversion layerformed on the aforementioned Fe-based electroplated steel sheet so as tocontact the Fe-based electroplating layer; and an electrodeposition coatinglayer formed on the chemical conversion layer. The Fe-based electroplatedsteel sheet in this embodiment has excellent resistance to cracking in resistancewelding at a welded portion. Therefore, an electrodeposition-coated steelsheet formed using the Fe-based electroplated steel sheet disclosed herein isparticularly suitable for application to automotive parts. It is preferable thatthe electrodeposition-coated steel sheet in this embodiment have a chemicalconversion layer formed directly on the Fe-based electroplating layer. Inother words, it is preferable that the electrodeposition-coated steel sheet in thisembodiment have no additional coated or plated layer besides the Fe-basedelectroplating layer. The types of the chemical conversion layer and theelectrodeposition coating layer are not limited, and publicly known chemicalconversion layers and electrodeposition coating layers may be used. Thechemical conversion layer may be, for example, a zinc phosphate layer or azirconium layer. The electrodeposition coating layer is not limited as long asit is an electrodeposition coating layer for automotive use. The thickness ofthe electrodeposition coating layer varies depending on the application.However, it is preferably about 10 μm or more in the dry state. It is preferablyabout 30 μm or less in the dry state. According to this embodiment, it is alsopossible to provide an Fe-based electroplated steel sheet for electrodepositioncoating to apply electrodeposition coating.

[0082] <Method of Producing Electrodeposition-coated Steel Sheet>Next, a method of producing the aforementioned electrodepositioncoatedsteel sheet will be described. The aforementioned electrodepositioncoatedsteel sheet may be produced with a method of producing anelectrodeposition-coated steel sheet, the method comprising: subjecting the Fe30based electroplated steel sheet to chemical conversion treatment, withoutadditional coating or plating treatment, to obtain a chemical-conversiontreatedsteel sheet with a chemical conversion layer formed in contact with theFe-based electroplating layer; and subjecting the chemical-conversion-treatedsteel sheet to electrodeposition coating treatment to obtain anelectrodeposition-coated steel sheet with an electrodeposition coating layerformed on the chemical conversion layer. Regarding the chemical conversiontreatment and electrodeposition coating treatment, conventional methods maybe followed. Prior to the chemical conversion treatment, degreasing, waterwashing, and if necessary, surface conditioning treatment may be performed toclean the surface of the Fe-based electroplated steel sheet. Thesepretreatments are followed by the chemical conversion treatment. Themethods of degreasing and water washing are not limited, and conventionalmethods may be followed. In the surface conditioning treatment, surfaceconditioners containing Ti colloids or zinc phosphate colloids can be used, forexample. Regarding the application of these surface conditioners, no specialprocess is required and conventional methods may be followed. For example,the desired surface conditioner is dissolved in a certain deionized water andstirred thoroughly to obtain a treatment solution at a predeterminedtemperature (usually room temperature, i.e., 25 °C to 30 °C ). Then, the steelsheet is immersed in the obtained treatment solution for a predetermined time(e.g., 20 seconds to 30 seconds). The steel sheet is then subjected to thesubsequent chemical conversion treatment without being dried. Regardingthe chemical conversion treatment, conventional methods may be followed.For example, the desired chemical conversion treatment agent is dissolved ina certain deionized water and stirred thoroughly to obtain a treatment solutionat a predetermined temperature (usually 35 °C to 45 °C ). Then, the steel sheetis immersed in the obtained treatment solution for a predetermined time (e.g.,60 seconds to 120 seconds). As the chemical conversion treatment agent, forexample, a zinc phosphate treatment agent for steel, a zinc phosphate treatmentagent for combined use of steel and aluminum, or a zirconium treatment agentmay be used. The steel sheet is then subjected to the subsequentelectrodeposition coating. Regarding the electrodeposition coating,conventional methods may be followed. After pretreatment such as waterwashing, if necessary, the steel sheet is immersed in an electrodepositioncoating material that has been thoroughly stirred to obtain the desired thicknessof electrodeposition coating by electrodeposition treatment. As theelectrodeposition coating, anionic electrodeposition coating as well as cationicelectrodeposition coating can be used. Furthermore, for example, top coatingmay be applied after the electrodeposition coating, depending on theapplication.

