Ceramic article manufacturing method and ceramic article
Patent Information
- Application Number
- JP2020174681
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-10-23
- Filing Date
- 2020-10-16
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2040-10-16
AI Technical Summary
Silica-based ceramic materials used in additive manufacturing face challenges with low laser light absorption, leading to poor mechanical strength and high porosity due to rapid cooling and amorphous phase formation, which is unsuitable for applications requiring high accuracy and strength, such as casting cores.
A method involving the use of silicon dioxide powder with an absorber like terbium oxide or praseodymium oxide, followed by laser irradiation and heat treatment at specific temperatures to convert amorphous silica to cristobalite, combined with a metal component-containing liquid to repair cracks and enhance mechanical strength.
The method produces silica-based ceramic articles with high molding precision and excellent mechanical strength, suitable for casting cores, by forming a phase-separated structure with cristobalite and improved crack repair, maintaining shape accuracy and thermal stability.
Abstract
Description
[Technology Field]
[0001] The present invention relates to a method for manufacturing silica-based ceramic articles using additive manufacturing technology, and to ceramic articles produced by such manufacturing method. [Background technology]
[0002] Additive manufacturing technology, which involves adding material based on three-dimensional data of a model to be manufactured to obtain a desired object, is becoming increasingly popular for applications such as creating prototypes in a short time or manufacturing small quantities of items. In the manufacture of metal articles, direct fabrication is widely used, in which a laser beam is irradiated onto metal powder based on three-dimensional data of the model, causing the powder to solidify and form the object. This method makes it possible to obtain dense and diverse articles by effectively melting and solidifying the metal powder.
[0003] In recent years, efforts have been made to establish additive manufacturing technology using ceramic powder as a raw material. However, unlike metals, common ceramics such as aluminum oxide and zirconium oxide have low absorption capacity for laser light. Therefore, a lot of energy is required to melt the ceramic powder, but the laser light diffuses, resulting in uneven melting and making it difficult to obtain the necessary molding precision.
[0004] Therefore, Patent Document 1 discloses a technique for producing a molded object with high precision by suppressing light diffusion by adding an absorber that absorbs laser light to the raw material powder. [Prior art documents] [Patent Documents]
[0005] [Patent Document 1] Japanese Patent Publication No. 2019-19051 [Overview of the project] [Problems that the invention aims to solve]
[0006] Among ceramics, silica-based materials are widely used as materials for casting cores. A casting core is a mold that is fitted into the cavity of a mold when creating a casting with an internal cavity, and is ultimately removed from the cast article. Cores are required to not undergo chemical reactions with the molten metal being poured into them, to have excellent heat resistance, and to be easily removed at the end of the casting process. Therefore, silica-based structures that are soluble in alkaline solutions are suitable as casting cores. Here, "silica-based" means that silicon dioxide is the main component. In this invention, the main component refers to the component (element or compound) that is present in the largest amount by mass ratio.
[0007] If casting cores can be manufactured using additive manufacturing technology, it will be possible to cast complex shapes at low cost. Since the dimensional and surface accuracy of the cast article is affected by the dimensions and surface condition of the core, silica-based molded objects used as cores require high molding accuracy and high mechanical strength to withstand the casting process.
[0008] Patent Document 1 describes silica-based materials as molding powders used in direct fabrication methods. However, because silica-based materials have high viscosity in the liquid phase, they tend to become spherical when molten by laser irradiation, and the solidified portion tends to be porous. Furthermore, the molten portion cools rapidly after the laser light passes through, so most of the solidified portion becomes amorphous. Even when liquid-phase sintering occurs due to laser irradiation, the liquid phase portion cools rapidly after the laser light passes through, becoming amorphous. For these reasons, although silica-based fabricated objects fabricated by the method disclosed in Patent Document 1 have excellent fabrication accuracy, they have a large amorphous portion, which may result in insufficient mechanical strength depending on the application, such as for casting cores.
[0009] This invention was made to solve the aforementioned problems and provides a technology for manufacturing silica-based ceramic articles with high molding accuracy and excellent mechanical strength using a direct molding method. [Means for solving the problem]
[0010] The manufacturing method of the ceramic article according to the present invention is as follows. (i) A step of arranging a powder mainly composed of silicon dioxide and containing an absorber that absorbs light of a predetermined wavelength; (ii) A step of sintering, melting, and solidifying the powder by irradiating the powder with a laser containing light of the predetermined wavelength; (iii) A step of heating the shaped object formed by repeating the steps (i) and (ii) at a temperature of 1470 °C or higher and lower than 1730 °C. It is characterized by having the above steps.
[0011] Further, the ceramic article according to the present invention is a ceramic article containing Tb or Pr and mainly composed of silicon dioxide, wherein the silicon content is more than 80% by mass, and 70% or more of the silicon dioxide is cristobalite.
Effect of the Invention
[0012] According to the present invention, it becomes possible to manufacture a silica-based ceramic structure with high shaping accuracy and excellent mechanical strength using a direct shaping method.
Brief Description of the Drawings
[0013]
FIG. 1
FIG. 2
FIG. 3
FIG. 4
FIG. 5
FIG. 6
[0014] The method for manufacturing a ceramic article according to the present invention includes the following steps. (i) A step of arranging a powder mainly composed of silicon dioxide, which contains an absorber that absorbs light of a predetermined wavelength. (ii) A step of sintering, melting, and solidifying the powder by irradiating it with a laser containing light of the predetermined wavelength. (iii) A step of heating the molded object formed by repeating the steps in (i) and (ii) above at a temperature of 1470°C or higher and less than 1730°C.
[0015] The following will describe embodiments of the present invention with reference to the drawings, but the present invention is not limited to the following specific examples or drawings, and can be modified within the scope of the technical concept of the present invention.
[0016] The present invention is preferably used in direct fabrication methods, specifically powder bed fusion and directed energy layering (so-called cladding), which deposits the fabrication material by melting it. By applying the present invention, it is possible to achieve good fabrication accuracy while significantly improving the mechanical strength of the resulting silica-based fabricated object.
[0017] Silica refers to silicon dioxide. Silica exists in polymorphic forms, regardless of its state (amorphous, crystalline, or crystalline structure). "Polymorphism" refers to the ability to take on multiple different crystalline forms despite having the same chemical composition.
[0018] The basic fabrication process using powder bed fusion is explained using Figures 1(a) to 1(h).
[0019] First, powder 101 is placed on a base 130 installed on a stage 151, and a powder layer 102 of a predetermined thickness is formed using a roller 152 (Figures 1(a) and (b)). A laser beam emitted from a laser beam source 180 is irradiated onto the surface of the powder layer 102 while scanning with a scanner unit 181 based on the fabrication data (slice data) generated from the three-dimensional shape data of a model having the desired shape. In the laser beam irradiation area 182, the powder is sintered or melted and solidified to form a solidified area 100 (Figure 1(c)). Next, the stage 151 is lowered to form a new powder layer 102 on top of the solidified area 100 (Figure 1(d)), and the laser beam is irradiated based on the fabrication data. These processes are repeated to form a fabricated object 110 of the desired shape (Figures 1(e) and (f)). Finally, the unsolidified powder 103 is removed, and if necessary, unwanted parts of the molded object are removed or the molded object is separated from the base to obtain the molded object (Figures 1(g) and (h)).
[0020] Next, the cladding method will be explained using Figures 2(a) to (c). Powder is ejected from multiple powder supply holes 202 in the cladding nozzle 201, and a laser beam 203 is irradiated onto the area where the powder is focused, thereby additionally forming a solidified portion 100 at the desired location based on the molding data (Figure 2(a)). By performing this process continuously, a molded object 110 of the desired shape is obtained (Figures 2(b) and (c)). Finally, if necessary, unnecessary parts of the molded object are removed and the molded object is separated from the base.
[0021] In direct fusion methods such as powder bed direct fusion and cladding, the silicon dioxide-based powder, melted by laser beam irradiation, is rapidly cooled and solidified from the surroundings, forming a solidified material mainly composed of amorphous silica. Because the amorphous silica-based material formed through this melting and solidification process has low density, it cannot achieve high mechanical strength.
[0022] Cristobalite is one of the crystalline forms that silica can take. Because cristobalite is a crystalline form that is stable at high temperatures, it can maintain a stable state even when exposed to the high temperatures of casting. Furthermore, because it has a higher density than amorphous silica, it also has superior mechanical strength at high temperatures. In addition, cristobalite has a higher solubility in alkaline solutions compared to other crystalline forms such as quartz, making it a suitable crystalline form for constituting casting cores.
[0023] Therefore, in this invention, the fabricated object produced by repeating steps (i) and (ii) is heat-treated at a temperature of 1470°C to less than 1730°C. Such heat treatment makes it possible to produce a fabricated object that is stable at high temperatures and has excellent mechanical strength. This is thought to be because the fabricated object, which is mainly amorphous silica immediately after fabrication, changes to cristobalite in which more than 70% by mass of the silicon contained in the fabricated object is combined with oxygen after the heat treatment.
