Method for manufacturing article having silicon carbide as main component, and raw-material powder used in the same
Patent Information
- Application Number
- JP2020209577
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-12-24
- Filing Date
- 2020-12-17
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2040-12-17
AI Technical Summary
Existing methods for manufacturing silicon carbide articles using powder bed fusion bonding face challenges such as void formation and require high energy input, especially when using organic materials like resins, and struggle to maintain shape integrity due to explosive temperature rises during combustion synthesis.
A method involving a raw material powder mixture of silicon carbide, metallic silicon, and carbon, with a silicon carbide content of 60-100 at%, and controlled spatial laser power density of 11-50 J/mm³, combined with a combustion synthesis process to suppress reaction propagation and temperature rise, is employed.
This approach allows for the production of silicon carbide articles with reduced energy consumption, without organic materials, and maintains shape integrity by limiting explosive temperature rises and void formation, enabling high-density objects.
Smart Images

Figure 00000011_0000 
Figure 00000011_0001 
Figure 00000011_0002
Abstract
Description
[Technology Field]
[0001] This invention relates to a technology for manufacturing articles mainly composed of silicon carbide using a powder bed fusion bonding method. [Background technology]
[0002] Additive manufacturing, or 3D printing, which involves irradiating metal or resin powder with a laser according to the 3D data of the item to be manufactured, is increasingly being used as a method for producing prototypes with complex shapes and small quantities of diverse items. In recent years, there has been a demand for the creation of items made not only from metals and resins, but also from inorganic compounds that are difficult to process, such as SiC and TiAl.
[0003] Patent Document 1 proposes a method for producing articles mainly composed of silicon carbide using a powder bed fusion method, with raw materials containing silicon carbide particles and molding resin particles such as nylon, polypropylene, and polyethylene terephthalate. Patent Document 2 discloses a method for fabricating objects using a powder containing silicon carbide and a boride metal having a melting point lower than the sublimation point of silicon carbide. [Prior art documents] [Patent Documents]
[0004] [Patent Document 1] Japanese Patent Publication No. 2017-171577 [Patent Document 2] Japanese Patent Publication No. 2019-64226 [Overview of the project] [Problems that the invention aims to solve]
[0005] As described in Patent Document 1, in a process of forming an object by heating a mixture of silicon carbide particles and molding resin particles, voids are formed inside the object when the irradiated area is sintered with a laser. Patent Document 2 utilizes the eutectic of silicon carbide and metal boride, allowing for the formation of a relatively dense object while suppressing the sublimation of silicon carbide. However, it is necessary to heat the object to over 2000°C, which is the melting point of metal boride, and high energy is required for the formation process.
[0006] For these reasons, there is a need for a technology that can produce articles mainly composed of silicon carbide using additive manufacturing, without using organic materials such as resins, and with less energy than conventional methods. [Means for solving the problem]
[0007] A first embodiment of the present invention is a method for manufacturing an article mainly composed of silicon carbide, comprising multiple steps of forming a layer of raw material powder and irradiating the layer with a laser based on data from a three-dimensional model, wherein the raw material powder is a mixed powder of silicon carbide powder, metallic silicon powder, and carbon powder, with silicon carbide powder present in a proportion of 60 at% or more and less than 100 at%, and the spatial laser power density of the laser in the laser irradiation step is 11 J / mm². 3 More than 50J / mm 3 The following characteristics apply:
[0008] Furthermore, a second embodiment of the present invention is a raw material powder for producing an article mainly composed of silicon carbide using a powder bed fusion bonding method, wherein the raw material powder is a mixed powder of silicon carbide powder, metallic silicon powder, and carbon powder, and is characterized in that it contains silicon carbide powder in a proportion of 60 at% or more and less than 100 at%. [Effects of the Invention]
[0009] According to the present invention, articles mainly composed of silicon carbide can be manufactured by powder bed fusion bonding using less energy than conventional methods, without using organic materials such as resins. [Brief explanation of the drawing]
[0010] [Figure 1] This is a schematic diagram of the apparatus according to the present invention. [Figure 2] (a) is a schematic diagram showing laser irradiation in a single continuous line, and (b) is a schematic diagram showing the irradiation sequence when the irradiation area is divided into rectangles and laser irradiation is performed discretely. [Figure 3] This diagram shows the relationship between the height of the fabricated object and the spatial laser power density based on the composition of the raw material powder.