[0083] <Automotive Part>According to this embodiment, it is also possible to provide anautomotive part that is at least partially made from the electrodeposition-coatedsteel sheet described above. The Fe-based electroplated steel sheet in thisembodiment has excellent resistance to cracking in resistance welding at awelded portion. Therefore, an electrodeposition-coated steel sheet using theFe-based electroplated steel sheet disclosed herein is particularly suitable forapplication to automotive parts. The automotive part made from theelectrodeposition-coated steel sheet may contain a steel sheet other than theelectrodeposition-coated steel sheet in this embodiment as the raw material.Since the electrodeposition-coated steel sheet in this embodiment has excellentresistance to cracking in resistance welding at a welded portion, cracking issuitably prevented from occurring at a welded portion even when theautomotive part made from the Fe-based electroplated steel sheet includes ahigh-strength hot-dip galvanized steel sheet as a welding counterpart. Thetypes of the automotive part at least partially made from the electrodeposition15coated steel sheet are not limited. However, the automotive part may be, forexample, a side sill part, a pillar part, or an automotive body.

[0084] [Embodiment 2]Next, an Fe-based electroplated steel sheet according to Embodiment 2of the present disclosure will be described.The Fe-based electroplated steel sheet in this embodiment may be anFe-based electroplated steel sheet comprising:a cold-rolled steel sheet; andan Fe-based electroplating layer formed on at least one surface of thecold-rolled steel sheet with a coating weight per surface of more than 20.0 g / m2,wherethe crystal orientations of the Fe-based electroplating layer and thecold-rolled steel sheet are integrated at a ratio of more than 50% at theinterface between the Fe-based electroplating layer and the cold-rolled steelsheet.As used herein, the cold-rolled steel sheet is a cold-rolled steel sheetwhere a test specimen of the cold-rolled steel sheet that is cut to a size of 50mm x 150 mm with a direction orthogonal to the rolling direction as thelengthwise direction is overlapped with a test galvannealed steel sheet that iscut to the same size having a hot-dip galvanized layer with a coating weightper surface of 50 g / m2 to obtain a sheet combination,next, using a single-phase AC (50 Hz) resistance welding machine ofservomotor pressure type, the sheet combination is inclined 5° to thelengthwise direction side of the sheet combination with respect to a planeperpendicular to a line connecting the central axes of an electrode pair (tipdiameter 6 mm) of the resistance welding machine, the lower electrode of theelectrode pair and the sheet combination are fixed so that a gap of 60 mm inthe lengthwise direction of the sheet combination and 2.0 mm in the thicknessdirection of the sheet combination is provided between the lower electrode andthe test specimen, the upper electrode of the electrode pair is movable, andresistance welding is applied to the sheet combination under the followingconditions: applied pressure: 3.5 kN, hold time: 0.16 seconds, and weldingcurrent and welding time to produce a nugget diameter of 5.9 mm, to obtain asheet combination with a welded portion, andthe sheet combination with a welded portion is then cut in half alongthe lengthwise direction of the test specimen to include a welded portion, across section of the welded portion is observed under an optical microscopy(magnification 200x), and a crack as long as 0.1 mm or more is observed.

[0085] The cold-rolled steel sheet in this embodiment is not particularlylimited if it is a steel sheet inferior in resistance to cracking in resistancewelding at a welded portion when combined with a galvanized steel sheet andevaluated by the following test. The chemical composition of the cold-rolledsteel sheet is not particularly limited. We have found that a cold-rolled steelsheet containing Si in an amount of 0.1 mass% or more in the steel is inferiorin resistance to cracking in resistance welding at a welded portion whenevaluated by the following test.

[0086] The cold-rolled steel sheet may be a cold-rolled steel sheet where thesheet combination with a welded portion is obtained by performing theresistance welding at a hold time of 0.24 seconds, a cross section of the weldedportion is observed under an optical microscopy (magnification 200x), and acrack as long as 0.1 mm or more is observed. In the case of the same cold30rolled steel sheet, the resistance to cracking in resistance welding at a weldedportion generally deteriorates as the hold time decreases. Therefore, if cracksas long as 0.1 mm or more are observed in a cold-rolled steel sheet when thefollowing test is performed at a hold time of 0.24 seconds, cracks as long as0.1 mm or more can be observed when the cross section of a welded portion isobserved under an optical microscopy (magnification 200x) even when theresistance welding is performed at a hold time of 0.16 seconds. If the coldrolledsteel sheet contains Si in an amount of 0.50 mass% or more in the steel,it is inferior in resistance to cracking in resistance welding at a welded portionwhen evaluated by the following test. However, it has also been confirmedthat even a cold-rolled steel sheet containing Si in an amount of less than 0.50mass% in the steel may be inferior in resistance to cracking in resistancewelding at a welded portion when evaluated by the following test.

