Powder for producing ceramic structure and method for producing ceramic structure using the same
Patent Information
- Application Number
- JP2021184894
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2021-11-12
- Publication Date
- 2024-11-14
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing ceramic structures used in applications requiring electrical properties, such as those in communications and aerospace, face challenges in achieving a low dielectric loss tangent due to the presence of small voids and uneven melting during laser-based additive manufacturing, which increases dielectric loss.
A raw material powder comprising specific ratios and particle sizes of inorganic compounds with varying thermal conductivities and absorptivity is used, ensuring uniform melting and reducing voids, thereby achieving a low dielectric loss tangent.
The solution enables the production of ceramic structures with high precision and low dielectric loss tangent, improving electrical signal transmission and mechanical strength.
Smart Images

Figure 00000021_0000 
Figure 00000021_0001 
Figure 00000021_0002
Abstract
Description
Technical Field
[0001] The present invention relates to a powder used when forming a ceramic structure by laser irradiation.
Background Art
[0002] Additive manufacturing technology (3D printer) for performing free-form shaping based on the shape data of a three-dimensional model is becoming widespread. In recent years, there has been a demand for a technology for manufacturing a high-strength ceramic structure with high precision using inorganic compound materials such as metal oxides and metal carbides, in addition to resins and metals that have conventionally been used as shaping materials for 3D printers.
[0003] Patent Document 1 discloses a raw material powder suitable for the powder bed fusion method and the cladding method. Specifically, absorber particles having a higher absorption ability for light of the wavelength contained in the laser light than other compositions are added to a powder containing inorganic compound particles with low absorption ability such as Al2O3 and ZrO2 that are the main components of the ceramic structure. The presence of absorber particles in the raw material powder suppresses the diffusion of laser light in the powder and realizes local heating and melting, enabling the production of a ceramic structure with high shaping accuracy and high mechanical strength.
[0004] Patent Document 2 discloses a technique in which a powder containing absorber particles as a main component of SiO2 is used as a raw material, shaping is performed by the powder bed fusion method, and heat treatment (hereinafter referred to as firing) is applied to the obtained shaped object. By firing, the components around the cracks generated in the ceramic structure during shaping are melted to fill the cracks, making it possible to obtain a ceramic structure with high mechanical strength.
Prior Art Documents
Patent Documents
[0005]
Patent Document 1
Patent Document 2
[0006] Ceramic structures have a wide range of applications, and in addition to mechanical and thermal properties, electrical properties are sometimes required. For example, ceramic structures used in the communications, aerospace, and medical fields require a low dielectric loss tangent (less than 0.01 at a frequency of 1 MHz). Dielectric loss tangent is a numerical value that represents the degree of electrical energy loss within a dielectric material, and the lower the dielectric loss tangent of the dielectric material, the more accurately it can transmit high-frequency electrical signals.
[0007] The dielectric loss tangent tends to increase as the number of small voids with major axes ranging from a few micrometers to tens of micrometers increases within the ceramic structure. It is believed that localized discharges (partial discharges) occurring in the internal voids when a voltage is applied to the ceramic structure contribute to the increase in the dielectric loss tangent. Therefore, in order to achieve a ceramic structure with a low dielectric loss tangent, it is necessary to minimize the number of small internal voids.
[0008] Patent Document 1 describes a method of lowering the melting point of raw material powder by mixing Al2O3 with ZrO2 or Gd2O3, which can form a eutectic with Al2O3. Since particles with different compositions, such as Al2O3 and ZrO2, or Al2O3 and Gd2O3, also have different thermal conductivity, heat from laser irradiation may not be transferred as easily to the particles with lower conductivity. As a result, the melting state of each particle becomes uneven, some particles remain unmelted, voids are formed within the fabricated object, and the dielectric loss tangent tends to increase.
[0009] Patent Document 2 describes how cracks in ceramic structures are reduced by firing them after fabrication, thereby improving their mechanical strength. However, it is unclear whether the small voids are reduced to a degree that allows for the achievement of a low dielectric loss tangent.
[0010] As mentioned above, powder bed fusion bonding has made it possible to fabricate ceramic structures with high mechanical strength and high precision, but research into reducing the dielectric loss tangent of these ceramic structures has not progressed.
[0011] The present invention provides a raw material powder that enables the production of ceramic structures with high precision and low dielectric loss tangent by powder bed fusion bonding. [Means for solving the problem]
[0012] The powder according to the present invention is a powder used in an additive manufacturing method in which a shape is formed by irradiating with laser light, and comprises inorganic compound particles A, inorganic compound particles B having a lower thermal conductivity than particles A, and absorber particles that exhibit higher absorption capacity than particles A and B for light of wavelengths contained in the laser light, wherein the average particle diameter of particles A is D(A) μm, the average particle diameter of particles B is D(B) μm, and the mass fraction of particles A in the powder is W(A) by weight, and the mass fraction of particles B is W(B) by weight, and the powder satisfies formulas (1) to (4). 5.0≦W(A) Formula (1) 5.0≦W(B) Formula (2) 60.0≦W(A)+W(B) Formula (3) 1.2≦D(A) / D(B)≦400.0 Formula (4) [Effects of the Invention]
[0013] If the powder of the present invention is used as a raw material powder in additive manufacturing technology, it becomes possible to manufacture ceramic structures with high precision and low dielectric loss tangent. [Brief explanation of the drawing]
[0014] [Figure 1] This diagram schematically illustrates the manufacturing process of ceramic structures using powder bed fusion bonding. [Figure 2] This is a binarized image of a ceramic structure's surface observed with a laser microscope. [Modes for carrying out the invention]
[0015] Regarding the powder according to the present invention, specific examples will be given for explanation. However, the present invention is not limited to the following specific examples and can be modified within the scope of the technical idea of the present invention.
