Active material, electrode, secondary battery, battery pack, and vehicle
Niobium titanium oxide with a monoclinic structure and controlled crystallite diameter addresses the low energy density and efficiency issues of titanium oxide-based batteries by enhancing lithium ion diffusion, resulting in improved charge/discharge performance and cycle life.
Patent Information
- Application Number
- JP2023043293
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-17
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-03-17
AI Technical Summary
Existing secondary batteries using titanium oxide as a negative electrode face challenges with low energy density and poor charge/discharge efficiency due to high electrode potential and limited lithium ion diffusion, leading to rapid cycle life deterioration.
The use of niobium titanium oxide with a monoclinic structure, featuring a crystal lattice composed only of shared vertices and controlled crystallite diameter, enhances lithium ion insertion and extraction efficiency, thereby improving charge/discharge performance and cycle life.
The niobium titanium oxide phase with specific crystal structure and diameter range allows for stable rapid charging and discharging, offering higher energy density and extended cycle life compared to conventional titanium oxide-based batteries.
Smart Images

Figure 2024132504000001_ABST
Abstract
Description
[Technical field]
[0001] FIELD OF THE DISCLOSURE Embodiments of the present invention relate to an active material, an electrode, a secondary battery, a battery pack, and a vehicle. [Background technology]
[0002] In recent years, research and development of secondary batteries such as non-aqueous electrolyte secondary batteries, such as lithium ion secondary batteries, as high energy density batteries, has been actively promoted. Secondary batteries such as non-aqueous electrolyte secondary batteries are expected to be used as power sources for vehicles such as hybrid electric vehicles and electric vehicles, and for uninterruptible power sources for mobile phone base stations. Therefore, in addition to high energy density, secondary batteries are also required to have excellent other performances such as rapid charge and discharge performance and long-term reliability. For example, secondary batteries capable of rapid charge and discharge not only significantly reduce charging time, but also improve the power performance of vehicles such as hybrid electric vehicles and efficiently recover regenerative energy from power.
[0003] In order to enable rapid charging and discharging, it is necessary that electrons and lithium ions can move quickly between the positive and negative electrodes. However, when a battery using a carbon-based negative electrode is repeatedly charged and discharged rapidly, dendrites of metallic lithium are precipitated on the electrode, which may cause heat generation or fire due to an internal short circuit.
[0004] Therefore, batteries that use metal composite oxides instead of carbonaceous materials for the anode have been developed. Among them, batteries that use titanium oxide for the anode are capable of stable rapid charging and discharging and have a longer life than batteries that use carbon-based anodes.
[0005] However, titanium oxide has a higher potential relative to metallic lithium than carbonaceous materials, i.e., it is more noble. Moreover, titanium oxide has a low capacity per weight. Therefore, batteries using titanium oxide in the negative electrode have a problem of low energy density.
[0006] For example, the electrode potential of titanium oxide is about 1.5 V (vs. Li / Li) based on metallic lithium.+ ), which is higher (more noble) than the potential of a carbon-based negative electrode. The potential of titanium oxide is the potential of Ti when electrochemically inserting and extracting lithium. 3+ and Ti 4+ The charge is electrochemically limited because it is caused by an oxidation-reduction reaction between the two. + It is also true that rapid charging and discharging of lithium ions can be performed stably at high electrode potentials of around 1000 kV. Therefore, it has been difficult to lower the electrode potential in order to improve the energy density.
[0007] On the other hand, in terms of capacity per unit weight, the theoretical capacity of titanium dioxide (anatase structure) is about 165 mAh / g, and Li4Ti5O 12 The theoretical capacity of spinel-type lithium-titanium composite oxides such as (TLO) is also about 180mAh / g. On the other hand, the theoretical capacity of general graphite-based electrode materials is 385mAh / g or more. Thus, the capacity density of titanium oxides is significantly lower than that of carbon-based negative electrodes. This is because there are few sites for occluding lithium in the crystal structure of titanium oxides, and lithium is easily stabilized in the structure, resulting in a decrease in the actual capacity.
[0008] In view of the above, new electrode materials containing Ti and Nb are being investigated. Such niobium titanium oxide materials are expected to have high charge / discharge capacity. In particular, the oxide represented by TiNb2O7 (TNO) has a high theoretical capacity of more than 380 mAh / g. Therefore, niobium titanium oxide is Li4Ti5O 12 It is expected to be a high-capacity material to replace [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2019-169343 A [Non-patent literature]
[0010] [Non-Patent Document 1] International Tables for Crystallography (2006). 1st online ed. Chester: International Union of Crystallography. [Non-Patent Document 2] "Practice of Powder X-ray Analysis" First Edition (2002) Edited by the X-ray Analysis Research Roundtable of the Japan Society for Analytical Chemistry, edited by Izumi Nakai and Fujio Izumi (Asakura Publishing) [Non-Patent Document 3] Jian-Tao Han, Yun-Hui Huang and John B. Goodenough, Chem. Mater. 2011, 23, 8, 2027-2029 Summary of the Invention [Problem to be solved by the invention]
[0011] The object is to provide an active material and an electrode capable of realizing a secondary battery exhibiting excellent charge / discharge efficiency and cycle life performance, a secondary battery and a battery pack exhibiting excellent charge / discharge efficiency and cycle life performance, and a vehicle equipped with this battery pack. [Means for solving the problem]
[0012] According to an embodiment, an active material is provided that includes a niobium titanium oxide phase having a monoclinic structure. The niobium titanium oxide phase has a crystal lattice in which the bond angle distortion in the (Nb, Ti)O6 octahedral site composed only of corner sharing is 0.8 σ 2 / deg 2 The niobium titanium oxide phase has a crystal structure including at least one octahedral site in a unit cell, the crystallite size of which is within the range of 85 nm to 130 nm.
[0013] According to another embodiment, an electrode is provided that includes an active material according to the above embodiments.
[0014] According to yet another embodiment, there is provided a secondary battery comprising a positive electrode, a negative electrode, and an electrolyte. The negative electrode is an electrode according to the above embodiment.
[0015] According to yet another embodiment, there is provided a battery pack including a secondary battery, the secondary battery of the battery pack including the secondary battery according to the above embodiment.
[0016] According to still another embodiment, a vehicle is provided that is equipped with a battery pack according to the above embodiment. [Brief description of the drawings]
[0017] [Figure 1] Schematic diagram showing the crystal structure of niobium titanium oxide Nb2TiO7. [Diagram 2] FIG. 2 is a schematic diagram showing the crystal structure of FIG. 1 as viewed from another direction. [Diagram 3] A schematic diagram showing only a portion of the crystal structure in FIG. [Figure 4] 1 is a graph showing the results of Rietveld analysis using a synchrotron X-ray diffraction pattern of an example of an active material according to an example. [Diagram 5] FIG. 1 is a cross-sectional view illustrating an example of a secondary battery according to an embodiment. [Figure 6] 6 is an enlarged cross-sectional view of a portion A of the secondary battery shown in FIG. 5. [Figure 7] FIG. 4 is a partially cutaway perspective view illustrating a schematic diagram of another example of a secondary battery according to an embodiment. [Figure 8] 8 is an enlarged cross-sectional view of a portion B of the secondary battery shown in FIG. 7. [Figure 9] FIG. 1 is a perspective view illustrating an example of a battery pack according to an embodiment. [Figure 10] FIG. 1 is an exploded perspective view illustrating an example of a battery pack according to an embodiment. [Figure 11] FIG. 11 is a block diagram showing an example of an electric circuit of the battery pack shown in FIG. [Figure 12] 1 is a partially see-through view illustrating an example of a vehicle according to an embodiment. [Figure 13]1 is a diagram illustrating an example of a control system for an electrical system in a vehicle according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] TNO has a steeper slope of the potential curve during charging and discharging than TLO. It has been confirmed that in batteries using TNO as the anode, the positive electrode potential increases slightly due to a shift in the operation window, and cycle life tends to deteriorate rapidly. The SOC shift occurs because the insertion and desorption of Li ions inside the TNO particles does not proceed smoothly, resulting in Li remaining in the lattice and reducing the charge and discharge efficiency.
[0019] Hereinafter, the embodiments will be described with reference to the drawings. Note that the same reference numerals are used to designate common components throughout the embodiments, and duplicated descriptions will be omitted. Each figure is a schematic diagram for explaining the embodiments and for facilitating understanding thereof, and the shapes, dimensions, ratios, etc. may differ from those of the actual device, but these can be appropriately modified in design by taking into consideration the following explanation and known techniques.
[0020] (First embodiment) According to a first embodiment, an active material is provided, which includes a niobium titanium oxide phase having a monoclinic crystal structure, in which the bond angle distortion in the NbTiO6 / TiO6 octahedral sites formed by corner sharing only in the crystal lattice is 0.8 σ 2 / deg 2 The niobium titanium oxide phase has a crystallite size of 85 nm to 130 nm. The crystal structure is a Nb2TiO7 type crystal structure or a Nb 10 Ti2O 29 In other words, typical examples of the niobium titanium oxide phase are the Nb2TiO7 phase and Nb 10 Ti2O 29 The composition comprises at least one phase selected from the group consisting of:
[0021] This active material was achieved by focusing on the (Nb, Ti)O6 octahedral distortion so that the insertion and removal of Li ions in the TNO particles can be performed smoothly. In conventional synthesis and grinding methods, the bond angle distortion (bond angle dispersion) of the octahedra sharing the corners is greater than 0.8, which suggests the possibility that the diffusion of Li ions in the lattice is hindered and the charge and discharge efficiency is low. Therefore, by using a thin-film swirling high-speed mixer to minimize damage to the particle surface during grinding, the bond angle distortion was significantly alleviated, making it possible to extend the charge and discharge efficiency and cell life.
[0022] In addition, the crystallite diameter of the niobium titanium oxide phase obtained by synthesis is set to 85 nm or more and 130 nm or less. In the niobium titanium oxide phase having a crystallite diameter within this range, the movement of Li ions in the crystal lattice during charging and discharging is facilitated, and an active material having excellent cycle life can be provided. If the crystallite diameter is smaller than 85 nm, the capacity and cycle life are reduced. If the crystallite diameter is larger than 130 nm, the particle diameter becomes too coarse, and the diffusion distance of lithium ions becomes long, resulting in poor rate performance.
[0023] The Nb2TiO7 phase is described below. The Nb2TiO7 phase is, for example, a compound represented by the general formula Nb 2-x M1 x Ti 1-y M2 y In this case, M1 and M2 include at least one selected from the group consisting of K, Zr, Sn, V, Ta, Mo, W, P, Y, Fe, Co, Cr, Mn, Ni, and Al. M1 and M2 may be the same or different from each other. The subscripts x and y are within the ranges of 0≦x<2 and 0≦y<1, respectively. It is preferable that the subscript x is 1 or less, and it is more preferable that the subscript x is 0.5 or less. In addition, when Li is inserted into the Nb2TiO7 phase, the composition is Li a Nb 2-x M1 x Ti 1-y M2 y O7, where the subscripts x and y are as above, and the subscript a is in the range 0≦a≦5.
[0024] As an example of a monoclinic crystal structure of a niobium titanium oxide phase, schematic diagrams of the monoclinic crystal structure of Nb2TiO7 having the symmetry of space group C2 / m are shown in Figures 1 to 3. The space group C2 / m referred to here refers to the symmetry of space group number 12 described in the International Tables for Crystallography (Non-Patent Document 1), specifically, in Vol. A: Space-group symmetry of the said material (2nd online edition (2016); ISBN: 978-0-470-97423-0, doi: 10.1107 / 97809553602060000114).
[0025] As shown in FIG. 1, in the crystal structure of monoclinic Nb2TiO7, metal ions 101 and oxide ions 102 form octahedrons 103 that function as the framework structure of the crystal structure. Nb ions and Ti ions are randomly arranged at the positions of the metal ions 101 in a ratio of Nb:Ti=2:1. The octahedrons 103 are arranged three-dimensionally alternately, so that void spaces 104 exist between the octahedrons 103. These void spaces 104 serve as hosts for lithium ions. Lithium ions can be inserted into this crystal structure in an amount of 0 moles to a maximum of 5.0 moles. Therefore, the composition when 0 to 5.0 moles of lithium ions are inserted is Li a It can be expressed as Nb2TiO7(0≦a≦5).