[0087] <Resistance to Cracking in Resistance Welding at Welded PortionWhen Combined with Galvanized Steel Sheet>The evaluation method of the resistance to cracking in resistancewelding at a welded portion will be described below with reference to FIGS.8A and 8B. As a sheet combination, a test specimen 6 that is cut to a size of50 mm x 150 mm with the transverse direction ("TD", direction orthogonal tothe rolling direction) as the lengthwise direction and the rolling direction asthe widthwise direction is overlapped with a test galvannealed steel sheet 5that is cut to the same size having a hot-dip galvanized layer with a coatingweight per surface of 50 g / m2. The sheet combination is assembled so thatthe surface to be evaluated (Fe-based electroplated layer) of the test specimen6 and the galvanized layer of the test galvannealed steel sheet 5 face each other.The sheet combination is fixed to a fixing stand 8 via spacers 7 of 2.0 mm thick.The spacers 7 are a pair of steel sheets, each measuring 50 mm long (lengthwisedirection) x 45 mm wide (widthwise direction) x 2.0 mm thick (thicknessdirection). As illustrated in FIG. 8A, the lengthwise end faces of the pair ofsteel sheets are aligned with the widthwise end faces of the sheet combination.Thus, the distance between the pair of steel sheets is 60 mm. The fixing stand8 is a single plate with a hole in the center.

[0088] Then, using a single-phase AC (50 Hz) resistance welding machine ofservomotor pressure type, the sheet combination is subjected to resistancewelding at a welding current and a welding time that result in a nugget diameterr of 5.9 mm while being deflected by applying pressure with a pair of electrodes9 (tip diameter: 6 mm) under the conditions of an applied pressure of 3.5 kNand a hold time of 0.18 seconds or 0.24 seconds, to form a sheet combinationwith a welded portion. The pair of electrodes 9 pressurize the sheetcombination from above and below in the vertical direction, with the lowerelectrode pressurizing the test specimen 6 through the hole in the fixing stand8. In applying pressure, the lower electrode of the pair of electrodes 9 andthe fixing stand 8 are fixed, and the upper electrode is movable so that thelower electrode is in contact with a plane that is an extension of a plane wherethe spacer 7 touches the fixing stand 8. The upper electrode is in contact withthe center of the test galvannealed steel sheet 5. The sheet combination iswelded with the sheet combination inclined 5° to the lengthwise direction sideof the sheet combination with respect to a plane perpendicular to a lineconnecting the central axes of the electrode pair of the resistance weldingmachine (horizontal direction in FIG. 8A). A gap of 60 mm in the lengthwisedirection of the sheet combination and 2.0 mm in the thickness direction of thesheet combination is formed between the lower electrode and the test specimen6 by the spacers. The hold time refers to the time between the end of weldingcurrent and the beginning of release of the electrodes. As illustrated in thelower part of FIG. 8B, the nugget diameter r means the distance between theends of a nugget 10 in the lengthwise direction of the sheet combination.

[0089] Then, the sheet combination with a welded portion is cut along the B15B line indicated in the upper part of FIG. 8B to include the center of the weldedportion including the nugget 10, and the cross section of the welded portion isobserved under an optical microscopy (200x) to evaluate the resistance tocracking in resistance welding at the welded portion using the followingcriteria. If the result is [Encircled circle] or O, the sheet combination is judged to havesatisfactory resistance to cracking in resistance welding at the welded portion.If the result is x, the sheet combination is judged to have poor resistance tocracking in resistance welding at the welded portion.[Encircled circle]: No cracks as long as 0.1 mm or more are observed at a hold time of 0.14seconds.O: Cracks as long as 0.1 mm or more are observed at a hold time of 0.14seconds, but no cracks as long as 0.1 mm or more are observed at a hold timeof 0.16 seconds.x: Cracks as long as 0.1 mm or more are observed at a hold time of 0.16 seconds.

[0090] Further, the resistance to cracking in resistance welding at the weldedportion may be evaluated using the following criteria under milder weldingconditions.[Encircled circle]: No cracks as long as 0.1 mm or more are observed at a hold time of 0.18seconds.O: Cracks as long as 0.1 mm or more are observed at a hold time of 0.18seconds, but no cracks as long as 0.1 mm or more are observed at a hold timeof 0.24 seconds.x: Cracks as long as 0.1 mm or more are observed at a hold time of 0.24 seconds.

[0091] An example of a crack in the test specimen 6 is schematicallyillustrated in the lower part of FIG. 12B, as indicated by reference numeral 11.

[0092] The Fe-based electroplating layer of the Fe-based electroplated steelsheet in this embodiment is the same as in the Embodiment 1 described above,and the description thereof is omitted. The crystal orientations of the Febasedelectroplating layer and the cold-rolled steel sheet are integrated at aratio of more than 50 % at the interface between the Fe-based electroplatinglayer and the cold-rolled steel sheet, as in the Embodiment 1 described above.The details of the ratio at which the crystal orientations of the Fe-basedelectroplating layer and the cold-rolled steel sheet are integrated at theinterface between the Fe-based electroplating layer and the cold-rolled steelsheet are the same as in the Embodiment 1 described above, and the descriptionthereof is omitted.