[0024] Furthermore, depending on the conditions under which steps (i) and (ii) are performed, the area irradiated by the laser beam may be exposed to the melting and solidification temperatures in a short time, which can lead to the formation of numerous cracks in the resulting object due to thermal stress. These cracks are distributed throughout the entire object, i.e., on the surface and inside. When the cross-section of the object is examined with a scanning electron microscope, most of the cracks are found to be several nanometers to several micrometers wide, and their lengths vary from several micrometers to several millimeters. If many such cracks are formed in the object, its mechanical strength will decrease.
[0025] In the case of molded objects where a decrease in mechanical strength due to cracks is a concern, it is preferable to allow the cracks in the molded object to absorb a metal-containing liquid before the heat treatment in step (iii). Heating transforms the amorphous silica contained in the molded object into cristobalite, which has higher mechanical strength, and at the same time, the metal-containing liquid selectively melts the area near the cracks, repairing the cracks and reducing the number of cracks in the molded object. As a result, the mechanical strength of the molded object can be significantly improved.
[0026] The metal component-containing liquid to be absorbed into the cracks is preferably one that can supply metal oxides to the cracks. For example, it is preferable that the metal component-containing liquid contains metal oxides, or contains components that generate metal oxides through heat treatment performed after absorption of the metal component-containing liquid. The metal component-containing liquid is preferably a composition that can supply metal oxides on its own, but it may also be a composition that generates metal oxides through compounding, solid solution, or diffusion with components contained in the molded object.
[0027] The metal component-containing liquid can be a solution, sol, or particle dispersion containing a metal element. The metal component-containing liquid can be any form, as long as its viscosity and concentration are adjusted so that the metal element is distributed throughout the entire object when the liquid is absorbed by the object in step (iii). The metal element is contained in the metal component-containing liquid in the form of, for example, a metal salt, a metal alkoxide, or particles containing the metal element. Examples of particles containing the metal element include metals, oxides, nitrides, carbides, borides, and hydroxides. The particle dispersion contains particles along with a solvent, dispersant, and stabilizer. Examples of solvents include water, organic solvents, and oils, while examples of dispersants include pH adjusters, silane coupling agents, and surfactants. Examples of stabilizers include pH adjusters, surfactants, chelating agents, and self-decomposition inhibitors, but are not limited to these.
[0028] When using a particle dispersion liquid, in which particles containing metal elements are dispersed in a solvent, as the metal component-containing liquid, it is preferable that the particles have a diameter sufficiently smaller than the width of the cracks in the fabricated object, in order to penetrate the entire crack. The strength of the fabricated object is thought to be greatly affected by cracks with a width of 1 μm or more. In order for particles to penetrate cracks with a width of 1 μm or more, the average particle diameter of the particles is preferably 300 nm or less, more preferably 50 nm or less, and even more preferably 30 nm or less. The concentration of metal elements in the metal component-containing liquid with dispersed particles can be easily adjusted by methods such as adjusting the particle composition and particle content, and a liquid containing high concentrations of metal elements can be produced. When a liquid containing high concentrations of metal elements is used as the metal component-containing liquid, it is possible to shorten the time required for the process of absorbing the metal component-containing liquid into the fabricated object and heat-treating it. In other words, cracks can be repaired with fewer absorption and heat-treating steps.
[0029] On the other hand, using solutions or sols containing metallic elements allows the metallic elements to penetrate even the finest cracks, enabling more precise crack repair than with particle dispersions. However, because it is difficult to produce solutions with high concentrations of metallic elements, the time required to repair cracks tends to be longer compared to when using particle dispersions.
[0030] The metal component-containing liquid is preferably one that, upon heating, produces a phase capable of forming a eutectic with the phases constituting the fabricated object. If the fabricated object contains multiple phases, it is sufficient that a phase capable of forming a eutectic with any of the phases contained in the fabricated object is formed. If the phase formed from the metal component-containing liquid by the heat treatment is a metal oxide, and this metal oxide phase and the phases contained in the fabricated object are in a relationship that allows for eutectic formation, then the area near the crack into which the metal component has penetrated melts at a temperature lower than the melting point of other parts of the fabricated object. Then, over time, the metal element or metal oxide diffuses into the interior of the fabricated object, and as the temperature decreases after heating is complete, crystals recrystallize within the fabricated object with a composition containing the metal element. As a result, while the shape of the fabricated object is maintained, only the area near the crack softens, achieving the effect of reducing or eliminating the crack.
[0031] The fact that component A and another component B can form a eutectic is sometimes expressed as "components A and B are in a eutectic relationship." A eutectic is a mixture of two or more crystals that crystallize simultaneously from a liquid phase containing two or more components. "Components A and B can form a eutectic" is synonymous with "components A and B have a eutectic state." When a eutectic state exists, a eutectic point (also called a eutectic point) exists. The eutectic point is the temperature at which eutectic formation occurs, and in a phase diagram where temperature is on the vertical axis and the component composition ratio is on the horizontal axis, it corresponds to the minimum value of the liquid phase curve. The composition corresponding to the eutectic point is called the eutectic composition (or eutectic composition). Therefore, the eutectic point of components A and B is lower than the melting points of components A and B individually.
[0032] Let component A be the compound component contained in the molded object that absorbs the metal component-containing liquid, and component B be the oxide of the metal element contained in the metal component-containing liquid. Assume that component A and component B are in a eutectic relationship. In this case, the localized melting that occurs in the cracks is presumed to be due to the following phenomenon.
[0033] When a molded object absorbs a liquid containing metal components, the surface of the object that forms cracks will contain metal oxides or metal elements that were present in the liquid. When heated in this state, the metal elements will change into metal oxides. Then, regardless of whether the liquid containing metal components is metal oxides or metal elements, component B will be present on the surface of the molded object that forms cracks. When further heat is applied in this state, it is thought that in the vicinity of the region on the surface of the molded object where component B is present, an amount of component A that has a eutectic composition or a composition close to the eutectic composition of component B will melt at a temperature lower than the melting point of the molded object, recrystallize, and contribute to crack repair. In other words, since an amount of component A corresponding to the amount of component B present in the crack melts, only the region near the crack softens, and it is thought that the effect of reducing or eliminating cracks while maintaining the shape of the molded object can be obtained.
[0034] The amount of Component B on the surface of the shaped object that constitutes the crack can be controlled by adjusting the number of times the metal component-containing liquid is absorbed into the crack and the concentration of the metal element contained in the metal component-containing liquid. In the vicinity of the region where Component B is present, Component A with an amount that results in a eutectic composition or a composition ratio close to the eutectic composition melts at a temperature lower than the melting point of the shaped object together with the amount of Component B. The greater the amount of Component B, the more possible it is to repair the crack over a wide range.
[0035] In order to melt the vicinity of the crack, the temperature of the heat treatment performed after absorbing the metal component-containing liquid into the crack of the shaped object is also important. Fig. 3 shows a phase diagram in the case where Component A, which is a compound contained in the shaped object, and Component B (metal oxide) formed from the metal component-containing liquid can form a eutectic. The horizontal axis represents the composition ratio of Component A and Component B, and the vertical axis represents the state at each composition.
[0036] Let the melting point of Component A be T m and the melting point of Component B be T i and the eutectic temperature of Component A and Component B be T E . Then, each temperature satisfies the relationship of T E < T m , T E < T i . In this case, it is preferable to set the maximum temperature T S that the shaped object reaches by the heat treatment performed after absorbing the metal component-containing liquid such that T E ≤ T S < T m . More preferably, T E ≤ T S < T m -(T m - T E ) / 2. Thereby, it is possible to selectively melt the vicinity of the crack at a temperature lower than the melting point T m of the shaped object to reduce or eliminate the crack, and it becomes easier to maintain the shape of the shaped object.
[0037] The technical concept of this invention is to improve the mechanical strength by generating cristobalite in the molded object. Therefore, the maximum temperature T when heating to repair cracks S The temperature range required for cristobalite formation in the fabricated object is between 1470°C and 1730°C. Therefore, it is crucial to appropriately select the combination of component A in the fabricated object and the metal component-containing liquid.
[0038] Depending on the composition of the metal component-containing liquid used, repeatedly applying the treatment of heating after absorbing the metal component-containing liquid can further reduce or eliminate cracks. The melting points of components A and B are T m <T i By selecting a combination that satisfies the relationship, a high effect can be obtained with a relatively small number of attempts. This is as shown in Figure 3, T m <T i In this case, because a high proportion of component A leads to a eutectic formation between component A and component B, the area near the crack can be melted at the eutectic temperature even with a low proportion of component B in the metal-containing liquid. m <T i It is not a mandatory requirement.
[0039] Considering the above, silicon dioxide (SiO2; melting point T m For molded objects whose main component is aluminum (melting point T = 1730°C), a liquid containing aluminum (aluminum-containing liquid) is preferable as the metal-containing liquid. Most of the aluminum elements contained in the aluminum-containing liquid are converted to alumina (Al2O3; melting point T = 1730°C) upon heating. i The temperature is 2070°C. And the eutectic temperature T of SiO2 and Al2O3 is... E The temperature is 1595°C. Since SiO2 corresponds to component A and Al2O3 corresponds to component B, T m <T i The following relationship is satisfied. Then, the temperature T of the heat treatment applied after the silicon dioxide-based molded object absorbs the aluminum-containing liquid is SThis can be set within a range of 1595°C to less than 1730°C, which allows for the generation of cristobalite in the fabricated object. S It is more preferable to set the temperature within a range of 1595°C or higher and 1663°C or lower.