BEST MODE FOR CARRYING OUT THE INVENTION
[0011] As one of the methods for producing an article mainly composed of a high melting point inorganic compound, a process called combustion synthesis is known. Combustion synthesis is a simple and economical method in which energy q is applied to (ignite) a part of the powder composed of the constituent elements of the inorganic compound to cause a chemical reaction, and the reaction heat Q generated during the chemical reaction is propagated into the powder as a combustion wave to promote the combination. For example, a combustion reaction in which a compound AB is produced by a chemical reaction between element A and element B is represented by formula (1). In the present invention, the main component of the article means a component that occupies 75 at% or more of the article. A + B + q → AB + Q ···(1)
[0012] q represents the input energy, Q represents the reaction heat, is represented in the unit [KJ / mol], and q < Q. The reaction phenomenon of formula (1) is a very short-time reaction that occurs within 1 second, and the temperature rises explosively. Note that formula (1) represents the stoichiometric relationship in an omitted form.
[0013] When producing silicon carbide, it is preferable to use the chemical reaction between metallic silicon (Si) as A and carbon (C) as B in formula (1).
[0014] If such a combustion synthesis process is applied to the powder bed melting and bonding method, it is expected that a shaped article with a high ratio of a desired inorganic compound can be produced with less energy. However, as described above, since the reaction heat generated in the combustion synthesis process propagates, the chemical reaction does not stay in the portion irradiated with the laser. In addition, since the temperature rises explosively, voids may occur in the sintered body, and it may be difficult to maintain the shape.
[0015] As a result of investigations to solve the above problems, it has been found that by previously adding an appropriate amount of silicon carbide generated by the reaction between metallic silicon and carbon to the powders of metallic silicon and carbon, the propagation of the chemical reaction and the temperature rise can be suppressed within a predetermined region.
[0016] However, the effects expected from the addition of silicon carbide depend on the composition ratio of the metal silicon powder, carbon powder, and silicon carbide powder. When producing silicon carbide, it is advisable to use a powder containing metal silicon, carbon, and silicon carbide as raw material powder, with the silicon carbide content being 80 at% or more. The silicon carbide powder added to the raw material powder suppresses the reactivity between the metal silicon and carbon, and restricts the propagation of the combustion wave associated with combustion synthesis. Furthermore, since silicon carbide absorbs heat and suppresses heat transfer to the surroundings, it is considered possible to perform shaping while confining the explosive temperature rise during shaping to the laser irradiation area. Also, the atomic ratio of carbon contained in the raw material powder is preferably not less than the atomic ratio of the metal silicon. By setting the atomic ratio of carbon to be not less than the atomic ratio of the metal silicon, the carbon remaining without reacting with the metal silicon can be utilized as C for combining with the metal silicon to be impregnated in the solid-phase impregnation process described later.
[0017] Fig. 1 shows an overview of a shaping apparatus 100 that can be suitably used for the powder bed melting and bonding method using the raw material powder according to the present invention. The shaping apparatus 100 is an apparatus for performing shaping using the powder bed melting and bonding method, and has a chamber 101 that can control the internal atmosphere by a gas introduction mechanism 113 and an exhaust mechanism 114. Inside the chamber 101, there are a shaping container 120 for shaping a three-dimensional object and a powder container 121 for accommodating the raw material powder, which is the shaping material (hereinafter, may be simply described as the shaping material or powder). Furthermore, it has a powder layer forming mechanism 106 for spreading the raw material powder accommodated in the powder container 121 over the shaping container 120 to form a powder layer 111.
