Methods of reducing metal residue in edge bead region from metal-containing resists

JP2024109695A5Active Publication Date: 2024-10-16INPRIA CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024079459
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2016-12-06
Filing Date
2024-05-15
Publication Date
2024-10-16
Estimated Expiration
2037-08-11

AI Technical Summary

Technical Problem

Existing edge bead removal solutions for metal-containing resists are inadequate in effectively reducing residual metal contamination along the wafer edge, particularly for metal-based radiation-sensitive materials used in semiconductor processing.

Method used

A method involving the use of organic solvents with additives such as carboxylic acids, inorganic fluorinated acids, and tetraalkylammonium compounds, along with sacrificial layers and anti-adhesion coatings, to enhance edge bead removal during the edge bead rinsing process.

Benefits of technology

Significantly reduces residual metal contamination, particularly tin, to acceptable levels, enabling effective incorporation of metal-based resists in semiconductor patterning processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide methods and devices for removing an edge bead on a wafer associated with a resist coating comprising metal-containing resist compositions.SOLUTION: The methods comprise: applying a first bead edge rinse solution along a wafer edge 128 following spin coating 122 of a wafer 120 with a metal-based resist composition 124; performing a bead edge rinse step 126 to remove the resist along the edge 128 of the substrate 120 to form an edged resist layer 130. The edge bead solution comprises an organic solvent and an additive comprising a carboxylic acid, an inorganic fluorinated acid, a tetraalkylammonium compound, or a mixture thereof. The methods also comprise applying a protective composition to the wafer prior to performing the edge bead rinse. The protective composition is a sacrificial material or an anti-adhesion material and is applied only to the wafer edge or across the entire wafer in the case of the protective composition.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to co-pending U.S. Provisional Patent Application No. 62 / 374,582 to Clark et al., entitled "Bead Washing for Metal Oxide Based Resists," filed on August 12, 2016, and to co-pending U.S. Provisional Patent Application No. 62 / 430,722 to Cardineau et al., entitled "Method of Reducing Metal Residue in Edge Bead Region from Metal-Containing Resists," filed on December 6, 2016, both of which are incorporated herein by reference.

[0002] The present invention relates to a process for reducing metal contamination along the wafer edge that potentially results from the use of metal-based patterning resists. [Background technology]

[0003] The fabrication of semiconductor circuits and devices has involved a continuous shrinkage of critical dimensions over each generation. As these dimensions shrink, new materials and methods are needed to meet the demands of fabricating and patterning ever smaller features. Patterning generally involves selectively exposing a thin layer of radiation-sensitive material (resist) to form a pattern that is then transferred to a subsequent layer or functional material. A promising new class of metal-based radiation resists has been discovered that are particularly suited to provide good absorption of extreme ultraviolet light and electron beam radiation while at the same time providing very high etch contrast. To provide practical applications for these new classes of resists, consideration of process integration to achieve the desired end product may be a critical step. Summary of the Invention [Means for solving the problem]

[0004] In a first aspect, the present invention relates to a method for removing an edge bead on a wafer associated with a resist coating comprising a metal-containing resist composition, the method comprising applying a first bead edge rinse solution along the wafer edge after spin-coating the wafer with the resist composition. In some embodiments, the edge bead solution comprises an organic solvent and an additive comprising a carboxylic acid, an inorganic fluorinated acid, a tetraalkylammonium compound, or mixtures thereof.

[0005] In a further aspect, the invention relates to a method for preparing a wafer for radiation-based patterning comprising applying a protective composition to the wafer, spin-coating a resist composition comprising a metal after applying the protective composition, and performing an edge bead rinse after spin-coating the resist composition through application of an edge bead rinse solution along an edge of the wafer.

[0006] In another aspect, the invention relates to an apparatus that includes a spindle including a wafer support, a dispenser having a nozzle configured to deposit a fluid along an edge of a wafer mounted on the spindle, and a reservoir of fluid configured to deliver the fluid to the nozzle for dispensing. Generally, the spindle is operatively connected to a motor configured to rotate the spindle. In some embodiments, the fluid includes an organic solvent with an additive including a surface modifier, an acidic compound, a tetraalkylammonium compound, or mixtures thereof. [Brief description of the drawings]

[0007] [Figure 1] 1 is a schematic perspective view of an edge bead relief apparatus shown with a wafer position for processing to perform edge bead relief; [Diagram 2] FIG. 1 is a schematic diagram showing steps for preparing a wafer with a resist layer after edge bead removal, with two processing steps shown. [Diagram 3] 1 is a photograph of a microscope image showing a wafer edge after edge beading. [Figure 4] 1 is a schematic diagram depicting the steps used to form a sacrificial layer on a substrate, which is then used to facilitate edge bead removal in a rinsing step. Inset A shows a top view of the wafer after the final rinse. [Diagram 5] 1 is a schematic diagram showing the steps used to form a sacrificial edge coating or sacrificial ring on a substrate to facilitate removal of the edge bead; inset A is a top view of the wafer with the sacrificial ring, and inset B shows the final structure with the bead edge rinsed. [Figure 6] Schematic diagram illustrating processing with an anti-adhesion edge coating to substantially avoid resist deposition along the edge and a bead edge rinse to further reduce residual metal contamination along the edge after processing, where inset A represents a top view of the wafer with the anti-adhesion edge coating, inset B represents a top view of the structure after resist deposition, and inset C represents a top view of the structure after edge bead rinse. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Edge bead removal processes have been developed to more effectively remove metal and metal-organic based resist materials and residues. Substrate edge resist buildup can be removed prior to patterning the substrate with radiation to reduce contamination of process equipment by resist materials. Edge bead removal solutions designed for conventional organic photoresists may not be sufficiently effective for removing metal-containing resists. Improved edge bead removal solutions can use selected solvents and may further contain additives such as acids to facilitate removal of resist buildup. In additional or alternative embodiments, a sacrificial layer, e.g., a polymer layer, can be placed on the wafer edge or across the entire wafer surface to facilitate removal of resist from the bead edge. Additionally, an anti-adhesion layer, e.g., a coating with a sufficiently low critical surface tension, can be placed along the substrate edge to reduce or eliminate initial adhesion of resist along the substrate edge. Due to improved patterning performance of metal-based resists, especially for fine patterning with extreme ultraviolet (EUV) light, it would be advantageous to provide a processing approach that can effectively incorporate metal-based resists into patterning processes with corresponding high performance equipment. Thus, the processes and corresponding compositions described herein contribute significantly to the practical application of metal-based resists.As used herein, substrate and wafer are used interchangeably to refer to structures that, unless otherwise noted, are generally but necessarily cylindrical in shape and typically have a thickness that is small relative to the dimensions associated with their planar extent.