[0040] In the case of molded objects whose main component is silicon dioxide, by allowing the cracks to absorb an aluminum-containing liquid, cracks can be reduced or eliminated even when heat-treated at a temperature more than 100°C lower than the melting point of SiO2. Thus, by heat-treating the molded object at a temperature sufficiently lower than the melting point of SiO2, which is the main component of the molded object, it is possible to obtain a molded object with improved mechanical strength while suppressing changes in the shape of the molded object.
[0041] Even when using a liquid containing zirconium (zirconium component-containing liquid) as a metal component-containing liquid, if component A is SiO2 (melting point T mi =1730℃), component B is ZrO2 (melting point T i =2715℃) and T m <T i It satisfies the relationship.
[0042] As explained above, by allowing a metal component that forms a eutectic with silica to be absorbed into cracks in an amorphous silica-based molded object produced by direct molding, and then heat-treating it at an appropriate temperature, silica-based ceramic articles with excellent mechanical strength can be obtained.
[0043] Furthermore, even if the powder itself contains metal elements used for crack repair, it will not reduce the cracks in the fabricated object. If the powder used for fabrication contains more than a certain amount of metal elements used for crack repair, the entire fabricated object will contain these metal elements, making it impossible to locally lower the melting point near the cracks. This can cause the entire fabricated object to melt upon heating, potentially leading to deformation. In other words, to repair cracks without reducing the fabrication accuracy of the object, it is important to apply heat treatment to the fabricated object while locally increasing the concentration of metal elements near the cracks.
[0044] In order to allow the metal component-containing liquid to be absorbed into cracks after molding and to locally melt only the area near the cracks, it is preferable that the powder does not contain 3.0% by mass or more of the oxides of the metal elements contained in the metal component-containing liquid. That is, if the molding powder contains metal elements contained in the metal component-containing liquid, the content is preferably less than 3.0% by mass of the total powder, and more preferably less than 2.0% by mass. By using such a powder in combination with the metal component-containing liquid, it is possible to realize articles with high molding accuracy and improved mechanical strength.
[0045] Next, the three steps included in the method for manufacturing ceramic articles according to the present invention will be described in detail.
[0046] <Process (i)> The device includes an absorber that absorbs light of wavelengths contained in the irradiating laser, and a powder mainly composed of silicon dioxide is placed on a base. The absorber can be selected according to the type of laser used, but terbium oxide or praseodymium oxide is particularly preferred.
[0047] Silicon dioxide (silica) is represented by the chemical formula SiO2. The bonding state of the SiO2 atoms contained in the powder is not particularly limited; it may be amorphous, crystalline (such as cristobalite or quartz), or a mixture thereof. Among these, powder mainly composed of cristobalite, which has high thermal conductivity, is particularly preferred because the powder melts easily upon laser irradiation. The SiO2 particles constituting the main component SiO2 powder are preferably close to a spherical shape to obtain high fluidity, as the powder is densely arranged in step (i), and preferably have an average particle diameter of 5 μm to 200 μm. A more preferred average particle diameter is 10 μm to 150 μm. In this invention, the average particle diameter refers not to that of individual particles, but to the median diameter of a group of particles having the same composition, i.e., the particle diameter (D) at which the cumulative frequency reaches 50%. 50) . Let it be assumed. The method for measuring the average particle size is not particularly limited, but it can be calculated as the equivalent circle diameter of the projection image from a micrograph of the powder, or it can be determined using dynamic light scattering.
[0048] The powder, whose main component is silicon dioxide, contains an absorber as a secondary component. Here, an absorber refers to a component (element or compound) that exhibits higher absorption than silicon dioxide for light of wavelengths contained in the laser used for molding. The absorber's absorption rate is preferably 10% or more, more preferably 40% or more, and even more preferably 60% or more, for light of wavelengths contained in the laser beam used. The absorption rate of the absorber alone can be measured using a general spectrometer. Specifically, an integrating sphere is used to irradiate a sample dish filled with the absorber alone with a assumed wavelength (near the laser wavelength used in manufacturing) and measure the absorption rate. Then, using the case without a sample as reference data, the absorption rate can be calculated from the ratio.
[0049] Such absorbers efficiently absorb the laser light used during manufacturing, and by becoming hot themselves, the temperature rises to other compositions within a region corresponding to the focal size of the laser beam. This enables effective localized heating, clarifying the interface between the process area (the area irradiated with laser light) and the non-process area (the area not irradiated with laser light), and improving the accuracy of the fabrication.
[0050] The absorber is preferably one in which at least a portion changes into another composition with relatively lower absorption upon laser irradiation. For example, a composition in which the valence state of the metal element changes due to the release of oxygen accompanying the increase in temperature, and it changes into another metal oxide with relatively lower absorption to laser light. Alternatively, a composition may change into a different composition from the powder state through decomposition such as bonding with other compositions contained in the gas or powder in the atmosphere, or the release of oxygen, and be incorporated into the fabricated object. Specific examples of absorbers include oxides, transition metal carbides, transition metal nitrides, Si3N4, AlN, borides, and silicides. Suitable compositions as absorbers include Tb4O7 and Pr6O 11These include Ti2O3, TiO, SiO, ZnO, antimond-doped tin oxide (ATO), indium-doped tin oxide (ITO), MnO, MnO2, Mn2O3, Mn3O4, FeO, Fe2O3, Fe3O4, Cu2O, CuO, Cr2O3, CrO3, NiO, V2O3, VO2, V2O5, V2O4, Co3O4, CoO, transition metal carbides, transition metal nitrides, Si3N4, AlN, borides, and silicides. Preferably, the transition metal carbides are TiC and ZrC. Preferably, the transition metal nitrides are TiN and ZrN. Preferably, the borides are TiB2, ZrB2, and LaB6. Preferably, the silicides are TiSi2, ZrSi2, and MoSi2. From these, it is preferable to select a composition with high affinity to the other compositions constituting the powder as the absorber. Since the powder is silicon dioxide, a metal oxide is preferred as the absorbent. From the viewpoint of having the highest affinity with silicon dioxide, SiO is preferred as the absorbent. The absorbent may be a single composition or a combination of multiple compositions.
[0051] Absorbers that exhibit good energy absorption from a laser beam are preferably finely and uniformly dispersed in the powder. This ensures that the reaction that occurs in the powder when irradiated with a laser beam is uniform, thereby improving the accuracy of the fabrication. From this viewpoint, the average particle size of the absorbers contained in the powder is preferably 1 μm or more and less than 10 μm, and more preferably 1 μm or more and less than 5 μm.
[0052] The amount of absorbent contained in the powder is preferably 0.5 vol% to 10 vol%. A concentration of 0.5 vol% or more ensures that, under typical laser beam usage conditions, at least one absorbent particle is probabilistically present in the laser beam irradiation area, allowing for sufficient absorption. Furthermore, a concentration of 10 vol% or less suppresses the rapid temperature rise of the powder caused by laser beam irradiation, thereby preventing scattering of molten material and thus reducing the accuracy of the fabrication.
[0053] When using Nd:YAG lasers or fiber lasers as the lasers for fabrication, for the following two reasons, the absorber should be terbium oxide (Tb4O7) or praseodymium oxide (Pr6O7), which can form a eutectic with silicon dioxide. 11 ) is particularly preferred. The first reason is that terbium oxide and praseodymium oxide exhibit good energy absorption for Nd:YAG lasers (wavelength: 1064 nm) and fiber lasers (wavelength: 1030-1100 nm). By including an absorber with sufficient energy absorption in the powder used for fabrication, the spread of heat within the powder is further suppressed and localized, reducing the thermal impact on non-fabricated areas, and thus further improving fabrication accuracy.
[0054] The second reason is that when the powder contains terbium oxide or praseodymium oxide, a phase separation structure is formed in the silica network in which two or more phases are intricately intertwined. As mentioned above, silica-based materials have high viscosity in the liquid phase, so the liquid silica melted by the laser beam becomes spherical, and the solidified part tends to have a structure in which spheres are connected in a network, i.e., it becomes porous. However, when the powder contains terbium oxide or praseodymium oxide, a phase separation structure is formed in which the silica phase network and the phase containing terbium oxide or praseodymium oxide are intricately intertwined, suppressing crack propagation and improving the mechanical strength of the fabricated object. In order to obtain a fine phase separation structure, it is preferable that the particle size of terbium oxide and praseodymium oxide be 1 μm or more and less than 10 μm. More preferably, it is 1 μm or more and less than 5 μm. This results in a fabricated object with higher mechanical strength.
[0055] To adjust the physical properties of the ceramic articles to be manufactured, the powder may contain other compositions besides silicon dioxide and absorbers in amounts of less than 10% by mass.
