AI Technical Summary
Existing foam sheets made from polylactic acid lack sufficient cushioning properties and sheet strength, particularly in terms of compressive stress and puncture resistance, which are crucial for applications as cushioning materials.
A foam sheet composition containing polylactic acid and a filler, with specific compressive stress and puncture strength characteristics, is developed to enhance cushioning properties and sheet strength, utilizing a continuous kneading process with a compressible fluid to ensure uniform foaming and dispersion of the filler.
The resulting foam sheet achieves high cushioning properties and sheet strength, with compressive stress of 0.2 Mpa or less and puncture strength of 2 N or more, ensuring durability and effectiveness as a cushioning material.
Smart Images

Figure 00000022_0000 
Figure 00000022_0001 
Figure 00000022_0002
Abstract
Description
[Technical Field]
[0001] This invention relates to foamed sheets, manufactured products, and methods for manufacturing foamed sheets. [Background technology]
[0002] Foamed sheets are lightweight, offer excellent cushioning properties, and are easily molded into various shapes, making them widely used as raw materials for manufactured products such as bags and containers (resin molded products). Thermoplastic resins such as polystyrene resins, polyolefin resins, and polyester resins are used as materials for foamed sheets.
[0003] In recent years, due to the growing demand for environmentally friendly materials, the use of biodegradable polymers that decompose naturally in the environment is being considered as a material for foamed sheets, among other polyester resins. Among these, polylactic acid is a plant-derived biodegradable polymer that has properties similar to polystyrene resins that have been conventionally used in foamed sheets, and is being considered for use as a material for foamed sheets because it has a relatively high melting point, toughness, transparency, and chemical resistance compared to other biodegradable polymers.
[0004] As an example of a foamed sheet using polylactic acid, a biodegradable resin laminated foamed sheet is disclosed in which a biodegradable resin film made of polylactic acid resin is laminated on one or both sides of a foamed base sheet made of polystyrene resin foam, and the puncture strength is 7.0 N or higher (see, for example, Patent Document 1). [Overview of the project] [Problems that the invention aims to solve]
[0005] One aspect of the present invention aims to provide a foamed sheet that can have high cushioning properties and sheet strength. [Means for solving the problem]
[0006] One embodiment of the foamed sheet according to the present invention contains polylactic acid and filler, has a compressive stress of 0.2 MPa or less when the buffering coefficient is 10 or less, and has a puncture strength of 2 N or more when the sheet thickness is 2 mm. [Effects of the Invention]
[0007] One aspect of the present invention provides a foamed sheet that can have high cushioning properties and sheet strength. It is possible. [Brief explanation of the drawing]
[0008] [Figure 1] This is a phase diagram showing the state of matter in relation to temperature and pressure. [Figure 2] This is a phase diagram for defining the range of compressible fluids. [Figure 3] This is a schematic diagram showing an example of a continuous kneading apparatus used in the production of polylactic acid-based compositions. [Figure 4] This is a schematic diagram showing an example of a continuous foaming sheet manufacturing apparatus used in the production of foamed sheets according to one embodiment. [Modes for carrying out the invention]
[0009] Embodiments of the present invention will be described in detail below. However, the embodiments are not limited by the following description and can be modified as appropriate without departing from the spirit of the invention. Furthermore, in this specification, the "~" indicating a numerical range means that the values before and after it are included as the lower and upper limits, respectively, unless otherwise specified.
[0010] <Foam sheet> One embodiment of the foamed sheet is a polylactic acid foam produced by foaming a composition containing polylactic acid (polylactic acid-based composition), having a compressive stress of 0.2 MPa or less when the buffering coefficient is 10 or less, and a puncture strength of 2 N or more when the sheet thickness is 2 mm.
[0011] The compressive stress is determined in accordance with the method for measuring the compressive stress-strain characteristics described in JIS K 6400-2:2012 and ISO 3386-1. The cushioning coefficient can be determined in accordance with JIS Z 0235:2002 and ISO 4651 as described above. The cushioning coefficient represents the performance of the foamed sheet according to one embodiment in absorbing impact energy, and is a value obtained by dividing the compressive stress obtained by a compression test by the compressive energy per unit volume (cushioning coefficient = compressive stress / compressive energy per unit volume).
[0012] The compressive stress may be the average value of the cushioning coefficients obtained by measuring a plurality of locations (for example, three locations) of the foamed sheet according to one embodiment and dividing each compressive stress by the compressive energy, which is used as the cushioning coefficient of the foamed sheet according to one embodiment.
[0013] The cases where the compressive stress exceeds 0.02 MPa and is 0.05 MPa or less (compressive stress A), exceeds 0.05 MPa and is 0.2 MPa or less (compressive stress B), and exceeds 0.2 MPa and is 0.3 MPa or less (compressive stress C) may be measured, and the cushioning coefficient in the case of compressive stress A, compressive stress B, or compressive stress C may be measured. In any of compressive stress A, compressive stress B, and compressive stress C, the lower the cushioning coefficient, the better the cushioning performance is exhibited.
[0014] Specifically, the compressive stress is measured as follows. That is, as a measuring device for the compressive stress, a universal testing machine AG-50X, AGS-5kNX manufactured by Shimadzu Corporation, and a calibrated load cell of 5 kN are used. A circle with a diameter of 50 mm is punched out or cut out evenly from a roll or a sheet. When the sheet is thin, the necessary number of sheets is punched out or cut out so that it becomes 25 mm to 35 mm (when a sample is sandwiched between a pressure plate and a support plate fixed to a universal testing machine and a force of 2.9 N to 3.0 N is applied). The sheet is sandwiched between the pressure plate and the support plate, and pressurized at a speed of (100 ± 20) mm / min to (40 ± 1)% of the thickness of the test piece. If the stress does not reach 0.3 Mpa, the compression amount may be changed to 70% of the thickness. Also, based on the measured value of the first compression at that time, the cushioning coefficient is determined in accordance with JIS Z 0235:2002 and ISO4651. The above is repeated three times, and the cushioning coefficient is determined based on the average value of the three times.
[0015] The compression set is determined in accordance with JIS K 6767:1999 or ISO1856. When the bulk density of the foamed sheet is 0.025 g / cm 3 ~0.250 g / cm 3 in the case of, it is preferably 15% or less, more preferably 12.5% or less. If the compression set is 15% or less, the cushioning performance can be maintained even when the foamed sheet is repeatedly used.
[0016] Specifically, the compression set is measured as follows. That is, the test piece has parallel upper and lower surfaces and is a rectangular parallelepiped with sides of 50 mm square and a thickness of about 25 mm. When the sample is thin, stack them to a thickness of about 25 mm. Use a vernier caliper to measure the initial thickness. Prepare three test pieces. It consists of two parallel flat plates with a smooth surface and a sufficient thickness that does not bend even when force is applied, and four or more bolts and nuts, and sandwich the test piece in a compression device with a structure that can compress 25% from the initial thickness of the test piece. Then, leave it continuously for 22 hours at (23 ± 2) °C and a relative humidity of (50 ± 5) % in a state compressed by 25% from the initial thickness. Then, remove the sample from the compression device, leave it for 24 hours at (23 ± 2) °C and a relative humidity of (50 ± 5) %, and then measure the thickness at the same location as the location where the initial thickness was measured. The compression set is calculated from the following formula (I). Compression set = (Initial thickness - Thickness after test) / Initial thickness × 100 ··· (I)
[0017] As physical property values representing the strength of the foamed sheet according to one embodiment, there are the tensile strength (tensile strength), flexural strength, puncture strength, etc. of the foamed sheet. When using the foamed sheet as a cushioning material, it is important that the contents do not break out. Among these, a high puncture strength is particularly required.