[0026] In FIG. 1, regions 105 and 106 are portions that have two-dimensional channels in the
[0100] and
[0010] directions. As shown in FIG. 2, the crystal structure of monoclinic Nb2TiO7 has a void portion 107 in the
[0001] direction. This void portion 107 has a tunnel structure that is favorable for the conduction of lithium ions, and serves as a conductive path in the
[0001] direction that connects regions 105 and 106. The existence of this conductive path enables lithium ions to travel between regions 105 and 106. Niobium titanium oxide also has a low resistance of 1.5 V (vs. Li / Li +Therefore, an electrode containing niobium titanium oxide as an active material can realize a battery capable of stable repeated rapid charging and discharging.
[0027] Furthermore, in the above crystal structure, when lithium ions are inserted into the voids 104, the metal ions 101 constituting the framework are reduced to trivalent, thereby maintaining the electrical neutrality of the crystal. In niobium titanium oxide, not only are Ti ions reduced from tetravalent to trivalent, but Nb ions are reduced from pentavalent to trivalent. Therefore, the reduction valence per active material weight is large. Therefore, even if many lithium ions are inserted, it is possible to maintain the electrical neutrality of the crystal. Therefore, the energy density is higher than that of compounds such as titanium oxide that contain only tetravalent cations.
[0028] FIG. 3 shows a schematic diagram including only two rows of octahedra on the front side ((101) side) of the crystal structure in FIG. 1. The octahedron 113, which is centered on the 2a site among the sites of the metal ion 101 (Nb ion or Ti ion), shares the oxide ion 102 with the adjacent octahedrons 123 and 143 only by corner sharing. Among the multiple octahedra centered on the 4i site, the octahedron 123 also shares the oxide ion 102 with other octahedra only by corner sharing, whereas the octahedrons 133, 143, and 153 share the oxide ion 102 with each other by edge sharing. The 2a site and 4i site referred to here refer to the metal ion sites described in the symmetry of the International Tables Volume A mentioned above.
[0029] Next, Nb 10 Ti2O 29 The phase is explained below. 10 Ti2O 29 The composition of the phase is, for example, the general formula Nb 10-z M1 z Ti 2-y M2 y O 29Here, M1 and M2 are the same as those for the Nb2TiO7 phase. The subscript z is in the range of 0≦z≦5, and the subscript y is in the range of 0≦y<1. In addition, Nb 10 Ti2O 29 When lithium ions are inserted into the phase, the composition is Li b Nb 10-z M1 z Ti 2-y M2 y O 29 Here, the subscripts z and y are as above, and the subscript b is in the range 0≦b≦22.
[0030] Nb 10 Ti2O 29 The basic framework structure of the phase is similar to the crystal structure of monoclinic Nb2TiO7 shown in Figures 1 to 3. However, Nb 10 Ti2O 29 The phase is typically represented by the space group C2 / m, but there are some reports that the unit cell is classified as the space group A2 / m. When lithium ions are inserted into the voids 104, the metal ions 101 that make up the framework are reduced to trivalent ions, thereby maintaining the electrical neutrality of the crystal. Nb 10 Ti2O 29 When lithium ions are inserted into the phase, the composition is Li x Nb 10 Ti2O 29 (0≦x≦22).
[0031] The monoclinic niobium titanium oxide phase includes the above-mentioned Nb2TiO7 phase and Nb 10 Ti2O 29 In addition to the phase, Nb 14 TiO 37 Phase and Nb 24 TiO 64 Phases such as Nb 14 TiO 37 Phase and Nb 24 TiO 64The crystal lattice of the Nb2TiO7 phase does not contain any (Nb, Ti)O6 octahedral sites that are composed only of corner sharing. In the crystal lattice, the area surrounding the octahedral sites that are composed only of corner sharing is more flexible than the area surrounding the octahedral sites that contain other types of sharing such as edge sharing. Therefore, the Nb2TiO7 phase and Nb 10 Ti2O 29 In this phase, Li ions can be easily inserted and removed, which results in good charge-discharge efficiency and cycle life performance.
[0032] The form of the active material (niobium titanium oxide) according to the embodiment is not particularly limited. The active material may include, for example, particles containing a niobium titanium oxide phase or particles consisting of a niobium titanium oxide phase. The active material may include, for example, a Nb2TiO7 phase and / or a Nb 10 Ti2O 29 The active material may have the form of primary particles that contain a single Nb2TiO7 phase, as well as such single or mixed niobium titanium oxide phase and further other phases. Alternatively, the active material may have the form of primary particles that contain a single Nb2TiO7 phase, as well as Nb 10 Ti2O 29 The niobium titanium oxide phase may be a mixture of primary particles and primary particles of a single phase, or a mixture of at least one of the single phase primary particles and primary particles of another phase. The primary particles may be aggregated to form secondary particles. The niobium titanium oxide phase particles may be a mixture of primary particles and secondary particles.
[0033] The average particle size of the primary particles of the niobium titanium oxide phase is preferably in the range of 0.1 μm to 10 μm. The average particle size here is the particle size D at which the volume cumulative frequency is 50% from the small particle size side in a particle size distribution chart obtained by the laser diffraction scattering method described later. 50 The particle size distribution chart may correspond to a histogram for the active material sample.
[0034] The particles of the niobium titanium oxide phase may have a carbon-containing layer on the surface. The carbon-containing layer may be attached to the surface of the primary particles, or may be attached to the surface of the secondary particles. Alternatively, the particles of the niobium titanium oxide phase may contain secondary particles formed by agglomeration of primary particles having a carbon-containing layer attached to the surface. Such secondary particles can exhibit excellent electrical conductivity because carbon is present between the primary particles. In an embodiment containing such secondary particles, an electrode using the active material can exhibit lower resistance, which is preferable.
[0035] <Method of manufacturing active material> The active material according to the embodiment can be produced, for example, by the synthesis method described below.
[0036] First, the starting materials are mixed. As the starting materials containing niobium and titanium, oxides or salts containing Nb and Ti are prepared. For example, Nb2O5 particles and TiO2 particles can be used as the starting materials. These starting materials are mixed according to the composition of the desired niobium titanium oxide phase.
[0037] The mixture of raw materials is put into pure water and mixed for 1 to 3 hours in a wet bead mill. At this time, various dispersants may be used to disperse well. The obtained slurry mixture is granulated and dried in a spray dryer. At this time, the particle size of the granules is set to about 5 μm to 30 μm. If the particle size is 5 μm or more, the progress of aggregation during the synthesis reaction can be suppressed, and if it is 30 μm or less, the thin film rotary crushing performed in the subsequent process is easy.
[0038] Next, the obtained aggregate is subjected to pre-baking (first baking). The pre-baking is desirably performed at a temperature of 600°C to 1100°C for 1 hour to 12 hours. By performing the pre-baking, it is possible to remove a small amount of impurity components (e.g., water, organic matter, etc.) adsorbed to the raw material powder. The pre-baking may be omitted.
[0039] The main firing (second firing) is preferably performed at a temperature of 900° C. to 1200° C. for 1 hour to 10 hours, and more preferably at a temperature of 950° C. to 1050° C. for 2.5 hours to 3.5 hours.
[0040] The obtained sintered granules are pulverized using a thin film swirling mixer. 50 The grinding conditions are set so that the particle size is 0.1 μm or more and 10 μm or less.
[0041] <Crystal structure measurement> The crystal structure of the active material can be confirmed by synchrotron radiation X-ray measurement and Rietveld analysis of the measurement results. As the equipment for synchrotron radiation X-ray measurement, for example, BL19B2 of the large synchrotron radiation facility SPring-8 operated by the National Research and Development Agency RIKEN (RIKEN) can be used.
[0042] The active material sample is filled into Lindemann glass (φ 0.3 mm) and measurements are performed at a wavelength of 0.8 Å. The measurement data is used to perform Rietveld analysis. In the Rietveld method, a diffraction pattern is calculated from a pre-estimated crystal structure model. By fitting all of these calculated values to the actual measured values, the parameters related to the crystal structure (lattice constants, atomic coordinates, occupancy, etc.) can be precisely analyzed. This makes it possible to investigate the characteristics of the crystal structure of the phases contained in the sample. The characteristics of the crystal structure that can be obtained include the symmetry of the crystal structure, i.e., the space group to which the crystal structure belongs, and the bond angle distortion (σ 2 / deg 2 ) are included.
[0043] As an analysis program, for example, RIETAN-FP is used. The analysis method using RIETAN-FP is explained in detail, for example, in Chapter 9 "Let's try using RIETAN-FP" of Non-Patent Document 2 ("Practical Application of Powder X-Ray Analysis," edited by the X-Ray Analysis Research Forum of the Japan Society for Analytical Chemistry, edited by Nakai Izumi and Izumi Fujio (Asakura Publishing)). RIETAN-FP is a program for Rietveld analysis that was distributed free of charge on its developer's online webpage (closed as of January 2023). As of March 2023, this program is available from the following web archive: http: / / web.archive.org / web / 20220209014122fw_ / http: / / fujioizumi.verse.jp / download / download.html.
[0044] Figure 4 shows an example of the results of a Rietveld analysis using a synchrotron radiation X-ray diffraction pattern. The example shown in Figure 4 is the result of an analysis performed with the space group C2 / m assuming a TiNb2O7 type crystal structure. The positions of the calculated peak 11 (solid line) and the observed peak 12 (plot) for the space group C2 / m both match the allowable Bragg reflection 14, and the peak intensity difference 13 between the calculated peak 11 and the observed peak 12 is small, as shown in Figure 4, in which a good fit was obtained. Nb 10 Ti2O 29 For the crystal structure, for example, the analysis is carried out with the space group being A2 / m.
[0045] When synchrotron radiation X-ray diffraction measurement is performed on the active material contained in the electrode, for example, a sample is prepared as follows.
[0046] First, in order to grasp the crystalline state of the active material, the active material is placed in a state in which lithium ions are completely removed. For example, when the active material is used in a negative electrode, the battery is placed in a completely discharged state. For example, the battery is discharged at a current of 0.1 C in a 25° C. environment until the rated end voltage or the battery voltage reaches 1.0 V, and the current value during discharge is set to 1 / 100 or less of the rated capacity, thereby placing the battery in a discharged state. Residual lithium ions may still be present even in the discharged state.
[0047] Next, the battery is disassembled in a glove box filled with argon, and the electrodes are removed and washed with an appropriate solvent. An example of an appropriate solvent is ethyl methyl carbonate. If the electrodes are not washed sufficiently, lithium ions remaining in the electrodes may cause impurity phases such as lithium carbonate and lithium fluoride to be mixed in. In that case, it is recommended to use an airtight container in which the measurement atmosphere can be in an inert gas. The washed electrodes are cut into strips with a width approximately equal to the diameter of the capillary used for synchrotron radiation X-ray diffraction to prepare the measurement sample. This sample is directly inserted into the capillary to perform the measurement.
[0048] At this time, the metal foil, conductive agent, and binder, which are the current collector, are measured in advance to grasp the peaks derived from them. Of course, if these are grasped in advance, this operation can be omitted. When the peak of the current collector and the peak of the active material overlap, it is desirable to peel off the active material-containing layer from the current collector and measure it. This is to separate the overlapping peaks when quantitatively measuring the peak intensity. The active material-containing layer may be physically peeled off, but it is easier to peel off by applying ultrasonic waves in a solvent. When ultrasonic treatment is performed to peel off the active material-containing layer from the current collector, the electrode mixture powder (including the active material, conductive agent, and binder) can be recovered by volatilizing the solvent. The recovered electrode mixture powder can be filled into a capillary and measured to perform synchrotron radiation X-ray diffraction measurement of the active material. The electrode mixture powder recovered by ultrasonic treatment can also be subjected to various analyses other than synchrotron radiation X-ray diffraction measurement.
[0049] <Confirmation of crystallite size> To determine the crystallite diameter (crystallite size), measurements can be performed using Cu-Kα radiation in a powder X-ray diffraction apparatus typically used in laboratories.