[0093] Next, a method of producing an Fe-based electroplated steel sheetaccording to Embodiment 2 will be described.A method of producing an Fe-based electroplated steel sheet accordingto one embodiment comprises:subjecting a cold-rolled steel sheet to Fe-based electroplating to obtaina pre-annealing Fe-based electroplated steel sheet with a pre-annealing Febasedelectroplating layer formed on at least one surface thereof with a coatingweight per surface of more than 20.0 g / m2; andthen subjecting the pre-annealing Fe-based electroplated steel sheet toannealing to obtain an Fe-based electroplated steel sheet.As used herein, the cold-rolled steel sheet is a cold-rolled steel sheetwhere a test specimen of the cold-rolled steel sheet that is cut to a size of 50mm x 150 mm with a direction orthogonal to the rolling direction as thelengthwise direction is overlapped with a test galvannealed steel sheet that iscut to the same size having a hot-dip galvanized layer with a coating weightper surface of 50 g / m2 to obtain a sheet combination,next, using a single-phase AC (50 Hz) resistance welding machine ofservomotor pressure type, the sheet combination is inclined 5° to thelengthwise direction side of the sheet combination with respect to a planeperpendicular to a line connecting the central axes of an electrode pair (tipdiameter 6 mm) of the resistance welding machine, the lower electrode of theelectrode pair and the sheet combination are fixed so that a gap of 60 mm inthe lengthwise direction of the sheet combination and 2.0 mm in the thicknessdirection of the sheet combination is provided between the lower electrode andthe test specimen, the upper electrode of the electrode pair is movable, andresistance welding is applied to the sheet combination under the followingconditions: applied pressure: 3.5 kN, hold time: 0.16 seconds, and weldingcurrent and welding time to produce a nugget diameter of 5.9 mm, to obtain asheet combination with a welded portion,the sheet combination with a welded portion is then cut in half alongthe lengthwise direction of the test specimen to include a welded portion, across section of the welded portion is observed under an optical microscopy(magnification 200x), and a crack as long as 0.1 mm or more is observed.

[0094] First, a cold-rolled steel sheet is produced. Regarding the method ofproducing a cold-rolled steel sheet, conventional methods may be followed.In one example, a cold-rolled steel sheet is produced by hot rolling a steel slabto obtain a hot-rolled sheet, then subjecting the hot-rolled sheet to acidcleaning, and then cold rolling the hot-rolled sheet to obtain a cold-rolled steelsheet.

[0095] The cold-rolled steel sheet according to this embodiment is notparticularly limited if it is a steel sheet inferior in resistance to cracking inresistance welding at a welded portion when combined with a galvanized steelsheet and evaluated by the test described above. The chemical compositionof the cold-rolled steel sheet is not particularly limited, either. If it is a coldrolledsteel sheet containing Si in an amount of 0.1 mass% or more in the steel,it is inferior in resistance to cracking in resistance welding at a welded portionwhen evaluated by the test described above.

[0096] The cold-rolled steel sheet may be a cold-rolled steel sheet where thesheet combination with a welded portion is obtained by performing theresistance welding at a hold time of 0.24 seconds, a cross section of the weldedportion is observed under an optical microscopy (magnification 200x), and acrack as long as 0.1 mm or more is observed. In the case of the same coldrolledsteel sheet, the resistance to cracking in resistance welding at a weldedportion generally deteriorates as the hold time decreases. Therefore, if cracksas long as 0.1 mm or more are observed in a cold-rolled steel sheet where thesheet combination with a welded portion is obtained by performing resistancewelding at a hold time of 0.24 seconds and a cross section of a welded portionis observed under an optical microscopy (magnification 200x), cracks as longas 0.1 mm or more can be observed when the cross section of a welded portionis observed under an optical microscopy (magnification 200x) even when theresistance welding is performed at a hold time of 0.16 seconds. If the coldrolledsteel sheet contains Si in an amount of 0.50 mass% or more in the steel,it is inferior in resistance to cracking in resistance welding at a welded portionwhen evaluated by the test described above. However, it has also beenconfirmed that even a cold-rolled steel sheet containing Si in an amount of lessthan 0.50 mass% in the steel may be inferior in resistance to cracking inresistance welding at a welded portion when evaluated by the test describedabove.

[0097] Next, the surface of the cold-rolled steel sheet is subjected to Fe-basedelectroplating to obtain a pre-annealing Fe-based electroplated steel sheet.The details of the Fe-based electroplating treatment have been described above,and the description thereof is omitted.

[0098] Then, the pre-annealing Fe-based electroplated steel sheet is subjectedto an annealing process in which the steel sheet is held in a temperature rangeof 650 °C to 900 °C for 30 seconds to 600 seconds in a reducing atmospherewith a dew point of -30 °C or lower and a hydrogen concentration from 1.0vol.% to 30.0 vol.%, and then cooled to obtain an Fe-based electroplated steelsheet. The details of the annealing process have been described above, andthe description thereof is omitted.

