Method for heat treating high strength cold rolled steel strip
Patent Information
- Application Number
- JP2021575078
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-06-17
- Filing Date
- 2020-06-11
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-06-11
AI Technical Summary
Current continuous production lines for cold rolled steel are limited by maximum annealing temperatures, cooling rates, and overaging times, preventing the achievement of a desired combination of high tensile strength, total elongation, and yield strength in steel strips suitable for automotive applications.
A heat treatment method for cold rolled steel strips involving soaking, controlled cooling, and heating to specific temperatures and times, resulting in a microstructure comprising polygonal ferrite, acicular ferrite, high bainitic ferrite, and partitioned martensite, with controlled compositions of elements like carbon, silicon, manganese, and aluminum, to enhance strength and elongation properties.
The method enables the production of cold rolled steel strips with yield strength of at least 500 MPa, tensile strength of at least 850 MPa, and total elongation of at least 14%, suitable for automotive components requiring high strength, formability, and weldability, using existing production lines.
Abstract
Description
Technical Field
[0001] The present invention relates to a method for heat-treating a high-strength cold-rolled steel strip.
Background Art
[0002] In the art, various types of cold-rolled steels and manufacturing processes have been proposed to meet the requirements for automotive applications. For example, from the viewpoint of formability, ultra-low-carbon steel is used for automotive steel strips. This steel grade exhibits a tensile strength of 280 to 380 MPa.
[0003] HSLA (High-Strength Low-Alloy) steels contain micro-alloying elements. They are hardened by a combination of precipitation and grain refinement.
[0004] Advanced high-strength steels (AHSS), such as dual-phase (DP) steels and transformation-induced plasticity (TRIP) steels, are currently typical of the high-ductility and high-strength steels used in the automotive industry. In DP steels, martensite exists within a ferrite matrix, so a tensile strength exceeding 450 MPa and good cold formability can be obtained.
[0005] In order to simultaneously achieve a high yield strength / tensile strength ratio and an even higher tensile strength, i.e., exceeding 800 MPa, steels having a composite (CP) microstructure containing ferrite, bainite, martensite and / or retained austenite have been developed. However, due to the difference in deformation ability between the ferrite, bainite or martensite structure and the retained austenite structure, these steels are generally inferior in stretch flange formability. Therefore, their use is limited to automotive parts that do not require high formability.
[0006] TRIP-type tempered martensitic steel (Q&P steel by quenching and distribution), consisting of tempered martensite and retained austenite as the matrix phase, and TRIP-type bainitic ferrite steel (TBF steel by austemper), consisting of bainitic ferrite and retained austenite as the matrix phase, have advantages (for example, the ability to provide high strength due to the hard tempered martensite and / or bainitic ferrite structure, and the ability to exhibit excellent elongation because the matrix is carbide-free), and fine retained austenite grains can be easily formed at the boundaries of the lath-like bainitic ferrite in the bainitic ferrite structure. Therefore, carbide-free bainitic ferrite steel or tempered martensitic steel is expected to achieve good elongation flangeability due to its uniform fine lath structure. Due to the non-uniformity of hardness resulting from the presence of only a small amount of martensite in these microstructures, these steel types can achieve good deep drawability.
[0007] However, limitations in current continuous production lines have prevented the desired beneficial combination of strength and ductility properties from being achieved with currently available steel recipes. These limitations include, among other things, that the reheating furnaces in current equipment for continuous annealing (CA) and continuous galvanizing (CG) lines are often only suitable for subjecting steel strips to transformation section heat treatment or recrystallization heat treatment. For example, the maximum annealing temperature for some current annealing lines is limited to 890°C. Furthermore, the cooling rate of current CA / CG lines is limited to a certain range. The available overaging time for many CA / CG lines is also limited, for example, to less than approximately 160 seconds, which imposes a serious time limit for completing any desired transformation during overaging.
[0008] For example, WO2013 / 144373A1 discloses a cold-rolled TRIP steel having a polygonal ferrite matrix, having a specific composition including chromium and a specific microstructure, and having a tensile strength of at least 780 MPa, which is said to enable production on conventional industrial annealing lines with overaging / austempered sections. That is, the austemper time may be less than 200 seconds for relatively high overaging / austempering temperatures.
[0009] EP2831296B1 and EP2831299 disclose TBF steel with a tensile strength of at least 980 MPa that can be manufactured on conventional production lines. However, the preferred overaging / austemper time is 280-320 seconds, which is far too long to enable production on a great many conventional production lines. In other words, the bainite transformation rate is too slow for conventional production lines to complete the bainite transformation within the limited time available in the overaging section required to obtain the desired microstructure. [Overview of the project] [Problems that the invention aims to solve]
[0010] The object of the present invention is to provide cold-rolled steel strips having a desired combination of high tensile strength and high total elongation (TE) characteristics at a reasonable yield strength (YS), for example, TS ≥ 850 MPa, TE ≥ 14%, and / or YS ≥ 500 MPa, particularly for use in automotive applications.
[0011] A further object of the present invention is to provide a method for heat-treating cold-rolled steel strips to obtain the desired combination of properties described above, in particular a heat treatment that can be carried out using an existing production line or a suitable alternative.
[0012] Another object of the present invention is to provide high-silicon cold-rolled steel strips having a desired combination of properties that can be manufactured in a conventional industrial production line.
[0013] Another object of the present invention is to enable the completion of bainite transformation in a conventional manufacturing line to obtain a desired microstructure by modifying the steel composition and heat treatment thereof for high-strength cold-rolled steel strips. [Means for solving the problem]
[0014] Taking these into consideration, the present invention relates to a method for heat-treating cold-rolled steel strips, The above method comprises the following steps: a) A step of soaking a cold-rolled steel strip at a temperature of (Ac3-60) or higher for a soaking time t2 of 1 to 150 seconds, thereby obtaining a cold-rolled steel strip having a microstructure that is at least partially austenitized; b) A step of cooling the uniformly heated steel strip obtained from step a) to a temperature T4 of Ms~(Ms-200); c) A step of heating the cooled steel strip obtained from step b) to a temperature of Bs to Ms, d) A step of heating the heated steel strip for a time t5 of 30 to 120 seconds at a temperature of Bs to Ms. e) A process of cooling the heated steel strip to ambient temperature. It includes, and as a result, the steel strip, by volume %, Polygonal ferrite (PF) + Acicular ferrite (AF) + Higher bainitic ferrite (HBF): 20-55 Polygonal ferrite (PF): 0-50 Low bainitic ferrite (LBF) + partitioned martensite (PM): 25-70 Residual austenite (RA): 5-20 Martensite (M): 0-15 It has a microstructure that includes, The steel strip has the following composition by mass: C:0.15~0.35 Mn: 1.50~4.00 Si: 0.50 to 2.00 Al: 0.01 to 1.50 P: less than 0.050 S: less than 0.020 N: less than 0.0080 In some cases 0 < Cr ≤ 1.00 0 < Cu ≤ 0.20 0 < Ni ≤ 0.50 0 < Mo ≤ 0.50 0 < Nb ≤ 0.10 0 < V ≤ 0.10 0 < Ti ≤ 0.10 [[ID=]26]0 < B ≤ 0.0030 0 < Ca ≤ 0.0050 0 < REM ≤ 0.0100 One or more elements selected from Iron and inevitable impurities: the balance having (Si + Al) in total is ≥ 0.60, REM is one or more rare earth metals, providing the above method.
[0015] The method of the present invention makes it possible to produce cold-rolled steel strips having a specific composition and microstructure, and a desirable combination of properties for automotive parts that require high strength, formability, and weldability.
