Production method of 780MPa-grade galvanized dual-phase steel for high-yield-strength automobile structure
Through the process of smelting-continuous casting-hot rolling-pickling-cold rolling-continuous hot-dip galvanizing and light finishing, the problems of uniformity and high cost of 780MPa-grade galvanized duplex steel are solved, and high yield strength and tensile resistance are achieved The strength matching meets the high-strength structure needs of automobiles and reduces production costs.
Patent Information
- Application Number
- CN202410974612.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-15
AI Technical Summary
The existing 780MPa grade galvanized duplex steel has high performance uniformity and cost, and there are differences in smelting processes, making it difficult to meet the needs of automobiles' high yield strength structures.
Using smelting-continuous casting-hot rolling-pickling-cold rolling-continuous hot-dip galvanizing and light finishing process flow, chemical composition and process parameters are controlled, including top-bottom reblowing smelting of converter, LF refining, 3+3 mode rough rolling, 7 Frame finish rolling, laminar flow cooling and continuous hot-dip galvanizing and light finishing processes ensure high strength and corrosion resistance of the steel strip.
It achieves matching of high yield strength, tensile strength and elongation, meets the needs of lightweight materials for automobiles, reduces production costs, and improves the overall performance of steel belts.
Smart Images

Figure CN118957406A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgical plates, and in particular relates to a production method of 780MPa grade galvanized dual-phase steel for high yield strength automobile structure. Background Art
[0002] In recent years, the global greenhouse effect, energy shortage and environmental pollution have become increasingly prominent, and energy conservation, emission reduction and green development have become the common development trend of all walks of life. In the automotive field, more and more product applications focus on the development and application of high-quality, low-carbon emission ultra-high strength steel, which can reduce weight and improve safety performance. In addition, as people's requirements for automobile quality and aesthetics continue to increase, the shapes of automobile parts are becoming more and more complex, and the demand for galvanized products is increasing day by day. Therefore, it is urgent to develop galvanized high-strength steel with better comprehensive performance, which is also the innovation trend of high-strength automotive steel in the future.
[0003] 780MPa grade galvanized duplex steel is an advanced high-strength steel widely used in the automotive field. Its microstructure is composed of two phases, ferrite and martensite. Ferrite provides the ductility of steel, while martensite provides strength. It has the characteristics of high strength, high work hardening index, high initial work hardening rate, good matching of strength and ductility, and high corrosion resistance, making it one of the preferred materials for lightweight steel for automobiles. It is mainly used in high-strength structural parts and connectors of automobiles, such as longitudinal beams, connecting plates, bumpers, bumpers, etc. The development of 780MPa grade galvanized duplex steel products for high yield strength automotive structures can meet users' lightweight material selection needs and realize differentiated product applications.
[0004] At present, the composition design of 780MPa galvanized duplex steel produced by Tangshan Vocational and Technical College of Science and Technology (a method for improving the performance uniformity of 780MPa galvanized duplex steel, application number 202110290916.5) is C: 0.07-0.10%, Si≤0.12%, Mn: 1.70-2.10%, Nb: 0.013-0.030%, Mo: 0.15-0.25%, B: 0.0010-0.0025%, which is different from the composition design of the present invention. The high content of Nb, Mo and B increases the product cost, and the soaking temperature of 750-780℃ is different from the process of the present invention; the composition of 800MPa cold-rolled hot-dip galvanized duplex steel produced by Wuhan Iron and Steel Co., Ltd. (a 800MPa cold-rolled hot-dip galvanized duplex steel and its production method, application number 201811126345.6) In the design: C: 0.05-0.10%, Nb: 0.010-0.050%, Mo: 0.05-0.30%, which is different from the composition design of the present invention; the composition design of the 780MPa grade cold-rolled hot-dip galvanized duplex steel produced by Shougang Corporation (a 780MPa grade cold-rolled hot-dip galvanized duplex steel and its preparation method, application number 201110439563.7) has a high content of Nb: 0.03-0.04%, Mo: 0.2-0.25%, which affects the product cost, and the coiling temperature is 640-700°C, which is different from the composition and process of the present invention. Summary of the invention
