Electrochemical device and electronic device

By adding silicon element to the negative electrode material layer of lithium-ion batteries, and using a combination of ethylene carbonate and specific compounds in the electrolyte, a stable SEI film is formed, which solves the problem of unstable interface films of lithium-ion batteries and improves battery performance. cycle stability and charge and discharge efficiency.

CN118782878APending Publication Date: 2024-10-15NINGDE AMPEREX TECHNOLOGY LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410763808.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

During the charge and discharge process of existing lithium-ion batteries, the properties of the solid electrolyte interface film are unstable, which affects the cycle stability and charge and discharge efficiency of the electrochemical device.

Method used

By adding 20% ​​to 50% silicon element to the negative electrode material layer, and using a combination containing ethylene carbonate and specific compounds in the electrolyte, an SEI film combining inorganic and organic substances is formed, and its mass percentage is controlled to improve Ion transport performance and stability of SEI membrane.

Benefits of technology

Significantly improves the charge and discharge efficiency and cycle stability of lithium-ion batteries, reduces the transmission impedance of lithium ions, and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118782878A_ABST
    Figure CN118782878A_ABST
Patent Text Reader

Abstract

The present application provides an electrochemical device and an electronic device, the electrochemical device comprises a negative pole piece and an electrolyte, the negative pole piece comprises a negative pole material layer, the negative pole material layer comprises a silicon element, the mass percentage of the silicon element is 20-50% based on the total mass of the negative pole material layer, the electrolyte comprises a compound of formula (I) and ethylene carbonate, based on the total mass of the electrolyte, the mass percentage content of the ethylene carbonate is 5%-40%. The negative electrode material layer comprises a silicon element, the electrolyte comprises the compound shown in the formula (I) and ethylene carbonate, and the mass percentage content of the silicon element and the ethylene carbonate is regulated and controlled within the range, so that the ion transmission performance and stability of a solid electrolyte interface are improved, and the charge-discharge efficiency and the cycle stability of an electrochemical device are improved. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of electrochemical technology, and in particular to an electrochemical device and an electronic device. Background Art

[0002] With the rapid development of electronic products, electrochemical devices are widely used in mobile phones, laptops, tablets, drones, electric vehicles, power tools, power storage systems, etc. due to their advantages such as high energy density, miniaturization and light weight. Especially in the field of 3C products, consumer users still have great demand for improving the battery life of electronic products, so higher requirements are put forward for the energy density of electrochemical devices.

[0003] During the first charge and discharge process of an electrochemical device, such as a lithium-ion battery, a large amount of solid electrolyte interphase (SEI) will be produced on the negative electrode surface. This is due to the formation of a thin film of stable compounds produced by the decomposition of the electrolyte between the electrolyte and the electrode of the lithium-ion secondary battery. Therefore, the properties of the SEI film depend largely on the composition of the electrolyte. The SEI film plays a key role in lithium-ion batteries. It helps protect electrode materials, stabilize the electrolyte interface, and regulate the transmission of lithium ions. Therefore, it is particularly important to select suitable electrolyte components to form an SEI film with suitable properties to improve the charge and discharge performance and cycle stability of lithium-ion batteries. Summary of the invention

[0004] The purpose of the present application is to provide an electrochemical device and an electronic device to improve the charge and discharge efficiency and cycle stability of the electrochemical device.

[0005] The first aspect of the present application provides an electrochemical device, which includes a negative electrode plate and an electrolyte, wherein the negative electrode plate includes a negative electrode material layer, the negative electrode material layer includes silicon element, and the mass percentage of the silicon element is 20% to 50% based on the total mass of the negative electrode material layer; the electrolyte includes a compound of formula (I) and ethylene carbonate:

[0006]

[0007] wherein R1 is selected from a fluorine atom, an alkyl group of C1 to C6 which is at least partially substituted with fluorine, a C6 to C 10 aryl, C1 to C6 oxygen-containing alkyl at least partially substituted with fluorine, C6 to C 10 The oxygen-containing aromatic group, wherein the O atom in R1 is not directly connected to the S atom; R2 and R3 are each independently selected from an unsubstituted or partially fluorinated C1 to C5 alkyl group, an unsubstituted or partially fluorinated C6 to C 10 In the case of an aryl group, R2 and R3 may be connected to form a ring.

[0008] Based on the total mass of the electrolyte, the mass percentage of ethylene carbonate is 5% to 40%. The negative electrode material layer includes silicon, the electrolyte includes the compound of formula (I) and ethylene carbonate, and the mass percentage of silicon and the mass percentage of ethylene carbonate are regulated within the above range, which is conducive to forming a SEI film combining inorganic and organic substances, improving the ion transport performance and stability of the SEI film, thereby improving the charge and discharge efficiency and cycle stability of the electrochemical device.

[0009] In one embodiment of the present application, the compound of formula (I) includes at least one of the following compounds:

[0010]

[0011]

[0012] The selection of the above compounds helps to improve the charge and discharge efficiency and cycle stability of electrochemical devices.

[0013] In one embodiment of the present application, the mass percentage of ethylene carbonate is 10% to 30% based on the total mass of the electrolyte. Adjusting the mass percentage of ethylene carbonate within the above range helps to improve the cycle stability and charge and discharge efficiency of the electrochemical device.

[0014] In one embodiment of the present application, based on the total mass of the electrolyte, the mass percentage of the compound of formula (I) is 3% to 50%. Regulating the mass percentage of the compound of formula (I) within the above range helps to improve the cycle stability and charge and discharge efficiency of the electrochemical device.

