Polyimide resin
Patent Information
- Application Number
- JP2022186762
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2022-11-22
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-11-26
AI Technical Summary
Conventional polyimide materials used in flexible printed circuit boards cause significant transmission loss and signal delay when transmitting high-frequency signals, particularly in 5G communications, due to high dielectric loss tangent and dielectric constant.
A polyimide resin formulation containing specific structural units derived from tetracarboxylic anhydrides and diamines, including ester bond-containing and biphenyl skeleton-containing units, with optimized content ratios to achieve low dielectric loss tangent and dielectric constant, resulting in a polyimide film with improved high-frequency characteristics.
The polyimide film exhibits low dielectric loss tangent of less than 0.004 at 10 GHz, reducing transmission loss and enabling high-frequency applications with excellent signal integrity.
Smart Images

Figure 2023079194000001 
Figure 2023079194000002 
Figure 2023079194000003
Abstract
Description
[Technical Field]
[0001] The present invention relates to a polyimide resin capable of forming a polyimide film that can be used as a substrate material for high-frequency band printed circuit boards and antenna boards, a polyimide film, a method for manufacturing the same, and a laminated film and a flexible printed circuit board containing the polyimide film. [Background technology]
[0002] Flexible printed circuit boards (hereinafter sometimes referred to as FPCs) are thin, lightweight, and flexible, enabling three-dimensional, high-density mounting. They are used in many electronic devices such as mobile phones and hard drives, contributing to their miniaturization and weight reduction. Conventionally, polyimide resin, which has excellent heat resistance, mechanical properties, and electrical insulation properties, has been widely used for FPCs. For example, copper-clad laminates (hereinafter sometimes abbreviated as CCLs) used in FPCs are known to be laminates having copper foil layers on one or both sides of a single or multi-layer polyimide film. In recent years, the fifth-generation mobile communication system, known as 5G, has been steadily gaining popularity (see, for example, Patent Document 1).
[0003] [Patent Document 1] Japanese Patent Publication No. 2021-161285 [Overview of the project] [Problems that the invention aims to solve]
[0004] However, conventionally used polyimide materials suffer from significant transmission loss when transmitting high-frequency signals used in 5G communication, resulting in drawbacks such as electrical signal loss and long signal delays. Therefore, polyimide films with low dielectric loss tangent (hereinafter sometimes referred to as Df) and relative permittivity (hereinafter sometimes referred to as Dk) are being investigated to reduce transmission loss, but polyimide films with sufficiently low relative permittivity and dielectric loss tangent have not yet been found.
[0005] Therefore, the object of the present invention is to provide a polyimide resin capable of forming a polyimide film with low Df that can form a CCL with low transmission loss in the high frequency band, a polyimide film, a method for manufacturing the same, and a laminated film and a flexible printed circuit board containing the polyimide film. [Means for solving the problem]
[0006] The present inventors, after diligent research to solve the above problems, arrived at the present invention. That is, the present invention provides the following preferred embodiments.
[0007] [1] A polyimide resin containing a constituent unit (A) derived from tetracarboxylic anhydride and a constituent unit (B) derived from diamine, The constituent unit (A) derived from tetracarboxylic anhydride includes a constituent unit (A1) derived from ester bond-containing tetracarboxylic anhydride and a constituent unit (A2) derived from biphenyl skeleton-containing tetracarboxylic anhydride. The diamine-derived structural unit (B) includes the biphenyl skeleton-containing diamine-derived structural unit (B1). The content of the aforementioned constituent unit (A1) is 15 to 75 mol% relative to the total amount of the aforementioned constituent unit (A). The content of the aforementioned constituent unit (A2) is 25 to 85 mol% relative to the total amount of the aforementioned constituent unit (A). The total content of the constituent unit (A1) and the constituent unit (A2) is 60 mol% or more relative to the total amount of the constituent unit (A). A polyimide resin in which the content of the aforementioned constituent unit (B1) exceeds 30 mol% relative to the total amount of the aforementioned constituent unit (B). [2] The constituent unit (A1) is given by formula (a1): [ka] [In formula (a1), Z represents a divalent organic group, R a1 These independently represent a halogen atom, an alkyl group which may have a halogen atom, an alkoxy group, an aryl group, or an aryloxy group. [s represents integers from 0 to 3, independently of each other.] The polyimide resin according to claim 1, wherein the constituent unit (a1) is derived from a tetracarboxylic anhydride represented by . [3] The constituent unit (A2) is given by formula (a2): [ka] [In formula (a2), R a2 These independently represent a halogen atom, an alkyl group which may have a halogen atom, an alkoxy group, an aryl group, or an aryloxy group. [t represents integers from 0 to 3, independently of each other.] A polyimide resin according to [1] or [2], wherein the constituent unit (a2) is derived from a tetracarboxylic anhydride represented by [1] or [2]. [4] The constituent unit (B1) is given by formula (b1): [ka] [In formula (b1), R b1 These independently represent a halogen atom, an alkyl group which may have a halogen atom, an alkoxy group, an aryl group, or an aryloxy group. [p represents an integer between 0 and 4] A polyimide resin according to any of [1] to [3], wherein the constituent unit (b1) is derived from a diamine represented by [1]. [5] The constituent unit (B) is given by formula (b2): [ka] [In formula (b2), R b2 R independently represents a halogen atom, an alkyl group which may have a halogen atom, an alkoxy group, an aryl group, or an aryloxy group, b2 The hydrogen atoms contained therein may be independently substituted by halogen atoms. W is independent of each other and is -O-, -CH2-, -CH2-CH2-, -CH(CH3)-, -C(CH3)2-, -C(CF3)2-, -COO-, -OOC-, -SO2-, -S-, -CO-, or -N(Rc )- represents R c This represents a monovalent hydrocarbon group having 1 to 12 carbon atoms, which may be substituted with hydrogen atoms or halogen atoms. m represents an integer from 0 to 4. [q represents an integer between 0 and 4, independently of each other.] A polyimide resin according to any one of [1] to [4], comprising a diamine-derived structural unit (b2) represented by [1]. [6] The polyimide resin according to [5], wherein in the constituent unit (b2), m is 3 and W is independently -O- or -C(CH3)2-. [7] A polyimide resin according to any of [1] to [6], wherein the glass transition temperature is 200 to 290°C. A polyimide film containing a polyimide resin as described in any of [8][1] to [7]. [9] The dielectric loss tangent at 10 GHz is less than 0.004, as described in [8].
[10] A polyimide film according to [8] or [9], having a thickness of 5 to 100 μm. A laminated film comprising a copper foil layer on one or both sides of a polyimide film as described in any of
[11] [8] to
[10] . A flexible printed circuit board containing a polyimide film as described in any of
[12] [8] to
[10] .
[13] A step of coating a polyimide resin precursor solution containing constituent units derived from tetracarboxylic anhydride and constituent units derived from diamine onto a substrate, and A method for producing a polyimide film according to any one of [8] to
[10] , comprising the step of imidizing a polyimide resin precursor by heat treatment at a temperature of 200°C or higher and 500°C or lower. [Effects of the Invention]
[0008] According to the present invention, it is possible to provide a polyimide-based film with low Df that can form a CCL with low transmission loss in the high-frequency band. [Brief explanation of the drawing]
[0009] [Figure 1] Figure 1 is a schematic diagram illustrating the method for determining the in-plane orientation index by transmission X-ray diffraction measurement. [Figure 2] Figure 2 shows the azimuth angle profile obtained by transmission X-ray diffraction measurement of the polyimide film of Example 4. [Figure 3] Figure 3 is a schematic diagram illustrating the method for determining molecular periodicity indices using reflection X-ray diffraction measurements. [Figure 4] Figure 4 shows the diffraction intensity profile obtained by reflection X-ray diffraction measurement of the polyimide film of Example 4. [Figure 5] Figure 5 is a schematic diagram illustrating the method for determining the in-plane anisotropy index by transmission X-ray diffraction measurement. [Figure 6] Figure 6 shows the azimuth angle profile obtained by transmission X-ray diffraction measurement of the polyimide film of Example 4. [Modes for carrying out the invention]
[0010] The embodiments of the present invention will be described in detail below. However, the scope of the present invention is not limited to the embodiments described herein, and various modifications can be made without departing from the spirit of the invention.
[0011] [Polyimide resin] The polyimide resin of the present invention contains a constituent unit (A) derived from tetracarboxylic anhydride (hereinafter sometimes simply referred to as constituent unit (A)) and a constituent unit (B) derived from diamine (hereinafter sometimes simply referred to as constituent unit (B)), wherein constituent unit (A) contains a constituent unit (A1) derived from ester group-containing tetracarboxylic anhydride (hereinafter sometimes simply referred to as constituent unit (A1)) and a constituent unit (A2) derived from biphenyl skeleton-containing tetracarboxylic anhydride (hereinafter sometimes simply referred to as constituent unit (A2)), and the constituent unit (B) derived from diamine is The material contains a component unit (B1) derived from a biphenyl skeleton-containing diamine (hereinafter sometimes simply referred to as component unit (B1)), wherein the content of component unit (A1) is 15 to 75 mol% of the total amount of component unit (A), the content of component unit (A2) is 25 to 85 mol% of the total amount of component unit (A), the combined content of component unit (A1) and component unit (A2) is 60 mol% or more of the total amount of component unit (A), and the content of component unit (B1) exceeds 30 mol% of the total amount of component unit (B). In this specification, polyimide may be abbreviated as PI. In the present invention, "derived constituent unit" means "derived constituent unit," and for example, "tetracarboxylic anhydride-derived constituent unit (A)" means "constituent unit (A) derived from tetracarboxylic anhydride."
[0012] The inventors have found that in a PI-based resin, a PI-based film with a low Df can be obtained when the content of constituent unit (A1) is 15 to 75 mol%, the content of constituent unit (A2) is 25 to 85 mol%, the total content of constituent unit (A1) and constituent unit (A2) is 60 mol% or more, and the content of constituent unit (B1) is more than 30 mol%. This is presumed to be because when the content of constituent unit (A1), constituent unit (A2), and constituent unit (B1) is within the above range, the PI-based resin is more likely to form a higher-order structure in which molecular rotation is suppressed, and the imide group concentration tends to decrease, which improves the moisture resistance of the PI-based resin, and as a result the Df of the resulting PI-based film tends to decrease.
[0013] On the other hand, if at least one of the constituent units (A1), (A2), their total amount, and the content of constituent unit (B1) is outside the above range, the Df of the resulting PI-based film tends to be higher.
[0014] <Constituent unit (A) derived from tetracarboxylic anhydride> The PI-based resin of the present invention contains a constituent unit (A) derived from tetracarboxylic anhydride.
[0015] (Constituent unit (A1) derived from ester group-containing tetracarboxylic anhydride) The constituent unit (A) includes the constituent unit (A1) derived from an ester group-containing tetracarboxylic anhydride. When the constituent unit (A) includes the constituent unit (A1), ester bonds having molecular orientation properties are incorporated into the PI-based resin, making orientation easier and reducing the Df of the resulting PI-based film. It also makes it easier to reduce the coefficient of linear expansion (hereinafter sometimes referred to as CTE) and improve the dimensional stability of the PI-based film. Furthermore, even at low temperatures such as 350°C or below, the Df tends to be low, so even when the CCL is produced by thermal imidizing a PI-based resin precursor coating film in a laminated configuration with copper foil, it is easier to suppress the degradation of the copper foil surface and obtain a CCL with excellent high-frequency characteristics.
[0016] In one embodiment of the present invention, the constituent unit (A1) is not particularly limited as long as it contains an ester bond, and the constituent unit (A1) may contain one or two or more ester bonds. However, from the viewpoint of easily reducing the Df of the resulting PI-based film, formula (a1): [ka] [In formula (a1), Z represents a divalent organic group, R a1 These independently represent a halogen atom, an alkyl group which may have a halogen atom, an alkoxy group, an aryl group, or an aryloxy group. [s represents integers from 0 to 3, independently of each other.] It is preferably a structural unit (a1) derived from a tetracarboxylic dianhydride represented by
[0017] R in formula (a1) a1 independently of one another represents a halogen atom, an alkyl group which may have a halogen atom, an alkoxy group, an aryl group, or an aryloxy group, and from the viewpoint of easily reducing Df of the obtained PI film, preferably independently of one another represents an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms. Examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, a 2-methyl-butyl group, a 3-methylbutyl group, a 2-ethyl-propyl group, an n-hexyl group and the like. Examples of the alkoxy group having 1 to 6 carbon atoms include a methoxy group, an ethoxy group, a propyloxy group, an isopropyloxy group, an n-butoxy group, an isobutoxy group, a sec-butoxy group, a tert-butoxy group, a pentyloxy group, a hexyloxy group, a cyclohexyloxy group and the like. Examples of the aryl group having 6 to 12 carbon atoms include a phenyl group, a tolyl group, a xylyl group, a naphthyl group, a biphenyl group and the like. R a1 The hydrogen atoms contained in may independently of one another be substituted with a halogen atom, and examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, an iodine atom. Among these, from the viewpoint of easily reducing Df of the PI film, R a1 independently of one another preferably includes an alkyl group having 1 to 6 carbon atoms, and more preferably an alkyl group having 1 to 3 carbon atoms. Also, s in formula (a1) independently of one another represents an integer of 0 to 3, preferably 0 or 1, and more preferably 0.
[0018] In formula (a1), Z represents a divalent organic group, preferably a divalent organic group having 4 to 40 carbon atoms, more preferably a divalent organic group having 4 to 40 carbon atoms having a cyclic structure, and even more preferably a divalent organic group having 4 to 40 carbon atoms having an aromatic ring. Among these, from the viewpoint of easily reducing the Df of the resulting PI-based film, Z is represented by formulas (z1), (z2), and (z3): [ka] [In formulas (z1) to (z3), R z11 ~R z14 These represent monovalent hydrocarbon groups that may independently contain a hydrogen atom or a halogen atom. R z2 These independently represent monovalent hydrocarbon groups that may have a halogen atom. n represents an integer from 1 to 4. j represents an integer between 0 and 3, independently of each other. * represents a combination. It is preferable that the divalent organic group is represented by formula (z1), and more preferably that the divalent organic group is represented by formula (z1).
[0019] In one embodiment of the present invention, R in equation (z1) z11 ~R z14 Each of these independently represents a monovalent hydrocarbon group which may have a hydrogen atom or a halogen atom. Examples of monovalent hydrocarbon groups include aromatic hydrocarbon groups, alicyclic hydrocarbon groups, and aliphatic hydrocarbon groups. Examples of aromatic hydrocarbon groups include phenyl groups, tolyl groups, xylyl groups, naphthyl groups, and aryl groups such as biphenyl groups. Examples of alicyclic hydrocarbon groups include cyclopentyl groups, cyclohexyl groups, and other cycloalkyl groups. Examples of aliphatic hydrocarbon groups include alkyl groups such as methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, sec-butyl group, tert-butyl group, n-pentyl group, 2-methyl-butyl group, 3-methylbutyl group, 2-ethyl-propyl group, n-hexyl group, n-heptyl group, n-octyl group, tert-octyl group, n-nonyl group, and n-decyl group. R z11 ~R z14 From the viewpoint of easily reducing the Df of PI-based films, each element independently preferably represents an alkyl group which may have a hydrogen atom or a halogen atom, more preferably 1 to 6 alkyl groups which may have a hydrogen atom or a halogen atom, even more preferably 1 to 3 alkyl groups which may have a hydrogen atom or a halogen atom, and particularly preferably a hydrogen atom.
[0020] In one embodiment of the present invention, R in equation (z2) z2 R independently represents a monovalent hydrocarbon group which may have a halogen atom, and examples of monovalent hydrocarbon groups include those listed above. z2 From the viewpoint of easily improving the mechanical and thermal properties of PI-based films, these terms independently preferably represent an alkyl group which may have a halogen atom, more preferably an alkyl group having 1 to 6 carbon atoms which may have a halogen atom, and even more preferably an alkyl group having 1 to 3 carbon atoms which may have a halogen atom. In this specification, mechanical properties refer to mechanical properties including flexural resistance, bending resistance, and elastic modulus, and improved mechanical properties refer to, for example, increased flexural resistance and / or increased elastic modulus. Thermal properties refer to thermal properties including glass transition temperature (hereinafter sometimes referred to as Tg), CTE, low thermal deformation and degradation, and low deformation after heating, and improved thermal properties refer to, for example, increased Tg and / or decreased CTE.