[0018] The tensile strength of the foamed sheet is determined in accordance with JIS K 6767:1999. The tensile strength determined in accordance with JIS K 6767:1999 is for a foamed sheet with a bulk density of 0.025 g / cm³. 3 ~0.250g / cm 3 In this case, a tensile strength of 0.3 MPa to 5.0 MPa is preferable. If the tensile strength of the foam sheet is between 0.3 MPa and 5.0 MPa, problems such as tearing can be reduced when used as a cushioning material.
[0019] The bending strength (rigidity) of the foamed sheet is determined in accordance with JIS K 7171. The bending strength determined in accordance with JIS K 7171 is preferably 50 MPa to 140 MPa, and more preferably 60 MPa to 120 MPa. If the bending strength of the foamed sheet is 50 MPa to 140 MPa, the bulk density of the foamed sheet is 0.025 g / cm³. 3 ~0.250g / cm 3 In this case, the foam sheet can have sufficient strength, so even if external pressure is applied to the foam sheet, it will not bend easily and will not break. Also, the bulk density of the foam sheet is 0.5 g / cm³. 3 ~0.8g / cm 3 In this case, the foam sheet may contain fine foam particles. Even in this case, if the flexural strength of the foam sheet is between 50 MPa and 140 MPa, the foam sheet can have sufficient strength.
[0020] The puncture strength is determined in accordance with JIS Z 1707 using a sample of the foam sheet according to one embodiment with a sheet thickness of 2 mm. If the sheet thickness of the foam sheet according to one embodiment is thin, multiple foam sheets according to one embodiment may be stacked to make the total sheet thickness 2 mm and the puncture strength may be measured. If the sheet thickness of the foam sheet is thick, the foam sheet may be cut to a sheet thickness of 2 mm and the puncture strength may be measured.
[0021] The aforementioned puncture strength is measured specifically as follows: Specifically, the test specimen is fixed in a jig, and a semicircular needle with a diameter of 1.0 mm and a tip radius of 0.5 mm is inserted at a test speed of (50 ± 5) mm / min using, for example, a Shimadzu universal testing machine AG-50X, AGS-5kNX, and a 50N load cell, and the maximum force (in N) until the needle penetrates is measured. At least five test specimens are taken, and the results are averaged across the entire width of the product.
[0022] Conventional Patent Document 1 did not examine the cushioning properties of biodegradable resin laminated foam sheets. For a foam sheet containing polylactic acid to be used as a cushioning material, it is necessary for the foam sheet to have high cushioning properties. Furthermore, it is important that the foam sheet has high sheet strength to prevent damage such as tearing when struck by sharp objects.
[0023] The inventors of this application conducted thorough research on foamed sheets containing polylactic acid and focused on the compressive stress and puncture strength of the foamed sheets. They found that if the compressive stress of a foamed sheet containing polylactic acid is 0.2 MPa or less when the buffering coefficient is 10 or less, and the puncture strength is 2 N or more when the sheet thickness is 2 mm, then the foaming of the polylactic acid can be made fine and uniform. As a result, they found that foamed sheets containing polylactic acid can contain fine and uniform foaming inside, thus improving both buffering properties and sheet strength.
[0024] Generally, the cushioning performance of a foam sheet improves with increasing thickness, but the foam sheet according to one embodiment can exhibit excellent cushioning and puncture resistance even when the foam sheet is thin. Therefore, the foam sheet according to one embodiment can achieve both cushioning and sheet strength at the same thickness.
[0025] Furthermore, the cushioning properties of the foamed sheet according to one embodiment can be evaluated from the cushioning coefficient of the foamed sheet according to one embodiment. The sheet strength of the foamed sheet according to one embodiment can be evaluated from the puncture strength.
[0026] In biodegradability tests of biodegradable plastics conducted in accordance with JIS K 6953-2, the number of days required for 90% biodegradation is preferably 180 days or less, more preferably 120 days or less, and even more preferably 60 days or less.
[0027] The foamed sheet according to one embodiment contains polylactic acid and fillers, and further contains other components as needed. Since the foamed sheet according to one embodiment is produced from a polylactic acid-based composition, it is also called a polylactic acid-based composition foamed sheet. The components contained in the foamed sheet according to one embodiment will now be described.
[0028] [Polylactic acid] Polylactic acid (PLA) is a type of aliphatic polyester resin, a polymer formed by the polymerization of lactic acid through ester bonds. Because PLA is biodegradable by microorganisms, it is environmentally friendly and has a low environmental impact, making it useful in relation to microplastics that remain in nature.
[0029] The lactic acid constituting polylactic acid may be either the D-form (D-lactic acid) or the L-form (L-lactic acid), or both.
[0030] Examples of polylactic acid include D-lactic acid homopolymers, L-lactic acid homopolymers, copolymers of D-lactic acid and L-lactic acid (DL-lactic acid); and ring-opening polymers of one or more lactides selected from the group consisting of D-lactide, L-lactide, and DL-lactide. These may be used individually or in combination of two or more.
[0031] When a copolymer of D-lactic acid and L-lactic acid is used as the polylactic acid, there are no particular restrictions on the ratio of D-lactic acid to L-lactic acid, and it can be appropriately selected according to the purpose. In copolymers of D-lactic acid and L-lactic acid, as the decrease in the less abundant optical isomer, crystallinity tends to increase, and the melting point and glass transition temperature tend to rise. Conversely, as the increase in the less abundant optical isomer, crystallinity tends to decrease, eventually becoming amorphous. Crystallinity is related to the heat resistance of the foamed sheet and the molding temperature of the foam, so it can be used appropriately depending on the application, and is not particularly limited.
[0032] Crystallinity refers to the degree of crystallinity and the rate of crystallization. High crystallinity means at least one of the following: a high degree of crystallinity and a fast rate of crystallization.
[0033] Polylactic acid may be synthesized as appropriate or commercially available, but in order to improve its buffering performance as a buffering material, the weight-average molecular weight of polylactic acid determined by gel permeation chromatography (GPC) is preferably 100,000 or more, and more preferably 150,000 or more. On the other hand, there is no particular upper limit to the weight-average molecular weight of polylactic acid, but it is preferably 350,000 or less in order to prevent the viscosity from becoming too high and to facilitate manufacturing.
[0034] The weight-average molecular weight (Mw) of the foamed sheet according to this embodiment is not particularly limited and can be appropriately selected depending on the purpose, but it can be measured using GPC. For example, the foamed sheet according to this embodiment is placed in a tetrahydrofuran (THF) solution and heated to 65°C to dissolve the polylactic acid. Then, the solution is filtered through a 0.45 μm membrane filter to remove undissolved substances such as fillers contained in the THF solution. The weight-average molecular weight (Mw) of the obtained foamed sheet is measured using GPC with a calibration curve created using polystyrene samples with known molecular weights as a standard. The weight-average molecular weight (Mw) of the foamed sheet may also be measured based on the following measurement conditions, for example. Note that four TSKgel SuperHM-N columns (manufactured by Tosoh Corporation) connected in series may be used as the column. (Measurement conditions) • Device: HLC-8320 (manufactured by Tosoh) • Column: TSKgel SuperHM-N (manufactured by Tosoh Corporation) x 4 • Detector: RI ·Measurement temperature: 40℃ • Mobile phase: tetrahydrofuran ·Flow rate: 0.6mL / min
[0035] From the viewpoint of biodegradability and recyclability, the polylactic acid content is preferably 98% by mass or more, and more preferably 99% by mass or more, relative to the total amount of organic matter in the foamed sheet according to one embodiment. When the polylactic acid content is 98% by mass or more, even if the polylactic acid biodegrades, the remaining non-biodegradable components can be suppressed.