[0015] In one embodiment of the present application, the mass percentage of the compound of formula (I) is 10% to 40% based on the total mass of the electrolyte. Regulating the mass percentage of the compound of formula (I) within the above range helps to further improve the cycle stability and charge and discharge efficiency of the electrochemical device.

[0016] In one embodiment of the present application, the electrolyte further comprises fluoroethylene carbonate, and the mass percentage of fluoroethylene carbonate is 5% to 30% based on the total mass of the electrolyte. Regulating the mass percentage of fluoroethylene carbonate within the above range helps to improve the cycle stability and charge and discharge efficiency of the electrochemical device.

[0017] In one embodiment of the present application, the electrolyte further comprises fluoroethylene carbonate, and the mass percentage of fluoroethylene carbonate is 10% to 30% based on the total mass of the electrolyte. Regulating the mass percentage of fluoroethylene carbonate within the above range helps to further improve the cycle stability and charge and discharge efficiency of the electrochemical device.

[0018] In one embodiment of the present application, the electrolyte includes a cyclic compound containing a sulfur-oxygen double bond, and the cyclic compound containing a sulfur-oxygen double bond includes at least one of 1,3-propane sultone, 1,4-butane sultone or 2,4-butane sultone; based on the total mass of the electrolyte, the mass percentage of the cyclic compound containing a sulfur-oxygen double bond is 0.1% to 5%. The electrolyte includes a cyclic compound containing a sulfur-oxygen double bond and regulates its mass percentage within the above range, so that the electrochemical device has good cycle stability.

[0019] In one embodiment of the present application, the electrochemical device includes a separator and a positive electrode sheet, and along the direction in which the electrode ear of the electrochemical device extends, the length of the separator beyond the positive electrode sheet is a μm, and the thickness of the separator is b μm, 0.0008≤b / a≤0.009, 1000≤a≤5000. By regulating the values ​​of b and b / a within the above range, the electrochemical device can have good cycle stability and charge and discharge efficiency while having good safety performance.

[0020] The second aspect of the present application provides an electronic device, which includes the electrochemical device provided by the first aspect of the present application. Since the electrochemical device provided by the present application has good charge and discharge efficiency and cycle stability, the electronic device provided by the present application has good performance.

[0021] Beneficial effects of this application:

[0022] The present application provides an electrochemical device and an electronic device, wherein the electrochemical device comprises a negative electrode plate and an electrolyte, wherein the negative electrode plate comprises a negative electrode material layer, wherein the negative electrode material layer comprises silicon element, and the mass percentage of silicon element is 20% to 50% based on the total mass of the negative electrode material layer; and the electrolyte comprises a compound of formula (I) and ethylene carbonate (EC), and the mass percentage of ethylene carbonate is 5% to 40% based on the total mass of the electrolyte. Ethylene carbonate undergoes a reduction reaction on the surface of the negative electrode to form an organic-rich SEI film containing lithium carbonate ions, and the compound of formula (I) contains SO2N groups that can form an interface film rich in inorganic substances such as Li3N and Li2S. By combining inorganic and organic substances, the ion transport performance and stability of the SEI film can be improved, thereby improving the charge and discharge efficiency and cycle stability of the electrochemical device.

[0023] Of course, implementing any product or method of the present application does not necessarily require achieving all of the advantages described above at the same time. DETAILED DESCRIPTION

[0024] The technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. All other embodiments obtained by those skilled in the art based on the present application belong to the scope of protection of the present application.

[0025] It should be noted that in the specific embodiments of the present application, a lithium-ion battery is used as an example of an electrochemical device to explain the present application, but the electrochemical device of the present application is not limited to a lithium-ion battery.

[0026] The present application provides an electrochemical device, which includes a negative electrode plate and an electrolyte, wherein the negative electrode plate includes a negative electrode material layer, the negative electrode material layer includes silicon element, and based on the total mass of the negative electrode material layer, the mass percentage of silicon element is 20% to 50%; for example, the mass percentage of silicon element can be 20%, 22%, 25%, 28%, 30%, 35%, 40%, 45%, 48%, 50% or a range consisting of any two values ​​therein. The electrolyte includes a compound of formula (I) and ethylene carbonate:

[0027]

[0028] wherein R1 is selected from a fluorine atom, an alkyl group of C1 to C6 which is at least partially substituted with fluorine, a C6 to C 10 aryl, C1 to C6 oxygen-containing alkyl at least partially substituted with fluorine, C6 to C 10 The oxygen-containing aromatic group in R1 is not directly connected to the S atom; R2 and R3 are each independently selected from unsubstituted or partially fluorinated C1 to C5 alkyl, unsubstituted or partially fluorinated C6 to C 10 aromatic group, R2 and R3 can be connected to form a ring; based on the total mass of the electrolyte, the mass percentage of ethylene carbonate is 5% to 40%, preferably 10% to 30%, for example, the mass percentage of ethylene carbonate can be 5%, 8%, 10%, 12%, 15%, 18%, 20%, 22%, 25%, 28%, 30%, 32%, 35%, 38%, 40% or a range consisting of any two of the values.

