Printed wiring board and method for manufacturing printed wiring board

JP2022075514A5Active Publication Date: 2024-10-02GOO CHEM IND
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2021156997
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-11-06
Filing Date
2021-09-27
Publication Date
2024-10-02
Estimated Expiration
2041-09-27

AI Technical Summary

Technical Problem

Existing printed wiring boards face issues with via conduction reliability due to tapered vias, which can lead to cracks and reduced conductivity.

Method used

A printed wiring board design incorporating a negative-type interlayer insulating layer composed of a carboxyl group-containing resin, an unsaturated compound with ethylenically unsaturated bonds, and a photopolymerization initiator, featuring a via hole with a reduced diameter portion and a larger diameter end, optimized through specific exposure and development processes.

Benefits of technology

The design enhances via conduction reliability by minimizing stress concentration and reducing the likelihood of conductor cracks, ensuring stable electrical connections between conductor layers.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide a printed wiring board including a via having high conduction reliability.SOLUTION: A printed wiring board 11 includes a first conductor layer 8, a second conductor layer 3, an interlayer insulating layer 7, a via hole 6 penetrating through the interlayer insulating layer 7, and a via conductor 9 arranged in the via hole 6. The interlayer insulating layer 7 is a cured product of a negative type photosensitive resin composition containing a carboxyl group-containing resin (A), an unsaturated compound (B) having at least one ethylenically unsaturated bond in one molecule, and a photopolymerization initiator (C). The via hole 6 has a first end 61 on the side of the first conductor layer 8, a second end 62 on the side of the second conductor layer 3, and a small diameter part 63 that is between the first end 61 and the second end 62 and has a diameter smaller than the second end 62.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure generally relates to printed wiring boards and methods for manufacturing printed wiring boards, and more particularly to printed wiring boards having an interlayer insulating layer with via holes and via conductors, and methods for manufacturing the printed wiring boards.

Background Art

[0002] In a printed wiring board, vias may be formed in an interlayer insulating layer.

[0003] For example, Patent Document 1 discloses a method for manufacturing a multilayer printed wiring board, including a step of irradiating a plastic film adhered to the surface of an insulating layer containing 35% by mass or more of an inorganic filler with a carbon dioxide laser to form blind vias having a top diameter of 100 μm or less.

Prior Art Documents

Patent Documents

[0004]

Patent Document 1

Summary of the Invention

Problems to be Solved by the Invention

[0005] However, according to the findings of the inventors, the invention described in Patent Document 1 has room for improvement in the conduction reliability of vias. Taper - shaped vias are likely to have reduced conduction reliability.

[0006] Through research and development on the material of the interlayer insulating layer, the inventors have obtained the finding that cracks may occur in the conductors of the vias in the interlayer insulating layer, which deteriorates the conduction reliability.

[0007] An object of the present disclosure is to provide a printed wiring board having vias with high conduction reliability and a method for manufacturing the printed wiring board.

Means for Solving the Problems

[0008] A printed circuit board according to one aspect of the present disclosure comprises a first conductor layer, a second conductor layer, an interlayer insulating layer interposed between the first conductor layer and the second conductor layer, via holes penetrating the interlayer insulating layer, and via conductors disposed within the via holes and providing electrical conductivity between the first conductor layer and the second conductor layer. The interlayer insulating layer is a cured product of a negative-type photosensitive resin composition containing a carboxyl group-containing resin (A), an unsaturated compound (B) having at least one ethylenically unsaturated bond in one molecule, and a photopolymerization initiator (C). The via hole has a first end which is the end on the first conductor layer side, a second end which is the end on the second conductor layer side, and a small-diameter portion located between the first end and the second end and having a diameter smaller than the diameter of the second end.

[0009] A method for manufacturing a printed circuit board according to one aspect of the present disclosure is a method for manufacturing the printed circuit board, comprising: preparing a negative-type photosensitive resin composition containing the carboxyl group-containing resin (A), an unsaturated compound (B) having at least one ethylenically unsaturated bond in one molecule, and a photopolymerization initiator (C), and a substrate having an insulating layer and a second conductor layer overlapping the insulating layer; placing a film made from the photosensitive resin composition on the substrate so as to cover the second conductor layer; exposing a negative pattern-like region of the film including the via hole pattern, and then developing it using an alkaline aqueous solution to produce the interlayer insulating layer and the via holes penetrating the interlayer insulating layer. [Effects of the Invention]

[0010] According to one aspect of this disclosure, a printed circuit board having vias with high conductivity and a method for manufacturing the printed circuit board can be provided. [Brief explanation of the drawing]

[0011] [Figure 1] Figures 1A, 1B, 1C, 1D, and 1E are cross-sectional views illustrating the process of manufacturing printed circuit boards. [Modes for carrying out the invention]

[0012] (1) Overview One embodiment relating to this disclosure will be described below.

[0013] The printed circuit board 11 according to this embodiment comprises a first conductor layer 8, a second conductor layer 3, an interlayer insulating layer 7 interposed between the first conductor layer 8 and the second conductor layer 3, via holes 6 penetrating the interlayer insulating layer 7, and via conductors 9 disposed within the via holes 6 to provide electrical conductivity between the first conductor layer 8 and the second conductor layer 3 (see Figure 1E). The interlayer insulating layer 7 is a cured product of a negative-type photosensitive resin composition containing a carboxyl group-containing resin (A), an unsaturated compound (B) having at least one ethylenically unsaturated bond in one molecule, and a photopolymerization initiator (C). The via hole 6 has a first end 61 which is the end on the first conductor layer 8 side, a second end 62 which is the end on the second conductor layer 3 side, and a small-diameter portion 63 located between the first end 61 and the second end 62 and having a diameter smaller than the diameter of the second end 62.

[0014] In this embodiment, an interlayer insulating layer 7 is prepared from a negative-type photosensitive resin composition containing a carboxyl group-containing resin (A), an unsaturated compound (B) having at least one ethylenically unsaturated bond in one molecule, and a photopolymerization initiator (C). Therefore, by exposing the film 4 prepared from the photosensitive resin composition in a patterned manner and then developing it with an alkaline aqueous solution, the interlayer insulating layer 7 can be prepared, and via holes 6 having small diameter portions 63 can be easily created.

[0015] The reason why the small-diameter portion 63 is easily formed is presumed to be as follows: When light is irradiated onto the surface of the film 4 formed from a negative-type photosensitive resin composition on which the first end 61 of the via hole 6 is formed, the film 4 is exposed, and the light is scattered inside the film 4, causing the wider areas to harden as you get closer to the depths of the film 4. As a result, the unhardened portion 5 that becomes the via hole 6 gradually becomes smaller, making it easier to form a small-diameter portion 63 with a diameter smaller than the first end 61. Furthermore, in the deeper parts of the film 4, light is absorbed by the film 4, making it difficult for light to reach the film, and the effect of light scattering is reduced, so the hardening of the film 4 does not progress easily. As a result, the diameter of the second end 62 becomes larger than the diameter of the small-diameter portion 63, and the via hole 6 tends to have a shape that widens from the small-diameter portion 63 to the second end 62.

[0016] In particular, it is preferable that the photosensitive resin composition has the characteristic that when a film 4 with a thickness of 5 μm to 100 μm is made from the photosensitive resin composition, ultraviolet light having spectral intensity at at least one wavelength in the wavelength range of 365 nm ± 65 nm is irradiated to the region of the film 4 excluding the circular portion with a diameter of 5 μm to 100 μm, and then the film 4 is developed with an alkaline aqueous solution, via holes 6 are formed in the circular portion, and the via holes 6 have a small diameter portion 63. In this case, it is preferable that the diameter of the small diameter portion 63 of the via hole 6 is 65% or more and less than 100% of the diameter of the second end 62, the diameter of the first end 61 is 65% or more of the diameter of the second end 62, and the diameter of the first end 61 is 100 μm or less. Such characteristics can be realized within the range of the composition of the photosensitive resin composition, which will be described in detail later. The method of irradiating the film 4 with ultraviolet light may be an exposure method using a negative mask, or a direct drawing method. Examples of specific test methods and conditions are described in the Examples section.

[0017] In addition, in the present embodiment, since the via hole 6 has such a shape, even if stress is generated in the via conductor 9 due to heat load or the like applied to the via conductor 9, cracks are unlikely to occur at the interface between the via conductor 9 and the second conductor layer 3. Therefore, a good conduction reliability between the first conductor layer 8 and the second conductor layer 3 is easily obtained by the via. This is presumably because, in the present embodiment, as described above, the inner surface of the via hole 6 of the interlayer insulating layer 7 has a shape in which the diameter increases from the small-diameter portion 63 to the second end 62, so that even if stress is generated in the via conductor 9, the stress is more likely to concentrate on the small-diameter portion 63 than on the second end 62 of the via.

[0018] The minimum diameter of the small-diameter portion 63 is preferably 65% or more and less than 100% of the diameter of the second end 62. In this case, conduction reliability by the via is particularly easily obtained. The minimum diameter of the small-diameter portion 63 is more preferably 95% or less of the diameter of the second end 62, and even more preferably 90% or less. Also, the minimum diameter of the small-diameter portion 63 is more preferably 67% or more of the diameter of the second end 62, and even more preferably 79% or more.

[0019] The diameter of the first end 61 is preferably 65% or more with respect to the diameter of the second end 62. In this case, by allowing the plating solution to penetrate into the via hole 6, it becomes easier to fabricate the via conductor 9. That is, it is easy to fabricate the via conductor 9 by the plating method. Therefore, better conduction reliability is more easily obtained. From the viewpoint of obtaining good resolution when fabricating the via hole 6, the diameter of the first end 61 is more preferably 70% or more with respect to the diameter of the second end 62, even more preferably 75% or more, and particularly preferably 80% or more. Also, the diameter of the first end 61 is preferably less than 130% with respect to the diameter of the second end 62, more preferably less than 120%, even more preferably less than 110%, and particularly preferably less than 100%.

[0020] Also, the diameter of the first end 61 is preferably 100 μm or less. In this case, it becomes easier to fabricate the via conductor 9 in the via hole 6 by the plating method or the like. Therefore, better conduction reliability is more easily obtained. Also, the diameter of the first end 61 is, for example, 5 μm or more.

[0021] (2) Photosensitive resin composition Hereinafter, the details of the photosensitive resin composition of the present embodiment will be specifically described. In the following description, "(meth)acryl" means at least one of "acryl" and "methacryl". For example, (meth)acrylate means at least one of acrylate and methacrylate.

[0022] The photosensitive resin composition according to the present embodiment contains a carboxyl group-containing resin (A), an unsaturated compound (B) having at least one ethylenically unsaturated bond in one molecule, and a photopolymerization initiator (C).

[0023] The carboxyl group-containing resin (A) preferably contains a carboxyl group-containing resin (A1) having a bisphenol fluorene skeleton represented by the following formula (1). When the carboxyl group-containing resin (A) has a bulky bisphenol fluorene skeleton, when the film 4 formed from the photosensitive resin composition is irradiated with ultraviolet rays, light scattering hardly occurs in the deep part. Further, since the carboxyl group-containing resin (A1) has a bisphenol fluorene skeleton, high heat resistance and insulation reliability can be imparted to the cured product of the photosensitive resin composition.

[0024] [Chemical formula]

[0025] In formula (1), R1 to R8 are each independently hydrogen, an alkyl group having 1 to 5 carbon atoms, or a halogen. That is, each of R1 to R8 in formula (1) may be hydrogen, but may also be an alkyl group having 1 to 5 carbon atoms or a halogen. Even if the hydrogen in the aromatic ring is substituted with a low molecular weight alkyl group or a halogen, it does not adversely affect the physical properties of the carboxyl group-containing resin (A1). On the contrary, in some cases, the heat resistance or flame retardancy of the cured product of the photosensitive resin composition containing the carboxyl group-containing resin (A1) is improved by the substitution.