[0009] To aid in edge bead removal, new rinse solutions have been identified for processing wafers coated with metal-based or metal-containing patterned resists. Resist compositions containing metals can generally be considered to contain more than a contaminant amount of metal, for example at least 0.1 weight percent metal, and some metal-containing resists of particular interest are further described below. For semiconductor fine patterning and other radiation-based lithography processes, patterned resists are generally spin-coated onto wafers to form a relatively uniform resist layer across most of the wafer surface. Even if some of the excess resist spins off from the wafer surface, spin-coating can result in beads along the wafer edge where the resist is deposited relative to the resist layer covering most of the wafer. Since the edge itself is not patterned using lithography, it is generally desirable to remove edge beads to facilitate processing of the wafer for patterning and reduce contamination. New rinse compositions for effectively removing edge beads of metal-based or metal-containing resists can include suitable organic solvents and additives, such as carboxylic acids, inorganic fluorinated acids, tetraalkylammonium fluorides with strong acids, or combinations thereof. Removal of the edge bead of metal-based or metal-containing resists can also help reduce unwanted residual metal after the patterning process. After the bead edge rinse, wafer patterning generally continues using the usual steps for resist-based patterning.

[0010] During photoresist processing, an edge bead removal (EBR) rinse step is commonly used. The EBR process is usually performed before any heat treatment or baking after photoresist deposition and involves rinsing the peripheral edge of the wafer or substrate with a solvent to remove the photoresist in selected areas. This EBR process serves to reduce contamination of tools and machinery that handle or manipulate the wafer or substrate. It is desirable to use a metal-based photoresist to reduce the residual amount of metal, e.g., tin, in the EBR area. Standard EBR solvents based on organic solvents designed to remove polymer resists may not be as effective as desired to reduce the concentration of residual metal, e.g., tin, on the edge area of ​​the wafer surface to the desired level. In addition, the methods and materials described herein may be advantageous for processing resists containing a wide variety of metals, such as Hf, Zr, In, Te, Sb, Ni, Co, Ti, W, Ta, Mo, and combinations thereof, and the present disclosure contemplates such use.

[0011] A new class of radiation-based resists can be based on metal oxide chemistry (metal oxo / hydroxo compositions) that uses radiation-sensitive ligands to control the stability and processability of the resist. The first set of new radiation-based resists uses peroxo ligands as radiation-sensitive stabilizing ligands. Peroxo-based metal oxo-hydroxo compounds are described, for example, in U.S. Pat. No. 9,176,377 B2 to Stowers et al., entitled "Patterned Inorganic Layers, Radiation Based Patterning Compositions and Corresponding Methods," which is incorporated herein by reference. Related resist compounds are discussed in U.S. Pat. App. Pub. No. 2013 / 0224652 A1 to Bass et al., entitled "Metal Peroxo Compounds With Organic Co-ligands for Electron Beam, Deep UV and Extreme UV Photoresist Applications," which is incorporated herein by reference. Effective types of resists have been developed using alkyl ligands such as those described in U.S. Pat. No. 9,310,684 B2 to Meyers et al., entitled "Organometallic Solution Based High Resolution Patterning Compositions," U.S. Patent Application Publication No. 2016 / 0116839 A1 to Meyers et al., entitled "Organometallic Solution Based High Resolution Patterning Compositions and Corresponding Methods," and U.S. Patent Application Publication No. 15 / 291738, entitled "Organotin Oxide Hydroxide Patterning Compositions, Precursors, and Patterning," all of which are incorporated herein by reference.Tin compositions are exemplified in these patent documents, and the data presented herein focus on tin-based resists, but the edge bead removal solutions described herein are expected to be effective for other metal-based resists described below.

[0012] With particular reference to tin-based resists of interest, these resists are based on the chemistry of organometallic compositions represented by the formula R z SnO (2-(z / 2)-(x / 2)) (OH) x wherein 0 < z ≦ 2 and 0 < (z + x) ≦ 4, and R is a hydrocarbyl group having 1 to 31 carbon atoms. However, at least some of the oxo / hydroxo ligands can be formed post-deposition based on in-situ hydrolysis of compositions represented by the formula R n SnX 4-n wherein n = 1 or 2 and X is a ligand having a hydrolyzable M-X bond. Generally, suitable hydrolyzable ligands (X in RSnX3) include alkynide RC≡C, alkoxide RO - , azide N3 - , carboxylate RCOO - , halide, and dialkylamide. Thus, in some embodiments, all or part of the oxo-hydroxy composition can be replaced with Sn-X compositions or mixtures thereof. The R-Sn boundary is generally radiation sensitive and forms the basis for the radiation-processable aspect of the resist. However, some of the R z SnO (2-(z / 2)-(x / 2)) (OH) x compositions can be replaced with MO ((m / 2)-l / 2) (OH) l wherein 0 < z ≦ 2, 0 < (z + w) ≦ 4, m = the formal valence of M m+ , 0 ≦ l ≦ m, y / z = (0.05 to 0.6), and M = M’ or Sn, where M’ is a non-tin metal of Groups 2 to 16 of the periodic table and R is a hydrocarbyl group having 1 to 31 carbon atoms. Thus, the resist processed during edge bead rinse is R z SnO (2-(z / 2)-(x / 2)) (OH)x , R' n SnX 4-n and / or M.O. ((m / 2)-l / 2) (OH) l In this case, generally a significant portion of the composition contains alkyl-tin bonds. Other resist compositions include compositions having metal carboxylate bonds (e.g., acetate, propanoate, butanoate, benzoate, and other ligands), such as, for example, dibutyltin diacetate.