[0029] By regulating the mass percentage of silicon element within the above range, the space required for the expansion of nano-silicon particles can be met during the charging and discharging process of the electrochemical device, thereby effectively alleviating the phenomenon of material rupture caused by the expansion of nano-silicon particles and improving the energy density and cycle performance of the electrochemical device. As a cyclic ester, ethylene carbonate (EC) has a high lithium salt dissociation ability and can improve the transmission performance of lithium ions. However, cyclic esters have poor stability and are easy to decompose by ring opening. Excessive addition will deteriorate the interface impedance and cause the battery performance to deteriorate. By regulating the mass percentage of EC within the above range, the electrolyte can have good lithium ion transmission performance and reduce the problem of EC ring opening decomposition leading to deterioration of the interface film that hinders lithium ion transmission and increases the interface impedance. During the cycle of lithium-ion batteries, EC undergoes reduction and decomposition on the negative electrode surface. EC has strong polarity and can form a stable complex with lithium ions, thereby forming a layer of organic-rich SEI film including lithium carbonate ions and other organic polymers. The organic-rich SEI film has good stability and good ion transmission performance, and the compound of formula (I) contains SO2N groups, which can form an interface film rich in inorganic substances such as Li3N and Li2S. Therefore, the electrolyte includes the compound of formula (I) and ethylene carbonate at the same time, and can form an SEI film containing the above organic and inorganic substances at the same time, improve the stability and ion transmission performance of the SEI film, reduce the transmission impedance of ions (such as lithium ions), enable the ions to be quickly deintercalated during the charge and discharge process, and improve the charge and discharge efficiency and cycle stability of the electrochemical device.

[0030] The negative electrode material layer of the present application includes silicon element, which is introduced by silicon-based materials, and the silicon-based materials can be selected from at least one of silicon-carbon composite materials, silicon-oxygen composite materials, micron silicon, Si-Sn alloy, Si-Mg alloy, Si-Ge alloy or Si-Zn alloy. In some embodiments, the above-mentioned silicon-carbon composite material can be carbon nanopore-loaded silicon.

[0031] In one embodiment of the present application, the compound of formula (I) includes at least one of the following compounds:

[0032]

[0033]

[0034]

[0035] By selecting the above compounds, it is helpful to increase the content of inorganic matter in the SEI film, further improve the ion transport performance of the SEI film, thereby improving the efficiency of lithium ion deintercalation during the charge and discharge process, and further improve the charge and discharge efficiency and cycle stability of the electrochemical device.

[0036] In one embodiment of the present application, based on the total mass of the electrolyte, the mass percentage of the compound of formula (I) is 3% to 50%, preferably 10% to 40%. For example, the mass percentage of the compound of formula (I) can be 3%, 5%, 8%, 10%, 13%, 15%, 18%, 20%, 23%, 25%, 27%, 30%, 33%, 35%, 37%, 40%, 43%, 45%, 48%, 50% or a range consisting of any two of the numerical values. The present application can form a SEI film composed of inorganic and organic substances at the negative electrode interface by combining the compound of formula (I) with EC to improve the lithium ion transmission performance; the mass percentage of the compound of formula (I) is regulated within the above range, so that the SEI film has better toughness, reduces the risk of its rupture, and reduces the problem of ion transmission obstruction caused by excessive thickness of the interface film, thereby improving the cycle stability and charge and discharge efficiency of the electrochemical device.

[0037] In one embodiment of the present application, the electrolyte further comprises fluoroethylene carbonate (FEC), and the mass percentage of fluoroethylene carbonate is 5% to 30%, preferably 10% to 30%, based on the total mass of the electrolyte. For example, the mass percentage of fluoroethylene carbonate can be 5%, 8%, 10%, 13%, 15%, 18%, 20%, 23%, 25%, 27%, 30% or a range consisting of any two of the numerical values. FEC is a good lithium-ion battery electrolyte additive. Adding FEC to the electrolyte can form a cross-linked high-toughness polymer protective layer at the electrode interface, reducing the side reaction between the silicon-based material and the electrolyte. By regulating the mass percentage of fluoroethylene carbonate within the above range, it is beneficial to further reduce the reaction between the silicon-based material and the electrolyte, thereby further improving the cycle stability of the electrochemical device, and improving the problem that the formed polymer protective layer is too thick to hinder the transmission of lithium ions, thereby improving the charge and discharge efficiency of the electrochemical device.

[0038] In one embodiment of the present application, the electrolyte includes a cyclic compound containing a sulfur-oxygen double bond, and the cyclic compound containing a sulfur-oxygen double bond includes at least one of 1,3-propane sultone, 1,4-butane sultone or 2,4-butane sultone; based on the total mass of the electrolyte, the mass percentage of the cyclic compound containing a sulfur-oxygen double bond is 0.1% to 5%. For example, the mass percentage of the cyclic compound containing a sulfur-oxygen double bond can be 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5% or a range consisting of any two of the values. The mass percentage of the cyclic compound containing a sulfur-oxygen double bond is regulated within the above range, and the sulfur-oxygen double bond compound and the compound of formula (I) can play a synergistic role in the film formation process, which is conducive to forming a more stable interface film on the surface of the negative electrode, reducing the side reaction between the silicon-based material and the electrolyte, and therefore, the electrochemical device has good cycle stability.

[0039] In the present application, the electrolyte also includes a lithium salt and a base solvent. The present application has no particular restrictions on the type of lithium salt, and lithium salts known in the art can be used. For example, the lithium salt may include but is not limited to at least one of LiBF4, LiPF6, LiAsF6, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3 and LiPO2F2; the present application has no particular restrictions on the base solvent, as long as the purpose of the present application can be achieved. For example, it may contain at least one of a carbonate compound, a carboxylate compound, an ether compound or other organic solvents. The above-mentioned carbonate compounds may include but are not limited to chain carbonate compounds or other cyclic carbonate compounds, and the above-mentioned chain carbonate compounds may include but are not limited to at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC) or ethyl methyl carbonate (EMC). The above-mentioned other cyclic carbonate compounds may include but are not limited to at least one of propylene carbonate (PC), butylene carbonate (BC) or vinyl ethylene carbonate (VEC). The above-mentioned carboxylate compounds may include but are not limited to at least one of ethyl acetate, propyl acetate, propyl propionate or ethyl propionate. The above-mentioned ether compounds may include but are not limited to at least one of dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, ethoxymethoxyethane, 2-methyltetrahydrofuran or tetrahydrofuran. The above-mentioned other organic solvents may include but are not limited to at least one of dimethyl sulfoxide, 1,2-dioxolane, cyclopentane, methyl cyclopentane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, formamide, dimethylformamide, trimethyl phosphate, triethyl phosphate, trioctyl phosphate or phosphate.