[0026] The carboxyl group-containing resin (A1) can be synthesized, for example, by reacting an epoxy compound (a1) having a bisphenol fluorene skeleton represented by formula (1) with an unsaturated group-containing carboxylic acid (a2), and then reacting the resulting intermediate with an acid anhydride (a3).

[0027] The epoxy compound (a1) has a structure as shown in formula (2) below, for example. In formula (2), n is an integer in the range of 0 to 20. In order to appropriately control the molecular weight of the carboxyl group-containing resin (A1), it is more preferable that the average of n is in the range of 0 to 1. If the average of n is in the range of 0 to 1, an excessive increase in the molecular weight of the carboxyl group-containing resin (A1) is easily suppressed. In formula (2), R1 to R8 are each independently hydrogen, an alkyl group having 1 to 5 carbon atoms, or a halogen.

[0028] [ka]

[0029] Unsaturated group-containing carboxylic acids (a2) include, for example, compounds that have only one ethylenically unsaturated group in a single molecule. More specifically, the unsaturated group-containing carboxylic acid (a2) contains, for example, at least one compound selected from the group consisting of acrylic acid, methacrylic acid, ω-carboxy-polycaprolactone (n≒2) monoacrylate, crotonic acid, cinnamic acid, 2-acryloyloxyethyl succinic acid, 2-methacryloyloxyethyl succinic acid, 2-acryloyloxyethyl phthalic acid, 2-methacryloyloxyethyl phthalic acid, 2-acryloyloxypropyl phthalic acid, 2-methacryloyloxypropyl phthalic acid, 2-acryloyloxyethyl maleic acid, 2-methacryloyloxyethyl maleic acid, β-carboxyethyl acrylate, 2-acryloyloxyethyl tetrahydrophthalic acid, 2-methacryloyloxyethyl tetrahydrophthalic acid, 2-acryloyloxyethyl hexahydrophthalic acid, and 2-methacryloyloxyethyl hexahydrophthalic acid. Preferably, the unsaturated group-containing carboxylic acid (a2) contains acrylic acid. Furthermore, if the unsaturated group-containing carboxylic acid (a2) contains acrylic acid, it is preferable that the acrylic acid is present in 50 mol% or more of the unsaturated group-containing carboxylic acid (a2), more preferably 80 mol% or more, even more preferably 85 mol% or more, and particularly preferably 90 mol% or more.

[0030] Appropriate methods can be used to react the epoxy compound (a1) with the unsaturated group-containing carboxylic acid (a2). For example, a reactive solution can be obtained by adding the unsaturated group-containing carboxylic acid (a2) to a solvent solution of the epoxy compound (a1), and then adding a thermal polymerization inhibitor and a catalyst as needed, and stirring and mixing. An intermediate can be obtained by reacting this reactive solution by a conventional method at a temperature preferably between 60°C and 150°C, more preferably between 80°C and 120°C. The solvent in this case can contain at least one component selected from the group consisting of ketones such as methyl ethyl ketone and cyclohexanone, aromatic hydrocarbons such as toluene and xylene, and acetate esters such as ethyl acetate, butyl acetate, cellosolve acetate, butyl cellosolve acetate, carbitol acetate, butyl carbitol acetate, propylene glycol monomethyl ether acetate, and dialkyl glycol ethers. The thermal polymerization inhibitor may contain at least one component selected from the group consisting of, for example, hydroquinone, methylhydroquinone, and hydroquinone monomethyl ether. The catalyst may contain at least one component selected from the group consisting of, for example, tertiary amines such as benzyldimethylamine and triethylamine, quaternary ammonium salts such as trimethylbenzylammonium chloride and methyltriethylammonium chloride, triphenylphosphine, and triphenylstybin.

[0031] It is preferable that the catalyst contains triphenylphosphine. That is, it is preferable to react the epoxy compound (a1) with the unsaturated group-containing carboxylic acid (a2) in the presence of triphenylphosphine. In this case, the ring-opening addition reaction between the epoxy group in the epoxy compound (a1) and the unsaturated group-containing carboxylic acid (a2) is particularly promoted, and a reaction rate (conversion rate) of 95% or more, 97% or more, or nearly 100% can be achieved.

[0032] It is also preferable to react the epoxy compound (a1) with the unsaturated group-containing carboxylic acid (a2) under air bubbling. In this case, the addition polymerization reaction of the unsaturated group can be suppressed, thereby preventing an increase in the molecular weight of the intermediate and gelation of the intermediate solution. Furthermore, excessive discoloration of the final product, the carboxyl group-containing resin (A1), can be suppressed.

[0033] When reacting epoxy compound (a1) with unsaturated group-containing carboxylic acid (a2), the amount of unsaturated group-containing carboxylic acid (a2) per mole of epoxy group in epoxy compound (a1) is preferably 0.8 moles or more and 1.2 moles or less. In this case, a photosensitive resin composition with excellent photosensitivity and stability can be obtained.

[0034] The intermediate thus obtained comprises a hydroxyl group produced by the reaction between the epoxy group of the epoxy compound (a1) and the carboxyl group of the unsaturated group-containing carboxylic acid (a2).

[0035] Next, the intermediate is reacted with acid anhydride (a3). Acid anhydride (a3) ​​contains, for example, acid dianhydride (a4).

[0036] Acidic dianhydride (a4) is a compound having two acid anhydride groups. Acidic dianhydride (a4) can contain tetracarboxylic anhydrides. Examples of acidic dianhydride (a4) include 1,2,4,5-benzenetetracarboxylic dianhydride, benzophenone tetracarboxylic dianhydride, methylcyclohexene tetracarboxylic dianhydride, tetracarboxylic dianhydride, naphthalene-1,4,5,8-tetracarboxylic dianhydride, ethylene tetracarboxylic dianhydride, 9,9'-bis(3,4-dicarboxyphenyl)fluorene dianhydride, glycerin bis-anhydrotrimellitate monoacetate, and ethylene The composition may contain at least one compound selected from the group consisting of glycol bis-anhydrotrimellitate, 3,3',4,4'-diphenylsulfontetracarboxylic dianhydride, 1,3,3a,4,5,9b-hexahydro-5(tetrahydro-2,5-dioxo-3-furanyl)naphtho[1,2-c]furan-1,3-dione, 1,2,3,4-butanetetracarboxylic dianhydride, and 3,3',4,4'-biphenyltetracarboxylic dianhydride. In particular, it is preferable that the acid dianhydride (a4) contains 3,3',4,4'-biphenyltetracarboxylic dianhydride. In this case, the photosensitive resin composition can suppress the tackiness of the film 4 produced from the photosensitive resin composition while ensuring good developability, and can also improve the insulation reliability and plating resistance of the cured product.

[0037] Acid anhydride (a3) ​​may contain acid monoanhydride (a5). Acid monoanhydride (a5) is a compound having one acid anhydride group. Acid monoanhydride (a5) can contain dicarboxylic acid anhydrides. Acid monoanhydride (a5) can contain one or more compounds selected from the group consisting of, for example, phthalic anhydride, 1,2,3,6-tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylnadic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, succinic anhydride, methylsuccinic anhydride, maleic anhydride, citraconic anhydride, glutaric anhydride, cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride, and itaconic anhydride. It is particularly preferable that acid monoanhydride (a5) contains 1,2,3,6-tetrahydrophthalic anhydride. In other words, it is preferable that the acid anhydride (a3) ​​contains 1,2,3,6-tetrahydrophthalic anhydride. In this case, while ensuring good developability of the photosensitive resin composition, the tackiness of the film 4 formed from the photosensitive resin composition can be further suppressed, and the insulation reliability and plating resistance of the cured product can be further improved. The amount of 1,2,3,6-tetrahydrophthalic anhydride relative to the total acid anhydride (a5) is preferably in the range of 20 mol% to 100 mol%, and more preferably in the range of 40 mol% to 100 mol%, but is not limited thereto.

[0038] Various methods can be used to react the intermediate with the acid anhydride (a3). For example, a reactive solution is obtained by adding the acid anhydride (a3) ​​to a solvent solution of the intermediate, and then adding a thermal polymerization inhibitor and a catalyst as needed, and stirring. This reactive solution is reacted by conventional methods, more preferably at a temperature of 60°C to 150°C, and particularly preferably at 80°C to 120°C, to obtain a carboxyl group-containing resin (A1) having a bisphenol fluorene skeleton. Suitable solvents, catalysts, and polymerization inhibitors can be used, and the solvents, catalysts, and polymerization inhibitors used in the synthesis of the intermediate can also be used as is.

[0039] It is preferable that the catalyst contains triphenylphosphine. That is, it is preferable to react the intermediate with the acid anhydride (a3) ​​in the presence of triphenylphosphine. In this case, the reaction between the intermediate and the acid anhydride (a3) ​​is particularly promoted, and a reaction rate (conversion rate) of 90% or more, 95% or more, 97% or more, or nearly 100% can be achieved.

[0040] When the acid anhydride (a3) ​​contains an acid dianhydride (a4), the amount of acid dianhydride (a4) per mole of epoxy group of epoxy compound (a1) is preferably 0.05 moles or more and 0.24 moles or less. In this case, a carboxyl group-containing resin (A1) having a bisphenol fluorene skeleton with appropriately adjusted acid value and molecular weight can be easily obtained.

[0041] Furthermore, if the acid anhydride (a3) ​​further contains an acid monoanhydride (a5), it is preferable that the amount of acid monoanhydride (a5) is 0.3 moles or more and 0.7 moles or less per mole of epoxy groups of the epoxy compound (a1). In this case, a carboxyl group-containing resin (A1) having a bisphenol fluorene skeleton with appropriately adjusted acid value and molecular weight can be easily obtained.

[0042] It is also preferable to react the intermediate with the acid anhydride (a3) ​​under air bubbling. In this case, excessive molecular weight increase of the resulting carboxyl group-containing resin (A1) having a bisphenol fluorene skeleton is suppressed, which particularly improves the developability of the photosensitive resin composition with an alkaline aqueous solution.

[0043] The components of the photosensitive resin composition other than the carboxyl group-containing resin (A1) having a bisphenol fluorene skeleton will be described below.

[0044] As previously described, the photosensitive resin composition contains a carboxyl group-containing resin (A), an unsaturated compound (B) having at least one ethylenically unsaturated bond in one molecule, and a photopolymerization initiator (C).

[0045] The carboxyl group-containing resin (A) may contain only the carboxyl group-containing resin (A1) having a bisphenol fluorene skeleton, or it may contain only the carboxyl group-containing resin other than the carboxyl group-containing resin (A1) having a bisphenol fluorene skeleton. Alternatively, it may contain both the carboxyl group-containing resin (A1) having a bisphenol fluorene skeleton and the carboxyl group-containing resin other than the carboxyl group-containing resin (A1). The carboxyl group-containing resin other than the carboxyl group-containing resin (A1) having a bisphenol fluorene skeleton includes the carboxyl group-containing resin that does not have a bisphenol fluorene skeleton (hereinafter also referred to as carboxyl group-containing resin (A2)).

[0046] The carboxyl group-containing resin (A2) may contain, for example, a compound having a carboxyl group and not being photopolymerizable (hereinafter referred to as component (A2-1)). Component (A2-1) may contain, for example, a polymer of an ethylenically unsaturated monomer containing an ethylenically unsaturated compound having a carboxyl group. The ethylenically unsaturated compound having a carboxyl group may include compounds such as acrylic acid, methacrylic acid, and ω-carboxy-polycaprolactone (n≒2) monoacrylate. The ethylenically unsaturated compound having a carboxyl group may also include reaction products of pentaerythritol triacrylate, pentaerythritol trimethacrylate, etc., with a dibasic acid anhydride. The ethylenically unsaturated monomer may further contain ethylenically unsaturated compounds that do not have a carboxyl group, such as 2-(meth)acryloyloxyethyl phthalate, 2-(meth)acryloyloxyethyl-2-hydroxyethyl phthalate, and (meth)acrylic acid esters of linear or branched aliphatic or alicyclic groups (which may have some unsaturated bonds in the ring).