[0013] While the metal oxo / hydroxo or carboxylate-based resists mentioned above are particularly desirable, in some embodiments, some other high-performance resists may be suitable. Specifically, other metal-based resists include those with high etch selectivity to templates, fill materials, and buffer hardmasks. These may include resists such as metal oxide nanoparticle resists (e.g., Jiang, Jing; Chakrabarty, Souvik; Yu, Mufei et al., "Metal Oxide Nanoparticle Photoresists for EUV Patterning", Journal Of Photopolymer Science And Technology 27(5), 663-666 2014, which is incorporated herein by reference) or other metal-containing resists (A Platinum-Fullerene Complex for Patterning Metal Containing Nanostructures, DX Yang, A. Frommhold, DS He, ZY Li, RE Palmer, MA Lebedeva, TW Chamberlain, ANKhlobystov, APG Robinson, Proc SPIE Advanced Lithography, 2014, which is incorporated herein by reference). Other metal-based resists are described in U.S. Patent Application Publication No. 2009 / 0155546A1 to Yamashita et al., entitled "Film-Forming Composition, Method for Pattern Formation, and Three-Dimensional Mold," and U.S. Patent No. 6,566,276 to Maloney et al., entitled "Method of Making Electronic Materials," both of which are incorporated herein by reference.

[0014] In electronics processing, it is generally desirable to mitigate trace metal contamination and therefore to remove tin and / or other metal residues potentially resulting from resists using organometallic-based resists. The improved edge bead removal solution generally includes an organic solvent and one or more additives where the additives allow for improved metal removal. Suitable additives include, for example, organic acids, inorganic fluoroacids, tetraalkylammonium halides, and mixtures thereof. Suitable additives may also function as complexing or chelating agents, such as carboxylates, dicarboxylates, halides, phosphates, phosphonates, sulfates, sulfonates, and mixtures thereof. The additives may also function as surfactants and / or chelating agents. Thus, the conjugated anions of the various acids listed herein may be added as chelating agents. Similarly, the non-ionic surfactant Triton TMSurfactants such as -X can also be used as additives. The additives can be selected to be soluble in the organic solvent. The solution can include from about 0.1% to about 25% by weight of the additive, in further embodiments from about 0.2% to about 20% by weight, and in additional embodiments from about 0.25% to about 20% by weight. One of ordinary skill in the art will recognize that other ranges of additive concentrations within the above explicit ranges are contemplated and are within the scope of the present disclosure. Suitable organic solvents include, for example, glycol ethers such as propylene glycol methyl ether (PGME), propylene glycol methyl ethyl acetate (PGMEA), propylene glycol butyl ether (PGBE), ethylene glycol methyl ether, and esters thereof, alcohols such as ethanol, propanol, isopropyl alcohol, isobutyl alcohol, hexanol, ethylene glycol, propylene glycol, cyclic esters such as gamma-butyrolactone, esters such as n-butyl acetate, ethyl acetate, and / or mixtures thereof, ketones such as heptanone, liquid cyclic carbonates such as propylene carbonate, butylene carbonate, and any mixtures thereof. A mixed solvent containing about 50 to about 90% by weight PGMEA, about 1% to about 20% by weight PGME, about 1% to about 10% by weight γ-bryrolactone, and about 1% to about 20% by weight n-butyl acetate has been proposed as a desirable EBR solution having desirable rheology and evaporation characteristics in U.S. Patent No. 8,227,182 to Lee et al., entitled "Methods of Forming a Photosensitive Film," which is incorporated herein by reference. Suitable organic acids include, for example, carboxylic acids such as acetic acid, citric acid, oxalic acid, 2-nitrophenylacetic acid, 2-ethylhexanoic acid, dodecanoic acid, and the like; sugar acids such as ascorbic acid, tartaric acid, glucuronic acid, and the like; sulfonic acids such as benzenesulfonic acid, p-toluenesulfonic acid, and the like; phosphoric acids such as phosphate esters and bis(2-ethylhexyl) phosphate; hydrofluoric acid (HF), sulfuric acid (H2SO4), and any mixtures thereof. Suitable inorganic fluoroacids include, for example, hexafluorosilicic acid, hexafluorophosphoric acid, fluoroboric acid, and the like.Suitable tetraalkylammonium compounds include, for example, tetramethylammonium fluoride, tetrabutylammonium fluoride, tetrabutylammonium fluorosilicate, and the like, or mixtures thereof.

[0015] Multiple rinse steps can be performed to achieve the desired level of edge cleaning. In some embodiments, the edge rinse can be performed 1, 2, 3, 4, 5, 6, 10, or 11 or more times with the same solution to achieve the desired reduction in metal. Additionally, two different rinse solutions can be applied during the edge bead rinse process. Each different solution can be independently selected from the solutions described above. Generally, for wafers having a diameter of about 3 inches to about 18 inches, the solution can be delivered in an amount of about 0.05 milliliters (mL) to about 50 mL, in further embodiments about 0.075 mL to about 40 mL, and in other embodiments about 0.1 mL to about 25 mL during each application. In some embodiments, the solution can be sprayed at a flow rate of about 5 mL / min to about 50 mL / min, and the solution can be applied for about 1 second to about 5 minutes, and in further embodiments about 5 seconds to about 2 minutes. One of ordinary skill in the art will recognize that other ranges of solution applications and application volumes within the above explicit ranges are contemplated and are within the scope of the present disclosure.