[0036] The lactic acid content in polylactic acid can be calculated from the proportion of materials that form the polylactic acid. If the material ratio is unknown, for example, analysis using gas chromatography-mass spectrometry (GC-MS) can be performed, and the components can be identified by comparison with known polylactic acid as a standard sample. Specifically, by determining a calibration curve in advance using known polylactic acid as a standard sample, the ratio of polylactic acid in the foamed sheet according to one embodiment can be determined. In addition, if necessary, the area ratio of spectra obtained by NMR measurement or other analytical methods can be combined to calculate the ratio. When using GC-MS, the polylactic acid content can be measured under the following conditions, for example. (Measured by GCMS) • GCMS:QP2010 auxiliary equipment, Frontier Lab Py3030D, manufactured by Shimadzu Corporation. • Separation column: Frontier Lab Ultra ALLOY UA5-30M-0.25F • Sample heating temperature: 300℃ • Column oven temperature: 50°C (held for 1 minute) ~ heating rate 15°C / min ~ 320°C (held for 6 minutes) • Ionization method: Electron Ionization (EI) method • Detection mass range: 25~700 (m / z)
[0037] [Filler] The filler has the function of adjusting the size and amount of bubbles contained in the foamed sheet according to one embodiment, and can be used as a foaming nucleating agent. By including the filler, the foamed sheet according to one embodiment can achieve a fine and uniform foam diameter, thereby achieving both puncture strength and cushioning properties.
[0038] Inorganic fillers, organic fillers, and the like can be used as fillers. These may be used individually or in combination of two or more types.
[0039] Since foaming occurs at the interface between the filler and polylactic acid, it is preferable to disperse the filler finely and uniformly.
[0040] The filler content is preferably 0.1% to 5.0% by mass. When the filler content is 0.1% or more by mass, it is sufficient to function as a foaming nucleus, and when the filler content is 5.0% or less by mass, the properties of the foamed sheet can be maintained, such as exhibiting sufficient impact resistance. The filler content is more preferably 0.2% to 4.0% by mass, and even more preferably 0.3% to 2.0% by mass.
[0041] Examples of inorganic fillers include talc, kaolin, calcium carbonate, layered silicates, zinc carbonate, wollastonite, silica, alumina, magnesium oxide, titanium oxide, calcium silicate, sodium aluminate, calcium aluminosilicate, magnesium silicate, glass balloons, carbon black, zinc oxide, antimony trioxide, zeolite, hydrotalcite, metal fibers, metal whiskers, ceramic whiskers, potassium titanate, boron nitride, graphite, glass fibers, and carbon fibers.
[0042] Examples of organic fillers include naturally occurring polymers such as starch, cellulose microparticles, wood flour, okara (soy pulp), rice husks, and wheat bran, as well as modified versions thereof, and also sorbitol compounds, benzoic acid and its metal salts, phosphate ester metal salts, and rosin compounds.
[0043] Among these, inorganic fillers are preferred due to their environmental impact. Among inorganic fillers, silica, titanium dioxide, and layered silicates are more preferred because they can be dispersed at the nanoscale and allow for uniform bubble formation.
[0044] [Other ingredients] Other components are generally included in foamed sheets and can be added in amounts that do not affect biodegradability. There are no particular restrictions on such additions, and they can be appropriately selected according to the purpose. Examples include, but are not limited to, aliphatic polyester resins other than polylactic acid, high molecular weight polymers such as polymethyl methacrylate resin (PMMA) and polystyrene added to control the foaming state, crosslinking agents, and other additives added for other purposes.
[0045] (Aliphatic polyester resins other than polylactic acid) Examples of aliphatic polyester resins other than polylactic acid include polyglycolic acid, poly(3-hydroxybutyrate), poly(3-hydroxybutyrate·3-hydroxyhexanoate), poly(3-hydroxybutyrate·3-hydroxyvalate), polycaprolactone, polybutylene succinate, and poly(butylene succinate·adipate). These may be used individually or in combination of two or more.
[0046] (Crosslinking agent) The crosslinking agent is not particularly limited as long as it is a compound that reacts with the hydroxyl groups and / or carboxylic acid groups of polylactic acid. For example, epoxy crosslinking agents (crosslinking agents having epoxy groups) or isocyanate crosslinking agents (crosslinking agents having isocyanate groups) are preferably used. As these crosslinking agents, for example, epoxy-functional (meth)acrylic-styrene crosslinking agents having two or more epoxy groups in the molecule, or polyisocyanates having two or more isocyanate groups in the molecule are preferred. Epoxy-functional (meth)acrylic-styrene crosslinking agents having three or more epoxy groups in the molecule, or polyisocyanates having three or more isocyanate groups in the molecule are more preferred because they can introduce a branched structure to polylactic acid, efficiently improve melt strength, and reduce the residue of unreacted substances. Using such crosslinking agents can suppress bubble coalescence and rupture, and improve the foaming ratio.
[0047] Here, an epoxy-functional (meth)acrylic-styrene crosslinking agent having two or more epoxy groups in its molecule is a polymer obtained by copolymerizing an epoxy-group-containing (meth)acrylic monomer with a styrene monomer.
[0048] Examples of (meth)acrylic monomers having epoxy groups include monomers containing 1,2-epoxy groups, such as glycidyl acrylate and glycidyl methacrylate. Examples of styrene monomers include styrene and α-methylstyrene.
[0049] An epoxy-functional (meth)acrylic-styrene crosslinking agent having two or more epoxy groups in its molecule may contain (meth)acrylic monomers that do not have epoxy groups as copolymer components. Examples of such (meth)acrylic monomers include methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, cyclohexyl acrylate, methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, and cyclohexyl methacrylate.
[0050] Examples of polyisocyanates having two or more isocyanate groups in the molecule include 1,6-hexamethylene diisocyanate, 3-isocyanate-methyl-3,5,5-trimethylcyclohexyl isocyanate (isophorone diisocyanate), 1,4-tetramethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, methylcyclohexyl-2,4-diisocyanate, and methylcyclohexyl-2 Aliphatic diisocyanates such as ,6-diisocyanate, xylylene diisocyanate, 1,3-bis(isocyanate)methylcyclohexane, tetramethylxylylene diisocyanate, transcyclohexane-1,4-diisocyanate, lysine diisocyanate, isophorone diisocyanate, hydrogenated diphenylmethane diisocyanate, hydrogenated tolylene diisocyanate, hydrogenated xylylene diisocyanate, hydrogenated tetramethylxylylene diisocyanate, cyclohexane diisocyanate, and other alicyclic polyisocyanates, 2,4-toluylene diisocyanate Aromatic diisocyanates such as sorbinate, 2,6-toluylene diisocyanate, diphenylmethane-4,4'-isocyanate, 1,5'-naphthene diisocyanate, toridine diisocyanate, diphenylmethylmethane diisocyanate, tetraalkyldiphenylmethane diisocyanate, 4,4'-dibenzyle diisocyanate, 1,3-phenylene diisocyanate, lysine ester triisocyanate, triphenylmethane triisocyanate, 1,6,11-undecane triisocyanate, and 1,8-isocyanate-4,4-isocyanate. Examples include triisocyanate compounds such as annetomethyloctane, 1,3,6-hexamethylene triisocyanate, bicycloheptane triisocyanate, adducts of trimethylolpropane and 2,4-toluylene diisocyanate, and adducts of trimethylolpropane and diisocyanates such as 1,6-hexamethylene diisocyanate, as well as modified polyisocyanate compounds obtained by reacting polyhydric alcohols such as glycerin and pentaerythritol with the aforementioned aliphatic and aromatic diisocyanate compounds and the aforementioned triisocyanate compounds.These can be used individually or in combination of two or more types.