[0050] First, the target sample is crushed until the average particle size is about 5 μm. The average particle size can be determined by laser diffraction. The crushed sample is filled into a holder portion with a depth of 0.2 mm formed on a glass sample plate. At this time, care is taken to ensure that the sample is sufficiently filled into the holder portion. Also, care is taken to ensure that there are no cracks or gaps due to insufficient filling of the sample. Next, another glass plate is used from the outside to sufficiently press and smooth the surface. At this time, care is taken to ensure that there are no unevenness from the reference surface of the holder due to overfilling or underfilling. Next, the glass plate filled with the sample is placed in a powder X-ray diffractometer, and an X-ray diffraction (XRD) pattern is obtained using Cu-Kα radiation.
[0051] When the active material contained in the electrode is used as a sample, for example, the electrode composite powder recovered by dismantling the battery and performing ultrasonic treatment as described above can be used. Alternatively, the battery is dismantled and the electrodes are cleaned, and the cleaned electrodes are cut to have an area approximately equal to the area of the holder of the powder X-ray diffraction apparatus to prepare a measurement sample. This sample is directly attached to a glass holder and then measured.
[0052] As an apparatus for powder X-ray diffraction measurement, for example, SmartLab manufactured by Rigaku Co., Ltd. is used. The measurement conditions are as follows: X-ray source: Cu target Output: 45kV 200mA Soller slit: 5° for both incidence and reception Step width (2θ): 0.02 deg Scan speed: 20deg / min Semiconductor detector: D / teX Ultra 250 Measurement range: 5°≦2θ≦90° Sample plate holder: Flat glass sample plate holder (thickness 0.5 mm).
[0053] When using other equipment, perform measurements using standard Si powder for powder X-ray diffraction to find conditions that give measurement results for peak intensity, half-width, and diffraction angle equivalent to those obtained by the above equipment, and then measure the sample under those conditions.
[0054] The conditions of the XRD measurement are such that an XRD pattern applicable to Rietveld analysis can be obtained. To collect data for Rietveld analysis, specifically, the step width is set to 1 / 3-1 / 5 of the minimum half-width of the diffraction peak, and the measurement time and / or X-ray intensity are appropriately adjusted so that the intensity at the peak position of the most intense reflection is 5000 cps or more.
[0055] The diffraction peak with the strongest diffraction intensity in the obtained X-ray diffraction spectrum is selected. For example, for the Nb2TiO7 phase, the peak of the (110) plane is measured. The crystallite size can be calculated from the half-width of the obtained peak. Here, the crystallite size is calculated from the Scherrer formula shown in the following Equation 1 and Equation 2.
[0056] Crystallite size (nm) = Kλ / βcosθ (1) β = (β e 2 -β o 2 ) 1 / 2 (2) Here, K is the Scherrer constant and is set to 0.9, λ is the wavelength of X-rays and is set to 0.15406 nm, θ is the Bragg angle, β is the integral width of the diffraction peak, and β e : Half-width of the diffraction peak, and β o : Corrected half-width value (0.07°).
[0057] <Measurement of the composition of niobium titanium oxide phase> The composition of the niobium titanium oxide phase in the active material can be analyzed, for example, by using inductively coupled plasma (ICP) optical emission spectroscopy.
[0058] Specifically, the composition of the active material incorporated in the battery is measured by ICP emission spectroscopy according to the following procedure.
[0059] First, the electrode containing the active material is removed from the secondary battery and washed according to the procedure described above. The washed electrode is placed in a suitable solvent and irradiated with ultrasonic waves. For example, the electrode is placed in ethyl methyl carbonate in a glass beaker and vibrated in an ultrasonic cleaner, whereby the active material-containing layer can be peeled off from the current collector.
[0060] Next, the peeled active material-containing layer is dried under reduced pressure. The obtained active material-containing layer is pulverized in a mortar or the like to produce a powder containing the target active material, conductive agent, binder, etc. A liquid sample containing the active material can be prepared by dissolving this powder in an acid. Examples of the acid that can be used at this time include hydrochloric acid, nitric acid, sulfuric acid, and hydrogen fluoride. The liquid sample can be subjected to ICP emission spectroscopy to determine the composition of the components in the active material, for example, the composition of the niobium titanium oxide phase.
[0061] <Average particle size measurement> The electrode mixture powder described in the section on synchrotron radiation X-ray diffraction measurement above is sintered to burn off the conductive agent and binder. The remaining active material particles are dispersed in N-methyl-2-pyrrolidone (NMP) solvent and ultrasonically treated to break up secondary particles and other aggregates, thereby obtaining a dispersion solution of active material primary particles as a sample for particle size distribution measurement. The particle size distribution of the constituent particles of this dispersion solution is measured using a laser diffraction distribution measurement device. For example, a Microtrack MT3100II manufactured by Microtrack Bell Co., Ltd. can be used as the measurement device.
[0062] The ultrasonic treatment for obtaining the dispersion solvent is carried out by a sample supply system attached to the laser diffraction distribution measurement device. For example, the ultrasonic treatment is carried out for 300 seconds at an output of 40 W. The particle diameter D at which the volume cumulative frequency is 50% from the small particle diameter side in the particle size distribution chart obtained by the laser diffraction scattering method is 50 is the average primary particle size.
[0063] According to a first embodiment, an active material is provided, which includes a niobium titanium oxide phase having a monoclinic crystal structure, and in which the bond angle distortion in the (Nb, Ti)O6 octahedral site formed by only corner sharing is 0.8 σ 2 / deg 2 The unit lattice contains at least one octahedral site having the following structure: The crystallite diameter of the niobium titanium oxide phase is 85 nm or more and 130 nm or less. Such an active material can realize a secondary battery that exhibits excellent charge / discharge efficiency and cycle life performance.
[0064] Second embodiment According to a second embodiment, an electrode is provided.
[0065] The electrode according to the second embodiment includes the active material according to the first embodiment. This electrode can be a battery electrode that includes the active material according to the first embodiment as a battery active material. The electrode as a battery electrode can be, for example, a negative electrode that includes the active material according to the first embodiment as a negative electrode active material.
[0066] Such an electrode may include a current collector and an active material-containing layer. The active material-containing layer may be formed on one or both sides of the current collector. The active material-containing layer may include an active material and, optionally, a conductive agent and a binder.
[0067] The active material-containing layer may contain a single active material according to the first embodiment, or may contain two or more types of active materials according to the first embodiment, or may contain a mixture of one or more types of active materials according to the first embodiment and one or more types of other active materials.
[0068] For example, when the active material according to the first embodiment is contained as a negative electrode active material, examples of other active materials include lithium titanate having a ramsdellite structure (e.g., Li 2+y Ti3O7, 0≦y≦3), lithium titanates with spinel structure (e.g., Li 4+x Ti5O 12, 0≦x≦3), titanium dioxide (TiO2), anatase type titanium dioxide, rutile type titanium dioxide, niobium pentoxide (Nb2O5), hollandite type titanium composite oxide, orthorhombic titanium-containing composite oxide, and monoclinic niobium titanium oxide that does not contain (Nb, Ti)O6 octahedral sites composed only of corner sharing.
[0069] As an example of the above-mentioned orthorhombic titanium-containing composite oxide, Li 2+a M I 2-b Ti 6-c M II d O 14+σ In this case, the compound represented by M I is at least one selected from the group consisting of Sr, Ba, Ca, Mg, Na, Cs, Rb and K. II is at least one selected from the group consisting of Zr, Sn, V, Nb, Ta, Mo, W, Y, Fe, Co, Cr, Mn, Ni, and Al. The subscripts in the composition formula are 0≦a≦6, 0≦b<2, 0≦c<6, 0≦d<6, and -0.5≦σ≦0.5. Specific examples of orthorhombic titanium-containing composite oxides include Li 2+a Na2Ti6O 14 (0≦a≦6).
[0070] As an example of a monoclinic niobium titanium oxide that does not contain NbO6 octahedral sites or TiO6 octahedral sites that are composed only of corner sharing, Li x Nb 14 TiO 37 and 0≦x≦29. Other examples include compounds such as Li x Nb 24 TiO 64 and 0≦x≦49. In the crystal structures of these compounds, sharing other than vertex sharing, such as edge sharing, is formed at any octahedral site.
[0071] The conductive agent is blended to improve the current collecting performance and to reduce the contact resistance between the active material and the current collector. Examples of the conductive agent include carbonaceous materials such as vapor grown carbon fiber (VGCF), carbon black such as acetylene black, graphite, carbon nanotubes, and carbon nanofibers. One of these may be used as the conductive agent, or two or more may be used in combination as the conductive agent. Alternatively, instead of using a conductive agent, a carbon coating or an electronically conductive inorganic material coating may be applied to the surface of the active material particles.
[0072] The binder is blended to fill the gaps between the dispersed active materials and to bind the active materials and the current collector. Examples of the binder include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine-based rubber, styrene butadiene rubber, polyacrylic acid compounds, imide compounds, carboxymethylcellulose (CMC), and salts of CMC. One of these may be used as the binder, or two or more may be used in combination as the binder.
[0073] The mixing ratio of the active material, conductive agent and binder in the active material-containing layer can be appropriately changed depending on the application of the electrode. For example, when the electrode is used as a negative electrode of a secondary battery, it is preferable to mix the active material (negative electrode active material), conductive agent and binder at a ratio of 68% by mass or more and 96% by mass or less, 2% by mass or more and 30% by mass or less, and 2% by mass or more and 30% by mass or less, respectively. By making the amount of the conductive agent 2% by mass or more, the current collection performance of the active material-containing layer can be improved. In addition, by making the amount of the binder 2% by mass or more, the binding property between the active material-containing layer and the current collector becomes sufficient, and excellent cycle performance can be expected. On the other hand, it is preferable to make the conductive agent and the binder 30% by mass or less, respectively, in order to increase the capacity.
[0074] The current collector is made of a material that is electrochemically stable at the potential at which lithium (Li) is inserted and removed from the active material. For example, when the active material is used as a negative electrode active material, the current collector is preferably made of copper, nickel, stainless steel, or aluminum, or an aluminum alloy containing one or more elements selected from Mg, Ti, Zn, Mn, Fe, Cu, and Si. The thickness of the current collector is preferably 5 μm or more and 20 μm or less. A current collector having such a thickness can balance the strength and weight of the electrode.
[0075] The current collector may also include a portion on the surface of which the negative electrode active material-containing layer is not formed, and this portion can function as a negative electrode current collecting tab.
[0076] The electrode can be produced, for example, by the following method. First, an active material, a conductive agent, and a binder are suspended in a solvent to prepare a slurry. This slurry is applied to one or both sides of a current collector. Next, the applied slurry is dried to obtain a laminate of an active material-containing layer and a current collector. After that, the laminate is pressed. In this manner, an electrode is produced.
[0077] Alternatively, the electrode may be prepared by the following method: first, the active material, the conductive agent, and the binder are mixed to obtain a mixture, then the mixture is formed into pellets, and then the pellets are placed on a current collector to obtain an electrode.
[0078] The electrode according to the second embodiment includes the active material according to the first embodiment, and therefore, such an electrode can realize a secondary battery that exhibits excellent charge / discharge efficiency and cycle life performance.
[0079] (Third embodiment) According to the third embodiment, a secondary battery including a negative electrode, a positive electrode, and an electrolyte is provided. This secondary battery includes the electrode according to the second embodiment as the negative electrode. That is, the secondary battery according to the third embodiment includes an electrode including the active material according to the first embodiment as a battery active material as the negative electrode.
[0080] The secondary battery may further include a separator disposed between the positive electrode and the negative electrode. The negative electrode, the positive electrode, and the separator may constitute an electrode group. The electrolyte may be held in the electrode group.
[0081] Moreover, such a secondary battery can further include an exterior member that houses the electrode group and the electrolyte.
[0082] Furthermore, such a secondary battery may further include a negative electrode terminal electrically connected to the negative electrode and a positive electrode terminal electrically connected to the positive electrode.
[0083] Such a secondary battery may be, for example, a lithium secondary battery. The secondary battery also includes a non-aqueous electrolyte secondary battery that contains a non-aqueous electrolyte.
[0084] The negative electrode, the positive electrode, the electrolyte, the separator, the exterior member, the negative electrode terminal, and the positive electrode terminal will be described in detail below.