[0016] <Ceramic structure> The ceramic structure in the present invention is composed of inorganic compounds and may be in any of a crystalline state, an amorphous state, or a mixture thereof. Inorganic compounds include metal and non-metal oxides, nitrides, carbides, and borides. The present invention is particularly suitable for the production of ceramic structures of metal oxides and non-metal oxides. Hereinafter, the ceramic structure may sometimes be simply referred to as a structure.
[0017] (Void in the ceramic structure) Generally, structures produced by additive manufacturing technology contain many spaces of various sizes such as voids and cracks. In the present invention, a space with a major axis of 1 μm to 50 μm is called a "void", and a space with a major axis exceeding 50 μm is called a "crack". The reason that many voids are contained in the structure is considered to be that a part where the melting of the powder does not proceed sufficiently is formed while the raw material powder is irradiated with laser light.
[0018] The shaping by the powder bed fusion method is performed by irradiating the raw material powder while scanning a laser beam based on the shape data of the three-dimensional model to be manufactured. From the viewpoint of shaping efficiency, a higher scanning speed is preferable, and raw material powder that melts with short-time laser beam irradiation is desired.
[0019] Al2O3, which is widely used as a ceramic material, has a high melting point of about 2072°C and low light absorption ability in a wide wavelength range from ultraviolet to infrared. Therefore, in Patent Documents 1 and 2, Al2O3, a material that forms a eutectic with Al2O3 (eutectic material), and an absorber are mixed to lower the melting point of the raw material powder and perform shaping.
[0020] A thermal conductivity difference occurs between two types of particles having differences in composition, crystal structure, etc. When laser light is irradiated onto a powder in which these two types of particles are mixed, since the way heat is transferred differs depending on the type of particle, even if the particles with higher thermal conductivity melt, the particles with lower thermal conductivity may not melt, and the melting state of the powder may become non-uniform. In parts where melting does not proceed sufficiently, the voids between the particles cannot be filled, and voids remain in the structure.
[0021] Patent Documents 1 and 2 describe ZrO2, Gd2O3, and SiO2 as materials that form eutectics with Al2O3. Table 1 shows the thermal conductivity, melting point, and specific gravity of Al2O3 and each eutectic material. The thermal conductivity of each eutectic material is lower than that of Al2O3.
[0022]
Table 1
[0023] Among the eutectic materials listed in Table 1, since SiO2 has a lower melting point than Al2O3, if a raw material powder in which Al2O3 and SiO2 are mixed is used, an effect is expected that SiO2 will preferentially melt and fill the voids. However, in reality, even when a ceramic structure is fabricated using the mixed powder of Al2O3 and SiO2 described in Patent Documents 1 and 2, the voids in the structure cannot be sufficiently reduced, and a low dielectric tangent cannot be realized. When the ratio of SiO2 in the raw material powder is increased or the heating temperature is increased by raising the irradiation power of the laser light, the structure may melt and the shape may collapse.
[0024] Patent documents 1 and 2 use a powder mixture of Al2O3 particles and SiO2 particles with a larger particle size than the Al2O3 particles. The inventors have succeeded in uniformly melting particles with different thermal conductivity in the powder by making the particle size of the particles with lower thermal conductivity smaller than the particle size of the particles with higher thermal conductivity (reducing particle size). By reducing the particle size of the particles with lower thermal conductivity, the time it takes for the particles with lower thermal conductivity to melt can be brought closer to the time it takes for the particles with higher thermal conductivity to melt, thereby enabling uniform melting of the powder in the laser irradiation area.
[0025] Then, by devising the particle size ratio and mixing ratio of multiple types of particles with different thermal conductivity contained in the powder, we obtained a powder suitable as a raw material for additive manufacturing technology, which enables the realization of ceramic structures with few voids and low dielectric loss tangent.
[0026] The present invention will be described in detail below.
[0027] <Raw material powder> The raw material powder according to the present invention includes inorganic compound particles A, inorganic compound particles B with a lower thermal conductivity than particles A, and absorber particles that exhibit higher absorption capacity than particles A and B for light of wavelengths contained in laser light. Particles A, B, and absorber particles are of different types. Here, "different types" means that the components, chemical composition, crystallinity, etc., of the particles differ among the multiple particles.
[0028] Particle A, particle B, and absorber particle each refer to units that exist independently within the powder. For example, if particle A exists in the powder as a secondary particle formed by the bonding of multiple primary particles, then the secondary particle is called particle A.
[0029] Inorganic compound particles A and B are the main components of the ceramic structure. Particles A and B are single-composition particles composed of metallic or nonmetallic oxides or nitrides with low absorption capacity for infrared light. The raw material powder can also be described as a mixed powder of powder A, which consists of multiple particles A; powder B, which consists of multiple particles B; and absorber powder, which consists of multiple absorber particles. Particles A and B, which are the main components of the ceramic structure, are those that are present in the raw material powder at a concentration of 5.0 [weight%] or more each, and whose total is 60% or more by weight of the raw material powder. If the mass fractions of particles A and B in the raw material powder are W(A) [weight%] and W(B) [weight%], they can be expressed by the following formula. 5.0≦W(A) Formula (1) 5.0≦W(B) Formula (2) 60.0≦W(A)+W(B) Formula (3)
[0030] (Inorganic particles A and B) Among the particles in the raw material powder that form the main components of the ceramic structure, particles with relatively high thermal conductivity are designated as particle A, and particles with lower thermal conductivity than particle A are designated as particle B. Particles A and B can be selected according to the properties required for the ceramic structure to be manufactured. When manufacturing oxide-based ceramic structures, it is preferable that both particle A and B are composed of metal oxides and / or metalloid oxides.