[0056] In this specification, materials are sometimes represented using chemical formulas, such as SiO2 and Tb4O7 mentioned above. However, the elemental composition ratio of the actual material does not need to strictly match the ratio in the chemical formula, as long as it satisfies the spirit of the present invention. That is, the valence of the metal elements constituting a material may differ slightly from the valence assumed from the chemical formula. For example, if the absorber is SiO, the elemental composition ratio of the absorber can be Si:O=1:1.30 and still be included in the present invention. From the viewpoint of obtaining sufficient light absorption capacity, a more preferable elemental composition ratio is one in which the deviation from the stoichiometric ratio is within ±15%.
[0057] The molding process is carried out on a base. The base material can be appropriately selected and used from materials commonly used in the manufacture of molded objects, such as ceramics, metals, and glass, taking into consideration the intended use of the molded object and the manufacturing conditions. If the molded object is heated together with the base in step (iii), it is preferable to use heat-resistant ceramics for the base.
[0058] In the powder bed fusion method, as shown in Figure 1, powder is placed over the entire surface of the base to a predetermined thickness using rollers or blades. In the cladding method, as shown in Figure 2, powder is sprayed from a nozzle at the laser beam irradiation position, and the powder is placed on the base or the object placed on the base in a way that builds up the powder.
[0059] <Process (ii)> In the subsequent step (ii), the powder placed in step (i) is sintered, or melted and solidified, by irradiating it with a laser based on the fabrication data generated from the three-dimensional shape data of the model to be fabricated.
[0060] In the powder bed fusion method, as shown in Figure 1, in step (i), a laser beam is scanned and irradiated onto a predetermined area of the powder layer, which has been placed on the base to a predetermined thickness, to sinter, melt, or solidify the powder. In the cladding method, as shown in Figure 2, in step (i), powder is sprayed and supplied onto the base to selectively place the powder in the area to be fabricated, while simultaneously irradiating it with a laser beam to melt and solidify the powder.
[0061] When a laser beam is irradiated onto powder, absorbers contained in the powder absorb the energy, and this energy is converted into heat, causing the powder to melt. If the powder sinters, a portion of the particles melt. Once the laser beam has passed and irradiation is complete, the heat from the molten area escapes into the atmosphere and surroundings, causing cooling and the formation of a solidified area. Because the temperature changes rapidly during the melting and solidification processes, the majority of the formed object becomes amorphous silica. In addition, the rapid temperature changes often generate stress on the surface and inside of the object, leading to the formation of cracks. If cracks are formed, they can sometimes be reduced by subsequent heating processes. Furthermore, by introducing a process to absorb a metal component-containing liquid, which will be described in detail later, cracks can be further reduced or eliminated.
[0062] As mentioned above, when a powder mainly composed of silicon dioxide contains terbium oxide or praseodymium oxide, the powder melts and forms a network of connected spherical silica molecules, resulting in a phase-separated structure in which two or more phases are intricately intertwined. When this structure is subjected to heat treatment in step (iii), the silica crystallizes into cristobalite, improving the mechanical strength of the fabricated object.
[0063] The type of laser beam is not particularly limited, but YAG lasers and fiber lasers in the 1 μm wavelength band, and CO2 lasers in the 10 μm wavelength band are preferred. In particular, YAG lasers and fiber lasers in the 1 μm wavelength band are preferred because they exhibit high absorption of terbium oxide and praseodymium oxide.
[0064] <Step (iii)> As shown in the flowchart in Figure 4, in step (iii), the molded object formed by repeating steps (i) and (ii) multiple times is heated at a temperature of 1470°C or higher but less than 1730°C. The number of repetitions corresponds to the number of slices n in the slice data generated from the three-dimensional shape data of the object to be manufactured.
[0065] The fabricated object is created by placing a new powder layer in step (i) on top of the solidified layers formed in steps (i) and (ii). When a laser beam is scanned over the placed powder based on the fabrication data generated from the three-dimensional shape data of the fabrication model, the powder in the area irradiated by the laser beam melts and solidifies. At this time, the surface layer of the previously formed solidified layer also melts and becomes one with the later formed solidified layer. By repeating steps (i) and (ii) alternately, a fabricated object with a desired shape corresponding to the three-dimensional shape data of the fabrication model can be obtained.
[0066] If the molded object formed by repeating steps (i) and (ii) contains numerous cracks, it is preferable to perform a treatment to allow the molded object to absorb a metal component-containing liquid before applying the heat treatment, as shown in the flow chart of Figure 5.
[0067] The method for causing the molded object to absorb the metal-containing liquid is not particularly limited, as long as the necessary amount of the liquid can be supplied to the cracks throughout the entire crack in the molded object. The molded object may be immersed in the metal-containing liquid to impregnate it, or it may be sprayed onto the molded object in a mist or applied to the surface with a brush to allow absorption. Furthermore, multiple of these methods may be combined, or the same method may be repeated multiple times.
[0068] As mentioned above, for molded objects primarily composed of silica, metal component-containing liquids such as aluminum-containing liquids and zirconium-containing liquids (liquids containing zirconium) can be used, but aluminum-containing liquids are particularly preferred. The following will explain in detail the case where an aluminum-containing liquid is used as the metal component-containing liquid.
[0069] The aluminum component-containing liquid is preferably composed of, for example, a raw material containing aluminum, a solvent, and a stabilizer. Various aluminum compounds can be used as the raw material containing aluminum, and aluminum metal alkoxides and chlorides can be used.
[0070] In the case of an aluminum component-containing solution that includes aluminum as a metal alkoxide, it is preferable to include aluminum alkoxide, an organic solvent, and a stabilizer. For example, first, the aluminum alkoxide is dissolved in an organic solvent to prepare a solution of aluminum alkoxide. Specific examples of aluminum alkoxides include aluminum sec-butoxide, aluminum ethoxide, aluminum n-butoxide, aluminum tert-butoxide, and aluminum isopropoxide. The amount of organic solvent added to the aluminum alkoxide is preferably 5 to 30 molar ratios relative to the compound. More preferably, it is 10 to 25 molar ratios. In this invention, a molar ratio of 5 for M relative to N means that the molar amount of M added is 5 times the molar amount of N. If the concentration of aluminum alkoxide in the solution is too low, a sufficient amount of aluminum component cannot be absorbed into the molded object. On the other hand, if the concentration of aluminum alkoxide in the solution is too high, the aluminum component in the solution will aggregate, making it impossible to uniformly distribute the aluminum component in the crack areas of the molded object.
[0071] As organic solvents for dissolving aluminum alkoxides, alcohols, carboxylic acids, aliphatic or alicyclic hydrocarbons, aromatic hydrocarbons, esters, ketones, ethers, or mixtures of two or more of these solvents can be used. Preferred alcohols include methanol, ethanol, 2-propanol, butanol, 2-methoxyethanol, 2-ethoxyethanol, 1-methoxy-2-propanol, 1-ethoxy-2-propanol, 1-propoxy-2-propanol, 4-methyl-2-pentanol, 2-ethylbutanol, 3-methoxy-3-methylbutanol, ethylene glycol, diethylene glycol, and glycerin. Preferred aliphatic or alicyclic hydrocarbons include n-hexane, n-octane, cyclohexane, cyclopentane, and cyclooctane. Preferred aromatic hydrocarbons include toluene, xylene, and ethylbenzene. Preferred esters include ethyl formate, ethyl acetate, n-butyl acetate, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, and ethylene glycol monobutyl ether acetate. Preferred ketones include acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone. Examples of ethers include dimethoxyethane, tetrahydrofuran, dioxane, and diisopropyl ether. When preparing an aluminum-containing solution, it is preferable to use alcohols from among the various solvents mentioned above in terms of solution stability.
[0072] Because aluminum alkoxides are highly reactive with water, they undergo rapid hydrolysis upon contact with moisture in the air or the addition of water, resulting in turbidity and precipitation of the solution. To prevent this, it is preferable to add a stabilizer to stabilize the solution. Examples of stabilizers include β-diketone compounds such as acetylacetone, 3-methyl-2,4-pentanedione, 3-ethyl-2,4-pentanedione, and trifluoroacetylacetone; β-ketoester compounds such as methyl acetoacetate, ethyl acetoacetate, butyl acetoacetate, allyl acetoacetate, benzyl acetoacetate, isopropyl acetoacetate, tert-butyl acetoacetate, isobutyl acetoacetate, ethyl 3-oxohexanoate, ethyl 2-methylacetoacetate, ethyl 2-fluoroacetoacetate, and 2-methoxyethyl acetoacetate; and alkanolamines such as monoethanolamine, diethanolamine, and triethanolamine. The amount of stabilizer added is preferably 0.1 to 3 molar ratios relative to the aluminum alkoxide. More preferably, it is 0.5 to 2 molar ratios.
[0073] The solution may be prepared by reacting at room temperature or by refluxing.