[0047] The carboxyl group-containing resin (A2) may contain a compound having a carboxyl group and an ethylenically unsaturated group (hereinafter referred to as component (A2-2)). Alternatively, the carboxyl group-containing resin (A2) may contain only component (A2-2). Component (A2-2) contains, for example, a resin (referred to as the first resin (x)) which is a reaction product of an intermediate, which is a reaction product of an epoxy compound (x1) having two or more epoxy groups in one molecule and an ethylenically unsaturated compound (x2), and at least one compound (x3) selected from the group of polycarboxylic acids and their anhydrides. The first resin (x) is obtained, for example, by adding compound (x3) to an intermediate obtained by reacting the epoxy group in the epoxy compound (x1) with the carboxyl group in the ethylenically unsaturated compound (x2). The epoxy compound (x1) can contain appropriate epoxy compounds such as cresol novolac type epoxy compounds, phenol novolac type epoxy compounds, and biphenyl novolac type epoxy compounds. In particular, the epoxy compound (x1) preferably contains at least one compound selected from the group consisting of biphenyl novolac type epoxy compounds and cresol novolac type epoxy compounds. The epoxy compound (x1) may contain only a biphenyl novolac type epoxy compound, or only a cresol novolac type epoxy compound. In this case, since the main chain of the epoxy compound (x1) contains an aromatic ring, the degree to which the cured product of the photosensitive resin composition is significantly corroded by an oxidizing agent, such as potassium permanganate, can be reduced. The epoxy compound (x1) may also contain a polymer of an ethylenically unsaturated compound (z). The ethylenically unsaturated compound (z) may contain a compound having an epoxy group (z1), such as glycidyl (meth)acrylate, or further contain a compound without an epoxy group (z2), such as 2-(meth)acryloyloxyethyl phthalate. The ethylenically unsaturated compound (x2) preferably contains at least one of acrylic acid and methacrylic acid. Compound (x3) contains one or more compounds selected from the group consisting of polycarboxylic acids such as phthalic acid, tetrahydrophthalic acid, and methyltetrahydrophthalic acid, and anhydrides of these polycarboxylic acids.In particular, compound (x3) preferably contains at least one polycarboxylic acid selected from the group consisting of phthalic acid, tetrahydrophthalic acid, and methyltetrahydrophthalic acid.

[0048] Component (A2-2) may contain a resin (referred to as the second resin (y)) which is a reaction product of a polymer of an ethylenically unsaturated monomer containing an ethylenically unsaturated compound having a carboxyl group and an ethylenically unsaturated compound having an epoxy group. The ethylenically unsaturated monomer may further contain an ethylenically unsaturated compound that does not have a carboxyl group. The second resin (y) is obtained by reacting an ethylenically unsaturated compound having an epoxy group with some of the carboxyl groups in the polymer. The ethylenically unsaturated monomer may further contain an ethylenically unsaturated compound that does not have a carboxyl group. Examples of ethylenically unsaturated compounds having a carboxyl group include acrylic acid, methacrylic acid, ω-carboxy-polycaprolactone (n≒2) monoacrylate, pentaerythritol triacrylate, pentaerythritol trimethacrylate, and the like. Ethylene-unsaturated compounds that do not have a carboxyl group include, for example, 2-(meth)acryloyloxyethyl phthalate, 2-(meth)acryloyloxyethyl-2-hydroxyethyl phthalate, and (meth)acrylic acid esters of linear or branched aliphatic or alicyclic groups (which may have some unsaturated bonds in the ring). Ethylene-unsaturated compounds that have an epoxy group preferably contain glycidyl (meth)acrylate.

[0049] The carboxyl group-containing resin (A) may contain only carboxyl group-containing resin (A1), only carboxyl group-containing resin (A2), or both carboxyl group-containing resin (A1) and carboxyl group-containing resin (A2). Preferably, the carboxyl group-containing resin (A) contains 25% by mass or more of carboxyl group-containing resin (A1), more preferably 40% by mass or more, even more preferably 60% by mass or more, and particularly preferably 100% by mass. In this case, excellent photosensitivity and developability with an alkaline aqueous solution can be ensured for the photosensitive resin composition. Furthermore, the heat resistance and insulation reliability of the cured product of the photosensitive resin composition can be particularly improved. Moreover, the tackiness of the film 4 formed from the photosensitive resin composition can be sufficiently reduced.

[0050] The weight-average molecular weight of the carboxyl group-containing resin (A) is preferably 700 or more and 100,000 or less. When the weight-average molecular weight of the carboxyl group-containing resin (A) is 700 or more, the tackiness of the film 4 formed from the photosensitive resin composition is easily suppressed, and the insulation reliability and plating resistance of the cured product of the photosensitive resin composition can be improved. When the weight-average molecular weight of the carboxyl group-containing resin (A) is 100,000 or less, the developability of the photosensitive resin composition with an alkaline aqueous solution tends to be good. The weight-average molecular weight of the carboxyl group-containing resin (A) is more preferably 900 or more and 60,000 or less, even more preferably 1,200 or more and 10,000 or less, and particularly preferably 1,400 or more and 5,000 or less. The weight-average molecular weight of the carboxyl group-containing resin (A) is calculated, for example, from the measurement results by gel permeation chromatography under the following conditions.

[0051] GPC equipment: SHODEX SYSTEM 11 manufactured by Showa Denko Corporation. Columns: SHODEX KF-800P, KF-005, KF-003, KF-001 (4 in series) Mobile phase: THF, Flow rate: 1ml / min, Column temperature: 45℃, Detector: RI, Conversion: Polystyrene.

[0052] The carboxyl group-containing resin (A) preferably contains a component with an acid value of 65 mg KOH / g or more and 150 mg KOH / g or less. In this case, the developability of the photosensitive resin composition with an alkaline aqueous solution is particularly improved, and by developing the film 4 after exposure with an alkaline aqueous solution, via holes 6 having small diameter portions 63 are particularly easily formed. It is more preferable that the acid value is 70 mg KOH / g or more and 145 mg KOH / g or less, even more preferable that it is 75 mg KOH / g or more and 140 mg KOH / g or less, and particularly preferable that it is 85 mg KOH / g or more and 135 mg KOH / g or less.

[0053] The unsaturated compound (B) can impart photocurability to the photosensitive resin composition. The unsaturated compound (B) may contain at least one compound selected from the group consisting of monofunctional (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, and polyfunctional (meth)acrylates such as diethylene glycol di(meth)acrylate, trimethylolpropane di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, ε-caprolactone-modified pentaerythritol hexaacrylate, and tricyclodecanedimethanol di(meth)acrylate.

[0054] In particular, the unsaturated compound (B) preferably contains a trifunctional compound, that is, a compound having three unsaturated bonds in one molecule. In this case, the resolution when the film 4 formed from the photosensitive resin composition is exposed and developed is improved, and the developability of the photosensitive resin composition with an alkaline aqueous solution is particularly improved. The trifunctional compound may contain at least one compound selected from the group consisting of trimethylolpropane tri(meth)acrylate, EO-modified trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, ethoxylated isocyanurate tri(meth)acrylate, ε-caprolactone-modified tris-(2-acryloxyethyl) isocyanurate, and ethoxylated glycerin tri(meth)acrylate.

[0055] The unsaturated compound (B) may also preferably contain a phosphorus-containing compound (phosphorus-containing unsaturated compound). In this case, the flame retardancy of the cured product of the photosensitive resin composition is improved. Examples of phosphorus-containing unsaturated compounds include 2-methacryloyloxyethyl acid phosphate (specifically, product numbers Light Ester P-1M and Light Ester P-2M from Kyoeisha Chemical Co., Ltd.), 2-acryloyloxyethyl acid phosphate (specifically, product number Light Acrylate P-1A from Kyoeisha Chemical Co., Ltd.), diphenyl-2-methacryloyloxyethyl phosphate (specifically, product number MR-260 from Daihachi Kogyo Co., Ltd.), and the HFA series from Showa Polymer Co., Ltd. (specifically, Diphenyl-2-methacryloyloxyethyl phosphate from Daihachi Kogyo Co., Ltd.). It may contain at least one compound selected from the group consisting of (e.g., catalog numbers HFA-6003 and HFA-6007, which are addition reaction products of pentaerythritol hexaacrylate and HCA (9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide), and catalog numbers HFA-3003 and HFA-6127, which are addition reaction products of caprolactone-modified dipentaerythritol hexaacrylate and HCA (9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide).

[0056] The unsaturated compound (B) may contain a prepolymer. The prepolymer may contain at least one compound selected from the group consisting of, for example, a prepolymer obtained by polymerizing a monomer having an ethylenically unsaturated bond and then adding an ethylenically unsaturated group, and oligo(meth)acrylate prepolymers. The oligo(meth)acrylate prepolymers may contain at least one component selected from the group consisting of, for example, epoxy(meth)acrylate, polyester(meth)acrylate, urethane(meth)acrylate, alkyd resin(meth)acrylate, silicone resin(meth)acrylate, and spiran resin(meth)acrylate.

[0057] The photopolymerization initiator (C) preferably contains a photopolymerization initiator (C1) which includes at least one selected from the group consisting of acylphosphine oxide-based photopolymerization initiators, α-aminoalkylphenone-based photopolymerization initiators, and oxime ester-based photopolymerization initiators. In this case, when the photosensitive resin composition is exposed to ultraviolet light, high light absorption can be imparted to the photosensitive resin composition. When the photosensitive resin composition has good light absorption, light is easily absorbed when the film 4 formed from the photosensitive resin composition is exposed, so photocuring proceeds easily. Furthermore, because light is absorbed within the film 4, the amount of light that reaches the depths is reduced. Therefore, the effects of light scattering in the depths are particularly less likely to occur, and photocuring of the film 4 proceeds particularly slowly in the depths compared to the surface. Therefore, when via holes 6 are fabricated by photolithography, small diameter portions 63 are particularly easily formed.

[0058] The photopolymerization initiator (C1) more preferably contains an acylphosphine oxide-based photopolymerization initiator. In this case, the photosensitive resin composition can be imparted with high light absorption.

[0059] Acylphosphine oxide photopolymerization initiators include, for example, monoacylphosphine oxide photopolymerization initiators such as 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide and 2,4,6-trimethylbenzoyl-ethyl-phenyl-phosphinate, as well as bis-(2,6-dichlorobenzoyl)phenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-2,5-dimethylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-4-propylphenylphosphine oxide, and bis-(2,6-dichlorobenzoyl)-1-naphthylphosphine oxide. The acylphosphine oxide-based photopolymerization initiator may contain at least one component selected from the group consisting of bisacylphosphine oxide-based photopolymerization initiators such as phenyl oxide, bis-(2,6-dimethoxybenzoyl)phenylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,5-dimethylphenylphosphine oxide, bis-(2,4,6-trimethylbenzoyl)phenylphosphine oxide, and (2,5,6-trimethylbenzoyl)-2,4,4-trimethylpentylphosphine oxide. The acylphosphine oxide-based photopolymerization initiator preferably contains at least one of 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide and bis-(2,4,6-trimethylbenzoyl)phenylphosphine oxide, and more preferably contains 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide.

[0060] The α-aminoalkylphenone-based photopolymerization initiator may contain at least one component selected from the group consisting of, for example, 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, and 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone.

[0061] Oxime ester-based photopolymerization initiators may contain at least one component selected from the group consisting of, for example, 1,2-octanedione, 1-[4-(phenylthio)-,2-(O-benzoyl oxime)], ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]-,1-(O-acetyl oxime).