[0018] The exhaust mechanism 114 may be provided with a pressure adjustment mechanism such as a butterfly valve for adjusting the pressure, or may be a configuration (generally called blow substitution) that can adjust the atmosphere inside the chamber by gas supply and the accompanying pressure increase.
[0019] The bottoms of the shaping container 120 and the powder container 122 can be vertically positioned by the lifting mechanism 108 respectively. The bottom of the shaping container 120 is configured as a stage 107 on which the base plate 121 is installed. The moving direction and the moving amount of the lifting mechanism 108 are controlled by the control unit 115, and the moving amounts of the bottom of the powder container 122 and the stage are determined according to the layer thickness of the powder layer 111 to be formed. Usually, since the lifting mechanism 108 moves up and down at a height of several tens of micrometers, it is desirable that the height resolution be 1 μm or less.
[0020] The base plate 121 is a plate made of a fusible material such as stainless steel. When melting and solidifying the first layer of powder arranged on the plate, its surface is melted together with the shaping material, and a structure for fixing the shaped object to the base plate 121 is formed. Then, during shaping, the position of the shaped object on the base plate 121 can be held so as not to shift. After shaping is completed, the base plate 121 is mechanically separated from the shaped object. In order to improve the adhesion between the base plate and the shaped object, a Ti film may be pre-coated on the shaping surface of the base plate.
[0021] The powder layer forming mechanism 106 has a powder storage part for storing raw powder and a supply mechanism for supplying the raw powder from the powder container 122 to the shaping container 120. Further, in order to level the powder layer to a set thickness on the base plate 121, it has at least one of a squeegee and a roller. In order to increase the density of the obtained shaped object and promote the chemical reaction of the powder, it is preferable to have both a squeegee and a roller, and after adjusting the thickness of the powder layer with the squeegee, pressurize it with the roller to increase the density of the powder layer.
[0022] The molding apparatus 100 further includes an energy beam source 102 for inducing combustion synthesis in the raw material, scanning mirrors 103A and 103B for scanning the energy beam 112 in two axes, and an optical system 104 for focusing the energy beam onto the irradiation area. Since the energy beam 112 is irradiated from outside the chamber 101, the chamber 101 is provided with an introduction window 105 for introducing the energy beam 112 into the chamber. The power density and scanning position of the energy beam are controlled by the control unit 115 according to the data of the three-dimensional model of the object to be molded and the characteristics of the molding material acquired by the control unit 115. In addition, the positions of the molding container 120 and the optical system 104 are adjusted in advance so that the desired beam diameter is obtained on the surface of the powder layer 111. The beam diameter on the surface of the powder layer 111 is preferably 30 to 100 μm as it affects the molding accuracy.
[0023] Galvano mirrors can be suitably used as scanning mirrors 103A and 103B. Since galvano mirrors operate at high speed while reflecting energy beams, it is desirable that they be made of a lightweight material with a low coefficient of thermal expansion.
[0024] Lasers are widely used for the energy beam 112. YAG lasers are often used, but CO2 lasers or semiconductor lasers may also be used. The driving method may be pulsed or continuous irradiation. The laser is preferably selected according to the absorption wavelength of the powder, and it is sufficient if it has wavelengths where the absorption by the powder is 50% or more, and more preferably if it has wavelengths where the absorption is 80% or more.
[0025] There are two methods for controlling the laser irradiation intensity: controlling the in-plane laser power density and controlling the spatial laser power density. In-plane laser power density is the laser irradiation intensity per unit area, and its unit is J / mm². 2 It is expressed as follows. On the other hand, spatial laser power density is the laser irradiation intensity per unit volume, and is expressed in J / mm². 3It is expressed as follows. When forming an object by controlling the film thickness, as in a 3D printer, it is appropriate to consider the spatial laser power density. The spatial laser power density J is expressed by the following equation. J = W / (P × V × D)
[0026] Here, W is the laser irradiation power, P is the laser irradiation pitch, V is the laser scanning speed, and D is the powder application thickness. In a typical device, the outputtable laser power W is 10 to 1000 W, the laser irradiation pitch P is typically 5 to 500 μm, the laser scanning speed is typically 10 to 10000 mm / sec, and the powder application thickness D is typically 5 to 500 μm. When fabricating using the raw material powder of the present invention, the parameters W, P, V, and D are controlled within the above ranges, and the spatial laser power density J is set to 11 to 50 J / mm². 3 You should adjust it within the range of 10 J / mm. 3 This is the energy required to fully melt the powder, with an upper limit of 30 J / mm². 3 This is the region where molding becomes impossible due to the volatilization of the powder.