[0005] The purpose of the present invention is to provide a production method of 780MPa grade galvanized dual-phase steel for high yield strength automobile structure. The 780MPa grade galvanized dual-phase steel with high yield strength of the present invention has the characteristics of high strength, high work hardening index, high initial work hardening rate, good matching of strength and ductility, high corrosion resistance, etc., which meets the requirements of automobile lightweight material selection and user differentiated application, and the mechanical properties meet the following requirements: yield strength R p0.2 : 500-650MPa, tensile strength R m ≥780MPa, elongation A 50 ≥14%.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0007] The present invention provides a method for producing 780MPa grade galvanized dual-phase steel for high yield strength automobile structure, comprising:
[0008] (1) Smelting-continuous casting production process: molten iron pretreatment-converter-LF refining-slab continuous casting; oxygen blowing decarburization and heating are carried out in the converter top and bottom combined blowing smelting, and aluminum iron, manganese iron, silicon iron and chromium iron are added in the converter steelmaking process for deoxidation and alloying, and the P and S components are controlled to prevent the steel liquid from overoxidation. The steelmaking temperature is ≥1600℃; LF refining outside the furnace adopts the LF full-process argon blowing process, and the target composition is adjusted according to the molten steel composition. The molten steel composition for the casting machine is C: 0.13-0.17%, Si: 0.10-0.30%, Mn: 1.9-2.3%, P≤0.020%, S≤0.015%, Al T: 0.010-0.060%, Cr: 0.2-0.5%, Ti≤0.03%, Ca: 0.0008-0.0025%, the rest is Fe and impurities; slab continuous casting superheat 15-40℃, casting speed controlled at 0.8-1.5m / min;
[0009] (2) Hot rolling production process: heating of ingot - rough rolling - finishing rolling - coiling; ingot furnace time is 160-320min, furnace temperature is 1200-1280℃, rough rolling adopts 3+3 mode 2-stand rolling mill, finishing rolling adopts 7-stand rolling mill, finishing rolling start temperature is 960-1050℃, finishing rolling final temperature is 850-920℃, hot rolled steel strip thickness is 2.3-4.0mm; cooling adopts laminar cooling equipment, coiling temperature is 530-610℃;
[0010] (3) Pickling and cold rolling process: After the hot-rolled steel strip is pickled to remove the surface iron oxide scale, it is cold-rolled in a 5-stand cold rolling mill with a cold rolling reduction rate of 50-70% and a thickness of 0.7-2.0 mm;
[0011] (4) Continuous hot-dip galvanizing and skin-passing process: The cold-hardened steel strip is unrolled and welded for continuous production. The furnace speed is 50-140 m / min, the average heating temperature is 780-840°C, and it is slowly cooled to 660-710°C, then cooled to 440-470°C. The temperature of the zinc pot is 440-480°C, the top temperature of the top roller cooling tower is ≤240°C, the skin-passing elongation is 0.4%-0.8%, and the straightening elongation is ≤0.3%.
[0012] Furthermore, the chemical composition of the dual-phase steel in mass percentage is C: 0.14%, Si: 0.16%, Mn: 2.04%, P: 0.016%, S: 0.003%, Alt: 0.033%, Cr: 0.37%, Ti: 0.012%, Ca: 0.0021%, and the rest is Fe and impurities.
[0013] Furthermore, the mechanical properties of the dual-phase steel meet the following requirements: yield strength R p0.2 :579-620MPa,.
[0014] Furthermore, the mechanical properties of the dual-phase steel meet the following requirements: tensile strength R m :849-868MPa.
[0015] Furthermore, the mechanical properties of the dual-phase steel meet the following requirements: elongation A 50 :18.5-20.0%.
[0016] Compared with the prior art, the beneficial technical effects of the present invention are:
[0017] The 780MPa grade galvanized dual-phase steel of the present invention has the characteristics of high strength, high work hardening index, high initial work hardening rate, good matching of strength and ductility, and high corrosion resistance, which meets the requirements of lightweight material selection for automobiles and differentiated applications of users. Mechanical properties: yield strength R p0.2 : 500-650MPa, tensile strength R m ≥780MPa, elongation A 50 ≥14%. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The present invention will be further described below in conjunction with the accompanying drawings.
[0019] Figure 1 The microstructure diagram of the embodiment of the present invention. DETAILED DESCRIPTION
[0020] The present invention is described in detail below through specific examples. The examples are only intended to help understand the present invention but are not intended to limit the present invention.
[0021] Example
[0022] According to the above steelmaking production process requirements, the actual slab chemical composition is shown in Table 1.
[0023] Table 1 Chemical composition of the present invention (wt%)
[0024]
[0025] According to the above hot rolling process requirements, the hot rolling thickness is 2.3-4.0mm, and the actual process is shown in Table 2.
[0026] Table 2 Hot rolling process of the embodiment of the present invention
[0027]
[0028] According to the above cold rolling, hot dip galvanizing and skin-passing process requirements, the cold rolling thickness is 0.7-2.0mm, and the actual hot dip galvanizing and skin-passing process is shown in Table 3.