[0062] The photopolymerization initiator (C) may contain a photopolymerization initiator (C2) containing components other than those listed above, in addition to the photopolymerization initiator (C1) containing the above components. The photopolymerization initiator (C2) preferably contains at least one of an α-hydroxyacetophenone-based photopolymerization initiator and a thioxanthone-based photopolymerization initiator. In this case, particularly high light absorption can be imparted to the photosensitive resin composition. It is more preferable that the photopolymerization initiator (C2) contains an α-hydroxyacetophenone-based photopolymerization initiator.

[0063] The α-hydroxyacetophenone-based photopolymerization initiator preferably contains, for example, 1-hydroxycyclohexyl-phenyl ketone.

[0064] The thioxanthone-based photopolymerization initiator preferably contains, for example, 2,4-diethylthioxanthene-9-one.

[0065] It is also preferable that the photopolymerization initiator (C) contains 4,4-bis(diethylamino)benzophenone (C3). That is, it is also preferable that the photosensitive resin composition contains a photopolymerization initiator (C1) and 4,4-bis(diethylamino)benzophenone (C3), or contains a photopolymerization initiator (C1), a photopolymerization initiator (C2), and 4,4-bis(diethylamino)benzophenone (C3). In this case, when the film 4 formed from the photosensitive resin composition is partially exposed and then developed, the hardening of the unexposed portion is particularly easily suppressed. This makes it particularly easy to form via holes 6 having small diameter portions 63.

[0066] The amount of 4,4-bis(diethylamino)benzophenone (C3) is preferably within the range of 0.5% to 20% by mass relative to the photopolymerization initiator (C1). When the amount of 4,4-bis(diethylamino)benzophenone (C3) is 0.5% by mass or more, curing in unexposed areas is particularly easily suppressed. Also, when the amount of 4,4-bis(diethylamino)benzophenone (C3) is 20% by mass or less, the 4,4-bis(diethylamino)benzophenone (C3) is less likely to inhibit the electrical insulation properties of the cured product of the photosensitive resin composition. The amount of bis(diethylamino)benzophenone (C3) is particularly preferably within the range of 1% to 18% by mass relative to the photopolymerization initiator (C1). If the photosensitive resin composition contains an organic filler (E), the organic filler (E) may cause light scattering within the photosensitive resin composition during exposure. In this case, a problem may arise in which good resolution cannot be obtained in the photosensitive resin composition. Therefore, it may be difficult to form a small-diameter portion 63 in the via hole 6. However, if 4,4-bis(diethylamino)benzophenone (C3) is within the above range, the photosensitive resin composition is likely to have good resolution, and therefore the small-diameter portion 63 is particularly likely to form in the via hole 6.

[0067] The photosensitive resin composition preferably contains epoxy resin (D). Epoxy resin (D) can impart thermosetting properties to the photosensitive resin composition. Preferably, epoxy resin (D) contains a crystalline epoxy resin. In this case, the developability of the photosensitive resin composition can be improved. Furthermore, epoxy resin (D) may further contain amorphous epoxy resin. Here, "crystalline epoxy resin" refers to an epoxy resin with a melting point, and "amorphous epoxy resin" refers to an epoxy resin without a melting point.

[0068] The crystalline epoxy resin preferably contains one or more components selected from the group consisting of, for example, 1,3,5-tris(2,3-epoxypropyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, hydroquinone-type crystalline epoxy resin (specifically, product name YDC-1312 from Nippon Steel Chemical & Material Co., Ltd.), biphenyl-type crystalline epoxy resin (specifically, product name YX-4000 from Mitsubishi Chemical Corporation), diphenyl ether-type crystalline epoxy resin (specifically, product name YSLV-80DE from Nippon Steel Chemical & Material Co., Ltd.), bisphenol-type crystalline epoxy resin (specifically, product names YSLV-70XY and YSLV-80XY from Nippon Steel Chemical & Material Co., Ltd.), tetrakisphenolethane-type crystalline epoxy resin (specifically, product name GTR-1800 from Nippon Kayaku Co., Ltd.), and bisphenol fluorene-type crystalline epoxy resin.

[0069] It is preferable that the crystalline epoxy resin has two or more epoxy groups in one molecule. In this case, cracks are less likely to occur in the cured product of the photosensitive resin composition when subjected to repeated temperature changes.

[0070] The crystalline epoxy resin preferably has an epoxy equivalent of 150 g / eq to 300 g / eq. This epoxy equivalent is the gram weight of the crystalline epoxy resin containing 1 gram equivalent of epoxy groups. The crystalline epoxy resin has a melting point. For example, the melting point of the crystalline epoxy resin is between 70°C and 180°C.

[0071] In particular, it is preferable that the epoxy compound (D) contains a crystalline epoxy resin with a melting point of 110°C or lower. In this case, the developability of the photosensitive resin composition with an alkaline aqueous solution is particularly improved. The crystalline epoxy resin with a melting point of 110°C or lower can contain at least one component selected from the group consisting of, for example, biphenyl-type epoxy resin (specifically, product number YX-4000 from Mitsubishi Chemical Corporation), diphenyl ether-type epoxy resin (specifically, product number YSLV-80DE from Nippon Steel Chemical & Material Chemicals Co., Ltd.), bisphenol-type epoxy resin (specifically, product numbers YSLV-70XY and YSLV-80XY from Nippon Steel Chemical & Material Chemicals Co., Ltd.), and bisphenol fluorene-type crystalline epoxy resin.

[0072] Amorphous epoxy resins include, for example, phenol novolac type epoxy resin (specifically, product code EPICLON N-775 from DIC Corporation), cresol novolac type epoxy resin (specifically, product code EPICLON N-695 from DIC Corporation), bisphenol A novolac type epoxy resin (specifically, product code EPICLON N-865 from DIC Corporation), bisphenol A type epoxy resin (specifically, product code jER1001 from Mitsubishi Chemical Corporation), bisphenol F type epoxy resin (specifically, product code jER4004P from Mitsubishi Chemical Corporation), bisphenol S type epoxy resin (specifically, product code EPICLON EXA-1514 from DIC Corporation), bisphenol AD ​​type epoxy resin, biphenyl novolac type epoxy resin (specifically, product code NC-3000 from Nippon Kayaku Co., Ltd.), hydrogenated bisphenol A type epoxy resin (specifically, product code ST-4000D from Nippon Steel Chemical & Material Co., Ltd.), and naphthalene type epoxy resin (specifically, product code EPICLON from DIC Corporation). HP-4032, EPICLON HP-4700, EPICLON HP-4770), Tertiary butylcatechol type epoxy resin (specifically, DIC Corporation's product code EPICLON HP-820), Dicyclopentadiene type epoxy resin (specifically, DIC Corporation's product code EPICLON HP-7200), Adamantane type epoxy resin (specifically, Idemitsu Kosan Co., Ltd.'s product code ADAMANTATEX-E-201), Special bifunctional epoxy resin (specifically, Mitsubishi Chemical Corporation's product codes YL7175-500 and YL7175-1000; DIC Corporation's product codes EPICLON TSR-960, EPICLON TER-601, EPICLON TSR-250-80BX, EPICLON 1650-75MPX, EPICLON EXA-4850, EPICLON EXA-4816, EPICLON EXA-4822, and EPICLON EXA-9726;It is preferable to contain at least one component selected from the group consisting of (product code YSLV-120TE manufactured by Nippon Steel Chemical & Material Co., Ltd.), rubber-like core-shell polymer-modified bisphenol A type epoxy resin (specifically, product code MX-156 manufactured by Kaneka Corporation), rubber-like core-shell polymer-modified bisphenol F type epoxy resin (specifically, product code MX-136 manufactured by Kaneka Corporation), and rubber particle-containing bisphenol F type epoxy resin (specifically, product code KaneAce MX-130 manufactured by Kaneka Corporation).

[0073] When the photosensitive resin composition contains epoxy resin (D), it is preferable that the photosensitive resin composition contains both crystalline epoxy resin and amorphous epoxy resin. In this case, the plating resistance and insulation properties of the cured product made from the photosensitive resin composition can be further improved.

[0074] The epoxy resin (D) may contain a phosphorus-containing epoxy resin. In this case, the flame retardancy of the cured product of the photosensitive resin composition is improved. The phosphorus-containing epoxy resin may be contained in a crystalline epoxy resin or in an amorphous epoxy resin. Examples of phosphorus-containing epoxy resins include phosphorus-modified bisphenol F type epoxy resins (specific examples include product numbers EPICLON EXA-9726 and EPICLON EXA-9710 from DIC Corporation) and product number EPOTOTE FX-305 from Nippon Steel Chemical & Material Co., Ltd.

[0075] It is preferable that the photosensitive resin composition does not contain fillers. In this case, light scattering in the deeper parts of the film 4 is suppressed, making it particularly easier to form via holes 6 having small diameter portions 63. If the photosensitive resin composition contains fillers, it is preferable that the material, particle size, and amount of fillers be appropriately set so that light scattering within the film 4 is moderately reduced.

[0076] The photosensitive resin composition may contain an organic filler (E). Note that the organic filler (E) does not contain melamine. In this case, it is preferable that the material, particle size, and amount of the organic filler (E) are appropriately set as described above. The organic filler (E) imparts thixotropy to the photosensitive resin composition, thereby improving the storage stability of the photosensitive resin composition. Furthermore, the adhesion of the cured product to the plating layer is improved. It is preferable that the organic filler (E) has a reactive group. Having a reactive group allows the organic filler (E) to have high compatibility in the photosensitive resin composition, imparting stronger thixotropy to the photosensitive resin composition, further improving the storage stability of the photosensitive resin composition. Furthermore, the adhesion between the cured product and the plating layer is further improved. The reactive group of the organic filler (E) more preferably includes at least one group selected from the group consisting of carboxyl groups, amino groups, epoxy groups, vinyl groups, and hydroxyl groups, and even more preferably includes at least one of carboxyl groups and amino groups. In this case, the storage stability of the photosensitive resin composition is further improved. In addition, the adhesion of the cured product to the plating layer is further improved. It is particularly preferable that the reactive group of the organic filler (E) contains a carboxyl group. In this case, the developability of the photosensitive resin composition is improved. At the same time, the carboxyl group of the organic filler (E) can react with the epoxy resin (D) in the photosensitive resin composition during thermal curing. As a result, the cured product after thermal curing can contain organic filler (E) uniformly dispersed inside. Furthermore, unreacted carboxyl groups of the organic filler (E) can also be modified during the stage of roughening the surface of the cured product. That is, organic filler (E) located near the surface of the cured product is more easily altered during the stage of roughening the surface of the cured product. The organic filler (E) thus altered is more easily removed from the cured product when a rough surface is applied to it. As a result, a rough surface can be applied to the surface of the cured product, improving the adhesion between the cured product and the plating layer. Furthermore, the inclusion of a carboxyl group in the organic filler (E) reduces the non-uniformity of the coating film caused by the fluidity of the photosensitive resin composition. This makes it easier to achieve a uniform film thickness in the layer formed by the photosensitive resin composition.Furthermore, it becomes easier to form via holes 6 having small diameter portions 63 in the interlayer insulating layer 7 made from the photosensitive resin composition.

[0077] When the organic filler (E) contains a carboxyl group, the carboxyl group is formed as a side chain in the product by polymerizing or crosslinking a carboxylic acid monomer such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, fumaric acid, or itaconic acid. The carboxylic acid monomer has a carboxyl group and a polymerizable unsaturated double bond. The organic filler (E) enhances the thixotropy of the photosensitive resin composition, thereby improving the stability (especially storage stability) of the photosensitive resin composition. Furthermore, when the organic filler (E) contains a carboxyl group, it can improve the developability of the cured product and improve the compatibility with crystalline epoxy resins, thereby preventing crystallization in the photosensitive resin composition. The carboxyl group content of the organic filler (E) is not particularly limited, but it is preferable that the acid value of the organic filler (E) is 1 mg KOH / g or more and 60 mg KOH / g or less, as determined by acid-base titration. If the acid value is less than 1 mg KOH / g, the stability of the photosensitive resin composition and the developability of the cured product may decrease. If the acid value is greater than 60 mg KOH / g, the moisture resistance reliability of the cured product may decrease. It is more preferable that the acid value of the organic filler (E) is between 3 mg KOH / g and 40 mg KOH / g.