[0040] The present application has no particular restrictions on the mass percentage of lithium salt and base solvent in the electrolyte, as long as the purpose of the present application can be achieved. For example, based on the total mass of the electrolyte, the mass percentage of lithium salt can be 8% to 20%, for example, the mass percentage of lithium salt can be 8%, 10%, 13%, 15%, 18%, 20% or a range consisting of any two of the values. The mass percentage of the base solvent can be 0% to 84%, for example, the mass percentage of the base solvent can be 0%, 3%, 5%, 8%, 10%, 13%, 15%, 18%, 20%, 30%, 33%, 35%, 37%, 40%, 43%, 45%, 47%, 50%, 53%, 55%, 57%, 60%, 63%, 65%, 67%, 70%, 73%, 75%, 78%, 80%, 84% or a range consisting of any two of the values.

[0041] In the present application, the features of the different components contained in the above-mentioned electrolyte can be combined, and the implementation modes covered by the above-mentioned combination are all within the protection scope of the present application.

[0042] In one embodiment of the present application, the electrolyte may include a compound of formula (I), EC, a lithium salt, and a base solvent; the mass percentages of the compound of formula (I), EC, and the lithium salt are as described above, and the mass percentage of the base solvent is 0% to 84% based on the total mass of the electrolyte. The electrochemical device includes an electrolyte having the above characteristics, which is beneficial to improving its charge and discharge efficiency and cycle stability.

[0043] In one embodiment of the present application, the electrolyte may include a compound of formula (I), EC, FEC, a lithium salt, and a base solvent; the mass percentages of the compound of formula (I), EC, FEC, and the lithium salt are as described above, and the mass percentage of the base solvent is 0% to 79% based on the total mass of the electrolyte. The electrochemical device includes an electrolyte having the above characteristics, which is conducive to further improving its charge and discharge efficiency and cycle stability.

[0044] In one embodiment of the present application, the electrolyte may include a compound of formula (I), EC, a lithium salt, a base solvent, and a cyclic compound containing a sulfur-oxygen double bond; the mass percentages of the compound of formula (I), EC, a lithium salt, and the cyclic compound containing a sulfur-oxygen double bond are as described above, and the mass percentage of the base solvent is 0% to 83% based on the total mass of the electrolyte. The electrochemical device includes an electrolyte having the above characteristics, which is conducive to further improving its charge and discharge efficiency and cycle stability.

[0045] In one embodiment of the present application, the electrolyte may include a compound of formula (I), EC, FEC, a cyclic compound containing a sulfur-oxygen double bond, a lithium salt, and a base solvent; the mass percentages of the compound of formula (I), EC, FEC, a cyclic compound containing a sulfur-oxygen double bond, and a lithium salt are as described above, and the mass percentage of the base solvent is 0% to 78% based on the total mass of the electrolyte. The electrochemical device includes an electrolyte having the above characteristics, which is conducive to further improving its charge and discharge efficiency and cycle stability.

[0046] In one embodiment of the present application, the electrochemical device includes an isolation membrane and a positive electrode plate. Along the extension direction of the electrochemical device electrode ear, the length of the isolation membrane beyond the positive electrode plate is a μm, the thickness of the isolation membrane is b μm, 0.0008≤b / a≤0.009, 1000≤a≤5000. For example, the value of b / a can be 0.0008, 0.001, 0.002, 0.003, 0.004, 0.005, 0.006, 0.007, 0.008, 0.009 or a range consisting of any two of these values, and the value of a can be 1000, 1300, 1500, 1800, 2000, 2300, 2500, 2800, 3000, 3300, 3500, 3800, 4000, 4300, 4500, 4800, 5000 or a range consisting of any two of these values. In the present application, the direction along which the tab of the electrochemical device extends is the width direction of the positive electrode sheet. By regulating the values ​​of b / a and a within the above range, the risk of short circuit between the positive and negative electrodes can be reduced, and the space of the electrochemical device will not be wasted, resulting in the loss of mass energy density of the electrochemical device, so that the electrochemical device has a higher energy density. In addition, the addition of the compound of formula (I) improves the thermal shock resistance of the isolation membrane. If the FEC compound is added, the thermal shock resistance of the isolation membrane can be further improved. The isolation membrane that meets the above characteristics can also further reduce the temperature increase inside the electrochemical device under high temperature abuse, reduce the thermal shrinkage of the isolation membrane, and make the electrochemical device have good cycle stability and charge and discharge efficiency while further improving its safety performance. In the present application, the thickness b of the isolation membrane can be 4μm to 18μm. For example, the value of b can be 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18 or a range consisting of any two of the values.