[0085] 1) Negative electrode The negative electrode may include a negative electrode current collector and a negative electrode active material-containing layer. The negative electrode current collector and the negative electrode active material-containing layer may be the current collector and the active material-containing layer that can be included in the electrode according to the second embodiment, respectively. The negative electrode active material-containing layer includes the active material according to the first embodiment as a negative electrode active material.
[0086] Among the details of the negative electrode, those parts that overlap with the details explained in the second embodiment will be omitted.
[0087] The density of the negative electrode active material-containing layer (excluding the current collector) is 1.8 g / cm 3 More than 3.5g / cm 3 The density of the negative electrode active material-containing layer is preferably 2.5 g / cm or less. A negative electrode having a density in this range of the negative electrode active material-containing layer is excellent in energy density and electrolyte retention. 3 More than 2.9g / cm 3 It is more preferable that:
[0088] The negative electrode can be produced, for example, by the same method as the electrode according to the second embodiment.
[0089] 2) Positive electrode The positive electrode can include a positive electrode current collector and a positive electrode active material-containing layer. The positive electrode active material-containing layer can be formed on one or both sides of the positive electrode current collector. The positive electrode active material-containing layer can include a positive electrode active material, and optionally a conductive agent and a binder.
[0090] As the positive electrode active material, for example, an oxide or a sulfide can be used. The positive electrode may contain one type of compound alone as the positive electrode active material, or may contain a combination of two or more types of compounds. Examples of the oxide and the sulfide include compounds into which Li or Li ions can be inserted and desorbed.
[0091] Examples of such compounds include manganese dioxide (MnO2), iron oxide, copper oxide, nickel oxide, lithium manganese composite oxide (e.g., Li x Mn2O4 or Li x MnO2; 0 < x ≦ 1), lithium nickel composite oxide (e.g., Li x NiO2; 0 < x ≦ 1), lithium cobalt composite oxide (e.g., Li x CoO2; 0 < x ≦ 1), lithium nickel cobalt composite oxide (e.g., Li x Ni 1-y Co y O2; 0 < x ≦ 1, 0 < y < 1), lithium manganese cobalt composite oxide (e.g., Li x Mn y Co 1-y O2; 0 < x ≦ 1, 0 < y < 1), lithium manganese nickel composite oxide having a spinel structure (e.g., Li x Mn 2-y Ni y O4; 0 < x ≦ 1, 0 < y < 2), lithium phosphate having an olivine structure (e.g., Li x FePO4; 0 < x ≦ 1, Li x Fe 1-y Mn y PO4; 0 < x ≦ 1, 0 < y ≦ 1, Lix CoPO4; 0 < x ≤ 1), iron sulfate (Fe2(SO4)3), vanadium oxide (e.g., V2O5), and lithium nickel cobalt manganese composite oxide (Li x Ni 1-y-z Co y Mn z O2; 0 < x ≤ 1, 0 < y < 1, 0 < z < 1, y + z < 1) are included.
[0092] Among the above, examples of more preferable compounds as the positive electrode active material include lithium manganese composite oxide having a spinel structure (e.g., Li x Mn2O4; 0 < x ≤ 1), lithium nickel composite oxide (e.g., Li x NiO2; 0 < x ≤ 1), lithium cobalt composite oxide (e.g., Li x CoO2; 0 < x ≤ 1), lithium nickel cobalt composite oxide (e.g., Li x Ni 1-y Co y O2; 0 < x ≤ 1, 0 < y < 1), lithium manganese nickel composite oxide having a spinel structure (e.g., Li x Mn 2-y Ni y O4; 0 < x ≤ 1, 0 < y < 2), lithium manganese cobalt composite oxide (e.g., Li x Mn y Co 1-y O2; 0 < x ≤ 1, 0 < y < 1), lithium iron phosphate (e.g., Li x FePO4; 0 < x ≤ 1), and lithium nickel cobalt manganese composite oxide (Li x Ni 1-y-z Co y Mn z O2; 0 < x ≤ 1, 0 < y < 1, 0 < z < 1, y + z < 1) are included. When these compounds are used as the positive electrode active material, the positive electrode potential can be increased.
[0093] When a room temperature molten salt is used as the electrolyte of the battery, lithium iron phosphate, Li xIt is preferable to use a positive electrode active material containing VPO4F (0≦x≦1), lithium manganese composite oxide, lithium nickel composite oxide, lithium nickel cobalt composite oxide, or a mixture thereof. These compounds have low reactivity with room temperature molten salts, so that the cycle life can be improved. Details of the room temperature molten salt will be described later.
[0094] The primary particle size of the positive electrode active material is preferably 100 nm or more and 1 μm or less. A positive electrode active material with a primary particle size of 100 nm or more is easy to handle in industrial production. A positive electrode active material with a primary particle size of 1 μm or less can smoothly diffuse lithium ions in the solid.
[0095] The specific surface area of the positive electrode active material is 0.1 m 2 / g or more 10m 2 / g or less. 2 A positive electrode active material having a specific surface area of 10m / g or more can secure sufficient sites for absorbing and releasing Li ions. 2 A positive electrode active material having a specific surface area of 100 / g or less is easy to handle in industrial production and can ensure good charge-discharge cycle performance.
[0096] The binder is blended to fill the gaps between the dispersed positive electrode active material and to bind the positive electrode active material and the positive electrode current collector. Examples of the binder include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine-based rubber, polyacrylic acid compounds, imide compounds, carboxymethyl cellulose (CMC), and salts of CMC. One of these may be used as the binder, or two or more may be used in combination as the binder.
[0097] The conductive agent is blended to improve current collection performance and reduce contact resistance between the positive electrode active material and the positive electrode current collector. Examples of the conductive agent include vapor grown carbon fiber (VGCF), carbon black such as acetylene black, and carbonaceous materials such as graphite. One of these may be used as the conductive agent, or two or more may be combined and used as the conductive agent. The conductive agent may also be omitted.
[0098] In the positive electrode active material-containing layer, the positive electrode active material and the binder are preferably mixed in an amount of 80% by mass to 98% by mass and 2% by mass to 20% by mass, respectively.
[0099] By making the amount of binder 2% by mass or more, sufficient electrode strength can be obtained. In addition, the binder can function as an insulator. Therefore, by making the amount of binder 20% by mass or less, the amount of insulator contained in the electrode is reduced, and the internal resistance can be reduced.
[0100] When a conductive agent is added, the positive electrode active material, the binder, and the conductive agent are preferably mixed in proportions of 77% by mass or more and 95% by mass or less, 2% by mass or more and 20% by mass or less, and 3% by mass or more and 15% by mass or less, respectively.
[0101] By making the amount of the conductive agent 3% by mass or more, the above-mentioned effects can be achieved. Also, by making the amount of the conductive agent 15% by mass or less, the ratio of the conductive agent in contact with the electrolyte can be reduced. If this ratio is low, decomposition of the electrolyte during high-temperature storage can be reduced.
[0102] The positive electrode current collector is preferably an aluminum foil or an aluminum alloy foil containing one or more elements selected from Mg, Ti, Zn, Ni, Cr, Mn, Fe, Cu, and Si.
[0103] The thickness of the aluminum foil or aluminum alloy foil is preferably 5 μm or more and 20 μm or less, more preferably 15 μm or less. The purity of the aluminum foil is preferably 99 mass% or more. The content of transition metals such as iron, copper, nickel, and chromium contained in the aluminum foil or aluminum alloy foil is preferably 1 mass% or less.
[0104] The positive electrode current collector may also include a portion on the surface of which the positive electrode active material-containing layer is not formed, and this portion can function as a positive electrode current collecting tab.
[0105] The positive electrode can be produced, for example, by using a positive electrode active material in the same manner as in the electrode according to the second embodiment.
[0106] 3) Electrolyte The electrolyte may be, for example, a liquid nonaqueous electrolyte or a gel nonaqueous electrolyte. The liquid nonaqueous electrolyte is prepared by dissolving an electrolyte salt as a solute in an organic solvent. The concentration of the electrolyte salt is preferably 0.5 mol / L or more and 2.5 mol / L or less.
[0107] Examples of the electrolyte salt include lithium salts such as lithium perchlorate (LiClO4), lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), lithium trifluoromethanesulfonate (LiCF3SO3), and lithium bistrifluoromethylsulfonylimide (LiN(CF3SO2)2), and mixtures thereof. The electrolyte salt is preferably one that is difficult to oxidize even at high potentials, and LiPF6 is most preferred.
[0108] Examples of organic solvents include cyclic carbonates such as propylene carbonate (PC), ethylene carbonate (EC), and vinylene carbonate (VC); chain carbonates such as diethyl carbonate (DEC), dimethyl carbonate (DMC), and methyl ethyl carbonate (MEC); cyclic ethers such as tetrahydrofuran (THF), 2-methyl tetrahydrofuran (2MeTHF), and dioxolane (DOX); chain ethers such as dimethoxyethane (DME) and diethoxyethane (DEE); γ-butyrolactone (GBL), acetonitrile (AN), and sulfolane (SL). These organic solvents can be used alone or as a mixed solvent.
[0109] The gelled non-aqueous electrolyte is prepared by combining a liquid non-aqueous electrolyte with a polymeric material, such as polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyethylene oxide (PEO), or a mixture thereof.
[0110] Alternatively, as the nonaqueous electrolyte, in addition to liquid nonaqueous electrolytes and gel nonaqueous electrolytes, room temperature molten salts containing lithium ions (ionic melts), polymer solid electrolytes, inorganic solid electrolytes, and the like may be used.
[0111] Room temperature molten salts (ionic melts) refer to organic salts consisting of a combination of organic cations and anions that can exist as a liquid at room temperature (15°C or higher and 25°C or lower). Room temperature molten salts include room temperature molten salts that exist as a liquid by themselves, room temperature molten salts that become liquid when mixed with an electrolyte salt, room temperature molten salts that become liquid when dissolved in an organic solvent, and mixtures of these. In general, the melting point of room temperature molten salts used in secondary batteries is 25°C or lower. In addition, organic cations generally have a quaternary ammonium skeleton.
[0112] The polymer solid electrolyte is prepared by dissolving an electrolyte salt in a polymer material and solidifying it.
[0113] The inorganic solid electrolyte is a solid substance that has Li-ion conductivity. Here, Li-ion conductivity is defined as a Li-ion conductivity of 1×10 -6 It means that the inorganic solid electrolyte has a lithium ion conductivity of 1.0 S / cm or more. Examples of the inorganic solid electrolyte include oxide-based solid electrolytes and sulfide-based solid electrolytes. Specific examples of the inorganic solid electrolyte are as follows.
[0114] The oxide-based solid electrolyte has a NASICON (Sodium (Na) Super Ionic Conductor) type structure and is represented by the general formula Li 1+x It is preferable to use a lithium phosphate solid electrolyte represented by Mα2(PO4)3. In the above general formula, Mα is, for example, one or more selected from the group consisting of titanium (Ti), germanium (Ge), strontium (Sr), zirconium (Zr), tin (Sn), aluminum (Al), and calcium (Ca). The subscript x is within the range of 0≦x≦2.
[0115] A specific example of a lithium phosphate solid electrolyte having a NASICON structure is Li 1+x Al x Ti 2-x LATP compound represented by (PO4)3, where 0.1≦x≦0.5; Li 1+x Al y Mβ 2-yA compound represented by (PO4)3, where Mβ is one or more selected from the group consisting of Ti, Ge, Sr, Zr, Sn, and Ca, 0 ≦ x ≦ 1, and 0 ≦ y ≦ 1; Li 1+x Al x Ge 2-x A compound represented by (PO4)3, where 0 ≦ x ≦ 2; and Li 1+x Al x Zr 2-x A compound represented by (PO4)3, where 0 ≦ x ≦ 2; Li 1+x+y Al x Mγ 2-x Si y P 3-y O 12 A compound represented by, where Mγ is one or more selected from the group consisting of Ti and Ge, 0 < x ≦ 2, and 0 ≦ y < 3; Li 1+2x Zr 1-x Ca x Examples of the compound represented by (PO4)3, where 0 ≦ x < 1, can be given.