[0078] The organic filler (E) preferably has an average primary particle diameter of 1 μm or less. Having an average primary particle diameter of 1 μm or less improves the developability of the photosensitive resin composition. Furthermore, it allows for finer roughness of the surface formed on the cured product, increasing the surface area of ​​the cured product and thus enhancing the anchoring effect and improving adhesion between the rough surface and the plating layer.

[0079] The average primary particle size of the organic filler (E) is not particularly limited in its lower limit, but is preferably 0.001 μm or larger. The average primary particle size is determined by a laser diffraction particle size distribution analyzer, D 50It is measured as follows. The average primary particle diameter of the organic filler (E1) is more preferably 0.4 μm or less, and even more preferably 0.1 μm or less. In this case, the scattering of light in the photosensitive resin composition during exposure can be suppressed, thereby further improving the resolution of the photosensitive resin composition and making it easier to form via holes 6 having small diameter portions 63 in the interlayer insulating layer 7. In addition, the roughness of the rough surface formed on the cured product can be made particularly fine.

[0080] The organic filler (E) is preferably dispersed in the photosensitive resin composition with a maximum particle size of less than 1.0 μm, and more preferably with a maximum particle size of less than 0.5 μm. The maximum particle size is determined by a laser diffraction particle size distribution analyzer, D 50 The maximum particle diameter is measured as follows. Alternatively, the maximum particle diameter is measured by observing the cured product with a transmission electron microscope (TEM). The organic filler (E) may aggregate in the photosensitive resin composition (for example, it may form secondary particles), in which case the maximum particle diameter refers to the size of the particles after aggregation. If the maximum particle diameter of the organic filler (E) in the dispersed state is within the above range, scattering during exposure is suppressed in the photosensitive resin composition, which further improves the resolution of the photosensitive resin composition and makes it easier to form via holes 6 with small diameter portions 63 in the interlayer insulating layer 7. In addition, the roughness of the rough surface formed on the cured product can be made even finer. Note that if particle aggregation occurs, the maximum particle diameter is usually larger than the average primary particle diameter.

[0081] The organic filler (E) preferably contains a rubber component. Alternatively, the organic filler (E) may contain only a rubber component. The rubber component can impart flexibility to the cured product of the photosensitive resin composition. The rubber component may be composed of a resin. The rubber component preferably contains at least one polymer selected from crosslinked acrylic rubber, crosslinked NBR, crosslinked MBS, and crosslinked SBR. In this case, the rubber component can impart excellent flexibility to the cured product of the photosensitive resin composition. Furthermore, it can impart a more appropriate rough surface to the cured product. Here, the rubber component includes a crosslinked structure formed when the monomers constituting the polymer are copolymerized. NBR is generally a copolymer of butadiene and acrylonitrile and is classified as nitrile rubber. MBS is generally a copolymer composed of three components: methyl methacrylate, butadiene, and styrene, and is classified as butadiene-based rubber. SBR is generally a copolymer of styrene and butadiene and is classified as styrene rubber. Specific examples of organic fillers (E) include JSR Corporation's product numbers XER-91-MEK, XER-32-MEK, and XSK-500. XER-91-MEK is a crosslinked rubber (NBR) having carboxyl groups with an average primary particle size of 0.07 μm, and is provided in a methyl ethyl ketone dispersion containing 15% by weight of this crosslinked rubber, with an acid value of 10.0 mgKOH / g. XER-32-MEK is a dispersion in which a polymer (linear particles) of carboxyl group-modified hydrogenated nitrile rubber is dispersed in methyl ethyl ketone at a content of 17% by weight relative to the total volume of the dispersion. XSK-500 is a crosslinked rubber (SBR) having carboxyl groups and hydroxyl groups with an average primary particle size of 0.07 μm, and is provided in a methyl ethyl ketone dispersion containing 15% by weight of this crosslinked rubber. Thus, the organic filler (E) may be in the form of a dispersion and incorporated into the photosensitive resin composition. That is, the rubber component can be incorporated into the photosensitive resin composition in the form of a dispersion. In addition to the above, specific examples of the organic filler (E) include JSR Corporation's product no. XER-92, etc.

[0082] The photosensitive resin composition may contain a silane coupling agent. In this case, the dispersibility of the organic filler (E) can be improved. Furthermore, the resolution of the photosensitive resin composition can also be improved.

[0083] Silane coupling agents are, for example, compounds containing silicon atoms and 2 to 4 hydrolyzable groups selected from the group consisting of -OCH3, -OC2H5, and -OCOCH3 groups. In addition to hydrolyzable groups, silane coupling agents may also contain reactive groups such as amino groups, epoxy groups, vinyl (allyl) groups, methacrylic groups, mercapto groups, isocyanate groups, sulfide groups, or methyl groups.

[0084] Examples of silane coupling agents include amino compounds such as 3-(2-aminoethylamino)propyldimethoxymethylsilane, 3-(2-aminoethylamino)propyltriethoxysilane, 3-(2-aminoethylamino)propyltrimethoxysilane, 3-aminopropyldiethoxymethylsilane, 3-aminopropyltriethoxysilane, and 3-aminopropyltrimethoxysilane; epoxy compounds such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidyloxypropyl(dimethoxy)methylsilane, and diethoxy(3-glycidyloxypropyl)methylsilane; 3-acryloxypropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, and 3- Examples include (meth)acrylates such as methacryloxypropylmethyldiethoxysilane, vinyl compounds such as vinyltrimethoxysilane, vinyltriethoxysilane, p-styryltrimethoxysilane, diethoxymethylvinylsilane, and vinyltris(2-methoxyethoxy)silane, allyl compounds such as allyltriethoxysilane and allyltrimethoxysilane, styryl compounds such as p-styryltrimethoxysilane, isocyanates such as 3-isocyanatopropyltrimethoxysilane and 3-isocyanatopropyltriethoxysilane, ureidopropyltrimethoxysilane and 3-ureidopropyltriethoxysilane, mercapto compounds such as (3-mercaptopropyl)triethoxysilane and (3-mercaptopropyl)trimethoxysilane, sulfides such as bis(triethoxysilylpropyl)tetrasulfide, tetraethyl orthosilicate, and methyltrimethoxysilane.

[0085] The photosensitive resin composition may contain melamine. In this case, the degree to which the cured product of the photosensitive resin composition is significantly corroded by an oxidizing agent containing, for example, potassium permanganate, can be reduced. That is, by including melamine in the photosensitive resin composition, it becomes more difficult to thin the thickness of the layer containing the cured product when roughening the surface of the cured product in a pre-plating step. By imparting a rough surface to the cured product in this way, the adhesion between the cured product of the photosensitive resin composition and the plating layer made of copper, gold, etc., can be improved. The melamine is 2,4,6-triamino-1,3,5-triazine, which is generally available from commercially available compounds. It is preferable that the melamine has an average particle size of 20 μm or less, preferably 15 μm or less, and is dispersed in the photosensitive resin composition. When melamine is uniformly dispersed in the photosensitive resin composition, it becomes easier for the melamine to further coordinate with metal elements. This can further improve the adhesion of the photosensitive resin composition. The lower limit of the average particle size of melamine is not particularly limited, but it can be 0.01 μm or larger. The average particle size of melamine is determined by a laser diffraction particle size distribution analyzer while melamine is dispersed in an uncured photosensitive resin composition. 50 It is measured as follows.

[0086] The photosensitive resin composition may contain an inorganic filler. In this case, the curing shrinkage of the film formed from the photosensitive resin composition is reduced. Furthermore, the dielectric loss tangent can be lowered. The inorganic filler may contain one or more materials selected from the group consisting of, for example, barium sulfate, silica, carbon nanotubes, talc, bentonite, aluminum hydroxide, magnesium hydroxide, and titanium oxide.

[0087] The photosensitive resin composition according to this embodiment may contain an organic solvent. The organic solvent is used for purposes such as liquefying or varnishing the photosensitive resin composition, adjusting viscosity, adjusting coatability, and adjusting film-forming properties.

[0088] The organic solvent may contain one or more compounds selected from the group consisting of, for example, linear, branched, secondary, or polyhydric alcohols such as ethanol, propyl alcohol, isopropyl alcohol, hexanol, and ethylene glycol; ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene and xylene; petroleum-based aromatic mixed solvents such as the Swazole series (manufactured by Maruzen Petrochemical Co., Ltd.) and the Solvesso series (manufactured by Exxon Chemical Co., Ltd.); cellosolves such as cellosolve and butyl cellosolve; carbitols such as carbitol and butyl carbitol; propylene glycol alkyl ethers such as propylene glycol methyl ether; polypropylene glycol alkyl ethers such as dipropylene glycol methyl ether; acetate esters such as ethyl acetate, butyl acetate, cellosolve acetate, and carbitol acetate; and dialkyl glycol ethers.

[0089] The carboxyl group-containing resin (A) is preferably in the range of 5% to 85% by mass, more preferably in the range of 10% to 75% by mass, and even more preferably in the range of 30% to 60% by mass, relative to the solid content of the photosensitive resin composition. The solid content refers to the total amount of all components after excluding volatile components such as solvents from the photosensitive resin composition.

[0090] The unsaturated compound (B), which has at least one ethylenically unsaturated bond in one molecule, is preferably in the range of 5% to 45% by mass relative to the carboxyl group-containing resin (A). Having the unsaturated compound (B) within this range makes it particularly easy to create via holes 6 with small diameter portions 63. The unsaturated compound (B) is more preferably in the range of 10% to 42% by mass relative to the carboxyl group-containing resin (A), and even more preferably in the range of 21% to 40% by mass.

[0091] The photopolymerization initiator (C) is preferably in the range of 1% by mass or more and 30% by mass or less relative to the carboxyl group-containing resin (A). When the proportion of the photopolymerization initiator (C) is 1% by mass or more relative to the carboxyl group-containing resin (A), the photosensitive resin composition tends to have good light absorption properties. When the photosensitive resin composition has good light absorption properties, it is easier to increase the degree of curing of the surface of the interlayer insulating layer 7 and reduce the water absorption of the interlayer insulating layer 7. In addition, it is easier to form via holes 6 having small diameter portions 63 in the interlayer insulating layer 7. When the photopolymerization initiator (C) is 30% by mass or less relative to the carboxyl group-containing resin (A), the cured film of the photosensitive resin composition tends to have good electrical insulation properties.

[0092] The photopolymerization initiator (C) is more preferably in the range of 1.5% to 25% by mass, even more preferably in the range of 2% to 20% by mass, and particularly preferably in the range of 3% to 10% by mass, relative to the carboxyl group-containing resin (A).

[0093] When the photosensitive resin composition contains epoxy resin (D), it is preferable that the total equivalent weight of epoxy groups contained in epoxy resin (D) is 0.1 to 5 relative to one equivalent weight of carboxyl groups in carboxyl group-containing resin (A). Having an equivalent weight of 0.1 or more epoxy groups in epoxy resin (D) relative to one equivalent weight of carboxyl groups in carboxyl group-containing resin (A) allows the photosensitive resin composition to be imparted with thermosetting properties. Having an equivalent weight of 5 or less epoxy groups in epoxy resin (D) relative to one equivalent weight of carboxyl groups in carboxyl group-containing resin (A) allows the photosensitive resin composition to have good developability. It is more preferable that the equivalent weight of epoxy groups in epoxy resin (D) is 0.3 to 4, even more preferable that it is 0.5 to 3, and particularly preferable that it is 0.7 to 2, relative to one equivalent weight of carboxyl groups in carboxyl group-containing resin (A).