[0047] The present application has no particular restrictions on the material of the isolation membrane, as long as the purpose of the present application can be achieved. For example, the isolation membrane may include at least one of polyethylene, polypropylene, polyvinylidene fluoride, polyethylene terephthalate, polyimide or aramid. For example, polyethylene may include at least one of high-density polyethylene, low-density polyethylene or ultra-high molecular weight polyethylene. The surface of the isolation membrane of the present application may include a porous layer. The present application has no particular restrictions on the porous layer on the surface of the isolation membrane, as long as the purpose of the present application can be achieved. For example, the porous layer is arranged on at least one surface of the isolation membrane, and the porous layer may include at least one of inorganic particles or binders. The porous layer can improve the heat resistance, oxidation resistance and electrolyte wetting performance of the isolation membrane, and enhance the adhesion between the isolation membrane and the pole piece. The size of the pore size is not particularly limited, as long as the purpose of the present application can be achieved. For example, the size of the pore size can be 0.01μm to 1μm. For example, the inorganic particles may include at least one of aluminum oxide (Al2O3), silicon oxide (SiO), magnesium oxide (MgO), titanium oxide (TiO2), hafnium oxide (HfO2), tin oxide (SnO2), cerium oxide (CeO2), nickel oxide (NiO), zinc oxide (ZnO), calcium oxide (CaO), zirconium oxide (ZrO2), yttrium oxide (Y2O3), silicon carbide (SiC), boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide, or barium sulfate, etc. For example, the binder of the porous layer may include at least one of polyvinylidene fluoride, a copolymer of vinylidene fluoride-hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, sodium carboxymethyl cellulose, polyvinyl pyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene, or polyhexafluoropropylene, etc.

[0048] The negative electrode sheet of the present application also includes a negative electrode current collector. The present application has no special restrictions on the negative electrode current collector, as long as the purpose of the present application can be achieved. For example, the negative electrode current collector may include but is not limited to copper foil, aluminum foil, nickel foil or carbon-based current collector, for example, the thickness of the negative electrode current collector is 4μm to 10μm. The present application has no special restrictions on the thickness of the negative electrode material layer, as long as the purpose of the present application can be achieved, for example, the thickness of the negative electrode material layer is 30μm to 150μm. The present application has no special restrictions on the thickness of the negative electrode sheet, as long as the purpose of the present application can be achieved, for example, the thickness of the negative electrode sheet is 50μm to 350μm. In the present application, the negative electrode material layer can be arranged on one surface in the thickness direction of the negative electrode current collector, or on two surfaces in the thickness direction of the negative electrode current collector. It should be noted that the "surface" here can be the entire area of ​​the negative electrode current collector or a part of the negative electrode current collector. The present application has no special restrictions, as long as the purpose of the present application can be achieved. The negative electrode material layer of the present application may also include a conductive agent and a binder.

[0049] The negative electrode material layer of the present application may also contain a carbon material, and the carbon material may be selected from at least one of natural graphite, artificial graphite, mesophase microcarbon beads, hard carbon, and soft carbon. Based on the total mass of the negative electrode material layer, the content of the carbon material may range from 10% to 70%. The negative electrode material layer of the present application may also include a binder and a conductive agent.

[0050] The present application has no particular restrictions on the positive electrode plate, as long as the purpose of the present application can be achieved. For example, the positive electrode plate includes a positive electrode current collector and a positive electrode material layer disposed on at least one surface of the positive electrode current collector. The present application has no particular restrictions on the positive electrode current collector, as long as the purpose of the present application can be achieved. For example, the positive electrode current collector may include aluminum foil or aluminum alloy foil, etc. The positive electrode material layer of the present application includes positive electrode active materials. The present application has no particular restrictions on the type of positive electrode active materials, as long as the purpose of the present application can be achieved. For example, the positive electrode active material may include LiCo 1-y M y O2、LiNi 1-y M y O2、LiMn 2-y M y O4、LiNi x Co y Mn z M 1-x-y-z O2, etc., M includes at least one of Fe, Co, Ni, Mn, Mg, Cu, Zn, Al, Sn, B, Ga, Cr, Sr, V, Ti, etc., 0≤y≤1, 0≤x≤1, 0≤z≤1, x+y+z≤1. For example, the positive electrode active material may also include at least one of lithium cobalt oxide (LiCoO2), lithium manganese oxide (LiMn2O4), lithium nickel oxide (LiNiO2), lithium iron phosphate (LiFePO4), lithium manganese iron phosphate, etc., and the above positive electrode active materials may be doped and / or coated. The present application has no special restrictions on the thickness of the positive electrode current collector, as long as the purpose of the present application can be achieved. For example, the thickness of the positive electrode current collector is 4μm to 12μm. The present application has no special restrictions on the thickness of the positive electrode material layer, as long as the purpose of the present application can be achieved. For example, the thickness of the positive electrode material layer is 30μm to 120μm. The present application has no particular limitation on the thickness of the positive electrode sheet, as long as the purpose of the present application can be achieved. For example, the thickness of the positive electrode sheet is 50 μm to 250 μm. The positive electrode material layer of the present application may also include a conductive agent and a binder.

[0051] The above-mentioned conductive agent and binder are not particularly limited, as long as the purpose of the application can be achieved. For example, the conductive agent may include at least one of conductive carbon black, acetylene black, Ketjen black, lamellar graphite, graphene, carbon nanotubes, carbon nanowires or carbon fibers. The binder may include at least one of polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer, styrene-acrylate copolymer, styrene-butadiene copolymer, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylic acid salt, sodium carboxymethyl cellulose (CMC-Na), polyvinyl acetate, polyvinyl pyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene, polyhexafluoropropylene, styrene-butadiene rubber (SBR), carboxymethyl cellulose (CMC), polyaniline, polyimide, polyamide-imide, polysiloxane, epoxy resin, polyester resin or polyurethane resin etc.