[0027] During the fabrication process, the base plate 121 is placed on the stage 107, and the inside of the chamber 101 is replaced with an inert gas such as nitrogen or argon. Once the replacement is complete, a powder layer 111 is formed on the base plate 121 by the powder layer formation mechanism 106. The powder layer 111 is formed with a thickness corresponding to the slice pitch, i.e., the layering pitch, of the slice data generated from the three-dimensional shape data of the object to be fabricated. Then, the energy beam 112 is scanned according to the slice data, and the laser is irradiated onto the powder in a predetermined area.
[0028] Once the laser irradiation for one layer based on the slice data is complete, the lifting mechanism 108 lowers the build stage 107 by the layer pitch, and raises the bottom of the material container 122 according to the layer pitch. Then, the powder layer formation mechanism 106 moves the raw material powder from the material container 122 to the build container 120, lays the powder on top of the layer that has been scanned with the energy beam to form a new powder layer, and scans and irradiates with the energy beam 112.
[0029] As described above, in the region irradiated with the energy beam 112, the surface of the layer previously scanned by the energy beam 112 is solidified again. When the area directly below the area irradiated with the energy beam 112 in the new powder layer is an already solidified area, the beam irradiation area of the new powder layer solidifies with the material mixed at the boundary with the previously melted and solidified area and bonds to each other. By repeating these operations, the shaped object 110 can be formed.
[0030] When irradiating the powder layer with a laser, as shown in Fig. 2(b), it is preferable to irradiate discretely by dividing the irradiation area into rectangles. The size of one area divided into rectangles is preferably 5 mm × 5 mm or less, more preferably 2 mm × 2 mm or less. As shown in Fig. 2(a), when the laser is continuously scanned in one stroke, reaction heat accumulates at each folded part, resulting in variations in the composition of the shaped object or the generation of voids. However, if irradiation is performed discretely as shown in Fig. 2(b), the propagation of the combustion wave can be restricted in the in-plane direction, and variations in reaction heat within the shaping plane can be suppressed. The irradiation area does not have to be rectangular and may be polygonal or circular. Even when it is not rectangular, it is preferably 2 25 mm or less per area, 2 more preferably 5 mm or less per area.
[0031] The particle diameter of the particles contained in the raw material powder containing the powder according to the present invention is preferably 0.5 μm or more and 100 μm or less, more preferably 1 μm or more and 70 μm or less. If the particles contained in the raw material powder are within this range, particle fluidity suitable for forming a powder layer during shaping can be obtained, and it becomes possible to shape a fine shaped object. The particle diameter referred to here means the Feret diameter (directional diameter) measured using a microscope.
[0032] Furthermore, the average particle diameter of each of the SiC, Si, and C particles is preferably made smaller for a composition with a higher melting point or sublimation point, and it is preferably in the relationship of C powder < SiC powder < Si powder. By making the particles of C and SiC, which have a high melting point or sublimation point among the raw material powders, smaller, the molten Si can cover the C and SiC particles, promoting the reaction and suppressing sublimation. The average particle diameter referred to here is such that for the various powders contained in the raw material powder in which the SiC, Si, and C powders are mixed, it is advisable to measure the Feret diameter (directional diameter) for at least 1000 particles of each of the various powders using a microscope and obtain the average value. When the SiC, Si, and C powders before mixing are available, or when the powders can be separated by type from the mixed powder, the median diameter measured using a laser diffraction particle size distribution measuring device for each type is taken as the average particle diameter.