[0016] The present invention solves the problem of slow bainite transformation rate by introducing an appropriate amount of proeutectoid ferrite, controlling its morphology, obtaining fine grains of austenite by controlling the maximum annealing temperature and time, and using modified quenching and partitioning processes in the production line.
[0017] This method according to the present invention can be carried out within the limitations regarding the maximum temperature, cooling rate range, and overaging time window of the annealing section at the production speeds typical of these production lines, using existing continuous annealing lines and galvanizing lines.
[0018] Cold-rolled steel strips can be coated with Zn, for example, by hot-dip galvanizing or electro-galvanizing. The hot-dip galvanizing process can be easily integrated into the heat treatment according to the present invention.
[0019] The terms used to describe the critical transformation temperature of steel are as well known to those skilled in the art and are listed below. Ae3: The temperature at which the transformation from ferrite to austenite or from austenite to ferrite occurs under equilibrium conditions. Ac3: The temperature at which the transformation from ferrite to austenite ends during heating. Ac3 is usually higher than Ae3, but tends towards Ae3 because the heating rate tends to become zero. In this invention, Ac3 is measured at a heating rate of 3°C / second. Ar3: The temperature at which austenite begins to transform into ferrite during cooling. Bs: The temperature at which the transformation from austenite to bainite begins during cooling. Bn: The nose temperature of the bainite transformation in the time-temperature transformation (TTT) curve of steel. At this temperature, the transformation from austenite to bainite exhibits the fastest reaction rate. Ms: The temperature at which the transformation from austenite to martensite begins during cooling. Mf: The temperature at which the transformation from austenite to martensite is completed during cooling. The practical problem with Mf is that during cooling, the proportion of martensite approaches the maximum achievable amount only asymptotically. This means that it takes a very long time for the final martensite to form. Therefore, for practical reasons, in the context of this invention, Mf is considered to be the temperature at which 90% of the maximum achievable amount of martensite has been formed.
[0020] These critical phase transformation temperatures can be determined by dilatometer experiments. Alternatively, the Ac3, Bs, Bn, and Ms points of the steel according to the present invention can be calculated in advance based on its composition using available software, such as JmatPro or the following empirical formula.
number
[0021] In this specification, unless otherwise specified, all temperatures are expressed in Celsius, all compositions are expressed in weight percent (W%), and all microstructures are expressed in volume percent (V%). [Brief explanation of the drawing]
[0022] [Figure 1] Figure 1 shows EBSD maps illustrating the microstructural characteristics of low-temperature bainitic ferrite and / or partitioned martensite (Figure 1a) and high-temperature bainitic ferrite (Figure 1b), respectively. [Figure 2] Figure 2 shows the histograms of the misorientation angle for low-temperature and high-temperature bainitic ferrite. [Figure 3] Figure 3 shows a generally applicable time-to-temperature profile of an embodiment of the method according to the present invention. [Modes for carrying out the invention]
[0023] Following the description of the composition, the steps and microstructure of the method according to the present invention are shown.
[0024] composition Carbon: 0.15~0.35% A sufficient amount of carbon is necessary for strength and stabilization of retained austenite, the latter providing a TRIP effect. Considering this, the amount of carbon is 0.15% or more, preferably 0.17% or more, to ensure the required strength and elongation. Increasing the carbon content increases the strength of the steel, the amount of retained austenite, and the carbon content within the retained austenite. However, if the carbon content is higher than 0.25%, the weldability of the steel decreases significantly. For applications requiring welding, the carbon content is preferably 0.15-0.25%, more preferably 0.17-0.23%.
[0025] Silicon: 0.50~2.00% Silicon is an essential element in the steel composition according to the present invention for obtaining the described microstructure. Its main function is to prevent carbon from precipitation in the form of iron carbide (most commonly cementite) and to suppress the decomposition of retained austenite. Silicon contributes to strength properties and appropriate transformation behavior. Furthermore, silicon contributes to improved ductility, work hardening, and stretch flange formability by suppressing austenite grain growth during annealing. A minimum of 0.50% Si is required to sufficiently suppress carbide formation. However, high silicon content leads to the formation of silicon oxide on the strip surface, reducing surface quality, coating properties, and workability. In addition, the Ac3 temperature of steel having this composition increases with increasing silicon content. This may affect the feasibility of producing steel strips using existing production lines in terms of the maximum top temperature achievable in the annealing section. Considering these factors, the silicon content is 2.00% or less. Preferably, the Si content is 0.80 to 1.80%, from the viewpoint of suppressing carbide formation, promoting austenite stabilization, and improving wettability. More preferably, the Si content is 1.00 to 1.60%.
[0026] Aluminum: 0.01~1.50% The primary function of aluminum is to deoxidize molten steel before casting. More than 0.01% Al is required for deoxidation of molten steel. Furthermore, aluminum has similar functions to silicon, preventing carbide formation and stabilizing retained austenite. Al is considered less effective than Si. It has no significant impact on strengthening. Small amounts of Al can be used to partially replace Si, adjusting the transformation temperature and critical cooling rate to obtain acicular ferrite (AF) and increase the bainite transformation rate. Al is added for these purposes. Therefore, the Al content is preferably 0.03% or higher. High levels of Al may raise the ferrite-to-austenite transformation point to a level incompatible with current equipment, making it difficult to obtain a microstructure where the main phase is a low-temperature transformation product. As the Al content increases, the risk of cracking during casting increases. Considering this, the upper limit is 1.50%, preferably 1.00%, and more preferably 0.70%.
[0027] Regarding the relationship between the proportion of Si and Al, the composition satisfies the condition Si + Al ≥ 0.60, preferably Si + Al ≥ 1.00. Advantageously, the Al content is less than 0.5 times the Si content.
[0028] Manganese: 1.50-4.00% Manganese is necessary to obtain the microstructure of the steel strip according to the present invention from the viewpoint of hardening properties and stabilization of retained austenite. Mn also affects the formation of protereminate ferrite and the bainitic ferrite transformation rate at high temperatures. A certain amount of Si and / or Al is required to suppress the formation of carbides in the bainitic ferrite. The Ac3 temperature increases as the Si and Al content increases. Mn is also adjusted to balance the phase transformation point Ac3, which has increased as a result of the presence of Si and Al. If the Mn content is less than 1.50%, it is difficult to obtain the described microstructure. Therefore, Mn needs to be added at a concentration of 1.50% or more. However, if there is an excess amount of Mn, macrosegregation is likely to occur, leading to undesirable band formation in the steel. Furthermore, an excess amount of Mn slows down the bainite transformation rate, resulting in an excessive amount of fresh martensite, and consequently, reduced stretch flange formability. Therefore, the Mn content is 4.00% or less, preferably 3.50% or less, and more preferably 1.80 ≤ Mn ≤ 3.00%.
[0029] Phosphorus: <0.050% Phosphorus is an impurity in steel. It segregates at grain boundaries and reduces workability. Its content should be less than 0.050%, preferably less than 0.020%.
[0030] Sulfur: <0.020% Sulfur is also an impurity in steel. S forms sulfide inclusions, such as MnS, which cause cracking and reduce the elongation flange formability of the steel. The S content should preferably be as low as possible, for example, less than 0.020%, preferably less than 0.010%, and more preferably less than 0.005%.
[0031] Nitrogen: <0.0080% Nitrogen is another unavoidable impurity in steel. It precipitates as nitrides containing microalloying elements and is present in solid solutions, contributing to strengthening. Excess nitrides reduce elongation, elongation flangability, and bendability. Therefore, advantageously, the nitrogen content is less than 0.0080%, preferably less than 0.0050%, and more preferably less than 0.0040%.