[0051] By including a crosslinking agent, melt tension can be imparted, and the foaming ratio of the foamed sheet can be adjusted. Means for imparting melt tension include dispersing fillers such as layered silicates at the nano level, crosslinking the resin composition using a crosslinking agent or crosslinking aid, crosslinking the resin composition using an electron beam, and adding another resin composition having high melt tension.
[0052] (Additives) Examples of additives include heat stabilizers, antioxidants, and plasticizers. These may be used individually or in combination of two or more.
[0053] Regarding the content of other components, from the standpoint of recyclability, it is preferable that the content is 2% by mass or less, and more preferably 1% by mass or less, relative to the total amount of organic matter in the foamed sheet.
[0054] In one embodiment, it is preferable that the foamed sheet substantially does not contain organic compounds having a boiling point of -20°C or higher and less than 150°C. "Substantially contained" means that even if analyzed, the detected value is below the lower limit of the analytical instrument, or below the detected value when the same procedure is performed on the raw material polylactic acid. "Substantially contained" means that the organic compound content is substantially 0% by mass, not 0% by mass. That is, organic compounds may be present as unavoidable impurities, for example, at a concentration of 0.1% by mass or less. Examples of organic compounds with a boiling point of -20°C or higher and less than 150°C include volatile components. If the volatile components are, for example, organic solvents or blowing agents such as butane, their presence in the foamed sheet affects the dimensional stability of the foamed sheet and also impacts the environment. In one embodiment, the foamed sheet can use a blowing agent other than organic compounds such as CO2, and the volatile component content can be substantially reduced to 0% by mass, thus allowing for safe handling without generating odors.
[0055] <Physical properties of foamed sheets> The physical properties of the foamed sheet according to one embodiment will be described in terms of bulk density, expansion ratio, average cell diameter, sheet thickness, and amount of residual volatile components.
[0056] (Bulk density) The bulk density of the foamed sheet according to one embodiment is preferably 0.025 g / cm 3 ~0.250 g / cm 3 more preferably 0.031 g / cm 3 ~0.125 g / cm 3 even more preferably 0.036 g / cm 3 ~0.083 g / cm 3 If the bulk density is within the above preferred range, the foamed sheet according to one embodiment can have an excellent balance between sheet strength and cushioning properties.
[0057] The bulk density refers to the density of the internal volume when the foamed sheet is filled in a container. The method for measuring the bulk density is not particularly limited, and any appropriate method for measuring the bulk density can be used. For example, it can be measured by the following method. Measure the outer dimensions of the foamed sheet left standing for 24 hours or more in an environment of temperature 23°C and relative humidity 50% to obtain the bulk volume. Then, measure the weight of this foamed sheet. The bulk density of the foamed sheet is obtained by dividing the weight of the foamed sheet by the bulk volume.
[0058] (Expansion ratio) The expansion ratio of the foamed sheet according to one embodiment is preferably 5 to 50 times, more preferably 10 to 40 times, and even more preferably 15 to 35 times. If the expansion ratio is within the above preferred range, the foamed sheet according to one embodiment can maintain the cushioning performance and strength.
[0059] Note that the expansion ratio of the foamed sheet according to one embodiment can be obtained by dividing the density (true density ρ0) of the polylactic acid-based composition constituting the foamed sheet by the bulk density (ρ1) as shown in the following formula (1). Here, the true density is the density of the raw material polylactic acid, and it may be a literature value or the actual measurement of the raw material pellets. The true density is about 1.25 g / cm 3 is. Expansion ratio = True density (ρ0) / Bulk density (ρ1) ... (1)
[0060] (Average foam diameter) The average foam diameter of the foamed sheet according to one embodiment is preferably 10 μm to 200 μm, more preferably 20 μm to 100 μm, and even more preferably 30 μm to 80 μm, although this also depends on the bulk density.
[0061] The average foam diameter can be adjusted as appropriate by factors such as the filler content, the dispersion state of the foam, and the melt tension of the foam sheet, but is not limited to these factors. For example, if the bulk density is 0.025 g / cm³ 3 ~0.250g / cm 3 In this case, the average foam diameter is preferably 100 μm or less.
[0062] The method for measuring the average foam diameter is not particularly limited and can be appropriately selected depending on the purpose. For example, a foam sheet can be cross-sectioned using an ion milling device, and the cross-section can be photographed with a scanning electron microscope (SEM) to obtain an SEM image. The obtained cross-sectional SEM image (magnification, for example, 3000x) can be binarized using Image-Pro Premier software (manufactured by mediacy) to separate the gray component corresponding to foam (voids) from the white component corresponding to the resin. Next, the average particle size (Ferret diameter) of the gray component corresponding to foam within a predetermined range (for example, 35 μm × 20 μm) can be determined. The average foam diameter can be calculated by calculating the average value of only the gray component (foam) with a Ferret diameter of 0.5 μm or more.
[0063] (Sheet thickness) The sheet thickness of the foamed sheet according to one embodiment is preferably 1.0 mm to 10.0 mm, more preferably 1.5 mm to 7.0 mm, and even more preferably 2.0 mm to 5.0 mm. If the sheet thickness is within the above preferred range, the foamed sheet according to one embodiment can be foamed finely and uniformly, so the foamed sheet according to one embodiment can be easily molded and can have sufficient cushioning properties.
[0064] The sheet thickness may be the average thickness. Alternatively, the average thickness may be calculated by measuring the thickness of the foam sheet at multiple points in the cross-section of the foam sheet and taking the average of these measured thicknesses.
[0065] In one embodiment, the foamed sheet has a compressive stress of 0.2 MPa or less when the buffering coefficient is 10 or less, preferably 0.02 MPa to 0.1 MPa, and more preferably 0.02 MPa to 0.05 MPa. If the compressive stress is 0.2 MPa or less, the sheet exhibits excellent buffering properties.
[0066] In one embodiment, the foamed sheet has a puncture strength of 2N or more when the sheet thickness is 2 mm, preferably 2.5N to 5N, and more preferably 3N to 5N. If the puncture strength is 2N or more, it is possible to suppress tearing caused by protrusions, etc., when used as a cushioning material.
[0067] <Method for manufacturing foamed sheets> A method for manufacturing a foamed sheet according to one embodiment includes a kneading step and a foaming step, and further includes other steps as necessary. In the method for manufacturing a foamed sheet according to one embodiment, the kneading step and the foaming step may be performed simultaneously or separately.
[0068] [Mixing process] In the mixing process, polylactic acid and filler are mixed in the presence of a compressible fluid at a temperature lower than the melting point of polylactic acid. In the mixing process, it is preferable to add a blowing agent in addition to the polylactic acid and filler in order to promote foaming more efficiently. The mixture containing polylactic acid, filler, and blowing agent before foaming is also called a polylactic acid-based composition (masterbatch).