[0021] In one embodiment of the present invention, from the viewpoint of easily reducing the Df of the PI-based film and easily improving bending resistance, R in formula (z1) z11 ~R z14 In a benzene ring having Rz11 ~R z14 At least one of them may be a monovalent hydrocarbon group having a halogen atom, but R z11 ~R z14 It is preferable that all of them are hydrogen atoms.
[0022] In formula (z2), j represents 0 to 3 independently of each other. In one embodiment of the present invention, from the viewpoint of easily reducing the Df of the PI-based film, j is preferably 0 or 1, more preferably 0, and even more preferably all j are 0.
[0023] In formula (z1), n represents an integer from 1 to 4, and from the viewpoint of easily reducing the Df of the PI-based film, it preferably represents an integer from 1 to 3, more preferably 1 or 2, and particularly preferably 2.
[0024] In one preferred embodiment of the present invention, formula (a1) is formula (a1') or formula (a1"): [ka] It is preferable that the PI resin is represented by the formula (a1), particularly formula (a1') or formula (a1"), as a constituent unit (A1). When the PI resin contains a constituent unit derived from a tetracarboxylic anhydride represented by formula (a1), particularly formula (a1') or formula (a1"), the Df of the resulting PI film is easily reduced. Furthermore, even at low temperatures such as 350°C or below, the Df tends to be low, so even when the CCL is produced by thermal imidizing a PI resin precursor coating film in a laminated configuration with copper foil, the deterioration of the copper foil surface is easily suppressed, and a CCL with excellent high-frequency characteristics is easily obtained.
[0025] In the PI resin of the present invention, the content of constituent unit (A1) is 15 mol% or more, preferably 20 mol% or more, more preferably 27 mol% or more, even more preferably 30 mol% or more, even more preferably 35 mol% or more, particularly preferably 40 mol% or more, particularly more preferably 45 mol% or more, and 75 mol% or less, preferably 70 mol% or less, more preferably 65 mol% or less, and even more preferably 60 mol% or less, based on the total amount of constituent unit (A). When the content of constituent unit (A1) is within the above range, orientation of the PI resin is likely to occur, the Df of the resulting PI film is likely to be reduced, and the bending resistance is likely to be improved. The proportion of the constituent unit is, for example, 1 It can be measured using 1H-NMR, or it can be calculated from the raw material charging ratio.
[0026] (Constituent unit (A2) derived from biphenyl skeleton-containing tetracarboxylic anhydride) The constituent unit (A) includes the constituent unit (A2) derived from a biphenyl skeleton-containing tetracarboxylic anhydride. When constituent unit (A) includes the aforementioned constituent unit (A2), the Df of the PI-based film is easily reduced.
[0027] In one embodiment of the present invention, the constituent unit (A2) is not particularly limited as long as it contains a biphenyl skeleton, and the constituent unit (A2) may contain one or more biphenyl skeletons. Furthermore, in one embodiment of the present invention, it is preferable that the constituent unit (A2) contains a biphenyl skeleton but does not contain an ester bond, and in this specification, a constituent unit derived from a tetracarboxylic anhydride that contains both an ester bond and a biphenyl skeleton is classified not as constituent unit (A2) but as a constituent unit (A1) derived from an ester bond-containing tetracarboxylic anhydride.
[0028] In one embodiment of the present invention, the constituent unit (A2) is given by formula (a2): [ka] [In formula (a2), R a2These independently represent a halogen atom, an alkyl group which may have a halogen atom, an alkoxy group, an aryl group, or an aryloxy group. [t represents integers from 0 to 3, independently of each other.] It is preferable that the constituent unit (a2) is derived from a tetracarboxylic anhydride represented by .
[0029] R in equation (a2) a2 Each of these independently represents a halogen atom, an alkyl group which may have a halogen atom, an alkoxy group, an aryl group, or an aryloxy group. From the viewpoint of easily reducing the Df of the resulting PI-based film and easily improving its bending resistance, each of these preferably independently represents a C1-C6 alkyl group, a C1-C6 alkoxy group, or a C6-C12 aryl group. Examples of C1-C6 alkyl groups, C1-C6 alkoxy groups, and C6-C12 aryl groups are those exemplified above. a2 The hydrogen atoms contained in may be independently substituted with halogen atoms, and examples of halogen atoms are those listed above. Among these, R is selected from the viewpoint of easily reducing the Df of the resulting PI-based film and easily improving its bending resistance. a2 These are, independently of each other, preferably alkyl groups having 1 to 6 carbon atoms, and more preferably alkyl groups having 1 to 3 carbon atoms.
[0030] The bonding positions of the two carboxylic acid anhydrides bonded to the benzene ring constituting the biphenyl skeleton in formula (a2) are not particularly limited, and may be 3,4- or 2,3- independently of each other, based on the single bond connecting the two benzene rings. From the viewpoint of easily reducing the Df of the resulting PI-based film and easily improving its flexural resistance, it is preferable that it be 3,4-. t represents an integer from 0 to 3 independently of each other, and from the viewpoint of easily reducing the Df of the resulting PI-based film and easily improving its flexural resistance, it is preferably an integer from 0 to 2, more preferably 0 or 1.
[0031] In a preferred embodiment of the present invention, formula (a2) is formula (a2'): [ka] It is preferable that it be represented as such. When the PI resin contains a constituent unit derived from a tetracarboxylic anhydride represented by formula (a2), particularly formula (a2'), as a constituent unit (A2), the Df of the resulting PI film is easily reduced and the bending resistance is easily improved. Furthermore, even at low temperatures such as 350°C or below, the Df tends to be low, so even when the CCL is produced by thermal imidizing a PI resin precursor coating film in a laminated configuration with copper foil, the deterioration of the copper foil surface is easily suppressed, and a CCL with excellent high-frequency characteristics is easily obtained.
[0032] In the present invention, the content of constituent unit (A2) is 25 mol% or more, preferably 30 mol% or more, more preferably 35 mol% or more, even more preferably 40 mol% or more, even more preferably 45 mol% or more, and 85 mol% or less, preferably 80 mol% or less, more preferably 75 mol% or less, even more preferably 70 mol% or less, and even more preferably 65 mol% or less, based on the total amount of constituent unit (A). When the content of constituent unit (A2) is within the above range, orientation of the PI resin is likely to occur, and therefore the Df of the PI film is likely to be reduced. The proportion of the constituent units is, for example, 1 It can be measured using 1H-NMR, or it can be calculated from the raw material charging ratio.
[0033] In the PI resin of the present invention, the total content of constituent unit (A1) and constituent unit (A2) is 60 mol% or more, preferably 70 mol% or more, more preferably 80 mol% or more, even more preferably 90 mol% or more, even more preferably 95 mol% or more, and preferably 100 mol% or less, relative to the total amount of constituent unit (A). When the total content of constituent unit (A1) and constituent unit (A2) is within the above range, orientation of the PI resin is likely to occur, and the Df of the PI film is easily reduced.
[0034] (Component unit (A3)) In one embodiment of the present invention, the constituent unit (A) may include constituent units (A3) derived from tetracarboxylic anhydride other than constituent units (A1) and (A2).
[0035] In one embodiment of the present invention, the constituent unit (A3) is a constituent unit derived from a tetracarboxylic anhydride that does not contain either an ester bond or a biphenyl skeleton, for example, formula (1): [ka] [In equation (1), Y is given by equations (31) to (38): [ka] [In formulas (31) to (38), R 19 ~R 26 and R 23’ ~R 26’ Each of these independently represents a hydrogen atom, a C1-C6 alkyl group, a C1-C6 alkoxy group, or a C6-C12 aryl group, and R 19 ~R 26 and R 23’ ~R 26’ The hydrogen atoms contained therein may be independently substituted by halogen atoms. V 1 and V 2 These are independent of each other, single bonds (except when e+d=1), -O-, -CH2-, -CH2-CH2-, -CH(CH3)-, -C(CH3)2-, -C(CF3)2-, -SO2-, -S-, -CO-, -N(R j )-, formula (a) [ka] (In formula (a), R 27 ~R 30 Each of these independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. D independently represents a single bond, -C(CH3)2-, or -C(CF3)2. i represents an integer from 1 to 3. * represents a bond. R j This represents a monovalent hydrocarbon group having 1 to 12 carbon atoms, which may be substituted with a hydrogen atom or a halogen atom. e and d represent integers between 0 and 2, independently of each other (where e + d is not 0). f represents an integer between 0 and 3. g and h represent integers between 0 and 4, independently of each other. * indicates a bond. [Represents a tetravalent organic group represented by ] Examples of constituent units derived from tetracarboxylic anhydrides are shown.
[0036] In equations (31) to (33), R 19 ~R 26 and R 23’ ~R 26’ Each of these independently represents a hydrogen atom, a C1-C6 alkyl group, a C1-C6 alkoxy group, or a C6-C12 aryl group. Examples of alkyl groups having 1 to 6 carbon atoms, alkoxy groups having 1 to 6 carbon atoms, and aryl groups having 6 to 12 carbon atoms include those exemplified above. 19 ~R 26 and R 23’ ~R 26’ The hydrogen atoms contained therein may be independently substituted with halogen atoms, and examples of such halogen atoms include those exemplified above. Among these, R is preferred from the viewpoint of easily improving the mechanical and thermal properties of the PI film. 19 ~R 26 and R 23’ ~R 26’ Each of these is independently preferably a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, more preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and even more preferably a hydrogen atom.
[0037] In equation (31), V 1 and V 2 These are independent of each other, single bonds (except when e+d=1), -O-, -CH2-, -CH2-CH2-, -CH(CH3)-, -C(CH3)2-, -C(CF3)2-, -SO2-, -S-, -CO-, -N(R j)- or formula (a) represents, and from the viewpoint of easily improving the mechanical and thermal properties of PI-based films, preferably a single bond (except when e+d=1), -O-, -CH2-, -C(CH3)2-, -C(CF3)2-, or -CO-, and more preferably a single bond (except when e+d=1), -O-, -C(CH3)2-, or -C(CF3)2-. j represents a monovalent hydrocarbon group having 1 to 12 carbon atoms, which may be substituted with hydrogen atoms or halogen atoms. Examples of monovalent hydrocarbon groups having 1 to 12 carbon atoms include methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, isobutyl group, sec-butyl group, tert-butyl group, n-pentyl group, 2-methyl-butyl group, 3-methylbutyl group, 2-ethyl-propyl group, n-hexyl group, n-heptyl group, n-octyl group, tert-octyl group, n-nonyl group, and n-decyl group, which may be substituted with halogen atoms. Examples of halogen atoms are the same as those listed above.
[0038] In formula (31), e and d independently represent integers between 0 and 2 (wherein e + d is not 0), and preferably represent 0 or 1 from the viewpoint of easily reducing the Df of the PI-based film. Also, e + d preferably represents 1.
[0039] In formulas (32) and (33), f represents an integer between 0 and 3, and from the viewpoint of easily reducing the Df of the PI-based film, it preferably represents 0 or 1, more preferably 0.
[0040] In formula (33), g and h represent integers between 0 and 4, independently of each other, and preferably represent integers between 0 and 2, more preferably 0 or 1, from the viewpoint of easily improving the mechanical and thermal properties of the PI-based film. Also, g + h preferably represents an integer between 0 and 2. When f is 1 or greater, multiple g and h may be the same or different, independently of each other.
[0041] In equation (a), R 27 ~R 30Each of these independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. Examples of alkyl groups having 1 to 6 carbon atoms include those exemplified above. Among these, R is selected from the viewpoint of easily improving the mechanical and thermal properties of PI-based films. 27 ~R 30 Each of these elements independently represents, preferably, a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and more preferably, a hydrogen atom.
[0042] In formula (a), D represents a single bond, -C(CH3)2-, or -C(CF3)2. Having such a structure for D makes it easier to improve the mechanical and thermal properties of the PI-based film. i represents an integer from 1 to 3, and is preferably 1 or 2 from the viewpoint of easily improving the mechanical and thermal properties of the PI-based film. If i is 2 or greater, multiple Z and R are present. 27 ~R 30 These elements may be identical or different, and may be independent of each other.
[0043] Among these, from the viewpoint of easily reducing the Df of the resulting PI-based film and easily improving its bending resistance, it is preferable that Y in formula (1) is from formulas (42) to (49) or formula (53): [ka] The constituent units are derived from tetracarboxylic anhydrides represented by formula (1), more preferably Y in formula (1) is a constituent unit derived from tetracarboxylic anhydrides represented by formula (42), formula (46), formula (49), or formula (53). Note that * in the formula represents a bond.
[0044] <Diamine-derived structural unit (B)> The PI-based resin of the present invention contains a diamine-derived structural unit (B).
[0045] (Constituent unit (B1) derived from biphenyl skeleton-containing diamine) The constituent unit (B) includes the constituent unit (B1) derived from a biphenyl skeleton-containing diamine. When the constituent unit (B) includes the constituent unit (B1), the Df of the resulting PI-based film is easily reduced, which in turn makes it easier to reduce the transmission loss of an electrical circuit made of the PI-based film. Furthermore, when the constituent unit (B) includes the constituent unit (B1), the bending resistance of the resulting PI-based film is easily improved.
[0046] In one embodiment of the present invention, the constituent unit (B1) is not particularly limited as long as it contains a biphenyl skeleton, and the constituent unit (B1) may contain one or more biphenyl skeletons. In one embodiment of the present invention, from the viewpoint of easily reducing the Df of the resulting PI-based film and easily improving the bending resistance, the constituent unit (B1) is given by formula (b1): [ka] [In formula (b1), R b1 These independently represent a halogen atom, an alkyl group which may have a halogen atom, an alkoxy group, an aryl group, or an aryloxy group. [p represents an integer between 0 and 4] It is preferable that the constituent unit (b1) is derived from a diamine represented by .
[0047] In equation (b1), R b1 Each of these independently represents a halogen atom, an alkyl group which may have a halogen atom, an alkoxy group which may have a halogen atom, an aryl group which may have a halogen atom, preferably a halogen atom, an alkyl group which may have a halogen atom, an alkoxy group which may have a halogen atom, more preferably a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group which has 1 to 6 carbon atoms, or an aryl group which has 6 to 12 carbon atoms. Examples of alkyl groups having 1 to 6 carbon atoms, alkoxy groups which have 1 to 6 carbon atoms, and aryl groups which have 6 to 12 carbon atoms are those exemplified above. b1The hydrogen atoms contained therein may be independently substituted with halogen atoms, and examples of such halogen atoms include fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms. From the viewpoint of easily reducing the Df of the resulting PI-based film and easily improving bending resistance and dimensional stability, R b1 These are preferably, independently of each other, an alkyl group having 1 to 6 carbon atoms or a fluorinated alkyl group having 1 to 6 carbon atoms. From the viewpoint of easily improving adhesion to substrates such as copper foil, it is more preferably an alkyl group having 1 to 6 carbon atoms that does not contain fluorine, even more preferably an alkyl group having 1 to 3 carbon atoms that does not contain fluorine, and particularly preferably a methyl group.
[0048] In formula (b1), p represents an integer between 0 and 4, independently of each other. From the viewpoint of easily reducing the Df of the PI-based film and easily improving bending resistance and dimensional stability, p is preferably an integer between 0 and 2, more preferably 0 or 1.
[0049] In formula (b1), the -NH2 group bonded to each benzene ring may be bonded to the ortho, meta, or para position, or to the α, β, or γ position, relative to the single bond connecting each benzene ring. From the viewpoint of easily reducing the Df of the PI-based film and easily improving dimensional stability, it is preferable that the bond be to the meta or para position, or to the β or γ position, more preferably to the para or γ position.