[0052] In some embodiments of the present application, the mass ratio of the positive electrode active material, the conductive agent, and the binder in the positive electrode material layer may be (70 to 98):(0.5 to 15):(1 to 15).

[0053] The preparation process of the electrochemical device is well known to those skilled in the art, and the present application has no particular limitation. For example, it may include but is not limited to the following steps: stacking the positive electrode sheet, the separator and the negative electrode sheet in order, and winding, folding and other operations as needed to obtain an electrode assembly of a wound structure, placing the electrode assembly in a packaging bag, injecting the electrolyte into the packaging bag and sealing it to obtain an electrochemical device; or, stacking the positive electrode sheet, the separator and the negative electrode sheet in order, and then fixing the four corners of the entire stacked structure with tape to obtain an electrode assembly of a stacked structure, placing the electrode assembly in a packaging bag, injecting the electrolyte into the packaging bag and sealing it to obtain an electrochemical device. In addition, overcurrent protection elements, guide plates, etc. may also be placed in the packaging bag as needed to prevent the pressure inside the electrochemical device from rising and overcharging and discharging. The present application does not limit the packaging bag, and those skilled in the art may select it according to actual needs, as long as the purpose of the present application can be achieved. For example, an aluminum-plastic film packaging bag may be used.

[0054] The second aspect of the present application provides an electronic device, which includes the electrochemical device provided by the first aspect of the present application. Since the electrochemical device provided by the present application has good charge and discharge efficiency and cycle stability, the electronic device provided by the present application has good performance.

[0055] The electronic device of the present application is not particularly limited, and it can be any electronic device known in the prior art. In some embodiments, the electronic device can include but is not limited to a laptop computer, a pen-input computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, an LCD TV, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery or a lithium-ion capacitor, etc.

[0056] Example

[0057] The following examples and comparative examples are given to more specifically describe the embodiments of the present application. Various tests and evaluations were performed according to the following methods. In addition, unless otherwise specified, "parts" and "%" are based on mass.

[0058] Test methods and equipment:

[0059] Measurement of the length of the separator extending beyond the positive electrode:

[0060] Disassemble the lithium-ion battery, take out the electrode assembly from the packaging bag, and obtain the negative electrode sheet, separator and positive electrode sheet stacked in sequence. Along the extension direction of the electrode ear of the electrochemical device, that is, along the width direction of the positive electrode sheet, measure the length of the separator extending beyond the edge of the positive electrode sheet as aμm. If it is an electrode assembly with a wound structure, it is necessary to unfold the electrode assembly to obtain the negative electrode sheet, separator and positive electrode sheet stacked in sequence, and then measure the length a of the separator extending beyond the edge of the positive electrode sheet.

[0061] Charge and discharge efficiency test:

[0062] The charge and discharge efficiency of lithium-ion batteries is evaluated by the first efficiency. During the first charge and discharge process of lithium-ion batteries, the battery is charged to 4.45V at a constant current of 0.5C, and then charged to 0.025C at a constant voltage of 4.45V. The charge capacity obtained before this is C0. After standing for 5 minutes, the battery is discharged to 3.0V at 0.5C, and the discharge capacity is D0. The first efficiency of the whole battery = D0 / C0.

[0063] Cyclic stability test:

[0064] The cycle stability of lithium-ion batteries is evaluated by the cycle capacity retention rate. Place the lithium-ion battery in a 25°C constant temperature test box and let it stand for 30 minutes to allow the lithium-ion battery to reach a constant temperature. Charge to 4.45V at a constant current of 0.5C, then charge at a constant voltage to a current of 0.025C, let it stand for 5 minutes, and discharge to 3.0V at a constant current of 0.5C, and record it as the initial discharge capacity C1. Follow this step for 200 cycles, record the discharge capacity C2 after 200 cycles, and calculate the cycle capacity retention rate of the lithium-ion battery. Cycle capacity retention rate (%) = C2 / C1×100%.

[0065] Test of mass percentage of silicon element:

[0066] The lithium-ion battery discharged at 0.5C to 3.0V was disassembled, the negative electrode plate was removed, and it was soaked in dimethyl carbonate (DMC) for 20 minutes, and then rinsed with DMC and acetone in turn. The negative electrode plate was then placed in an oven and baked at 80°C for 12 hours to obtain the negative electrode plate. The negative electrode plate was dried at 100°C in a vacuum oven for 24 hours, and 1g of the powdered sample of the negative electrode material layer on the negative electrode plate was scraped off with a blade, and then the mass percentage of silicon element in the negative electrode material layer was tested using an ICP (Inductively coupled plasma) analyzer.

[0067] Thermal shock test:

[0068] Place the lithium-ion battery in a 25℃ constant temperature test box and let it stand for 30 minutes to allow the lithium-ion battery to reach a constant temperature. Charge to 4.45V at a constant current of 0.5C, then charge to a current of 0.025C at a constant voltage. Place the lithium-ion battery to be tested vertically in the box and heat it to T=100℃ at a rate of 5±2℃ and keep it for 100 minutes. If the lithium-ion battery passes, heat it to T+1℃ and keep it at a constant temperature for 100 minutes, and increase the temperature by 1℃ each time until the lithium-ion battery fails to pass the test. Stop the test and record this temperature as the thermal shock temperature of the lithium-ion battery.

[0069] The passing standard is that the lithium-ion battery under test does not catch fire or explode during the 100-minute constant temperature test. Three batteries are tested in each group. If all three batteries pass the test, they are considered passed. If any one of them catches fire or explodes, it is considered failed.