[0033] Even when using the raw material powder containing the powder according to the present invention, if the intensity of the laser irradiated is too strong, an explosive reaction will occur. Therefore, in order to prevent an explosive reaction from occurring, it is advisable to control the power density of the laser irradiated to the raw material powder within a predetermined range according to the composition of the raw material powder. Specifically, it is preferable to irradiate the laser to such an extent that Si and C do not completely combine, and Si (melting point 1414 °C), which has a lower melting point than the decomposition point of SiC, 2545 °C, melts and functions as a binder that physically binds other powders. Furthermore, it is also preferable to irradiate the laser to such an extent that an intermediate product SixCy in which a part of the crystal structure of Si is substituted with C is formed. The solidified product bonded by this Si and the shaped product containing SixCy can be converted entirely to SiC by heat treatment later.
[0034] When the produced shaped product contains voids, impregnation may be performed to improve the strength.
[0035] In the case of a SiC shaped product, solid-phase impregnation, liquid-phase impregnation, and gas-phase impregnation are known. Among them, solid-phase impregnation and liquid-phase impregnation are preferable because the strength of the shaped product can be increased relatively easily. In particular, solid-phase impregnation can improve the strength in a short time and is preferable.
[0036] When performing solid-phase impregnation on a SiC object, it is preferable to first support carbon in the voids of the object, and then pour in molten silicon to convert the voids into SiC.
[0037] The solid-phase impregnation procedure involves first immersing the molded object in liquid resin and degassing it in a vacuum to impregnate the voids with the liquid resin. After removing any excess liquid resin from the surface of the molded object, the resin is heated to harden it, and then heated further until it carbonizes, thereby supporting carbon within the voids. Subsequently, the resulting molded object is brought into contact with molten silicon in a vacuum to impregnate the voids with silicon, and the voids can be converted to SiC by heating at 1450-1700°C. After the voids are converted to SiC, excess silicon adheres to the surface of the molded object, but this can be removed by post-treatment such as polishing or etching.
[0038] The resin used to support carbon in the voids of the molded object should not contain metal components. If metal components are present, they will react with silicon in the molded object to form excess compounds. Furthermore, the higher the carbon residue rate of the resin, the higher the SiC ratio in the voids can be. The carbon residue rate of the resin is preferably 50% or more, more preferably 60% or more, and phenolic resin is particularly preferred.
[0039] Furthermore, in order to allow the resin to penetrate the voids, the viscosity of the resin is preferably 1000 mPa·s or less, and more preferably 500 mPa·s or less.
[0040] When liquid-phase impregnation is performed on SiC molded objects, commercially available SiC polymer (polycarbosilane) can be used as the SiC impregnation material. The fabricated object is immersed in the SiC polymer solution, and vacuum degassing is performed to introduce the SiC polymer solution into the voids of the object. After removing excess liquid from the surface of the object, heat treatment is performed in an inert gas at 800 to 1300°C to mineralize the SiC polymer. Since the SiC polymer is a SiC ceramic precursor containing organic matter, approximately 30 wt.% is lost by volatilization during heat treatment. Therefore, the porosity of the object can be reduced by repeating the impregnation and heat treatment process multiple times. The SiC obtained by heat-treating the SiC polymer at 800 to 1300°C has an amorphous structure, but crystallization and hardness can be improved by subsequent heat treatment at around 1600°C. [Examples]
[0041] Examples and comparative examples relating to the present invention will be described below. However, the type, composition, particle size, shape, laser power, etc. of the powder described below should be appropriately changed depending on the configuration of the apparatus to which the invention is applied and various conditions, and this is not intended to limit the invention to the scope of disclosure herein.