[0050] In a preferred embodiment of the present invention, formula (b1) is formula (b1'): [ka] It is preferable that it be represented as such. When the PI resin contains a diamine-derived structural unit represented by formula (b1), particularly formula (b1'), as a structural unit (B1), the Df of the resulting PI film is easily reduced, and the bending resistance is easily improved. Furthermore, even at low temperatures such as 350°C or below, the Df tends to be low, so even when the CCL is produced by thermal imidizing a PI resin precursor coating film in a laminated configuration with copper foil, the deterioration of the copper foil surface is easily suppressed, and a CCL with excellent high-frequency characteristics is easily obtained.
[0051] The content of constituent unit (B1), preferably constituent unit (b1), is greater than 30 mol%, preferably 35 mol% or more, more preferably 40 mol% or more, even more preferably 50 mol% or more, particularly preferably 60 mol% or more, particularly more preferably 70 mol% or more, extremely preferably 80 mol% or more, and extremely preferably 90 mol% or more, relative to the total amount of constituent unit (B). Furthermore, there is no particular upper limit to the content of constituent unit (B1), preferably constituent unit (b1), and it may be 100 mol% or less relative to the total amount of constituent unit (B). When the content of constituent unit (B1), preferably constituent unit (b1), is within the above range, it is easier to reduce the Df of the resulting PI-based film and to improve its bending resistance. The proportion of the constituent units is, for example, 1 It can be measured using 1H-NMR, or it can be calculated from the raw material charging ratio.
[0052] (Component unit (B2)) In one embodiment of the present invention, it is preferable that the constituent unit (B) includes a diamine-derived constituent unit (B2) (hereinafter sometimes simply referred to as constituent unit (B2)) having two or more aromatic rings, each aromatic ring being bonded via a divalent organic group. The divalent organic group in constituent unit (B) may be, for example, an alkylene group which may have a halogen atom, -O-, -COO-, -OOC-, -SO2-, -S-, -CO- or -N(R c )- and others are examples, R c-V(C1-C2-) represents a monovalent hydrocarbon group having 1 to 12 carbon atoms, which may be substituted with hydrogen or halogen atoms. Among these, the divalent organic groups in the constituent unit (B) are -O-, -CH2-, -CH2-CH2-, -CH(CH3)-, -C(CH3)2-, -C(CF3)2-, -COO-, -OOC-, -SO2-, -S-, -CO-, or -N(R2-C c )- is preferable.
[0053] The constituent unit (B2) is given by formula (b2): [ka] [In formula (b2), R b2 These independently represent a halogen atom, an alkyl group which may have a halogen atom, an alkoxy group, an aryl group, or an aryloxy group. W is independent of each other and is -O-, -CH2-, -CH2-CH2-, -CH(CH3)-, -C(CH3)2-, -C(CF3)2-, -COO-, -OOC-, -SO2-, -S-, -CO-, or -N(R c )- represents R c This represents a monovalent hydrocarbon group having 1 to 12 carbon atoms, which may be substituted with hydrogen atoms or halogen atoms. m represents an integer from 1 to 4. [q represents an integer between 0 and 4, independently of each other.] The diamine-derived constituent unit (b2) represented by (hereinafter sometimes simply referred to as constituent unit (b2)), formula (2): [ka] [In equation (2), X is given by equation (65): [ka] (In formula (65), * represents a bond) This represents a divalent organic group. Examples include diamine-derived structural units represented by . Among these, structural unit (B2) is preferably structural unit (b2) from the viewpoint of easily reducing the Df of the resulting PI-based film and easily improving its bending resistance. When structural unit (B) includes structural unit (B2), particularly structural unit (b2), the Df of the resulting PI-based film is easily reduced, as a result, the transmission loss of the electronic circuit containing the resulting PI-based film is easily reduced, and the bending resistance of the resulting PI-based film is easily improved.
[0054] In equation (b2), R b2 Each of these independently represents a halogen atom, an alkyl group which may have a halogen atom, an alkoxy group which may have a halogen atom, an aryl group which may have an aryloxy group which may have a halogen atom, preferably a halogen atom which has a C1-C6 alkyl group which has a C1-C6 alkoxy group which has a C1-C6 alkoxy group which has a C1-C6 aryl group which has a C6-C12 aryl group which has a C6-C12 aryl group which may have a C1-C6 alkyl group which has a C1-C6 alkoxy group which has a C1-C6 alkoxy group which has a C6-C12 aryl group which may have a C6-C12 aryl group which may have a C6-C12 aryl group which may have a C1-C6 alkoxy group which has1-C6 aryl group which may have a C6-C12 aryl group which may have a C1-C6 alkoxy group which has a C1-C6 aryl group which may have a C1-C6 alkoxy group which has a C1-C6 aryl group which may have a C1-C6 alkoxy group which has a C1-C6 aryl group which may have a C1-C6 alkoxy group which has a C1-C6 alkoxy group which has a C1-C6 aryl group which has a C1-C12 aryl group which may have a C1-C12 alkoxy group which may have a C1-C12 aryl group which may have a C1 b2 The hydrogen atoms contained therein may be independently substituted with halogen atoms, and examples of such halogen atoms are the same as those described above. From the viewpoint of easily reducing the Df of the resulting PI-based film and easily improving bending resistance and dimensional stability, R b2 These are preferably, independently of each other, an alkyl group having 1 to 6 carbon atoms or a fluorinated alkyl group having 1 to 6 carbon atoms. From the viewpoint of easily improving adhesion to substrates such as copper foil, it is more preferably an alkyl group having 1 to 6 carbon atoms that does not contain fluorine, even more preferably an alkyl group having 1 to 3 carbon atoms that does not contain fluorine, and particularly preferably a methyl group.
[0055] In formula (b2), q represents an integer between 0 and 4, independently of each other. From the viewpoint of easily reducing the Df of the resulting PI-based film and easily improving bending resistance and dimensional stability, it is preferably an integer between 0 and 2, more preferably 0 or 1.
[0056] In equation (b2), W is independently of each other -O-, -CH2-, -CH2-CH2-, -CH(CH3)-, -C(CH3)2-, -C(CF3)2-, -COO-, -OOC-, -SO2-, -S-, -CO-, or -N(R c From the viewpoint of easily reducing the Df of the resulting PI-based film and easily improving bending resistance and dimensional stability, it is preferable to represent -O-, -CH2-, -C(CH3)2-, -C(CF3)2-, -COO-, -OOC- or -CO-, and from the viewpoint of easily improving adhesion to substrates such as copper foil, it is more preferable to represent -O-, -CH2- or -C(CH3)2-, and even more preferably -O- or -C(CH3)2-. c This represents a monovalent hydrocarbon group having 1 to 12 carbon atoms, which may be substituted with hydrogen atoms or halogen atoms. Examples of monovalent hydrocarbon groups having 1 to 12 carbon atoms are those exemplified above, which may be substituted with halogen atoms. Examples of halogen atoms are the same as those exemplified above.
[0057] In formula (b2), m is an integer from 1 to 4, and is preferably an integer from 1 to 3, more preferably 2 or 3, from the viewpoint of easily reducing the Df of the resulting PI-based film and easily improving bending resistance and dimensional stability. When m is 2 or more, multiple W, R b2 , and q may be the same or different from each other, and the positions of -W- relative to -NH2 on each benzene ring may be the same or different.
[0058] In formula (b2), -W- may be bonded to the ortho, meta, or para position, or to the α, β, or γ position, relative to the -NH2 of each benzene ring. From the viewpoint of easily reducing the Df of the resulting PI-based film and easily improving flexural resistance and dimensional stability, it is preferably bonded to the meta or para position, or the β or γ position, more preferably to the para or γ position.
[0059] In one embodiment of the present invention, from the viewpoint of easily reducing the Df of the obtained PI-based film, easily improving bending resistance, and easily improving the adhesion between the obtained PI-based film and copper foil, it is preferable that in formula (b2), m is 3 and W independently represents -O- or -C(CH3)2-, and formula (b2) is formula (b2'): [ka] It is more preferable that it be represented as follows. When the PI resin contains the constituent unit (b2), in particular the diamine-derived constituent unit represented by formula (b2'), it is easier to obtain a PI film with a low Df and excellent adhesion to copper foil. Furthermore, even at low temperatures such as 350°C or below, the Df tends to be low, so even when the CCL is produced by thermal imidizing a PI resin precursor coating film in a laminated configuration with copper foil, it is easier to suppress the deterioration of the copper foil surface and obtain a CCL with excellent high-frequency characteristics.
[0060] In one embodiment of the present invention, the constituent unit (b2) may include, in addition to, a constituent unit derived from a diamine represented by formula (b2'), or in place of said constituent unit, a constituent unit derived from a diamine in formula (b2) where m is 1 and W represents -O-.
[0061] In one embodiment of the present invention, the content of the structural unit (B2) is preferably 0 mol% or more, more preferably 0.3 mol% or more, still more preferably 0.5 mol% or more, even more preferably 0.8 mol% or more, particularly preferably 1 mol% or more, particularly more preferably 5 mol% or more, and extremely preferably 8 mol% or more, based on the total amount of the structural units (B). When the content of the structural unit (B2) is at least the above lower limit, it is easy to improve the adhesion of the obtained PI-based film to a substrate such as a copper foil. Further, the upper limit of the content of the structural unit (B2) is preferably 75 mol% or less, more preferably 60 mol% or less, still more preferably 40 mol% or less, even more preferably 30 mol% or less, particularly preferably 20 mol% or less, based on the total amount of the structural units (B). When the content of the structural unit (B2) is at most the above upper limit, the mechanical properties such as the CTE of the obtained PI-based film tend to be easily improved. The ratio of the above structural units can be measured using, for example 1 H-NMR, or can also be calculated from the charging ratio of the raw materials.
[0062] (Structural unit (B3)) The PI-based resin may contain a structural unit (B3) derived from a diamine other than the structural units (B1) and (B2) (hereinafter, may be simply abbreviated as the structural unit (B3)). Examples of the structural unit (B3) include a structural unit derived from a diamine in which m in the formula (b2) is 0, and X in the formula (2) is the formula (61) to the formula (64): [Chemical formula] [In the formula (61), R a , R b , W, t, u, and n are each independently the same as R a , R b , W, t, u, and n in the formula (60), In the formula (62), ring A represents a cycloalkane ring having 3 to 8 carbon atoms, R d represents an alkyl group having 1 to 20 carbon atoms, r is 0 or more and represents an integer less than or equal to (the number of carbon atoms of ring A - 2), S1 and S2 each independently represent an integer from 0 to 20, In equations (61) to (64), * represents a combination. Examples include diamine-derived structural units represented by [the formula shown].
[0063] R in equation (62) d represents an alkyl group having 1 to 20 carbon atoms, preferably an alkyl group having 1 to 10 carbon atoms, and examples of such alkyl groups include those exemplified above. In formula (62), r is 0 or greater and represents an integer less than or equal to "the number of carbon atoms in ring A minus 2". r is preferably 0 or greater, and preferably 4 or less. In formula (62), S1 and S2 independently represent integers from 0 to 20. S1 and S2 independently are preferably 0 or greater, more preferably 2 or greater, and preferably 15 or less.
[0064] Specific examples of constituent units (B3) include diamine-derived constituent units represented by formulas (71), (74), (77), (78), (89), or (90) in formula (2), where X is (71), (74), (77), (78), (89), or (90). In these formulas, * represents a bond. [ka]
[0065] Among these, it is preferable that X in formula (2) is a constituent unit derived from the diamine represented by formula (74), that is, a constituent unit derived from p-phenylenediamine.
[0066] In one embodiment of the present invention, when constituent unit (B) contains constituent unit (B3), the content of constituent unit (B3) is preferably 25 mol% or less, more preferably 20 mol% or less, even more preferably 10 mol% or less, and preferably 0.01 mol% or more, relative to the total amount of constituent unit (B).
[0067] In one embodiment of the present invention, the PI resin may contain halogen atoms, preferably fluorine atoms, which can be introduced by, for example, the halogen-containing substituents described above. When the PI resin contains fluorine atoms, the dielectric constant of the resulting PI film is easily reduced. Preferred fluorine-containing substituents for incorporating fluorine atoms into the PI resin include, for example, fluoro groups and trifluoromethyl groups. Furthermore, in another embodiment of the present invention, it is preferable that the PI resin does not contain fluorine atoms, from the viewpoint of easily improving the adhesion of the resulting PI film to a substrate such as copper foil. Also, since the presence of fluorine in the PI resin tends to weaken the interactions between molecular chains, the absence of fluorine atoms tends to make the PI resin more likely to adopt a higher-order structure with suppressed molecular rotation. As a result, it is easier to reduce the Df of the PI film of the present invention and improve its bending resistance.
[0068] When a PI-based resin contains halogen atoms, the content of halogen atoms, particularly fluorine atoms, in the PI-based resin is preferably 0.1 to 35% by mass, more preferably 0.1 to 30% by mass, even more preferably 0.1 to 20% by mass, and particularly preferably 0.1 to 10% by mass, based on the mass of the PI-based resin. If the halogen atom content is above the lower limit, it is easier to improve the heat resistance and dielectric properties of the resulting PI-based film. If the halogen atom content is below the upper limit, it is advantageous in terms of cost, makes it easier to reduce the CTE of the PI-based film, and facilitates the synthesis of the PI-based resin. Dielectric properties refer to properties related to dielectric properties, including relative permittivity and dielectric loss tangent, and an increase or improvement in dielectric properties indicates a decrease in relative permittivity and / or dielectric loss tangent.
[0069] In one embodiment of the present invention, the imidation rate of the PI resin is preferably 90% or more, more preferably 93% or more, even more preferably 95% or more, and usually 100% or less. From the viewpoint of easily improving mechanical properties, thermal properties, and dielectric properties, it is preferable that the imidation rate is above the lower limit mentioned above. The imidation rate represents the ratio of the molar amount of imide bonds in the PI resin to twice the molar amount of constituent units derived from the tetracarboxylic acid compound in the PI resin. If the PI resin contains a tricarboxylic acid compound, the imidation rate represents the ratio of the molar amount of imide bonds in the PI resin to the sum of twice the molar amount of constituent units derived from the tetracarboxylic acid compound and the molar amount of constituent units derived from the tricarboxylic acid compound. The imidation rate can be determined by methods such as IR or NMR.
[0070] In one embodiment of the present invention, the weight-average molecular weight of the PI resin on a polystyrene basis (hereinafter, the weight-average molecular weight may be referred to as Mw) is preferably 100,000 or more, more preferably 110,000 or more, even more preferably 120,000 or more, particularly preferably 130,000 or more, preferably 1,000,000 or less, more preferably 700,000 or less, even more preferably 500,000 or less, and particularly preferably 300,000 or less. When Mw is above the lower limit, it is easier to improve mechanical properties such as bending resistance. When Mw is below the upper limit, it is advantageous in terms of processability during film formation.
[0071] In one embodiment of the present invention, the ratio (Mw / Mn) of the Mw of the PI resin to the number average molecular weight (hereinafter, the number average molecular weight may be referred to as Mn) is preferably 4.0 or higher, more preferably 4.2 or higher, even more preferably 4.5 or higher, particularly preferably 4.7 or higher, preferably 8.0 or lower, more preferably 7.0 or lower, even more preferably 6.0 or lower, and particularly preferably 5.5 or lower, on a polystyrene basis. Mw and Mn can be determined by gel permeation chromatography (hereinafter, sometimes referred to as GPC) measurement on a standard polystyrene basis.
[0072] In one embodiment of the present invention, from the viewpoint of easily reducing the Df of the obtained PI-based film and easily improving the bending resistance, the Tg of the PI-based resin is preferably 290 ° C or lower, more preferably less than 290 ° C, still more preferably 280 ° C or lower, even more preferably 275 ° C or lower, particularly preferably 260 ° C or lower, especially preferably 250 ° C or lower, and particularly more preferably 240 ° C or lower. Further, from the viewpoint of easily enhancing the heat resistance of the PI-based film, the Tg of the PI-based resin is preferably 200 ° C or higher, more preferably 202 ° C or higher, and still more preferably 205 ° C or higher. The Tg of the PI-based resin can be measured by dynamic viscoelasticity measurement, and can be measured, for example, by the method described in the examples.