[0032] The steel composition may contain one or more arbitrary elements as follows:
[0033] Copper: 0~0.20% Copper is not required in embodiments of steel having this composition, but may be present. In some embodiments, the presence of Cu may be unavoidable depending on the manufacturing process. Less than 0.05% of copper is considered a residual element. Copper as an alloying element may be added up to 0.20%. This facilitates the removal of scale formed during the hot rolling stage in manufacturing the starting steel strip, and further improves corrosion resistance if the cold-rolled steel strip is used as is without surface treatment, or improves wettability with molten zinc in the case of Zn-coated strips. Cu can contribute to precipitation hardening by promoting bainite structure, causing solid solution hardening, and precipitation as ε-copper from the ferrite matrix. Cu also reduces the amount of hydrogen entering the steel, and as a result improves delayed fracture properties. However, if added in excess, Cu causes high-temperature brittleness. Therefore, when Cu is added, the Cu content should be 0.20% or less.
[0034] Chromium: 0-1.00%; Nickel: 0-0.50%; Molybdenum: 0-0.50% Chromium, nickel, and molybdenum are not essential elements, but they may be present as residual elements in the steel composition. The acceptable level of residual Cr, Ni, or Mo is 0.05% each. As alloying elements, they have similar effects that are useful in improving the hardening properties of steel, promoting the formation of bainite ferrite, and stabilizing retained austenite. Therefore, Cr, Ni, and Mo are effective in controlling the microstructure. To obtain this effect fully, it is preferable that the content of Cr, Ni, or Mo in the steel be at least 0.05%. However, if each is added in excess, the effect saturates, the bainite transformation rate becomes excessively slow, and the desired microstructure cannot be obtained in production lines where overaging time is limited. Therefore, the amount of Cr is limited to a maximum of 1.00%. Ni is simply used to reduce the high-temperature brittleness characteristic when a relatively large amount of Cu is added. This effect of Ni becomes noticeable when the Ni content is >[Cu(%) / 3]. The amounts of Ni and Mo, if present, are limited to a maximum of 0.50% each.
[0035] Niobium: 0-0.100%; Vanadium: 0-0.100%; Titanium: 0-0.100% The acceptable levels of niobium, vanadium, and titanium as residual elements are 0.005% each. Adding one or more of these elements can refine the microstructure of hot-rolled intermediate and final products. These elements have a precipitation-enhancing effect and may alter the morphology of bainitic ferrite. They also contribute beneficially to optimizing applications that depend on properties such as the ductility and bendability of the stretched edge. To obtain these effects, the lower limit of any of these elements, if present, must be adjusted to 0.005% or higher. The effect saturates when the content of Nb, Ti, and V exceeds 0.10%. Therefore, when adding these elements, their content is adjusted to between 0.005% and 0.100%. Preferably, the upper limits are 0.050% or less for Nb and Ti, and 0.100% or less for V. This is because excessive addition leads to excessive carbide precipitation and reduced workability. Furthermore, from the viewpoint of processability and cost, it is preferable that the total of Ti + Nb + V does not exceed 0.100%.
[0036] Boron: 0-0.0030% Boron is another optional element, and when added, its concentration is adjusted to between 0.0003% and 0.0030%. The acceptable level of boron as a residual element is 0.0003%. The addition of boron improves quenchability and also helps increase tensile strength. To obtain these effects of boron, the lower limit needs to be 0.0003%, preferably 0.0005%. However, if an excess of boron is added, the effect saturates. Advantageously, boron is adjusted to 0.0025% or less, preferably 0.0020% or less.
[0037] In another preferred embodiment of the present invention, Ti and / or Nb and / or V and / or Ni and / or Cu and / or Cr and / or Mo and / or B are not added as alloying elements in order to reduce the cost of the final product while still obtaining a cold-rolled high-strength steel strip having the desired properties.
[0038] Calcium: 0-0.0050%; Rare Earth Elements (REM): 0-0.0100% Furthermore, the composition according to the present invention may optionally contain one or two elements selected from Ca and rare earth metals (REM) in amounts consistent with the treatment for controlling MnS inclusions. If present as residual elements, the acceptable level is 0.0005%. If added as alloying elements, Ca is adjusted to a value of 0.0050% or less, and REM is adjusted to a value of 0.0100% or less. Ca and / or REM combine with sulfur and oxygen, resulting in the formation of oxysulfides. These oxysulfides do not have an adverse effect on ductility (as in the case of elongated manganese sulfides formed when neither Ca nor REM is present). This effect saturates when the Ca content is higher than 0.0050% or the REM content is higher than 0.0100%. Preferably, the amount of Ca, if present, is adjusted to a value of less than 0.0030%, more preferably 0.0020% or less. Preferably, the amount of REM, if present, is adjusted to a value of 0.0080% or less, more preferably 0.0050% or less.
[0039] The remainder of the steel composition consists of iron and unavoidable impurities.
[0040] The chemical composition of the steel according to the present invention is compatible with the capacity of conventional continuous manufacturing lines.
[0041] Microorganism Cold-rolled steel strips heat-treated according to the present invention have a composite microstructure comprising 20-55% polygonal ferrite (PF), acicular ferrite (AF), and high bainitic ferrite (HBF), up to 50% PF, 25-70% low bainitic ferrite (LBF), and distributed martensite (PM), 5-20% retained austenite (RA), and 0-15% fresh martensite (M).
[0042] In this invention, the microstructure forms functional groups that can be observed using an optical microscope and a scanning electron microscope. Polygonal ferrite (PF) refers to ferrite formed during transformation interval annealing or during slow cooling at temperatures above Bs. Acicular ferrite (AF) refers to ferrite formed during cooling at temperatures between Bs and Ms. High-temperature bainitic ferrite (HBF) is ferrite formed during austemper at temperatures between Bs and Bn. Low-temperature bainitic ferrite (LBF) is ferrite formed during austemper at temperatures between Bn and Ms. Partitioned martensite (PM) refers to martensite formed during rapid cooling (quenching) and overaging (partitioned) heat treatment.
[0043] Bainitic ferrite and distributed martensite PM is obtained during quenching and distribution when the quenching stop temperature is between Ms and Mf and distribution is performed at temperatures between the quenching stop temperature and Bn. BF is obtained by the transformation of untransformed austenite during distribution (overaging). The amount of PM depends on the quenching temperature. The amount of BF is a function of the temperature and time of distribution. Note that in this application, the expression "distributed martensite" is used instead of tempered martensite. Generally in metallurgy, tempered martensite contains carbide precipitates resulting from tempering. In the modified quenching and distribution process according to the present invention, due to the presence of Si and Al and the very short duration of the distribution process, carbide formation is delayed during overaging. As a result, carbon is distributed from martensite to austenite, resulting in carbon-rich retained austenite with higher stability, and distributed martensite does not contain carbides. BF exists in the form of ultrafine-grained plates. PM has a similar substructure to BF, but possesses finer-sized ferrite laths, resulting in retained austenite with finer grain sizes. Precipitation of carbides between the ferrite laths is known to adversely affect ductility and is suppressed by alloying with Si and / or Al. Bainitic ferrite is carbide-free, in contrast to conventional bainite which contains carbides. Bainitic ferrite is also different from ferrite with a low dislocation density (proeutectoid).
[0044] The carbide-free BF and PM microstructures provide high strength, which is due to an intermediate hard bainitic ferrite structure containing supersaturated carbon and having a high dislocation density. Because the bainitic ferrite is carbide-free and fine retained austenite grains may be present at the boundaries of the lath-like bainitic ferrite, the bainitic ferrite structure also contributes to the desired high elongation.