[0070] Example 1-1

[0071] <Preparation of positive electrode sheet>

[0072] The positive electrode active material lithium cobalt oxide, conductive carbon black, and polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 95:2.5:2.5, and then N-methylpyrrolidone (NMP) is added as a solvent to prepare a slurry with a solid content of 75%, and stirred evenly. The slurry is evenly coated on one surface of a positive electrode current collector aluminum foil with a thickness of 10μm, and dried at 90°C to obtain a positive electrode sheet with a positive electrode material layer with a coating thickness of 110μm. After the above steps are completed, the single-sided coating of the positive electrode sheet is completed. After that, the above steps are repeated on the other surface of the positive electrode sheet to obtain a positive electrode sheet with a double-sided coating of positive electrode active materials. After the coating is completed, the positive electrode sheet is cut into a specification of 74mm×867mm and welded to the pole ear for standby use. The thickness of the single-sided positive electrode material layer after cold pressing is 75μm, and the compaction density of the positive electrode material layer is 4g / cm 3 .

[0073] <Preparation of negative electrode sheet>

[0074] Silicon-carbon composite material (carbon nanopore loaded silicon, based on the total mass of silicon-carbon composite material, silicon content is 50%), artificial graphite, negative electrode binder sodium carboxymethyl cellulose (CMC-Na), negative electrode binder styrene-butadiene rubber are mixed in a mass ratio of 70:20:2:8, deionized water is added, and mixed evenly under the action of a vacuum mixer to obtain a negative electrode slurry with a solid content of 30wt%. The negative electrode slurry is evenly coated on one side of a negative electrode current collector copper foil with a thickness of 12μm, and dried at 120°C to obtain a negative electrode sheet with a single-sided negative electrode material layer coated with a coating thickness of 143μm, and then the above steps are repeated on the other side of the copper foil to obtain a negative electrode sheet with a double-sided negative electrode material layer, and then cold pressed and cut to obtain a negative electrode sheet with a specification of 78mm×875mm. Among them, based on the total mass of the negative electrode material layer, the mass percentage of silicon element is 35%. The thickness of the single-sided negative electrode material layer after cold pressing is 80 μm, and the compaction density of the negative electrode material layer is 1 g / cm 3 .

[0075] <Preparation of Electrolyte>

[0076] In an argon atmosphere glove box with a water content of less than 10ppm, propylene carbonate (PC) and diethyl carbonate (DEC) are mixed at a mass ratio of PC:DEC = 2:8 to obtain a base solvent, and then lithium salt lithium hexafluorophosphate (LiPF6), ethylene carbonate and the compound of formula (I-1) are added and mixed evenly to obtain an electrolyte. Wherein, based on the total mass of the electrolyte, the mass percentage of lithium salt lithium hexafluorophosphate is 12.5%, the mass percentage of ethylene carbonate is 25%, the mass percentage of the compound of formula (I-1) is 50%, and the remainder is the base solvent.

[0077] <Preparation of Separator Film>

[0078] A polyethylene (PE) film with a thickness of b=15 μm (provided by Celgard) was used.

[0079] <Preparation of lithium-ion batteries>

[0080] The positive electrode sheet, separator, and negative electrode sheet prepared above are stacked in order, so that the separator is located between the positive electrode and the negative electrode to play a role of isolation, and the length a of the separator beyond the edge of the positive electrode along the extension direction of the electrode ear of the electrochemical device is 5000 μm, and the electrode assembly is wound. The electrode assembly is placed in an aluminum-plastic film packaging bag, and the electrolyte is injected after drying. The lithium-ion battery is obtained through vacuum packaging, standing, formation (0.1C constant current charging to 4.45V, and then constant voltage charging until the current drops to 0.02C), degassing, trimming and other processes.

[0081] Example 1-2 to Example 1-10

[0082] Except that the relevant parameters of the mass percentage of the compound of formula (I) and ethylene carbonate are adjusted according to Table 1 in <Preparation of Electrolyte>, the mass percentage of the base solvent is changed accordingly, and the mass percentage of LiPF6 remains unchanged, the rest is the same as Example 1-1.

[0083] Example 1-11 to Example 1-17

[0084] Except that the type of the compound of formula (I) is adjusted according to Table 1 in <Preparation of Electrolyte>, the rest is the same as Example 1-3.

[0085] Example 1-18 to Example 1-19

[0086] Except for <Preparation of Negative Electrode Plate>, the mass percentage of silicon element is adjusted as shown in Table 1 by adjusting the mass percentage of silicon-carbon composite material in the negative electrode material layer. When the mass percentage of silicon-carbon composite material changes, the mass percentage of artificial graphite changes accordingly. The rest is the same as Examples 1-3.

[0087] Comparative Example 1-1 to Comparative Example 1-8

[0088] Except that the parameters related to the contents of the compound of formula (I) and ethylene carbonate are adjusted according to Table 1 in <Preparation of Electrolyte>, the mass percentage of the base solvent changes accordingly, and the mass percentage of LiPF6 remains unchanged, the rest is the same as Example 1-3.

[0089] Example 2-1 to Example 2-15

[0090] The preparation of the electrolyte is the same as that of Examples 1-3, except that a cyclic compound containing a sulfur-oxygen double bond and / or fluoroethylene carbonate is added according to Table 2 and the mass percentage thereof and the type of the cyclic compound containing a sulfur-oxygen double bond are adjusted, the mass percentage of the base solvent is changed accordingly, and the mass percentage of LiPF6 remains unchanged.