[0042] As raw material powders, we used a mixture of SiC powder, Si powder, and C powder. The details of each powder are as follows. SiC: Average particle size 15.0μm Manufactured by Shinano Electric Refining Co., Ltd. (Product name: SSC-A15) Si powder: average particle size 45.0μm Manufactured by Kojun Chemical Laboratory Co., Ltd. (Product name: SIE19PB) C powder: Average particle size is 5.0 μm Manufactured by Kojun Chemical Laboratory Co., Ltd. (Product name: CCE03PB)
[0043] Raw material powders were prepared by varying the mixing ratio of SiC, Si, and C powders, and each raw material powder was irradiated with a laser under multiple laser irradiation conditions (spatial laser power density) to perform fabrication.
[0044] The required amounts of SiC, Si, and C powders were weighed out and mixed in a ball mill.
[0045] The mixed powder was placed in the material container 122, and the chamber was evacuated and Ar gas was introduced multiple times to replace the chamber with an N2 atmosphere. The raw material powder from the powder container 122 was spread to a uniform thickness on the stainless steel base plate 121 placed on the stage 107 by the powder layer forming mechanism 106. The height of the stage 107 was adjusted so that the powder thickness was 50 μm.
[0046] Next, the powder was irradiated with a laser to perform the fabrication process. An Nd:YAG laser with a wavelength of 1060 nm was used. The laser power was set to 100 W, the irradiation pitch to 40 μm, and the scanning speed was adjusted to achieve a spatial laser power density of 11–75 J / mm². 3 The dimensions were varied within the specified range, and the object was fabricated according to a three-dimensional model of a rectangular prism measuring 4mm x 4mm x 250μm. After the first layer of laser irradiation was completed, the powder was spread and laser irradiation was performed in the same manner as the first layer, and this process was repeated until the fabricated object reached the desired height.
[0047] As a comparative example, a raw material powder consisting of SiC powder was subjected to a spatial laser power density of 11-50 J / mm². 3 The laser was irradiated within the specified range, and the fabrication process was carried out in the same manner as in the example.
[0048] Because the stainless steel used for the base plate has high thermal conductivity, the heat generated by the laser will dissipate if the irradiation energy is low. If the irradiation energy of the laser is low, the adhesion between the printed object and the base plate will be poor. Therefore, before starting the printing of a rectangular prism model, the spatial laser power density should be set to 100 J / mm². 3 I created three layers of material, and then created a base for creating the rectangular prism model.
[0049] The height of the fabricated object was measured without separating it from the plate. Figure 3 shows the relationship between the height of the fabricated object and the spatial laser power density for each raw material powder composition.
[0050] The feasibility of the fabricated object was evaluated based on the difference between the height of the obtained object and the height of the cube model (250 μm). Table 1 summarizes the mixing ratios of the raw material powders 1-9 used for fabrication, the spatial laser power density of the irradiation laser, and the evaluation results. The evaluation criteria are as follows. "—" in the table indicates that the criteria were not yet considered. A: Height is 200 μm or more B: Height is between 170 μm and less than 200 μm C: Height less than 170 μm D: Unable to create shapes.
[0051] In the Grade A printed object, the amount of material loss per layer due to laser irradiation is kept to a level where the powder melts and the density increases. In the Grade B printed object, although the amount of material loss is greater than in Grade A, the explosive temperature rise due to combustion synthesis is suppressed, and the scattering of raw material powder from the build area is suppressed, making it possible to create the desired object by adjusting the slice data and build conditions. In Grade C, the explosive temperature rise due to combustion synthesis could not be suppressed, the raw material powder volatilized, and insufficient powder remained in the build area. As a result, the build accuracy was extremely low not only in the height direction but also in the build surface direction. In Grade D, the powder did not melt, and build was not possible.
[0052] In Table 1, each powder contains metallic silicon powder and carbon powder in the same atomic ratio, but a deviation of approximately ±10% from the target atomic ratio is acceptable.
[0053] [Table 1]
[0054] SiC has no melting point and decomposes at 2545°C, while the decomposition point of C powder, a constituent element of SiC, is 3642°C, and the melting point of Si powder is 1414°C. Powders 1 to 9 were irradiated with a laser under conditions that caused combustion synthesis of Si and C and increased the temperature to melt the Si powder. Powders 1 to 6 were irradiated with a spatial laser power density of 11.1 [J / mm²]. 3 The composition of the fabricated objects, created by irradiating them with a laser, was confirmed by X-ray diffraction. In all fabricated objects, the SiC powder was bonded with Si in some parts, and the Si diamond lattice was partially replaced by C atoms. 0.98 C 0.02 It was confirmed that the part included the following.