[0045] In this invention, bainitic ferrite is divided into two types: bainitic ferrite formed at high temperatures from Bs to Bn (referred to as high bainitic ferrite (HBF)) and bainitic ferrite formed at low temperatures from Bn to Ms (referred to as low bainitic ferrite (LBF)). When the cross-section of a steel strip etched with 3% nital is observed with a scanning electron microscope accompanied by EBSD analysis, the average aspect ratio of HBF (defined as the length of the short axis divided by the length of the long axis) is higher than 0.35, and the average aspect ratio of LBF is lower than 0.35. The reason for this distinction is that the grain size and grain shape of bainitic ferrite (HBF) formed at higher temperatures above Bn are similar to those of AF, making it difficult to distinguish HBF from AF using SEM. Similar to AF, HBF has a larger grain size, lower dislocation density, and softer texture than LBF, and acts to increase the elongation of the steel. On the other hand, due to the finer plate size, the strength of LBF is higher than that of HBF, which contributes to the strength of the steel strip and also improves formability. PM has a similar microstructure to LBF, except that the size of the ferrite lath and the grain size of retained austenite decrease with decreasing formation temperature. However, because this change is gradual, it is not possible to clearly distinguish between LBF and PM by SEM observation. In this invention, LBF and PM are grouped together as a single microstructure because their contributions to the properties of the steel are also similar.
[0046] A key feature of the high-strength steel strip according to the present invention is that the bainitic ferrite may have a composite microstructure containing HBF and LBF+PM. Therefore, a high-strength cold-rolled steel strip with high elongation and good formability can be obtained.
[0047] To obtain a good balance of high strength and elongation, 25-70% LBF+PM is required. If the amount of LBF+PM is too low, the strength of the steel strip will be insufficient. However, if the amount of LBF+PM is too high, the influence of other ferrites (PF, AF, and HBF) and retained austenite on elongation may be impaired. Therefore, the total amount of LBF+PM is 25-70%, preferably 35-65%. PM formed during the quenching process can accelerate the BF transformation rate of untransformed austenite during overaging. To ensure that the bainite transformation is completed within the time available in a typical current production line, the amount of PM can be adjusted by controlling the quenching stop temperature to below the Ms point of the steel. The lower the quenching stop temperature, the more PM is formed. Steels with a high alloying element content require more PM.
[0048] The formation of HBF in this invention is due to heating of the strip by latent heat generated by the bainite transformation or by heating by applying a hot-dip galvanizing process. The formation of HBF in this invention allows for the acceleration of the bainite transformation, if any, as needed, so that the bainite transformation can be completed in a limited time in the overaging section of an existing production line. Depending on the amount of PF and AF resulting from the soaking and cooling stages, the amount of HBF is controlled so that the total amount of PF, AF, and HBF is 20-55%, preferably 25-50%. As mentioned above, HBF has similar functions to PF and AF. If a sufficient amount of PF and AF has been formed in the previous section, and to obtain a steel strip of higher strength, the amount of HBF should be minimized to 0%. If the amount of PF and AF is insufficient, the amount of HBF can be increased. However, the amount of HBF should be controlled so that the total amount of PF, AF, and HBF is 20-55%, preferably 25-50%.
[0049] Polygonal ferrites and acicular ferrites Proutetic ferrite is softer than bainitic ferrite and functionally increases the elongation of steel strips. By introducing a certain amount of proutetic ferrite and controlling the properties of the ferrite, the bainite transformation rate is increased, the stability of retained austenite is enhanced by increasing the carbon content in retained austenite, and the elongation is further increased. Using the present invention, two types of proutetic ferrite can be produced during annealing depending on the formation temperature. The ferrite phase formed during austenitization at the transformation interval temperature or the ferrite phase formed during cooling at high temperatures above the Bs temperature in the slow cooling section is polygonal or blocky and is called polygonal ferrite (PF). This type of ferrite has been shown to increase elongation but decrease yield strength and formability. The ferrite formed at low temperatures in the fast cooling section between Bs and Ms temperatures is almost needle-shaped, has a smaller grain size than PF and is called needle-shaped ferrite (AF). Morphologically it is similar to HBF, but the amount of dislocations is relatively small. The presence of AF can increase elongation without sacrificing strength and formability.
[0050] Since PF, AF, and HBF have similar functions for the tensile properties in the steel according to the present invention, there may be three types of these ferritic microstructures, or one or two of them may be present. To ensure high elongation, the volume fractions of PF, AF, and HBF are 20% or more, preferably 25% or more. In any case, the total amount of PF, AF, and HBF must be controlled to 55% or less, preferably 50% or less. If these ferritic microstructures are excessively abundant (more than 55%), the final microstructure will not contain enough low-bainitic ferrite, and therefore the strength will decrease.
[0051] When PF is present in steel, it is necessary to control the grain size, morphology, and distribution of PF. Steel strips can have higher elongation if they have smaller grain sizes of PF and a dispersed distribution of PF. According to the present invention, when observed with an SEM or optical microscope, the PF structure is equiaxed embedded between BF structures and uniformly dispersed as smaller grains, whereas the morphological structure of PF in conventional TRIP steel strips is elongated along the rolling direction. This morphological structure is thought to allow for uniform stress distribution during processing and maximize the TRIP effect of retained austenite. To obtain this morphological structure, the amount of PF formed during soaking needs to be 50% or less, preferably 10-40%. This embodiment is particularly suitable for steel compositions containing relatively large amounts of Mn, Al, and Si, where the recrystallization rate of ferrite is slow. PF is a partially recrystallized microstructure and has higher hardness than recrystallized ferrite. The presence of PF with a partially recrystallized microstructure is beneficial for local ductility. Advantageously, the particle size of PF in the present invention is 10 μm or less, preferably 8 μm or less, and more preferably 5 μm or less.
[0052] In one embodiment of the present invention, the amount of PF is preferably 0%. In this case, the total amount of AF and HBF is controlled so that AF + HBF is 20 to 55%, preferably 25 to 50%.
[0053] Retained austenite Retained austenite (also known as retained austenite) refers to the region exhibiting a face-centered cubic (FCC) phase in the final microstructure. Retained austenite enhances ductility, partly through the TRIP effect, which manifests as an increase in uniform elongation. To exhibit the TRIP effect, the volume fraction of retained austenite is 5% or more, preferably 7% or more. Below 5%, the desired level of ductility and uniform elongation cannot be achieved. The upper limit is determined mainly by the composition and processing parameters of the manufacturing line. If the amount of retained austenite is excessively high for a given composition, the carbon content of the retained austenite becomes excessively low. In that case, the retained austenite is not sufficiently stable, and the local ductility (stretch flange formability) may decrease to an unacceptable level. Therefore, the upper limit of the volume fraction of retained austenite is 20%, preferably 15%.
[0054] The carbon concentration in retained austenite affects the TRIP properties. Retained austenite is particularly effective in improving elongation properties when the carbon concentration is 0.90% or higher. If the carbon content is too low, the retained austenite will not be stable enough to produce a TRIP effect. Therefore, advantageously, the carbon content in retained austenite is 0.90% or higher, preferably 0.95% or higher. It is preferable that the carbon concentration in retained austenite be as high as possible, with an upper limit of about 1.6% generally imposed by the actual processing conditions. The carbon content and stability of retained austenite can be adjusted by controlling the amount of ferrite.