[0031] Particle A preferably contains a composition selected from the group consisting of, for example, Al2O3, ZrO2·Y2O3, Y2O3, and SiO2, and is particularly preferably Al2O3. Since Al2O3 has particularly high thermal conductivity among metal oxides and metalloid oxides, it can quickly transfer the heat emitted from the absorber particles by absorbing laser light to the entire powder, enabling fabrication in a shorter time. In addition, since Al2O3 forms a eutectic with many types of inorganic compounds, it is possible to fabricate objects in combination with various compositions.
[0032] It is preferable that particle A contains a composition that forms a eutectic with the composition constituting particle B. When particle A and particle B form a eutectic relationship, the melting point of the raw material powder can be lowered. For example, even if the melting point of the composition contained in particle A is high, the melting point is lowered by forming a eutectic with the composition contained in particle B, making it easier to melt. Furthermore, when the molten state in which inorganic particle A and inorganic particle B have melted and mixed solidifies, crystalline phases mix between the multiple compositions, forming a complex and interwoven interface. As a result, even when external stress is applied, cracks along the interface are less likely to occur, and the strength is improved.
[0033] Inorganic particle B can be selected from the group consisting of, for example, SiO2, ZrO2·Y2O3, 3Al2O3·2SiO2, and 2MgO·2Al2O3·5SiO2.
[0034] The melting point of inorganic particle B, which has a relatively low thermal conductivity, is preferably lower than that of inorganic particle A, and more preferably 1900°C or lower, which can be easily reached by laser irradiation. This allows for rapid melting due to the heat obtained from the absorber particles during laser irradiation. Furthermore, by firing at a relatively low temperature after fabrication that does not impair the shape of the structure, the composition of inorganic particle B is melted, and the effect of filling and reducing remaining voids in the structure can be expected. From this viewpoint, inorganic particle B is particularly preferably SiO2. SiO2 has a low melting point of 1650°C and can also form a eutectic with compositions such as Al2O3.
[0035] Preferred combinations of particle A and particle B when manufacturing oxide-based ceramic structures include Al2O3-Gd2O3, Al2O3-GdAlO3, Al2O3-Y2O3, Al2O3-YAlO3, and Al2O3-Y3Al5O 12 Examples include Al2O3-ZrO2 and Al2O3-SiO2.
[0036] The inventors conducted thorough research and discovered that by further satisfying the following equation (4), the melting rates of particles A and B, which are the main components of the ceramic structure, can be brought closer together, even though particles A and B have different thermal conductivity. 1.2≦D(A) / D(B)≦400 Formula (4)
[0037] D(A)[μm] and D(B)[μm] are the particle diameters of particle A and particle B, respectively.
[0038] Here, the particle diameter of inorganic particle A refers to the average particle diameter of multiple inorganic particle A particles, and the particle diameter of inorganic particle B refers to the average particle diameter of multiple inorganic particle B particles. If inorganic particle A and inorganic particle B are composed of single particles, the average particle diameter of each particle is expressed directly. If inorganic particle A and inorganic particle B are produced by agglomerating minute particles, the average particle diameter of the inorganic particles after agglomeration is expressed. It is preferable that all the minute particles constituting inorganic particle A and inorganic particle B have the same composition, but they may also contain particles with different compositions.
[0039] The particle size can be calculated using the following method: The powder is measured using a laser diffraction / scattering particle size analyzer. The median diameter (also called the median value), which is the particle size at which the cumulative frequency reaches 50% (D50) in the measured powder, is defined as the average particle size.
[0040] This invention reduces voids in a ceramic structure when the raw material powder contains particle A, which is the main component of the ceramic structure, and particle B, which has a lower thermal conductivity than particle A. In particular, when the thermal conductivity of particle A is K(A) [W / m·K] and the thermal conductivity of particle B is K(B) [W / m·K], the effect is significant when K(A) / K(B) is between 2.0 and 50.0, and even more significant when it is between 3.0 and 30.0.
[0041] In equation (4), D(A) / D(B) is more preferably 1.4 to 150, and even more preferably 1.4 to 60. By setting D(A) / D(B) within the above range, the time required for each particle A and B to dissolve can be made closer, and the entire powder in the laser irradiation area can be uniformly melted. As a result, the voids are reduced further, and an even lower dielectric loss tangent can be achieved.
[0042] The particle size D(A) of particle A is preferably 2.0 [μm] or more and 100 [μm] or less, more preferably 5.0 [μm] or more and 70.0 [μm] or less, and even more preferably 10.0 [μm] or more and 30.0 [μm] or less. The particle size D(B) of inorganic particle B is preferably 0.1 [μm] or more and 50.0 [μm] or less, more preferably 1.0 [μm] or more and 40.0 [μm] or less, and even more preferably 5.0 [μm] or more and 20.0 [μm] or less.
[0043] W(A) is preferably 8.0% by weight or more and 88.0% by weight or less, and more preferably 18.0% by weight or more and 78.0% by weight or less. When W(A) is within the above range, a certain amount of particles A with high thermal conductivity is present, so the heat emitted from the absorber particles by laser irradiation can be efficiently transferred to the entire powder in the irradiated area. As a result, it becomes possible to fabricate ceramic structures in a shorter time.
[0044] When the melting point of particle B is lower than that of particle A, W(B) is preferably 10.0 [weight%] or more and 90.0 [weight%] or less, and more preferably 20.0 [weight%] or more and 80.0 [weight%] or less. When W(B) is within the above range, the voids between particles are more easily filled by the melting of particle B, which has a lower melting point, making it easier to achieve a low dielectric loss tangent. Furthermore, in the firing process described later, it becomes possible to process at a lower temperature corresponding to the melting point of particle B, making it easier to achieve both high molding accuracy and low dielectric loss.
[0045] W(A) + W(B) is preferably 80.0% by weight or more, and more preferably 90.0% by weight or more.