[0069] (Foaming agent) Examples of foaming agents that easily produce foamed sheets with a high foaming ratio include hydrocarbons such as propane, n-butane, isobutane, n-pentane, isopentane, and lower alkanes such as hexane; ethers such as dimethyl ether; halogenated hydrocarbons such as methyl chloride and ethyl chloride; and physical foaming agents such as compressible fluids (also called compressible gases) such as carbon dioxide and nitrogen. Among these, it is preferable to use compressible fluids such as carbon dioxide and nitrogen because they are odorless, safe to handle, and have a low environmental impact. As a result, the foamed sheet according to one embodiment is substantially free of organic compounds with a boiling point of -20°C or higher and less than 150°C. That is, the content of organic compounds with a boiling point of -20°C or higher and less than 150°C is substantially 0% by mass.
[0070] Aliphatic polyester resins such as polylactic acid have the property of rapidly decreasing melt viscosity after their melting point, so when mixing fillers with polylactic acid, the fillers tend to aggregate. When the fillers are small, the aggregation of fillers is particularly pronounced. Therefore, in this embodiment, it is preferable to mix the polylactic acid and fillers using a compressible fluid. This allows the fillers to be uniformly dispersed in the polylactic acid.
[0071] It is preferable that the compressible fluid is the same as the blowing agent. When the compressible fluid is the same as the blowing agent, the mixing and foaming of the filler can be carried out in a single process, thereby reducing the environmental impact.
[0072] This explains why it is preferable to use a compressible fluid for mixing fillers and polylactic acid. Generally, compressible fluids plasticize resins such as aliphatic polyester resins, and the melt viscosity of the resin tends to decrease (see "Latest Application Technologies of Supercritical Fluids," NTS). At first glance, a decrease in melt viscosity and an improvement in kneadability seem contradictory. In fact, by applying pressure without using a compressible fluid in the mixing of general fillers, the free volume of the resin can be reduced, increasing the interaction between resins (increasing viscosity). However, the resin becomes more difficult to plasticize ("k. Yang. R. Ozisik R. Polymer, 47.2849 (2006)"). reference).
[0073] It has been known that compressible liquids have the property of plasticizing (softening) resins, and that raising the temperature of a compressible liquid causes the resin to become liquid-like. When fillers are dispersed in a resin under these conditions, it is as if the fillers are dispersed in a liquid, and the fillers aggregate in the liquid. Therefore, a resin composition in which the fillers are highly dispersed cannot be obtained. In other words, it was thought that it was difficult to use compressible liquids for mixing resins and fillers because resins do not have a viscosity suitable for kneading in the presence of a compressible fluid.
[0074] The inventors of this invention investigated whether a compressible fluid could be used in the mixing of polylactic acid and filler. As a result, they found that, in the presence of a compressible fluid, if the temperature is lower than the melting point of polylactic acid, the polylactic acid has a viscosity suitable for mixing, and the filler can be mixed with the polylactic acid. In particular, polylactic acid, whose melt viscosity decreases rapidly above its melting point, could previously only be mixed in a state of low melt viscosity. However, in this embodiment, the filler can be mixed even when the polylactic acid is in a high viscosity state, and the compressible fluid can be used directly as a foaming agent.
[0075] (Compressible fluid) Examples of substances that can be used in the form of a compressible fluid include carbon monoxide, carbon dioxide, nitrous oxide, nitrogen, methane, ethane, propane, 2,3-dimethylbutane, ethylene, and dimethyl ether. Among these, carbon dioxide is preferred because it has a critical pressure of approximately 7.4 MPa and a critical temperature of approximately 31°C, can easily produce a supercritical state, and is non-flammable and easy to handle. These compressible fluids may be used individually or in combination of two or more.
[0076] Here, the compressible fluid used in the production of polylactic acid resin compositions will be explained using Figures 1 and 2. Figure 1 is a phase diagram showing the state of a substance in relation to temperature and pressure. Figure 2 is a phase diagram defining the range of compressible fluids. In this embodiment, a compressible fluid means the state in which a substance exists in any of the regions (1), (2), and (3) shown in Figure 2 within the phase diagram shown in Figure 1.
[0077] In these regions, substances become extremely dense and are known to behave differently than they do at room temperature and pressure. When a substance exists in region (1), it becomes a supercritical fluid. A supercritical fluid is a fluid that exists as a non-condensable, high-density fluid in a temperature and pressure region beyond the limit (critical point) where gas and liquid can coexist, and does not condense even when compressed. When a substance exists in region (2), it becomes a liquid, but it represents a liquefied gas obtained by compressing a substance that is in a gaseous state at room temperature (25°C) and atmospheric pressure (1 atm). When a substance exists in region (3), it is in a gaseous state, but it represents a high-pressure gas with a pressure of 1 / 2 (1 / 2Pc) or higher than the critical pressure (Pc).
[0078] The solubility of the compressible fluid changes depending on the type of resin, the combination of compressible fluid, temperature, and pressure, so the amount of compressible fluid supplied needs to be adjusted as appropriate. For example, when the compressible fluid is carbon dioxide, in the case of a combination of polylactic acid and carbon dioxide, the amount of carbon dioxide supplied is preferably 2% to 30% by mass. If the amount of carbon dioxide supplied is 2% by mass or more, the problem of limited plasticization effect can be suppressed. If the amount of carbon dioxide supplied is 30% by mass or less, the carbon dioxide and polylactic acid will separate, and the foamed sheet can have a uniform thickness.
[0079] (Mixing device) For the production of polylactic acid-based compositions, a continuous process or a batch process can be used in the kneading equipment. However, it is preferable to select the appropriate reaction process considering equipment efficiency, product characteristics, quality, etc.
[0080] As for the mixing equipment, single-screw extruders, twin-screw extruders, kneaders, shaftless cage-type mixing tanks, Sumitomo Heavy Industries' Bivolac, Mitsubishi Heavy Industries' N-SCR, Hitachi's spectacle blades, grid blades, or Kenix or Sulzer type SMLX static mixer equipped tubular polymerization tanks can be used, as they can handle viscosities suitable for mixing. From the standpoint of color tone, self-cleaning polymerization equipment such as finishers, N-SCRs, and twin-screw extruders can be used. Among these, finishers and N-SCRs are preferred in terms of production efficiency, resin color tone, stability, and heat resistance.
[0081] A continuous kneading apparatus, such as the one shown in Figure 3, can be used as the kneading apparatus. Figure 3 is a schematic diagram showing an example of a continuous kneading apparatus used in the production of polylactic acid-based compositions. As shown in Figure 3, the continuous kneading apparatus 10 comprises an extruder 11, quantitative feeders 12A and 12B, and a gas introduction section 13.
[0082] The extruder 11 has a raw material mixing and melting area a, a compressible fluid supply area b, a kneading area c, a compressible fluid removal area d, and a molding area e inside. For example, a twin-screw extruder can be used as the extruder 11. The screw bore, the ratio of the screw shaft diameter L to the screw shaft length D L / D, etc., of the extruder 11 can be set to any size as appropriate.
[0083] The quantitative feeder 12A introduces polylactic acid, which is a raw material for the foamed sheet, into the raw material mixing and melting area a. The quantitative feeder 12B supplies filler, which is a raw material for the foamed sheet, into the raw material mixing and melting area a.
[0084] The gas inlet 13 supplies compressible fluid from the gas tank 131 to the compressible fluid supply area b using a metering pump 132.
[0085] The continuous kneading device 10 generates a polylactic acid-based composition by kneading polylactic acid and filler together with a compressible fluid in the raw material mixing and melting area a, compressible fluid supply area b, kneading area c, and compressible fluid removal area d within the extruder 11. Next, in the molding area e, the polylactic acid-based composition is molded into pellets or the like.