[0055] Martensite Martensite (M) is formed fresh in the final cooling section after austempering. Martensite suppresses the elongation at the yield point and increases the work hardening index (n-value), which is desirable for achieving stability, neck-free deformation, and strain uniformity in the final pressed part. Even 1% fresh martensite in the final steel strip can achieve tensile response, and therefore press behavior, comparable to that of conventional duplex steel. However, the presence of fresh martensite impairs formability due to crack formation along the interface between martensite and LBF / HBF. Therefore, the amount of fresh martensite needs to be controlled to 15% or less, preferably 10% or less.
[0056] carbide Carbides may exist as fine precipitates formed in austemper when the overaging temperature is excessively high or the overaging time is excessively long, or as pearlite formed during cooling when the cooling rate is excessively slow. According to the present invention, the microstructure of the steel of the present invention is pearlite-free and carbide-free. Pearlite-free means that the amount of layered microstructure containing cementite and ferrite is less than 5%. Carbide-free means that the amount of carbides is below the detection limit of standard X-ray measurement.
[0057] Characterization of microstructures As described above, the microstructural components classified as steel according to the present invention can be quantitatively determined by the techniques described below. The volume fraction of the components is measured by considering the volume fraction as equivalent to the area fraction and measuring the area fraction of a polished surface using a commercially available image processing program or other appropriate technique.
[0058] PF, fresh martensite, RA, and pearlite can be distinguished using an optical microscope (OM) and / or a scanning electron microscope (SEM). When samples etched with a 10% sodium metabisulfite aqueous solution (SMB) are characterized by OM, pearlite is observed as dark regions, PF as light gray regions, and fresh martensite as light brown regions. When samples etched with a 3% nital solution are characterized by SEM, PF is observed as smooth-surfaced grains without retained austenite, and pearlite is observed as a layered microstructure containing both cementite and ferrite. The remaining microstructures are observed as gray regions characterized by plate- or lath-like ferrite substructures, and RA is dispersed within the grains as white or light gray regions with no identifiable carbides. This microstructural group is called the bainitic ferrite-like microstructure. This may include mixtures of HBF, LBF, AF, and PM. These microstructures are morphologically similar and therefore cannot be clearly distinguished using OM and SEM.
[0059] In this invention, electron backscatter diffraction (EBSD) is used to further separate the bainitic ferrite-like microstructure into two distinct groups. The first group consists of PM and LBF, and the second group consists of AF and HBF. From the measured EBSD data, retained austenite can first be distinguished from other microstructures by creating Fe(γ) partitions from Fe(α). Fresh martensite (M) is then separated from the bainitic ferrite-like microstructure by dividing Fe(α) into partitions with high average image quality (IQ) and partitions with low average IQ. The low-IQ partitions are classified as martensite, and the high-IQ partitions are classified as bainitic ferrite-like microstructures. The method for distinguishing between the two group types is described below with reference to Figure 1. In bainitic ferrite (high-IQ partitions), regions with orientation differences of 15° or more between adjacent structures are identified. Some regions are considered to have the same crystal orientation and are defined in this invention as bainite plates. For the bainite plates detected in this manner, the diameter of a circle having the same area as the bainite plate is determined. The diameter of the equivalent circle of the bainite plate is determined using images from EBSD analysis at a magnification of 3000. The aspect ratio (defined as the length of the minor axis divided by the length of the major axis) is also determined by fitting the ellipse to the bainite plate. Similarly, the diameter of the equivalent circle of all bainite plates and the aspect ratio of the equivalent ellipse of all bainite plates are measured within the measurement area (approximately 100 × 100 μm), and the average value is defined as the average particle size and average aspect ratio of the bainite plates of the present invention.
[0060] The inventors systematically studied the effect of austemper temperature on the microstructure of bainite ferrite. The austemper temperature ranges from (Ms-200) to Bs. It was found that the average grain size and average aspect ratio of bainite plates increase with increasing austemper temperature. In particular, a sharp change is observed in the aspect ratio of bainite plates between samples austempered at temperatures below 440°C, which is below Bn of the steel used in the method according to the present invention, and samples austempered at temperatures above 460°C, which is above Bn. Therefore, a critical mean aspect ratio of 0.35 is defined to distinguish between two groups of bainite ferrite-like microstructures. The aspect ratio of the group consisting of LBF and PM is 0.35 or less, and the aspect ratio of the group consisting of HBF and AF is greater than 0.35.
[0061] In addition to differences in morphology and grain size of bainite plates, the complex crystallographic orientation difference relationships between the HBF, AF group and the LBF, PM group also differ. Figure 2 shows the orientation difference angle distribution of the steel according to the present invention. The 60° peak represents the orientation difference between adjacent particles and coincides with the orientation difference having a Kurdjumov-Sachs (KS / KS) relationship, which is 60°. <111> and 60° <110> These peaks arise from the relationship between the axes and angles and correspond to martensite. The peak at 53°~54° is due to the orientation difference between particles obtained by phase transformation, following the Nishiyama-Wassermann and Kurdjumov-Sachs (NW / KS) relationships. According to prior art (see A.-F. Gourgues, HM Flower, and TC Lindley, Materials Science and Technology, January 2000, Vol. 16, p. 26-40), acicular ferrite and upper bainite grow with the austenite matrix in the Nishiyama-Wassermann relationship, while lower bainite and martensite are composed of very complex packets with the matrix in the Kurdjumov-Sachs relationship. Similar to these results, it is estimated that the peak at 53~54° corresponds to the formation of HBF and AF, and the peak at 60° corresponds to the formation of LBF and PM. As the austemper temperature increases, the peaks at 53-54° become more distinct and their heights increase, while the peak at 60° decreases in height. In this invention, the relative amounts of the HBF, AF group and the LBF, PM group can be determined by the ratio of the heights of the two peaks.
[0062] Some retained austenite is dispersed as a very small-grained film between bainite plates and cannot be detected by EBSD; therefore, the percentage of retained austenite measured by EBSD is always lower than the actual value. Thus, a conventional method for measuring retained austenite content, based on XRD intensity analysis, can be used. The volume fraction of retained austenite is determined at a thickness of 1 / 4 of the steel strip. The amount of cementite is also measured from this XRD analysis. Samples prepared from steel strips are mechanically and chemically polished and then analyzed by measuring the integrated intensities of the (200), (220), and (311) planes of fcc iron, and the integrated intensities of the (200), (211), and (220) planes of bcc iron, respectively, using a Co-Ka X-ray diffractometer. The amount of retained austenite (RA) and the lattice constant of retained austenite were determined using Rietveld analysis. The carbon content in retained austenite is given by the following formula:
number
[0063] Mechanical properties A cold-rolled steel strip having the above microstructure and composition, and heat-treated according to the present invention, has the following properties: Yield strength (YS) of at least 500 MPa; and / or Tensile strength (TS) of at least 850 MPa; and / or At least 14% total elongation (TE); and / or It has.
[0064] Preferably, cold-rolled and heat-treated strips possess all of these properties.
[0065] Method steps According to the method of the present invention, a cold-rolled steel strip having the above composition is heat-treated to obtain the microstructure and properties. The cold-rolled steel strip obtained by cold rolling is subjected to heat treatment in the same manner as in a continuous annealing line. A typical design of the method is schematically shown in Figure 3. The cold-rolled steel strip is heated to a temperature of (Ac3-60) or higher, for example, using a heating rate of at least 0.5°C / second, preferably to a temperature of (Ac3-60) to (Ac3+20), usually to a predetermined austenitizing temperature T2, and held at this temperature for a time t2 (step a). Then, it is cooled to a temperature of Ms or lower, typically Ms to (Ms-200) T4, usually using a two-stage cooling with a controlled cooling rate (step b). Next, the steel strip is heated, sometimes below Ms, typically from a temperature of (T4~Ms) to above Ms (step c), and then treated for austemper at a temperature of Ms~Bs, typically T4~Bn, at a temperature of T5 for a time of t5 (step d). Then, optionally, the steel strip is heated to a temperature of Bn~Bs at a temperature of T6 for a time of t6. This may be a temperature at which hot-dip galvanizing is possible. Finally, the steel strip is cooled to room temperature (step e). The process parameters and effects of each step are described below.