[0099] According to this embodiment, it is also possible to provide anelectrodeposition-coated steel sheet comprising: a chemical conversion layerformed on the Fe-based electroplated steel sheet in this embodiment so as tocontact the Fe-based electroplating layer; and an electrodeposition coatinglayer formed on the chemical conversion layer, as in the Embodiment 1described above. Further, it is possible to provide an Fe-based electroplatedsteel sheet for electrodeposition coating to apply electrodeposition coating.The details of the electrodeposition-coated steel sheet and a method ofproducing the electrodeposition-coated steel sheet are the same as in theEmbodiment 1 described above, and the description thereof is omitted.

[0100] Further, this embodiment also can provide an automotive part, as in theEmbodiment 1 described above. The details of the automotive part have beendescribed above, and the description thereof is omitted.

[0101] The present disclosure will be specifically described based on theexamples below.EXAMPLES

[0102] (Example 1)Cast steel samples were prepared by smelting steel with the chemicalcompositions listed in Tables 1 and 3, and they were subjected to hot rolling,acid cleaning, and cold rolling to obtain cold-rolled steel sheets with athickness of 1.6 mm.

[0103] [Table 1]

[0104] [Table 3]"-" indicates a content at inevitable impurity level.

[0105] Then, each cold-rolled steel sheet was subjected to degreasing withalkali, followed by electrolytic treatment with the steel sheet as the cathodeunder the conditions described below to produce a pre-annealing Fe-basedelectroplated steel sheet having an Fe-based electroplating layer on one surface.The coating weight of the Fe-based electroplating layer was controlled bycurrent passage time. Subsequently, the pre-annealing Fe-based electroplatedsteel sheets were subjected to reduction annealing at 15% H2-N2 and a soakingzone temperature of 800 °C , with the dew point of the atmosphere adjusted aslisted in Tables 2-1, 2-2, and 4, to obtain Fe-based electroplated steel sheets.The reduction annealing was performed for 100 seconds.[Electrolytic Conditions]Bath temperature: 50 °C pH: 2.0Current density: 45 A / dm2Fe-based electroplating bath: containing 1.5 mol / L of Fe2+ ionsElectrode (anode): iridium oxide electrode

[0106] From each Fe-based electroplated steel sheet thus prepared, the coatingweight per surface of the Fe-based electroplating layer, and the ratio at whichthe crystal orientations of the Fe-based electroplating layer and the Si20containing cold-rolled steel sheet are integrated at the interface between theFe-based electroplating layer and the Si-containing cold-rolled steel sheet weredetermined according to the methods described above.

[0107] The resistance to cracking in resistance welding at a welded portionwas also investigated for each Fe-based electroplated steel sheet thus prepared.The following describes the measurement and evaluation methods of theresistance to cracking in resistance welding at a welded portion.

[0108] <Resistance to Cracking in Resistance Welding at Welded PortionWhen Combined with Galvanized Steel Sheet>For each Fe-based electroplated steel sheet, the resistance to crackingin resistance welding at a welded portion was evaluated with the methoddescribed above when combined with a test galvannealed steel sheet (1.6 mmthick) having a tensile strength of 980 MPa and a coating weight per surfaceof 50 g / m2, with a Si content of less than 0.50%, where the resistance tocracking in resistance welding was not an issue at a hold time of 0.18 seconds.The welding time was 0.36 seconds and the hold times were 0.18 seconds and0.24 seconds. The nugget diameter was measured by changing the weldingcurrent for each Example No., and the evaluation was performed at the weldingcurrent where the nugget diameter was 5.9 mm. When no cracks were foundin the combined test galvannealed steel sheet, it was taken as example data.This is because if a crack occurs in the combined sheet, the stress on the Febasedelectroplated steel sheet to be evaluated is dispersed, making itimpossible to perform appropriate evaluation.

[0109] The results of the above tests are listed in Tables 2-1, 2-2, and 4. Theresults demonstrate that the Fe-based electroplated steel sheets in our examples,in which Fe-based electroplating layers were formed under the conditionsconforming to the present disclosure before continuous annealing, exhibitedexcellent resistance to cracking in resistance welding at a welded portion. InReference Examples 1 and 2, no particular problems were observed in theresistance to cracking in resistance welding at a welded portion since the Sicontent was less than 0.5%. In each of our examples where the coatingweight of the Fe-based electroplating layer was 25.0 g / m2 or more, cracks aslong as 0.1 mm or more were not observed even at a hold time of 0.18 seconds,and the resistance to cracking in resistance welding at a welded portion wasparticularly good. In Tables 2-1 and 2-2, the coating weight of the Fe-basedelectroplating layer is indicated as "-" for the examples where no Fe-basedelectroplating layer was formed. In Reference Examples No. 17, 30, and 46where annealing processes at high dew point were performed, the ratio at whichthe crystal orientations of the Fe-based electroplating layer and the Sicontainingcold-rolled steel sheet were integrated at the interface between theFe-based electroplating layer and the Si-containing cold-rolled steel sheet waslow because of the annealing at high dew point, and the resistance to crackingin resistance welding at a welded portion was good. In these referenceexamples, the pre-annealing Fe-based electroplated steel sheets were heated toa soaking zone temperature of 800 °C at an average heating rate of at least 10°C / s in the temperature range of 400 °C to 650 °C , and then subjected toreduction annealing.