[0086] (Raw material mixing and melting area) In the raw material mixing and melting area a, polylactic acid and filler are mixed and heated. The heating temperature is set to be above the melting temperature of polylactic acid to melt the polylactic acid, creating a polylactic acid-based composition containing the filler within the molten polylactic acid. This allows the compressible fluid supplied to the extruder 11 in the subsequent compressible fluid supply area b to be uniformly mixed with the polylactic acid-based composition.
[0087] (Compressible fluid supply area) In the compressible fluid supply area b, a compressible fluid is supplied into the extruder 11 to plasticize the molten polylactic acid contained in the polylactic acid composition.
[0088] (Mixing area) In the kneading area c, the temperature of the kneading area c is set to achieve a viscosity suitable for kneading the filler. The set temperature varies depending on the specifications of the continuous kneading device 10, the type, structure, and molecular weight of the polylactic acid, and is adjusted as appropriate. For example, when the weight-average molecular weight Mw of the polylactic acid is about 200,000, kneading was generally performed at a temperature 10°C to 20°C above the melting point of the polylactic acid. In contrast, in this embodiment, the polylactic acid-based composition has a relatively high viscosity even at temperatures below the melting point of the polylactic acid, so the polylactic acid-based composition can be kneaded at a temperature below the melting point of the polylactic acid.
[0089] A temperature lower than the melting point of polylactic acid is preferably -20°C to -80°C, and more preferably -30°C to -60°C.
[0090] The temperature of the kneading area c can be set lower than the melting point of polylactic acid. For example, if the temperatures of the raw material mixing / melting area a, the compressible fluid supply area b, and the compressible fluid removal area d are 190°C, the set temperature of the kneading area c can be 150°C.
[0091] The set temperature should be determined based on the current value of the stirring power of the continuous mixing device 10, etc.
[0092] (Compressible fluid removal area) In the compressible fluid removal area d, the pressure valve 14 installed in the extruder 11 is opened to discharge the compressible fluid inside the extruder 11 to the outside.
[0093] (Molding and processing area) In molding area e, the polylactic acid composition is molded into a polylactic acid composition having any desired shape, such as pellets.
[0094] The pressure in each area of the extruder 11 can be set as appropriate; for example, the pressure from the compressible fluid supply area b to the compressible fluid removal area d can be set to 7 MPa.
[0095] In this embodiment, a polylactic acid-based composition that has been molded into any shape may be mixed and kneaded again with polylactic acid to form a polylactic acid-based composition. In this case, an extruder similar to the extruder 11 may be used, and the process may be carried out in the same manner as the raw material mixing / melting area a, compressible fluid supply area b, kneading area c, compressible fluid removal area d, and molding area e.
[0096] [Foaming process] The foaming process involves removing the compressible fluid contained in the polylactic acid composition and causing the polylactic acid composition to foam.
[0097] Compressible fluid can be removed by reducing the pressure inside the extruder 11 of the continuous mixing device 10.
[0098] During the foaming process, it is preferable to heat the material to a temperature above the melting point of polylactic acid.
[0099] In the foaming process, the compressible fluid dissolved in the polylactic acid composition vaporizes and precipitates at the interface with the filler when the solubility of the compressible fluid is changed by operations such as reduced pressure or heating, causing foaming. Since foaming is initiated by the filler, a polylactic acid foam with uniform and fine foam can only be produced when the filler is uniformly dispersed in the polylactic acid.
[0100] [Other processes] Other processes can be any process that is normally carried out in the manufacture of foamed sheets, and can be selected as appropriate depending on the purpose. Examples include a molding process for processing polylactic acid foam into foamed sheets, and a printing process for applying markings to the surface of the foamed sheets.
[0101] The molding method is not particularly limited, and commonly used molding methods for thermoplastic resins can be used. Examples of molding methods include using molds such as vacuum forming, pressure forming, vacuum pressure forming, and press forming to form polylactic acid foam into a sheet to produce a foamed sheet.
[0102] A foamed sheet according to one embodiment is obtained by molding polylactic acid foam into a sheet shape through a molding process.
[0103] The printing process is not particularly limited and can be used as long as it is a method that can apply printing or the like to the surface of the foamed sheet according to one embodiment.
[0104] One embodiment of the foamed sheet contains polylactic acid and filler, has a compressive stress of 0.2 MPa or less when the buffering coefficient is 10 or less, and a puncture strength of 2 N or more when the sheet thickness is 2 mm. As a result, fine and uniform foam can be formed within the foamed sheet. When polylactic acid is heated to a temperature near its melting point, its viscosity decreases rapidly, making it prone to foam collapse and foam coalescence, making it difficult to refine and homogenize the foam. Even with the inclusion of polylactic acid, the foamed sheet according to one embodiment can contain fine and uniform foam by having a compressive stress of 0.2 MPa or less when the buffering coefficient is 10 or less, and a puncture strength of 2 N or more when the sheet thickness is 2 mm. Therefore, the foamed sheet according to one embodiment can improve both buffering capacity and sheet strength.
[0105] In one embodiment, the foamed sheet can achieve a compressive stress of 0.05 MPa or less. As a result, the foamed sheet in one embodiment can enhance its cushioning properties even at a compressive stress of 0.05 MPa or less.
[0106] The foamed sheet according to one embodiment can achieve a puncture strength of 5N or less. This ensures that the foamed sheet according to one embodiment can reliably maintain its cushioning properties.
[0107] The foamed sheet according to one embodiment can achieve a puncture strength of 3N or more. This allows the foamed sheet according to one embodiment to maintain a more reliable increase in sheet strength.
[0108] In one embodiment, the foamed sheet can have a thickness of 1 mm to 10 mm. This allows the foamed sheet according to one embodiment to have improved cushioning and sheet strength.
[0109] In one embodiment, the foamed sheet can have a foaming ratio of 5 to 50 times. This allows the foamed sheet according to one embodiment to have even greater cushioning properties.
[0110] According to one embodiment, the foamed sheet has a bulk density of 0.025 g / cm³. 3 ~0.250g / cm 3This makes it possible. As a result, the foamed sheet according to one embodiment can have a good balance of sheet strength and cushioning properties.
[0111] A foamed sheet according to one embodiment can substantially contain no organic compounds with a boiling point of -20°C or higher and less than 150°C. Since a foamed sheet according to one embodiment can be foamed using a compressible fluid such as CO2 or N2 as a foaming agent, the content of organic solvents and volatile components such as butane used in the foaming agent, which are organic compounds with a boiling point of -20°C or higher and less than 150°C, can be substantially reduced to 0% by mass. Therefore, a foamed sheet according to one embodiment has excellent dimensional stability and can drastically reduce its environmental impact.
[0112] In one embodiment, the foamed sheet can have a polylactic acid content of 98% by mass or more relative to the total amount of organic matter in the foamed sheet. As a result, the foamed sheet according to one embodiment can be biodegraded with high efficiency when reused after use, and can be easily recycled.
[0113] In one embodiment, the foamed sheet can have a filler content of 0.1% to 5.0% by mass. This allows the foamed sheet according to one embodiment to further reliably improve its cushioning properties.
[0114] As described above, the foamed sheet according to one embodiment has high cushioning properties and sheet strength, and can therefore be suitably used as a packaging material, cushioning material, etc.
[0115] <Product> A product according to one embodiment includes a foamed sheet according to one embodiment, and further includes other components as needed. The other components are not particularly limited as long as they are commonly used in resin products, and can be appropriately selected depending on the purpose.
[0116] Examples of manufactured products (also referred to as "consumer goods") according to one embodiment include, for example, household goods such as bags, packaging containers, trays, tableware, cutlery, stationery, and cushioning materials. This concept of manufactured products includes not only raw materials such as rolls of sheets as intermediates for processing manufactured products, but also components consisting of manufactured products such as tray handles, and products equipped with manufactured products such as trays with attached handles.