[0094] The content of the organic filler (E) is preferably 1% by mass or more and 100% by mass or less relative to the carboxyl group-containing resin (A). A content of 1% by mass or more of the organic filler (E) allows for a moderate roughening of the surface of the cured product of the photosensitive resin composition, thereby improving the adhesion between the rough surface of the cured product and the plating layer. A content of 100% by mass or less of the organic filler (E) makes it easier for the photosensitive resin composition to have good developability. The content of the organic filler (E) is more preferably 1.5% by mass or more and 50% by mass or less, even more preferably 2% by mass or more and 30% by mass or less, and particularly preferably 3% by mass or more and 20% by mass or less, relative to the carboxyl group-containing resin (A). In this case, via holes 6 having small diameter portions 63 are particularly easy to produce.

[0095] When the photosensitive resin composition contains a silane coupling agent, the content of the silane coupling agent is preferably 0.01% by mass or more and 7% by mass or less relative to the organic filler (E). This range in proportion of the silane coupling agent prevents aggregation of the organic filler (E) in the photosensitive resin composition and improves dispersibility. More preferably, the proportion of the silane coupling agent is 0.05% by mass or more and 5% by mass or less relative to the organic filler (E). This range in proportion of the silane coupling agent more efficiently prevents aggregation of the organic filler (E1) in the photosensitive resin composition and more effectively improves dispersibility.

[0096] When the photosensitive resin composition contains melamine, the melamine content is preferably 0.1% by mass or more and 10% by mass or less relative to the carboxyl group-containing resin (A). In this case, it exhibits good developability in an alkaline aqueous solution, and via holes 6 having small diameter portions 63 are more easily formed in the interlayer insulating layer 7. The melamine content is more preferably 0.3% by mass or more and 9% by mass or less, even more preferably 0.5% by mass or more and 8% by mass or less, and particularly preferably 1% by mass or more and 6% by mass or less, relative to the carboxyl group-containing resin (A).

[0097] The proportion of inorganic filler in the photosensitive resin composition is set as appropriate, but the inorganic filler content is preferably 0% by mass or more and 200% by mass or less relative to the carboxyl group-containing resin (A). In this case, good resolution can be obtained, and via holes 6 having small diameter portions 63 are more easily formed in the interlayer insulating layer 7. The inorganic filler content is more preferably 0% by mass or more and 150% by mass or less, even more preferably 0% by mass or more and 100% by mass or less, even more preferably 0% by mass or more and 50% by mass or less, and particularly preferably 0% by mass or more and 20% by mass or less, relative to the carboxyl group-containing resin (A).

[0098] When a photosensitive resin composition contains an organic solvent, it is preferable that the amount of organic solvent be adjusted so that the organic solvent evaporates quickly when the coating film formed from the photosensitive resin composition is dried, that is, so that no organic solvent remains in the dried film. In particular, it is preferable that the proportion of the organic solvent to the entire photosensitive resin composition be 0% by mass or more and 99.5% by mass or less, and more preferably 15% by mass or more and 60% by mass or less. Note that the preferred proportion of the organic solvent varies depending on the application method, so it is preferable that the proportion be appropriately adjusted according to the application method.

[0099] The photosensitive composition may further contain components other than those described above, as long as they do not impair the effects of this embodiment.

[0100] The photosensitive resin composition may contain at least one resin selected from the group consisting of tolylene diisocyanate, morpholine diisocyanate, isophorone diisocyanate, and hexamethylene diisocyanate blocked with caprolactam, oxime, malonic acid ester, etc.; butylated urea resin; various thermosetting resins other than those mentioned above; UV-curable epoxy (meth)acrylate; resins obtained by adding (meth)acrylic acid to epoxy resins such as bisphenol A type, phenol novolac type, cresol novolac type, and alicyclic type; and polymer compounds such as diallyl phthalate resin, phenoxy resin, urethane resin, melamine resin, and fluororesin.

[0101] The photosensitive resin composition may contain a curing agent for curing the epoxy compound (D). The curing agent may contain at least one component selected from the group consisting of, for example, imidazole derivatives such as imidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 4-phenylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-(2-cyanoethyl)-2-ethyl-4-methylimidazole; amine compounds such as dicyandiamide, benzyldimethylamine, 4-(dimethylamino)-N,N-dimethylbenzylamine, 4-methoxy-N,N-dimethylbenzylamine, and 4-methyl-N,N-dimethylbenzylamine; hydrazine compounds such as adipic acid hydrazide and sebacate hydrazide; phosphorus compounds such as triphenylphosphine; acid anhydrides; phenols; mercaptans; Lewis acid amine complexes; and onium salts. Commercially available products containing these components include, for example, 2MZ-A, 2MZ-OK, 2PHZ, 2P4BHZ, and 2P4MHZ (all trade names for imidazole compounds) from Shikoku Chemicals Co., Ltd., and U-CAT3503N, UCAT3502T (both trade names for dimethylamine blocked isocyanate compounds), DBU, DBN, U-CATSA102, and U-CAT5002 (all bicyclic amidine compounds and their salts) from Sunapro Co., Ltd.

[0102] The photosensitive resin composition may contain an adhesion promoter. Examples of adhesion promoters include guanamine derivatives such as acetoguanamine (2,4-diamino-6-methyl-1,3,5-triazine) and benzoguanamine (2,4-diamino-6-phenyl-1,3,5-triazine), as well as S-triazine derivatives such as 2,4-diamino-6-methacryloyloxyethyl-S-triazine, 2-vinyl-4,6-diamino-S-triazine, 2-vinyl-4,6-diamino-S-triazine isocyanuric acid adduct, and 2,4-diamino-6-methacryloyloxyethyl-S-triazine isocyanuric acid adduct, silane coupling agents, melamine derivatives, and the like.

[0103] The photosensitive resin composition may contain a rheology control agent. The rheology control agent facilitates the optimization of the viscosity of the photosensitive resin composition. Examples of rheology control agents include urea-modified medium-polarity polyamide (product numbers BYK-430 and BYK-431 from BIG Chemie Japan Co., Ltd.), polyhydroxycarboxylic acid amide (product number BYK-405 from BIG Chemie Japan Co., Ltd.), modified urea (product numbers BYK-410, BYK-411, and BYK-420 from BIG Chemie Japan Co., Ltd.), high-molecular-weight urea derivative (product number BYK-415 from BIG Chemie Japan Co., Ltd.), urea-modified urethane (product number BYK-425 from BIG Chemie Japan Co., Ltd.), polyurethane (product number BYK-428 from BIG Chemie Japan Co., Ltd.), castor oil wax, polyethylene wax, polyamide wax, bentonite, kaolin, and clay.

[0104] The photosensitive resin composition may contain at least one component selected from the group consisting of curing accelerators; colorants; copolymers such as silicones and acrylates; leveling agents; thixotropic agents; polymerization inhibitors; anti-halation agents; flame retardants; defoamers; antioxidants; surfactants; and polymer dispersants.

[0105] The photosensitive resin composition of this embodiment may be prepared by any appropriate method. For example, the photosensitive resin composition can be prepared by mixing and stirring the raw materials of the photosensitive resin composition. Alternatively, the photosensitive resin composition may be prepared by kneading using an appropriate kneading method, such as a three-roll mill, ball mill, or sand mill. If the raw materials contain liquid components, low-viscosity components, etc., the portion of the raw materials excluding the liquid components, low-viscosity components, etc. may be kneaded first to prepare a mixture, and then the liquid components, low-viscosity components, etc. may be added to the resulting mixture and mixed to prepare the photosensitive resin composition. If the photosensitive resin composition contains a solvent (E), some or all of the solvent may be mixed first, and then mixed with the remainder of the raw materials.

[0106] The photosensitive resin composition preferably has properties that allow it to be developed with an aqueous sodium carbonate solution, even if the film 4 is 25 μm thick. In this case, a sufficiently thick electrical insulating layer can be fabricated from the photosensitive resin composition by photolithography, making the photosensitive resin composition widely applicable for fabricating the interlayer insulating layer 7 in the printed circuit board 11. Of course, it is also possible to fabricate an electrical insulating layer thinner than 25 μm from the photosensitive resin composition.

[0107] Whether a 25 μm thick film 4 can be developed with an aqueous sodium carbonate solution can be confirmed by the following method: A wet coating is prepared by applying a photosensitive resin composition to a suitable substrate 1, and this wet coating is heated at 80°C for 40 minutes to form a 25 μm thick film 4. A negative mask having an exposure area that transmits ultraviolet light and a non-exposure area that blocks ultraviolet light is directly applied to the film 4, and 500 mJ / cm³ is applied to the film 4. 2 Exposure is performed by irradiating with ultraviolet light under the specified conditions. After exposure, a 1% Na2CO3 aqueous solution at 30°C is sprayed onto the film 4 at a spray pressure of 0.2 MPa for 90 seconds, followed by spraying with pure water at a spray pressure of 0.2 MPa for 90 seconds. After this treatment, the film 4 is observed, and if the parts corresponding to the unexposed areas of the film 4 are removed and no residue is observed, it can be determined that the 25 μm thick film 4 is developable with sodium carbonate aqueous solution. Similarly, it can be confirmed whether films 4 of other thicknesses (e.g., 30 μm) are developable with sodium carbonate aqueous solution.

[0108] (2.2) Manufacturing of the printed circuit board 11 The manufacturing method of the printed circuit board 11 according to this embodiment will be described in detail with reference to Figures 1A to 1E.

[0109] In manufacturing the printed circuit board 11, for example, a photosensitive resin composition and a substrate are prepared. The substrate has an insulating layer 2 and a second conductive layer 3 that overlaps the insulating layer 2. A film 4 made from the photosensitive resin composition is placed on the substrate so as to cover the second conductive layer 3, and a negative pattern-like region of the film 4, including the pattern of via holes 6, is exposed to light, and then developed using an alkaline aqueous solution. This creates an interlayer insulating layer 7 and via holes 6 that penetrate the interlayer insulating layer 7.

[0110] Specifically, for example, first, a base material 1 is prepared as shown in Figure 1A. The base material 1 comprises an insulating layer 2 and a second conductor layer 3. The second conductor layer 3 is a conductor wiring.

[0111] A photosensitive resin composition is applied to the substrate and, if necessary, dried to produce a film 4 that covers the second conductive layer 3, as shown in Figure 1B. The method for applying the photosensitive resin composition is selected from known methods, such as immersion, spray, spin coating, roll coating, curtain coating, and screen printing. When drying the photosensitive resin composition, it is heated to a temperature of, for example, 60°C to 130°C.

[0112] The coating 4 may be prepared by layering a dry film made from a photosensitive resin composition onto a substrate. The dry film is formed on a suitable support, such as one made of polyester, by applying the photosensitive resin composition to the support and then drying it. This yields a dry film with a support, comprising the dry film and a support that supports the dry film. In this dry film with a support, the dry film is layered on the substrate 1 so as to cover the second conductive layer 3, and then pressure is applied to the dry film and the substrate 1. This results in a coating 4 made of the dry film being layered on the substrate 1.

[0113] Next, the film 4 is exposed. For example, a negative pattern-like region of the film 4 that includes the pattern of via holes 6 is exposed. In this case, for example, ultraviolet light is irradiated onto the film 4 through a negative mask. The negative mask comprises an exposure area that transmits ultraviolet light and a non-exposure area that blocks ultraviolet light, and the pattern of the non-exposure area includes the pattern of via holes 6. The negative mask is, for example, a phototool such as a mask film or a dry plate. The ultraviolet light source is selected from the group consisting of, for example, chemical lamps, low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, xenon lamps and metal halide lamps.