[0116] In addition, as the oxide-based solid electrolyte, in addition to the above lithium phosphate solid electrolyte, Li x PO y N z An amorphous LIPON compound represented by, where 2.6 ≦ x ≦ 3.5, 1.9 ≦ y ≦ 3.8, and 0.1 ≦ z ≦ 1.3 (for example, Li 2.9 PO 3.3 N 0.46 ); A garnet-type structure La 5+x A x La 3-x Mδ2O 12 A compound represented by, where A is one or more selected from the group consisting of Ca, Sr, and Ba, Mδ is one or more selected from the group consisting of Nb and Ta, and 0 ≦ x ≦ 0.5; Li3Mδ 2-x L2O 12 A compound represented by, where Mδ is one or more selected from the group consisting of Nb and Ta, L may contain Zr, and 0 ≦ x ≦ 0.5; Li 7-3x Al x La3Zr3O 12 A compound represented by, where 0 ≦ x ≦ 0.5; Li 5+x La3Mδ 2-x Zr x O12 where Mδ is at least one selected from the group consisting of Nb and Ta, and 0≦x≦2. LLZ compounds (e.g., Li7La3Zr2O 12 ); and La 2 / 3-x Li x Examples of such compounds include those represented by TiO3, where x is 0.3≦x≦0.7.
[0117] One or more of the above compounds can be used as the solid electrolyte. Two or more of the above solid electrolytes can also be used.
[0118] The electrolyte may be an aqueous electrolyte that contains water.
[0119] The aqueous electrolyte includes an aqueous solvent and an electrolyte salt. The aqueous electrolyte is, for example, liquid. The liquid aqueous electrolyte is an aqueous solution prepared by dissolving an electrolyte salt as a solute in an aqueous solvent. The aqueous solvent is, for example, a solvent containing water in an amount of 50% by volume or more. The aqueous solvent may be pure water.
[0120] The aqueous electrolyte may be a gel aqueous electrolyte obtained by combining an aqueous electrolyte solution with a polymeric material, such as polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyethylene oxide (PEO), etc.
[0121] 4) Separator The separator is formed, for example, from a porous film containing polyethylene (PE), polypropylene (PP), cellulose, or polyvinylidene fluoride (PVdF), or a synthetic resin nonwoven fabric. From the viewpoint of safety, it is preferable to use a porous film formed from polyethylene or polypropylene. This is because these porous films melt at a certain temperature and are capable of cutting off electric current.
[0122] 5) Exterior materials As the exterior member, for example, a container made of a laminate film or a metal container can be used.
[0123] The thickness of the laminate film is, for example, 0.5 mm or less, preferably 0.2 mm or less.
[0124] The laminate film is a multi-layer film including a plurality of resin layers and a metal layer interposed between the resin layers. The resin layers include polymeric materials such as polypropylene (PP), polyethylene (PE), nylon, and polyethylene terephthalate (PET). The metal layer is preferably made of aluminum foil or aluminum alloy foil for weight reduction. The laminate film can be molded into the shape of the exterior member by sealing it by heat fusion.
[0125] The thickness of the wall of the metal container is, for example, 1 mm or less, more preferably 0.5 mm or less, and even more preferably 0.2 mm or less.
[0126] The metal container is made of, for example, aluminum or an aluminum alloy. The aluminum alloy preferably contains elements such as magnesium, zinc, and silicon. When the aluminum alloy contains transition metals such as iron, copper, nickel, and chromium, the content of the transition metals is preferably 100 ppm by mass or less.
[0127] The shape of the exterior member is not particularly limited. The shape of the exterior member may be, for example, flat (thin), rectangular, cylindrical, coin-shaped, or button-shaped. The exterior member can be appropriately selected depending on the battery dimensions and the application of the battery.
[0128] 6) Negative terminal The negative electrode terminal can be made of a material that is electrochemically stable at the Li absorption / release potential of the negative electrode active material and has electrical conductivity. Specifically, the material of the negative electrode terminal can be copper, nickel, stainless steel, aluminum, or an aluminum alloy containing at least one element selected from the group consisting of Mg, Ti, Zn, Mn, Fe, Cu, and Si. The material of the negative electrode terminal is preferably aluminum or an aluminum alloy. The negative electrode terminal is preferably made of the same material as the negative electrode current collector in order to reduce the contact resistance with the negative electrode current collector.
[0129] 7) Positive terminal The positive electrode terminal has a potential range of 3V to 4.5V with respect to the redox potential of lithium (vs. Li / Li + ) and can be formed from a material that is electrically stable and conductive. Examples of the material for the positive electrode terminal include aluminum and an aluminum alloy containing at least one element selected from the group consisting of Mg, Ti, Zn, Mn, Fe, Cu, and Si. The positive electrode terminal is preferably formed from the same material as the positive electrode current collector in order to reduce the contact resistance with the positive electrode current collector.
[0130] Next, the secondary battery according to the embodiment will be described more specifically with reference to the drawings.
[0131] Fig. 5 is a cross-sectional view showing an example of a secondary battery, and Fig. 6 is an enlarged cross-sectional view of part A of the secondary battery shown in Fig. 5.
[0132] The secondary battery 100 shown in Figures 5 and 6 includes a bag-shaped exterior member 2 shown in Figure 5, an electrode group 1 shown in Figures 5 and 6, and an electrolyte (not shown). The electrode group 1 and the electrolyte are stored in the bag-shaped exterior member 2. The electrolyte (not shown) is held in the electrode group 1.
[0133] The bag-shaped exterior member 2 is made of a laminate film including two resin layers and a metal layer interposed between them.
[0134] As shown in Fig. 5, the electrode group 1 is a flat wound-type electrode group. As shown in Fig. 6, the flat wound-type electrode group 1 includes a negative electrode 3, a separator 4, and a positive electrode 5. The separator 4 is interposed between the negative electrode 3 and the positive electrode 5.
[0135] The negative electrode 3 includes a negative electrode current collector 3a and a negative electrode active material-containing layer 3b. In the negative electrode 3, in a portion located at the outermost shell of the wound-type electrode group 1, the negative electrode active material-containing layer 3b is formed only on the inner surface side of the negative electrode current collector 3a as shown in Fig. 6. In the other portions of the negative electrode 3, the negative electrode active material-containing layer 3b is formed on both sides of the negative electrode current collector 3a.
[0136] The positive electrode 5 includes a positive electrode current collector 5a and a positive electrode active material-containing layer 5b formed on both sides of the positive electrode current collector 5a.
[0137] As shown in FIG. 5, the negative electrode terminal 6 and the positive electrode terminal 7 are located near the outer peripheral end of the wound electrode group 1. The negative electrode terminal 6 is connected to a portion located at the outermost shell of the negative electrode current collector 3a. The positive electrode terminal 7 is connected to a portion located at the outermost shell of the positive electrode current collector 5a. The negative electrode terminal 6 and the positive electrode terminal 7 extend to the outside from an opening of the bag-shaped exterior member 2. A thermoplastic resin layer is provided on the inner surface of the bag-shaped exterior member 2, and the opening is closed by heat sealing.
[0138] The secondary battery according to the embodiment is not limited to the secondary battery having the configuration shown in FIGS. 5 and 6, but may be a battery having the configuration shown in FIGS.
[0139] FIG. 7 is a partially cutaway perspective view that illustrates a schematic diagram of another example of a secondary battery. FIG. 8 is an enlarged cross-sectional view of part B of the secondary battery shown in FIG.
[0140] The secondary battery 100 shown in Figures 7 and 8 includes an electrode group 1 shown in Figures 7 and 8, an exterior member 2 shown in Figure 7, and an electrolyte (not shown). The electrode group 1 and the electrolyte are housed in the exterior member 2. The electrolyte is held in the electrode group 1.
[0141] The exterior member 2 is made of a laminate film including two resin layers and a metal layer interposed between them.
[0142] The electrode group 1 is a laminated type electrode group, as shown in Fig. 8. The laminated type electrode group 1 has a structure in which negative electrodes 3 and positive electrodes 5 are alternately laminated with separators 4 interposed therebetween.
[0143] The electrode group 1 includes a plurality of negative electrodes 3. Each of the plurality of negative electrodes 3 includes a negative electrode current collector 3a and a negative electrode active material-containing layer 3b supported on both sides of the negative electrode current collector 3a. The electrode group 1 also includes a plurality of positive electrodes 5. Each of the plurality of positive electrodes 5 includes a positive electrode current collector 5a and a positive electrode active material-containing layer 5b supported on both sides of the positive electrode current collector 5a.
[0144] The negative electrode current collector 3a of each negative electrode 3 includes a portion on one side where the negative electrode active material-containing layer 3b is not supported on any surface. This portion serves as a negative electrode current collector tab 3c. As shown in FIG. 8, the negative electrode current collector tab 3c does not overlap with the positive electrode 5. The negative electrode current collector tabs 3c are electrically connected to a belt-shaped negative electrode terminal 6. The tip of the belt-shaped negative electrode terminal 6 is pulled out to the outside of the exterior member 2.
[0145] Although not shown, the positive electrode current collector 5a of each positive electrode 5 includes a portion on one side where the positive electrode active material-containing layer 5b is not supported on any surface. This portion serves as a positive electrode current collector tab. The positive electrode current collector tab does not overlap with the negative electrode 3, similar to the negative electrode current collector tab 3c. The positive electrode current collector tab is located on the opposite side of the electrode group 1 to the negative electrode current collector tab 3c. The positive electrode current collector tab is electrically connected to a strip-shaped positive electrode terminal 7. The tip of the strip-shaped positive electrode terminal 7 is located on the opposite side of the negative electrode terminal 6 and is drawn out to the outside of the exterior member 2.
[0146] The secondary battery according to the third embodiment contains the active material according to the first embodiment as a negative electrode active material, and therefore the secondary battery can exhibit excellent charge / discharge efficiency and cycle life performance.
[0147] (Fourth embodiment) According to a fourth embodiment, there is provided a battery pack including a plurality of secondary batteries according to the third embodiment.
[0148] In such a battery pack, the individual cells may be electrically connected in series or parallel, or may be arranged in a combination of series and parallel connections.
[0149] Next, an example of a battery pack according to an embodiment will be described with reference to the drawings.
[0150] Fig. 9 is a perspective view showing an example of a battery pack. The battery pack 200 shown in Fig. 9 includes five cells 100a to 100e, four bus bars 21, a positive electrode lead 22, and a negative electrode lead 23. Each of the five cells 100a to 100e is a secondary battery according to the third embodiment.
[0151] The bus bar 21 connects, for example, the negative electrode terminal 6 of one cell 100a and the positive electrode terminal 7 of the adjacent cell 100b. In this way, the five cells 100 are connected in series by the four bus bars 21. That is, the battery pack 200 in FIG. 9 is a five-series battery pack. Although no example is shown, in a battery pack including a plurality of cells electrically connected in parallel, for example, the plurality of negative electrode terminals are connected to each other by a bus bar and the plurality of positive electrode terminals are connected to each other by a bus bar, thereby electrically connecting the plurality of cells.
[0152] The positive electrode terminal 7 of at least one of the five cells 100a to 100e is electrically connected to a positive electrode lead 22 for external connection. Also, the negative electrode terminal 6 of at least one of the five cells 100a to 100e is electrically connected to a negative electrode lead 23 for external connection.
[0153] The battery pack according to the fourth embodiment includes the secondary battery according to the third embodiment, and therefore the battery pack can exhibit excellent charge / discharge efficiency and cycle life performance.
[0154] Fifth embodiment According to a fifth embodiment, there is provided a battery pack. The battery pack includes the battery assembly according to the fourth embodiment. The battery pack may include a single secondary battery according to the third embodiment, instead of the battery assembly according to the fourth embodiment.
[0155] Such a battery pack may further include a protection circuit. The protection circuit has a function of controlling charging and discharging of the secondary battery. Alternatively, a circuit included in a device (e.g., electronic device, automobile, etc.) that uses the battery pack as a power source may be used as the protection circuit for the battery pack.
[0156] The battery pack may further include an external terminal for current flow. The external terminal for current flow is for outputting current from the secondary battery to the outside and / or inputting current from the outside to the secondary battery. In other words, when the battery pack is used as a power source, current is supplied to the outside through the external terminal for current flow. When the battery pack is charged, a charging current (including regenerative energy from the power of an automobile or the like) is supplied to the battery pack through the external terminal for current flow.