[0117] Examples of bags include shopping bags, grocery bags, and garbage bags.
[0118] Examples of stationery items include clear files and patches.
[0119] Conventional foamed sheets had large foam diameters and significant variations, resulting in problems with sheet properties such as strength and flexibility. The manufactured product according to one embodiment has superior physical properties and can be applied to uses other than the above-mentioned household goods. For example, it can be widely applied to industrial materials, daily necessities, agricultural products, food products, pharmaceuticals, cosmetics, and other sheet and packaging materials. [Examples]
[0120] The embodiments will be described in more detail below with reference to examples and comparative examples, but the embodiments are not limited to these examples and comparative examples.
[0121] <Example 1> [Production of foam sheets] The foamed sheets were produced using the continuous mixing apparatus 10 shown in Figure 3 and the continuous foamed sheet production apparatus shown in Figure 4, so the explanation will be given with reference to Figures 3 and 4.
[0122] (Masterbatch preparation) The polylactic acid-based composition was prepared using the continuous mixing apparatus 10 shown in Figure 3. First, polylactic acid (Revode 110, manufactured by HISUN, melting point 160°C) and titanium dioxide (TTO-55(C), manufactured by Ishihara Sangyo Co., Ltd., average particle size 0.004 μm), which is a filler (foaming nucleating agent), were supplied to the raw material mixing and melting area a so that the total filler flow rate was 10 kg / h. The flow rate of polylactic acid was set to 9.7 kg / h, and the flow rate of filler was set to 0.3 kg / h. Next, carbon dioxide, a compressible fluid, was supplied to the compressible fluid supply area b at a flow rate of 0.99 kg / h (equivalent to 10% by mass relative to polylactic acid). Then, the polylactic acid, filler, and compressible fluid were kneaded in the mixing area c to obtain a polylactic acid-based composition containing 3% by mass of filler. Next, the compressible fluid in the extruder 11 was evacuated in the compressible fluid removal area d, and the polylactic acid composition containing 3% by mass of filler was extruded in strand form in the molding area e, cooled, and then pelletized with a cutter. This yielded a polylactic acid foam containing 3% by mass of filler (a masterbatch containing 3% by mass of filler).
[0123] The temperatures in each area were set as follows: raw material mixing and melting area a and compressible fluid supply area b were 190°C, kneading area c was 150°C, compressible fluid removal area d was 190°C, and molding area e was 190°C.
[0124] The pressure in each area was set to 7.0 MPa in the compressible fluid supply area b and the mixing area c, and to 0.5 MPa in the compressible fluid removal area d.
[0125] The obtained masterbatch contained 20 coarse particles of 10 μm or larger per gram, as determined by the following measurement method. -Number of coarse filler particles- 50 mg of masterbatch was remelted to form a 10 μm thin film. The number of coarse particles with a particle size of 10 μm or larger, attributed to the filler, was counted using an optical microscope (Nikon FX-21, 100x magnification). This procedure was repeated five times, and the average value was taken as the number of coarse filler particles.
[0126] (Preparation of foam sheets) Next, a continuous foaming sheet forming apparatus 20 shown in Figure 4 was used. The continuous foaming sheet forming apparatus 20 is equipped with a first extruder 21A and a second extruder 21B connected in series. (Masterbatch preparation) The 3 mass% filler-containing masterbatch obtained in the continuous kneading apparatus 10 shown in Figure 3 was supplied to the quantitative feeder 22A, and polylactic acid (Revode 110, manufactured by HISUN, melting point 160°C) was supplied to the quantitative feeder 22B. Then, the 3 mass% filler-containing masterbatch and polylactic acid were supplied to the raw material mixing and melting area a of the first extruder 21A so that their total flow rates were 10 kg / hr. To ensure that the filler flow rate was 0.5 mass%, the flow rate of the obtained 3 mass% filler-containing masterbatch was set to 1.67 kg / h and the flow rate of the polylactic acid was set to 8.33 kg / h.
[0127] Next, carbon dioxide, a compressible fluid, was supplied to the compressible fluid supply area b from the gas inlet 23A at a flow rate of 0.99 kg / h (equivalent to 10% by mass relative to polylactic acid). In addition, isocyanurate (Duranate TPA-100, Asahi Kasei Corporation), a crosslinking agent, was supplied from the gas inlet 23B at a flow rate of 0.05 kg / h (0.5% relative to the resin).
[0128] Then, a masterbatch containing 3% by mass of filler, polylactic acid, and a crosslinking agent were kneaded with a compressible fluid in kneading area c and supplied to the second extruder 21B.
[0129] The mixture kneaded in the kneading area c was supplied to the second extruder 21B at a discharge rate of 10 kg / h from a circular mold (slit diameter 70 mm) attached to the tip of the second extruder 21B, and kneaded in the second heating area d while cooling the resin temperature to 140°C. Then, the compressible fluid was removed from the mixture and it was extruded and foamed, and the cylindrical polylactic acid foamed sheet extruded and foamed from the slit 241 of the circular die 24 was placed along the cooling mandrel 25, and its outer surface was cooled and molded by blowing air from the air ring. After that, the cooled and molded polylactic acid resin foamed sheet was cut with a cutter to make a flat sheet, passed through the roller 26, and then wound up with the winding roller 27 to obtain a foamed sheet.
[0130] The temperatures in each area were set as follows: in the first extruder 21A, the raw material mixing and melting area a and the compressible fluid supply area b were set to 190°C, the kneading area c was set to 150°C, and in the second extruder 21B, the second heating area d was set to 140°C.
[0131] The pressure in each area was set to 7.0 MPa from the compressible fluid supply area b to the second extruder heating area d.
[0132] <Examples 2 and 3> In Example 1, the foam sheets of Examples 2 and 3 were prepared in the same manner as in Example 1, except that the amount of filler was changed to the value shown in Table 1.
[0133] <Example 4> A foamed sheet was prepared in the same manner as in Example 1, except that the type of filler was changed to silica (QSG-30, manufactured by Shin-Etsu Chemical Co., Ltd., average particle size 0.004 μm).
[0134] <Examples 5 and 6> A foamed sheet was prepared in the same manner as in Example 1, except that the type of crosslinking agent was changed to a glycidyl ester-containing crosslinking agent (Joncryl 4368C, BASF).
[0135] <Example 7> In Example 1, the procedure was carried out in the same manner as in Example 1, except that the feed was changed to 8 kg / hr, and a foamed sheet with a thickness of 0.8 mm was produced.
[0136] <Comparative Example 1> A foamed sheet was prepared in the same manner as in Example 1, except that the filler and crosslinking agent were not included.
[0137] <Comparative Example 2> In Example 1, a foamed sheet was prepared in the same manner as in Example 1, except that the filler was changed to heavy calcium carbonate (Softon 2200, manufactured by Shiraishi Calcium Co., Ltd., average particle size 1.000 μm). The average particle size of the filler after kneading was 0.420 μm.
[0138] <Comparative Example 3> A foamed sheet was prepared in the same manner as in Example 5, except that the content of the crosslinking agent was changed.
[0139] Table 1 shows the components of the foamed sheets in each example and comparative example.
[0140] <Physical properties> The physical properties of the obtained foamed sheet were measured, including bulk density, average foam diameter, sheet thickness, buffer coefficient, and puncture strength. The measurement results are shown in Table 1.