[0055] With a mixing ratio of powders 1 to 6, the spatial laser power density was 15 [J / mm²]. 3 Then, four rectangular objects measuring 4mm x 3mm x 40mm were fabricated on a stainless steel base plate.
[0056] For two of the four printed objects on the base plate, a sufficient amount of liquid phenolic resin (Sumitomo Bakelite PR-50607B) was first dropped onto the objects, and then degassed in a vacuum. After wiping off the excess phenolic resin from the surface of the objects, the objects were heated to 160°C on a hot plate to heat-cur the phenolic resin.
[0057] Subsequently, the printed object was separated from the base plate using a diamond wire saw. Microscopic observation of the cut surface of the phenolic resin-impregnated object confirmed that the phenolic resin had sufficiently permeated the voids. Furthermore, no chipping occurred in the object when it was separated from the base plate.
[0058] On the other hand, some of the printed objects that were not impregnated with phenolic resin developed small chips at the edges when separated from the base plate. The objects that were not impregnated with phenolic resin were used for strength comparison with the objects that were impregnated, so no further processing was performed on them.
[0059] The molded object impregnated with phenolic resin was immersed in liquid phenolic resin, degassed under vacuum, and then re-impregnated. Finally, the phenolic resin was carbonized by heat treatment at 800°C for 30 minutes.
[0060] After carbonization of the phenolic resin, the volume and weight of the fabricated object were measured, and the porosity was determined. From the measured porosity, the amount of Si required for SiC impregnation was calculated. φ2mm alumina balls were placed on the bottom of the crucible as a setter to prevent the fabricated object from sticking to the crucible. The fabricated object was then placed in the crucible, and approximately 20% more Si pieces than the calculated required amount were placed on top of it. Heat treatment was then performed. The heat treatment was carried out at 1500°C for 1 hour in an Ar atmosphere at a pressure of 2600 Pa. Since excess Si adhered to the surface of the fabricated object, it was reshaped into a 4mm x 3mm x 40mm strip by grinding and polishing. Microscopic observation of the surface of the impregnated fabricated object revealed a significant reduction in cracks and holes.
[0061] Four-point bending tests were performed on both the unimpregnated and solid-phase-impregnated molded objects using an Instron universal tester (model 4507, load cell 1KN). The evaluation conditions are as follows. Atmosphere: In the air Crosshead travel speed: 0.5 mm / min Distance between support points: L=30 Jig material: SiC
[0062] When comparing the values of four-point bending tests on objects manufactured under the same manufacturing conditions, specifically those with solid-phase impregnation and those without, it was confirmed that in both cases, solid-phase impregnation increased the bending strength of the manufactured objects by more than four times.
[0063] After performing a four-point bending test evaluation, the composition of the solid-phase impregnated fabricated objects was confirmed using the X-ray beam method. It was found that all fabricated objects contained 75 at% or more SiC and 25 at% or less Si.
[0064] From the above results, it was confirmed that by adding an appropriate amount of silicon carbide powder to a raw material powder containing metallic silicon powder and carbon powder, and controlling the spatial laser power density irradiated according to the mixing ratio of the raw material powders, the explosive reaction heat caused by combustion synthesis can be suppressed, making fabrication possible.
[0065] Specifically, the raw material powder contains silicon carbide powder in a proportion of 60 at% to less than 100 at%, and the spatial laser power density is 11 J / mm². 3 More than 50J / mm 3 The following lasers should be used for irradiation. Furthermore, the laser should contain silicon carbide powder in a ratio of 75 at% to 95 at% and have a spatial laser power density of 15 J / mm². 3 More than 35J / mm 3 It is preferable to irradiate with the following lasers.