[0110] [Table 2-1]Table 2-1Underlined if outside the appropriate range of the present disclosure.

[0111] [Table 2-2]Underlined if outside the appropriate range of the present disclosure.RemarksTable 2-2

[0112] [Table 4]

[0113] (Example 2)Cast steel samples were prepared by smelting steel with the chemicalcompositions listed in Table 5, and they were subjected to hot rolling, acidcleaning, and cold rolling to obtain cold-rolled steel sheets with a thickness of1.6 mm.

[0114] [Table 5]"-" indicates a content at inevitable impurity level.

[0115] Then, each cold-rolled steel sheet was subjected to degreasing withalkali, followed by electrolytic treatment with the steel sheet as the cathodeunder the conditions described below to produce a pre-annealing Fe-basedelectroplated steel sheet having an Fe-based electroplating layer on one surface.The coating weight of the Fe-based electroplating layer was controlled bycurrent passage time. Subsequently, the pre-annealing Fe-based electroplatedsteel sheets were subjected to reduction annealing at 15% H2-N2 and a soakingzone temperature of 800 °C , with the dew point of the atmosphere adjusted aslisted in Table 6, to obtain Fe-based electroplated steel sheets. The reductionannealing was performed for 100 seconds.[Electrolytic Conditions]Bath temperature: 50 °C pH: 2.0Current density: 45 A / dm2Fe-based electroplating bath: containing 1.5 mol / L of Fe2+ ionsElectrode (anode): iridium oxide electrode

[0116] From each Fe-based electroplated steel sheet thus prepared, the coatingweight per surface of the Fe-based electroplating layer, and the ratio at whichthe crystal orientations of the Fe-based electroplating layer and the Si20containing cold-rolled steel sheet are integrated at the interface between theFe-based electroplating layer and the Si-containing cold-rolled steel sheet weredetermined according to the methods described above.

[0117] The resistance to cracking in resistance welding at a welded portionwas also investigated for each Fe-based electroplated steel sheet thus prepared.The following describes the measurement and evaluation methods of theresistance to cracking in resistance welding at a welded portion.

[0118] <Resistance to Cracking in Resistance Welding at Welded PortionWhen Combined with Galvanized Steel Sheet>For each Fe-based electroplated steel sheet, the resistance to crackingin resistance welding at a welded portion was evaluated with the methoddescribed above when combined with a test galvannealed steel sheet (1.6 mmthick) having a tensile strength of 590 MPa and a coating weight per surfaceof 50 g / m2, with a Si content of less than 0.1%, where the resistance tocracking in resistance welding was not an issue at a hold time of 0.14 seconds.The welding time was 0.36 seconds and the hold times were 0.14 seconds and0.16 seconds. The nugget diameter was measured by changing the weldingcurrent for each Example No., and the evaluation was performed at the weldingcurrent where the nugget diameter was 5.9 mm. When no cracks were foundin the combined test galvannealed steel sheet, it was taken as example data.This is because if a crack occurs in the combined sheet, the stress on the Febasedelectroplated steel sheet to be evaluated is dispersed, making itimpossible to perform appropriate evaluation.

[0119] The results of the above tests are listed in Table 6. The resultsdemonstrate that the Fe-based electroplated steel sheets in our examples, inwhich Fe-based electroplating layers were formed under the conditionsconforming to the present disclosure before continuous annealing, exhibitedexcellent resistance to cracking in resistance welding at a welded portion. Ineach of our examples where the coating weight of the Fe-based electroplatinglayer was 25.0 g / m2 or more, cracks as long as 0.1 mm or more were notobserved even at a hold time of 0.14 seconds, and the resistance to cracking inresistance welding at a welded portion was particularly good. In Table 6, thecoating weight of the Fe-based electroplating layer is indicated as "-" for theexamples where no Fe-based electroplating layer was formed.