[0141] [Bulk density] The bulk volume of a foamed sheet was determined from its external dimensions after being left for more than 24 hours in an environment with a temperature of 23°C and a relative humidity of 50%. Next, the weight (g) of this foamed sheet was accurately weighed. The bulk density was calculated by dividing the weight of the foamed sheet by its bulk volume, as shown in formula (2) below. Bulk density = weight of foam sheet / bulk volume of foam sheet ... (2)
[0142] [Average foam diameter] The obtained foamed sheet was cross-sectionally processed using an ion milling apparatus, and the cross-section was observed using SEM. The obtained cross-sectional SEM images (magnification 3000x) were binarized using Image-Pro Premier (mediacy) software to separate the gray component (corresponding to foaming (voids)) from the resin component (white). The average particle size (ferret diameter) was determined within a 35 μm × 20 μm area, and the average foam diameter was calculated for the gray component (foaming) with a ferret diameter of 0.5 μm or more. The average foam diameter was calculated as the average of three foaming locations.
[0143] [Sheet thickness] The obtained foamed sheet was cross-sectionally processed using an ion milling apparatus, and the cross-section was observed using SEM. The obtained cross-sectional SEM images (magnification 100x) were used with Image-Pro Premier software (mediacy). A 1mm area was measured 10 times as one field of view, and the average value for one field of view was calculated. This was done for three fields of view, and the average value of the three fields of view was taken as the sheet thickness.
[0144] [Content of residual volatile components] 1 part by mass of the obtained foamed sheet was added to 2 parts by mass of 2-propanol, dispersed by ultrasound for 30 minutes, and then stored in a refrigerator (5°C) for at least one day to extract the volatile components from the composition. The supernatant of the stored dispersion was analyzed by gas chromatography (GC-14A, Shimadzu Corporation) to quantify and measure the volatile components in the composition. As a reference, polylactic acid resin (Revode110) was measured using the same procedure, and if the value was below the reference, it was considered to be the detection limit. If the volatile components were below the detection limit, it was evaluated as ○, and if the volatile components exceeded the detection limit, it was evaluated as ×. (Measurement conditions) • Equipment: GC-14A (manufactured by Shimadzu Corporation) • Column: CBP20-M 50-0.25 • Detector: FID ·Injection volume: 1μL~5μL Carrier gas: He 2.5 kg / cm³ 2 Hydrogen flow rate: 0.6 kg / cm³ 2 • Airflow rate: 0.5 kg / cm² 2 • Chart speed: 5mm / min Sensitivity: Range 101 × Atten 20 Column temperature: 40°C Injection Temp: 150℃
[0145] [Buffering properties] The cushioning properties of the obtained foamed sheet were evaluated using the cushioning coefficient. To determine the buffer coefficient, the compressive stress was first measured. A universal testing machine (AG-50X, manufactured by Shimadzu Corporation) and a calibrated 5kN load cell were used to measure the compressive stress. Circles with a diameter of 50 mm were punched out evenly from the sheet. At this time, the required number of sheets were punched out so that the thickness of the sheet would be 25 mm to 35 mm when the sample was placed between the pressure plate and the support plate fixed to the universal testing machine and a force of 2.9 N to 3.0 N was applied. The sheet was then placed between the pressure plate and the support plate and compressed at a speed of (100 ± 20) mm / min until it reached (40 ± 1)% of the thickness of the test piece. If the stress did not reach 0.3 MPa, the compression amount was changed to 70% of the thickness. Then, based on the first measured compressive stress, the buffer coefficient was determined in accordance with JIS Z 0235:2002 and ISO 4651. The above procedure was repeated three times, and the average of the three buffer coefficients was calculated. The average of the three calculated buffer coefficients was used as the buffer coefficient for the foamed sheet and evaluated according to the following evaluation criteria. The buffer coefficient was measured when the compressive stress was greater than 0.02 MPa but less than or equal to 0.05 MPa (compressive stress A), greater than 0.05 MPa but less than or equal to 0.2 MPa (compressive stress B), and greater than 0.2 MPa but less than or equal to 0.3 MPa (compressive stress C). Buffer coefficient = compressive stress / compressive energy per unit volume ... (3) (Evaluation Criteria) ◎: The buffer coefficients for compressive stresses A, B, and C are all 10 or less. ○: The buffer coefficient is 10 or less under compressive stresses A and B, but not 10 or less under compressive stress C. △: The buffering coefficient is 10 or less under compressive stress A, but not 10 or less under compressive stresses B and C. ×: The buffer coefficients for compressive stresses A, B, and C are not all 10 or less.
[0146] [Piercing strength] Using a sample of foamed sheet with a sheet thickness of 2 mm, the puncture strength was determined in accordance with JIS Z 1707. The sheet strength of the foamed sheet was evaluated based on the puncture strength.
[0147] [Table 1]
[0148] Table 1 confirms that the foamed sheets obtained in Examples 1 to 6 met the aforementioned conditions for both puncture strength and cushioning (puncture strength of 2N or higher and cushioning of ◎ or ○). In contrast, the foamed sheets obtained in Comparative Examples 1 to 3 did not meet the aforementioned conditions for at least one of puncture strength or cushioning, resulting in an unacceptable deterioration of quality. Therefore, it was confirmed that the foamed sheets obtained in Comparative Examples 1 to 3 could not achieve all the required properties and had practical problems.
[0149] Therefore, unlike the foam sheets of Comparative Examples 1 to 3, the foam sheets of Examples 1 to 6 can achieve a compressive stress of 0.2 MPa or less at which the buffering coefficient is 10 or less, and a puncture strength of 2.4 N or more as determined by JIS Z 1707 when the sheet thickness is 2 mm. As a result, the foam sheets of Examples 1 to 6 can have excellent buffering properties and sheet strength.
[0150] As described above, embodiments have been explained, but these embodiments are presented as examples only, and the present invention is not limited by these embodiments. The above embodiments can be implemented in various other forms, and various combinations, omissions, substitutions, and modifications are possible without departing from the spirit of the invention. These embodiments and their variations are included in the scope and spirit of the invention, as well as in the claims of the invention and its equivalents. [Explanation of symbols]
[0151] 10 Continuous mixing device 20 Continuous foaming sheet forming machine [Prior art documents] [Patent Documents]
[0152] [Patent Document 1] Japanese Patent Publication No. 2012-030571
Claims
1. The product uses as a raw material a foamed sheet which contains polylactic acid and a filler, has a compressive stress of 0.2 MPa or less when the cushioning coefficient is 10 or less, and has a puncture strength of 2 N or more when the sheet thickness is 2 mm.
2. 2. A product using the foamed sheet according to claim 1 as a raw material, wherein the compressive stress is 0.05 MPa or less.
3. 3. A product using, as a raw material, the foamed sheet according to claim 1 or 2, which has a puncture strength of 5N or less.
4. A product using, as a raw material, the foamed sheet according to any one of claims 1 to 3, which has a puncture strength of 3N or more.
5. A product using, as a raw material, the foamed sheet according to any one of claims 1 to 4, which has a sheet thickness of 1 mm to 10 mm.
6. Bulk density is 0.025 g / cm 3 ~0.250g / cm 3 A product utilizing the foamed sheet according to any one of claims 1 to 5 as a raw material.
7. 7. A product using the foamed sheet according to claim 1 as a raw material, which is substantially free of organic compounds having a boiling point of -20°C or more and less than 150°C.
8. 8. A product using the foamed sheet according to claim 1 as a raw material, wherein the content of the polylactic acid is 98% by mass or more based on the total amount of organic matter in the foamed sheet.
9. A product using the foamed sheet according to any one of claims 1 to 8 as a raw material, wherein the content of the filler is 0.1% by mass to 5.0% by mass.