[0073] The Tg of the PI-based resin can be adjusted by appropriately adjusting the types and structures of the constituent units constituting the PI-based resin, as well as the molecular weight and production method of the PI-based resin, particularly the imidization conditions, etc. For example, it can be adjusted within the above range by adjusting within the range described as a preferred embodiment in the above description.
[0074] In one embodiment of the present invention, from the viewpoint of easily reducing the Df of the obtained PI-based film, the E’ of the PI-based resin at 280 ° C is preferably 3×10 8 Pa or less, more preferably 2×10 8 Pa or less, still more preferably 1.5×10 8 Pa or less, even more preferably 1×10 8 Pa or less, particularly preferably 0.8×10 8 Pa or less. Further, from the viewpoint of easily suppressing the deformation during processing of the PI-based film, the E’ of the PI-based resin at 280 ° C is preferably 1×10 4 Pa or more, more preferably 1×10 5 Pa or more, still more preferably 1×10 6 Pa or more. The E’ of the PI-based resin can be measured by dynamic viscoelasticity measurement, and can be measured, for example, by the method described in the examples.
[0075] In one embodiment of the present invention, if the E' and Tg of the PI resin at 280°C are within the above range, the PI resin is more likely to form a desirable higher-order structure in which rotational motion is suppressed. This is presumed to suppress the rotation of polar groups in the PI resin, reducing the loss of electrical energy as thermal motion, and thereby making it easier to reduce the Df of the PI film. Furthermore, polyamic acid, a precursor of PI resin, begins imidation at around 200°C. Generally, polyamic acid has a high degree of freedom in its molecular structure, but after imidation, it becomes relatively rigid and the degree of freedom in its molecular structure decreases. If the Tg of the PI resin is preferably 200-290°C, the thermal imidation temperature exceeds the Tg of the PI resin during the progression of imidation, and the amic acid moiety and imide moiety move simultaneously to form a higher-order structure. This makes it easier to form a desirable higher-order structure in which the rotational motion of the resin as a whole is suppressed. Also, preferably, E' at 280°C is 3 × 10⁻⁶ 8 When the Pa is less than a certain value, the imide moieties can move sufficiently flexibly when forming higher-order structures, making it easier for the resin as a whole to form a desirable higher-order structure with suppressed rotational motion. As a result, even at low temperatures such as 350°C or below, the Df can be kept low. Therefore, even when the CCL is manufactured by thermal imidizing a PI-based resin precursor coating film in a laminated configuration with copper foil, degradation of the copper foil surface can be suppressed, and CCL with excellent high-frequency characteristics can be obtained.
[0076] The E' of the PI resin at 280°C can be adjusted by appropriately adjusting the types and compositions of the constituent units of the PI resin, as well as the molecular weight and manufacturing method of the PI resin, particularly the imidation conditions. For example, it can be adjusted to the range described as a preferred embodiment in the above description.
[0077] [Method for producing polyimide resins] The PI-based resin of the present invention is preferably produced by a method comprising the steps of reacting a tetracarboxylic anhydride with a diamine to obtain a PI-based resin precursor, and imidizing the obtained PI-based resin precursor. In addition to tetracarboxylic acid compounds, dicarboxylic acid compounds and tricarboxylic acid compounds may also be reacted.
[0078] Examples of tetracarboxylic anhydrides used in the synthesis of PI-based resin precursors include aromatic tetracarboxylic acid compounds such as aromatic tetracarboxylic dianhydrides, and aliphatic tetracarboxylic acid compounds such as aliphatic tetracarboxylic dianhydrides. Tetracarboxylic acid compounds may be used individually or in combination of two or more. In addition to dianhydrides, tetracarboxylic acid compounds may also be tetracarboxylic acid compound analogs such as acid chloride compounds.
[0079] Specific examples of tetracarboxylic acid compounds include pyromellitic anhydride (sometimes referred to as PMDA), 4,4'-(4,4'-isopropylidene diphenoxy)diphthalic anhydride (sometimes referred to as BPADA), 1,4,5,8-naphthalenetetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride (sometimes referred to as BPDA), 4,4'-(hexafluoroisopropylidene)diphthalic dianhydride (sometimes referred to as 6FDA), and 4,4'-oxydiphthalic anhydride. Substance (hereinafter sometimes referred to as ODPA), 2,2',3,3'-, 2,3,3',4'- or 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 2,3',3,4'-biphenyltetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, p-phenylenebis(trimellitic acid monoesteric acid dianhydride) (hereinafter sometimes referred to as TAHQ), esterified product of trimellitic anhydride and 2,2',3,3',5,5'-hexamethyl-4,4'-biphenol (hereinafter referred to as TMPBP) (may be), 4,4'-bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-ylcarbonyloxy)biphenyl (hereinafter sometimes referred to as BP-TME), 2,3',3,4'-diphenyl ether tetracarboxylic dianhydride, bis(2,3-dicarboxyphenyl) ether dianhydride, 3,3”,4,4”-p-terphenyl tetracarboxylic dianhydride, 2,3,3”,4”-p-terphenyl tetracarboxylic dianhydride, 2,2”,3,3”-p-terphenyl tetracarboxylic dianhydride, 2,2-bis(2, 3-Dicarboxyphenyl)-propane dianhydride, 2,2-bis(3,4-dicarboxyphenyl)-propane dianhydride, bis(2,3-dicarboxyphenyl)methane dianhydride, bis(3,4-dicarboxyphenyl)methane dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, 1,1-bis(3,4-dicarboxyphenyl)ethane dianhydride, 1,2,7,8-,1,2,6,7-phenanthrene-tetracarboxylic acid dianhydride, 1,2,9,10-phenanthrene-tetracarboxylic acid dianhydride, 2,2-bis(3,4-Dicarboxyphenyl)tetrafluoropropane dianhydride, 1,2,4,5-cyclohexanetetracarboxylic acid dianhydride (hereinafter sometimes referred to as HPMDA), 2,3,5,6-cyclohexanetetracarboxylic acid dianhydride, 2,3,6,7-naphthalenetetracarboxylic acid dianhydride, 1,2,5,6-naphthalenetetracarboxylic acid dianhydride, cyclopentane-1,2,3,4-tetracarboxylic acid dianhydride, 4,4'-bis(2,3-dicarboxyphenoxy)diphenylmethane dianhydride, 1,2, 3,4-Cyclobutanetetracarboxylic dianhydride (hereinafter sometimes referred to as CBDA), norbornane-2-spiro-α'-spiro-2”-norbornane-5,5',6,6'-tetracarboxylic anhydride, p-phenylenebis(trimellitate anhydride), 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 2,3,6,7-anthracenetetracarboxylic dianhydride, 4,8-dimethyl-1,2,3,5,6,7-hexahydronaphthalene-1,2,5,6-tetracarboxylic dianhydride , 2,6-dichloronaphthalene-1,4,5,8-tetracarboxylic dianhydride, 2,7-dichloronaphthalene-1,4,5,8-tetracarboxylic dianhydride, 2,3,6,7-tetrachloronaphthalene-1,4,5,8-tetracarboxylic dianhydride, 2,3,6,7-tetrachloronaphthalene-2,3,6,7-tetracarboxylic dianhydride, 1,4,5,8-tetrachloronaphthalene-1,4,5,8-tetracarboxylic dianhydride, 1,4,5,8-tetrachloronaphthalene-2,3,6,7-tetracarboxylic dianhydride Dianhydride, 2,3,8,9-perylene-tetracarboxylic acid dianhydride, 3,4,9,10-perylene-tetracarboxylic acid dianhydride, 4,5,10,11-perylene-tetracarboxylic acid dianhydride, 5,6,11,12-perylene-tetracarboxylic acid dianhydride, pyrazine-2,3,5,6-tetracarboxylic acid dianhydride, pyrrolidine-2,3,4,5-tetracarboxylic acid dianhydride, thiophene-2,3,4,5-tetracarboxylic acid dianhydride, bis(2,3-dicarboxyphenyl)sulfone dianhydride, bis(3,Examples include 4-dicarboxyphenyl)sulfone dianhydride. Among these, BPDA, TAHQ, and BP-TME are preferred from the viewpoint of easily reducing the Df of the resulting PI-based film and improving its bending resistance. These tetracarboxylic acid compounds can be used individually or in combination of two or more.
[0080] Examples of diamine compounds used in the synthesis of PI-based resin precursors include aliphatic diamines, aromatic diamines, and mixtures thereof. In this embodiment, "aromatic diamine" refers to a diamine having an aromatic ring, and its structure may include an aliphatic group or other substituents. This aromatic ring may be a monoring or a fused ring, and examples include, but are not limited to, a benzene ring, a naphthalene ring, anthracene ring, and a fluorene ring. Among these, a benzene ring is preferred. "Aliphatic diamine" refers to a diamine having an aliphatic group, and its structure may include other substituents, but it does not have an aromatic ring.
[0081] Specific examples of diamine compounds include 1,4-diaminocyclohexane, 4,4'-diamino-2,2'-dimethylbiphenyl (hereinafter sometimes referred to as m-Tb), 4,4'-diamino-3,3'-dimethylbiphenyl, 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl (hereinafter sometimes referred to as TFMB), 4,4'-diaminodiphenyl ether, 1,3-bis(3-aminophenoxy)benzene (hereinafter sometimes referred to as 1,3-APB), and 1,4-bis(4-aminophenoxy)benzene (hereinafter referred to as 1,4-A (sometimes written as PB), 1,3-bis(4-aminophenoxy)benzene, 2,2'-bis[4-(4-aminophenoxy)phenyl]propane, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dihydroxy-4,4'-diaminobiphenyl, 2,2-bis-[4-(3-aminophenoxy)phenyl]propane, bis[4-(4-aminophenoxy)]biphenyl, bis[4-(3-aminophenoxy)biphenyl, bis[1-(4-aminophenoxy)]biphenyl, bis[1-(3-aminophenoxy)]biphenyl, bi s[4-(4-aminophenoxy)phenyl]methane, bis[4-(3-aminophenoxy)phenyl]methane, bis[4-(4-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(4-aminophenoxy)]benzophenone, bis[4-(3-aminophenoxy)]benzophenone, 2,2-bis-[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2-bis-[4-(3-aminophenoxy)phenyl]hexafluoropropane, 4,4'-methylenedi-o-th Luidine, 4,4'-methylenedi-2,6-xylidine, 4,4'-methylene-2,6-diethylaniline, 4,4'-methylenedianiline, 3,3'-methylenedianiline, 4,4'-diaminodiphenylpropane, 3,3'-diaminodiphenylpropane, 4,4'-diaminodiphenylethane, 3,3'-diaminodiphenylethane, 4,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, 3,3-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, benzidine, 3,3'-diaminobiphenyl, 3,3'-Dimethoxybenzidine, 4,4"-Diamino-p-terphenyl, 3,3"-Diamino-p-terphenyl, m-Phenylenediamine, p-Phenylenediamine (hereinafter sometimes referred to as p-PDA), 2,2-Bis[4-(4-aminophenoxy)phenyl]propane (hereinafter sometimes referred to as BAPP), 1,4-Bis(4-aminophenoxy)benzene, 1,3-Bis(4-aminophenoxy)benzene, Resorcinol-Bis(3-aminophenyl) ether, 4,4'-[1,4-Phenylenebis(1-methylethylidene)] ]bisaniline, 4,4'-[1,3-phenylenebis(1-methylethylidene)]bisaniline, bis(p-aminocyclohexyl)methane, bis(p-β-amino-tert-butylphenyl)ether, bis(p-β-methyl-δ-aminopentyl)benzene, p-bis(2-methyl-4-aminopentyl)benzene, p-bis(1,1-dimethyl-5-aminopentyl)benzene, 1,5-diaminonaphthalene, 2,6-diaminonaphthalene, 2,4-bis(β-amino-tert-butyl)toluene, 2,4-diaminotoluene, m-xyl Len-2,5-diamine, p-xylene-2,5-diamine, m-xylylenediamine, p-xylylenediamine, piperazine, 4,4'-diamino-2,2'-bis(trifluoromethyl)bicyclohexane, 4,4'-diaminodicyclohexylmethane, 4,4"-diamino-p-terphenyl, bis(4-aminophenyl)terephthalate, 1,4-bis(4-aminophenoxy)-2,5-di-tert-butylbenzene, 4,4'-(1,3-phenylenediisopropylidene)bisaniline, 1,4-bis[2-(4-aminophenyl)- 2-Propylbenzene, 2,4-diamino-3,5-diethyltoluene, 2,6-diamino-3,5-diethyltoluene, 4,4'-bis(3-aminophenoxy)biphenyl, 4,4'-(hexafluoropropyridene)dianiline, 1,2-diaminoethane, 1,3-diaminopropane, 1,4-diaminobutane, 1,5-diaminopentane, 1,6-diaminohexane, 1,2-diaminopropane, 1,2-diaminobutane, 1,3-diaminobutane, 2-methyl-1,2-diaminopropane, 2-methyl-1,3-diaminopropane, 1,3-Bis(aminomethyl)cyclohexane, 1,4-Bis(aminomethyl)cyclohexane, norbornanediamine, 2'-Methoxy-4,4'-diaminobenzanilide, 4,4'-diaminobenzanilide, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, 9,9-Bis[4-(4-aminophenoxy)phenyl]fluorene, 9,9-Bis[4-(3-aminophenoxy)phenyl] Examples include [phenyl]fluorene, 4,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, 2,5-diamino-1,3,4-oxadiazole, bis[4,4'-(4-aminophenoxy)]benzanilide, bis[4,4'-(3-aminophenoxy)]benzanilide, 2,6-diaminopyridine, and 2,5-diaminopyridine. Among these, m-Tb and BAPP are preferred from the viewpoint of easily reducing the Df of the resulting PI-based film and easily improving its bending resistance. Diamine compounds can be used alone or in combination of two or more.
[0082] Furthermore, the PI-based resin precursor may be obtained by further reacting other tetracarboxylic acids, dicarboxylic acids, and tricarboxylic acids, as well as their anhydrides and derivatives, in addition to the tetracarboxylic acid compound used in the synthesis of the PI-based resin precursor, to the extent that it does not impair the various physical properties of the resulting PI-based film.
[0083] Other tetracarboxylic acids include the hydrate adducts of the anhydrides of the above-mentioned tetracarboxylic acid compounds.
[0084] Examples of dicarboxylic acid compounds include aromatic dicarboxylic acids, aliphatic dicarboxylic acids and their related acid chloride compounds, acid anhydrides, etc., and two or more may be used in combination. Specific examples include dicarboxylic acid compounds of terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid, 4,4'-biphenyldicarboxylic acid, 3,3'-biphenyldicarboxylic acid, and chain hydrocarbons having 8 or fewer carbon atoms, as well as compounds in which two benzoic acids are linked by a single bond, -O-, -CH2-, -C(CH3)2-, -C(CF3)2-, -SO2-, or phenylene group, and their acid chloride compounds.
[0085] Examples of tricarboxylic acid compounds include aromatic tricarboxylic acids, aliphatic tricarboxylic acids and their related acid chloride compounds, acid anhydrides, etc., and two or more may be used in combination. Specific examples include 1,2,4-benzenetricarboxylic acid anhydride; 2,3,6-naphthalentricarboxylic acid-2,3-anhydride; and compounds in which phthalic anhydride and benzoic acid are linked by a single bond, -O-, -CH2-, -C(CH3)2-, -C(CF3)2-, -SO2-, or phenylene group.