[0016] An apparatus for edge bead removal is shown in Figure 1. Referring to Figure 1, a wafer processing apparatus 100 includes a spindle 102 having a hollow core 104 connected to a motor for rotating the spindle and a pump configured to apply a negative pressure to the hollow core of the spindle, a chuck 106 operatively connected to the spindle for rotation therewith, and a fluid dispenser 108 configured to dispense a fluid 110 to an edge of one or both sides of a wafer supported on the chuck 106 and held in place by the negative pressure in the hollow core 104. A wafer 112 is shown in Figure 1 suitably positioned within the apparatus. The fluid dispenser 108 may include a nozzle or the like for directing a fluid towards the wafer. A reservoir 114 is operatively connected to the fluid dispenser 108 for supplying a fluid. The reservoir may be a container suitable for holding a fluid connected with tubing, hoses, or the like, and fluid movement from the reservoir 114 may be driven using gravity or a pump or the like. The negative pressure applied to the hollow core 104 may be provided by a negative pressure device 116. The negative pressure device may be a pump, aspirator, blower, or the like. The spindle 102 may also be connected to a motor 118. The motor may have an appropriate design and mounting to spin the spindle 102 for wafer processing. A specific apparatus design for edge bead processing is described in U.S. Pat. No. 8,826,926 B2 to Chalom et al., entitled "Methods of Profiling Edges and Removing Edge Beads," which is incorporated herein by reference.

[0017] The edge bead rinse process is shown diagrammatically in FIG. 2. As shown in the left image, a substrate 120 is obtained and coated 122 with a metal-based resist 124. A bead edge rinse step 126 is then performed to remove the resist along the edge 128 of the substrate 120 to form an edged resist layer 130. The edge bead rinse process is further described above in terms of compositions, amounts of compositions, and delivery devices. The resulting structure 132 with edged resist layer 130 can then be used for the patterning step of the substrate 120. Coating of the wafer with resist can be performed, for example, by depositing about 0.25 mL to about 20 mL of resist solution in an appropriate configuration onto a stationary wafer, and then spinning the wafer at, for example, 250 rpm to 10,000 rpm for a time period of about 5 seconds to about 15 minutes to spread the resist. The spin rotation speed can be varied over the spin rotation time as needed. Those skilled in the art will recognize that other ranges of fluid volumes, spin rotation speeds, and spin rotation times within the above explicit ranges are contemplated and are within the scope of the present disclosure.

[0018] To perform the rinse step, the wafer can generally be spun at a low to moderate speed during fluid deposition and then spun at a higher speed after fluid deposition. The edge bead rinsing solution can be applied to the backside as well as the edge of the wafer. For example, the wafer can be spun at 5 rpm to 10,000 rpm during fluid deposition, and in further embodiments 50 rpm to 5000 rpm. The liquid deposition process can be performed for 1 second to 5 minutes, and in further embodiments about 5 seconds to about 3 minutes. Following liquid deposition, the wafer can be spun at a speed of at least 500 rpm, and in further embodiments 750 rpm to 6000 rpm, and the spinning after liquid deposition can be performed for 2 seconds to 10 minutes, and in further embodiments 5 seconds to about 5 minutes. The spin speed can be varied over the spin time as needed. One of ordinary skill in the art will recognize that other ranges of spin speeds and spin times within the above explicit ranges are contemplated and are within the scope of the present disclosure. The post-deposition spin-on can be followed by a subsequent rinse step, and the process can be optionally repeated.

[0019] After applying the edge bead solution to remove the edge bead, the edge of the wafer may appear visibly clean to inspection, as shown in FIG. 3 with a clean edge 134. As mentioned above, the edge bead rinsing process may include multiple rinsing steps with the same and / or different rinsing solutions to achieve the desired results. To fully evaluate the metal removal, the wafer may be inspected for residual metal. A suitable technique that has been put into practice to evaluate trace metals generally involves inductively coupled plasma mass spectrometry (ICP-MS). A variation of this analytical technique, called vapor phase decomposition-inductively coupled plasma mass spectrometry (VPD-ICP-MS), can be used to evaluate silicon wafer surfaces. This technique can be used to determine the residual metal per unit area of ​​the wafer surface along the edge. For the tin-based resist described in the examples, the amount of residual tin obtained is approximately 100×10 of the wafer area based on the wafer area of ​​the rinsed region. 10 atoms / cm 2 In the following, in a further embodiment, about 25×10 10 atoms / cm 2 or less, and in additional embodiments, about 10×10 10 atoms / cm 2 A person of ordinary skill in the art will recognize that other ranges of residual tin within the explicit ranges above are contemplated and are within the present disclosure.

[0020] In addition to using improved EBR solutions as described above, a coating can be applied along or across the substrate edge to further facilitate the reduction of residual metal along the wafer edge after EBR processing. Such coatings are generally insoluble in photoresist coating solutions and may or may not be completely or substantially removed as part of a subsequent EBR process. After the coating is applied, a resist solution can be deposited, which may or may not cover the coating as further described below. In some embodiments, a suitable coating can be a sacrificial material, such as polystyrene or amorphous carbon, which may or may not cover the entire substrate. Also, it may or may not be selectively removed with the resist coating during a subsequent EBR process. If the coating covers the entire wafer, the remaining coating can be used as a differentially etchable layer in the patterning stack, as in the case of amorphous carbon. In other embodiments, a suitable polymer coating, for example polystyrene, can be coated only along the periphery of the wafer and at least partially removed in a subsequent EBR process. In this case, the coating can be removed by EBR processing of the resist material, or alternatively, can be removed alternately by separate EBR processes. In other embodiments, a suitable coating, such as a surface modification layer coating or an anti-adhesion coating, may cover only the periphery of the wafer to prevent resist solution from adhering to the surface of the coating during resist deposition, and may or may not be removed in the subsequent EBR process.