[0074] In the case of an aluminum-containing solution that includes aluminum as a chloride, it is preferable to include an aluminum salt and water. The aluminum salt is not particularly limited as long as it is water-soluble. Nitrates, sulfates, acetates, and chlorides are particularly preferred. Depending on the type of aluminum salt, the aqueous solution may become unstable, in which case it is advisable to add a stabilizer to stabilize the solution. As a stabilizer, it is preferable to include at least one of the following: an organic acid, a surfactant, or a chelating agent. As organic acids, for example, acrylic acid, 2-hydroxyethyl acrylate, 2-acryloxyethyl succinic acid, 2-acryloxyethyl hexahydrophthalic acid, 2-acryloxyethyl phthalic acid, 2-methylhexanoic acid, 2-ethylhexanoic acid, 3-methylhexanoic acid, and 3-ethylhexanoic acid are preferred. As surfactants, for example, ionic surfactants such as sodium oleate, potassium fatty acid, sodium alkyl phosphate, alkylmethylammonium chloride, and alkylaminocarboxylate salts, and nonionic surfactants such as polyoxyethylene lauric acid fatty acid esters and polyoxyethylene alkylphenyl ethers are preferred.Examples of chelating agents include hydroxy acids such as glycolic acid, ascorbic acid, citric acid, malonic acid, gluconic acid, oxalic acid, succinic acid, malic acid, tartaric acid, and lactic acid; amino acids such as glycine, alanine, glutamic acid, aspartic acid, histidine, phenylalanine, asparagine, arginine, glutamine, cysteine, leucine, lysine, proline, serine, tryptophan, valine, and tyrosine; diethylenetriaminepentaacetic acid (DTPA), hydroxyethylethylenediaminetriacetic acid (HEDTA), triethylenetetraaminehexaacetic acid (TTHA), 1,3-propanediaminetetraacetic acid (PDTA), and 1,3-diamino-6-hydroxypropyl Preferred aminocarboxylic acids include ropanetetraacetic acid (DPTA-OH), hydroxyethyliminodiacetic acid (HIDA), dihydroxyethylglycine (DHEG), glycol etherdiaminetetraacetic acid (GEDTA), dicarboxymethylglutamic acid (CMGA), and (S,S)-ethylenediaminedisuccinic acid (EDDS); phosphonic acids such as 1-hydroxyethylidene-1,1-diphosphonic acid (HEDP), 2-phosphobutanone-1,2,4-tricarboxylic acid (PBTC), ethylenediaminetetra(methylenephosphonic acid), diethylenetriaminepenta(methylenephosphonic acid), and nitrilotris(methylenephosphonic acid); and aromatic acids such as salicylic acid.
[0075] The method for producing the aluminum component-containing liquid is not limited. It is preferable to prepare it by mixing an aluminum salt, water, and a stabilizer, but it may also be prepared by mixing all of them at once. Alternatively, the metal salt and stabilizer may be mixed first and then water may be added and mixed, or the metal salt and water may be mixed first and then the stabilizer may be added and mixed, or the stabilizer and water may be mixed first and then the metal salt may be added and mixed.
[0076] Furthermore, it is also preferable to use a particle dispersion liquid as the aluminum component-containing liquid, which consists of particles containing aluminum, a dispersant, and a solvent.
[0077] As particles containing the element aluminum, aluminum particles or alumina particles can be used. Aluminum particles or alumina particles may be produced by crushing the respective materials using a top-down method, synthesized using a bottom-up method such as a hydrothermal reaction from metal salts, hydrates, hydroxides, carbonates, etc., or commercially available products may be used.
[0078] The particle size is 300 nm or less, more preferably 50 nm or less, and even more preferably 30 nm or less, in order to penetrate cracks.
[0079] The shape of the fine particles is not particularly limited and may be spherical, granular, columnar, ellipsoidal, cubic, rectangular, needle-shaped, columnar, plate-shaped, scaly, or pyramidal.
[0080] The dispersant preferably contains at least one of the following: an organic acid, a silane coupling agent, and a surfactant. Preferred organic acids include, for example, acrylic acid, 2-hydroxyethyl acrylate, 2-acryloxyethyl succinic acid, 2-acryloxyethyl hexahydrophthalic acid, 2-acryloxyethyl phthalic acid, 2-methylhexanoic acid, 2-ethylhexanoic acid, 3-methylhexanoic acid, and 3-ethylhexanoic acid. Preferred silane coupling agents include, for example, 3-acryloxypropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, hexyltrimethoxysilane, octyltriethoxysilane, and decyltrimethoxysilane. Preferred surfactants include, for example, ionic surfactants such as sodium oleate, potassium fatty acid, sodium alkyl phosphate, alkylmethylammonium chloride, and alkylaminocarboxylate salts, and nonionic surfactants such as polyoxyethylene lauric acid fatty acid esters and polyoxyethylene alkylphenyl ethers.
[0081] As solvents, alcohols, ketones, esters, ethers, ester-modified ethers, hydrocarbons, halogenated hydrocarbons, amides, water, oils, or mixtures of two or more of these solvents may be used. Preferred alcohols include methanol, ethanol, 2-propanol, isopropanol, 1-butanol, and ethylene glycol. Preferred ketones include acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone. Preferred esters include ethyl acetate, propyl acetate, butyl acetate, 4-butyrolactone, propylene glycol monomethyl ether acetate, and methyl 3-methoxypropionate. Preferred ethers include ethylene glycol monomethyl ether, diethylene glycol monobutyl ether, butyl carbitol, 2-ethoxyethanol, 1-methoxy-2-propanol, and 2-butoxyethanol. A preferred modified ether is propylene glycol monomethyl ether acetate. Preferred hydrocarbons include, for example, benzene, toluene, xylene, ethylbenzene, trimethylbenzene, hexane, cyclohexane, and methylcyclohexane. Preferred halogenated hydrocarbons include, for example, dichloromethane, dichloroethane, and chloroform. Preferred amides include, for example, dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone. Preferred oils include, for example, mineral oil, vegetable oil, wax oil, and silicone oil.
[0082] The particle dispersion may be prepared by simultaneously mixing aluminum particles or alumina particles with a dispersant and a solvent, or by mixing aluminum particles or alumina particles with a dispersant first and then mixing in the solvent. Alternatively, the aluminum or alumina fine particles may be mixed with the solvent first and then the dispersant may be mixed, or the dispersant may be mixed with the solvent first and then the aluminum or alumina fine particles may be mixed.
[0083] In step (iii) above, to allow the aluminum-containing liquid to be absorbed into the cracks formed in the fabricated object and to locally melt the area near where the aluminum element is present, the heating temperature and the amount of aluminum element in the cracks should be adjusted. The amount of aluminum element in the cracks can be adjusted by the concentration of aluminum in the aluminum-containing liquid, the method of absorbing the aluminum-containing liquid into the cracks, and the number of times this is done. It is also possible to adjust this by sequentially repeating the process of absorbing the aluminum-containing liquid and heating. In particular, increasing the amount of aluminum element present in the cracks makes the area near the cracks more easily melted. By adjusting the amount of aluminum element present in the cracks in this way, the shape of the fabricated object can be maintained without distortion, the complex and precise shapes formed by the direct fabrication method can be preserved, the shape of the fabricated object can be obtained almost exactly as designed, and fabrication with high accuracy can be achieved.
[0084] A silica object that has absorbed an aluminum-containing liquid is heated to a temperature above the eutectic point of the eutectic phase formed by silica and aluminum oxide, but below the melting point of silica (1710°C). This causes the aluminum oxide generated from the aluminum-containing liquid, or the amount of silica that corresponds to the amount of aluminum oxide initially present in the aluminum-containing liquid, to melt in the cracks on the surface and inside the silica object. In other words, since there is more aluminum oxide on the surface of the object in contact with the aluminum-containing liquid than in areas away from the cracks, the area near the cracks approaches the eutectic composition, allowing for selective melting. By heating the silica near the cracks after the aluminum-containing liquid absorption process so that the maximum temperature is between 1595°C and 1730°C, the silica can be transformed into cristobalite while simultaneously reducing or eliminating the cracks.
[0085] The heating time is irrelevant as long as the area near the crack reaches the maximum temperature mentioned above. Specifically, the molded object should be heated to a temperature between 1595°C and 1730°C, which is the temperature you want the area near the crack to reach.
[0086] The heating method is not particularly limited. The molded object, which has absorbed an aluminum-containing liquid, may be heated by irradiating it with an energy beam, or it may be heated in an electric furnace. When heating with an energy beam, it is advisable to determine in advance, using a thermocouple or similar device, the relationship between the amount of heat input from the energy beam and the temperature of the molded object, so that the object is heated to the preferred temperature described above.
[0087] During the heat treatment process, the surface layer or areas near cracks of the molded object may melt and adhere to the setter. Therefore, when placing the molded object in the setter during the heat treatment process, it is preferable that the setter be inert. Examples of inert setters include platinum in an atmospheric environment and iridium in a low-oxygen environment.