[0157] Next, an example of a battery pack according to an embodiment will be described with reference to the drawings.
[0158] Fig. 10 is an exploded perspective view showing an example of a battery pack, and Fig. 11 is a block diagram showing an example of an electric circuit of the battery pack shown in Fig. 10.
[0159] The battery pack 300 shown in Figs. 10 and 11 includes a container 31, a lid 32, a protective sheet 33, a battery pack 200, a printed wiring board 34, wiring 35, and an insulating plate (not shown).
[0160] 10 is a bottomed, square container having a rectangular bottom. The container 31 is configured to be able to accommodate a protective sheet 33, a battery pack 200, a printed wiring board 34, and wiring 35. The lid 32 has a rectangular shape. The lid 32 covers the container 31 to accommodate the battery pack 200 and the like. Although not shown, the container 31 and the lid 32 are provided with openings or connection terminals for connection to an external device or the like.
[0161] The battery pack 200 includes a plurality of cells 100, a positive electrode lead 22, a negative electrode lead 23, and an adhesive tape 24.
[0162] At least one of the plurality of unit cells 100 is a secondary battery according to the third embodiment. Each of the plurality of unit cells 100 is electrically connected in series as shown in FIG. 11. The plurality of unit cells 100 may be electrically connected in parallel, or may be connected in a combination of series and parallel connections. When the plurality of unit cells 100 are connected in parallel, the battery capacity is increased compared to when they are connected in series.
[0163] The adhesive tape 24 fastens the plurality of unit cells 100. The plurality of unit cells 100 may be fixed using heat shrink tape instead of the adhesive tape 24. In this case, the protective sheets 33 are disposed on both side surfaces of the battery pack 200, the heat shrink tape is wrapped around the battery pack 200, and the heat shrink tape is then thermally shrunk to bind the plurality of unit cells 100 together.
[0164] One end of the positive electrode lead 22 is connected to the battery pack 200. One end of the positive electrode lead 22 is electrically connected to the positive electrode of one or more cells 100. One end of the negative electrode lead 23 is connected to the battery pack 200. One end of the negative electrode lead 23 is electrically connected to the negative electrode of one or more cells 100.
[0165] The printed wiring board 34 is disposed along one of the short side surfaces of the inner surface of the container 31. The printed wiring board 34 includes a positive connector 342, a negative connector 343, a thermistor 345, a protection circuit 346, wiring 342a and 343a, an external terminal 350 for supplying electricity, a positive wiring (positive wiring) 348a, and a negative wiring (negative wiring) 348b. One main surface of the printed wiring board 34 faces one side of the battery pack 200. An insulating plate (not shown) is interposed between the printed wiring board 34 and the battery pack 200.
[0166] The other end 22a of the positive electrode lead 22 is electrically connected to the positive electrode connector 342. The other end 23a of the negative electrode lead 23 is electrically connected to the negative electrode connector 343.
[0167] The thermistor 345 is fixed to one main surface of the printed wiring board 34. The thermistor 345 detects the temperature of each of the cells 100, and transmits a detection signal to the protection circuit 346.
[0168] The external terminal 350 for current supply is fixed to the other main surface of the printed wiring board 34. The external terminal 350 for current supply is electrically connected to a device present outside the battery pack 300. The external terminal 350 for current supply includes a positive terminal 352 and a negative terminal 353.
[0169] The protection circuit 346 is fixed to the other main surface of the printed wiring board 34. The protection circuit 346 is connected to the positive terminal 352 via a positive wiring 348a. The protection circuit 346 is connected to the negative terminal 353 via a negative wiring 348b. The protection circuit 346 is also electrically connected to the positive electrode connector 342 via a wiring 342a. The protection circuit 346 is electrically connected to the negative electrode connector 343 via a wiring 343a. Furthermore, the protection circuit 346 is electrically connected to each of the plurality of single cells 100 via the wiring 35.
[0170] The protective sheet 33 is disposed on both inner surfaces in the long side direction of the container 31 and on the inner surface in the short side direction that faces the printed wiring board 34 via the battery pack 200. The protective sheet 33 is made of, for example, resin or rubber.
[0171] The protection circuit 346 controls charging and discharging of the multiple cells 100. In addition, the protection circuit 346 cuts off electrical connection between the protection circuit 346 and external terminals 350 (positive terminal 352, negative terminal 353) for supplying electricity to an external device, based on a detection signal transmitted from the thermistor 345, or a detection signal transmitted from each of the cells 100 or the battery pack 200.
[0172] An example of the detection signal transmitted from the thermistor 345 is a signal that detects that the temperature of the cell 100 is equal to or higher than a predetermined temperature. An example of the detection signal transmitted from each cell 100 or the battery pack 200 is a signal that detects overcharging, overdischarging, and overcurrent of the cell 100. When detecting overcharging or the like for each cell 100, the battery voltage may be detected, or the positive electrode potential or the negative electrode potential may be detected. In the latter case, a lithium electrode used as a reference electrode is inserted into each cell 100.
[0173] The protection circuit 346 may be a circuit included in a device (such as an electronic device or an automobile) that uses the battery pack 300 as a power source.
[0174] As described above, the battery pack 300 includes the external terminal 350 for current supply. Therefore, the battery pack 300 can output a current from the assembled battery 200 to an external device and input a current from the external device to the assembled battery 200 via the external terminal 350 for current supply. In other words, when the battery pack 300 is used as a power source, the current from the assembled battery 200 is supplied to the external device through the external terminal 350 for current supply. When the battery pack 300 is charged, a charging current from the external device is supplied to the battery pack 300 through the external terminal 350 for current supply. When the battery pack 300 is used as an in-vehicle battery, regenerative energy of the vehicle's power can be used as the charging current from the external device.
[0175] The battery pack 300 may include a plurality of assembled batteries 200. In this case, the assembled batteries 200 may be connected in series, in parallel, or in a combination of series and parallel connections. The printed wiring board 34 and the wiring 35 may be omitted. In this case, the positive electrode lead 22 and the negative electrode lead 23 may be used as a positive terminal 352 and a negative terminal 353, respectively, of the external terminal 350 for current supply.
[0176] Such a battery pack is used in applications that require excellent cycle performance, for example, when a large current is drawn. Specifically, the battery pack is used, for example, as a power source for electronic devices, a stationary battery, or an on-board battery for various vehicles. An example of the electronic device is a digital camera. The battery pack is particularly suitable for use as an on-board battery.
[0177] The battery pack according to the fifth embodiment includes the secondary battery according to the third embodiment or the battery pack according to the fourth embodiment, and therefore the battery pack can exhibit excellent charge / discharge efficiency and cycle life performance.
[0178] Sixth embodiment According to a sixth embodiment, a vehicle is provided. The vehicle is equipped with the battery pack according to the fifth embodiment.
[0179] In such a vehicle, the battery pack, for example, recovers regenerative energy of the vehicle's motive power. The vehicle may include a mechanism (regenerator) that converts the kinetic energy of the vehicle into regenerative energy.
[0180] Examples of vehicles include, for example, two to four wheel hybrid electric vehicles, two to four wheel electric vehicles, power assisted bicycles, and rail vehicles.
[0181] The mounting position of the battery pack in the vehicle is not particularly limited. For example, when the battery pack is mounted in an automobile, the battery pack can be mounted in the engine compartment, the rear of the vehicle body, or under the seat of the vehicle.
[0182] The vehicle may be equipped with a plurality of battery packs. In this case, the batteries included in each battery pack may be electrically connected in series, electrically connected in parallel, or electrically connected in a combination of series and parallel connections. For example, when each battery pack includes a battery pack, the battery packs may be electrically connected in series, electrically connected in parallel, or electrically connected in a combination of series and parallel connections. Alternatively, when each battery pack includes a single battery, the batteries may be electrically connected in series, electrically connected in parallel, or electrically connected in a combination of series and parallel connections.
[0183] Next, an example of a vehicle according to an embodiment will be described with reference to the drawings.
[0184] FIG. 12 is a partially see-through view that diagrammatically illustrates an example of a vehicle.
[0185] A vehicle 400 shown in Fig. 12 includes a vehicle body 40 and a battery pack 300 according to the fifth embodiment. In the example shown in Fig. 12, the vehicle 400 is a four-wheeled automobile.
[0186] The vehicle 400 may be equipped with a plurality of battery packs 300. In this case, the batteries (e.g., single cells or assembled batteries) included in the battery pack 300 may be connected in series, in parallel, or in a combination of series and parallel connections.
[0187] 12 illustrates an example in which the battery pack 300 is mounted in an engine room located in the front of the vehicle body 40. As described above, the battery pack 300 may be mounted, for example, in the rear of the vehicle body 40 or under a seat. This battery pack 300 can be used as a power source for the vehicle 400. In addition, this battery pack 300 can recover regenerative energy for the motive power of the vehicle 400.
[0188] Next, an embodiment of a vehicle according to the present embodiment will be described with reference to FIG.
[0189] Fig. 13 is a diagram illustrating an example of a control system for an electrical system in a vehicle. The vehicle 400 illustrated in Fig. 13 is an electric vehicle.
[0190] The vehicle 400 shown in FIG. 13 comprises a vehicle body 40, a vehicle power supply 41, a vehicle ECU (ECU: Electric Control Unit) 42 which is a higher-level control device of the vehicle power supply 41, an external terminal (terminal for connecting to an external power supply) 43, an inverter 44, and a drive motor 45.
[0191] The vehicle 400 has a vehicle power supply 41 mounted, for example, in an engine compartment, the rear of the vehicle body, or under a seat. Note that in the vehicle 400 shown in Fig. 13, the mounting location of the vehicle power supply 41 is shown diagrammatically.
[0192] The vehicle power supply 41 includes a plurality of (eg, three) battery packs 300a, 300b, and 300c, a battery management unit (BMU) 411, and a communication bus 412.
[0193] The battery pack 300a includes an assembled battery 200a and an assembled battery monitoring device 301a (for example, VTM: Voltage Temperature Monitoring). The battery pack 300b includes an assembled battery 200b and an assembled battery monitoring device 301b. The battery pack 300c includes an assembled battery 200c and an assembled battery monitoring device 301c. The battery packs 300a to 300c are battery packs similar to the above-mentioned battery pack 300, and the assembled batteries 200a to 200c are assembled batteries similar to the above-mentioned battery pack 200. The assembled batteries 200a to 200c are electrically connected in series. The battery packs 300a, 300b, and 300c can be removed independently and replaced with another battery pack 300.
[0194] Each of the assembled batteries 200a to 200c includes a plurality of unit cells connected in series. At least one of the plurality of unit cells is the secondary battery according to the third embodiment. Each of the assembled batteries 200a to 200c is charged and discharged via a positive terminal 413 and a negative terminal 414.
[0195] The battery management device 411 communicates with the assembled battery monitoring devices 301a to 301c, and collects information on the voltage, temperature, and the like of each of the cells 100 included in the assembled batteries 200a to 200c included in the vehicle power supply 41. In this way, the battery management device 411 collects information on the maintenance of the vehicle power supply 41.
[0196] The battery management unit 411 and the assembled battery monitoring units 301a to 301c are connected via a communication bus 412. In the communication bus 412, one set of communication lines is shared by a plurality of nodes (the battery management unit 411 and one or more assembled battery monitoring units 301a to 301c). The communication bus 412 is a communication bus configured based on, for example, the CAN (Control Area Network) standard.
[0197] The battery pack monitoring devices 301a to 301c measure the voltage and temperature of each of the cells constituting the battery packs 200a to 200c based on commands communicated from the battery management device 411. However, the temperature can be measured at only a few points per battery pack, and it is not necessary to measure the temperatures of all the cells.
[0198] The vehicle power supply 41 may also have an electromagnetic contactor (for example, a switch device 415 shown in FIG. 13) that switches between the presence and absence of an electrical connection between the positive terminal 413 and the negative terminal 414. The switch device 415 includes a pre-charge switch (not shown) that is turned on when the assembled batteries 200a to 200c are charged, and a main switch (not shown) that is turned on when the output from the assembled batteries 200a to 200c is supplied to a load. Each of the pre-charge switch and the main switch includes a relay circuit (not shown) that is switched on or off by a signal supplied to a coil disposed near the switch element. The electromagnetic contactor such as the switch device 415 is controlled based on a control signal from the battery management device 411 or the vehicle ECU 42 that controls the operation of the entire vehicle 400.