[0114] When the coating 4 is made from a dry film, when exposing the coating 4, for example, the support is peeled off from the coating 4 beforehand before exposing the coating 4. Alternatively, the coating 4 may be exposed by irradiating the coating 4 with ultraviolet light while the support remains on top of the coating 4, allowing the support to pass through, and then the support may be peeled off from the exposed coating 4.

[0115] Other methods besides using a negative mask may be employed as the exposure method. For example, the film 4 may be exposed using a direct writing method in which ultraviolet light emitted from a light source is irradiated only on the portion of the film 4 to be exposed. The light source applied to the direct writing method is selected from the group consisting of, for example, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, g-line (436 nm), h-line (405 nm), i-line (365 nm), and combinations of two or more of the g-line, h-line, and i-line.

[0116] It is preferable that the ultraviolet light irradiated onto the film 4 has spectral intensity at at least one wavelength in the wavelength range of 365 nm ± 65 nm. Furthermore, it is preferable that the ultraviolet light irradiated onto the film 4 does not have spectral intensity at wavelengths of 435 nm or higher. When the ultraviolet light irradiated onto the film 4 has spectral intensity at at least one wavelength in the wavelength range of 365 nm ± 65 nm, the curing of the film 4 proceeds more easily. In addition, if the ultraviolet light contains light with wavelengths of 435 nm or higher, the diameter of the second end 62 of the via hole 6 formed in the interlayer insulating layer 7 after development tends to become smaller. This is presumed to be because light with long wavelengths of 435 nm or higher is not easily absorbed by the photosensitive resin composition and therefore easily penetrates deep into the film 4, causing light scattering to occur in the deep parts of the film 4. The ultraviolet light irradiated onto the coating 4 preferably has spectral intensity at at least one wavelength in the 365nm ± 45nm wavelength range and no spectral intensity above 415nm, even more preferably has spectral intensity at at least one wavelength in the 365nm ± 30nm wavelength range and no spectral intensity above 400nm, and particularly preferably has spectral intensity at at least one wavelength in the 365nm ± 15nm wavelength range and no spectral intensity above 385nm.

[0117] Next, the film 4 is developed with an alkaline aqueous solution to create an interlayer insulating layer 7 having via holes 6. At this time, as already explained, via holes 6 having small diameter portions 63 are easily formed. By developing the film 4, the uncured portion 5 of the film 4 shown in Figure 1C is removed, thereby providing the via holes 6 as shown in Figure 1D. In the developing process, an appropriate developer can be used depending on the composition of the photosensitive resin composition. The developer is, for example, an alkaline aqueous solution containing at least one of alkali metal salts and alkali metal hydroxides, or an organic amine. More specifically, the alkaline aqueous solution contains at least one component selected from the group consisting of sodium carbonate, potassium carbonate, ammonium carbonate, sodium bicarbonate, potassium bicarbonate, ammonium bicarbonate, sodium hydroxide, potassium hydroxide, ammonium hydroxide, tetramethylammonium hydroxide, and lithium hydroxide. The solvent in the alkaline aqueous solution may be water alone, or a mixture of water and a hydrophilic organic solvent such as lower alcohols. The organic amine contains at least one component selected from the group consisting of, for example, monoethanolamine, diethanolamine, triethanolamine, monoisopropanolamine, diisopropanolamine, and triisopropanolamine.

[0118] The alkaline aqueous solution preferably contains at least one of an alkali metal salt and / or alkali metal hydroxide, and is particularly preferably sodium carbonate. In this case, improvements to the working environment and reductions in the burden of waste disposal can be achieved.

[0119] Since the photosensitive resin composition according to this embodiment has good developability, residue of the uncured photosensitive resin composition is less likely to remain at the bottom of the via hole 6 after development. For this reason, it is easy to form via holes 6 having a small diameter portion 63.

[0120] Next, the developed film 4 may be heat-cured by heating. The heating conditions are, for example, a heating temperature within the range of 120°C to 200°C and a heating time within the range of 20 minutes to 180 minutes. Heat-curing the film 4 in this way improves the strength, hardness, chemical resistance, and other properties of the interlayer insulating layer 7.

[0121] If necessary, the coating 4 may be further irradiated with ultraviolet light either before or after heating, or both. In this case, the photocuring of the coating 4 can be further advanced.

[0122] As described above, an interlayer insulating layer 7 made of a cured photosensitive resin composition is provided on the substrate 1. Subsequently, a first conductor layer 8, which is a conductor wiring, can be fabricated on the interlayer insulating layer 7 and via conductors 9 can be fabricated in the via holes 6 by a known method such as the additive method. As a result, a printed circuit board 11 is obtained, which comprises the first conductor layer 8, the second conductor layer 3, the interlayer insulating layer 7, via holes 6, and via conductors 9, as shown in Figure 1E. In Figure 1E, the via conductors 9 fill the entire via hole 6, but the via conductors 9 may be a film that covers the inner surface of the via hole 6.

[0123] Furthermore, before fabricating the via conductor 9, the entire inner surface of the via hole 6 and a portion of the outer surface of the interlayer insulating layer 7 may be roughened. In this case, the adhesion between the substrate 1 and the via conductor 9 can be improved.

[0124] The roughening of a portion of the outer surface of the interlayer insulating layer 7 and the entire inner surface of the via hole 6 can be carried out using the same procedure as a general desmear treatment using an oxidizing agent. For example, the outer surface of the interlayer insulating layer 7 can be roughened by bringing an oxidizing agent into contact with it. However, the procedure is not limited to this, and other appropriate roughening methods such as plasma treatment, UV treatment, or ozone treatment may also be employed.

[0125] The oxidizing agent may be an oxidizing agent available as a desmear solution. Such an oxidizing agent may contain, for example, at least one permanganate selected from the group consisting of sodium permanganate and potassium permanganate.

[0126] In providing the via conductor 9, an initial conductor can be formed by applying electroless metal plating to a portion of the roughened outer surface and the inner surface of the via hole 6. Subsequently, the via conductor 9 can be formed by depositing metal from the electrolytic plating solution onto the initial conductor through electrolytic metal plating. [Examples]

[0127] The present disclosure will be described in detail below with reference to examples. However, the present disclosure is not limited to the following examples, and various modifications are possible depending on the design, as long as the objectives of the present disclosure are achieved.

[0128] 1. Synthesis of carboxyl group-containing resins [Synthesis Examples 1-6: Bisphenol fluorene skeleton-containing resins] A mixture was prepared by adding the components shown in the "First Reaction" column of Table 1 to a four-necked flask equipped with a reflux condenser, thermometer, air inlet, and stirrer, and stirring them under air bubbling. This mixture was then heated in the flask under air bubbling while stirring at the reaction temperature and reaction time shown in the "Reaction Conditions" column. This prepared a solution of the intermediate.

[0129] Next, the components shown in the "Second Reaction" column of Table 1 were added to the intermediate solution in the flask, and the mixture was heated under air bubbling while stirring at the reaction temperature and time shown in the "Reaction Conditions (1)" column. Subsequently, the mixture was heated under air bubbling while stirring at the reaction temperature and time shown in the "Reaction Conditions (2)" column. This yielded a 65% by mass solution of the carboxyl group-containing resin. The weight-average molecular weight and acid value of the carboxyl group-containing resin are shown in Table 1.

[0130] The details of the components shown in column (a1) of Table 1 are as follows: • Epoxy compound 1: A bisphenol fluorene type epoxy compound represented by formula (2), where R1 to R8 in formula (2) are all hydrogen atoms, in an epoxy equivalent weight of 250 g / eq. • Epoxy compound 2: A bisphenol fluorene type epoxy compound represented by formula (2), in which R1 and R5 are both methyl groups, and R2-R4 and R6-R8 are all hydrogen atoms, with an epoxy equivalent weight of 279 g / eq.

[0131] [Synthesis Example 7: Biphenylnovolac skeleton-containing resin] A mixture was prepared by adding 288 parts by mass of biphenyl novolac epoxy resin (manufactured by Nippon Kayaku Co., Ltd., product code NC-3000-H, epoxy equivalent 288 g / eq), 155 parts by mass of diethylene glycol monoethyl ether acetate, 0.2 parts by mass of methyl hydroquinone, 72 parts by mass of acrylic acid, and 3 parts by mass of triphenylphosphine to a four-necked flask equipped with a reflux condenser, thermometer, air blowing tube, and stirrer. This mixture was heated in the flask at 115°C for 12 hours while stirring under air bubbling. This prepared an intermediate solution.

[0132] Next, 85 parts by mass of tetrahydrophthalic anhydride and 86.3 parts by mass of diethylene glycol monoethyl ether acetate were added to the intermediate solution in the flask, and the mixture was heated at 90°C for 4 hours while stirring under air bubbling. This yielded a 65% by mass solution of carboxyl group-containing resin B-1. The weight-average molecular weight of carboxyl group-containing resin B-1 was 8026, and the acid value was 69 mgKOH / g.

[0133] 2. Preparation of the composition The components shown in Tables 2 and 3 below were kneaded using a three-roll mill and then stirred and mixed in a flask to obtain the composition. The details of the components shown in Tables 2 and 3 are as follows. Unsaturated compound A: Trimethylolpropane triacrylate. • Photopolymerization initiator A: 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, manufactured by BASF, catalog number Irgacure TPO. • Photopolymerization initiator B: 1-hydroxycyclohexylphenyl ketone, manufactured by BASF, catalog number Irgacure 184. • Photopolymerization initiator C:4,4'-bis(diethylamino)benzophenone. • Photopolymerization initiator D: 2,4-diethylthioxanthene-9one. Crystalline epoxy resin A: Bisphenol-type crystalline epoxy resin, manufactured by Nippon Steel Chemical & Material Co., Ltd., product number YSLV-80XY, melting point 75-85°C, epoxy equivalent 192 g / eq. Amorphous epoxy resin solution A: Long-chain carbon chain-containing bisphenol A type epoxy resin, manufactured by DIC Corporation, product number EPICLON EXA-4816, liquid resin, solution obtained by dissolving 410 g / eq of epoxy equivalent in diethylene glycol monoethyl acetate with a solid content of 90%. • Organic filler A dispersion: A dispersion (manufactured by JSR Corporation, product number XER-91-MEK; acid value 10.0 mgKOH / g) in which cross-linked rubber (NBR) with an average primary particle size of 0.07 μm is dispersed in methyl ethyl ketone at a content of 15% by weight relative to the total volume of the dispersion. • Organic filler B: Glycidyl-modified acrylonitrile butadiene rubber with an average primary particle size of 0.3 μm. Additive A: 3-glycidoxypropyltrimethoxysilane. • Additive B: Melamine. Solvent A: Methyl ethyl ketone.

[0134] 3. Evaluation of the composition (1) Preparation of test pieces Test pieces were prepared using the compositions of each example composition as follows.

[0135] The compositions of each example were applied to a polyethylene terephthalate film using an applicator, then heated at 80°C for 5 minutes, followed by drying at 95°C for 20 minutes to form a dry film with a thickness of 35 μm on the film.

[0136] A glass epoxy copper-clad laminate (FR-4 type) with a copper foil thickness of 17.5 μm was prepared. A surface area of ​​approximately 1 μm thickness on this glass epoxy copper-clad laminate was roughened by treatment with an etching agent (product code CZ-8101, manufactured by MEC Corporation). The dry film described above was heat-laminated onto one entire surface of this glass epoxy copper-clad laminate using a vacuum laminator. The heat lamination conditions were set to 0.5 MPa, 80°C, and 1 minute. This formed a film consisting of the dry film on the glass epoxy copper-clad laminate. Ultraviolet light with a wavelength of 365 nm was then applied to this film through a negative mask with a pattern including circular shapes with a diameter of 80 μm and a non-exposed area, and through a polyethylene terephthalate film, at an integrated light intensity of 250 mJ / cm². 2 The irradiation was carried out under the following conditions. Subsequently, the polyethylene terephthalate film was peeled off from the coating.