[0066] By performing the molding process within this range, it is possible to provide the heat necessary to trigger reactions between elements or compounds, while suppressing the explosive reaction heat caused by combustion synthesis, thereby manufacturing a molded object primarily composed of silicon carbide.
[0067] Once the fabrication process was complete, the object was separated from the base plate and heat-treated in an Ar atmosphere at 1500°C for 1 hour. X-ray diffraction of the treated object confirmed that this heat treatment caused the Si to molten and react with the remaining C powder within the object, converting it to SiC. Since the 1500°C heat treatment temperature is significantly lower than the decomposition temperature of SiC and C, no decomposition of SiC and C occurred, resulting in a dense object. [Explanation of symbols]
[0068] 100 Modeling equipment 107 Modeling Stage 110 Sculptures 111 Powder bed 112 Energy Beam
Claims
1. 1. A method for producing a silicon carbide based article, comprising: forming a layer of raw material powder; irradiating the layer with a laser based on data of a three-dimensional model; multiple times, the raw material powder is a mixed powder of silicon carbide powder, metallic silicon powder, and carbon powder, and contains the silicon carbide powder in a ratio of 60 at% or more and less than 100 at%, A method for manufacturing an article, characterized in that the average particle size of the silicon carbide powder is smaller than the average particle size of the silicon metallic powder, and the average particle size of the carbon powder is smaller than the average particle size of the silicon carbide powder.
2. 2. The method for manufacturing an article according to claim 1, wherein the raw material powder contains the silicon carbide powder in a ratio of 75 at % or more and 95 at % or less.
3. 3. The method for manufacturing an article according to claim 1, wherein the atomic ratio of carbon powder contained in the raw material powder is equal to or greater than the atomic ratio of metallic silicon.
4. 4. The method for manufacturing an article according to claim 1, wherein in the step of irradiating the laser, an irradiation area to be irradiated with the laser is divided into a plurality of areas, and the laser is irradiated discretely.
5. The method for manufacturing an article as described in claim 4, characterized in that the spatial laser power density of the laser in the laser irradiation step is 11 J / mm 3 or more and 50 J / mm 3 or less, and the multiple regions are each a rectangular region of 5 mm x 5 mm or less.
6. a step of impregnating a shaped object obtained by carrying out the step of forming a layer of the raw material powder and the step of irradiating with the laser a plurality of times with a liquid resin; a step of heating the shaped object impregnated with the liquid resin to carbonize the resin; impregnating the shaped object obtained by carbonizing the resin with molten metallic silicon; heating the shaped article impregnated with the metallic silicon to convert the metallic silicon into silicon carbide; The method of claim 1 , further comprising:
7. The method for producing an article according to claim 6, wherein the resin is a phenolic resin.
8. 8. The method for manufacturing an article according to claim 6, further comprising a step of post-treating a surface of the obtained shaped article after the step of converting the silicon metal into silicon carbide.
9. A raw material powder for producing an article mainly composed of silicon carbide, comprising: The raw material powder is a mixed powder of silicon carbide powder, metallic silicon powder, and carbon powder, The silicon carbide powder is contained in an amount of 60 at% or more and less than 100 at%, A raw material powder, wherein an average particle size of the silicon carbide powder is smaller than an average particle size of the silicon metal powder, and an average particle size of the carbon powder is smaller than an average particle size of the silicon carbide powder.
10. 10. The raw material powder according to claim 9, wherein the atomic ratio of carbon contained in the raw material powder is equal to or greater than the atomic ratio of metallic silicon.
11. 11. The raw material powder according to claim 9, wherein the particle diameter of the particles contained in the raw material powder is 0.5 μm or more and 100 μm or less.
12. A raw material powder according to any one of claims 9 to 11, characterized in that the metallic silicon powder is contained in an amount of 2.5% or more and 20 at % or less.
13. A raw material powder described in any one of claims 9 to 12, characterized in that the carbon powder is contained in a proportion of 2.5% or more and 20 at % or less.