[0120] [Table 6]Table 6INDUSTRIAL APPLICABILITY

[0121] The Fe-based electroplated steel sheet produced with the methoddisclosed herein not only has excellent resistance to cracking in resistancewelding, especially internal cracking, at a welded portion when combined witha galvanized steel sheet, but also has high strength and excellent formability,making it suitable not only as the raw material used in automotive parts butalso as the raw material for applications requiring similar properties in fieldssuch as home appliances and construction materials.REFERENCE SIGNS LIST

[0122] 1 Fe-based electroplated steel sheet2 Si-containing cold-rolled steel sheet3 Fe-based electroplating layer5 Test galvannealed steel sheet6 Test specimen7 Spacer8 Fixing stand9 Electrode10 Nugget11 Crack

Claims

1. An Fe-based electroplated steel sheet comprising: a Si-containing cold-rolled steel sheet containing Si in an amount of 0.1 mass% or more and 3.0 mass% or less; and an Fe-based electroplating layer formed on at least one surface of the Si-containing cold-rolled steel sheet with a coating weight per surface of more than 20.0 g / m2, wherein crystal orientations of the Fe-based electroplating layer and the Si10 containing cold-rolled steel sheet are integrated at a ratio of more than 50 % at an interface between the Fe-based electroplating layer and the Si-containing cold-rolled steel sheet.

2. The Fe-based electroplated steel sheet according to claim 1, wherein the Si-containing cold-rolled steel sheet contains Si in an amount of 0.50 mass% or more and 3.0 mass% or less.

3. The Fe-based electroplated steel sheet according to claim 1 or 2, wherein the Fe-based electroplating layer is formed with a coating weight per surface of 25.0 g / m2 or more.

4. The Fe-based electroplated steel sheet according to any one of claims 1 to 3, wherein the Si-containing cold-rolled steel sheet has a chemical composition containing, in addition to Si, in mass%, C: 0.8 % or less, Mn: 1.0 % or more and 12.0 % or less, P: 0.1 % or less, S: 0.03 % or less, N: 0.010 % or less, and Al: 1.0 % or less, with the balance being Fe and inevitable impurities.

5. The Fe-based electroplated steel sheet according to claim 4, wherein the chemical composition further contains at least one selected from the group consisting of B: 0.005 % or less, Ti: 0.2 % or less, Cr: 1.0 % or less, Cu: 1.0 % or less, Ni: 1.0 % or less, Mo: 1.0 % or less, Nb: 0.20 % or less, V: 0.5 % or less, Sb: 0.200 % or less, Ta: 0.1 % or less, W: 0.5 % or less, Zr: 0.1 % or less, Sn: 0.20 % or less, Ca: 0.005 % or less, Mg: 0.005 % or less, and REM: 0.005 % or less.

6. The Fe-based electroplated steel sheet according to any one of claims 1 to 5, wherein the Fe-based electroplating layer has a chemical composition containing at least one element selected from the group consisting of B, C, P, N, O, Ni, Mn, Mo, Zn, W, Pb, Sn, Cr, V, and Co, in a total amount of 10 mass% or less, with the balance being Fe and inevitable impurities.

7. An Fe-based electroplated steel sheet comprising: a cold-rolled steel sheet; and an Fe-based electroplating layer formed on at least one surface of the cold-rolled steel sheet with a coating weight per surface of more than 20.0 g / m2, wherein crystal orientations of the Fe-based electroplating layer and the cold rolled steel sheet are integrated at a ratio of more than 50 % at an interface between the Fe-based electroplating layer and the cold-rolled steel sheet, and the cold-rolled steel sheet is a cold-rolled steel sheet where a test specimen of the cold-rolled steel sheet that is cut to a size of 50 mm x 150 mm with a direction orthogonal to a rolling direction as a lengthwise direction is overlapped with a test galvannealed steel sheet that is cut to the same size having a hot-dip galvanized layer with a coating weight per surface of 50 g / m2 to obtain a sheet combination, next, using a 50-Hz single-phase AC resistance welding machine of servomotor pressure type, the sheet combination is inclined 5° to a lengthwise direction side of the sheet combination with respect to a plane perpendicular to a line connecting central axes of an electrode pair with a tip diameter of 6 mm of the resistance welding machine, a lower electrode of the electrode pair and the sheet combination are fixed so that a gap of 60 mm in a lengthwise direction of the sheet combination and 2.0 mm in a thickness direction of the sheet combination is provided between the lower electrode and the test specimen, an upper electrode of the electrode pair is movable, and resistance welding is applied to the sheet combination under a set of conditions: applied pressure: 3.5 kN, hold time: 0.16 seconds, and welding current and welding time to produce a nugget diameter of 5.9 mm, to obtain a sheet combination with a welded portion, and the sheet combination with a welded portion is then cut in half along a lengthwise direction of the test specimen to include a welded portion, a cross section of the welded portion is observed under an optical microscopy at a magnification of 200x, and a crack as long as 0.1 mm or more is observed.