[0088] In process (iii), phases (crystal grains) containing silicon dioxide, terbium, or praseodymium are formed within the fabricated object, along with phases (crystal grains) containing aluminum. However, their grain sizes (e.g., average grain size) differ significantly. This is thought to be because the cracks and their vicinity melt, and the material moves in a direction that reduces surface energy, thus reducing or eliminating the cracks. Furthermore, as heating progresses, the aluminum components distributed in the crack areas diffuse into the crystalline and amorphous interior of the fabricated object, and the crystals in the fabricated object recrystallize while containing the aluminum components. In addition to the reduction or elimination of cracks within the fabricated object, the formation of a phase separation structure consisting of multiple phases with different average grain sizes improves the machinability of the fabricated object, enabling precise finishing with fewer chips.
[0089] <Ceramic articles> The ceramic articles of the present invention preferably have a phase separation structure comprising two or more, and more particularly three or more, phases. A preferred combination of the three phases is a phase mainly composed of SiO2, a phase mainly composed of a rare earth silicate containing terbium or praseodymium, and a phase mainly composed of Al2O3, which is an oxide of a metal element contained in a metal component-containing liquid. SiO2, rare earth silicate, and Al2O3 form a eutectic relationship with each other, and a complex phase separation structure consisting of the three phases can be stably formed.
[0090] The phase mainly composed of SiO2 is formed when amorphous silica is transformed into cristobalite by the heating process in step (iii). The phase mainly composed of rare earth silicates containing terbium or praseodymium is preferably in the form of Si2Tb2O7 or Si2Pr2O7. Each phase can be identified, for example, by structural analysis using X-ray diffraction, electron diffraction, or EBSD (Electron Backscattering Diffraction). The crystal structure of each phase varies somewhat depending on the manufacturing process, but it is preferable that the three phases forming the eutectic are composed of the crystal structures described above.
[0091] Cristobalite exists in two forms, α-cristobalite and β-cristobalite, with a phase transition temperature of approximately 240°C. Because a rapid volume change occurs at this phase transition temperature, cristobalite has traditionally been considered a material vulnerable to temperature changes. However, in this invention, even when silica is converted to cristobalite, excellent mechanical strength against temperature changes is obtained. This is thought to be due to the silica-based structure having a phase-separated structure consisting of multiple phases, such as Tb2Si2O7 and Pr2Si2O7 phases, in addition to cristobalite. It is believed that having a phase-separated structure consisting of multiple phases in the silica-based structure slows down the volume change due to thermal expansion at the phase transition temperature, thereby suppressing the rapid volume change associated with temperature changes.
[0092] When used as a core for casting, the Si content of the ceramic article of the present invention is preferably more than 80% by mass in terms of oxide (SiO2). If the Si content is 80% by mass or less, the solubility in alkaline solutions required for use as a casting core cannot be obtained. Examples of alkaline solutions include aqueous sodium hydroxide solution or aqueous potassium hydroxide solution.
[0093] The Tb or Pr contained in the ceramic article of the present invention is preferably 1.0% by mass or more and 20% by mass or less in terms of oxide (in terms of Tb2O3 and Pr2O3), and more preferably 3.0% by mass or more and 15% by mass or less. If the Tb or Pr is less than 1.0% by mass, the amount of laser energy absorbed will be small, which may prevent the acquisition of high-precision molded objects. If the Tb or Pr is greater than 20% by mass, the solubility in alkaline aqueous solutions required for casting cores cannot be obtained.
[0094] In the ceramic articles of the present invention, 70% by mass or more of the silicon dioxide is cristobalite bonded with oxygen. If the amount of cristobalite is less than 70% by mass, there is a risk that the necessary strength for use as a casting core will not be obtained. Preferably, 90% by mass or more, and more preferably 95% by mass or more, of the silicon dioxide is cristobalite.
[0095] The porosity of the ceramic articles of the present invention is preferably 10% or more and 40% or less. If the porosity is less than 10%, the bending strength becomes too high, which may cause the casting to crack when used as a core for casting. If the porosity is greater than 40%, the necessary strength as a structure cannot be obtained. As will be described in detail later, in this invention, porosity refers to open porosity.
[0096] In the present invention, the boron (B) content in the ceramic article is preferably less than 1000 ppm. If the B content is higher than 1000 ppm, the softening point decreases, and the heat resistance required for a casting core may not be obtained.
[0097] <Method for evaluating physical properties> (mechanical strength) The mechanical strength of the fabricated object was evaluated by a three-point bending test based on R1601, the JIS standard for room-temperature bending strength testing of fine ceramics. For each of the 10 test specimens, the three-point bending strength was calculated as follows: P [N] was the maximum load at fracture, L [mm] was the distance between external supports, w [mm] was the width of the specimen, and t [mm] was the thickness of the specimen. 3×P×L / (2×w×t2) (Formula 1) The values were calculated using the following methods and then averaged.
[0098] (Porosity) The porosity of the fabricated object was evaluated using a method based on JIS standard R1634, which is the method for measuring the density and open porosity of sintered fine ceramics. Specifically, for three ceramic articles similar to the samples used for measuring mechanical strength, the porosity was calculated using {(W3-W1) / (W3-W2)} × 100, where W1 was the dry mass of the fabricated object, W2 was the mass in water, and W3 was the mass when saturated with water, and these values were averaged.
[0099] (Relative density) The relative density [%] was calculated by dividing the bulk density (mass divided by volume) of the fabricated object by the theoretical density. The theoretical density was calculated from the crystal structure. The crystal structure was identified by performing Rietveld analysis after X-ray diffraction measurements.
[0100] (Crystal structure) The phases contained in the ceramic articles were identified by X-ray diffraction measurement after polishing the cross-section of the central part of the object to be measured to create a measurement surface.
[0101] The content of each phase in the sample was calculated using the following method. Simultaneous SEM-EDX and EBSD analysis was performed at 10 different locations on the measurement surface with a field of view size of 100 μm × 100 μm, and the composition and crystalline phases were mapped. For the 10 maps created, the area ratio occupied by each phase was determined, and the proportion of each phase in the sample was calculated from the average of these values. If small phases are present, the composition and crystalline structure can be similarly analyzed using a transmission electron microscope (TEM).
[0102] The grain size of the crystal grains constituting the phase was calculated by observing more than 300 crystal grains within the same phase observed on the measurement surface using EBSD, and calculating the average value of the equivalent circle diameter of each crystal grain.
[0103] (composition analysis) The Si, Tb, Pr, Al, and Zr content in powders, molded objects, or ceramic articles was measured by inductively coupled plasma atomic emission spectrometry (ICP-AES), while the content of other elements, including B, was measured by GDMS or ICP-MS. [Examples]
[0104] (Example 1) SiO2 powder with an average particle size of approximately 38 μm and Tb4O7 powder with an average particle size of 4 μm were prepared, and each powder was weighed so that Si was 90.0 mass% on an oxide basis (SiO2 basis) and Tb was 10.0 mass% on an oxide basis (Tb4O7 basis) (Table 1). The SiO2 powder mainly consists of cristobalite. Each weighed powder was mixed in a dry ball mill for 30 minutes to obtain a mixed powder. In this invention, the average particle size is the median diameter (also called the median value), which is the particle size at which the cumulative frequency is 50% (D50). Compositional analysis of the mixed powder by ICP emission spectrometry revealed that the aluminum oxide content was less than 1 mass%.
[0105] [Table 1]
[0106] Next, the object of Example 1 was fabricated in the same manner as shown in Figure 1. The shape of the fabricated object was a rectangular parallelepiped measuring 5 mm × 42 mm × 6 mm. A 3D Systems ProXDMP 100 (product name) equipped with a 50 W fiber laser (beam diameter 65 μm) was used to form the object.
[0107] First, a 20 μm thick first powder layer made of the aforementioned powder was formed on the alumina base 130 using a roller (Figure 1(a), (b)).
[0108] Next, a 47.5W laser beam was scanned and irradiated onto the powder layer, melting and solidifying the material powder in a rectangular area of 5mm x 42mm, forming a solidified area 100 (Figure 1(c)). The drawing speed at this time was 60mm / s and the drawing pitch was 80μm. The drawing lines were positioned at a 45-degree angle to each side of the rectangle, as shown in Figure 6(a).
[0109] Next, a 20 μm thick powder layer was newly formed using a roller to cover the solidification section 100. A laser beam was scanned across the powder layer, melting and solidifying the material powder in a rectangular area of 5 mm × 42 mm, thereby forming the solidification section 100 (Figures 1(d), (e)). At this time, as shown in Figure 6(b), the laser was scanned in a direction perpendicular to the first layer's drawing line to melt and solidify the powder. This process was repeated until the height of the solidification section reached 6 mm, and 14 objects measuring 42 mm × 5 mm × 6 mm were fabricated.
[0110] When the surface of the fabricated object was observed with an optical microscope, the Ra value of the surface of the fabricated object, measured while avoiding the pores, was 30 μm or less.
[0111] Each fabricated object was separated from its alumina base, and 13 of them were polished to obtain 40mm x 4mm x 3mm specimens for use in three-point bending strength tests and porosity measurements.
[0112] Porosity was evaluated on the test specimens prepared for porosity measurement, and the porosity was found to be 18.4%. Furthermore, X-ray diffraction measurements of the polished surface revealed that the crystalline phase in the ceramic article was almost entirely amorphous.