[0137] Next, the film was developed by spraying it with an alkaline aqueous solution (1% Na2CO3 aqueous solution) at 30°C at a spray pressure of 0.2 MPa for 90 seconds, followed by spraying it with pure water at a spray pressure of 0.2 MPa for 90 seconds. Subsequently, the film was heated at 180°C for 120 minutes. This formed an interlayer insulating layer and via holes penetrating this interlayer insulating layer on the printed circuit board. A test piece was then obtained.

[0138] The following evaluations were performed on these test pieces. Note that composition example 11 could not be developed and therefore was not evaluated. Also, composition example 14 was not evaluated because some areas showed peeling of the film due to insufficient curing during development.

[0139] (2) Measurement of the diameter of the first end and the diameter of the second end The test piece was cut in half along a plane parallel to the via hole axis, and the cross-section was photographed using an electron microscope (SEM). From the resulting images, the diameters of the first and second ends of the via hole were measured. The value of (diameter of first end ÷ diameter of second end) × 100 (%) was also calculated.

[0140] (3) Presence or absence of a small diameter section From the images obtained in "(2) Measurement of the diameter of the first end and the diameter of the second end" above, we confirmed whether a small-diameter section existed between the first and second ends of the via hole and evaluated it as follows. A: A small diameter section exists between the first and second ends, and the minimum diameter of the small diameter section is 65% or more but less than 100% of the diameter of the second end. B: A small diameter section exists between the first and second ends, and the minimum diameter of the small diameter section is less than 65% of the diameter of the second end. C: There is no small-diameter section between the first and second ends.

[0141] (4) Via shape evaluation Based on the images obtained in "(2) Measurement of the diameter of the first end and the diameter of the second end" above, the shape of the via hole was evaluated as follows. A: The value of (Diameter of the first end ÷ Diameter of the second end) × 100 (%) is 80% or more, and there is a smaller diameter section between the first and second ends that is 65% or more but less than 100% of the diameter of the second end. B: The value of (diameter of the first end ÷ diameter of the second end) × 100 (%) is 75% or more and less than 80%, and there is a smaller diameter section between the first and second ends that is 65% or more and less than 100% of the diameter of the second end. C: The value of (Diameter of the first end ÷ Diameter of the second end) × 100 (%) is 65% or more and less than 75%, and there is a smaller diameter section between the first and second ends that is 65% or more and less than 100% of the diameter of the second end. D: The value of (diameter of the first end ÷ diameter of the second end) × 100 (%) is less than 65%, and there is a small diameter section between the first and second ends. E: No small diameter section exists.

[0142] The results of the above evaluation tests are shown in Tables 2 and 3 below.

[0143] 4. Evaluation of printed circuit boards (1) Preparation of test pieces Except for the film formation method and film thickness during film preparation, the diameter of the circular pattern during exposure, the wavelength and integrated light intensity of ultraviolet light, and the spraying time of the alkaline aqueous solution during development, which are as shown in Tables 4 to 6, test pieces were prepared using the method described in "(1) Preparation of Test Pieces" in "1. Evaluation of Composition" above. In cases where multiple values ​​are listed in the wavelength column, ultraviolet light with each of the specified wavelengths was irradiated simultaneously.

[0144] The following evaluations were performed on these test pieces. Note that comparative example 1 could not be developed and therefore was not evaluated. Also, comparative example 3 was not evaluated because there were areas where the film peeled off due to insufficient curing during development.

[0145] (2) Measurement of the diameter of the first end and the diameter of the second end The test piece was cut in half along a plane parallel to the via hole axis, and the cross-section was observed using an electron microscope (SEM). From the resulting images, the diameter of the first end and the diameter of the second end of the via hole were measured. The value of (diameter of first end ÷ diameter of second end) × 100 (%) was also calculated.

[0146] (3) Presence or absence of a small diameter section From the images obtained in "(2) Measurement of the diameter of the first end and the diameter of the second end" above, we confirmed whether a small-diameter section existed between the first and second ends of the via hole and evaluated it as follows. A: A small diameter section exists between the first and second ends, and the minimum diameter of the small diameter section is 65% or more but less than 100% of the diameter of the second end. B: A small diameter section exists between the first and second ends, and the minimum diameter of the small diameter section is less than 65% of the diameter of the second end. C: There is no small-diameter section between the first and second ends.

[0147] (4) Via shape evaluation Based on the images obtained in "(2) Measurement of the diameter of the first end and the diameter of the second end" above, the shape of the via hole was evaluated as follows. A: The value of (Diameter of the first end ÷ Diameter of the second end) × 100 (%) is 80% or more, and there is a smaller diameter section between the first and second ends that is 65% or more but less than 100% of the diameter of the second end. B: The value of (diameter of the first end ÷ diameter of the second end) × 100 (%) is 75% or more and less than 80%, and there is a smaller diameter section between the first and second ends that is 65% or more and less than 100% of the diameter of the second end. C: The value of (Diameter of the first end ÷ Diameter of the second end) × 100 (%) is 65% or more and less than 75%, and there is a smaller diameter section between the first and second ends that is 65% or more and less than 100% of the diameter of the second end. D: The value of (diameter of the first end ÷ diameter of the second end) × 100 (%) is less than 65%, and a smaller diameter section exists between the first and second ends. E: No small diameter section exists.

[0148] (5) Via connection reliability For the test pieces, the outer surface of the interlayer insulation layer was roughened using the desmear treatment described below, which is a common pre-processing step before plating.

[0149] The interlayer insulation layer was first swollen using a desmear swelling solution (Swelling Dip Securigant P, manufactured by Atotec Japan Co., Ltd.) at 70°C for 10 minutes to swell the surface of the interlayer insulation layer, and then the interlayer insulation layer was washed with hot water. Next, the surface of the interlayer insulation layer was roughened by treating it with a desmear solution (an oxidizing agent containing potassium permanganate; Concentrate Compact CP, manufactured by Atotec Japan Co., Ltd.) at 70°C for 10 minutes, and then the interlayer insulation layer was washed with hot water. Then, the surface of the interlayer insulation layer was treated with a neutralizing solution (Reduction Solution Securigant P, manufactured by Atotec Japan Co., Ltd.) at 40°C for 5 minutes to remove any residue, and then the interlayer insulation layer was washed with water.

[0150] Next, an initial conductor was fabricated by electroless copper plating on the interlayer insulating layer, and then heated at 150°C for 1 hour. Next, a current density of 2A / dm² was applied to the initial conductor. 2The material was subjected to electrolytic copper plating under the specified conditions, followed by heating at 180°C for 30 minutes. This created a first conductor layer with a thickness of 33 μm on the interlayer insulating layer, and also created via conductors within the via holes.

[0151] Next, a temperature cycling test was conducted, in which the test piece was exposed to -55°C for 15 minutes, followed by exposure to 125°C for 15 minutes, and this cycle was repeated 500 times. The electrical resistance between the first and second conductor layers through the via conductor was measured before and after the test, and the rate of change was evaluated as follows. A: The rate of change in resistance before and after the temperature cycling test is less than 8%. B: The rate of change in resistance before and after the temperature cycling test is 8% or more but less than 10%. C: The rate of change in resistance value before and after the temperature cycling test is 10% or more.

[0152] The results of the above evaluation tests are shown in Tables 4-6 below.

[0153] [Table 1]

[0154] [Table 2]

[0155] [Table 3]

[0156] [Table 4]

[0157] [Table 5]

[0158] [Table 6] [Explanation of Symbols]

[0159] 3. Second Conductor Layer 4. Coating 6 via holes 61 First end 62 Second end 63 Small diameter section 7 interlayer insulating layer 8. First Conductor Layer 9 via conductors

Claims

1. a first conductor layer, a second conductor layer, an interlayer insulating layer interposed between the first conductor layer and the second conductor layer, a via hole penetrating the interlayer insulating layer, and a via conductor disposed in the via hole and electrically connecting the first conductor layer and the second conductor layer; the interlayer insulating layer is a cured product of a negative photosensitive resin composition containing a carboxyl group-containing resin (A), an unsaturated compound (B) having at least one ethylenically unsaturated bond in one molecule, and a photopolymerization initiator (C); the via hole has a first end which is an end on the first conductor layer side, a second end which is an end on the second conductor layer side, and a small diameter portion located between the first end and the second end and having a diameter smaller than a diameter of the second end, The minimum diameter of the small diameter portion is 65% or more and less than 100% of the diameter of the second end, Printed wiring board.

2. The diameter of the first end is 65% or more of the diameter of the second end. The printed wiring board according to claim 1 .

3. The diameter of the first end is 100 μm or less. The printed wiring board according to claim 1 or 2.

4. The carboxyl group-containing resin (A) contains a carboxyl group-containing resin (A1) having a bisphenol fluorene skeleton, The printed wiring board according to claim 1 .

5. The weight average molecular weight of the carboxyl group-containing resin (A) is 700 or more and 100,000 or less. The printed wiring board according to claim 1 .

6. The carboxyl group-containing resin (A) contains a component having an acid value of 65 mg KOH / g or more and 150 mg KOH / g or less. The printed wiring board according to claim 1 .

7. The percentage of the unsaturated compound (B) is 5% by mass or more and 45% by mass or less relative to the carboxyl group-containing resin (A), The printed wiring board according to claim 1 .

8. The percentage of the photopolymerization initiator (C) is 1% by mass or more and 30% by mass or less relative to the carboxyl group-containing resin (A), The printed wiring board according to claim 1 .

9. The photopolymerization initiator (C) contains at least one selected from the group consisting of an acylphosphine oxide-based photopolymerization initiator, an α-aminoalkylphenone-based photopolymerization initiator, and an oxime ester-based photopolymerization initiator. The printed wiring board according to claim 1 .

10. The photosensitive resin composition further contains an epoxy resin (D), The printed wiring board according to claim 1 .

11. The epoxy group equivalent of the epoxy resin (D) is 0.1 or more and 5 or less relative to 1 carboxyl group equivalent of the carboxyl group-containing resin (A). The printed wiring board according to claim 10.

12. The photosensitive resin composition further contains an organic filler (E). The printed wiring board according to claim 1 .

13. The organic filler (E) has a reactive group. The printed wiring board according to claim 12.

14. The reactive group includes at least one group selected from the group consisting of a carboxyl group, an amino group, an epoxy group, a vinyl group, and a hydroxyl group. The printed wiring board according to claim 13.

15. The ratio of the organic filler (E) to the carboxyl group-containing resin (A) is 1 mass% or more and 100 mass% or less. The printed wiring board according to any one of claims 12 to 14.

16. A method for producing a printed wiring board according to any one of claims 1 to 15, comprising: preparing a negative photosensitive resin composition containing the carboxyl group-containing resin (A), the unsaturated compound (B) having at least one ethylenically unsaturated bond in one molecule, and the photopolymerization initiator (C), as well as a substrate having an insulating layer and the second conductor layer overlapping the insulating layer; A film made of the photosensitive resin composition is laminated on the substrate so as to cover the second conductor layer; and exposing a negative pattern region of the coating, the region including the via hole pattern, to light, and then performing a development process using an alkaline aqueous solution, thereby forming the interlayer insulating layer and the via hole penetrating the interlayer insulating layer. A method for manufacturing a printed wiring board.

17. The method of claim 17, further comprising: forming the coating by overlaying a dry film made from the photosensitive resin composition on the substrate. The method for producing a printed wiring board according to claim 16 .

18. In exposing the coating, the coating is irradiated with light having a spectral intensity at at least one wavelength in a wavelength range of 365 nm ± 65 nm and no spectral intensity at a wavelength of 435 nm or more. The method for producing a printed wiring board according to claim 16 or 17.