[0066] In the first step, to achieve a microstructure that is at least partially austenitized, the cold-rolled steel is soaked at a temperature of (Ac3-60) or higher, for example, (Ac3-60) to (Ac3+20), for a soaking time t2 of 1 to 150 seconds. Annealing at a temperature of (Ac3-60) or higher is necessary because the steel strip heat-treated according to the present invention requires a certain amount of low-temperature transformation phases (e.g., bainitic ferrite and retained austenite) that transform from high-temperature austenite, and a predetermined amount of ferrite. If T2 is higher than (Ac3+20), austenite grains grow. This affects the grain size and distribution of retained austenite and also slows the rate of bainite transformation after the overaging process. An excess amount of fresh martensite formed during final cooling may be formed as a result of this incomplete bainite transformation, which increases strength but reduces ductility and formability. Furthermore, a uniform austenite structure with large grains is obtained, suppressing the formation of PF and AF in the next cooling section, and as a result, a sufficient amount of ferrite cannot be obtained within the current cooling schedule of the available production line. A uniform austenite structure with large grain size also causes insufficient elongation of the steel strip. It has been observed that the uniformity of the austenite has a significant impact on the formation of PF and AF in the cooling section. If T2 is lower than (Ac3-60), an excess of more than 45% may be formed, and therefore the strength of the steel strip may be insufficient. On the other hand, the austenite that is formed may not be sufficient for the formation of LBF and retained austenite. Therefore, the annealing temperature needs to be (Ac3-60) or higher, but advantageously (Ac3+20) or lower, preferably (Ac3-50) to (Ac3+10). If t2 is longer than 150 seconds, the grain size of austenite and ferrite increases, and the elongation decreases. If the annealing time t2 is shorter than 1 second, the reverse transformation to austenite may not proceed sufficiently, and / or the carbides in the steel strip may not be sufficiently dissolved. Therefore, the annealing time t2 is 1 second to 150 seconds, for example, 10 seconds to 120 seconds, preferably 1 second to 100 seconds.
[0067] In the next cooling step, the strip, which is at least partially austenitized, is cooled to a temperature T4 below Ms, typically Ms~(Ms-200). The purpose of this cooling is to adjust the amount of ferrite and partitioned martensite and prevent pearlite formation.
[0068] In one embodiment of the present invention, the steel strip processed in this manner is directly cooled to a temperature T4 at a cooling rate of at least 15°C / second, thereby preventing the formation of pearlite. If the cooling rate is excessively slow, an excess amount of ferrite may be formed, or even pearlite may be formed. Preferably, V4 is 20°C / second or higher. The upper limit of the cooling rate is not particularly limited, as long as no temperature change occurs in the steel strip when cooling stops. To reduce temperature non-uniformity of the steel strip, the cooling rate is preferably 100°C / second or lower in standard equipment. If the average cooling rate exceeds 80°C / second in most available facilities, very large variations in the microstructure can occur in both the longitudinal and strip width directions. Therefore, a suitable cooling rate V4 is 15 to 80°C / second, preferably 20 to 70°C / second.
[0069] In other embodiments of the present invention, to adjust the amount of ferrite and equalize the strip temperature, this cooling can be performed by two-stage cooling. This is compatible with most continuous annealing lines or hot-dip galvanizing lines currently in use, which include two connected cooling sections. First, the steel strip is cooled to a temperature T3 of 800-500°C, preferably 750-550°C, at a cooling rate V3, typically at least 1°C / sec, e.g., 2-15°C / sec, preferably 3-10°C / sec (referred to as the slow cooling section). Then, the steel strip is further cooled to a temperature T4, typically at least 15°C / sec, e.g., 15-100°C / sec, preferably 20-70°C / sec (referred to as the fast cooling section). Since the length of each section in the continuous annealing line is fixed, the cooling rates V3 and V4 can be controlled relative to a given line speed by adjusting the T3 temperature. As T3 increases, V3 decreases and V4 increases. During this cooling process, some PF may form in the slow-cooling section, and some AF may form in the fast-cooling section. For a fixed line speed, the amount of PF formed in the slow-cooling section depends primarily on T3, and the amount of AF primarily on V4. Therefore, T3 is selected within an appropriate range to control the amount of ferrite and prevent pearlite formation. If T3 is excessively low (e.g., below 500°C), excess PF may form in the slow-cooling section, and excess AF may also form in the fast-cooling section. Furthermore, if the resulting V4 is less than 15°C / sec, pearlite may form. If T3 is excessively high (e.g., above 800°C), insufficient PF may form, and if the resulting V4 is excessively high, less AF will be formed. Therefore, T3 should be between 800 and 500°C, preferably between 750 and 550°C / sec.
[0070] As described above, in a conventional annealing or galvanizing line design, PF is obtained in the slow cooling section of soaking process a) and process b), and AF is obtained in the fast cooling section of process b). To adjust the amount of ferrite, soaking temperatures T2 and intermediate temperatures T3 between the slow and fast cooling sections can be used. If the higher T2 is used, less PF is generated during soaking, and then by selecting the lower T3, more PF can be obtained in the slow cooling section and more AF in the fast cooling section. If the lower T2 is used, a sufficient amount of PF is generated during soaking, and then by selecting the higher T3, the amount of PF formed in the slow cooling section and the amount of AF formed in the fast cooling section can be limited.
[0071] After cooling to a temperature T4 of Ms or less, preferably Ms~(Ms-200), some amount of martensite is obtained. The lower the T4, the more martensite is formed. T4 is adjusted according to the steel composition to effectively accelerate the bainite transformation rate in the subsequent distribution process. For steels with high alloying element content, a lower T4 is applied. If T4 is too high, the amount of PM formed will be insufficient. The bainite transformation of untransformed austenite cannot be completed in the overaging (distribution) stage, and excess fresh martensite may be formed in the subsequent cooling process to ambient temperature. If T4 is too low, excess PM is formed, and the amount of retained austenite decreases. Therefore, T4 is preferably Ms~(Ms-200), more preferably (Ms-50)~(Ms-150). Since the amount of PM depends only on the T4 temperature, the steel strip is heated as quickly as possible to a distribution temperature of Ms to Bs in order to make the remaining time available in the overaging section available for bainite transformation. In practice, depending on the heating capacity of the production line and to facilitate temperature homogenization of the steel strip, the total time t4 of step c), including any holding time, is preferably 10 seconds or less, more preferably 5 seconds or less. In some cases, heating step c) may include short heating at temperatures below Ms, for example, Ms to (Ms-200), for example, (Ms-50) to (Ms-150).