8. The Fe-based electroplated steel sheet according to claim 7, wherein the cold-rolled steel sheet is a cold-rolled steel sheet where the sheet combination with a welded portion is obtained by performing the resistance welding with the hold time being 0.24 seconds, a cross section of the welded portion is observed under the optical microscopy at a magnification of 200x, and a crack as long as 0.1 mm or more is observed.

9. An electrodeposition-coated steel sheet comprising: a chemical conversion layer formed on the Fe-based electroplated steel sheet as recited in any one of claims 1 to 8 so as to contact the Fe-based electroplating layer; and an electrodeposition coating layer formed on the chemical conversion layer.

10. An automotive part at least partially made from the electrodeposition-coated steel sheet as recited in claim 9.

11. A method of producing an electrodeposition-coated steel sheet, the method comprising: subjecting the Fe-based electroplated steel sheet as recited in any one of claims 1 to 8 to chemical conversion treatment, without additional coating or plating treatment, to obtain a chemical-conversion-treated steel sheet with a chemical conversion layer formed in contact with the Fe-based electroplating layer; and subjecting the chemical-conversion-treated steel sheet to electrodeposition coating treatment to obtain an electrodeposition-coated steel sheet with an electrodeposition coating layer formed on the chemical conversion layer.

12. A method of producing an Fe-based electroplated steel sheet, the method comprising: subjecting a cold-rolled steel sheet containing Si in an amount of 0.1 mass% or more and 3.0 mass% or less to Fe-based electroplating to obtain a pre-annealing Fe-based electroplated steel sheet with a pre-annealing Fe-based electroplating layer formed on at least one surface thereof with a coating weight per surface of more than 20.0 g / m2; and then subjecting the pre-annealing Fe-based electroplated steel sheet to annealing in an atmosphere with a dew point of -30 °C or lower to obtain an Fe-based electroplated steel sheet.

13. The method of producing an Fe-based electroplated steel sheet according to claim 12, wherein the cold-rolled steel sheet contains Si in an amount of 0.5 mass% or more and 3.0 mass% or less.

14. A method of producing an Fe-based electroplated steel sheet, the method comprising: subjecting a cold-rolled steel sheet to Fe-based electroplating to obtain a pre-annealing Fe-based electroplated steel sheet with a pre-annealing Fe based electroplating layer formed on at least one surface thereof with a coating weight per surface of more than 20.0 g / m2; and then subjecting the pre-annealing Fe-based electroplated steel sheet to annealing to obtain an Fe-based electroplated steel sheet, wherein the cold-rolled steel sheet is a cold-rolled steel sheet where a test specimen of the cold-rolled steel sheet that is cut to a size of 50 mm x 150 mm with a direction orthogonal to a rolling direction as a lengthwise direction is overlapped with a test galvannealed steel sheet that is cut to the same size having a hot-dip galvanized layer with a coating weight per surface of 50 g / m2 to obtain a sheet combination, next, using a 50-Hz single-phase AC resistance welding machine of servomotor pressure type, the sheet combination is inclined 5° to a lengthwise direction side of the sheet combination with respect to a plane perpendicular to a line connecting central axes of an electrode pair with a tip diameter of 6 mm of the resistance welding machine, a lower electrode of the electrode pair and the sheet combination are fixed so that a gap of 60 mm in a lengthwise direction of the sheet combination and 2.0 mm in a thickness direction of the sheet combination is provided between the lower electrode and the test specimen, an upper electrode of the electrode pair is movable, and resistance welding is applied to the sheet combination under a set of conditions: applied pressure: 3.5 kN, hold time: 0.16 seconds, and welding current and welding time to produce a nugget diameter of 5.9 mm, to obtain a sheet combination with a welded portion, and the sheet combination with a welded portion is then cut in half along a lengthwise direction of the test specimen to include a welded portion, a cross section of the welded portion is observed under an optical microscopy at a magnification of 200x, and a crack as long as 0.1 mm or more is observed.

15. The method of producing an Fe-based electroplated steel sheet according to claim 14, wherein the cold-rolled steel sheet is a cold-rolled steel sheet where the sheet combination with a welded portion is obtained by performing the resistance welding with the hold time being 0.24 seconds, a cross section of the welded portion is observed under an optical microscopy at a magnification of 200x, and a crack as long as 0.1 mm or more is observed.

16. The method of producing an Fe-based electroplated steel sheet according to any one of claims 12 to 15, wherein the Fe-based electroplating is performed in an Fe-based electroplating bath containing at least one element selected from the group consisting of B, C, P, N, O, Ni, Mn, Mo, Zn, W, Pb, Sn, Cr, V, and Co, so that the at least one element is contained in the preannealing Fe-based electroplating layer in a total amount of 10 mass% or less.