[0046] (Absorbing particles) Absorbing particles are those particles among the various types of particles contained in the raw material powder that exhibit the highest absorption capacity for light of wavelengths contained in the laser light used for molding. The absorption rate of the absorbing particles is preferably 10% or more, more preferably 40% or more, and even more preferably 60% or more, relative to the light of wavelengths contained in the laser light used.
[0047] The absorber particles efficiently absorb the laser light used during manufacturing, causing them to become hot. The heat emitted by the absorber particles is transferred to other particles within a region corresponding to the focal size of the laser beam, resulting in a temperature increase and melting, which enables fabrication using additive manufacturing technology. Furthermore, the absorber particles enable localized heating corresponding to the focal size of the laser beam, improving fabrication accuracy.
[0048] The absorptivity of absorber particles can be measured using a general spectrometer. Specifically, a sample containing the absorber particles is placed in a sample dish and placed in an integrating sphere. The absorptivity is calculated from the ratio of the electromagnetic wave spectrum measured by irradiating it with a assumed wavelength (near the laser wavelength used in manufacturing) to the value measured without the sample.
[0049] The absorbent particles are SiO, TiO, Ti2O3, ZnO, antimond-doped tin (ATO), indium-doped tin (ITO), MnO, MnO2, Mn2O3, Mn3O4, FeO, Fe2O3, Fe3O4, Cu2O, CuO, Cr2O3, CrO3, NiO, V2O3, VO2, V2O5, V2O4, Co3O4, CoO, Tb4O7, Pr6O 11 Preferably, the material contains at least one selected from the group consisting of ZrN, ZrC, ZrSi, and AlN. Because these absorber particles have high infrared light absorption capacity, they can absorb laser light and transfer the amount of heat necessary to melt the entire powder in the laser-irradiated area to the surroundings.
[0050] The mass fraction of absorber particles contained in the raw material powder is preferably 0.1 [weight%] or more and 20.0 [weight%] or less, more preferably 0.2 [weight%] or more and 20.0 [weight%] or less, and even more preferably 0.5 [weight%] or more and 20.0 [weight%] or less. When the absorber particles are within the above range, it becomes easy to ensure that at least one absorber particle is present within a region equivalent to the focal size of the laser beam, thereby reducing unevenness in the fabrication process depending on the location.
[0051] For the reasons stated above, W(A) + W(B) in equation (3) is preferably less than 99.9 [weight%], more preferably less than 99.8 [weight%], and even more preferably less than 99.5 [weight%].
[0052] The particle size of the absorbent particles is preferably 0.1 [μm] to 20.0 [μm], more preferably 1.0 [μm] to 10.0 [μm], and even more preferably 1.0 [μm] to 5.0 [μm]. Within this range, the particles can be uniformly dispersed in the powder without agglomeration. Regarding the particle size of the absorbent particles, similar to inorganic particles A and B, if they are individual particles, the particle size is expressed as is; if they are produced by agglomerating minute particles, the particle size of the particles after agglomeration is expressed.
[0053] While particles A and B are the main components of the ceramic structure, absorber particles are intended to absorb laser light and are often not necessary components for achieving the desired properties of the ceramic structure. In such cases, the addition of absorber particles increases the amount of unwanted components, making it difficult to control the properties. Therefore, it is preferable that the absorber particles contain the same metalloid or metallic elements as particles A or B. By having the absorber particles contain the same metalloid or metallic elements as particles A or B, the addition of unwanted components to the ceramic structure is suppressed, making it easier to design the material to achieve the desired properties.
[0054] Absorber particles containing SiO are particularly preferred. Among the absorber particles exemplified earlier, SiO has a low melting point and melts rapidly while generating heat when irradiated with a laser, allowing for the creation of structures with a smooth surface and minimal irregularities. Furthermore, the SiO remaining in the fabricated object during firing reacts with oxygen and changes to SiO2. This change is accompanied by an increase in volume, so in addition to the melting effect described above, the volume increase also effectively fills the voids, enabling the achievement of an even lower dielectric constant.
[0055] Furthermore, the raw material powder may contain particles C other than particles A, particles B, and absorbent particles. If the mass fraction of particle C in the raw material powder is 5.0 [weight%] or more, particle C also becomes a major component of the ceramic structure. In such cases, it is preferable that particle C and particle A or particle C and particle B satisfy the relationship of the present invention.
[0056] The method for producing each particle is not particularly limited. Manufacturing methods such as dry (fumed) method, wet method, gas-phase reaction method, and spray-drying method can be used.
[0057] <Particle mixing process> It is preferable that the absorber particles in the powder are uniformly dispersed, and it is preferable that the degree of dispersion, as described later, is 0.80 or less. This allows the heat generated from the absorber particles to be uniformly transferred to the powder in the laser irradiation area, making it easier to match the melting rate of inorganic particles other than the absorber particles. As a result, a structure with few voids and a low dielectric loss tangent can be obtained.
[0058] It is preferable that the powder undergoes a mixing process before being used in the manufacture of structures. The mixing process is preferably carried out using mixing equipment such as a V-type mixer, ball mill, or rocking mixer.
[0059] From the viewpoint of uniformly dispersing absorbent particles, efficiently dispersing particles A and B, which have different specific gravities and particle sizes, in a short mixing time, and suppressing excessive impact on the particles, it is particularly preferable to use a V-type mixer.
[0060] <Manufacturing process for ceramic structures> The powder according to the present invention can be used as a raw material powder for additive manufacturing, which involves heating by irradiating with laser light. The manufacturing process for ceramic structures using additive manufacturing includes the following steps (i) and (ii). Steps (i) and (ii) are repeated depending on the shape of the ceramic structure to be manufactured. (i) Steps to place the raw material powder into the laser light irradiation area. (ii) A process of irradiating the raw material powder with laser light based on 3D modeling data.
[0061] As a specific example of a manufacturing process for ceramic structures, the case using powder bed fusion sintering will be explained with reference to Figure 1.