[0072] In the subsequent heating step d), the cooled strip is heated to a temperature T5 of Ms to Bs, preferably Bn, for a time t5 of 30 to 120 seconds. Heating to this temperature range T5 causes the untransformed austenite to transform into low bainite ferrite (LBF), with carbon distribution occurring in the martensite formed beforehand. If T5 is too low, the bainite transformation is too slow and insufficient during overaging, and an excess of fresh martensite may form during cooling after overaging, which increases strength but reduces the required elongation. On the other hand, the carbon distribution may be insufficient to stabilize the retained austenite. If T5 is too high, an excess of HBF is obtained in the overaged section, and the required strength cannot be obtained. The preferred range for T5 is (Bn-50) to Bn in order to achieve a fast bainite transformation rate. If the heating time t5 is less than 30 seconds, the bainite transformation is incomplete, and the carbon distribution in the martensite and bainite is also insufficient. If t5 exceeds 120 seconds, there is a risk that carbide formation will begin, leading to a decrease in the carbon content in the retained austenite. The maximum time for t5 is limited, among other things, by the total time available at a given rate on the production line. Preferably, t5 is between 40 and 100 seconds.
[0073] The temperature of the steel strip can rise due to the latent heat generated by the bainite transformation during overaging, so when the steel strip reaches a temperature higher than that of Bn, a small amount of high-temperature bainite ferrite is formed.
[0074] The heated strip is then cooled to ambient temperature according to the performance of the production line, during which some fresh martensite may form. The steel strip is then cooled to below 300°C at a cooling rate V7 of at least 1°C / sec, preferably at least 5°C / sec, and then further cooled to ambient temperature. Cooling to ambient temperature can be forced cooling or uncontrolled natural cooling. In practical embodiments, the heated steel strip is cooled to a temperature T7 of (Ms-50) to Mf at a cooling rate V7 of 5.0 to 10.0°C / sec. Further cooling from T7 to ambient temperature is preferably carried out at a cooling rate V8 of 5.0 to 20.0°C / sec, more preferably 6.0 to 15.0°C / sec.
[0075] In one embodiment, to ensure that a partially austenitized cold-rolled strip having a fine grain size is obtained, the soaking step is carried out at a transformation interval annealing temperature of (Ac3-50) to (Ac3+10), preferably with a soaking time t2 of 1 to 100 seconds. The fraction of PF formed at the soaking temperature is advantageously 40% or less.
[0076] Advantageously, the heating process prior to the soaking process is carried out in two sub-steps. The two sub-steps include heating the cold-rolled strip to a temperature T1 of 680-740°C, preferably 700-720°C, at a heating rate V1 of 10.0-30.0°C / second, preferably 15.0-25.0°C, and further heating from temperature T1 to the soaking temperature range at a heating rate V2 of 0.5-4.0°C / second, preferably 1.0-3.0°C / second. During the slow heating from T1 to the soaking temperature T2, recovery and recrystallization occur in the ferrite, and solid solution of carbides and ferrite occurs during the austenite transformation. T1 and V2 affect the progress of these processes and affect the uniformity of the austenite grain size and the distribution of alloying elements in the austenite phase. Advantageously, the soaking time t2 is controlled according to the heating rate V2 to ensure the avoidance of solid solution of all carbides and uneven austenite grain size.
[0077] In one embodiment, the method according to the present invention includes a further heating step between heating step d) and cooling step e), wherein the steel strip obtained from step d) is subjected to additional heating at Bs to Bn, preferably (Bs-50) to Bn, typically at a fixed temperature T6. The additional heating time t6 is advantageously 5 to 30 seconds, preferably 10 to 20 seconds. This additional heating increases the formation of retained austenite to high-temperature bainite ferrite, completing the bainite transformation. As a result, the amount of martensite formed in the subsequent cooling section is reduced, improving strength and ductility. Carbon is also further distributed into the retained austenite, making it more stable. If this additional heating is applied to a given overaging section, and therefore to a given total time therein, the time t5 is further shortened to meet the available time. For example, the sum of t4 + t5 + t6 is 30 to 120 seconds.
[0078] In a preferred embodiment, this additional heating includes an integrated hot-dip galvanizing process, and the steel strip obtained from step c) is coated with a Zn coating or a Zn alloy coating.
[0079] Steel strips heat-treated according to the present invention may be provided with a coating, preferably a zinc coating or a zinc alloy coating. Preferably, the zinc coating is a galvanized or galvannealed coating. The Zn coating may include a Zn alloy containing Al as an alloying element. A preferred zinc bath composition contains 0.10 to 0.35% Al, with the remainder being zinc and unavoidable impurities. Another preferred Zn bath containing Mg and Al as the main alloying elements has the following composition: 0.5 to 3.8% Al, 0.5 to 3.0% Mg, and up to 0.2% of one or more additional elements as optional components, with the remainder being zinc and unavoidable impurities. Examples of additional elements include Pb, Sb, Ti, Ca, Mn, Sn, La, Ce, Cr, Ni, Zr, and Bi.
[0080] A coating, such as a protective coating of Zn or a Zn alloy, may be applied in a separate step. Preferably, the hot-dip galvanizing step is integrated into the method according to the present invention, as described above.
[0081] Depending on the circumstances, temper rolling may be performed on the annealed and zinc-coated strips according to the present invention to fine-tune the tensile properties and modify the surface appearance and roughness according to specific requirements arising from the intended use.
[0082] Cold-rolled steel strips themselves are typically manufactured according to the following general method: The steel composition described above is prepared and cast into a slab. The cast slab is reheated to a temperature of 1100-1300°C and then subjected to hot rolling. Typically, the slab is hot-rolled in 5-7 stands until it reaches a final dimension suitable for further cold rolling. Finish rolling is typically performed at a fully austenitic state above 800°C, preferably above 850°C. The strips obtained from the hot-rolling process in this manner can be coiled, for example, at a winding temperature of typically 700°C or lower. The hot-rolled strips are pickled and cold-rolled to obtain cold-rolled steel strips with the appropriate gauge. Preferably, the reduction in cold rolling is typically 30-80%. To reduce the rolling load during cold rolling, coiled strips or semi-cold-rolled strips may be subjected to hot batch annealing. The batch annealing temperature needs to be between 500 and 700°C.
[0083] Thin slab casting, strip casting, etc., may also be applied. In this case, it is permissible for the manufacturing method to skip at least a part of the hot rolling process.
[0084] The present invention also relates to a heat-treated cold-rolled steel strip having the composition and microstructure described above.
[0085] The present invention also exists in articles manufactured from heat-treated cold-rolled strips according to the present invention, such as structural components, engineering components, or automotive components. [Examples]
[0086] Steel having the composition shown in Table 1 was cast into a 25 kg ingot with dimensions of 200 mm × 110 mm × 110 mm using vacuum induction. Cold-rolled strips with a thickness of 1 mm were produced using the following process schedule. The ingot was reheated at 1225°C for 2 hours. The ingot was roughly rolled from 140 mm to 35 mm. The rough-rolled ingot was reheated at 1200°C for 30 minutes. The material was hot-rolled from 35mm to 4mm in 6 passes. • Runout table cooling: The table was cooled from the finish rolling temperature (FRT) (approximately 850-900°C) to 600°C at a rate of 40°C / second. • Furnace cooling: The strip was transferred to a furnace preheated to 600°C, and then cooled to room temperature to simulate the cooling process. • Pickling: Next, the hot-rolled strips were pickled with HCl at 85°C to remove the oxide layer. • Cold rolling: Hot-rolled strips were cold-rolled into 1mm strips. • Heat treatment according to the present invention: The annealing process was simulated using a continuous annealing simulator (CASIM) with a cold-rolled sheet of appropriate size. Samples for microstructural observation, tensile testing, and hole expansion testing were machined from strips processed in this manner.