[0021] Thus, the improved process may involve coating the edge surface region or the entire surface of the wafer with a secondary sacrificial material prior to coating the metal-based resist. In additional or alternative embodiments, the improved process may include coating the wafer edge surface region with a surface treatment layer that prevents the edge surface region from being wetted by the resist precursor solution. In general, neither the sacrificial layer nor the anti-adhesion layer requires a baking step prior to resist coating and EBR, providing a desirable process flow. Without wishing to be limited by theory, it is believed that the anti-adhesion material and process inhibits adhesion of metal-containing species to the substrate surface, which facilitates more complete removal of the photoresist with reduced metal residues upon application of an appropriate EBR solvent or mixture. The improved rinse solution described herein has proven particularly effective in removing residual tin atoms and may be used as a stand-alone EBR solution or in combination with the sacrificial layer or surface treatment layer described herein. As illustrated by the materials and methods in the examples, the level of residual tin after EBR processing can be reduced to an acceptable level using the methods described herein.

[0022] The choice of composition for the sacrificial material may be influenced by whether the coating covers the entire substrate / wafer only at the edge. In general, the sacrificial material may or may not be completely removed during the bead edge rinse, as long as the presence of the sacrificial material favors the removal of metal ions from the bead edge along the bead edge. If a sacrificial layer covers the wafer, it may also be removable when the corresponding resist is removed with or without irradiation. Specifically, the sacrificial material may be selected for removal using a developer for the resist. Additionally or alternatively, the sacrificial layer, such as an amorphous carbon layer or a spin-on carbon layer, may be removed during an etching step on the wafer / substrate material. Spin-on carbon materials are commercially available from JSR Corporation (Japan). See, for example, U.S. Pat. No. 9,102,129 B2 to Krishnamurthy et al., entitled "Spin-on Carbon Compositions for Lithographic Processing," incorporated herein by reference. The spin-on carbon material may be coated using a suitable coating process and may be dried, for example, by heating. Deposition of a CVD carbon layer is described, for example, in U.S. Patent Application Publication No. 2007 / 0037014 to Nagata, entitled "Method of Forming a Protective Film and a Magnetic Recording Medium Having a Protective Film Formed by the Method," which is incorporated herein by reference. A sacrificial coating is described that modifies the surface edge of a substrate in the absence of heating or other post-treatment, allowing removal of the tin-based resist along with the edge portion of the protective coating during EBR processing. A specific example using polystyrene as an edge coating for use with a tin-based resist is described below.

[0023] The process of covering a substrate with a sacrificial material over the entire substrate is shown generally in FIG. 4. After the substrate 150 is obtained, a layer of sacrificial material is applied 152 onto the substrate 150 to form a sacrificial layer 154. The application of the sacrificial layer 154 can be performed using, for example, spin coating, spray coating, knife edge coating, a coating solution suitable for depositing amorphous carbon using chemical vapor deposition (CVD) or other suitable coating techniques or combinations thereof as described above. A resist precursor solution can then be deposited 156 to form a resist layer 158. The resist precursor solution is typically applied by spin coating, although spray coating or other coating processes can be used. After forming the resist layer 158, an edge bead-relief step 160 can be performed to form an edged structure 162 having an edged sacrificial layer 164 and an edged resist layer 166. The edge bead-relief process is described further above and can be used in conjunction with the process of FIG. 4 as well. A top view of the edged structure 162 is shown in inset A of FIG. 4.

[0024] The process of covering the substrate with the sacrificial material can follow the procedure used to deposit the resist. A precursor solution for the sacrificial material can be deposited on a stationary wafer with appropriate coverage. The wafer can then be spun to distribute the fluid on the wafer surface. The amount of fluid can be selected based on the fluid properties such as concentration, viscosity, the desired thickness of the sacrificial material after drying, and other relevant parameters adjusted based on empirical evaluation. Generally, the amount of fluid can be about 0.1 mL to about 100 mL, and in further embodiments, about 0.25 mL to about 25 mL. After the fluid is deposited, the wafer can be spun to distribute the fluid on the wafer in order to spread the fluid. In this case, the wafer can be spun at 250 rpm to 10,000 rpm, and in further embodiments, 450 rpm to 6000 rpm for a time period of 2 seconds to 10 minutes, and in further embodiments, 5 seconds to 5 minutes. The spin rotation speed can be varied over the spin rotation time as needed. Multiple deposition and spin rotation steps can be used as needed to achieve the desired coating. A person of ordinary skill in the art will recognize that other ranges of fluid amounts, spin speeds and spin times within the explicit ranges above are contemplated and are within the present disclosure.

[0025] The use of a sacrificial layer along the edge is illustrated diagrammatically in FIG. 5. After obtaining a substrate 180, a sacrificial layer coating material can be applied 182 along the edge of the substrate 180 to form an edge-protected structure 184 having a sacrificial ring 186 on the substrate 180. The application of the sacrificial layer coating material can be performed along the edge, for example, using a bead-relief device modified to deliver the coating material along the edge. During delivery of the coating material, the substrate can be spun at a speed consistent with maintaining at least a substantial portion of the coating material along the edge. A top view of the edge-protected structure 184 is shown in inset A of FIG. 5. A resist solution can then be deposited 188 on the edge-protected structure 184 to form a resist layer 190. An edge bead-relief process 192 then removes both the sacrificial ring 186 and the resist material along the edge to form an edged structure 194 having an edged resist layer 196 on the substrate 180. The edge bead-relief process is described further above and can be used in conjunction with the processing of FIG. 5 as well. A top view of edged structure 194 is shown in inset B of FIG.

[0026] An alternative approach to providing a clean bead edge involves applying an edge coating surface treatment that inhibits resist from depositing on the surface along the edge. In particular, an edge coating composition can be applied whose critical surface tension is less than that of the resist coating composition. Critical surface tension (CST) is a property of a solid surface. Most inorganic solids, such as the surface of a silicon wafer, are hard and have a correspondingly high critical surface tension. Thus, most liquids will wet the silicon wafer. Coatings with low surface tension, such as silanes or fluorinated compounds, can be applied as surface treatments to act as anti-adhesion coatings along the wafer edge. The anti-adhesion coating can be applied on the wafer edge before applying the resist. Once the resist is applied, the resist is substantially non-sticky along the edge. The application of the resist is then followed by a bead edge rinse to remove any small amounts of resist that may remain along the edge. After the bead edge rinse, processing continues as normal. Because the edge is not patterned, the anti-adhesion coating along the edge does not need to be removed or processable during the wafer patterning process.