[0062] First, the raw material powder 101 is placed on the molding surface of the base 130 installed on the stage 151 and spread to a predetermined thickness using the roller 152. The powder spread to a predetermined thickness is called the powder layer 102 (Figures 1(a) and (b)). Based on the three-dimensional shape data of the item to be manufactured, the surface of the powder layer 102 is irradiated with laser light emitted from the laser light source 180 while scanning with the scanner unit 181. In the area 182 irradiated with laser light, the powder sintersects or melts and then solidifies, forming a solidified area 100 (Figure 1(c)). Next, the stage 151 is lowered to form a new powder layer 102 on top of the solidified area 100 (Figure 1(d)). The newly formed powder layer 102 is irradiated with laser light in the same manner as in Figure 1(c), forming a solidified area 100 in the irradiated area. At this time, by adjusting the laser beam output to the extent that the surface layer on the newly formed powder layer 102 side of the previously formed solidified part melts, the previously formed solidified part and the later formed solidified part can be joined together. By repeating this series of steps, the solidified parts 100 formed layer by layer are joined together to form a single object 110 of the desired shape (Figures 1(e) and (f)). Finally, the unsolidified powder 103 is removed, and if necessary, unnecessary parts of the object are removed or the object is separated from the base (Figures 1(g) and (h)).
[0063] In the manufacturing process of the present invention, it is preferable to have a step of firing the manufactured ceramic mixed structure after repeating steps (i) and (ii) the required number of times. There are no restrictions on the heating means in the firing step, and resistance heating, induction heating, infrared lamp heating, laser heating, electron beam heating, etc., can be appropriately selected and used depending on the purpose. By firing, the voids in the structure can be further reduced and the dielectric loss tangent can be lowered. In other words, even if some voids remain in the ceramic structure after fabrication, the voids can be reduced by going through the firing step. If the voids cannot be sufficiently reduced by firing alone, firing may be performed after impregnation with a liquid containing a component that repairs the voids.
[0064] The firing temperature should preferably be below the melting point of the ceramic structure and at a temperature where crystal growth does not occur, depending on the main components of the ceramic structure. If particles A and B form a eutectic, firing should be performed within the range of the eutectic temperature + 50°C. If particle B is SiO2, the firing temperature should preferably be between 1600°C and 1730°C, and more preferably between 1650°C and 1710°C. Within this range, the SiO2 melts, filling the voids without distorting the shape of the structure.
[0065] <Evaluation method for powders> (Particle size) The particle size of a particle is defined as the median diameter (also called the median value), which is the average particle size. In powders, the median diameter is the particle size at which the cumulative frequency reaches 50% (D50). The average particle size can be measured using a laser diffraction / scattering particle size analyzer. If single-particle powder is not available, a mixed powder can be classified using a multi-part classifier (for example, an elbow jet classifier manufactured by Nippon Steel Mining Co., Ltd.), and the average particle size can be measured for each type of particle.
[0066] (Thermal conductivity) If a powder consisting of a single type of particle is available, the thermal conductivity is measured by compressing 10.0 g of the powder at 30 MPa to form a cylindrical pellet with a diameter of 3 cm, and then measuring it using a conductivity measuring device.
[0067] If only mixed powder is available, the mixed powder is classified using a multi-part classification device (for example, an elbow jet classifier manufactured by Nippon Steel Mining Co., Ltd.), and the separated particles are pelletized as described above and measured using a thermal conductivity measuring device.
[0068] (Dispersion degree) The dispersion index for absorber particles was calculated using a scanning electron microscope. The powder containing absorber particles was observed in a 500x magnified field of view at an acceleration voltage of 5.0kV. The observed images were then processed using the image processing software "ImageJ" (available from https: / / imagej.nih.gov / ij / ) and the index was calculated as follows.
[0069] The image was binarized so that only absorber particles were extracted. The centroid coordinates were calculated for each absorber particle (n), and the distance dn min between each absorber particle and its nearest absorber particle was calculated. If the average nearest-neighbor distance between absorber particles in the image is denoted as d ave, the dispersion is given by the following formula.
[0070]
number
[0071] The variance was calculated for five randomly observed fields using the procedure described above, and the average value was used as the variance evaluation index. A smaller variance evaluation index indicates better variability.
[0072] <Evaluation Methods for Ceramic Structures> (porosity) The obtained ceramic structure was impregnated with 10 ml of black oil-based ink. The surface of the impregnated structure was polished with Φ10 mm sandpaper, and the polished surface was observed at 20x magnification using an optical microscope.
[0073] The observed images were binarized using the image processing software "ImageJ" (available from https: / / imagej.nih.gov / ij / ). Figure 2 shows an example of a binarized image. In the binarized image, the bright areas 202 represent the ceramic structure, and the dark areas 201 represent the voids within the ceramic structure. Let Sd be the area of the dark areas 201 in the binarized image, and S be the area of the entire image. The porosity is calculated as Sd × 100 / S. A smaller porosity indicates fewer voids.
[0074] The measurement method described above allows ink to penetrate even smaller voids than those measured by porosity (described later), and directly visualizes this process. Therefore, it is possible to evaluate the relative importance of even the smallest gaps, which cannot be seen with porosity measurement methods. Consequently, it is possible to obtain correlations with physical properties that are affected even by fine gaps, such as dielectric loss tangent.