[0086] In the production of PI-based resin precursors, the amounts used of diamine compounds, tetracarboxylic acid compounds, dicarboxylic acid compounds, and tricarboxylic acid compounds can be appropriately selected according to the desired ratio of each constituent unit of the PI-based resin precursor. In the present invention, the total number of moles of diamine compound used relative to 1 mole of total tetracarboxylic acid compound is defined as the amine ratio. In a preferred embodiment of the present invention, the amine ratio is preferably 0.90 moles or more, more preferably 0.999 moles or less, and also preferably 1.001 moles or more, more preferably 1.10 moles or less, relative to 1 mole of total tetracarboxylic acid compound. In one embodiment of the present invention, when the amine ratio is 1 or less, the amine ratio is preferably 0.90 moles or more and 0.999 moles or less, more preferably 0.95 moles or more and 0.997 moles or less, and even more preferably 0.97 moles or more and 0.995 moles or less. In one embodiment of the present invention, when the amine ratio is 1 or more, the amine ratio is preferably 1.001 moles or more and 1.1 moles or less, more preferably 1.002 moles or more and 1.05 moles or less, and even more preferably 1.003 moles or more and 1.03 moles or less. When the amine ratio is close to 1.0 mole, the molecular weight tends to increase rapidly during synthesis, while when it deviates significantly from 1.0 mole, the molecular weight of the resulting PI-based resin tends to decrease. When the molecular weight increases rapidly, it grows non-uniformly within the synthesis mass, and the physical properties of the PI-based resin obtained from the PI-based resin precursor tend to be unstable. On the other hand, if the molecular weight is too low, the mechanical properties tend to deteriorate.
[0087] The reaction temperature between the diamine compound and the tetracarboxylic acid compound is preferably 50°C or lower, more preferably 40°C or lower, and even more preferably 30°C or lower. When the reaction temperature is below the above upper limit, the Df of the resulting PI-based film is easily reduced and the bending resistance is easily improved. This tendency is particularly pronounced in PI-based resins containing ester bonds, especially in PI-based films containing PI-based resins containing constituent unit (A1). Furthermore, the reaction temperature between the diamine compound and the tetracarboxylic acid compound is preferably 5°C or higher, more preferably 10°C or higher, and even more preferably 15°C or higher. When the reaction temperature is above the above lower limit, the reaction rate is easily increased and the polymerization time tends to be shortened. The reaction time is not particularly limited and may be, for example, 0.5 to 72 hours, preferably 3 to 24 hours. When the reaction time is within the above range, it is easier to reduce the Df of the resulting PI-based film and improve its bending resistance.
[0088] The reaction between a diamine compound and a tetracarboxylic acid compound is preferably carried out in a solvent. The solvent is not particularly limited as long as it does not affect the reaction, but examples include alcoholic solvents such as water, methanol, ethanol, ethylene glycol, isopropyl alcohol, propylene glycol, ethylene glycol methyl ether, ethylene glycol butyl ether, 1-methoxy-2-propanol, 2-butoxyethanol, and propylene glycol monomethyl ether; phenolic solvents such as phenol and cresol; esteric solvents such as ethyl acetate, butyl acetate, ethylene glycol methyl ether acetate, propylene glycol methyl ether acetate, and ethyl lactate; lactoneic solvents such as γ-butyrolactone (hereinafter sometimes referred to as GBL) and γ-valerolactone; acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, 2-heptanone, and methyl ethyl ether. Examples of solvents include ketone solvents such as isobutyl ketone; aliphatic hydrocarbon solvents such as pentane, hexane, and heptane; alicyclic hydrocarbon solvents such as ethylcyclohexane; aromatic hydrocarbon solvents such as toluene and xylene; nitrile solvents such as acetonitrile; ether solvents such as tetrahydrofuran and dimethoxyethane; chlorine-containing solvents such as chloroform and chlorobenzene; amide solvents such as N,N-dimethylacetamide (hereinafter sometimes referred to as DMAc) and N,N-dimethylformamide (hereinafter sometimes referred to as DMF); sulfur-containing solvents such as dimethyl sulfone, dimethyl sulfoxide, and sulfolane; carbonate solvents such as ethylene carbonate and propylene carbonate; pyrrolidone solvents such as N-methylpyrrolidone (hereinafter sometimes referred to as NMP); and combinations thereof. Among these, from the viewpoint of solubility, phenolic solvents, lactone solvents, amide solvents, pyrrolidone solvents, and more preferably amide solvents can be suitably used.
[0089] In one embodiment of the present invention, the boiling point of the solvent used in the reaction between the diamine compound and the tetracarboxylic acid compound is preferably 230°C or lower, more preferably 200°C or lower, and even more preferably 180°C or lower, from the viewpoint of easily reducing the Df of the resulting PI-based film and easily improving its bending resistance. Furthermore, the boiling point of the solvent is preferably 100°C or higher, more preferably 120°C or higher, from the viewpoint of easily reducing the Df of the resulting PI-based film and easily improving its bending resistance.
[0090] The reaction between the diamine compound and the tetracarboxylic acid compound may be carried out under an inert atmosphere such as a nitrogen atmosphere or an argon atmosphere, or under reduced pressure, as needed. Preferably, the reaction is carried out under an inert atmosphere, such as a nitrogen atmosphere or an argon atmosphere, while stirring in a strictly controlled dehydrated solvent.
[0091] The resulting PI-based resin precursor may be isolated by conventional methods, or the reaction solution containing the PI-based resin precursor obtained by the synthesis of the PI-based resin precursor may be used in the production of the PI-based resin without isolation.
[0092] It is preferable to produce the PI-based resin by imidizing the PI-based resin precursor through heat treatment at a temperature of 200°C to 500°C.
[0093] In the present invention, the imidation temperature is preferably 500°C or lower, more preferably 400°C or lower, even more preferably less than 350°C, even more preferably 340°C or lower, particularly preferably 330°C or lower, particularly more preferably 310°C or lower, and most preferably 300°C or lower. Furthermore, from the viewpoint of easily improving the imidation rate and easily improving Df, the imidation temperature is preferably 200°C or higher, more preferably 210°C or higher, and even more preferably 220°C or higher. Heating may also be carried out in stages. For example, after heating at a relatively low temperature of 50 to 150°C to remove the solvent, imidation may be carried out by gradually heating to a temperature in the range of 200°C to 500°C, preferably 200°C to less than 400°C, and more preferably 200°C to less than 350°C.
[0094] In one embodiment of the present invention, the reaction time for imidization is preferably 0.5 to 24 hours, more preferably 1 to 12 hours. Also in one embodiment of the present invention, the time for maintaining a temperature of 200°C or higher is preferably 10 to 90 minutes, more preferably 15 to 70 minutes, and even more preferably 20 to 50 minutes.
[0095] PI resins can be separated, purified, and isolated by conventional methods, such as filtration, concentration, extraction, crystallization, recrystallization, column chromatography, or combinations thereof.
[0096] [Polyimide film] A PI-based film containing the PI-based resin of the present invention can have a low Df. Furthermore, in a preferred embodiment of the present invention, the PI-based film also exhibits excellent bending resistance. In particular, the PI-based resin of the present invention can form a PI-based film with a low Df even at low imidation temperatures. Therefore, the present invention also includes PI-based films containing the PI-based resin of the present invention. The present invention also includes PI-based films containing a PI-based resin obtained by imidizing a PI-based resin precursor by heat treatment at 200°C to 500°C, preferably 200°C to less than 400°C, and more preferably 200°C to less than 350°C.
[0097] In one embodiment of the present invention, the content of PI resin in the PI film is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more, relative to the total amount of the PI film of the present invention. Furthermore, there is no particular upper limit to the content of PI resin, and it is, for example, 100% by mass or less, preferably 99% by mass or less, and more preferably 95% by mass or less, relative to the total amount of the PI film. When the content of PI resin is within the above range, it is easy to improve mechanical properties, thermal properties, and dielectric properties.
[0098] The PI-based film of the present invention may optionally contain fillers. Examples of fillers include metal oxide particles such as silica and alumina, inorganic salts such as calcium carbonate, and polymer particles such as fluororesins and cycloolefin polymers. Fillers can be used alone or in combination of two or more types. When fillers are included, their content is preferably 50% by mass or less, more preferably 40% by mass or less, even more preferably 30% by mass or less, and preferably 0.01% by mass or more, based on the total mass of the PI-based film.
[0099] Furthermore, in one embodiment of the present invention, the PI-based film of the present invention may contain additives as needed. Examples of additives include antioxidants, flame retardants, crosslinking agents, surfactants, compatibilizers, imidation catalysts, weathering agents, lubricants, antiblocking agents, antistatic agents, antifogging agents, anti-drip agents, and pigments. Additives can be used individually or in combination of two or more. The content of each additive can be appropriately selected within a range that does not impair the effects of the present invention. When various additives are included, their total content is preferably 7% by mass or less, more preferably 5% by mass or less, even more preferably 4% by mass or less, and preferably 0.001% by mass or more, based on the total mass of the PI-based film. The PI-based resin of the present invention may also contain the filler and the additives.
[0100] In one embodiment of the present invention, the PI-based film of the present invention preferably has an in-plane orientation index (hereinafter sometimes simply referred to as the in-plane orientation index) of 58 or higher, as defined by the following formula 1. An in-plane orientation index of 58 or higher makes it easier to reduce the Df of the PI-based film. In X-ray diffraction measurements, diffraction peaks indicate a periodic structure at a distance corresponding to the diffraction angle 2θ. A strong peak intensity indicates a large number of components with a periodic structure, or that the periodicity of those components is highly regular. Furthermore, if the diffraction peak is strongly detected at a specific azimuth angle, it indicates that a periodic structure is formed in the direction of that azimuth angle, or that the molecular backbone is oriented perpendicular to the azimuth angle. In X-ray measurements of PI-based films, it is known that many diffraction peaks are detected, reflecting multiple periodicities in the higher-order structure of the molecular chains of the PI-based resin, as shown in Figure 4, for example. If the in-plane orientation index defined in Equation 1 is 58 or higher, it means that a certain amount of PI-based resin is oriented along the film plane, and that these are distributed perpendicular to the film at a distance corresponding to the diffraction angle 2θ = 16°. When PI-based resin forms such a regular higher-order structure, it is presumed that the rotational motion of the resin's molecular chains is suppressed for some reason, and the Df of the PI-based film is reduced. On the other hand, if the in-plane orientation index defined in Equation 1 is less than 58, the rotational motion of the resin's molecular chains is not sufficiently suppressed, and the Df of the PI-based film cannot be sufficiently reduced.
[0101] In-plane orientation index = (180-FWHM) / 180×100 (Equation 1) [In Equation 1, FWHM represents the full width at half maximum of the peak appearing at the azimuth angle corresponding to the ND direction of the film, in the azimuth profile at 2θ = 16°, obtained by analyzing the two-dimensional diffraction pattern of a transmission X-ray diffraction measurement performed by incidenting X-rays parallel to the TD direction of the film.]
[0102] The in-plane orientation index can be determined by measuring the FWHM using transmission X-ray measurement and substituting the obtained FWHM value into equation (1).
[0103] The measurement method for FWHM will be explained below using Figures 1 and 2. Figure 1 is a schematic diagram illustrating the method for determining the in-plane orientation index by transmission X-ray diffraction measurement. Note that in Figure 1, the size of the test specimen, such as the aspect ratio, has been adjusted for clarity of explanation and is not limited to this.
[0104] First, a test specimen for measurement is prepared by cutting and / or stacking films. The size of the test specimen is not limited as long as it is large enough to obtain sufficient resolution and diffraction intensity, but preferably, the width in the MD direction is 0.5 to 3 cm, the width in the TD direction is 0.5 to 2 mm, and the thickness in the ND direction is 100 μm or more. The upper limit of the thickness in the ND direction is preferably 2 mm. This thickness can be obtained by stacking multiple films. Next, as shown in Figure 1, the test specimen 1a is set in the X-ray apparatus so that the direction of X-ray irradiation is parallel to the TD direction of the film. Then, X-rays are incident on the test specimen 1a from the X-ray source 2a, and a two-dimensional diffraction pattern is obtained by the detector 3a. The obtained two-dimensional diffraction pattern is corrected using a two-dimensional diffraction pattern (air blank) obtained without setting up the test specimen 1a. Furthermore, from the two-dimensional diffraction pattern, an azimuth profile at 2θ=16° is obtained such that the azimuth profiles at 0° and 180° correspond to the MD direction of the test specimen 1a, and the azimuth profiles at 90° and 270° correspond to the ND direction of the test specimen 1a. The diffraction intensity for each azimuth angle is the average value of the diffraction intensity in the range of 2θ=15.5 to 16.5°.
[0105] In the resulting azimuth profile (2θ = 0 to 360°), the full width at half maximum (FWHM) of the peaks at 90° and 270° is determined, and the average of the two FWHMs is defined as FWHM. The FWHM represents the peak intensity at 90° or 270° and the width of the peak at the position where the intensity is half of the minimum intensity in the azimuth angle range of -90° to +90° of that peak intensity. For example, in the azimuth profile shown in Figure 2, the FWHM of the peak at 270°, which corresponds to the ND direction, is the width of the peak at the position indicated by 4 in Figure 2, where the intensity is half of the minimum intensity in the range of 180 to 360°, and is indicated by 5 in Figure 2. In this specification, the MD direction is the direction parallel to the machine flow direction during manufacturing within the film plane, the TD direction is the direction perpendicular to the machine flow direction, and the ND direction is the thickness direction of the film, i.e., the direction perpendicular to the film plane. If the direction of the MD direction and TD direction within the film plane is unknown, it shall be determined by the following method. In the transmission X-ray measurement, the azimuth profile at 2θ=16°, measured by irradiating with X-rays from the ND direction, is defined as the MD direction, where the scattering intensity is strongest.
[0106] Furthermore, the above X-ray apparatus can be set to the following measurement conditions. ·X-ray source: Cu-Kα ray Voltage: 40kV ·Current: 20mA • Camera length: 70mm • Exposure time: 10 minutes • Beam diameter: 0.25mm
[0107] The sharper the peak appearing in the ND direction, the smaller the FWHM value becomes, and the larger the in-plane orientation index in the formula can be.
[0108] In the PI-based film of the present invention, the in-plane orientation index is preferably 60 or higher, more preferably 62 or higher, even more preferably 64 or higher, even more preferably 66 or higher, particularly preferably 68 or higher, and particularly more preferably 69 or higher. When the in-plane orientation index is above the lower limit of the above, it is easier to reduce the Df of the PI film. The upper limit of the in-plane orientation index is preferably 95 or lower, more preferably 90 or lower, even more preferably 85 or lower, and even more preferably 80 or lower. When the in-plane orientation index is below the upper limit of the above, it is easier to suppress the anisotropy of mechanical properties associated with molecular orientation. The in-plane orientation index can be determined by the above method, and may also be determined by the method described in the examples, for example.
[0109] The in-plane orientation index can be adjusted by appropriately adjusting the type and composition of the constituent units of the PI resin, the molecular weight of the PI resin, and the manufacturing method such as coating conditions and imidation conditions. For example, it may be adjusted to the above range by adopting preferred embodiments described herein, particularly those described as improving dielectric properties. For example, it may be adjusted by using preferred constituent units of the PI resin and their content, preferred solvents contained in the PI resin precursor solution, and preferred imidation conditions. Adding ester bonds to PI resins tends to increase the in-plane orientation index, while increasing the amount of flexible components in PI resins tends to decrease the in-plane orientation index.
[0110] (molecular periodicity index) In one embodiment of the present invention, the PI-based film of the present invention preferably has a molecular periodicity index represented by the following formula 2 of 7.0 or higher. Molecular periodicity index = I(16°) / I(min) (Equation 2) [I(16°) represents the maximum diffraction intensity in the diffraction intensity profile obtained by reflection X-ray diffraction measurement at 2θ = 15.5~16.5°. I(min) represents the minimum diffraction intensity in the diffraction intensity profile obtained by reflection X-ray diffraction measurement at 2θ = 20 to 30°.
[0111] The molecular periodicity index is determined by measuring I(16°) and I(min) using reflection X-ray diffraction and substituting them into Equation 2.
[0112] The measurement methods for I(16°) and I(min) will be explained below using Figures 3 and 4. Figure 3 is a schematic diagram illustrating the method for determining the molecular periodicity index by reflection X-ray diffraction measurement. Note that the size of the test specimen (e.g., aspect ratio) in Figure 3 has been adjusted for clarity of explanation and is not limited to these specifications.
[0113] First, a test specimen for measurement is prepared by cutting and / or stacking the film. The size of the test specimen is not limited as long as it is large enough to obtain sufficient resolution and diffraction intensity, but preferably the width in the MD direction is 0.5 to 5 cm and the width in the TD direction is 0.5 to 5 cm. Next, as shown in Figure 3, the measurement sample 1b is attached to the sample holder 6 such that the ND direction of the film is parallel to the normal direction of the surface of the sample holder 6, i.e., the direction perpendicular to the surface, and when the sample holder 6 is installed in the X-ray apparatus, the MD direction of the film is parallel to the line 7 connecting the detection positions of the X-ray source 2b and the detector 3b. Next, while maintaining the parallelism between line 7 and the MD direction, a reflectance measurement of the film surface is performed in the range of 2θ = 5 to 30° to obtain the diffraction profile A of the film. Next, the film is cut to a length of 2.5 cm in the MD direction and 3 cm in the TD direction to obtain a sample 1b for measurement. Then, as shown in Figure 3, the sample 1b for measurement is attached to the sample holder 6 such that the ND direction of the film is parallel to the normal direction of the surface of the sample holder 6, i.e., the direction perpendicular to the surface, and that when the sample holder 6 is installed in the X-ray apparatus, the line 7 connecting the detection positions of the X-ray source 2b and the detector 3b is parallel to the TD direction of the film. Next, a reflectance measurement of the film surface is performed in the range of 2θ = 5 to 30° to obtain the diffraction profile B of the film. In the reflectance measurement, the X-ray source and detector should be moved in the range of 2θ = 5 to 30° on the Rowland circle while maintaining that the line 7 and the TD direction are parallel. Each diffraction profile is blank-corrected by subtracting the background. The average of the blank-corrected diffraction profile A and diffraction profile B is taken as the diffraction intensity profile of the film. From the diffraction intensity profile of the film, the maximum diffraction intensity in the range of 2θ = 15.5 to 16.5° is defined as I(16°), and the minimum diffraction intensity in the range of 2θ = 20 to 30° is defined as I(min). For example, in the diffraction intensity profile shown in Figure 4, I(16°) is the maximum diffraction intensity in the range of 2θ = 15.5 to 16.5° (8 in the figure), and I(min) is the minimum diffraction intensity in the range of 2θ = 20 to 30° (9 in the figure). Furthermore, the above X-ray apparatus can be set to the following measurement conditions. ·X-ray source: Cu-Kα ray • Tube voltage: 40kV ·Tube current: 150mA • Divergent slit: 1° • Scattering slit: 1° • Light-receiving slit: 0.15mm • Divergence vertical limiting slit: 10mm • Measurement range: 2θ = 5~30° Measurement step: 0.02° • Scan speed: 0.5° / min • Sample holder: Aluminum sample plate
[0114] When the molecular periodicity index expressed in Equation 2 is 7.0 or higher, the Df of PI-based films is more easily reduced. It is estimated that if PI-based resins are distributed while maintaining a distance corresponding to the diffraction angle 2θ = 16°, the rotational motion of the resin's molecular chains is suppressed for some reason, and the Df of the PI-based film is reduced. However, if the molecular periodicity index is 7.0 or higher, it is estimated that a lower Df will result because there will be more components arranged at such a constant distance regardless of the orientation of the molecular chains.
[0115] In the PI-based film of the present invention, the molecular periodicity index is preferably 7.1 or higher, more preferably 7.3 or higher, even more preferably 7.5 or higher, even more preferably 7.7 or higher, and particularly preferably 7.8 or higher. When the molecular periodicity index is above the lower limit of the above, it is easier to reduce the Df of the PI-based film. The upper limit of the molecular periodicity index is preferably 20 or lower, more preferably 15 or lower, even more preferably 12 or lower, and even more preferably 10 or lower. The molecular periodicity index can be determined by the above method, or for example, by the method described in the examples.
[0116] The molecular periodicity index can be adjusted by appropriately adjusting the types and composition of the constituent units of the PI resin, the molecular weight of the PI resin, and the manufacturing method such as the imidation conditions. For example, it may be adjusted to the above range by adopting preferred embodiments as described herein, particularly embodiments that improve dielectric properties. For example, it may be adjusted by using preferred constituent units of the PI resin and their content, preferred solvents contained in the PI resin precursor solution, and preferred imidation conditions. When ester bonds are included in PI-based resins, the molecular periodicity index tends to increase, and when the amount of flexible components in PI-based resins increases, the molecular periodicity index tends to decrease.
[0117] (In-plane anisotropy index) In one embodiment of the present invention, the PI-based film of the present invention preferably has an in-plane anisotropy index A defined by the following formula 3 that is 0.8 or more and 1.2 or less, and an in-plane anisotropy index B defined by the following formula 4 that is greater than 1.1. In-plane anisotropy index A = I(MD) / I(TD) (Equation 3) In-plane anisotropy index B = I(MAX) / I(MIN) (Equation 4) [In equations 3 and 4, in the azimuth angle profile at 2θ=16° obtained by analyzing the two-dimensional diffraction pattern of a transmission X-ray diffraction measurement performed by incidenting X-rays parallel to the ND direction of the film, I(MD) represents the diffraction intensity corresponding to the MD direction of the film, I(TD) represents the diffraction intensity corresponding to the TD direction, I(MAX) represents the maximum value of the diffraction intensity, and I(MIN) represents the minimum value of the diffraction intensity.]
[0118] The in-plane anisotropy indices A and B are determined by measuring I(MD), I(TD), I(MAX), and I(MIN) by transmission X-ray diffraction and substituting them into equations 3 and 4.
[0119] The measurement methods for I(MD), I(TD), I(MAX), and I(MIN) will be explained below using Figures 5 and 6. Figure 5 is a schematic diagram illustrating the method for determining the in-plane anisotropy index by transmission X-ray diffraction measurement. Note that the size of the test specimen (e.g., aspect ratio) in Figure 5 has been adjusted for clarity of explanation and is not limited to these parameters.
[0120] First, a test specimen for measurement is prepared by cutting and / or stacking the film. The size of the test specimen is not limited as long as it is large enough to obtain sufficient resolution and diffraction intensity, but preferably the width in the MD direction is 0.5 cm to 3 cm and the width in the TD direction is 0.5 cm to 3 cm. The width in the ND direction is preferably adjusted to 0.1 mm to 2 mm. Next, as shown in Figure 5, the test specimen 1c is set in the X-ray apparatus so that the direction of X-ray irradiation is parallel to the ND direction of the film. Then, X-rays are incident on the test specimen 1c from the X-ray source 2c, and a two-dimensional diffraction pattern is obtained by the detector 3c. The obtained two-dimensional diffraction pattern is corrected using a two-dimensional diffraction pattern (air blank) obtained without setting up the test specimen 1c. Furthermore, from the two-dimensional diffraction pattern, an azimuth profile at 2θ=16° is obtained such that the azimuth profiles at 0° and 180° correspond to the MD direction of the test specimen 1c, and the azimuth profiles at 90° and 270° correspond to the TD direction of the test specimen 1c. The diffraction intensity for each azimuth angle is the average value of the diffraction intensity in the range of 2θ=15.5 to 16.5°. In the resulting azimuth profile (2θ = 0 to 360°), the diffraction intensities at 0° and 180° are determined, and their average value is defined as I(MD). The diffraction intensities at 90° and 270° are also determined, and their average value is defined as I(TD). Furthermore, in the resulting azimuth profile (2θ = 0 to 360°), the maximum diffraction intensity in the range of 0 to 360° is defined as I(MAX), and the minimum diffraction intensity is defined as I(MIN). For example, in the azimuth profile shown in Figure 4, I(MD) is the average of the diffraction intensity of 10 at 0° and the diffraction intensity of 12 at 180°, I(TD) is the average of the diffraction intensity of 11 at 90° and the diffraction intensity of 14 at 270°, I(MAX) is the maximum value in the range of 0 to 360° (15 in the figure), and I(MIN) is the minimum value in the range of 0 to 360° (13 in the figure). Furthermore, the above X-ray apparatus can be set to the following measurement conditions. ·X-ray source: Cu-Kα ray • Camera length: 70mm • Exposure time: 10 minutes Voltage: 40kV ·Current: 20mA • Beam diameter: 0.25mm
[0121] In a PI-based film containing a PI-based resin containing a constituent unit (A) derived from tetracarboxylic anhydride and a constituent unit (B) derived from diamine, if the in-plane anisotropy index A defined by formula 3 is 0.8 or more and 1.2 or less, and the in-plane anisotropy index B defined by formula 4 is greater than 1.1, the Df of the PI-based film is more easily reduced.
[0122] The in-plane anisotropy index A represents the ratio of the orientation and degree of regularity of the resin's molecular chains in the MD direction and the TD direction. A value closer to 1 indicates a smaller difference in anisotropy between MD and TD. When the in-plane anisotropy index A is between 0.8 and 1.2, the film has isotropic properties within its plane and tends to have isotropic thermal and mechanical properties, making it easier to handle when processed into printed circuit boards. On the other hand, the in-plane anisotropy index B represents the ratio of the diffraction intensity in the direction with the strongest diffraction intensity to the direction with the weakest diffraction intensity in the azimuthal angle profile. If the in-plane anisotropy index B is greater than 1.1 despite the in-plane anisotropy index A being between 0.8 and 1.2, it is thought that the PI resin itself forms a higher-order structure with a distance corresponding to the diffraction angle 2θ = 16°. In such a structure, the rotational motion of the resin's molecular chains is easily suppressed, and it is estimated that the Df of the PI film is reduced.
[0123] In the PI-based film of the present invention, the in-plane anisotropy index A is preferably 0.8 or higher, more preferably 0.83 or higher, even more preferably 0.87 or higher, even more preferably 0.9 or higher, particularly preferably 0.93 or higher, particularly more preferably 0.97 or higher, preferably 1.2 or lower, more preferably 1.17 or lower, even more preferably 1.13 or lower, even more preferably 1.1 or lower, particularly preferably 1.07 or lower, and particularly more preferably 1.03 or lower. When the in-plane anisotropy index A is within the above range, the film tends to have thermally and mechanically isotropic properties, making it easier to handle when processing it as a printed circuit board.
[0124] In the PI-based film of the present invention, the in-plane anisotropy index B is preferably 1.12 or higher, more preferably 1.15 or higher, even more preferably 1.17 or higher, and still more preferably 1.2 or higher. When the in-plane anisotropy index B is above the lower limit of the above, it is easier to reduce the Df of the PI-based film. The upper limit of the in-plane anisotropy index B is preferably 3.0 or lower, more preferably 2.5 or lower, even more preferably 2.0 or lower, still more preferably 1.7 or lower, and particularly preferably 1.5 or lower. The in-plane anisotropy index can be determined by the above method, or for example, by the method described in the examples.
[0125] The in-plane anisotropy indices A and B can be adjusted by appropriately adjusting the types and compositions of the constituent units of the PI resin, the molecular weight of the PI resin, and the manufacturing method such as the imidation conditions. For example, they may be adjusted within the above range by adopting preferred embodiments as specified herein, particularly embodiments that improve dielectric properties. For example, they may be adjusted by using preferred constituent units of the PI resin and their content, preferred solvents contained in the PI resin precursor solution, and preferred imidation conditions. When ester bonds are included in the PI resin, the in-plane anisotropy index B tends to increase, and when there are many flexible components in the PI resin, the in-plane anisotropy index B tends to decrease.
[0126] In one embodiment of the present invention, the CTE of the PI-based film is preferably 50 ppm / K or less, more preferably 40 ppm / K or less, even more preferably 30 ppm / K or less, even more preferably 25 ppm / K or less, preferably 0 ppm / K or more, more preferably 5 ppm / K or more, even more preferably 8 ppm / K or more, and even more preferably 12 ppm / K or more. By setting the CTE within the above range, the CTE of the copper foil and the PI layer become close, so that peeling of the laminated film can be suppressed. The CTE can be measured, for example, by TMA and can be determined by the method described in the examples.
[0127] Printed circuits require low transmission loss. Transmission loss is expressed as the sum of dielectric loss, which is the loss caused by the electric field generated in the dielectric, and conductor loss, which is the loss caused by the current flowing through the conductor. It is known that dielectric loss is approximately proportional to the index E, which is expressed by equation (i). E = Df × (Dk) 1 / 2 (i) [In equation (i), Df represents the dielectric loss tangent and Dk represents the relative permittivity.] In the high-frequency range used in 5G FPCs, dielectric loss tends to increase, so there is a particular need for materials with a small value of the aforementioned index E that can suppress dielectric loss. On the other hand, high-frequency signals concentrate current at the very surface of the conductor. Therefore, conductor loss is related to the dielectric properties of the contacting dielectric and is approximately (Dk) 1 / 2 It is known to be proportional to [something].
[0128] As described above, the PI-based film of the present invention, which contains the PI-based resin of the present invention, has a predetermined content of constituent units (A1), (A2), and (B1) in the PI-based resin. Therefore, Df and Dk become smaller, and the dielectric loss index E and conductor loss also become smaller, thus reducing transmission loss in circuits containing the PI-based film.
[0129] In one embodiment of the present invention, the dielectric loss index E of the PI-based film at 10 GHz is preferably 0.01 or less, more preferably 0.009 or less, even more preferably 0.008 or less, even more preferably 0.007 or less, and particularly preferably 0.006 or less. The smaller the index E, the lower the transmission loss of the electronic circuit including the PI-based film; therefore, the lower limit of the index E is not particularly limited and may be, for example, 0 or more.
[0130] In one embodiment of the present invention, the Df of the PI-based film at 10 GHz is preferably less than 0.004, more preferably 0.0038 or less, even more preferably 0.0035 or less, even more preferably 0.0033 or less, particularly preferably 0.003 or less, particularly more preferably 0.0027 or less, and especially preferably 0.0024 or less, from the viewpoint of easily reducing the transmission loss of the electronic circuit including the PI-based film. The smaller the Df, the lower the transmission loss of the electronic circuit including the PI-based film; therefore, the lower limit of the Df is not particularly limited and may be, for example, 0 or more.
[0131] In one embodiment of the present invention, the Dk of the PI-based film at 10 GHz is preferably less than 3.50, more preferably 3.45 or less, even more preferably 3.40 or less, even more preferably 3.38 or less, and particularly preferably 3.36 or less.
[0132] The Df and Dk of a PI-based film can be measured using a vector network analyzer and a resonator, for example, by the method described in the examples.
[0133] In one embodiment of the present invention, the PI-based film of the present invention, which contains the PI-based resin of the present invention, has excellent bending resistance, particularly folding resistance, because the content of constituent units (A1), (A2), and (B1) in the PI-based resin satisfies a predetermined range, as described above. The number of folds until fracture in the MIT folding fatigue test of the PI-based film of the present invention, in accordance with ASTM standard D2176-16, is preferably 20,000 or more, more preferably 50,000 or more, even more preferably 100,000 or more, even more preferably 150,000 or more, and particularly preferably 200,000 or more. If the number of folds is above the lower limit above, the occurrence of cracks, breaks, creases, etc., can be effectively suppressed even with repeated bending. Furthermore, the upper limit of the number of folds is not particularly limited and may be, for example, 10,000,000 or less. The MIT folding fatigue test can be measured using an MIT folding fatigue tester.
[0134] The thickness of the PI-based film of the present invention can be appropriately selected depending on the application, preferably 5 μm or more, more preferably 10 μm or more, even more preferably 20 μm or more, preferably 500 μm or less, more preferably 300 μm or less, even more preferably 100 μm or less, particularly preferably 80 μm or less, and particularly more preferably 50 μm or less. The film thickness can be measured using a film thickness gauge or the like. Note that if the film of the present invention is a multilayer film, the above thickness represents the thickness of the single layer portion.
[0135] The PI-based film of the present invention may be subjected to surface treatments such as corona discharge treatment, plasma treatment, or ozone treatment by methods commonly used in industry.
[0136] Because the PI-based film of the present invention has a low Df, it can be suitably used as a substrate material for high-frequency band printed circuit boards and antenna boards. Copper foil layers (CCLs) used in FPCs are widely used as laminates having copper foil layers on one or both sides of a single or multiple layers of PI-based resin. When the PI-based film of the present invention is used as a resin layer, the PI-based film of the present invention can have a low Df even at low temperatures such as 350°C or less when imidizing. Therefore, even when the CCL is manufactured by thermal imidizing a PI-based resin precursor coating on copper foil, deterioration of the copper foil surface can be suppressed, and a CCL with excellent high-frequency characteristics can be obtained.
[0137] [Method for manufacturing polyimide films] The PI-based film of the present invention is produced by, for example, the following process: A step of coating a PI-based resin precursor solution containing the PI-based resin precursor of the present invention onto a substrate, and A process of imidizing a PI-based resin precursor by heat treatment at a temperature between 200°C and 500°C. It can be manufactured by a method that includes [a specific component].
[0138] <Coating process for polyimide resin precursor solution> (Preparation of PI resin precursor solution) A PI-based resin precursor solution comprises the PI-based resin precursor and a solvent, and can be prepared by mixing the PI-based resin precursor and the solvent. In one embodiment of the present invention, a reaction solution containing the PI-based resin precursor obtained by the synthesis of the PI-based resin precursor may be appropriately diluted with a solvent as needed and used as a PI-based resin precursor solution.
[0139] The solvent contained in the PI resin precursor solution is one of the solvents exemplified for use in the reaction between the diamine compound and the tetracarboxylic acid compound in the production of the PI resin precursor, and is preferably a lactone solvent, an amide solvent, a pyrrolidone solvent, and more preferably an amide solvent. Furthermore, in one embodiment of the present invention, the boiling point of the solvent contained in the PI resin precursor solution is preferably 230°C or lower, more preferably 200°C or lower, even more preferably 180°C or lower, and particularly preferably 170°C or lower, from the viewpoint of easily reducing the Df of the obtained PI film and easily improving its bending resistance, even at low imidation temperatures. Furthermore, the boiling point of the solvent is preferably 100°C or higher, more preferably 120°C or higher, from the viewpoint of easily reducing the Df of the obtained PI film and easily improving its bending resistance.
[0140] The content of the PI-based resin precursor in the PI-based resin precursor solution is preferably 8% by mass or more, more preferably 10% by mass or more, even more preferably 12% by mass or more, and particularly preferably 13% by mass or more, relative to the total amount of the PI-based resin precursor solution. Furthermore, it is preferably 30% by mass or less, more preferably 25% by mass or less, even more preferably 23% by mass or less, and particularly preferably 20% by mass or less. When the content of the PI-based resin precursor is within the above range, the processability during film formation is excellent.
[0141] (Coating of polyimide resin precursor solution) The coating process for PI-based resin precursor solution involves coating the substrate with the PI-based resin precursor solution to form a coating film.
[0142] In the coating process, a coating film is formed by coating the substrate with the composition using a known coating or application method. Known coating methods include, for example, wire bar coating, reverse coating, roll coating methods such as gravure coating, die coating, comma coating, lip coating, spin coating, screen printing coating, fountain coating, dipping, spraying, curtain coating, slot coating, and flow molding. When coating or applying a solution of PI-based resin precursor onto a substrate, a single layer of PI-based resin precursor may be coated onto the substrate, or multiple layers of PI-based resin precursor may be coated onto the substrate. When coating multiple layers of PI-based resin precursor onto a substrate, the coating may be applied in multiple stages and dried, or multiple layers may be applied simultaneously.
[0143] Examples of substrates include copper plates such as copper foil, SUS plates such as SUS foil and SUS belts, glass substrates, PET films, PEN films, other PI resin films other than the PI film of the present invention, and polyamide resin films. Among these, copper plates, SUS plates, glass substrates, PET films, and PEN films are preferred from the viewpoint of excellent heat resistance, and copper plates, SUS plates, glass substrates, or PET films are more preferred from the viewpoint of adhesion to the film and cost.
[0144] <Imidification Process> The imidization process is a process of imidizing a PI-based resin precursor coated on a substrate by heat treatment at a temperature between 200°C and 500°C. In one embodiment of the present invention, the imidation step is preferably a step in which, before imidizing the PI-based resin precursor, a PI-based resin precursor solution coated on a substrate is heated and dried at a relatively low temperature of, for example, less than 300°C, and the resulting dried film of the PI-based resin precursor is imidized by heat treatment at 200°C to 500°C. Furthermore, in one embodiment of the present invention, a PI-based film may be obtained by imidizing the dried film of the PI-based resin precursor on the substrate, or a PI-based film may be obtained by peeling the dried film of the PI-based resin precursor from the substrate and imidizing the dried film peeled from the substrate.
[0145] In one embodiment of the present invention, the drying temperature of the PI-based resin precursor coated on the substrate is not particularly limited as long as it is within the temperature range in which the solvent dries and solidifies. However, from the viewpoint of avoiding surface roughness due to rapid drying and suppressing wrinkles and distortions that occur during processing, it is preferably less than 300°C, more preferably 260°C or less, even more preferably 200°C or less, and even more preferably 180°C or less. Furthermore, from the viewpoint of productivity, it is preferably 50°C or higher, more preferably 80°C or higher, and even more preferably 100°C or higher.
[0146] The PI-based resin precursor in this invention can reduce the Df of the resulting PI-based film and improve its bending resistance, even when imidized at low temperatures. The heat treatment temperature in the imidization process, i.e., the imidization temperature, is preferably 500°C or lower, more preferably 400°C or lower, even more preferably less than 350°C, even more preferably 340°C or lower, particularly preferably 330°C or lower, particularly more preferably 310°C or lower, and most preferably 300°C or lower. When the imidization temperature is below the above upper limit, even when copper foil is used as the substrate, thermal degradation of the copper foil can be suppressed, making it easier to obtain CCL with excellent high-frequency characteristics. Furthermore, from the viewpoint of easily improving the imidization rate and easily reducing Df, the imidization temperature is preferably 200°C or higher, more preferably 210°C or higher, and even more preferably 220°C or higher. Furthermore, from the viewpoint of easily obtaining a smooth film, it is preferable to perform heating in stages. For example, the solvent may be removed by heating at a relatively low temperature of 50 to 150°C, and then imidation may be carried out by gradually heating to a temperature in the range of 200°C to 500°C, preferably 200°C to 400°C, and more preferably 200°C to less than 350°C.
[0147] In one embodiment of the present invention, the reaction time for imidization is preferably 30 minutes to 24 hours, more preferably 1 to 12 hours. Also in one embodiment of the present invention, the time for maintaining a temperature of 200°C or higher is preferably 5 minutes to 90 minutes, more preferably 15 minutes to 70 minutes, and even more preferably 20 minutes to 50 minutes.
[0148] After imidization, a PI-based film can be obtained by peeling off the coating film formed on the substrate from the substrate. In one embodiment of the present invention, if the substrate is copper foil, a PI-based film can be formed without peeling off the coating film from the copper foil, and the resulting laminated film, in which the PI-based film is laminated on the copper foil, can be used as CCL.
[0149] If the film of the present invention is a multilayer film, it can be manufactured by a multilayer film formation method such as co-extrusion, extrusion lamination, heat lamination, or dry lamination.
[0150] [Laminated film] Because the PI-based film of the present invention has a low Df, it can be suitably used for forming metal-clad laminates used in FPCs. Therefore, the present invention includes a laminated film that uses the PI-based film of the present invention as the PI layer and includes a PI layer and a metal foil layer. In one embodiment of the present invention, the laminated film of the present invention may include the metal foil layer on only one side of the PI layer or on both sides.
[0151] In one embodiment of the present invention, examples of metal foils include copper foil, SUS foil, and aluminum foil, but copper foil is preferred from the viewpoint of conductivity and metalworkability.
[0152] The PI-based film of the present invention can be suitably used for forming CCLs that have a low Df and excellent high-frequency characteristics and preferably excellent bending resistance, even at low thermal imidation temperatures. Therefore, in a preferred embodiment of the present invention, the laminated film of the present invention is preferably a laminated film that includes a copper foil layer on one or both sides of the PI-based film of the present invention.
[0153] In one embodiment of the present invention, the thickness of the metal foil layer, particularly the copper foil layer, is preferably 1 μm or more, more preferably 5 μm or more, and from the viewpoint of facilitating circuit miniaturization and improving bending resistance, it is preferably 100 μm or less, more preferably 50 μm or less, even more preferably 30 μm or less, and particularly preferably 20 μm or less. The thickness of the metal foil layer, particularly the copper foil layer, can be measured using a film thickness gauge or the like. When the PI-based film contains metal foil layers, particularly copper foil layers, on both sides, the thicknesses of each metal foil layer, particularly each copper foil layer, may be the same or different from each other.
[0154] In one embodiment of the present invention, the thickness of the laminated film is preferably 5 μm or more, more preferably 10 μm or more, even more preferably 15 μm or more, preferably 100 μm or less, more preferably 80 μm or less, and even more preferably 60 μm or less. The thickness of the laminated film can be measured using a film thickness gauge or the like.
[0155] The laminated film of the present invention may include other layers, such as functional layers, in addition to the PI-based film and metal foil layer, particularly the copper foil layer. Examples of functional layers include the layers described above, such as a thermoplastic PI-based resin layer containing a thermoplastic PI-based resin or an adhesive layer. Functional layers can be used alone or in combination of two or more types.
[0156] In one embodiment of the present invention, the laminated film of the present invention may be a two-layer metal-clad laminate composed of a metal foil layer and a PI layer, or a three-layer metal-clad laminate composed of a metal foil layer, a PI layer and an adhesive layer. However, from the viewpoint of heat resistance, dimensional stability and weight reduction, a two-layer metal-clad laminate without an adhesive layer is preferred. Furthermore, because the PI-based film of the present invention has a low Df even at low imidation temperatures, even when a laminated film in which the metal foil is copper foil is manufactured by thermal imidation of a PI-based resin precursor coating on copper foil, deterioration of the copper foil surface can be suppressed. Therefore, the laminated film of the present invention has excellent high-frequency characteristics even without including an adhesive layer.
[0157] Furthermore, in one embodiment of the present invention, the PI-based film and the metal foil layer, particularly the copper foil layer, may be in direct contact, or a functional layer may be inserted between the PI-based film and the metal foil layer, particularly the copper foil layer, and they may be in contact via the functional layer. However, from the viewpoint of easily improving mechanical and thermal properties, it is preferable that the PI-based film and the metal foil layer, particularly the copper foil layer, are in direct contact. The functional layer that may be inserted between the PI-based film and the metal foil layer of the present invention may be a thermoplastic PI layer. From the viewpoint of easily improving mechanical and thermal properties, it is preferable that the layer in direct contact with the metal foil layer, particularly the copper foil layer, is the PI film or a thermoplastic PI layer as the functional layer of the present invention.
[0158] [Method for manufacturing laminated film] The laminated film of the present invention is formed, for example, by the following steps: A step of coating a substrate with a PI-based resin precursor solution containing a constituent unit (A) derived from tetracarboxylic anhydride and a constituent unit (B) derived from diamine, and A process of imidizing a PI-based resin precursor by heat treatment at a temperature of 200°C to 500°C to form the PI-based film of the present invention on a substrate. It can be manufactured by a method that includes [a specific component].
[0159] In the method for manufacturing the laminated film of the present invention, the steps of "coating a PI-based resin precursor solution containing a PI-based resin precursor onto a substrate" and "imidizing the PI-based resin precursor by heat treatment at 200°C to 500°C to form the PI-based film of the present invention on a substrate" are similarly governed by the descriptions of each step described in the section on "Method for Manufacturing Polyimide Films."
[0160] In one embodiment of the present invention, the substrate is preferably a metal foil, and particularly preferably a copper foil. The description regarding the metal foil, and especially the copper foil, is similar to the description regarding the metal foil in the [Laminated Film] section.
[0161] The laminated film of the present invention can also be produced by a method other than the above method, for example, by applying and drying a PI-based resin precursor solution containing a structural unit (A) derived from a tetracarboxylic anhydride and a structural unit (B) derived from a diamine on another base material other than the metal foil contained in the laminated film, peeling the dried film of the PI-based resin precursor obtained from the base material, and laminating the peeled dried film of the PI-based resin precursor on a metal foil. As a method of laminating the dried film of the PI-based resin precursor and the metal foil, a method by pressing, a laminating method using a hot roll, etc. may be adopted, and in the laminating step, imidization of the PI-based resin precursor may be performed simultaneously. However, since the PI-based film of the present invention has a low Df even at a low imidization temperature, for example, even when producing a laminated film in which the metal foil is a copper foil by performing thermal imidization of the PI-based resin precursor coating film on the copper foil, deterioration of the copper foil surface can be suppressed. Therefore, the laminated film of the present invention has excellent high-frequency characteristics even if it is produced without going through the above-described laminating step.
[0162] 〔Flexible Printed Circuit Board〕 The PI-based film of the present invention has a low Df and excellent bending resistance, and thus can be suitably used as an FPC substrate material. Therefore, the present invention also includes an FPC substrate including the PI-based film of the present invention.
Examples
[0163] [[ID=MS13]]Hereinafter, the present invention will be described more specifically based on examples and comparative examples, but the present invention is not limited to the following examples.
[0164] The abbreviations used in the examples and comparative examples represent the following compounds: BPDA: 3,4,3’,4’-Biphenyltetracarboxylic dianhydride TAHQ: p-Phenylenebis(trimellitic monoester dianhydride) BP-TME: 4,4’-Bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-ylcarbonyloxy)biphenyl m-Tb: 2,2’-Dimethyl 4,4’-diaminobiphenyl BAPP: 2,2-bis(4-aminophenoxyphenyl)propane
[0165] [Synthesis of Polyimide Resin Precursor] (Example 1) 17.93 g (84.4 mmol) of m-Tb and 0.35 g (a0.9 mmol) of BAPP were dissolved in 284 g of DMAc, and then 19.35 g (42.2 mmol) of TAHQ was added and stirred at 20°C for 1 hour under a nitrogen atmosphere. Then 12.42 g (42.2 mmol) of BPDA was added and stirred at 20°C for 24 hours under a nitrogen atmosphere to obtain a PI resin precursor composition. The molar ratio of the diamine monomer to the acid dianhydride monomer used was 1.01.
[0166] (Examples 2 to 6 and Comparative Example 1) A PI resin precursor composition was obtained in the same manner as in Example 1, except that the types and compositions of the monomers used were changed as shown in Table 1, respectively. Unless otherwise specified, the order of adding the monomers was diamine first and then acid dianhydride. The diamines were added in the order of the diamines that induce the structural units (B1), (B2), and (B3), and the acid dianhydrides were added in the order of the acid dianhydrides that induce the structural units (A1), (A2), and (A3).
[0167] [Manufacture of Polyimide Film] Using the solvent used in the synthesis of the PI resin precursor, the PI resin precursor compositions obtained in Examples 2 to 6 and Comparative Example 1 were appropriately diluted within the range where the content of the PI resin precursor was 10% by mass or more to adjust the viscosity to 40,000 cps or less, thereby preparing a PI resin precursor solution. The PI resin precursor solution was formed into a film under any of the following film-forming conditions 1 and 2 as shown in Table 1, respectively, to obtain a PI film made of PI resin. In Example 4, the azimuth profile in the measurement of the in-plane orientation index is shown in Figure 2, the diffraction intensity profile in the measurement of the molecular periodicity index is shown in Figure 4, and the azimuth profile in the measurement of the in-plane anisotropy index is shown in Figure 6.
[0168] [Film-forming Condition 1] A PI resin precursor solution was poured onto a glass substrate, and a coating film of the PI resin precursor solution was formed using an applicator at a linear velocity of 0.4 m / min. The coating film was heated at 120°C for 30 minutes, and after peeling the resulting film from the glass substrate, the film was fixed to a metal frame. The film fixed to the metal frame was heated from 30°C to 270°C over 19 minutes in a 7% oxygen atmosphere, and then cooled to 200°C over 35 minutes to produce a PI film. The time at which a temperature of 220°C or higher was maintained was 23 minutes. The time at which a temperature of 200°C or higher was maintained was 34 minutes.
[0169] <Film forming conditions 2> A PI resin precursor solution was poured and molded onto a glass substrate, and a coating film of the resin precursor solution was formed using an applicator at a linear velocity of 0.4 m / min. The coating film was heated at 120°C for 30 minutes to dry. After peeling the obtained film from the glass substrate, the film was fixed to a metal frame. The film fixed to the metal frame was heated in a 1% oxygen atmosphere from 30°C to 320°C over 9 minutes, then heated at 320°C for 6 minutes, and cooled to 200°C over 15 minutes to produce a PI film. The time at which a temperature of 220°C or higher was maintained was 21 minutes. The time at which a temperature of 200°C or higher was maintained was 25 minutes.
[0170] <Measurement of glass transition temperature Tg> The Tg of the PI resins obtained in the examples and comparative examples was determined by measuring the PI film as follows. Using a dynamic viscoelasticity measuring device (DVA-220, manufactured by IT Measurement Control Co., Ltd.), measurements were performed with the following samples and under the following conditions. For each measurement temperature, the tanδ, which is the ratio of the storage modulus (E') to the loss modulus (E"), was determined, and a tanδ curve was obtained. The temperature at which the peak of the tanδ curve shows its maximum value was defined as Tg. Test specimen: A rectangular parallelepiped measuring 40 mm in length, 5 mm in width, and 50 μm in thickness (note that the thickness may vary depending on the film used). Experiment mode: Single frequency, constant rate heating Experimental method: Tensile Sample gripping distance: 15 mm Measurement temperature range: Starting from room temperature, the temperature is raised to 342 °C Temperature rising rate: 5 °C / min Frequency: 10 Hz Static / dynamic stress ratio: 1.8 Main collected data: (1) Storage modulus (E’) (2) Loss modulus (E”) (3) tanδ (E” / E’)
[0171] <Measurement of storage modulus (E’)> For the PI resins obtained in the examples and comparative examples, the E’ at 280 °C was determined by performing dynamic viscoelasticity measurement in the same manner as the measurement of Tg.
[0172] <Measurement of X-ray> (1) In-plane orientation index For the PI films obtained in the examples and comparative examples, wide-angle X-ray diffraction measurement by the transmission method was performed under the following conditions. · Equipment name: Small-angle and wide-angle X-ray scattering / diffraction equipment Nanoviwer manufactured by Rigaku Corporation · Detector: Pilatus 100k · X-ray source: Cu-Kα ray · Voltage: 40 kV · Current: 20 mA · Camera length: 70 mm · Exposure time: 10 minutes · Beam diameter: 0.25 mm
[0173] Specifically, four films were stacked in the ND direction such that the MD directions were aligned. The stacked films were cut using a trimming knife so that the width in the MD direction was 1 cm and the width in the TD direction was 1 mm, obtaining test pieces for measurement. Next, as shown in FIG. 1, the test piece for measurement 1a was set in the X-ray apparatus such that the irradiation direction of the X-ray was parallel to the TD direction of the film, X-rays were incident from the X-ray source 2a on the test piece for measurement 1a, and a two-dimensional diffraction image was obtained by the detector 3a. The obtained two-dimensional diffraction image was corrected using a two-dimensional diffraction image (air blank) obtained without setting the test piece for measurement 1a. Further, from the two-dimensional diffraction image, an azimuthal profile at 2θ = 16° was obtained such that 0° and 180° of the azimuthal profile corresponded to the MD direction of the test piece for measurement 1a and 90° and 270° of the azimuthal profile corresponded to the ND direction of the test piece for measurement 1a. The diffraction intensity at each azimuthal angle was the average value of the diffraction intensities in the range of 2θ = 15.5 to 16.5°. In the obtained azimuthal profile (2θ = 0 to 360°), the half-value widths of the peaks existing at 90° and 270° were determined, the average value of the two half-value widths was taken as the FWHM, and this was substituted into Equation 1 to obtain the in-plane orientation index. Note that the half-value width of the peak existing at 90° indicates the peak width at the central intensity position between the peak intensity existing at 90° and the minimum intensity in the range of 0 to 180° (that is, the peak width at the position where the intensity is half of the peak intensity existing at 90° based on the minimum intensity), and the half-value width of the peak existing at 270° indicates the peak width at the central intensity position between the peak intensity existing at 270° and the minimum intensity in the range of 180 to 360° (that is, the peak width at the position where the intensity is half of the peak intensity existing at 270° based on the minimum intensity).
[0174] (2) Molecular periodicity index For the PI films obtained in the examples and comparative examples, wide-angle X-ray diffraction measurement by the reflection method was performed under the following conditions. · Apparatus name: X-ray diffractometer RINT-2000 manufactured by Rigaku Corporation · X-ray source: Cu-Kα ray · Tube voltage: 40 kV · Tube current: 150 mA · Divergence slit: 1° • Scattering slit: 1° • Light-receiving slit: 0.15mm • Divergence vertical limiting slit: 10mm • Measurement range: 2θ = 5~30° Measurement step: 0.02° • Scan speed: 0.5° / min • Sample holder: Aluminum sample plate (without bottom) manufactured by Rigaku Corporation • Detector: Rigaku Corporation, scintillation counter
[0175] Specifically, the film was cut to a length of 3 cm in the MD direction and 2.5 cm in the TD direction to obtain a sample 1b for measurement. Next, as shown in Figure 3, the sample 1b for measurement was attached to the sample holder 6 such that the ND direction of the film was parallel to the normal direction of the surface of the sample holder 6, i.e., perpendicular to the surface, and that when the sample holder 6 was installed in the X-ray apparatus, the line 7 connecting the detection positions of the X-ray source 2b and the detector 3b was parallel to the MD direction of the film. Then, while maintaining the parallelism between line 7 and the MD direction, the reflectance measurement of the film surface was performed in the range of 2θ = 5 to 30° to obtain the diffraction profile A of the film. Next, the film was cut into sections of 2.5 cm in the MD direction and 3 cm in the TD direction to obtain a sample 1b for measurement. Then, as shown in Figure 3, the sample 1b for measurement was attached to the sample holder 6 such that the ND direction of the film was parallel to the normal direction of the surface of the sample holder 6, i.e., the direction perpendicular to the surface, and that the TD direction of the film was parallel to the line 7 connecting the detection positions of the X-ray source 2b and the detector 3b when the sample holder 6 was installed in the X-ray apparatus. Then, while maintaining the parallelism between line 7 and the TD direction, the reflectance measurement of the film surface was performed in the range of 2θ = 5 to 30° to obtain the diffraction profile B of the film. Each diffraction profile was blank-corrected by subtracting the background. The average of the blank-corrected diffraction profile A and diffraction profile B was used as the diffraction intensity profile of the film. From the diffraction intensity profile of the film, the maximum diffraction intensity in the range of 2θ = 15.5 to 16.5° was defined as I(16°), and the minimum diffraction intensity in the range of 2θ = 20 to 30° was defined as I(min). These values were substituted into Equation 2 to obtain the molecular periodicity index.
[0176] (3) In-plane anisotropy indices A, B The PI films obtained in the examples and comparative examples were subjected to transmission wide-angle X-ray diffraction measurements under the following conditions. • Equipment name: Nanoviewer, a small-angle / wide-angle X-ray scattering / diffraction device manufactured by Rigaku Corporation. • Detector: Pilatus 100k ·X-ray source: Cu-Kα ray • Camera length: 70mm • Exposure time: 10 minutes Voltage: 40kV ·Current: 20mA • Beam diameter: 0.25mm
[0177] Specifically, four films were stacked in the ND direction so that their MD directions coincided. A trimming knife was used to cut the stacked films so that their width in the MD direction was 2 cm and their width in the TD direction was 2 cm, thereby obtaining a test specimen for measurement. Next, as shown in Figure 5, the test specimen 1c was set in the X-ray apparatus so that the direction of X-ray irradiation was parallel to the ND direction of the film. Then, X-rays were incident on the test specimen 1c from the X-ray source 2c, and a two-dimensional diffraction pattern was obtained by the detector 3c. The obtained two-dimensional diffraction pattern was corrected using an air blank, which is a two-dimensional diffraction pattern obtained without setting up the test specimen 1c. Furthermore, from the two-dimensional scattering pattern, an azimuth profile was obtained at 2θ=16° such that the azimuth profile of 0° and 180° corresponds to the MD direction of the test specimen 1c, and the azimuth profile of 90° and 270° corresponds to the TD direction of the test specimen 1c. The diffraction intensity for each azimuth angle was the average value of the diffraction intensity in the range of 2θ=15.5~16.5°. In the obtained azimuth profile (2θ = 0 to 360°), the diffraction intensities at 0° and 180° were determined and their average value was defined as I(MD), and the diffraction intensities at 90° and 270° were determined and their average value was defined as I(TD). Furthermore, in the above obtained azimuth profile (2θ = 0 to 360°), the maximum diffraction intensity in the range of 0 to 360° was defined as I(MAX), and the minimum diffraction intensity was defined as I(MIN). Finally, these values were substituted into equations 3 and 4 to determine the in-plane anisotropy index A and the in-plane anisotropy index B.
[0178] <Measurement of weight-average molecular weight Mw and number-average molecular weight Mn> The polystyrene-based Mw and Mn of the PI resin precursor obtained through synthesis were measured using GPC. The GPC measurements were performed under the following conditions. (1) Pretreatment method The sample was diluted with DMF and then filtered through a 0.45 μm membrane filter to obtain the measurement solution. (2) Measurement conditions Column: Two TSKgel SuperAWM-H columns (6.0mm inner diameter, 150mm length) connected together. Eluent: DMF (with 10 mmol / L lithium bromide added, and 30 mmol / L phosphoric acid added) Flow rate: 0.6mL / min Detector: RI detector Column temperature: 40℃ Injection volume: 20μL Molecular weight standard: Standard polystyrene
[0179] <Measurement of linear thermal expansion coefficient (CTE)> The CTE of the PI films obtained in the examples and comparative examples was measured using a TMA under the following conditions, and the CTE from 50°C to 100°C during the second heating cycle was calculated. Equipment: Hitachi High-Tech Science Co., Ltd. TMA / SS7100 Load: 50.0 mN Temperature program: Heat from 20°C to 130°C at a rate of 5°C / min, hold at 130°C for 30 minutes, then cool from 130°C to 20°C at a rate of 10°C / min, hold at 20°C for 10 minutes (1st cycle). Subsequently, heat from 20°C to 130°C at a rate of 5°C / min, hold at 130°C for 10 minutes, then cool from 130°C to 20°C at a rate of 5°C / min (2nd cycle). Test specimen: Rectangular parallelepiped, 40mm long, 5mm wide, and 50μm thick (thickness may vary depending on the film used). Experimental method: Tensile Atmosphere: The atmosphere is low.
[0180] <Evaluation of the dielectric loss index E> The dielectric loss index E of the PI films obtained in the examples and comparative examples was calculated using the following formula. E = Df × (Dk) 1 / 2 (i) Df: Dielectric loss tangent Dk: relative permittivity
[0181] (Measurement of Df and Dk) The Df and Dk values of the PI films obtained in the examples and comparative examples were measured under the following conditions. The samples were conditioned at 23°C / 50%RH for at least 24 hours before measurement. Equipment: Compact USB Vector Network Analyzer manufactured by Anritsu Corporation (Product name: MS46122B) Cavity resonator manufactured by AET Co., Ltd. (TE mode, 10GHz type) Measurement frequency: 10GHz Measurement environment: 23℃ / 50%RH
[0182] Table 1 shows the measurement and evaluation results for the PI films obtained in the examples and comparative examples.
[0183] [Table 1]
[0184] As shown in Table 1, the PI-based films obtained in Examples 1 to 6 were found to have lower Df and lower dielectric loss index E compared to Comparative Example 1. Therefore, the PI-based resin of the present invention can form PI-based films with low Df and low dielectric loss index E. [Explanation of symbols]
[0185] 1a, 1b, 1c... Test specimens for measurement 2a, 2b, 2c...X-ray source 3a, 3b, 3c...detector 4. Positions where the intensity is half of the minimum intensity in the range of 180-360°. Width of the peak at position 5...4 6. Sample holder 7....Line connecting the detection positions of 2b and 3b 8. Maximum diffraction intensity in the range of 2θ = 15.5~16.5° 9. Minimum diffraction intensity at θ = 20-30° Diffraction intensity at 10···0° Diffraction intensity at 11-90° Diffraction intensity at 12°–180° 13. Minimum value in the range of 0 to 360° Diffraction intensity at 14-270° 15···Maximum value in the range of 0 to 360° Diffraction intensity at 16-360°
Claims
1. A polyimide-based resin containing a structural unit (A) derived from a tetracarboxylic acid anhydride and a structural unit (B) derived from a diamine, The structural unit (A) derived from a tetracarboxylic acid anhydride includes a structural unit (A1) derived from an ester bond-containing tetracarboxylic acid anhydride and a structural unit (A2) derived from a biphenyl skeleton-containing tetracarboxylic acid anhydride, The diamine-derived structural unit (B) contains a biphenyl skeleton-containing diamine-derived structural unit (B1), the content of the structural unit (A1) is 15 to 75 mol % based on the total amount of the structural unit (A); the content of the structural unit (A2) is 25 to 85 mol % based on the total amount of the structural unit (A), the total content of the structural units (A1) and (A2) is 60 mol% or more based on the total amount of the structural units (A); The content of the structural unit (B1) is more than 30 mol% based on the total amount of the structural unit (B), The structural unit (A1) is represented by the formula (a1): [In formula (a1), R a1 each independently represents a halogen atom, an alkyl group, an alkoxy group, an aryl group, or an aryloxy group which may have a halogen atom; Each s is independently an integer of 0 to 3; Z is represented by formula (z1), formula (z2), or formula (z3): In formulae (z1) to (z3), R z11 to R z14 each independently represent a hydrogen atom or a monovalent hydrocarbon group which may have a halogen atom; R z2 each independently represent a monovalent hydrocarbon group which may have a halogen atom; n represents an integer of 2 to 4; j's each independently represent an integer from 0 to 3; * represents a bond. is a divalent organic group represented by the formula: The structural unit (a1) is derived from a tetracarboxylic acid anhydride represented by the following formula: The structural unit (B1) is represented by the formula (b1): In formula (b1), R b1 each independently represents a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms; p represents an integer of 0 to 4. The polyimide resin is a structural unit (b1) derived from a diamine represented by the following formula:
2. The structural unit (A2) is represented by the formula (a2): 【Chemistry 1】 [In formula (a2), R a2 each independently represents a halogen atom, an alkyl group, an alkoxy group, an aryl group, or an aryloxy group which may have a halogen atom; t's each independently represent an integer from 0 to 3.
2. The polyimide resin according to claim 1, wherein the structural unit (a2) is derived from a tetracarboxylic acid anhydride represented by the following formula:
3. The structural unit (B) is represented by the formula (b2): 【Chemistry 2】 [In formula (b2), R b2 each independently represents a halogen atom, an alkyl group, an alkoxy group, an aryl group, or an aryloxy group which may have a halogen atom; R b2 may be substituted with a halogen atom, Each W is independently -O-, -CH 2 --, --CH 2 -CH 2 -, -CH(CH 3 ) -, -C(CH 3 ) 2 -, -C(CF 3 ) 2 -, -COO-, -OOC-, -SO 2 -, -S-, -CO- or -N(R c )-, R c represents a monovalent hydrocarbon group having 1 to 12 carbon atoms which may be substituted with a hydrogen atom or a halogen atom, m represents an integer of 0 to 4; and q each independently represents an integer of 0 to 4. The polyimide resin according to claim 1 or 2, further comprising a structural unit (b2) derived from a diamine represented by the following formula:
4. In the structural unit (b2), m is 3, and each W is independently —O— or —C(CH 3 ) 2 The polyimide resin according to claim 3, wherein
5. The polyimide resin according to any one of claims 1 to 4, which has a glass transition temperature of 200 to 290°C.
6. A polyimide film comprising the polyimide resin according to any one of claims 1 to 5.
7. The polyimide-based film according to claim 6, having a dielectric loss tangent at 10 GHz of less than 0.
004.
8. The polyimide film according to claim 6 or 7, which has a thickness of 5 to 100 μm.
9. A laminated film comprising a copper foil layer on one or both sides of the polyimide film according to any one of claims 6 to 8.
10. A flexible printed circuit board comprising the polyimide film according to any one of claims 6 to 8.