[0027] Suitable anti-adhesion compositions include, for example, fluorinated vinyl polymers such as polytetrafluoroethylene and their copolymers. The fluoropolymers can be fully fluorinated or not fully fluorinated, i.e., perfluoropolymers. Alkyl halide silanes may also be useful to provide anti-adhesion surfaces with low critical surface tension. Suitable silanes include, for example, alkyl trichlorosilanes such as heneicosafluorododecyltrichlorosilane (CST ≈ 6-7 dynes / cm at 25°C), heptadecylfluorodecyltrichlorosilane (CST ≈ 12 dynes / cm at 25°C), octadecyltrichlorosilane (CST ≈ 20-24 dynes / cm at 25°C). For resists with somewhat higher surface tensions, alkyl trialkoxysilanes can also provide sufficient anti-adhesion properties. Suitable alkyltrialkoxysilanes include, for example, methyltrimethoxysilane (CST ≈ 22.5 dynes / cm at 25°C), nonafluorohexyltrimethoxysilane (CST ≈ 23 dynes / cm at 25°C), or mixtures thereof. The illustrated alkyloxyhydroxytin-based resists illustrated herein had a surface tension of about 23 dynes / cm at 25°C. The selection of anti-adhesion coating materials can generally be influenced by the composition of the resist, but the coating composition generally has a critical surface tension of about 50 dynes / cm or less at 25°C, in further embodiments about 30 dynes / cm or less, and in further embodiments about 22 dynes / cm or less. Those skilled in the art will recognize that other ranges of critical surface tensions within the above explicit ranges are contemplated and are within the scope of the present disclosure.

[0028] The fluoropolymer can be distributed, for example, as a dispersion of polymeric microparticles. The dispersion liquid can be a fluorinated alkane, such as perfluorohexane, perfluorooctane, etc., or mixtures thereof. The silane can be distributed in a suitable solvent, such as methylene chloride, tetrahydrofuran (THF), toluene, or other suitable organic solvents, or mixtures thereof.

[0029] The application of an anti-adhesion coating along a substrate edge is shown diagrammatically in FIG. 6. After obtaining a substrate 210, a solution of a surface modification material is applied 212 to form an edge-protected structure 214 having an anti-adhesion edge coating 216 along the substrate 210. The application of the surface modification material to form the anti-adhesion edge coating 216 can be performed, for example, using an edge bead-resist device modified to deliver the material under suitable conditions to leave a substantial amount of coating material on the substrate edge. A top view of the edge-protected structure 214 is shown in inset A of FIG. 6. A resist precursor solution is then deposited 218 on the edge-protected structure 214 to form an edged resist layer 220. The application of the resist precursor solution can be performed using spin coating, spray coating or other suitable techniques. A top view of the structure having an edged resist layer 220 is shown in inset B of FIG. 6. An edge bead rinse is then performed 222 to remove any residual resist along the edge, and optionally all or a portion of the anti-adhesive edge coating 216, to form a rinsed structure 224 having a rinsed edge 226. The rinsed edge may or may not include any residual anti-adhesive edge coating. The edge bead rinse is performed as described above. A top view of the rinsed structure 224 is shown in inset C of FIG. 6.

[0030] With respect to the application of a sacrificial coating along the wafer edge as shown generally in FIG. 5 or the application of a surface modification composition as shown generally in FIG. 6, the wafer can generally be spun at a slow to moderate speed during fluid deposition and then spun at a higher speed after fluid deposition. For example, the wafer can be spun at 5 rpm to 500 rpm during fluid deposition, and in further embodiments 10 rpm to 250 rpm. The liquid deposition process can be performed for 5 seconds to 5 minutes, and in further embodiments about 15 seconds to about 3 minutes. Following liquid deposition, the wafer can be spun at a speed of at least 500 rpm, and in further embodiments 750 rpm to 4000 rpm, and the spinning after liquid deposition can be performed for 5 seconds to 10 minutes, and in further embodiments 10 seconds to about 5 minutes. The spin speed can be varied over the spin time as needed. One of ordinary skill in the art will recognize that other ranges of spin speeds and spin times within the above explicit ranges are contemplated and are within the scope of the present disclosure. The post-deposition spin-on can be followed by a subsequent rinse step, and the process can be optionally repeated.

[0031] In general, for any surface-modifying coating along the edge or on the wafer surface (e.g., sacrificial or anti-adhesion coating), the coating after drying may be about 10 microns thick or less in some embodiments, about 5 microns thick or less in some embodiments, and about 1 micron thick or less in further embodiments. In additional or alternative embodiments, thinner coatings may be desirable, such as coatings of about 1 nm to about 500 nm, coatings of about 5 nm to about 250 nm in further embodiments, and coatings of about 7 nm to about 100 nm in other embodiments. One of ordinary skill in the art will recognize that other ranges within the explicit thickness ranges above are contemplated and are within the scope of the present disclosure. Both the concentration and thickness of the liquid coating can be adjusted to achieve a coating of the desired thickness.

[0032] In all embodiments, one skilled in the art will recognize that the identity of the substrate is not limited other than by reasonable constraints recognized by those skilled in the art, such as size compatible with process equipment and sufficient mechanical strength to withstand processing. Suitable substrate surfaces may include silicon, such as single crystal silicon, polycrystalline silicon, amorphous silicon, ceramics, such as silicon oxide, titanium oxide, etc., or other suitable materials or combinations thereof. The substrate surface may or may not already be patterned prior to the initiation of further patterning processes where EBR treatment is part of a particular patterning step. EXAMPLES

[0033] Example 1 – Selected EBR Solvents and Carboxylic Acid Additives This example demonstrates the effectiveness of organic solvents with carboxylic acid additives for effective residue removal with a tin-based radiation patternable resist.