[0029] Table 3 Hot-dip galvanizing and skin-passing process of the embodiment of the present invention
[0030]
[0031] The mechanical properties of the steel strip according to the embodiment of the present invention were tested, and the test results are shown in Table 4.
[0032] Table 4 Mechanical properties of the steel strip in the embodiment of the present invention
[0033]
[0034] From the data in Table 4, it can be seen that the mechanical properties of the 780MPa grade galvanized dual-phase steel for high yield strength automobile structure of the present invention are as follows: yield strength R p0.2 : 579-620MPa, tensile strength R m : 849-868MPa, elongation A 50 : 18.5-20.0%. The steel strip product obtained by the above process has been used by users and has suitable performance and can be promoted for use.
[0035] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for producing 780MPa grade galvanized dual-phase steel for high yield strength automobile structure, characterized in that: include: (1) Smelting-continuous casting production process: molten iron pretreatment-converter-LF refining-slab continuous casting; oxygen blowing and decarburization are carried out during the converter top and bottom combined blowing smelting, and aluminum iron, manganese iron, silicon iron and chromium iron are added during the converter steelmaking process for deoxidation and alloying, and the P and S components are controlled to prevent the molten steel from overoxidation. The steelmaking temperature is ≥1600℃; LF refining outside the furnace adopts the LF full-process argon blowing process, and the target composition is adjusted according to the molten steel composition. The molten steel composition for the casting machine is C:
0. 13-0.17%, Si: 0.10-0.30%, Mn: 1.9-2.3%, P≤0.020%, S≤0.015%, Alt: 0.010-0.060%, Cr: 0.2-0.5%, Ti≤0.03%, Ca: 0.0008-0.0025%, the rest is Fe and impurities; slab continuous casting superheat 15-40℃, pulling speed controlled at 0.8-1.5m / min; (2) Hot rolling production process: heating of ingot - rough rolling - finishing rolling - coiling; ingot furnace time is 160-320min, furnace temperature is 1200-1280℃, rough rolling adopts 3+3 mode 2-stand rolling mill, finishing rolling adopts 7-stand rolling mill, finishing rolling start temperature is 960-1050℃, finishing rolling final temperature is 850-920℃, hot rolled steel strip thickness is 2.3-4.0mm; cooling adopts laminar cooling equipment, coiling temperature is 530-610℃; (3) Pickling and cold rolling process: After the hot-rolled steel strip is pickled to remove the surface iron oxide scale, it is cold-rolled in a 5-stand cold rolling mill with a cold rolling reduction rate of 50-70% and a thickness of 0.7-2.0 mm; (4) Continuous hot-dip galvanizing and skin-passing process: The cold-hardened steel strip is unrolled and welded for continuous production. The furnace speed is 50-140 m / min, the average heating temperature is 780-840°C, and it is slowly cooled to 660-710°C, then cooled to 440-470°C. The temperature of the zinc pot is 440-480°C, the top temperature of the top roller cooling tower is ≤240°C, the skin-passing elongation is 0.4%-0.8%, and the straightening elongation is ≤0.3%.
2. The method for producing 780MPa grade galvanized dual-phase steel for high yield strength automobile structure according to claim 1, characterized in that: The chemical composition of the dual-phase steel in mass percentage is C: 0.14%, Si: 0.16%, Mn: 2.04%, P: 0.016%, S: 0.003%, Alt: 0.033%, Cr: 0.37%, Ti: 0.012%, Ca: 0.0021%, and the rest is Fe and impurities.
3. The method for producing 780MPa grade galvanized dual-phase steel for high yield strength automobile structure according to claim 1, characterized in that: The mechanical properties of the dual-phase steel meet the following requirements: yield strength R p0.2 :579-620MPa,.
4. The method for producing 780MPa grade galvanized dual-phase steel for high yield strength automobile structure according to claim 1, characterized in that: The mechanical properties of the dual-phase steel meet the following requirements: tensile strength R m :849-868MPa.
5. The method for producing 780MPa grade galvanized dual-phase steel for high yield strength automobile structure according to claim 1, characterized in that: The mechanical properties of the dual-phase steel meet the following requirements: elongation A 50 :18.5-20.0%.
Citation Information
Cited By
Production method of 590MPa-grade zinc-aluminum-magnesium-plated dual-phase steel strip for automobile structure
CN120041749A
Production method of zinc-aluminum-magnesium-plated high-strength steel strip with yield strength of 390 MPa for completely-annealed and low-cost photovoltaic support
CN120099393A
Galvanized dual-phase steel of different yield strength grades and 780 mpa tensile strength grade and manufacturing method therefor
WO2026145022A1