[0087] Expansion coefficient measurements were performed on cold-rolled samples with dimensions of 10 mm × 5 mm × 1 mm (length along the rolling direction). Expansion tests were conducted using a Bahr dilatometer, model DIL805. All measurements were performed according to SEP1680. The critical phase transformation points Ac3, Ms, and Mf were determined from the quenched dilatometry curve. Bs and Bn were predicted using the available software JmatPro10. Phase fractions during annealing for different process parameters were determined from expansion curves simulating the annealing cycle.
[0088] Microstructure was determined using optical microscopy (OM) and scanning electron microscopy (SEM) with commercially available image processing programs. Microstructure was observed at a thickness of 1 / 4 in cross-sections of steel strips in the rolling direction and the direction normal to the rolling surface. The scanning electron microscope (SEM) used for EBSD measurements was a Zeiss Ultra55 machine equipped with a field emission gun (FEG-SEM) and an EDAX PEGASUS XM 4 HIKARI EBSD system. EBSD scans were captured using TexSEM Laboratories (TSL) software OIM (Orientation Imaging Microscopy) Data Collection. EBSD scans were evaluated with TSL OIM Analysis software. In all cases, the EBSD scan area was 100 × 100 μm, the step size was 0.1 μm, and the scan rate was approximately 80 frames / second.
[0089] Retained austenite was determined by XRD according to DIN EN13925 using D8 Discover GADDS (Bruker AXS) with Co-Kα radiation. The phase ratio was quantitatively determined by Rietveld analysis.
[0090] Tensile Test - JIS 5 test specimens (gauge length = 50 mm, width = 25 mm) were machined from annealed strips so that the tensile direction was parallel to the rolling direction. Room temperature tensile tests were performed using a Schenk TREBEL testing machine compliant with NEN-EN10002-1:2001 standard to determine the tensile properties (yield strength YS (MPa), maximum tensile strength UTS (MPa), total elongation TE (%)). Three tensile tests were performed for each condition, and the average value of the mechanical properties is reported.
[0091] Using the representation in Figure 3, the process parameters are shown in Table 2. In CASIM, the steel strip is cooled to T4 at V4 and then heated to T5 within 5 seconds. The resulting microstructure and tensile properties are shown in Table 3. All steel compositions of the present invention achieve the requirements for microstructure and tensile properties under the specified processing parameters. Steel A79 containing 0.5% Cr could not achieve the required elongation because bainite transformation was insufficient when T4 exceeded Ms (Examples 13 and 14). However, when T4 was less than or equal to Ms, some PM was formed, as a result allowing bainite transformation to be completed and the steel strip to obtain the required properties (Examples 11 and 12).
[0092] [Table 1]
[0093] [Table 2]
[0094] [Table 3]
Claims
1. 1. A method for heat treating cold rolled steel strip, comprising the steps of: The method comprises the steps of: a) soaking the cold rolled steel strip at a temperature between (Ac3-50) and (Ac3+10) for a soaking time t2 between 1 and 150 seconds, thereby obtaining a cold rolled steel strip having an at least partially austenitized microstructure; b) cooling the soaked steel strip obtained from step a) to a temperature T4 of Ms to (Ms-200), either by directly cooling the soaked steel strip obtained from step a) to a temperature T4 at a cooling rate V4 of at least 15°C / s or by cooling the soaked steel strip obtained from step a) to a temperature T3 of 800-500°C at a cooling rate V3 of at least 1°C / s and then cooling from temperature T3 to temperature T4 at a cooling rate V4 of at least 15°C / s; c) heating the cooled steel strip obtained from step b) to a temperature of Bs to Ms; d) heating the hot steel strip at a temperature between Bs and Ms for a time t5 between 30 and 120 seconds; e) cooling the heated steel strip to ambient temperature. so that the steel strip comprises, in volume percent: Polygonal ferrite (PF) + acicular ferrite (AF) + high bainitic ferrite (HBF): 20-55 Polygonal ferrite (PF): 0 to 50 Low bainitic ferrite (LBF) + distributed martensite (PM): 25-70 Retained austenite (RA): 5-20 Martensite (M): 0 to 15 and having a pearlite-free microstructure, where "pearlite-free" means that the amount of lamellar microstructure containing cementite and ferrite is less than 5%; The steel strip has the following composition, in mass %, C: 0.15-0.35 Mn: 1.50-4.00 Si:0.50~2.00 Al: 0.01~1.50 P: less than 0.050 S: less than 0.020 N: less than 0.0080 In some cases, 0<Cr≦1.00 0<Cu≦0.20 0<Ni≦0.50 0<Mo≦0.50 0<Nb≦0.10 0<V≦0.10 0<Ti≦0.10 0<B≦0.0030 0<Ca≦0.0050 0<REM≦0.0100 One or more elements selected from Iron and unavoidable impurities: balance having The sum of (Si+Al) is ≧0.60; The process wherein REM is one or more rare earth metals.
2. 2. The method according to claim 1, wherein step c) comprises heating the cooled steel strip obtained from step b) at a temperature T4 of between Ms and (Ms-200).
3. The method according to claim 1, wherein the total time t4 of step c) is 1 to 10 seconds.
4. A method according to any one of claims 1 to 3, wherein the heat-soaking time t2 is 1 to 100 seconds.
5. The method according to claim 1, wherein the cooling rate V3 is 2.0 to 15.0°C / sec and the temperature T3 is 750 to 550°C.
6. The method according to claim 1, wherein the cooling rate V4 is 20.0 to 70.0°C / sec and the temperature T3 is 750 to 550°C.
7. 7. The method according to any one of claims 1 to 6, further comprising, prior to step a), heating the cold rolled steel strip to a temperature of (Ac3-50) to (Ac3+10) at a heating rate of at least 0.5°C / s.
8. The method according to claim 1, further comprising, prior to step a), heating the cold rolled steel strip to a temperature T1 of 680-740°C at a heating rate V1 of 10.0-30.0°C / s, and further heating from temperature T1 to a temperature of (Ac3-50)-(Ac3+10) at a heating rate V2 of 0.5-4.0°C / s.
9. The method according to claim 8, wherein the heating rate V1 is 15.0 to 25.0° C. / sec, the temperature T1 is 700 to 720° C., and the heating rate V2 is 1.0 to 3.0° C. / sec.
10. The method according to any one of claims 1 to 9, wherein the heating in step d) is carried out at a temperature of Bn to (Ms+50).
11. The method of claim 10, wherein the heating in step d) is carried out for a time t5 of 40 to 100 seconds.
12. The heating in step d) is carried out at a temperature of Bn to Ms; 12. The method according to any one of the preceding claims, wherein the method comprises an additional heating step between step d) and step e) of heating the steel strip obtained from step d) at a temperature between Bs and Bn.
13. The method of claim 12, wherein the heating in the additional heating step is carried out for a time t6 of 5 to 30 seconds.
14. 14. The method of claim 12 or 13, wherein the additional heating step comprises a hot dip galvanizing process.
15. The method according to any one of the preceding claims, further comprising, after the heat treatment, a coating step of coating the heat treated steel strip with a protective coating.
16. The microstructure comprises, in volume percent: Polygonal ferrite (PF) + acicular ferrite (AF) + high bainitic ferrite (HBF): 25-50 Polygonal ferrite (PF): 10-40 Low bainitic ferrite (LBF) + distributed martensite (PM): 35-65 Retained austenite (RA): 7-15 Martensite (M): 0 to 10 and / or The method according to any one of claims 1 to 15, wherein the C content in the retained austenite (RA) is 0.90 wt% or more.
17. The resulting steel strip has the following properties: Yield strength (YS) of ≧500 MPa; Tensile strength (TS) of ≧850 MPa; Total Elongation (TE) ≧14% The method according to any one of claims 1 to 16, having at least one of the following characteristics: