Protective layer source

JP2023551406A5Inactive Publication Date: 2024-11-20APPLIED MATERIALS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023528983
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-11-19
Filing Date
2021-11-16
Publication Date
2024-11-20
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Current lithium-ion batteries face challenges with low energy capacity, limited charge/discharge cycles, and high internal resistance, necessitating faster charging, higher capacity, and reduced resistance for improved performance.

Method used

A roll-to-roll vacuum evaporation system for flexible substrates, utilizing electron beam sources and chemical vapor deposition to form multiple sacrificial and permanent anode layers, including lithium fluoride and lithium metal layers, to enhance anode structures in lithium-ion batteries.

Benefits of technology

The system enables high-quality anode prelithiation and protection, reducing electrochemical resistance, minimizing corrosion and oxidation, and improving coulombic efficiency, thus enhancing battery performance and cycling stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

A method, system, and apparatus for coating a flexible substrate are provided. The coating system includes a feed module housing a supply reel capable of providing a continuous sheet of flexible material, a take-up module housing a take-up reel capable of storing the continuous sheet of flexible material, and a processing module disposed downstream of the feed module. The processing module includes a plurality of sequentially arranged subchambers, each configured to perform one or more processing operations on the continuous sheet of flexible material. The processing module includes a coating drum capable of guiding the continuous sheet of flexible material through the plurality of subchambers along a moving direction. The subchambers are arranged radially around the coating drum, and at least one of the subchambers includes a deposition module. The deposition module includes a pair of electron beam sources positioned side-by-side along a transverse direction perpendicular to the moving direction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Field

[0001] Embodiments described herein generally relate to a vacuum deposition system and method for processing flexible substrates. More particularly, embodiments of the present disclosure relate to a roll-to-roll vacuum evaporation system and a method of forming at least two layers on a flexible substrate.

Background Art

[0002] Background Description of Related Art

[0002] Rechargeable electrochemical energy storage systems are becoming increasingly important in many areas of daily life. High-capacity energy storage devices such as lithium-ion (Li-ion) batteries and capacitors are increasingly being used in many applications including portable electronic devices, medical, transportation, grid-connected large-scale energy storage, renewable energy storage, and uninterruptible power supplies (UPS). In each of these applications, charge / discharge time and the capacity of the energy storage device are important parameters. Further, the size, weight, and / or cost of such energy storage devices are also important parameters. Additionally, low internal resistance is essential for high performance. The lower the resistance, the fewer the limitations encountered when the energy storage device supplies electrical energy. For example, in the case of a battery, the internal resistance affects performance by reducing the total amount of useful energy stored in the battery and the ability of the battery to supply a large current.

[0003]

[0003] Lithium-ion batteries are considered to have the highest potential for achieving the required capacity and cycles. However, currently configured lithium-ion batteries often lack the energy capacity and number of charge / discharge cycles for these growing applications.

[0004]

[0004] Therefore, in the art there is a need for energy storage devices that have improved cycles, can be manufactured more cost-effectively, are faster to charge, and have a larger capacity. There is also a need for components for energy storage devices that reduce the internal resistance of the storage device. [Overview of the project]

[0005]

[0005] Embodiments described herein generally relate to vacuum deposition systems and methods for processing flexible substrates. More specifically, embodiments of the present disclosure relate to roll-to-roll vacuum evaporation systems and methods for forming at least two layers on a flexible substrate.

[0006]

[0006] In one embodiment, a flexible substrate coating system is provided. The coating system includes a feed module housing a feed reel capable of providing a continuous sheet of flexible material. The coating system further includes a winding module housing a winding reel capable of storing the continuous sheet of flexible material. The coating system further includes a processing module arranged downstream of the feed module. The processing module includes a plurality of sequentially arranged sub-chambers, each sub-chamber configured to perform one or more processing operations on the continuous sheet of flexible material. The processing module further includes a coating drum capable of guiding the continuous sheet of flexible material through the plurality of sub-chambers along the direction of movement, the sub-chambers arranged radially around the coating drum, and at least one of the sub-chambers includes a deposition module. The deposition module includes a pair of electron beam sources positioned side by side along a transverse direction perpendicular to the direction of movement.

[0007]

[0007] The implementation may include one or more of the following: The deposition module is defined by a sub-chamber body having an edge shield positioned above the sub-chamber body. The edge shield has one or more openings defining a pattern of evaporated material to be deposited on a continuous sheet of flexible material. The edge shield has at least two openings, the first opening defining a first strip of the deposited material and the second opening defining a second strip of the deposited material. Each electron beam source includes an electron gun and at least one crucible capable of holding the evaporable material. The electron gun is operable to emit an electron beam toward the evaporable material placed in the crucible. Each electron beam source further includes an electron gun steering that can direct the electron beam of the electron gun from the evaporable material toward the continuous sheet of flexible material for electron irradiation of the deposited material toward the continuous sheet of flexible material. The deposition module further includes a photodetector positioned to monitor the plume of evaporated material emitted from the electron beam source. A photodetector is configured to perform emission spectroscopy to measure the intensity of one or more wavelengths of light associated with the plume of evaporated material. A pair of electron beam sources are configured to deposit a lithium fluoride film on a continuous sheet of flexible material. Multiple subchambers further include a first subchamber containing a sputtering source, the first subchamber being positioned upstream of the subchamber containing the deposition module. The sputtering source is configured to deposit at least one of aluminum, nickel, copper, alumina (Al2O3), boron nitride (BN), carbon, silicon oxide, or a combination thereof. The subchamber containing the deposition module further includes a second subchamber containing a thermal evaporation source. The thermal evaporation source is configured to deposit lithium metal. Multiple subchambers further include a third subchamber containing a second deposition module, similar to the deposition module and positioned downstream of the subchamber containing the deposition module. The second deposition module is configured to deposit lithium fluoride. The third sub-chamber further includes a fourth sub-chamber containing an organic thermal evaporation source.The coating system further includes a chemical vapor deposition (CVD) module positioned between the processing module and the winding module. The CVD module includes a multizone gas distribution assembly. The multizone gas distribution assembly is fluidically connected to a first gas source. The first gas source contains titanium tetrachloride (TiCl4), boron phosphate (BPO), and TiCl4(HSR)2(R=C6H). 11 The multizone gas distribution assembly is configured to supply at least one of the following: C5H9, or a combination thereof. The multizone gas distribution assembly is fluidically connected to a second gas source. The second gas source is configured to supply at least one of the following: hydrogen sulfide (H2S), carbon dioxide (CO2), perfluorodecyltrilorosilane (FDTS), and polyethylene glycol (PEG).

[0008]

[0008] In another embodiment, a method is provided for forming a pre-lithiated anode structure. The method comprises depositing a first sacrificial anode layer on a prefabricated electrode structure. The prefabricated electrode structure comprises a continuous sheet of flexible material coated with an anode material. The method further comprises depositing a second sacrificial anode layer on the first sacrificial anode layer. The method further comprises depositing a third sacrificial anode layer on the second sacrificial anode layer. The method further comprises densifying at least one of the first sacrificial anode layer, the second sacrificial anode layer, and the third sacrificial anode layer by exposing the sacrificial anode layer to an electron beam from a pair of electron beam sources.

[0009]

[0009] The implementation may include one or more of the following: The anode material is selected from graphite anode material, silicon anode material, or silicon-graphite anode material. The first sacrificial anode layer functions as a corrosion barrier that minimizes the electrochemical resistance between the anode material and / or the substrate and the second sacrificial anode layer. The first sacrificial anode layer includes a binary lithium compound, a ternary lithium compound, or a combination thereof. The first sacrificial anode layer is deposited using an electron beam evaporation source. The first sacrificial anode material layer 420 is a lithium fluoride layer. The second sacrificial anode material layer functions as a pre-lithification layer that supplies lithium to pre-lithify the prefabricated electrode structure. The second sacrificial anode layer is a lithium metal layer. The sacrificial anode layer of base 3 functions as an oxidation barrier that minimizes the electrochemical resistance between the lithium metal layer and the electrolyte deposited thereafter. The third sacrificial anode layer includes a binary lithium compound, a ternary lithium compound, a sulfide compound, an oxide combination, or a combination thereof. The third sacrificial anode layer is a lithium fluoride layer. A fourth sacrificial layer is deposited on the third sacrificial anode layer, and the fourth sacrificial layer functions as a wetting layer. The fourth sacrificial anode layer contains polymer materials selected from polymethyl methacrylate, polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride, poly(vinylidene fluoride)-co-hexafluoropropylene, polypropylene, nylon, polyamide, polytetrafluoroethylene, polychlorotrifluoroethylene, polyterephthalate, silicone, silicone rubber, polyurethane, cellulose acetate, polystyrene, poly(dimethylsiloxane), or any combination thereof.

[0010]

[0010] In yet another embodiment, a method for forming an anode structure is provided. The method comprises depositing a first persistent anode layer on a continuous sheet of flexible material. The method further comprises depositing a second persistent anode layer on the first persistent lithium anode layer. The method further comprises depositing a third persistent anode layer on the second persistent anode layer, the third persistent anode layer being a lithium metal layer. The method further comprises densifying at least one of the first persistent lithium anode layer, the second persistent anode layer, and the third persistent anode layer by exposure to electron beams from a pair of electron beam sources.

[0011]

[0011] The implementation may include one or more of the following: A first persistent anode layer functions as a corrosion barrier that minimizes electrochemical resistance between a continuous sheet of flexible material and a second persistent anode layer. The first persistent anode layer includes a first persistent anode material layer containing aluminum, nickel, copper, alumina (Al2O3), boron nitride (BN), carbon, silicon oxide, or a combination thereof. The first persistent anode layer is deposited using a sputtering source. A second persistent anode layer functions as a corrosion barrier that minimizes electrochemical resistance between a continuous sheet of flexible material and a third persistent anode layer. The second persistent anode layer includes a binary lithium compound, a ternary lithium compound, or a combination thereof. The second persistent anode layer is deposited using an electron beam evaporation source. The second persistent anode layer is a lithium fluoride layer.

[0012]

[0012] In yet another embodiment, a non-temporary computer-readable medium stores instructions that, when executed by a processor, cause a process to perform the operation of the above-described apparatus and / or method.

[0013]

[0013] To enable a detailed understanding of the above-mentioned features of this disclosure, a more specific description of the implementations briefly summarized above can be obtained by referring to the implementations, some of which are shown in the accompanying drawings. However, it should be noted that since this disclosure may also permit other equally valid embodiments, the accompanying drawings show only typical embodiments of this disclosure and should therefore not be considered to limit the scope of this disclosure. [Brief explanation of the drawing]

[0014] [Figure 1]

[0014] A schematic side view of a vacuum processing system according to one or more embodiments of the present disclosure is shown. [Figure 2]

[0015] A schematic diagram of a deposition module including an electron beam deposition source according to one or more embodiments of the present disclosure is shown. [Figure 3]

[0016] Figure 3 shows a flowchart summarizing one embodiment of a method for forming an anode structure according to one or more embodiments of the present disclosure. [Figure 4]

[0017] A schematic cross-sectional view of an anode electrode structure formed according to one or more embodiments of the present disclosure is shown. [Figure 5]

[0018] A flowchart summarizing one embodiment of a method for forming an anode structure according to one or more embodiments of the present disclosure is shown. [Figure 6]

[0019] A schematic cross-sectional view of yet another anode electrode structure formed according to one or more embodiments of the present disclosure is shown. [Modes for carrying out the invention]

[0015]

[0020] To facilitate understanding, the same symbols were used to indicate the same elements common to multiple figures where possible. It is assumed that elements and functions of one implementation can be beneficially incorporated into other implementations without further explanation.

[0016]

[0021] The following disclosure describes a roll-to-roll vacuum deposition system and a method of forming at least two layers on a flexible substrate. To provide a complete understanding of the various implementations of the present disclosure, specific details are set forth in the following description and in FIGS. 1-6. Other details that often pertain to well-known structures and systems associated with web coating, electrochemical cells, and secondary batteries are not described in the following disclosure to avoid unnecessarily obscuring the description of the various implementations.

[0017]

[0022] Many of the details, dimensions, angles, and other features shown in the figures are merely illustrative of particular implementations. Accordingly, other embodiments can have other details, components, dimensions, angles, and features without departing from the spirit and scope of the present disclosure. Further, additional implementations of the present disclosure can be implemented without using some of the details described below.

[0018]

[0023] The embodiments described herein are explained below with reference to a roll-to-roll coating system. The description of the devices described herein is exemplary and should not be understood or construed as limiting the scope of the implementations described herein. Also, although described as a roll-to-roll process, it should be understood that the implementations described herein can be performed on individual substrates.

[0019]

[0024] Energy storage devices, such as batteries, typically consist of a cathode, an anode electrode separated by a porous separator, and an electrolyte used as an ion-conductive matrix. Graphite anodes are current state-of-the-art, but the industry is moving from graphite-based anodes to silicon-blended graphite anodes to increase the energy density of the cell. However, silicon-blended graphite anodes often suffer from irreversible capacity loss that occurs during the first cycle. Therefore, a method for replenishing this first-cycle capacity loss is needed.

[0020]

[0025] The deposition of lithium metal is one such method to replenish this first cycle capacity loss of graphite and silicon mixed graphite anodes. There are numerous methods for depositing lithium metal (such as thermal evaporation, lamination, printing, etc.), but especially in high-volume production environments, it is necessary to address the handling of lithium metal deposited on spools prior to device stacking. To address these handling issues, anode web coatings often include a thin protective layer coating. Without the protective layer coating, the lithium metal surface is prone to harmful corrosion and oxidation. Lithium carbonate (Li2CO3) film is currently used as a protective layer coating for lithium. However, there are several issues with the lithium carbonate protective layer. For example, the carbonate coating consumes lithium, increasing the amount of "dead lithium" and accordingly reducing the Coulombic efficiency of the formed device. In current lithium carbonate deposition processes, lithium oxide, an undesirable SEI component rather than lithium carbonate, may be formed. Furthermore, the carbonate coating is difficult to activate due to the slow adsorption rate of carbonate, which can cause significant variations in the coating uniformity of the carbonate coating in both the vertical and horizontal directions. Additionally, CO2 adsorption lacks scalability in the line of sight, making it an inappropriate process for most high-volume protective layer coatings, including both sacrificial and protective applications.

[0021]

[0026] Vacuum web coating for pre-lithiation of anodes and protection of solid metal anodes includes the deposition of thick (3 - 20 microns) metallic lithium on both sides coated surfaces, and a calendared alloy type graphite anode and current collector, such as a copper foil, nickel foil, or metallized plastic web with a thickness of 6 microns or more. The pre-lithiation and solid metal anode web coating further includes, for example, a thin protective layer coating less than 1 micron. Without the protective layer coating, the surface of metallic lithium (by thermal evaporation or rolled foil) is prone to harmful corrosion and oxidation.

[0022]

[0027] Impurities in the substrate can react with lithium, potentially causing undesirable lithium corrosion. For example, alloy-type graphite anodes contain trace levels (>10 ppm) of residual moisture (O2 and H2O), which can be released during physical vapor deposition (PVD). This residual moisture trapped between the graphite anode and the metallic lithium coating can increase the electrochemical resistance of the interface (via the formation of lithium oxide). Vacuum degassing is operationally cumbersome due to the slow diffusion of trapped residual moisture. While not bound by theory, the controlled deposition of nanoscale (less than 100 nanometers thick) electrochemically active binary or ternary lithium compounds described herein is thought to act as a corrosion barrier between alloy-type graphite anodes, allowing metallic lithium to improve anode quality without significantly impacting ownership costs due to additional chemical costs. In the case of solid metal anodes, some copper foils contain trace amounts of antioxidants and other residual by-products from electrodeposition or rolling, which can react with lithium and cause undesirable lithium corrosion. While not bound by theory, the controlled deposition of nanoscale (less than 100 nanometers thick) electrochemically active binary or ternary lithium compounds described herein is thought to minimize lithium corrosion and lithium cracking along copper grain boundaries. Furthermore, for large-scale scaling, additional coating is considered a preferred approach rather than, for example, wet cleaning.

[0023]

[0028] Oxygen, nitrogen, and hydrogen (ONH) react with lithium during web unloading and cell assembly in a dry room environment to form an electrochemical insulating layer of lithium oxide on the newly deposited metallic lithium. While not bound by theory, the aforementioned binary and ternary lithium compounds, used as corrosion barriers between the substrate and lithium, are thought to also function as oxidation barriers between lithium and the environment, minimizing reactivity with air. In addition to lithium compounds, this disclosure has devised CVD hardware and methods for applying titanium disulfide and other reactive films via single and dual precursor chemical pathways. The aforementioned CVD hardware can also deposit conventional dry carbon dioxide.

[0024]

[0029] In some embodiments, methods and systems for forming lithium anode devices are provided. In some embodiments, a premetallation film stack containing metallic lithium metal sandwiched between a corrosion barrier and an oxidation barrier is produced using CVD and PVD modules described herein. The film stack can be adapted, in particular, for prelithiation of anodes in continuous lithium-ion batteries ("LIBs"), electric vehicles ("EVs"), for solid metal anode protection in household electrical appliances ("CEs"), or for manufacturing thin lithium tapes for consumables.

[0025]

[0030] In some embodiments, pre-lithiumated film stacks and methods for producing pre-lithiumated film stacks are provided. The pre-lithiumated film stack comprises a graphite-containing anode film (any binary or ternary lithium corrosion barrier film) (a lithium film formed by evaporation) and a binary or ternary lithium oxide barrier or sulfide or oxide barrier film.

[0026]

[0031] In another embodiment, a metal anode film stack and a method for manufacturing a metal anode film stack are provided. The metal anode film stack includes a metal current collector / a binary or ternary lithium corrosion barrier / a lithium metal anode film by deposition / and a binary or ternary lithium oxide barrier film.

[0027]

[0032] In yet another embodiment, a lithium transfer foil and a method for manufacturing the lithium transfer foil are provided. The lithium transfer foil comprises a carrier substrate / a binary or ternary lithium oxide barrier / a lithium film of less than 20 microns formed by evaporation / and a binary or ternary lithium oxide barrier.

[0028]

[0033] In some embodiments, the PVD and CVD modules described herein can be integrated into conventional vacuum web coaters and other lithium-ion battery chemical reactions that are typically unsuitable for toxic and spontaneously combustible precursors such as lithium fluoride (solid) and hydrogen disulfide (gaseous). In some embodiments, the PVD modules described herein utilize a transverse array of electron beam guns for crucible evaporation and post-treatment electron web irradiation to increase coating density or adjust coating composition. The PVD modules described herein can further deposit lithium and lithium compounds alone or in co-deposition mode. The CVD modules described herein enable dual-source and single-source precursors for conventional dry carbon dioxide gas treatment or low-temperature (<200°C) organic thiol-based titanium disulfide deposition.

[0029]

[0034] In some embodiments, the PVD and CVD modules described herein enable premetallation and the deposition of a corresponding protective layer for depositing a metallic lithium reservoir specific to cell and battery applications, which is either (1) sacrificial in that the anode coating is completely consumed after the first charge cycle, or (2) permanent in that the anode coating remains after the first charge cycle. The ability to control and accurately supply stable, electrochemically active lithium to the cell during electrolyte filling and SEI formation, and further prevent the conversion of metallic lithium to lithium oxide or other harmful compounds, facilitates high-quality, high-yield anode prelithiation and anode protective layer deposition. Controlled prelithiation of alloy-type anodes improves the Coulomb efficiency of lithium-ion batteries. Anode coatings with pinhole-free, electrochemically active protective layers prevent dendritic crystal formation.

[0030]

[0035] In some embodiments, CVD is used for the sacrificial protective layer and PVD for the permanent protective layer. In some embodiments, the PVD modules described herein, which house two materials in one standard web compartment, enable reactive alloying by co-deposition. The flexibility provided by non-standard chemicals and unconventional CVD and PVD source combinations allows for the effective modification of conventional web coaters to serve the business models of captive anode manufacturing and tool coating.

[0031]

[0036] In some embodiments, a hybrid PVD source is provided. The hybrid PVD source includes a resistance heating crucible and an electron beam heating crucible in a shared compartment. By positioning the two PVD sources in a shared compartment, the latency between the deposition of the lithium film and the protective layer on top is minimized. Both the lithium film and the protective layer on top can be deposited individually in two passes within a single compartment, or simultaneously in a single pass.

[0032]

[0037] Lithium metal deposited on one or both sides using the implementation described herein can be protected during winding and unwinding of downstream reels. The deposition of the protective film described herein offers several potential advantages. Firstly, reels containing lithium metal electrodes can be wound and unwound without the lithium metal touching adjacent electrodes. Secondly, a stable solid electrolyte interface (SEI) can be established to improve battery performance and enable high electrochemical utilization of lithium metal. The protective layer also helps to suppress or remove lithium dendrites, particularly during high current density operation. Furthermore, the use of the protective film reduces the complexity of the manufacturing system and ensures compatibility with existing manufacturing systems.

[0033]

[0038] As explained here, binary lithium compounds are not limited to these, but include lithium bismuth (Li3Bi), lithium carbonate (Li2CO3), lithium fluoride (LiF), lithium indium (Li13In3), lithium nitride (Li3N), lithium oxide (Li2O), lithium sulfide (Li2S), and lithium tin (Li 4.4 Sn), lithium phosphide (Li3P), lithium tin-phosphorus sulfide (Li 10 SnP2S 12 ), or combinations thereof.

[0034]

[0039] As explained here, ternary lithium compounds are not limited to these, but include lithium phosphate (Li3PO4), lithium thiophosphate (LPS; β-Li3PS4), and lithium spinel titanate (LTO; Li4Ti5O4). 12 ), including ternary lithium oxide, ternary lithium nitride, or combinations thereof.

[0035]

[0040] When used herein, the sacrificial film is designed to be consumed or destroyed for protective purposes before the first charge of the completed battery incorporating the anode structure, or while performing its function.

[0036]

[0041] When used herein, the persistent film is designed to provide one or more functions after the initial charge of a completed battery incorporating an anode structure.

[0037]

[0042] While the specific substrates on which some of the implementations described herein can be carried out are not limited, it should be noted that implementations are particularly beneficial on flexible substrates, including, for example, web-based substrates, panels, and individual sheets. The substrate may be in the form of foil, film, or sheet.

[0038]

[0043] It should also be noted that the flexible substrates or webs used in the embodiments described herein may typically be characterized by their flexibility. The term "web" can be used synonymously with the terms "strip" or "flexible substrate." For example, the webs described in the embodiments herein may be foils.

[0039]

[0044] It should be further noted that in some mounting configurations where the substrate is vertically oriented, the vertically oriented substrate can be angled with respect to the vertical plane. For example, in some embodiments, the substrate can be angled between approximately 1 and 20 degrees from the vertical plane. In some mounting configurations where the substrate is horizontally oriented, the horizontally oriented substrate can be angled with respect to the horizontal plane. For example, in some embodiments, the substrate can be angled between approximately 1 and 20 degrees from the horizontal plane. As used herein, the term “vertical” is defined as the principal or deposition surface of a flexible conductive substrate being perpendicular to the horizon. As used herein, the term “horizontal” is defined as the principal or deposition surface of a flexible conductive substrate being parallel to the horizon.

[0040]

[0045] It should be further noted that in this disclosure, “roll” or “roller” can be understood as a device that provides a surface to which a substrate (or a portion of a substrate) can make contact while the substrate is present in a processing system. At least some of the “roll” or “roller” referred to herein may include a circular shape for contacting the substrate being processed or a substrate that has already been processed. In some embodiments, the “roll” or “roller” may have a cylindrical or substantially cylindrical shape. A substantially cylindrical shape may be formed around a straight longitudinal axis or around a curved longitudinal axis. According to some embodiments, the “roll” or “roller” described herein may be adapted to make contact with a flexible substrate. For example, the “rolls” or “rollers” referred to herein may include guide rollers adapted to guide the substrate while the substrate is being processed (e.g., during a deposition process) or while the substrate is present in the processing system, spreader rollers adapted to apply a specified tension to the substrate to be coated, deflection rollers to deflect the substrate according to a defined movement path, processing rollers for supporting the substrate during processing, such as processing drums, coating rollers or coating drums, adjustment rollers, supply rolls, winding rolls, etc. The “rolls” or “rollers” described herein may include metal. In some embodiments, the surface of the roller device in contact with the substrate can be adapted to each substrate to be coated. Furthermore, according to some embodiments, the rollers described herein can be mounted on low-friction roller bearings, particularly those with a double-bearing roller structure. Thus, parallelism of the rollers in the transport device described herein can be achieved, and transverse “wobbling” of the substrate during substrate transport can be eliminated.

[0041]

[0046] Figure 1 shows a schematic side view of a flexible substrate coating system 100 according to one or more embodiments of the present disclosure. The flexible substrate coating system 100 may be an Applied Materials SMARTWEB® system adapted for manufacturing lithium-containing anode film stacks according to embodiments described herein. The flexible substrate coating system 100 can be used to manufacture lithium-containing anodes, in particular film stacks for lithium-containing anodes. The flexible substrate coating system 100 includes a common processing environment 101 on which some or all of the processing operations for manufacturing lithium-containing anodes can be performed. In one or more examples, the common processing environment 101 can operate as a reduced-pressure environment. In other examples, the common processing environment 101 can operate as an inert gas environment.

[0042]

[0047] The flexible substrate coating system 100 is configured as a roll-to-roll system including a feed module 102, a processing module 104, an optional chemical vapor deposition (CVD) module 106, and a winding module 108. The processing module 104 includes a chamber body 105 that defines a common processing environment 101.

[0043]

[0048] In some implementations, the processing module 104 includes a series of sequentially arranged processing modules or subchambers 110, 120, and 130, each configured to perform a single processing operation on a continuous sheet 150 of flexible material or a material web. In one or more examples, as shown in Figure 1, the subchambers 110-130 are arranged radially around the coating drum 155. The subchambers 110-130 are separated by partitions 112a-112d (collectively referred to as 112). For example, the first subchamber 110 is defined by partitions 112a and 112b, the second subchamber 120 is defined by partitions 112b and 112c, and the third subchamber 130 is defined by partitions 112c and 112d. In one or more examples, the subchambers 110-130 are closed off by partitions 112 except for a narrow, arc-shaped gap. Although the first sub-chamber 110 is shown to have a single sediment source 113, each sub-chamber 110-130 can be divided into two or more compartments, each containing a separate sediment source.

[0044]

[0049] In one implementation configuration as shown in Figure 1, the second sub-chamber 120 is divided into a first section 122 and a second section 124, each containing a deposition source 126 and 128, respectively, and the third sub-chamber 130 is divided into a third section 132 and a fourth section 134, each containing a deposition source 136 and 138. The sections can be closed or isolated from adjacent sections, except for narrow openings that allow deposition onto the coating drum 155. At least one of the deposition sources 113, 126, 128, 136, and 138 includes an electron beam gun. Furthermore, arrangements other than radial are also possible. For example, in another embodiment, the sub-chambers 110-130 can be positioned in a linear configuration.

[0045]

[0050] In some implementations, subchambers 1110 to 130 are independent modular subchambers, and each modular processing chamber is structurally isolated from the other modular subchambers. Therefore, each independent modular subchamber can be arranged, rearranged, replaced, or maintained independently without affecting each other. While three subchambers 110-130 are shown, it should be understood that the flexible substrate coating system 100 can contain any number of subchambers.

[0046]

[0051] The subchambers 110-130 may include any suitable structure, configuration, arrangement, and / or components that enable the flexible substrate coating system 100 to deposit lithium-containing anode film stacks, according to embodiments of the present disclosure. For example, but not limited to these, the subchambers may include a suitable deposition system including a coating source, power supply, individual pressure control, deposition control system, and temperature control. In some embodiments, the subchambers are provided with separate gas supplies. As described herein, the subchambers 110-130 are typically separated from each other to provide good gas separation. The flexible substrate coating system 100 described herein is not limited to the number of subchambers. For example, the flexible substrate coating system 100 may include, but is not limited to, three, six, or twelve subchambers.

[0047]

[0052] Subchambers 110-130 typically include one or more deposition sources 113, 126, 128, 136, and 138. Generally, one or more deposition sources described herein include an electron beam source and additional sources which can be selected from a group of CVD sources, PECVD sources, and various PVD sources. Electron beam sources are described in detail in Figure 2. One or more deposition sources 113, 126, 128, 136, and 138 may include one or more evaporation sources. Examples of evaporation sources include thermal evaporation sources and electron beam evaporation sources. In one or more examples, the evaporation source is a thermal evaporation source and / or an electron beam evaporation source. In some embodiments, the evaporation source is a lithium (Li) source. Furthermore, the evaporation source may also be an alloy of two or more metals. The material to be deposited (e.g., lithium fluoride) may be provided in a crucible. For example, aluminum may be evaporated by thermal evaporation technique or by electron beam evaporation technique.

[0048]

[0053] One or more deposition sources 113, 126, 128, 136, and 138 may include one or more sputtering sources. Examples of sputtering sources include magnetron sputtering sources, DC sputtering sources, AC sputtering sources, pulsed sputtering sources, radio frequency (RF) sputtering sources, or intermediate frequency (MF) sputtering sources. For example, MF sputtering with frequencies in the range of 5 kHz to 100 kHz, e.g., 30 kHz to 50 kHz, can be provided. As used herein, “magnetron sputtering” refers to sputtering performed using a magnetic assembly, i.e., a unit capable of generating a magnetic field. Typically, such a magnetic assembly includes permanent magnets. These permanent magnets are usually arranged within a rotating target or coupled to a planar target so that free electrons are trapped in a generated magnetic field produced beneath the rotating target surface. Such a magnetic assembly may also be arranged coupled to a planar cathode.

[0049]

[0054] In one or more examples, deposition source 113 is a sputtering source, deposition source 126 is an electron beam evaporation source, deposition source 128 is a thermal evaporation source, deposition source 136 is an electron beam evaporation source, and deposition source 138 is an organic thermal evaporation source.

[0050]

[0055] In some implementations, the CVD module 106 is positioned between the processing module 104 and the winding module 108, for example, upstream of the winding module 108 and downstream of the processing module 104. In some implementations, the CVD module 106 includes a processing area 170. The processing area 170 includes one or more deposition sources 172 for introducing a processing gas into the CVD module 106. In some implementations where double-sided coating is performed, the CVD module 106 includes an additional deposition source positioned to deposit material on the opposite side of a continuous sheet 150 of flexible material. In one or more examples, the deposition source 172 is a multizone gas distribution assembly or showerhead. The processing area 170 may include one or more electrodes for forming in-situ plasma within the CVD module 106. The processing area 170 can be coupled with a remote plasma source for supplying remote plasma to the processing area 170.

[0051]

[0056] In some embodiments, subchambers 110-130 are configured to process both sides of a continuous sheet 150 of flexible material. The flexible substrate coating system 100 is configured to process a continuous sheet of flexible material 150 oriented horizontally, but the flexible substrate coating system 100 can be configured to process substrates arranged in different orientations, for example, the continuous sheet of flexible material 150 can be oriented vertically. In some embodiments, the continuous sheet of flexible material 150 is a flexible conductive substrate. In some embodiments, the continuous sheet of flexible material 150 includes a conductive substrate having one or more layers formed thereon. In some embodiments, the conductive substrate is a copper substrate.

[0052]

[0057] In some embodiments, the flexible substrate coating system 100 includes a substrate transport device 152. The substrate transport device 152 may include any transport mechanism that can move a continuous sheet 150 of flexible material through processing areas of sub-chambers 110-130. The substrate transport device 152 may include a reel-to-reel system with a common take-up reel 154 located in a winding module 108, a coating drum 155 located in a processing module 104, and a supply reel 156 located in a dispensing module 102. The take-up reel 154, the coating drum 155, and the supply reel 156 can be heated individually. The take-up reel 154, the coating drum 155, and the supply reel 156 can be heated individually using an internal or external heat source located within each reel. The substrate transport device 152 may further include one or more auxiliary transport reels 153a, 153b positioned between the take-up reel 154, the coating drum 155, and the supply reel 156. According to one embodiment, at least one of the one or more auxiliary transfer reels 153a, 153b, winding reel 154, coating drum 155, and supply reel 156 can be driven and rotated by a motor.

[0053]

[0058] The flexible substrate coating system 100 includes a feed reel 156 and a take-up reel 154 for moving a continuous sheet of flexible material 150 through different sub-chambers 110-130. In some embodiments, the deposition source 113 of the first sub-chamber 110 includes a sputtering source configured to deposit a first layer on the continuous metal sheet 150 of flexible material. In one or more examples, the deposition source 113 is a sputtering source configured to deposit at least one of aluminum, nickel, copper, alumina (Al2O3), boron nitride (BN), carbon, silicon oxide, or a combination thereof. While not bound by theory, the first layer is thought to minimize corrosion and reduce bagginess of the underlying continuous metal sheet 150 of flexible material.

[0054]

[0059] The second sub-chamber 120 can be configured to deposit any of the binary, ternary, or polymer films described herein. In some embodiments, a deposition source 126 located in the first compartment 122 of the second sub-chamber 120 is an evaporation source configured to deposit a second layer on top of a first layer. In one or more examples, the deposition source 126 is an electron beam evaporation source, e.g., an electron beam evaporation source 210, configured to deposit a first lithium fluoride layer. In other examples, the deposition source 126 is an organic thermal evaporation source configured to deposit any of the polymer materials described herein. The second compartment 124 of the second sub-chamber 120 includes a deposition source 128 configured to deposit a third layer on top of a second layer. In one or more examples, the deposition source 128 is a thermal evaporation source configured to deposit a lithium metal layer. In other examples, the deposition source 128 is an organic thermal evaporation source configured to deposit any of the polymer materials described herein.

[0055]

[0060] The third sub-chamber 130 can be configured to deposit any of the binary, ternary, or polymer films described herein. In some implementations, the third compartment 132 of the third sub-chamber 130 includes a deposition source 136, which is a third evaporation source configured to deposit a fourth layer on top of the third layer. In one or more examples, the deposition source 136 is an electron beam evaporation source, e.g., an electron beam evaporation source 210, configured to deposit a second lithium fluoride layer. In other examples, the deposition source 136 is an organic thermal evaporation source configured to deposit any of the polymer materials described herein. The fourth compartment 134 of the third sub-chamber 130 includes a deposition source 138, which may be a fourth evaporation source configured to deposit a fifth layer on top of the fourth layer. In one or more examples, the deposition source 138 is an electron beam evaporation source configured to deposit a second lithium fluoride layer. In another example, the deposition source 138 is an organic thermal evaporation source configured to deposit one of the polymer materials described herein.

[0056]

[0061] The CVD module 106 can be configured to deposit any of the binary, ternary, or polymer films described herein. Furthermore, the CVD module can be configured to deposit metal sulfides, such as titanium disulfide (TiS2). In some implementations, the CVD module 106 is configured to deposit titanium tetrachloride (TiCl4), boron phosphate (BPO), and TiCl4(HSR)2 (wherein R=C6H 11 The CVD module 106 includes a first gas source 174 configured to supply at least one of the following: hydrogen sulfide (H2S), carbon dioxide (CO2), perfluorodecyltrichlorosilane (FDTS), and polyethylene glycol (PEG). The titanium disulfide film is conductive, typically has a high lithium diffusion coefficient at ambient temperature, and exhibits reversible lithium intercalation even after numerous discharge cycles. In some embodiments, the titanium disulfide film is prepared by a CVD process using titanium tetrachloride and organothiols. In one or more examples, titanium disulfide is prepared by treating titanium tetrachloride with an alkanethiol in hexane at ambient temperature. In other examples, the titanium disulfide film is produced at low pressure (0.1 mmHg) in a heated reaction zone within a temperature range of 200°C to 600°C.

[0057]

[0062] During operation, the continuous sheet 150 of flexible material is unwound from the supply reel 156 as indicated by the substrate movement direction indicated by arrow 109. The continuous sheet 150 of flexible material can be guided via one or more auxiliary transfer reels 153a, 153b. The continuous sheet 150 of flexible material can also be guided by one or more substrate guide control units (not shown) that control the proper movement of the continuous sheet 150 of flexible material, for example, by fine-tuning the orientation of the continuous sheet 150 of flexible material.

[0058]

[0063] After being unwound from the supply reel 156 and traveling on the auxiliary transfer reel 153a, the continuous sheet 150 of flexible material is then placed on the coating drum 155 and moved through the loading areas corresponding to the locations of one or more loading sources 113, 126, 128, 136, 138, and 172. During operation, the coating drum 155 rotates around the axis 151 so that the flexible substrate moves in the direction indicated by the arrow 109.

[0059]

[0064] The flexible substrate coating system 100 further includes a system controller 160 that can operate to control various aspects of the flexible substrate coating system 100. The system controller 160 facilitates the control and automation of the flexible substrate coating system 100 and may include a central processing unit (CPU), memory, and support circuits (or I / O). Software instructions and data can be coded and stored in memory to instruct the CPU. The system controller 160 can communicate with one or more components of the flexible substrate coating system 100, for example, via a system bus. A program (or computer instructions) readable by the system controller 160 determines which tasks can be performed on the substrate. In some aspects, the program is software readable by the system controller 160 and may include code to control the removal and replacement of multi-segment rings. Although shown as a single system controller 160, it should be understood that multiple system controllers can be used with the aspects described herein.

[0060]

[0065] Figure 2 shows a schematic diagram of a deposition module 200 comprising a pair of electron beam evaporation sources 210a, 210b (collectively 210) according to one or more embodiments of the present disclosure. The deposition module 200 can be used in a flexible substrate coating system 100. In some embodiments, the deposition module 200 replaces one of the compartments 122, 124, 132, and 134 located within the flexible substrate coating system 100. In one or more examples, the deposition module 200 replaces the first compartment 122 and the third compartment 132. The deposition module 200 is shown adjacent to a coating drum 155 of the flexible substrate coating system 100, which has a continuous sheet 150 of flexible material placed thereon. Although shown as part of the flexible substrate coating system 100, the deposition module can also be used with other coating systems.

[0061]

[0066] The deposition module 200 is defined by the sub-chamber body 220 with an edge shield 230 or a mask positioned on the sub-chamber body 220. The edge shield 230 includes one or more openings 232a, 232b (collectively 232) which define the pattern of the evaporated material deposited on the continuous sheet 150 of the flexible material. In one or more examples, the edge shield 230 includes two openings. As shown in Figure 2, the edge shield 230 defines the pattern of the material 240 deposited on the continuous sheet 150 of the flexible material. The patterned film 240 of the deposited material includes a first strip 242a of the deposited material and a second strip 242b of the deposited material, both extending in the substrate movement direction indicated by arrow 109 on the continuous sheet 150 of the flexible material. The edge shield 230 leaves an uncoated strip along the near edge 243 of the continuous sheet 150 of the flexible material, an uncoated strip along the far edge 245 of the continuous sheet 150 of the flexible material, and an uncoated strip 247 defined between the first strip 242a and the second strip 242b of the deposited material. In one or more examples, the edge shield 230 includes two openings 232a, 232b, where the first opening 232a defines the first strip 242a of the deposited material and the second opening 232b defines the second strip 242b of the deposited material.

[0062]

[0067] Each electron beam evaporation source 210a, 210b (collectively 210) includes at least one crucible 212a, 212b (collectively 212) and an electron gun 214a, 214b (collectively 214). The crucible 212 holds the evaporable material. The electron gun 214 is operable to emit an electron beam toward the evaporable material positioned within the crucible 212. During operation, electron beams 216a, 216b (collectively 216) from the electron gun 214 are directed toward the evaporable material. The material is heated and evaporated. The plume of evaporated material 218a, 218b (collectively 218) is attracted to a continuous sheet 150 of flexible material, where a patterned film 240 of the deposited material is formed on the continuous sheet 150 of flexible material.

[0063]

[0068] Electron guns 214a and 214b are also operable to emit electron beams toward the deposited film on the continuous sheet 150 of flexible material. For example, electron gun steering can direct the electron beams of electron guns 214a and 214b from the evaporative material toward the continuous sheet 150 of flexible material for electron irradiation of the deposited material on the continuous sheet 150 of flexible material. This electron irradiation can increase the density of the deposited film by direct heating.

[0064]

[0069] The electron guns 214a and 214b can be instantly switched on / off without any waiting time, providing better control over film deposition and patterning. The electron guns 214a and 214b can typically deposit higher quality materials than their resistance-heated counterparts. Furthermore, the electron guns 214a and 214b can vaporize solids, liquids, and / or powders, enabling the deposition of a variety of films.

[0065]

[0070] The electron beam evaporation sources 210a and 210b are positioned side by side along the transverse direction indicated by arrow 250, which is perpendicular to the direction of movement indicated by arrow 109. Positioning the electron beam evaporation sources 210a and 210b along the transverse direction makes the strip coating pattern shown in Figure 2 possible.

[0066]

[0071] In some embodiments, the deposition module 200 further includes photodetectors 260a, 260b (collectively 260). The photodetectors 260 can be mounted on the wall of the sub-chamber body 220. The photodetectors 260 can be positioned to monitor the plumes of evaporated material 218a, 218b to help adjust the quality of the deposited film. In one or more examples, the photodetectors 260 use emission spectroscopy (OES) to measure the intensity of one or more wavelengths of light associated with the plumes of evaporated material 218. The OES can communicate with the system 240212 controller 160 or a separate controller.

[0067]

[0072] Figure 3 shows a process flowchart summarizing one embodiment of a process sequence 300 for forming a pre-lithiumized anode structure according to one or more embodiments of the present disclosure. Figure 4 shows a schematic cross-sectional view of a pre-lithiumized anode structure 400 formed according to the process sequence 300 of Figure 3. The process sequence 300 can be used to pre-lithiumize a single-sided electrode structure or a double-sided electrode structure. The process sequence 300 can be performed using a coating system such as the flexible substrate coating system 100 shown in Figure 1, which includes, for example, the deposition module 200 of Figure 2.

[0068]

[0073] Optionally, in operation 305, the thickness of the pre-lithiumized layer to be deposited is determined. The thickness of the pre-lithiumized layer may be based on factors such as lithium loss during cell assembly, e.g., formation of Li2O, aging, e.g., formation of silicon dioxide, and cycling (e.g., formation of SEI).

[0069]

[0074] In operation 310, a ready-made electrode structure 410 is provided, including a substrate coated with an anode material. A continuous sheet 150 of flexible material can constitute the prefabricated electrode structure 410. The substrate may be a current collector as described herein. Examples of metals that can constitute the current collector include aluminum (Al), copper (Cu), zinc (Zn), nickel (Ni), cobalt (Co), tin (Sn), silicon (Si), manganese (Mn), magnesium (Mg), alloys thereof, or combinations thereof. The web or continuous sheet 150 of flexible material may include a polymer material, on which a current collector is subsequently formed. The polymer material may be a resin film selected from polypropylene films, polyethylene terephthalate (PET) films, polyphenylene sulfide (PPS) films, and polyimide (PI) films. The substrate may be a flexible substrate or web, such as a continuous sheet 150 of flexible material that can be used in a roll-to-roll coating system. In one embodiment, the substrate is a negative current collector, such as a copper current collector. In one embodiment, the prefabricated electrode structure 410 is a single-sided anode structure including a substrate coated with an anode material. In one or more examples, the prefabricated electrode structure 410 includes a copper current collector coated with a graphite anode material, a silicon anode material, or a silicon-graphite anode material formed thereon. In another embodiment, the prefabricated electrode structure 410 is a double-sided anode structure. In one or more examples, the double-sided anode structure includes a copper current collector coated on both sides with a graphite anode material, a silicon anode material, or a silicon-graphite anode material.

[0070]

[0075] In operation 320, a first sacrificial anode material, for example, a first sacrificial anode material layer 420, is deposited on the prefabricated electrode structure 410. The first sacrificial anode material layer 420 functions as a corrosion barrier that minimizes the electrochemical resistance between the anode and / or current collector and the lithium metal film deposited thereafter. The first sacrificial anode material layer 420 includes, essentially consists of, or comprises a binary lithium compound, a ternary lithium compound, or a combination thereof. The first sacrificial anode material layer 420 can be deposited using an electron beam evaporation source, for example, an electron beam evaporation source 210. In one or more examples, the first sacrificial anode material layer 420 is formed in a first compartment 122 of a second sub-chamber 120 using a first evaporation source, for example, an electron beam evaporation source 210 configured to deposit the first sacrificial anode material layer 420. In one or more examples, the first sacrificial anode material layer 420 is a lithium fluoride layer.

[0071]

[0076] In operation 330, a second sacrificial anode material, for example, a second sacrificial anode material layer 430, is deposited on the first sacrificial anode material layer 420. The second sacrificial anode material layer 430 functions as a pre-lithification layer that provides lithium to pre-lithify the prefabricated electrode structure 410. The second sacrificial anode material layer 430 contains lithium metal, is essentially composed of lithium metal, or is composed of lithium metal. The second sacrificial anode material layer 430 can be deposited using a thermal evaporation source. In one or more examples, the second sacrificial anode material layer 430 is formed in a second compartment 124 of a second sub-chamber 120 using a deposition source 128, which is a thermal evaporation source configured to deposit the second sacrificial anode material layer 430. In one or more examples, the second sacrificial anode material layer 430 is a lithium metal layer.

[0072]

[0077] In operation 340, a third sacrificial anode material, for example, a 32nd sacrificial anode material layer 440, is deposited on the second sacrificial anode material layer 430. The third sacrificial anode material layer 440 functions as an oxide barrier that minimizes the electrochemical resistance between the lithium metal layer and the electrolyte in the formed cell. The third sacrificial anode material layer 440 includes, essentially consists of, or comprises a combination of, a binary lithium compound, a ternary lithium compound, a sulfide compound, an oxide, or a combination thereof. The third sacrificial anode material layer 440 can be deposited using an electron beam evaporation source, for example, an electron beam evaporation source 210. In one or more examples, the third sacrificial anode material layer 440 is formed in a third compartment 132 of a third sub-chamber 130 using a deposition source 136, which can be an electron beam evaporation source configured to deposit the third sacrificial anode material layer 440. In one or more examples, the third sacrificial anode material layer 440 is a lithium fluoride layer.

[0073]

[0078] In operation 350, a fourth sacrificial anode material, for example, a fourth sacrificial anode material layer 450, is deposited on the third sacrificial anode material layer 440. The fourth sacrificial anode material layer 450 functions as a wetting layer that enhances the wetting of the electrolyte. The fourth sacrificial anode material layer 450 contains, is essentially made from, or consists of a polymer material. Exemplary polymer materials include, but are not limited to, polymethyl methacrylate, polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride, poly(vinylidene fluoride)-co-hexafluoropropylene, polypropylene, nylon, polyamide, polytetrafluoroethylene, polychlorotrifluoroethylene, polyterephthalate, silicone, silicone rubber, polyurethane, cellulose acetate, polystyrene, poly(dimethylsiloxane), or any combination thereof. The fourth sacrificial anode material layer 450 can be deposited using an organic thermal evaporator. In one or more examples, the fourth sacrificial anode material layer 450 is formed in the fourth compartment 134 of the third sub-chamber 130 using an organic thermal evaporation source 138 configured to deposit the fourth sacrificial anode material layer 450. In one or more examples, the fourth sacrificial anode material layer 450 is a poly(dimethylsiloxane) layer. In other examples, the fourth sacrificial anode material layer 450 is a hydrophilic polymer layer, such as a coating containing polyethylene glycol (PEG) with a water contact angle of less than 40 degrees.

[0074]

[0079] In operation 360, at least one of the previously deposited sacrificial anode material layers is subjected to a physical densification process. The sacrificial anode material layer may be subjected to electron irradiation or induction heating during the physical densification process. Electron irradiation or induction heating physically densifies the previously deposited sacrificial anode material layer. The densification process can be performed using an electron gun. In one or more examples, the densification process is performed using an electron gun 214. In other examples, a web or continuous sheet 150 of flexible material is heated by a radio frequency (RF) magnetic field induced by a Helmholtz coil that generates rapidly changing eddy currents.

[0075]

[0080] Optionally, in operation 370, the pre-lithiumized anode structure 400 can be inspected to verify the thickness determination performed during operation 305 and to determine the quality of the deposited material. The pre-lithiumized anode structure 400 can be inspected using a beta-ray detector or other metrology. The results can be used in feedback processing to update future recipes.

[0076]

[0081] In operation 380, the pre-lithiumized anode structure 400 is removed from the flexible substrate coating system 100. The pre-lithiumized anode structure 400 can be used to assemble a pre-lithiumized type lithium-ion battery with reduced first-cycle losses.

[0077]

[0082] Figure 5 shows a process flowchart summarizing one embodiment of a process sequence 500 for forming a metallic anode structure according to one or more embodiments of the present disclosure. Figure 6 shows a schematic cross-sectional view of an anode structure 600 formed according to the process sequence 500 of Figure 5. The process sequence 500 can be used to form a single-sided metallic anode structure or a double-sided metallic anode structure. The process sequence 500 can be performed using a coating system such as the flexible substrate coating system 100 shown in Figure 1, which includes, for example, the deposition module 200 of Figure 2.

[0078]

[0083] Optionally, in operation 505, the thickness of the deposited metal anode layer is determined. The thickness of the metal anode layer may be based on factors such as lithium loss during cell assembly, e.g., formation of Li2O, aging, e.g., formation of silicon dioxide, and cycling (e.g., SEI formation).

[0079]

[0084] In operation 510, a web or continuous sheet 150 of flexible material is provided. In some embodiments, the continuous sheet 150 of flexible material includes a current collector. In another embodiment, the web or continuous sheet 150 of flexible material includes a polymer material, on which a current collector is subsequently formed. The polymer material can be a resin film selected from polypropylene films, polyethylene terephthalate (PET) films, polyphenylene sulfite (PPS) films, and polyimide (PI) films. The continuous sheet 150 of flexible material may include a base layer 610. The base layer 610 may include a substrate. The substrate may be a current collector as described herein. Examples of metals that can constitute a current collector include aluminum (Al), copper (Cu), zinc (Zn), nickel (Ni), cobalt (Co), tin (Sn), silicon (Si), manganese (Mn), magnesium (Mg), alloys thereof, or combinations thereof. The substrate can be a flexible base material or web, such as the continuous sheet 150 of flexible material, which can be used in a roll-to-roll coating system. In one embodiment, the substrate is a negative current collector, such as a copper current collector.

[0080]

[0085] In operation 520, a first persistent anode material, for example, a first persistent anode material layer 620, is deposited on the substrate layer 610. In some embodiments, the first persistent anode material layer 620 functions as a corrosion barrier that minimizes electrochemical resistance between the current collector and the lithium metal anode film deposited thereafter. The first persistent anode material layer 620 includes, essentially consists of, or consists of aluminum, nickel, copper, alumina (Al2O3), boron nitride (BN), carbon, silicon oxide, or a combination thereof. While not bound by theory, the first persistent anode material layer 620 is considered to minimize corrosion and reduce sagging of the continuous metal sheet 150 of the flexible material beneath it. The first persistent anode material layer 620 can be deposited using a sputtering source. In one or more examples, the first persistent anode material layer 620 is formed in the first sub-chamber 110 using a deposition source 113, which is a sputtering source configured to deposit the first persistent anode material layer 620.

[0081]

[0086] In operation 530, a second persistent anode material, for example, a second persistent anode material layer 630, is deposited on the first persistent anode material layer 620. The second persistent anode material layer 630 functions as a corrosion barrier that minimizes the electrochemical resistance between the current collector and the subsequently deposited metal anode film. The second persistent anode material layer 630 includes, essentially consists of, or comprises a binary lithium compound, a ternary lithium compound, or a combination thereof. The second persistent anode material layer 630 can be deposited using an electron beam evaporation source. In one or more examples, the second persistent anode material layer 630 is formed in a first compartment 122 of a second sub-chamber 120 using a first evaporation source, for example, an electron beam evaporation source 210, configured to deposit the second persistent anode material layer 630. In one or more examples, the second persistent anode material layer 630 is a lithium fluoride layer.

[0082]

[0087] In operation 540, a third persistent anode material, for example, a third persistent anode material layer 640, is deposited on the second persistent anode material layer 630. The third persistent anode material layer 640 functions as a lithium metal anode layer. The third persistent anode material layer 640 contains lithium metal, is essentially composed of lithium metal, or is composed of lithium metal. The third persistent anode material layer 640 can be deposited using a thermal evaporation source. In one or more examples, the third persistent anode material layer 640 is formed in a second compartment 124 of the second sub-chamber 120 using a deposition source 128, which is a thermal evaporation source configured to deposit the third persistent anode material layer 640. In one or more examples, the third persistent anode material layer 640 is a lithium metal layer.

[0083]

[0088] In operation 550, a fourth persistent anode material, for example, a fourth persistent anode material layer 650, is deposited on the third persistent anode material layer 640. The fourth persistent anode material layer 650 functions as an oxide barrier that minimizes the electrochemical resistance between the lithium metal layer and the electrolyte in the formed cell. The fourth persistent anode material layer 650 includes, essentially consists of, or comprises a binary lithium compound, a ternary lithium compound, a sulfide compound, a combination of oxides, a polymer, or a combination thereof. The fourth persistent anode material layer 650 can be deposited using an electron beam evaporation source. In one or more examples, the fourth persistent anode material layer 650 is formed in a third compartment 132 of a third sub-chamber 130 using a deposition source 136, which may be an electron beam evaporation source or a thermal organic evaporation source configured to deposit the third persistent anode material layer 440. In one or more examples, the fourth persistent anode material layer 650 is a lithium fluoride layer.

[0084]

[0089] In operation 560, at least one of the previously deposited persistent anode material layers is subjected to a physical densification process. The persistent anode material layer may be subjected to electron irradiation or induction heating during the physical densification process. Electron irradiation or induction heating physically densifies the previously deposited sacrificial anode material layer. The densification process may be performed using an electron gun. In one or more examples, the densification process is performed using an electron gun 214. In other examples, a web or continuous sheet 150 of flexible material is heated by a radio frequency (RF) magnetic field induced by a Helmholtz coil that generates rapidly changing eddy currents.

[0085]

[0090] Optionally, in operation 570, the anode structure 600 can be inspected to verify the thickness determination performed during operation 505 and to determine the quality of the deposited material. The anode structure 600 can be inspected using a beta-ray detector or other metrology. The results can be used in feedback processing to update future recipes.

[0086]

[0091] In operation 580, the anode structure 600 is removed from the flexible substrate coating system 100. The anode structure 600 can be used to assemble a lithium-anode lithium-ion battery with reduced first-cycle losses.

[0087]

[0092] The implementation includes one or more of the following potential advantages: State-of-the-art EV and CE anode protection includes the ability to adjust the thickness of the premetallation. Activation is difficult because carbonate coatings consume lithium, reducing Coulomb efficiency, and slow adsorption rates can lead to significant variations in the uniformity of the longitudinal and transverse carbonate coatings. One or more embodiments of this disclosure include common coating structures that allow for rapid expansion of protective layer material systems compatible with solid electrolytes. In the case of prelithiation, one advantage of an electrochemically active protective layer is that it can simplify downstream workflows. Furthermore, extended handling time can be utilized when metallic lithium is sandwiched between two barriers. In addition, the protective layer can be tuned by electron beam irradiation to add functions such as improved wettability of the electrolyte. In the case of lithium metal anodes, one advantage of an electrochemically active protective layer is that it can address dendritic crystals. In both prelithiation anodes and lithium metal anodes, the electrochemically active coating is colorful and can benefit from advanced measurement-based processing control.

[0088]

[0093] The implementations and all functional operations described herein can be implemented in digital electronic circuits, or in computer software, firmware, or hardware, or combinations thereof, including the structural means and structural equivalents disclosed herein. The implementations described herein can be implemented as one or more non-temporary computer program products, i.e., as one or more computer programs tangibly implemented in machine-readable storage to be executed by or control the operation of a data processing device, such as a programmable processor, a computer, or multiple processors or computers.

[0089]

[0094] The processes and logic flows described herein can be executed by one or more programmable processors that run one or more computer programs that perform functions by manipulating input data to generate outputs. The processes and logic flows can also be executed by dedicated logic circuits, such as FPGAs (Field Programmable Gate Arrays) or ASICs (Application-Specific Integrated Circuits), or implemented in devices.

[0090]

[0095] The term "data processing device" encompasses all devices, machines, and equipment for processing data, including, for example, programmable processors, computers, or multiple processors or computers. In addition to hardware, a device may include code that constitutes the execution environment for the computer program in question, such as processor firmware, protocol stacks, database management systems, operating systems, or one or more combinations thereof. Processors suitable for executing computer programs include, for example, both general-purpose and specialized microprocessors, and any one or more processors in any type of digital computer.

[0091]

[0096] Computer-readable media suitable for storing computer program instructions and data include all forms of non-volatile memory, media, and memory devices, including, for example, semiconductor memory devices such as EPROM, EEPROM, and flash memory devices, magnetic disks such as internal hard disks or removable disks, magneto-optical disks, and CD-ROM and DVD-ROM disks. Processors and memory can be supplemented by or incorporated into special-purpose logic circuits.

[0092]

[0097] Embodiments of this disclosure further relate to any one or more of the following Examples 1 to 44.

[0093]

[0098] 1. A flexible substrate coating system comprising a feed module housing a supply reel capable of providing a continuous sheet of flexible material, a winding module housing a winding reel capable of storing the continuous sheet of flexible material, and a processing module arranged downstream of the feed module, wherein the processing module comprises a plurality of sequentially arranged sub-chambers, each configured to perform one or more processing operations on a continuous sheet of flexible material, and a coating drum capable of guiding a continuous sheet of flexible material through the plurality of sub-chambers along the direction of movement, the sub-chambers being arranged radially around the coating drum, and at least one of the sub-chambers comprising a deposition module including a pair of electron beam sources arranged side by side along a transverse direction perpendicular to the direction of movement.

[0094]

[0099] 2. The coating system according to Example 1, wherein the deposition module is defined by a sub-chamber body having an edge shield positioned on the sub-chamber body.

[0095]

[0100] 3. The coating system according to Example 1 or 2, wherein the edge shield has one or more openings that define a pattern of evaporated material deposited on a continuous sheet of flexible material.

[0096]

[0101] 4. The coating system according to any one of Examples 1 to 3, wherein the edge shield has at least two openings, the first opening defining a first strip of the deposited material and the second opening defining a second strip of the deposited material.

[0097]

[0102] 5. A coating system according to any one of Examples 1 to 4, wherein each electron beam source includes at least one crucible and an electron gun capable of holding an evaporable material.

[0098]

[0103] 6. A coating system according to any one of Examples 1 to 5, wherein the electron gun is operable to emit an electron beam toward an evaporable material placed in a crucible.

[0099]

[0104] 7. A coating system according to any one of Examples 1 to 6, further comprising an electron gun steering that can direct the electron beam of the electron gun from the evaporative material to the continuous sheet of flexible material in order to irradiate electrons onto the deposited material on the continuous sheet of flexible material.

[0100]

[0105] 8. A coating system according to any one of Examples 1 to 7, further comprising a deposition module and a photodetector positioned to monitor a plume of evaporated material emitted from an electron beam source.

[0101]

[0106] 9. A coating system according to any one of Examples 1 to 8, wherein a photodetector is configured to perform emission spectroscopy to measure the intensity of one or more wavelengths of light associated with the plume of evaporated material.

[0102]

[0107] 10. A coating system according to any one of Examples 1 to 9, wherein a pair of electron beam sources are configured to deposit a lithium fluoride film on a continuous sheet of flexible material.

[0103]

[0108] 11. A coating system according to any one of Examples 1 to 10, wherein a plurality of sub-chambers further include a first sub-chamber containing a sputtering source, and the first sub-chamber is positioned upstream of a sub-chamber containing a deposition module.

[0104]

[0109] 12. A coating system according to any one of Examples 1 to 11, wherein the sputtering source is configured to deposit at least one of aluminum, nickel, copper, alumina, boron nitride, carbon, silicon oxide, or a combination thereof.

[0105]

[0110] 13. A coating system according to any one of Examples 1 to 12, wherein the subchamber containing the deposition module further comprises a second subchamber containing a thermal evaporation source.

[0106]

[0111] 14. A coating system according to any one of Examples 1 to 13, wherein the thermal evaporation source is configured to deposit lithium metal.

[0107]

[0112] 15. A coating system according to any one of Examples 1 to 14, wherein the plurality of sub-chambers further include a second deposition module similar to the deposition module, and a third sub-chamber positioned downstream of the sub-chambers containing the deposition module.

[0108]

[0113] 16. A coating system according to any one of Examples 1 to 15, wherein a second deposition module is configured to deposit lithium fluoride.

[0109]

[0114] 17. The coating system according to any one of Examples 1 to 16, wherein the third sub-chamber further comprises a fourth sub-chamber containing an organic thermal evaporation source.

[0110]

[0115] 18. A coating system according to any one of Examples 1 to 17, further comprising a chemical vapor deposition (CVD) module positioned between a processing module and a winding module.

[0111]

[0116] 19. A coating system according to any one of Examples 1 to 18, wherein the CVD module includes a multizone gas distribution assembly.

[0112]

[0117] 20. A coating system according to any one of Examples 1 to 19, wherein a multizone gas distribution assembly is fluidically connected to a first gas source.

[0113]

[0118] 21. The first gas source is titanium tetrachloride, boron phosphate, TiCl4(HSR)2 (where R=C6H) 11A coating system according to any one of Examples 1 to 20, configured to supply at least one of the following (or C5H9, or a combination thereof).

[0114]

[0119] 22. A coating system according to any one of Examples 1 to 21, wherein a multizone gas distribution assembly is fluidically connected to a second gas source.

[0115]

[0120] 23. The coating system according to any one of Examples 1 to 22, wherein the second gas source is configured to supply at least one of hydrogen sulfide, carbon dioxide, perfluorodecyltrichlorosilane (FDTS), and polyethylene glycol (PEG).

[0116]

[0121] 24. A method for forming a prelithiated anode structure, comprising: depositing a first sacrificial anode layer on a prefabricated electrode structure including a continuous sheet of flexible material coated with an anode material; depositing a second sacrificial anode layer on the first sacrificial anode layer; depositing a third sacrificial anode layer on the second sacrificial anode layer; and densifying at least one of the first sacrificial anode layers, wherein the second and third sacrificial anode layers are formed by exposing the sacrificial anode layers to electron beams from a pair of electron beam sources.

[0117]

[0122] 25. The method according to Example 24, wherein the anode material is selected from a graphite anode material, a silicon anode material, or a silicon-graphite anode material.

[0118]

[0123] 26. The method according to Example 24 or 25, wherein the first sacrificial anode layer functions as a corrosion barrier that minimizes the electrochemical resistance between the anode material and / or substrate and the second sacrificial anode layer.

[0119]

[0124] 27. The method according to any one of Examples 24-26, wherein the first sacrificial anode layer comprises a binary lithium compound, a ternary lithium compound, or a combination thereof.

[0120]

[0125] 28. The method according to any one of Examples 24-27, wherein the first sacrificial anode layer is deposited using an electron beam evaporation source.

[0121]

[0126] 29. The method according to any one of Examples 24-28, wherein the first sacrificial anode layer is a lithium fluoride layer.

[0122]

[0127] 30. The method according to any one of Examples 24-29, wherein the second sacrificial anode material layer functions as a pre-lithification layer that supplies lithium for pre-lithification of the prefabricated electrode structure.

[0123]

[0128] 31. The method according to any one of Examples 24-30, wherein the second sacrificial anode layer is a lithium metal layer.

[0124]

[0129] 32. The method according to any one of Examples 24-31, wherein a third sacrificial anode layer functions as an oxidation barrier that minimizes the electrochemical resistance between the lithium metal layer and the subsequently deposited electrolyte.

[0125]

[0130] 33. The method according to any one of Examples 24 to 32, wherein the third sacrificial anode layer includes a binary lithium compound, a ternary lithium compound, a sulfide compound, an oxide combination, or a combination thereof.

[0126]

[0131] 34. The method according to any one of Examples 24-33, wherein the third sacrificial anode layer is a lithium fluoride layer.

[0127]

[0132] 35. The method according to any one of Examples 24-34, further comprising depositing a fourth sacrificial layer on a third sacrificial anode layer, wherein the fourth sacrificial layer functions as a wetting layer.

[0128]

[0133] 36. The method according to any one of Examples 24 to 35, wherein the fourth sacrificial anode layer comprises a polymer material selected from polymethyl methacrylate, polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride, poly(vinylidene fluoride)-co-hexafluoropropylene, polypropylene, nylon, polyamide, polytetrafluoroethylene, polychlorotrifluoroethylene, polyterephthalate, silicone, silicone rubber, polyurethane, cellulose acetate, polystyrene, poly(dimethylsiloxane), or any combination thereof.

[0129]

[0134] 37. A method for forming an anode structure, comprising: depositing a first persistent anode layer on a continuous sheet of a flexible material; depositing a second persistent anode layer on a first persistent lithium anode layer; depositing a third persistent anode layer, which is a lithium metal layer, on the second persistent anode layer; and densifying at least one of the first persistent lithium anode layers, wherein the second and third persistent anode layers are formed by exposing the persistent anode layers to electron beams from a pair of electron beam sources.

[0130]

[0135] 38. The method according to Example 37, wherein the first permanent anode layer functions as a corrosion barrier that minimizes electrochemical resistance between a continuous sheet of flexible material and a second permanent anode layer.

[0131]

[0136] 39. The method according to Example 37 or 38, wherein the first persistent anode layer comprises a first persistent anode material layer comprising aluminum, nickel, copper, alumina (Al2O3), boron nitride (BN), carbon, silicon oxide, or a combination thereof.

[0132]

[0137] 40. The method according to any one of Examples 37-39, wherein the first persistent anode layer is deposited using a sputtering source.

[0133]

[0138] 41. The method according to any one of Examples 37-40, wherein the second permanent anode layer functions as a corrosion barrier that minimizes electrochemical resistance between the continuous sheet of flexible material and the third permanent anode layer.

[0134]

[0139] 42. The method according to any one of Examples 37 to 41, wherein the second persistent anode layer comprises a binary lithium compound, a ternary lithium compound, or a combination thereof.

[0135]

[0140] 43. The method according to any one of Examples 37-42, wherein a second persistent anode layer is deposited using an electron beam evaporation source.

[0136]

[0141] 44. The method according to any one of Examples 37-42, wherein a second persistent anode layer is deposited using an electron beam evaporation source.

[0137]

[0142] While the foregoing relates to embodiments of the present disclosure, other and further embodiments can be devised without departing from their basic scope, the scope of which will be determined by the claims. All documents described herein, including priority documents and / or test procedures, are incorporated herein by reference to the extent that they do not contradict this text. As is evident from the above general description and specific embodiments, the forms of the present disclosure are illustrative and described, but various modifications can be made without departing from the spirit and scope of the present disclosure. Therefore, the present disclosure is not intended to be limited thereto. Similarly, the term “comprising” is to be considered synonymous with the term “inclusive” for the purposes of U.S. law. Similarly, whenever there is a transitional phrase “comprising” before a composition, element, or group of elements, it is understood that the same composition or group of elements is to be, or vice versa, with a transitional phrase “consisting essentially of,” “consisting of,” “selected from the group of consisting of,” or “is” before the description of the composition, element, or group of elements. When describing elements of this disclosure or exemplary forms or practices thereof, the articles “a,” “an,” “the,” and “the” are intended to indicate the presence of one or more elements.

[0138]

[0143] Specific embodiments and features have been described using a series of numerical upper and lower limits. Unless otherwise indicated, it should be understood that ranges are intended to include any combination of any two values, for example, any combination of any lower limit and any upper limit, any combination of any two lower limits, and / or any combination of any two upper limits. Specific lower limits, upper limits, and ranges are described in one or more of the following claims.

Claims

1. a delivery module housing a supply reel capable of providing a continuous sheet of flexible material; a take-up module housing a take-up reel capable of storing a continuous sheet of said flexible material; a processing module arranged downstream of the delivery module; 1. A flexible substrate coating system comprising: The processing module includes: a plurality of sub-chambers arranged in series, each configured to perform one or more processing operations on the continuous sheet of flexible material; and a coating drum capable of guiding the continuous sheet of flexible material along a direction of movement through the plurality of sub-chambers; Including, The subchambers are radially arranged around the coating drum, and at least one of the subchambers comprises: a deposition module including a pair of electron beam sources positioned side-by-side in a transverse direction perpendicular to the direction of travel; Flexible substrate coating system.

2. 10. The coating system of claim 1, wherein the deposition module is defined by a subchamber body having an edge shield positioned thereover, the edge shield having one or more apertures defining a pattern of evaporated material to be deposited on the continuous sheet of flexible material.

3. 3. The coating system of claim 2, wherein the edge shield has at least two apertures, a first aperture defining a first strip of deposited material and a second aperture defining a second strip of deposited material.

4. 10. The coating system of claim 1, wherein the deposition module further comprises an optical detector positioned to monitor a plume of evaporated material emitted from at least one of the pair of electron beam sources, the optical detector configured to perform optical emission spectroscopy to measure intensity of one or more wavelengths of light associated with the plume of evaporated material.

5. 2. The coating system of claim 1, wherein each electron beam source includes at least one crucible capable of holding an evaporable material and an electron gun, the electron gun operable to emit an electron beam toward the evaporable material positioned in the crucible, and each electron beam source further includes electron gun steering capable of directing the electron beam of the electron gun from the evaporable material to the continuous sheet of flexible material for electron irradiation of deposited material on the continuous sheet of flexible material.

6. The coating system of claim 1 , wherein the pair of electron beam sources are configured to deposit a lithium fluoride film onto the continuous sheet of flexible material.

7. 2. The coating system of claim 1, wherein the plurality of subchambers further comprises a first subchamber including a sputtering source, the first subchamber being positioned upstream of the subchamber including the deposition module, and the sputtering source configured to deposit at least one material selected from aluminum, nickel, copper, alumina, boron nitride, carbon, silicon oxide, or combinations thereof.

8. 10. The coating system of claim 1, wherein the subchamber containing the deposition module further comprises a second subchamber containing a thermal evaporation source, the thermal evaporation source configured to deposit lithium metal.

9. 2. The coating system of claim 1, wherein the plurality of subchambers further comprises a third subchamber, the third subchamber including a second deposition module similar to the deposition module and positioned downstream from the subchamber including the deposition module, the second deposition module configured to deposit lithium fluoride.

10. 10. The coating system of claim 1, further comprising a chemical vapor deposition (CVD) module positioned between the treatment module and the take-up module, the CVD module comprising a multi-zone gas distribution assembly or showerhead.

11. The multi-zone gas distribution assembly or the showerhead is fluidly connected to a first gas source, the first gas source being titanium tetrachloride, boron phosphate, TiCl 4 (HSR) 2 (Wherein, R is C 6 H 11 Or C 5 H 9 11. The coating system of claim 10, configured to provide at least one of:

12. 11. The coating system of claim 10, wherein the multi-zone gas distribution assembly or the showerhead is fluidly coupled to a second gas source, the second gas source configured to supply at least one of hydrogen sulfide, carbon dioxide, perfluorodecyltrichlorosilane (FDTS), and polyethylene glycol (PEG).

13. depositing a first sacrificial anode layer onto a prefabricated electrode structure comprising a continuous sheet of flexible material coated with an anode material; depositing a second sacrificial anode layer on the first sacrificial anode layer; depositing a third sacrificial anode layer on the second sacrificial anode layer; densifying at least one of the first sacrificial anode layer, the second sacrificial anode layer, and the third sacrificial anode layer by exposing the at least one of the first sacrificial anode layer, the second sacrificial anode layer, and the third sacrificial anode layer to an electron beam from a pair of electron beam sources; 4. A method of forming a prelithiated anode structure comprising:

14. 14. The method of claim 13, wherein the first sacrificial anode layer acts as a corrosion barrier to minimize electrochemical resistance between the anode material and / or substrate and the second sacrificial anode layer, the first sacrificial anode layer comprising a binary lithium compound, a ternary lithium compound, or a combination thereof.

15. 14. The method of claim 13, wherein the second sacrificial anode layer functions as a prelithiation layer that provides lithium for prelithiating the prefabricated electrode structure, the second sacrificial anode layer being a lithium metal layer, and the third sacrificial anode layer functions as an oxidation barrier to minimize electrochemical resistance between the lithium metal layer and a subsequently deposited electrolyte.

16. 14. The method of claim 13, wherein the third sacrificial anode layer comprises a binary lithium compound, a ternary lithium compound, a sulfide compound, a combination of oxides, or combinations thereof.

17. 14. The method of claim 13, further comprising depositing a fourth sacrificial anode layer on the third sacrificial anode layer, the fourth sacrificial anode layer functioning as a wetting layer, the fourth sacrificial anode layer comprising a polymeric material selected from polymethyl methacrylate, polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride, poly(vinylidene fluoride)-co-hexafluoropropylene, polypropylene, nylon, polyamide, polytetrafluoroethylene, polychlorotrifluoroethylene, polyterephthalate, silicone, silicone rubber, polyurethane, cellulose acetate, polystyrene, poly(dimethylsiloxane), or combinations thereof.

18. depositing a first permanent anode layer on a continuous sheet of flexible material; depositing a second permanent anode layer over the first permanent anode layer; depositing a third permanent anode layer on the second permanent anode layer, the third permanent anode layer being a lithium metal layer; densifying at least one of the first permanent anode layer, the second permanent anode layer, and the third permanent anode layer by exposing the at least one of the first permanent anode layer, the second permanent anode layer, and the third permanent anode layer to an electron beam from a pair of electron beam sources; 16. A method for forming an anode structure comprising:

19. The first permanent anode layer acts as a corrosion barrier to minimize electrochemical resistance between the continuous sheet of flexible material and the second permanent anode layer, and the first permanent anode layer may be made of any of a variety of materials, including aluminum, nickel, copper, alumina (Al 2 O 3 20. The method of claim 18, further comprising a first permanent anode material layer comprising silicon dioxide (SiO2), boron nitride (BN), carbon, silicon oxide, or a combination thereof, the first permanent anode layer being deposited using a sputtering source.

20. 20. The method of claim 18, wherein the second permanent anode layer acts as a corrosion barrier to minimize electrochemical resistance between the continuous sheet of flexible material and the third permanent anode layer, the second permanent anode layer comprising a binary lithium compound, a ternary lithium compound, or a combination thereof, and the second permanent anode layer is deposited using an electron beam evaporation source.