[0075] (Porosity) Porosity is evaluated according to the method based on JIS standard R1634, which is the measurement method for the density and open porosity of sintered fine ceramics. Specifically, for three cylindrical ceramic structures with a diameter of 20.0 mm and a thickness of 1.0 mm, the dry mass of the structure is W1, the mass in water is W2, and the saturated mass is W3, and the values calculated using the following formula are taken as the porosity. A lower porosity indicates fewer large pores such as cracks. {(W3-W1) / (W3-W2)}×100
[0076] The dry mass (W1) is measured by placing the ceramic structure in a constant temperature and humidity chamber, maintaining the temperature at 110°C for 1 hour, and then allowing it to cool. The mass in water (W2) is measured by suspending the saturated water sample with wire, submerging it below the water surface in a boiling bath, boiling it for 3 hours or more, and then allowing it to cool to room temperature. The mass of the saturated water sample is measured while it is still suspended in water by wire, and the mass of the jig is taken as the corrected value. The saturated water mass (W3) is measured after removing the saturated water sample from the water, quickly wiping the surface with a damp gauze to remove water droplets.
[0077] (Dielectric loss tangent) For evaluation, a cylindrical ceramic structure with a diameter of 20.0 mm and a thickness of 1.0 mm was fabricated, and the complex dielectric constant was measured three times under conditions of frequencies from 1 kHz to 1 MHz. The dielectric loss tangent at 1 MHz was calculated from each measurement, and the average value was defined as the dielectric loss tangent. The formula tanδ = ε'' / ε' was used to calculate the dielectric loss tangent, where δ represents the loss angle, ε'' represents the dielectric loss rate, and ε' represents the dielectric constant.
[0078] (Dimensional stability) Dimensional stability was assessed by checking the degree of error compared to the target dimensions. For a rectangular ceramic structure measuring 5.0 mm × 42.0 mm × 6.0 mm, the length of the 42.0 mm side (the longest side) of the fabricated structure was measured. The difference between this measurement and the dimensions of the 3D data created in CAD was calculated as the error (%). A smaller error value indicates better dimensional stability.
[0079] (Surface roughness) Surface roughness is determined by measuring the Ra value of the surface of a ceramic structure fabricated for dimensional stability evaluation using a laser microscope. A smaller surface roughness value indicates better surface smoothness.
[0080] (3-point bending strength) The bending strength of the structure is evaluated by a three-point bending test based on R1601, the JIS standard for room-temperature bending strength of fine ceramics.
[0081] Specifically, ten rectangular ceramic structures measuring 5.0 mm × 42.0 mm × 6.0 mm were fabricated and polished to a size of 3.0 mm × 30.0 mm × 4.0 mm, which were then used as evaluation samples.
[0082] For each sample, if the maximum load at fracture is P[N], and the distance between external supports (L) is 30[mm], the width of the specimen (w) is 4[mm], and the thickness of the specimen (t) is 3[mm], then 3×P×L / (2×w×t 2The three-point bending strength was calculated using the formula shown, and the average of these values was used as the three-point bending strength. A higher value indicates greater strength. [Examples]
[0083] [Example 1] <Powder 1> As shown in Table 2, Al2O3 powder with an average particle size of 24 μm, SiO2 powder with an average particle size of 10 μm, and SiO powder with an average particle size of 5 μm were prepared, and the thermal conductivity of each powder was measured using a thermal conductivity measuring device TPS2500 (Hot Disk). As shown in Table 2, a total of 10.0 kg was weighed so that the mass fraction of Al2O3 powder was 54.0 wt%, the mass fraction of SiO2 powder was 44.0 wt%, and the mass fraction of SiO powder was 2.0 wt%. Each weighed powder was placed in a V-type mixer (V20, Seishin Kigyo Co., Ltd.) and mixed at a rotation speed of 26 rpm for 15 minutes to obtain powder 1. The thermal conductivity of each particle is shown in Table 1. For powder 1, the dispersion of absorber particles was measured by binarizing the observation images obtained using a scanning electron microscope "JSM-7800" (JEOL Ltd.), and the results are shown in Table 4.
[0084] <Structure 1-A> The ceramic structure was fabricated using the same manufacturing process as described in Figure 1.
[0085] For the 3D printing process, we used the 3D SYSTEM ProXDMP 100 (product name), which is equipped with a 50W fiber laser (beam diameter 65μm).
[0086] First, powder 1 was spread evenly on an alumina base 130 using a roller to form the first powder layer with a thickness of 20 μm (Figure 1(a), (b)).
[0087] Next, a 47.5W laser beam was irradiated onto the powder layer while scanning, melting and then solidifying the material powder in a circular area with a diameter of 10 mm, thereby forming a solidified portion 100 (Figure 1(c)). The drawing speed at this time was 60 mm / s and the drawing pitch was 80 μm.
[0088] Next, a new powder layer with a thickness of 20 μm was formed to cover the surface of the solidification section 100. The powder layer was then irradiated with a scanning laser beam to melt and solidify the material powder in a circular area with a diameter of 10 mm, thereby forming the solidification section 100 (Figures 1(d), (e)).
[0089] At this time, the laser was scanned in a direction perpendicular to the first drawing line to melt and solidify the powder. This process was repeated until the height of the solidified layer reached 1.0 mm, and three cylindrical structures with a diameter of 10.0 mm and a thickness of 1.0 mm were fabricated. The three structures were individually used to evaluate porosity, dielectric loss tangent, and other properties.
[0090] The obtained structures were placed in an electric furnace and fired. Specifically, the temperature was raised to 1690°C in 2 hours and 40 minutes under an atmospheric environment, held at 1690°C for 20 minutes, then the power was turned off and the structure was cooled to below 200°C in 5 hours to obtain three structures 1-A.
[0091] <Structure 1-B> Except for setting the area for solidifying the material powder to a rectangle of 5.0 mm × 42.0 mm and changing the number of times the process is repeated until the height of the solidified area reaches 6.0 mm, ten rectangular parallelepiped structures measuring 42.0 mm × 5.0 mm × 6.0 mm were fabricated in the same manner as structure 1-A.
[0092] The obtained structures were placed in an electric furnace and fired. Specifically, the temperature was raised to 1690°C in 2 hours and 40 minutes under an atmospheric environment, held at 1690°C for 20 minutes, then the power was turned off and the structure was cooled to below 200°C in 5 hours to obtain 10 structures 1-B.