[0113] The molded objects, excluding the test specimens used for porosity measurement, were placed in an electric furnace and subjected to heating treatment. Specifically, the furnace was heated to 1610°C in an air atmosphere over 2.5 hours, held at 1610°C for 50 minutes, and then the power was turned off and the objects were cooled to below 200°C over 5.0 hours.
[0114] The composition of the obtained ceramic articles was measured by ICP-AES and found to be 90.3 mass% Si (in terms of SiO2) and 9.7 mass% Tb (in terms of Tb2O3). GDMS analysis revealed a B concentration of 0.4 ppm.
[0115] Next, in order to analyze the crystal structure of the ceramic articles, the articles were cut and polished. First, both sides of the ceramic article were cut with a wire saw, leaving the unpolished center intact, to obtain a 10mm x 4mm x 3mm test piece. Then, it was polished to a thickness of approximately 1.5mm in the H direction, and further polished to a mirror finish to obtain a 10mm x 4mm observation surface.
[0116] X-ray diffraction of the observation surface revealed that the crystalline phase in the ceramic article is composed of cristobalite (SiO2) and Tb2Si2O7 phase.
[0117] Furthermore, simultaneous SEM-EDX and EBSD analysis was performed on the observation surface. Ten different locations were analyzed within a 100 μm × 100 μm field of view to obtain composition and crystalline phase mappings. The results showed that the SiO2 portion was almost entirely cristobalite, accounting for 97% by mass. The remainder was amorphous silica, in which no Kikuchi pattern was detected by EBSD. The ratio of cristobalite to amorphous silica was calculated from the respective areas obtained by SEM-EDX and EBSD mapping, and the typical densities of cristobalite (2.3 g / cc) and amorphous silica (2.2 g / cc). The Tb2Si2O7 phase was scattered throughout the field of view, and the average equivalent circle diameter calculated from the area obtained by mapping was 2.3 μm.
[0118] A three-point bending test was performed on the test specimen used for strength testing, and the result was 7.2 [MPa].
[0119] The Si, Tb, Al, Zr, and B content, porosity, and three-point bending strength of the ceramic articles were evaluated. The results are shown in Table 2. The following examples and comparative examples were evaluated similarly, and the results are also shown in Table 2.
[0120] Table 1, which shows the weighing values of the powder, lists the content of Si, Al, and the absorbers Tb, Pr, and Si as SiO2, Al2O3, Tb4O7, and Pr6O 11 The values are expressed in terms of SiO2, Tb2O3, Pr2O3, Al2O3, and ZrO2, respectively. Table 2, which shows the evaluation results for ceramic articles, expresses the Si, Tb, Pr, Al, and Zr content in terms of values converted to SiO2, Tb2O3, Pr2O3, Al2O3, and ZrO2, respectively.
[0121] [Table 2]
[0122] (Example 2) A ceramic article was fabricated in the same manner as in Example 1, except that the fabricated object was impregnated with an aluminum-containing liquid before heat treatment.
[0123] The aluminum-containing solution was prepared as follows: Aluminum sec-butoxide was dissolved in 2-propanol (IPA), and ethyl acetoethyl (EAcAc) was added as a stabilizer. The molar ratio of each component was aluminum sec-butoxide:IPA:EAcAc = 1.04:5:2. The solution was then stirred at room temperature for approximately 3 hours to prepare the aluminum-containing solution.
[0124] In Example 2, a 3mm x 4mm x 3mm object, processed for testing, was immersed in a prepared aluminum-containing liquid, degassed under reduced pressure for 1 minute to allow the liquid to be absorbed into the object, and then air-dried for 1 hour.
[0125] Next, the molded object, which had absorbed the aluminum-containing liquid, was placed in an electric furnace and heated. The temperature was raised to 1610°C in 2.5 hours in an air atmosphere, held at 1610°C for 50 minutes, and then the power was turned off and it was cooled to below 200°C in 5.0 hours.
[0126] The surface of the obtained ceramic articles was polished, and the crystal structure was analyzed by X-ray diffraction and EBSD. The results showed that the SiO2 was cristobalite, with a proportion of 97% by mass. Furthermore, the Si2Tb2O7 phase was also observed.
[0127] (Example 3) Example 3 differs from Example 2 in that the process of absorbing an aluminum-containing liquid into the fabricated object and the process of heat treatment were repeated alternately twice each.
[0128] Three ceramic articles measuring W40mm x D4mm x H3mm were prepared for a three-point bending strength test, and one identical ceramic article was prepared for composition and structural evaluation.
[0129] The surface of the obtained ceramic articles was polished, and the crystal structure was analyzed by X-ray diffraction and EBSD. As a result, SiO2 was found to be cristobalite, with a proportion of 98 mass%. Furthermore, the Si2Tb2O7 phase was also observed.
[0130] (Example 4) A ceramic article was prepared in the same manner as in Example 1, except that it was impregnated with a zirconium-containing solution before heat treatment and the heat treatment temperature was set to 1670°C.
[0131] The zirconium-containing solution was prepared as follows: A solution was prepared by dissolving 85% by mass of zirconium butoxide (zirconium(IV) butoxide (hereinafter referred to as Zr(On-Bu)4)) in 1-butanol. The Zr(On-Bu)4 solution was then dissolved in 2-propanol (IPA), and ethyl acetoethyl (EAcAc) was added as a stabilizer. The molar ratio of each component was Zr(On-Bu)4:IPA:EAcAc = 1:15:2. The zirconium-containing solution was then prepared by stirring at room temperature for approximately 3 hours.
[0132] In Example 4, the above-mentioned molded object processed for testing was immersed in the zirconium-containing liquid and degassed under reduced pressure for 1 minute to allow the liquid to penetrate the inside of the molded object, after which it was air-dried for 1 hour. After that, the molded object impregnated with the zirconium-containing liquid was placed in an electric furnace and heated. The temperature was raised to 1670°C in an air atmosphere over 2.5 hours, held at 1670°C for 50 minutes, and then the power was turned off and it was cooled to below 200°C over 1.5 hours.
[0133] Next, the surface of the obtained ceramic articles was polished, and the crystal structure was analyzed by X-ray diffraction and EBSD. As a result, SiO2 was found to be cristobalite, with a proportion of 98 mass%. Furthermore, the Si2Tb2O7 phase was also observed.
[0134] (Example 5) Example 5 differs from Example 4 in that the process of impregnating the molded object with a zirconium-containing liquid and the process of heat treatment were repeated alternately twice each.
[0135] The ceramic materials prepared were three cubes measuring W40mm × D4mm × H3mm for three-point bending strength testing, one identical cube for composition and structural evaluation, and one cube measuring W5mm × D5mm × H5mm for wear resistance testing.
[0136] Evaluation of the fabricated silica-based structure revealed that the SiO2 was cristobalite, accounting for 99% by mass. Furthermore, the Si2Tb2O7 phase was also observed.
[0137] (Examples 6-9) Except for changing the mass ratio of SiO2 powder and Tb4O7 powder, the ceramic articles of Examples 6 to 9 were prepared by repeating the process of impregnating with an aluminum-containing liquid and the process of heat treatment twice alternately, similar to Example 3. The mass ratios of the mixed powders in each example are shown in Table 1.
[0138] (Examples 10 and 11) Except for changing the mass ratio of SiO2 powder and Tb4O7 powder, ceramic articles of Example 10 and Example 11 were prepared in the same manner as in Example 1. The mass ratios of the mixed powders for each example are shown in Table 1.
[0139] (Examples 12-14) Ceramic articles of Examples 12 to 14 were prepared using the same process as in Example 1, except that the heat treatment temperature was changed, using a powder mixture of SiO2 powder and Tb4O7 powder in the mass ratio shown in Table 1. The respective heat treatment temperatures are shown in Table 2.
[0140] (Examples 15 and 16) The powder used was prepared by weighing SiO2 powder and Tb4O7 powder in the mass ratios shown in Table 1, and then adding a trace amount of B2O3 powder and mixing them. Ceramic articles of Example 15 and Example 16 were prepared using the same process as in Example 1, except that the heat treatment temperature was set to 1470°C.
[0141] (Example 17) As an absorbent, Tb4O7 powder is used in Pr6O 11 The ceramic article of Example 17 was obtained by following the same procedure as in Example 1, except that the powder was replaced with a powder mixed in the mass ratio shown in Table 1.
[0142] (Example 18) The ceramic structure of Example 18 was obtained using the same procedure as in Example 2, except that the aluminum-containing liquid used was different. The mass ratio of the weighed SiO2 powder and Tb4O7 powder is shown in Table 1.
[0143] The aluminum-containing solution was prepared using alumina particles as follows: Alumina particles with an average particle size of 24 nm (manufactured by Kanto Chemical Co., Ltd.), 2-hydroxyethyl acrylate and 3-acryloxypropyltrimethoxysilane as dispersants, and methyl ethyl ketone as a solvent were mixed so that the alumina concentration in the dispersion was 70% by mass, and the mixture was uniformly stirred to obtain an alumina particle dispersion.