[0034] Experiments were performed with two different radiation patternable resists. The R1 resist comprised an organometallic tin oxyhydroxide resist containing a mixture of two different alkyl ligands, and the R2 resist comprised a mixture of an organometallic tin oxyhydroxide resist containing an alkyl ligand and a tin oxyhydroxide composition without an alkyl ligand. The resists were deposited on single crystal silicon wafers by spin coating. Immediately following resist deposition, the wafer was set to spin at 50 rpm while 5 mL of a rinse solution was dispensed onto the wafer to cover the entire wafer surface. Immediately after the rinse solution was dispensed, the wafer was spun at 1500 rpm for 45 seconds until dry. Optionally, following the spin drying of the first rinse solution, as shown in Table 1, a second separate rinse solution was dispensed onto the wafer and treated in the same manner, i.e., dispensed onto the wafer while spinning at 50 rpm, followed by spin drying at 1500 rpm for 45 seconds. If appropriate, the next volume of rinse solution was dispensed immediately after this high speed spin, and the procedure was repeated as above, typically five times, until after the high speed spin after the final rinse solution was applied. It is believed that the residue removal evaluated in these tests will approximate the effectiveness of an edge bead rinse process that rinses only the wafer edge.

[0035] Residual metal measurements were performed by ChemTrace® using vapor phase decomposition-inductively coupled plasma-mass spectrometry (VPD-ICP-MS) of the bevel edge. The results in Tables 1 and 2 were obtained using resist R1, and those in Table 3 were obtained using resist R2. To obtain the results in Table 1, a total of five rinse steps were performed with 5 ml per rinse step and one dry spin between each rinse step. In Tables 2 and 3, "n×mL" indicates multiple rinse steps of a particular volume with the same solution, such as 4×3 mL. Thus, 4×3 mL would indicate four rinse steps, each using 3 mL of solution. Table 4 lists the solvents and additives used in the previous tables. As the results show, R2 offers a greater challenge with respect to the desired removal of tin, but with the appropriate rinse solution, desirable results were obtained. However, for both resists, rinse solutions containing additives were successful in reducing.

[0036] [Table 1]

[0037] [Table 2]

[0038] [Table 3]

[0039] [Table 4]

[0040] Example 2 – Selected EBR Solvents and Fluorinated Acid Additives This example demonstrates the effectiveness of organic solvents containing fluorinated acid additives for effective bead edge rinsing with tin-based radiation patternable resists.

[0041] These experiments were carried out using the tin-based resist R1 and resist R2 mentioned in Example 1. The tests were carried out as described in Example 1, substituting the fluorinated additives. All of the tests in this example were carried out with one 5 mL EBR rinse step, followed by 5 x 5 mL rinses with the PGME / PGMEA solvent blend. The results obtained with R1 are shown in Table 5 and those obtained with R2 in Table 6. The notation N in the table stands for equivalent amount per liter using standard notation. These additives were particularly effective for the R2 resist. The solvents and additives for this example are shown in Table 7.

[0042] [Table 5]

[0043] [Table 6]

[0044] [Table 7]

[0045] Example 3 - Sacrificial Edge Underlayer This example demonstrates an improvement to the EBR process based on applying a sacrificial layer over the surface of the wafer.

[0046] A coating solution was applied to form a sacrificial underlayer coating over the entire wafer. The coating solution included 5 wt. % polystyrene dissolved in PGMEA and was applied to two wafers, and two additional wafers were used as controls. In each case, a 5 mL amount of the coating solution was dispensed onto a 100 mm wafer rotating at 50 rpm. Immediately after the dispensing process, the wafers were spun at 1500 rpm for 45 seconds. Next, a 1.5 mL amount of the organo-tin based resist solution R2 was dispensed onto three wafers (two edge-coated wafers and one control wafer) in a stationary position, and each wafer was spun at 1500 rpm for 45 seconds immediately after dispensing the resist solution.

[0047] At the end of the spinning of the wafer to spread the resist solution, an edge bead rinse (EBR) was performed as described in Example 1, using five rinse cycles with 5 mL of EBR rinse solution, except for the control wafers containing no resist, where no EBR rinse was performed. The EBR rinse solution was 65 / 35 vol% PGME / PGMEA for the control wafers containing resist but no edge coating, and for the wafers containing a sacrificial edge coating, the EBR solvent was either PGMEA or 2-heptanone. Measurements were taken to evaluate the tin concentration along the edge of the four wafers, and the results are shown in Table 8. The edge coating significantly improved the EBR process.

[0048] [Table 8]

[0049] Example 4 - Circumferential anti-adhesion coating This example demonstrates an improvement in EBR processing based on applying an anti-adhesive edge coating on the wafer.

[0050] Coating solutions were applied to form anti-adhesive edge coatings. The coating solutions contained 1 wt% poly(4,5-difluoro-2,2-bis(trifluoro-methyl)-1,3-dioxole-co-tetrafluoroethylene (FEO)) dissolved in perfluorooctane (Solution 1) or tetradecafluorohexane (Solution 2). Solution 1 and Solution 2 were applied to separate wafers, and two additional wafers were used as controls. To apply the coating solutions, a 5 mL amount of the coating solution was dispensed in the EBR machine along the edge of a 100 mm wafer rotating at 500 rpm. Immediately after the dispensing process, the wafer was spun at 1500 rpm for 45 seconds. Next, a 1.5 mL amount of the organo-tin based resist solution R2 was dispensed onto three wafers (two coated wafers and one control wafer) in a stationary position, and each wafer was spun at 1500 rpm for 45 seconds immediately after dispensing the resist solution.