[0093] <Rating> Structures 1-A and 1-B were evaluated. The evaluation items and results for each are shown in Tables 7 and 8. Ranking of evaluation items was performed according to the respective criteria.
[0094] (porosity) The porosity was calculated for structure 1-A according to the evaluation method described above. The evaluation rank was determined according to the following criteria. A: 9% or less B: 10% or more and 14% or less C: 15% or more and 19% or less D: 20% or more
[0095] (Porosity) Structure 1-A was evaluated using the evaluation method described above.
[0096] (Dielectric loss tangent) For structure 1-A, the dielectric loss tangent was measured using a 4284A precision LCR meter (Hewlett-Packard Corporation) according to the evaluation method described above. The evaluation rank was defined as follows. A: Less than 0.005 B: 0.005 or higher, less than 0.008 C: 0.008 or higher, less than 0.010 D:0.010 or more
[0097] (Dimensional stability) For the obtained structure 1-B, the length of the longest side, 42.0 mm, was measured with a caliper using the evaluation method described above, and the difference from the dimensions of the 3D data created in CAD was calculated. The evaluation rank was defined as follows. A: Less than 10% B: 10% or more but less than 15% C: 15% or more, less than 20% D: 20% or more
[0098] (Surface roughness) For one of the 10 structures 1-B, the Ra value was measured at 50x magnification using the line roughness measurement mode of the laser microscope "Vk-X200" (manufactured by Keyence Corporation), according to the evaluation method described above. The evaluation rank was defined as follows. A: 10μ or less B: 10μ or more and 20μ or less C: 20μ or more and 30μ or less D: 31μ or more
[0099] (3-point bending strength) After evaluating dimensional stability and surface roughness, ten structures 1-B were polished to obtain ten rectangular parallelepipeds measuring 3.0 mm × 30.0 mm × 4.0 mm. The three-point bending strength values were determined for these rectangular parallelepipeds according to the evaluation method described above.
[0100] [Examples 2-24] <Powder 2~24> As shown in Table 2, powders 2 to 24 were obtained using the same procedure as for powder 1, except that at least one of the types of particles A, B, and absorbent particles, the amount mixed, and the conditions were changed. For each of powders 2 to 24, the absorbent particles, particles A, and particles B were combined to make up 100 [weight]. Table 3 shows the results of determining the mixing conditions of powders 2 to 24 and the dispersion of absorbent particles, in the same manner as for powder 1.
[0101] <Structures 2~24> Using powders 2-24, structures 2-A to 24-A and structures 2-B to 24-B, as described in Examples 2-24, were prepared and fired in the same manner as structures 1-A and 1-B. Since the firing conditions were changed according to the type of particles mixed, the correspondence between each structure, powder, and firing conditions is shown in Table 6.
[0102] Using structures 2 to 24, the same evaluation as in Example 1 was performed, and the results are shown in Tables 7 and 8.
[0103] [Comparative Examples 1-7] <Powder 25~31> As shown in Table 4, powders 25 to 31 were obtained using the same procedure as for powder 1, except that at least one of the types, amounts, and conditions of particles A, B, and absorbent particles were changed. For each of powders 25 to 31, the absorbent particles, particles A, and particles B were combined to make up 100 [weight]. Table 5 shows the results of determining the mixing conditions of powders 25 to 31 and the dispersion of absorbent particles, in the same manner as for powder 1.
[0104] <Structures 25~31> Using powders 25-31, structures 25-A to 31-A and structures 25-B to 31-B, as described in Comparative Examples 1 to 7, were prepared in the same manner as structures 1-A and 1-B, and then fired. Since the firing conditions were changed according to the type of particles mixed, the correspondence between each structure, powder, and firing conditions is shown in Table 6.
[0105] Using structures 25-31, the same evaluation as in Example 1 was performed, and the results are shown in Tables 7 and 8.
[0106] These results confirm that molding is difficult with raw material powders that do not contain absorbents.
[0107] In a raw material powder where particle A is aluminum oxide particles and particle B is silicon dioxide particles, if all of equations (1) to (4) are satisfied, a ceramic structure with a porosity of 20% or less and a dielectric loss tangent of 0.01 or less could be obtained. On the other hand, powders that did not satisfy equation (4) had a porosity exceeding 20%, could not achieve a low dielectric loss tangent, and powder 31 with a D(A) / D(B) exceeding 400 could not be fabricated.