[0199] The inverter 44 converts the input DC voltage into a three-phase alternating current (AC) high voltage for driving the motor. The three-phase output terminals of the inverter 44 are connected to the three-phase input terminals of the drive motor 45. The inverter 44 is controlled based on a control signal from the battery management device 411 or the vehicle ECU 42 for controlling the operation of the entire vehicle. By controlling the inverter 44, the output voltage from the inverter 44 is adjusted.
[0200] The drive motor 45 rotates by electric power supplied from the inverter 44. A driving force generated by the rotation of the drive motor 45 is transmitted to the axles and drive wheels W via, for example, a differential gear unit.
[0201] Although not shown, the vehicle 400 is also equipped with a regenerative braking mechanism (regenerator). The regenerative braking mechanism rotates the drive motor 45 when the vehicle 400 is braked, and converts kinetic energy into regenerative energy as electrical energy. The regenerative energy recovered by the regenerative braking mechanism is input to the inverter 44 and converted into a direct current. The converted direct current is input to the vehicle power source 41.
[0202] One terminal of a connection line L1 is connected to the negative terminal 414 of the vehicle power supply 41. The other terminal of the connection line L1 is connected to a negative input terminal 417 of the inverter 44. A current detection unit (current detection circuit) 416 in the battery management device 411 is provided between the negative terminal 414 and the negative input terminal 417 on the connection line L1.
[0203] One terminal of a connection line L2 is connected to the positive electrode terminal 413 of the vehicle power supply 41. The other terminal of the connection line L2 is connected to a positive electrode input terminal 418 of the inverter 44. A switch device 415 is provided in the connection line L2 between the positive electrode terminal 413 and the positive electrode input terminal 418.
[0204] The external terminal 43 is connected to the battery management unit 411. The external terminal 43 can be connected to, for example, an external power source.
[0205] In response to operational inputs from the driver or the like, the vehicle ECU 42 coordinates with other management devices and control devices including the battery management device 411 to control the vehicle power supply 41, the switch device 415, the inverter 44, etc. Through the coordinated control of the vehicle ECU 42, etc., the output of power from the vehicle power supply 41 and the charging of the vehicle power supply 41 are controlled, and the entire vehicle 400 is managed. Data relating to the maintenance of the vehicle power supply 41, such as the remaining capacity of the vehicle power supply 41, is transferred between the battery management device 411 and the vehicle ECU 42 via a communication line.
[0206] The vehicle according to the sixth embodiment is equipped with the battery pack according to the fifth embodiment. Therefore, by installing such a battery pack, it is possible to provide a vehicle that can exhibit high performance and has high reliability. EXAMPLES
[0207] The above embodiment will now be described in more detail with reference to examples.
[0208] <Synthesis method> Example 1 Niobium titanium oxide was synthesized by the solid phase synthesis method described below.
[0209] First, Nb2O5 particles and TiO2 particles were mixed in a 1:1 molar ratio in a wet bead mill for 2 hours to obtain the Nb2TiO7 phase. The resulting mixed slurry was granulated and dried using a spray dryer. The resulting granulated particles were pre-fired (first firing) at a temperature of 800°C for 12 hours. After pre-firing, the resulting powder was placed in a platinum crucible and fired (second firing) at 1050°C for 3 hours. The resulting fired granules were mixed using a thin film swirling high-speed mixer "Filmix 80" manufactured by Primix Corporation to measure the average particle diameter D 50 The particles were pulverized so that the particle size was in the range of 1.0 μm to 3.5 μm, and the active material of Example 1 was obtained.
[0210] Example 2 Niobium titanium oxide was synthesized by the solid phase synthesis method described below.
[0211] First, Nb2O5 particles and TiO2 particles were mixed in a molar ratio of 1:1 using a dry ball mill to obtain the Nb2TiO7 phase. The resulting mixed powder was placed in an alumina crucible and pre-fired (first firing) at a temperature of 800°C for 12 hours. After pre-firing, the resulting powder was placed in a platinum crucible and pre-fired (second firing) at 1200°C for 5 hours. After pre-firing, the powder was lightly crushed in an agate mortar and passed through a 25 μm mesh sieve to remove coarse particles, thereby obtaining the active material of Example 2.
[0212] Example 3 An active material of Example 3 was obtained in the same manner as in Example 2, except that the particles after main firing obtained in Example 2 were pulverized at the same intensity as in Example 1 using a thin film rotary high-speed mixer.
[0213] Example 4 In order to obtain niobium titanium oxide, synthesis was carried out using the sol-gel method described in Non-Patent Document 3 (Chem. Mater. 2011, 23, 8, 2027-2029). Specifically, synthesis was carried out as follows. The pulverization was limited to a light degree to break up the agglomerations of the fired powder.
[0214] Nb2O5, hydrofluoric acid solution (HF:H2O = 40:70), Ti(OC3H7)4, ammonia, and citric acid monohydrate were used as starting materials. First, Nb2O5 was dissolved in hydrofluoric acid to obtain a clear solution. To remove F ions from the solution, ammonia was added to obtain a white Nb(OH)5 precipitate. After washing and drying the precipitate, Nb(OH)5 was dissolved in citric acid to obtain a Nb(V) citric acid solution. To this solution, a water-ethanol solution containing Ti(OC3H7)4 was added while adjusting the pH of the solution by adding ammonia. This final mixture containing Nb(V) and Ti(IV) ions was stirred at 90 °C to form a citric acid gel, and the gel was heated to 140 °C to obtain the precursor. The precursor was subjected to main calcination at 1500 °C to obtain a niobium titanium oxide powder with a high crystallite size of more than 85 nm. After firing, the powder was lightly crushed in an agate mortar and passed through a 25 μm mesh sieve to remove coarse particles, thereby obtaining the active material of Example 4.
[0215] Example 5 An active material of Example 5 was obtained in the same manner as in Example 4, except that after main-sintering, the particles were pulverized using a thin-film rotary high-speed mixer.
[0216] (Examples 6 to 11) The active materials of Examples 6 to 11 were obtained in the same manner as in Example 1, except that the raw materials were mixed in a predetermined ratio so as to obtain the composition shown in Table 1 below, with respect to the added elements other than the raw material Nb2O5 particles and TiO2 particles.
[0217] Example 12 Nb 10 Ti2O 29 The active material of Example 12 was obtained in the same manner as in Example 1, except that the molar ratio of Nb2O5 particles to TiO2 particles was 2.5:1 so as to obtain a phase.
[0218] Comparative Example 1 Niobium titanium oxide was synthesized by the solid-phase synthesis method described below. First, in order to obtain Nb2TiO7, Nb2O5 particles and TiO2 particles were mixed in a molar ratio of 1:1 using a dry ball mill. The obtained powder was placed in an alumina crucible and pre-fired (first firing) at a temperature of 800°C for 12 hours. After pre-fire, the obtained powder was placed in a platinum crucible and pre-fired (second firing) at 1200°C for 5 hours. After pre-fire, the fired powder was pulverized and mixed using a dry bead mill until the average particle size D50 was in the range of 1.0 μm to 3.5 μm, and the active material of Comparative Example 1 was obtained.
[0219] Comparative Example 2 The sintered granules obtained in Example 1 were milled using a dry ball mill to have an average particle diameter D 50 An active material of Comparative Example 2 was obtained in the same manner as in Example 1, except that the powder was pulverized to a particle size in the range of 1.0 μm to 3.5 μm.
[0220] Comparative Example 3 The active material of Comparative Example 3 was obtained by synthesis using the sol-gel method described in Non-Patent Document 3 (Chem. Mater. 2011, 23, 8, 2027-2029). Specifically, the synthesis was performed as follows. The pulverization was limited to a light degree to break up the agglomerations of the sintered powder.
[0221] Nb2O5, hydrofluoric acid solution (HF:H2O = 40:70), Ti(OC3H7)4, ammonia, and citric acid monohydrate were used as starting materials. First, Nb2O5 was dissolved in hydrofluoric acid to obtain a clear solution. To remove F ions from the solution, ammonia was added to obtain a white Nb(OH)5 precipitate. After washing and drying the precipitate, Nb(OH)5 was dissolved in citric acid to obtain a Nb(V) citric acid solution. To this solution, a water-ethanol solution containing Ti(OC3H7)4 was added while adjusting the pH of the solution by adding ammonia. This final mixture containing Nb(V) and Ti(IV) ions was stirred at 90 °C to form a citric acid gel, and the gel was heated to 140 °C to obtain the precursor. The precursor was subjected to main calcination at 900 °C to obtain a niobium titanium oxide powder. After firing, the powder was lightly crushed in an agate mortar and passed through a 25 μm mesh sieve to remove coarse particles, thereby obtaining an active material of Comparative Example 3.
[0222] Comparative Example 4 An active material of Comparative Example 4 was obtained in the same manner as in Comparative Example 3, except that the sintered powder obtained in Comparative Example 3 was pulverized at the same intensity as in Comparative Example 2 using a dry bead mill.
[0223] <Physical property evaluation> The crystal structure, crystallite size, and average particle size (D 50 ) was evaluated. Regarding the crystal structure, the synchrotron radiation X-ray diffraction measurement described above was performed to confirm the space group to which the niobium titanium oxide phase belongs, and the octahedral sites with only corner sharing were confirmed, and the bond angle distortion (σ 2 / deg 2 ) was extracted from the Rietveld analysis results. In addition, normal (laboratory level) powder X-ray diffraction measurements were performed, and the crystallite size was determined by the above-mentioned method using the Rietveld analysis results of the obtained X-ray spectrum. The average particle size was measured based on the laser diffraction scattering method as described above. These results are summarized in Table 2 below.
[0224] <Electrochemical measurements> Using the active materials obtained in each example, a cell for electrochemical measurement was produced according to the following procedure.
[0225] 100% by mass of the active material powder obtained in each example, 10% by mass of acetylene black as a conductive agent, 5% by mass of carbon nanofiber, and 10% by mass of polyvinylidene fluoride (PVdF) as a binder were added to N-methylpyrrolidone (NMP) and mixed to obtain a slurry. This slurry was applied to one side of a current collector made of aluminum foil with a thickness of 12 μm, dried, and pressed to obtain an electrode with a density of 2.4 g / cm. 3 An electrode (excluding the current collector) was prepared.
[0226] On the other hand, a liquid electrolyte was prepared by dissolving LiPF6 supporting salt at a concentration of 1 mol / L in a mixed solvent of ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 1:2.
[0227] The obtained electrode was used as a working electrode, and Li metal was used as a counter electrode and a reference electrode. A three-electrode beaker cell was fabricated using the prepared liquid electrolyte, and the electrochemical performance was evaluated as described below.
[0228] In this evaluation, in the three-electrode beaker cell for this measurement, lithium metal is used as the counter electrode, so the electrode potential of the prepared electrode is more noble than the counter electrode, and the electrode operates as a positive electrode. Therefore, the definition of charge and discharge is reversed when the electrode using the active material of each example is used as a negative electrode. Here, to avoid confusion, in this evaluation, the direction in which lithium ions are inserted into the electrode is unified as charge, and the direction in which they are removed is unified as discharge. Note that the active material according to the first embodiment operates as a negative electrode active material when combined with a known positive electrode material.
[0229] The fabricated electrochemical measurement cell was set at 1.0 V to 3.0 V (vs. Li / Li) based on the metallic lithium electrode. + ) potential range. The charge / discharge current was set to 0.2C (time discharge rate), and the 0.2C discharge capacity was confirmed at room temperature. The 0.2C discharge capacity is an index of energy density.
[0230] In addition, the coulombic efficiency associated with charging and discharging during the charge-discharge cycle was measured. Since the coulombic efficiency during the first charge-discharge cycle is affected by the reaction between the electrode and the electrolyte, the coulombic efficiency was examined from the charge capacity and discharge capacity at the 10th cycle, when the charge-discharge cycle becomes stable. The charge capacity at the 10th cycle is C c , discharge capacity is C d and the Coulomb efficiency is C d / C c × 100%.