[0051] At the end of the spinning of the wafer to spread the resist solution, an edge bead rinse (EBR) was performed as described in Example 1, using 5 cycles of rinsing with 5 mL of EBR rinse solution, except for the control wafer containing no resist, where no EBR rinse was performed. The EBR rinse solution was 65 / 35 vol% PGME / PGMEA for the control wafer containing resist but no coating, for the first wafer containing a sacrificial coating, the EBR was PGMEA, and for the wafer containing an anti-adhesive edge coating, the solvent used for EBR was the same as the solvent used to deposit the coating solution. Measurements were taken to evaluate the tin concentration along the edge of the four wafers, and the results are shown in Table 9. The edge coating significantly improved the EBR process.

[0052] [Table 9]

[0053] The above embodiments are intended to be illustrative and not limiting. Additional embodiments are within the scope of the claims. In addition, although the present invention has been described in relation to specific embodiments, those skilled in the art will recognize that changes in form and details may be made without departing from the spirit and scope of the present invention. Any incorporation by reference of the above documents is limited to not incorporating any subject matter contrary to the explicit disclosure herein. To the extent that a particular structure, composition and / or process is described herein with components, elements, ingredients or other divisions, the disclosure herein is understood to cover not only the specific embodiment, the embodiment that includes the particular component, element, ingredient, other division or combination thereof, but also the embodiment that is substantially composed of such specific component, ingredient or other division or combination thereof, which may include additional features that do not change the fundamental nature of the subject matter, as suggested in the description.

Claims

1. An apparatus for selectively removing metal-containing radiation sensitive materials, comprising: a wafer support configured to support a wafer including the layer of metal-containing radiation sensitive material; a dispenser configured to apply a fluid to at least a portion of a wafer mounted on the wafer support; a reservoir of a first fluid configured to deliver fluid to the dispenser for dispensing; The apparatus, wherein the first fluid comprises an organic compound having one or more carboxyl (--COOH) groups.

2. The device described in claim 1, wherein the metal-containing radiation-sensitive material comprises a metal selected from the group consisting of Sn, Hf, Zr, In, Te, Sb, Ni, Co, Ti, W, Ta, and Mo.

3. The device of claim 1, wherein the organic compound comprises a carboxylic acid.

4. The device of claim 1, wherein the organic compound comprises oxalic acid, citric acid, dihydroxyfumaric acid, acetic acid, 2-nitrophenylacetic acid, 2-ethylhexanoic acid, dodecanoic acid, tartaric acid, glucuronic acid, lactic acid, cyanoacetic acid, or a combination thereof.

5. The device of claim 1, wherein the organic compound comprises a fluorinated acid.

6. The apparatus of claim 1, wherein the first fluid comprises a second organic compound having one or more carboxyl (-COOH) groups.

7. The apparatus of claim 1, wherein the amount of the organic compound based on the total weight of the first fluid is between 0.1% by weight and 50% by weight.

8. The apparatus of claim 1, wherein the amount of the organic compound based on the total weight of the first fluid is between 0.25% by weight and 20% by weight.

9. The apparatus of claim 1, wherein the first fluid further comprises an organic solvent.

10. The apparatus of claim 9, wherein the organic solvent comprises a glycol ether or ester thereof, an alcohol, an ester, a ketone, a cyclic ester, a liquid cyclic carbonate, or a mixture thereof.

11. The apparatus of claim 9, wherein the organic solvent comprises propylene glycol methyl ether (PGME), propylene glycol methyl ether acetate (PGMEA), propylene glycol butyl ether (PGBE), ethylene glycol methyl ether, ethanol, propanol, isopropyl alcohol, isobutyl alcohol, hexanol, n-butyl acetate, ethyl acetate, ethylene glycol, propylene glycol, heptanone, propylene carbonate, butylene carbonate, gamma-butyrolactone, or a mixture thereof.

12. The apparatus of claim 1, wherein the first fluid comprises PGMEA and 0.2% to 20% by weight acetic acid.

13. The apparatus of claim 1, wherein the first fluid further comprises an inorganic fluorinated acid, a tetraalkylammonium compound, a sulfonic acid, sulfuric acid (H2SO4), a sugar acid, a phosphate ester, phosphoric acid, hydrofluoric acid (HF), a surfactant, water, or a mixture thereof.

14. The apparatus of claim 1, wherein the first fluid further comprises up to 30% by weight water.

15. The device of claim 1, wherein the metal-containing radiation-sensitive material comprises an alkyltin oxo / hydroxo moiety.

16. The device of claim 1, wherein the metal-containing radiation-sensitive material comprises Sn-C bonds, Sn-carboxylate bonds, or both.

17. The device of claim 1, further comprising a reservoir for a second fluid configured to deliver fluid to the dispenser for dispensing, the second fluid being different from the first fluid.

18. The apparatus of claim 1, further comprising a wafer on the wafer support, the wafer comprising a layer of metal-containing radiation-sensitive material.

19. The apparatus of claim 1, wherein the dispenser is configured to apply fluid to the entire surface of a wafer mounted on the wafer support.

20. The apparatus of claim 1, wherein the dispenser is configured to apply fluid along an edge of a wafer mounted on the wafer support to remove metal-containing radiation-sensitive material from an edge region of the wafer.

21. An apparatus as described in any one of claims 1 to 20, wherein the wafer support includes a spindle, the spindle being operably connected to a motor configured to rotate the spindle.

22. An apparatus as described in any one of claims 1 to 20, wherein the dispenser includes a nozzle configured to apply fluid to at least a portion of the wafer.

23. The apparatus, comprising: a spindle including the wafer support; a dispenser including a nozzle configured to apply a fluid to at least a portion of the wafer mounted on the spindle; and a reservoir of a first fluid configured to deliver the fluid to a nozzle for dispensing; the spindle is operably connected to a motor configured to rotate the spindle; The apparatus of any one of claims 1 to 20, wherein the first fluid comprises an organic solvent and an organic compound having one or more carboxyl (-COOH) groups.

24. The apparatus of claim 23, wherein the spindle has a hollow core, and the wafer support includes a negative pressure device configured to apply negative pressure within the hollow core to hold a wafer supported on the spindle based on the negative pressure.