[0108] [Table 2]
[0109] [Table 3]
[0110] [Table 4]
[0111] [Table 5]
[0112] [Table 6]
[0113] [Table 7]
[0114] [Table 8] [Explanation of Symbols]
[0115] 100 Solidified section 101 powder 102 Powder layer 103 Unsolidified powder 110 Sculptures 130 base 151 stages 152 Rollers 180 Energy beam sources 181 Scanner section
Claims
1. A powder used in additive manufacturing, which is heated to create a shape, Particles A of a first inorganic compound; Particles B of a second inorganic compound; Including, The thermal conductivity of the second inorganic compound is lower than the thermal conductivity of the first inorganic compound, and the melting point of the second inorganic compound is lower than the melting point of the first inorganic compound; The particle size of the particle B is smaller than the particle size of the particle A, A powder characterized in that when the average particle diameter of the particle A is D(A) μm, the average particle diameter of the particle B is D(B) μm, the mass fraction of the particle A in the powder is W(A) weight %, and the mass fraction of the particle B is W(B) weight %, the formulas (1) to (4) are satisfied. 5.0≦W(A) Formula (1) 5.0≦W(B) Formula (2) 60.0≦W(A)+W(B) Formula (3) D(A) / D(B)≦400 Formula (4)
2. A powder used in additive manufacturing, which is heated to create a shape, Particles A of a first inorganic compound; Particles B of a second inorganic compound; Including, The thermal conductivity of the second inorganic compound is lower than the thermal conductivity of the first inorganic compound; The specific gravity of the second inorganic compound is lower than the specific gravity of the first inorganic compound; The particle size of the particle B is smaller than the particle size of the particle A, A powder characterized in that when the average particle diameter of the particle A is D(A) μm, the average particle diameter of the particle B is D(B) μm, the mass fraction of the particle A in the powder is W(A) weight %, and the mass fraction of the particle B is W(B) weight %, the formulas (1) to (4) are satisfied. 5.0≦W(A) Formula (1) 5.0≦W(B) Formula (2) 60.0≦W(A)+W(B) Formula (3) D(A) / D(B)≦400 Formula (4)
3. A powder used in additive manufacturing, which is heated to create a shape, Particles A of a first inorganic compound; Particles B of a second inorganic compound; Including, The thermal conductivity of the second inorganic compound is lower than the thermal conductivity of the first inorganic compound; The particle size of the particle B is smaller than the particle size of the particle A, A powder characterized in that, when the average particle diameter of the particle A is D(A) μm, the average particle diameter of the particle B is D(B) μm, the mass fraction of the particle A in the powder is W(A) weight %, and the mass fraction of the particle B is W(B) weight %, the W(A) is larger than the W(B), and the formulas (1) to (4) are satisfied. 5.0≦W(A) Formula (1) 5.0≦W(B) Formula (2) 60.0≦W(A)+W(B) Formula (3) D(A) / D(B)≦400 Formula (4)
4. A powder used in additive manufacturing, which is heated to create a shape, Particles A of a first inorganic compound; Particles B of a second inorganic compound having a melting point of 1900° C. or less; Including, The thermal conductivity of the second inorganic compound is lower than the thermal conductivity of the first inorganic compound; The particle size of the particle B is smaller than the particle size of the particle A, A powder characterized in that when the average particle diameter of the particle A is D(A) μm, the average particle diameter of the particle B is D(B) μm, the mass fraction of the particle A in the powder is W(A) weight %, and the mass fraction of the particle B is W(B) weight %, the formulas (1) to (4) are satisfied. 5.0≦W(A) Formula (1) 5.0≦W(B) Formula (2) 60.0≦W(A)+W(B) Formula (3) D(A) / D(B)≦400 Formula (4)
5. A powder used in additive manufacturing, which is heated to create a shape, Particles A of a first inorganic compound; Particles B of a second inorganic compound; Including, the first inorganic compound is aluminum oxide; the second inorganic compound is silicon dioxide; The particle size of the particle B is smaller than the particle size of the particle A, A powder characterized in that when the average particle diameter of the particle A is D(A) μm, the average particle diameter of the particle B is D(B) μm, the mass fraction of the particle A in the powder is W(A) weight %, and the mass fraction of the particle B is W(B) weight %, the formulas (1) to (4) are satisfied. 5.0≦W(A) Formula (1) 5.0≦W(B) Formula (2) 60.0≦W(A)+W(B) Formula (3) D(A) / D(B)≦400 Formula (4)
6. 6. The powder according to claim 1, wherein the D(A) / D(B) ratio is 1.2 or more.
7. 7. The powder according to claim 1, wherein the D(A) / D(B) ratio is 150 or less.
8. 8. The powder according to claim 1, wherein the D(A) / D(B) is 60 or less.
9. The powder according to any one of claims 1 to 8, characterized in that, when the thermal conductivity of the first inorganic compound is K(A) and the thermal conductivity of the second inorganic compound is K(B), K(A) / K(B) is 2.0 or more and 50.0 or less.
10. The powder according to claim 1 , wherein the particles B contain the second inorganic compound which is amorphous.
11. 11. Powder according to claim 1, characterized in that the first inorganic compound is a metal oxide and / or a semi-metal oxide and the second inorganic compound is a metal oxide and / or a semi-metal oxide.
12. The powder according to claim 1 , wherein the particles A contain a composition that forms a eutectic with a composition constituting the particles B.
13. 13. The powder according to claim 1, wherein the melting point of said particles B is lower than the melting point of said particles A.
14. The powder according to claim 1 , wherein the W(B) is 10.0% by weight or more and 90.0% by weight or less.
15. The powder according to claim 1 , comprising absorber particles that exhibit a higher absorption ability than the particles A and the particles B with respect to light irradiated to the powder.
16. The powder according to claim 15 , wherein the absorber particles contain the same element as the metalloid element or metal element contained in the particles A or B.
17. 17. The powder according to claim 15 or 16, wherein the absorber particles have an absorptivity for the light of 10% or more.
18. 18. The powder according to any one of claims 15 to 17, characterized in that the absorber particles comprise at least one selected from the group consisting of SiO, TiO, Ti2O3, ZnO, antimony doped tin oxide (ATO), indium doped tin oxide (ITO), MnO, MnO2, Mn2O3, Mn3O4, FeO, Fe2O3, Fe3O4, Cu2O, CuO, Cr2O3, CrO3, NiO, VO3, VO2, VO5, VO4, Co3O4, CoO, Tb4O7, Pr6O11, ZrN, ZrC, ZrSi, and AlN.
19. 18. The powder according to claim 15, wherein the absorber particles comprise SiO.
20. The powder according to any one of claims 1 to 19, characterized in that the melting point of said particle B is 1900°C or less.
21. 21. The powder according to claim 1, wherein the particles A comprise aluminum oxide and the particles B comprise silicon dioxide.
22. 22. A powder according to any one of the preceding claims, characterized in that W(A) is greater than W(B).
23. A method for producing a ceramic structure, comprising the steps of: forming the ceramic structure by a powder bed fusion process using the powder according to any one of claims 1 to 22.
24. A method for producing a ceramic structure, comprising shaping the powder according to any one of claims 1 to 22 by heating it with laser light.