[0231] Next, in order to examine the rate performance and cycle life performance of the battery, a nonaqueous electrolyte battery (rated capacity 1000 mAh) was fabricated using the active material powder obtained in each example according to the following procedure.
[0232] (Preparation of negative electrode) A slurry was obtained by mixing 100% by mass of the active material powder obtained in each example, 10% by mass of acetylene black as a conductive agent, 5% by mass of carbon nanofiber, 10% by mass of polyvinylidene fluoride (PVdF) as a binder with N-methylpyrrolidone (NMP). This slurry was applied to both sides of a current collector made of aluminum foil with a thickness of 12 μm, and dried under vacuum at 130° C. for 12 hours to obtain a laminate. After that, the density of the active material-containing layer was 2.4 g / cm 3 The laminate was rolled so that the negative electrode was obtained (excluding the current collector).
[0233] (Preparation of positive electrode) A mixture was obtained by mixing 90 parts by mass of commercially available lithium cobalt oxide (LiCoO2) with 5 parts by mass of acetylene black as a conductive assistant. Next, this mixture was dispersed in NMP to obtain a dispersion liquid. PVdF as a binder was mixed with this dispersion liquid in a ratio of 5 parts by mass relative to the lithium cobalt oxide to prepare a positive electrode slurry. This slurry was applied to both sides of a current collector made of 12 μm aluminum foil using a blade. This was dried under vacuum at 130 °C for 12 hours to obtain a laminate. Thereafter, the density of the active material-containing layer was 2.2 g / cm 3 The laminate was rolled so that the cathode was obtained (excluding the current collector).
[0234] (Preparation of electrode groups) The positive and negative electrodes thus prepared were laminated with a polyethylene separator sandwiched therebetween to obtain a laminate. The laminate was then wound and pressed to obtain a flat wound electrode group. A positive electrode terminal and a negative electrode terminal were connected to the electrode group.
[0235] (Preparation of non-aqueous electrolyte) A mixed solvent of ethylene carbonate and diethyl carbonate (volume ratio 1:1) was prepared. Lithium hexafluorophosphate (LiPF6) was dissolved in this solvent at a concentration of 1 M. Thus, a liquid nonaqueous electrolyte was prepared.
[0236] (Assembly of non-aqueous electrolyte batteries) The electrode group produced as described above was placed in a battery exterior made of an aluminum laminate film, a nonaqueous electrolyte was injected, and the opening was then heat sealed to produce a nonaqueous electrolyte battery.
[0237] (Charge / discharge test) A discharge rate test was carried out using the obtained laminated battery. The battery was charged at a rate of 0.2 C so that the cell voltage reached 3.0 V, and charging was terminated when the current value reached a value equivalent to 0.05 C. First, the discharge capacity C at a rate of 0.2 C was 0.2 After measuring the discharge rate capacity C5 at 5C, the ratio of the 5C discharge capacity to the 0.2C discharge capacity (C5 / C 0.2 ) × 100% was calculated as the 5C discharge capacity retention rate.
[0238] Next, an accelerated life test was performed at 45°C. In the charge / discharge test, 500 cycles of charge / discharge were repeated at a cell voltage of 1.5V to 3.0V with a charge / discharge current value of 0.2C (time discharge rate) (one cycle is one charge and one discharge), and the discharge capacity retention rate after 500 cycles was examined. The discharge capacity after 500 cycles was divided by the initial discharge capacity and multiplied by 100 to calculate the cycle capacity retention rate (%) when the initial discharge capacity was 100%.
[0239] The above results are summarized in Tables 1 to 3 below. Table 1 shows the composition of the crystal phase of the niobium titanium oxide synthesized in each example and the synthesis method thereof. Table 2 shows the space group to which the niobium titanium oxide phase in the active material of each example belongs, the octahedral sites composed only of corner sharing, the bond angle distortion and crystallite size in the octahedral sites, and the average particle size (D 50 Table 3 shows the 0.2C discharge capacity and Coulombic efficiency (charge / discharge efficiency) obtained by electrochemical measurement of a three-electrode beaker cell using the active material of each example, and the 5C discharge capacity retention rate (rate performance) and cycle capacity retention rate (life performance) obtained by electrochemical measurement of a laminated nonaqueous electrolyte battery using the active material of each example in the negative electrode.
[0240] [Table 1]
[0241] [Table 2]
[0242] [Table 3]
[0243] The niobium titanium oxide phase contained in the active material synthesized in each example contained at least one octahedral site in the unit lattice that was composed only of corner sharing, as shown in Table 2. For all of the active materials in Examples 1 to 12, the bond angle distortion of the octahedral site was 0.8σ 2 / deg 2 The crystallite diameter of the niobium titanium oxide phase was 85 nm or more. In contrast, in Comparative Examples 1, 2, and 4, the bond angle distortion of the octahedral site with only corner sharing was 0.8σ 2 / deg 2In Comparative Example 3, the crystallite diameter of the niobium titanium oxide phase was less than 85 nm. As shown in Table 3, the beaker cells using the active materials of each example showed similar low-rate (0.2 C) discharge capacities, and the capacity retention rates in high-rate (50 C) discharge of the nonaqueous electrolyte batteries using the active materials of each example were also similar. However, in terms of the Coulombic efficiency of the beaker cells and the cycle capacity retention rates of the nonaqueous electrolyte batteries, the test cells using the active materials of Examples 1 to 12 showed superior performance compared to the cells using the active materials of Comparative Examples 1 to 4.
[0244] According to at least one of the above-described embodiments and examples, an active material is provided, in which the bond angle distortion in the (Nb, Ti)O6 octahedral site composed only of corner sharing is 0.8 σ 2 / deg 2 The active material includes a niobium titanium oxide phase having a monoclinic crystal structure containing at least one octahedral site in a unit lattice, the crystal lattice system of the niobium titanium oxide phase being in the range of 85 nm to 130 nm. Such an active material can realize a secondary battery that can exhibit excellent charge / discharge efficiency and cycle life performance.
[0245] Several embodiments according to the present invention will be described below. [1] The niobium titanium oxide phase has a monoclinic crystal structure, and the crystal lattice of the niobium titanium oxide phase has a bond angle distortion of 0.8 σ at the (Nb, Ti)O6 octahedral sites composed of only corner sharing. 2 / deg 2 and the crystallite diameter of the niobium titanium oxide phase is within the range of 85 nm or more and 130 nm or less. [2] The niobium titanium oxide phase contains primary particles, and the primary particles have an average particle diameter D 50 The active material according to [1], wherein the average particle size is in the range of 0.1 μm or more and 10 μm or less. [3] The niobium titanium oxide phase is Nb2TiO7 phase and Nb 10 Ti2O 29The active material according to [1] or [2], comprising at least one phase selected from the group consisting of phases. [4] The active material described in [3], wherein the at least one phase contains at least one selected from the group consisting of K, Zr, Sn, V, Ta, Mo, W, P, Y, Fe, Co, Cr, Mn, Ni and Al. [5] The niobium titanium oxide phase has a monoclinic crystal structure belonging to the space group C2 / m, and the bond angle distortion at the 2a site in the monoclinic crystal structure as described in the symmetry of the International Tables Volume A is 0.8 σ 2 / deg 2 The active material according to any one of [1] to [4] below. [6] An electrode comprising the active material according to any one of [1] to [5]. [7] The electrode according to [6], wherein the electrode includes an active material-containing layer that contains the active material. [8] A positive electrode; A negative electrode; Electrolytes and A secondary battery comprising: The secondary battery according to the present invention, wherein the negative electrode is the electrode according to [6] or [7]. [9] A battery pack comprising the secondary battery described in [8].
[0246]
[10] An external terminal for supplying current; Protection circuit and The battery pack according to [9], further comprising:
[11] A battery comprising a plurality of the secondary batteries, The battery pack according to [9] or
[10] , wherein the secondary batteries are electrically connected in series, in parallel, or in a combination of series and parallel.
[12] A vehicle equipped with a battery pack described in any one of [9] to
[11] .
[13] A vehicle as described in
[12] , including a mechanism for converting kinetic energy of the vehicle into regenerative energy.
[0247] Although some embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included in the scope and spirit of the invention, and are included in the scope of the invention and its equivalents described in the claims. [Explanation of symbols]
[0248] Reference Signs List 1...electrode group, 2...exterior member, 3...negative electrode, 3a...negative electrode current collector, 3b...negative electrode active material-containing layer, 3c...negative electrode current collector tab, 4...separator, 5...positive electrode, 5a...positive electrode current collector, 5b...positive electrode active material-containing layer, 6...negative electrode terminal, 7...positive electrode terminal, 21...bus bar, 22...positive electrode side lead, 23...negative electrode side lead, 24...adhesive tape, 31...container, 32...lid, 33...protective sheet, 34...printed wiring board, 35 ...wiring, 40...vehicle body, 41...vehicle power source, 42...electrical control device, 43...external terminal, 44...inverter, 45...driving motor, 100...secondary battery, 101...metal ion, 102...oxide ion, 103...octahedron, 104...void portion, 105...region, 106...region, 107...void portion, 113...octahedron, 123...octahedron, 133...octahedron, 143...octahedron, 153...octahedron, 200 ... battery pack, 200a... battery pack, 200b... battery pack, 200c... battery pack, 300... battery pack, 300a... battery pack, 300b... battery pack, 300c... battery pack, 301a... battery pack monitoring device, 301b... battery pack monitoring device, 301c... battery pack monitoring device, 342... positive connector, 343... negative connector, 345... thermistor, 346... protection circuit, 342a... wiring, 343a... Wiring, 350...external terminal for current flow, 352...positive terminal, 353...negative terminal, 348a...positive wiring, 348b...negative wiring, 400...vehicle, 411...battery management device, 412...communication bus, 413...positive terminal, 414...negative terminal, 415...switch device, 416...current detection unit, 417...negative input terminal, 418...positive input terminal, L1...connection line, L2...connection line, W...drive wheel.
Claims
1. The niobium titanium oxide phase has a monoclinic structure, and the niobium titanium oxide phase has a crystal lattice structure consisting of only corner sharing (Nb, Ti)O 6 Bond angle distortion at the octahedral site is 0.8 σ 2 / deg 2 and the crystallite diameter of the niobium titanium oxide phase is within the range of 85 nm to 130 nm.
2. The niobium titanium oxide phase contains primary particles, and the average particle diameter D 50 The active material according to claim 1 , wherein the average particle diameter is in the range of 0.1 μm or more and 10 μm or less.
3. The niobium titanium oxide phase is Nb 2 TiO 7 phase and Nb 10 Ti 2 O 29 3. The active material of claim 1 , comprising at least one phase selected from the group consisting of:
4. 4. The active material of claim 3, wherein the at least one phase contains at least one selected from the group consisting of K, Zr, Sn, V, Ta, Mo, W, P, Y, Fe, Co, Cr, Mn, Ni, and Al.
5. The niobium titanium oxide phase has a monoclinic crystal structure belonging to the space group C2 / m, and the bond angle distortion at the 2a site in the monoclinic crystal structure as described in the symmetry of the International Tables Volume A is 0.8 σ 2 / deg 2 3. The active material according to claim 1, wherein:
6. An electrode comprising the active material according to claim 1 or 2.
7. The electrode according to claim 6 , wherein the electrode comprises an active material-containing layer that contains the active material.
8. A positive electrode and A negative electrode; Electrolytes and A secondary battery comprising: The negative electrode of the secondary battery is the electrode according to claim 6.
9. A battery pack comprising the secondary battery according to claim 8.
10. An external terminal for supplying electricity; Protection circuit and The battery pack of claim 9 further comprising:
11. A battery comprising a plurality of the secondary batteries, The battery pack according to claim 9 , wherein the secondary batteries are electrically connected in series, in parallel, or in a combination of series and parallel.
12. A vehicle equipped with the battery pack according to claim 9.
13. The vehicle of claim 12, further comprising a mechanism for converting kinetic energy of the vehicle into regenerative energy.
Citation Information
Patent Citations
Electrode, secondary battery, battery pack, and vehicle
JP2019169350A