[0144] (Example 19) Ceramic articles were prepared in the same manner as in Example 3, except that SiO powder was used as the absorbent in the mass ratio shown in Table 1. SiO powder with an average particle size of 5 μm was used.
[0145] Three silica-based structures measuring W40mm x D4mm x H3mm were fabricated for three-point bending strength testing, and one identical silica-based structure was fabricated for composition and structural evaluation.
[0146] The surface of the obtained silica-based structure was polished, and its crystal structure was analyzed by X-ray diffraction and EBSD. As a result, it was found that the SiO2 was cristobalite, and its proportion was 98% by mass.
[0147] (Examples 20 and 21) Ceramic articles of Examples 20 and 21 were prepared by the same process as in Example 4. However, they differed from Example 4 in that SiO2 powder, Al2O3 powder, and SiO powder as an absorber were weighed in the mass ratios shown in Table 1, a zirconium component-containing solution was used as the metal component-containing solution, and the heat treatment temperature was 1680°C. The Al2O3 powder used had an average particle size of 20 μm. For the zirconium component-containing solution, an aqueous zirconium acetate solution prepared to have a zirconia content of 30% by mass was used.
[0148] The ceramic articles of the examples other than Example 15 had a lower amount of B compared to the structure of Example 15, and had a higher mechanical strength of 5.0 MPa or more. Also, when the ceramic articles of Examples 15 and 16 were heated to 1600°C, the corners of the structure of Example 15 deformed slightly. Example 15, which contained a large amount of B, had lower heat resistance compared to the other examples.
[0149] In the ceramic articles of Examples 1 to 16 and Example 18, the Si2Tb2O7 phase was observed, while in the ceramic article of Example 17, the Si2Pr2O7 phase was observed. This suggests that a phase separation structure was formed within the structure, improving its mechanical strength. Furthermore, these structures are presumed to have the effect of suppressing temperature changes in the coefficient of thermal expansion and easing thermal stress.
[0150] Examples 2 to 9 and Examples 18 to 21, in which a metal component-containing liquid was absorbed and then heat-treated, showed reduced or eliminated cracks and even higher strength due to the formation of the Al2O3 phase.
[0151] Furthermore, when the surface of the ceramic articles was observed under a microscope, the Ra value of the structural surface, measured while avoiding pores, was 30 μm or less for all of the ceramic articles in the examples.
[0152] (Comparative Example 1) As shown in Table 1, a ceramic article of Comparative Example 1 was fabricated in the same manner as in Example 1, except that the amount of Tb4O7 powder mixed with SiO2 powder was increased to approximately 27.0% by mass, and the drawing pitch of the irradiated laser beam was set to 170 μm. The resulting ceramic article had a high porosity of 45.0% and a low three-point bending strength of 1.2 MPa.
[0153] (Comparative Example 2) As shown in Table 1, when the molding process was carried out in the same manner as in Example 1, except that the mass ratio of Tb4O7 powder used in the molding process was increased to approximately 27.0% by mass, the amount of Tb2Si2O7 in the molded object increased. The amount of Si contained in the ceramic article was 80% by mass or less in terms of oxide. When 0.1 g of the molded object from Comparative Example 2 was placed in 20 ml of a 20% by mass sodium hydroxide aqueous solution, the container was sealed, and the state was maintained at 100°C for 450 minutes, but 0.02 g of the molded object remained undissolved.
[0154] Therefore, the ceramic article of Comparative Example 2 is considered to have insufficient solubility in sodium hydroxide for use as a casting core.
[0155] (Comparative Example 3) A ceramic article was fabricated in the same manner as in Example 1, except that the heating temperature after fabrication was set to 1440°C. When the crystal structure of the ceramic article was evaluated in the same manner as in Example 1, it was found to be mostly amorphous silica, and the three-point bending strength, evaluated in the same manner as in Example 1, was low at 2.0 MPa.
[0156] (Comparative Example 4) When ceramic articles were fabricated in the same manner as in Example 1, except that the post-molding heating temperature was set to 1740°C, the corners and rhombuses became rounded and deformed.
[0157] In Comparative Example 4, the molded object was heated at 1740°C, which exceeds the melting point of silicon dioxide (1730°C). As a result, the silicon dioxide entered the liquid phase, and it is believed that the shape could not be maintained. [Industrial applicability]
[0158] According to the present invention, it is possible to provide a method for manufacturing ceramic articles that can improve the mechanical strength of molded objects while retaining the characteristics of the direct molding method, which allows for the creation of complex shapes using silica-based materials. Furthermore, it is possible to provide ceramic articles with improved mechanical strength while maintaining shape accuracy. Moreover, ceramic articles of the present invention that suppress rapid shape changes due to thermal expansion can be used as cores for metal casting. [Explanation of Symbols]
[0159] 100 Solidified section 101 powder 102 Powder layer 103 Unsolidified powder 110 Sculptures 130 base 151 stages 152 Rollers 180 Laser beam sources 181 Scanner section 190 Liquid spray nozzles 201 Cladding Nozzle 202 Powder supply hole 203 Laser beam
Claims
1. (i) disposing a powder including an absorber that absorbs light having a wavelength included in the irradiated laser beam and silicon dioxide; (ii) irradiating the powder with a laser beam to sinter or melt and solidify the powder; (iii) a step of heat treating the shaped object formed by repeating the steps (i) and (ii) at 1470° C. or more and less than 1730° C.; 1. A method for producing a ceramic article comprising the steps of:
2. A method for manufacturing a ceramic structure, wherein the absorber has a higher absorption ability for light having a wavelength contained in the laser beam than the silicon dioxide.
3. 3. The method for manufacturing a ceramic article according to claim 1, wherein the absorber has an absorptivity of 10% or more for light having a wavelength contained in the laser beam.
4. The absorber is Tb 4 O 7 Or P 6 O 11 The method for producing a ceramic article according to any one of claims 1 to 3, characterized in that
5. The absorbent is Ti 2 O 3 , TiO, SiO, ZnO, antimony-doped tin oxide (ATO), indium-doped tin oxide (ITO), MnO, MnO 2 , Mn 2 O 3 , Mn 3 O 4 , FeO, Fe 2 O 3 , Fe 3 O 4 , Cu 2 O, CuO, Cr 2 O 3 , CrO 3 , NiO, V 2 O 3 , V.O. 2, V 2 O 5 , V 2 O 4 , Co 3 O 4 4. The method for producing a ceramic article according to claim 1, further comprising at least one selected from the group consisting of CoO.
6. The absorber is a transition metal carbide, a transition metal nitride, or Si 3 N 4 4. The method for producing a ceramic article according to claim 1, further comprising at least one selected from the group consisting of AlN, borides, and silicides.
7. The method for producing a ceramic article according to any one of claims 1 to 6, characterized in that the average particle size of the silicon dioxide is 5 µm or more and 200 µm or less, and the average particle size of the absorbent is 1 µm or more and less than 10 µm.
8. 8. The method for producing a ceramic article according to claim 1, wherein the absorbent is contained in the powder in an amount of 0.5 vol % or more and 10 vol % or less.
9. A method for manufacturing a ceramic article described in any one of claims 1 to 8, characterized in that the ceramic article contains cristobalite.
10. A method for manufacturing a ceramic article described in any one of claims 1 to 9, wherein the shaped object to be heat treated contains aluminum oxide.
11. A method for producing a ceramic article described in any one of claims 1 to 10, wherein the powder contains aluminum oxide.
12. A method for manufacturing a ceramic article described in any one of claims 1 to 11, wherein the shaped object to be heat treated contains aluminum element or zirconium element.
13. The step (iii) comprises adding a metal component-containing liquid containing a metal element to the shaped object before the heat treatment.
13. The method of claim 1, further comprising the step of: absorbing
14. The method for producing a ceramic article according to claim 13, characterized in that the metal oxide, which is an oxide of a metal element, is capable of forming a eutectic with silicon dioxide.
15. 15. The method for producing a ceramic article according to any one of claims 1 to 14, wherein a melting point of silicon dioxide is Tm, and a eutectic temperature of a metal oxide and silicon dioxide contained in the shaped article to be heat-treated is TE, where TE is a maximum temperature TS reached by the shaped article in the heat treatment of step (iii) and satisfies the relationship TE≦TS<Tm. A method for producing a ceramic article according to any one of claims 1 to 7.
16. 16. The method for manufacturing a ceramic article according to claim 1, wherein the melting point of silicon dioxide is Tm and the melting point of the metal oxide contained in the shaped article to be heat-treated is Ti, and the relationship Tm<Ti is satisfied.
17. A ceramic article comprising silicon dioxide, comprising: A ceramic article, characterized in that 70 mass% or more of the silicon dioxide is cristobalite.
18. The ceramic article according to claim 17, characterized in that the Si content, calculated as oxide, is greater than 80 mass %.
19. 19. The ceramic article of claim 17 or 18, wherein the ceramic article comprises aluminum oxide or zirconium oxide.
20. 20. The ceramic article according to any one of claims 17 to 19, which is a casting core.