[0091] Example 3-1 to Example 3-5

[0092] Except that the isolation membrane with different parameters is selected in <Preparation of isolation membrane> so that the values ​​of a, b and b / a are as shown in Table 3, the rest is the same as Example 1-3.

[0093] The preparation parameters and performance parameters of each embodiment and comparative example are shown in Tables 1 to 3.

[0094] Table 1

[0095]

[0096]

[0097] Note: “ / ” in Table 1 means there is no corresponding parameter or substance.

[0098] From Examples 1-1 to 1-19 and Comparative Examples 1-1 to 1-8, it can be seen that the type of compound of formula (I) is selected within the scope of the present application, and the mass percentage of ethylene carbonate and the mass percentage of silicon are regulated, while the comparative examples do not simultaneously meet the above characteristics. Compared with the above comparative examples, in the examples of the present application, the lithium-ion battery has a higher capacity retention rate and first efficiency, indicating that the lithium-ion battery has better cycle stability and charge and discharge efficiency.

[0099] In the electrolyte, the mass percentage of the compound of formula (I) usually affects the charge and discharge efficiency and cycle stability of the lithium ion battery. It can be concluded from Examples 1-1 to 1-5 and Comparative Examples 1-2 to 1-5 that when the mass percentage of the compound of formula (I) is too high, such as in Comparative Example 1-4, the capacity retention rate and the initial efficiency of the lithium ion battery are low; when the mass percentage of the compound of formula (I) is too low, such as in Comparative Example 1-2, the capacity retention rate and the initial efficiency of the lithium ion battery are low; when the compound of formula (I) is not contained, such as in Comparative Example 1-5, the capacity retention rate and the initial efficiency of the lithium ion battery are low; indicating that when the mass percentage of the compound of formula (I) is too high or too low, the cycle stability and the charge and discharge efficiency of the lithium ion battery cannot be improved. By regulating the mass percentage of the compound of formula (I) within the scope of the present application, an inorganic-rich interface film is formed, the ion transport performance of the SEI film is further improved, and the transmission impedance of lithium ions is reduced, thereby improving the capacity retention rate and the initial efficiency of the lithium-ion battery, indicating that the lithium-ion battery has better cycle stability and charge and discharge efficiency.

[0100] The electrolyte includes EC and the mass percentage of EC usually affects the charge and discharge efficiency and cycle stability of the lithium ion battery. It can be seen from Examples 1-3, Examples 1-6 to Examples 1-10, and Comparative Examples 1-1 to Comparative Examples 1-4 that when the mass percentage of EC is too low, such as Comparative Example 1-2, the capacity retention rate and the first efficiency of the lithium ion battery are low. When the mass percentage of EC is too high, such as Comparative Example 1-3, the capacity retention rate and the first efficiency of the lithium ion battery are low. When the electrolyte does not contain EC, such as Comparative Example 1-1, the capacity retention rate and the first efficiency of the lithium ion battery are low, indicating that when the electrolyte does not contain EC and the mass percentage of EC is too high or too low, the cycle stability and charge and discharge efficiency of the lithium ion battery cannot be improved. By adjusting the mass percentage of EC within the scope of this application, the transmission performance of lithium ions can be improved, and the lithium ion battery can have a higher capacity retention rate and first efficiency, indicating that the lithium ion battery has better cycle stability and charge and discharge efficiency.

[0101] The type of compound of formula (I) usually affects the charge and discharge efficiency and cycle stability of lithium ion batteries. It can be seen from Examples 1-3, 1-11 to 1-17 that the use of compounds of formula (I) within the scope of the present application can make the lithium ion battery have a higher capacity retention rate and initial efficiency, indicating that the lithium ion battery has good cycle stability and charge and discharge efficiency.

[0102] In the negative electrode material layer, the mass percentage of silicon element usually affects the charge and discharge efficiency and cycle stability of the lithium-ion battery. It can be seen from Examples 1-3, 1-18 and 1-19 that by regulating the mass percentage of silicon element within the scope of this application, the lithium-ion battery can have a higher capacity retention rate and initial efficiency, indicating that the lithium-ion battery has good cycle stability and charge and discharge efficiency.

[0103] Table 2

[0104]

[0105] Note: “ / ” in Table 2 means there is no corresponding parameter or substance.

[0106] The mass percentage of FEC usually affects the cycle stability and charge-discharge efficiency of lithium-ion batteries. When FEC is further added to the electrolyte and the mass percentage of FEC is within the scope of this application, such as Example 2-1 to Example 2-4, the lithium-ion battery has a higher cycle capacity retention rate and initial efficiency. By using FEC as a good lithium-ion battery electrolyte additive, adding FEC to the electrolyte can form a cross-linked high-toughness polymer protective layer at the electrode interface, reducing the side reaction between the silicon-based material and the electrolyte. This shows that the cycle stability and charge-discharge efficiency of the lithium-ion battery are further improved.

[0107] The type and mass percentage of the cyclic compound containing a sulfur-oxygen double bond usually affect the cycle stability and charge-discharge efficiency of the lithium-ion battery. When the electrolyte further adds a cyclic compound containing a sulfur-oxygen double bond, and the type and mass percentage of the cyclic compound containing a sulfur-oxygen double bond are within the scope of the present application, such as Examples 2-5 to 2-7, and Example 2-15, the lithium-ion battery has a higher cycle capacity retention rate and first efficiency. The sulfur-oxygen double bond compound and the compound of formula (I) can play a synergistic role in the film formation process, which is conducive to forming a stable SEI film with better ion transport performance on the negative electrode surface. It shows that the cycle stability and charge-discharge efficiency of the lithium-ion battery are further improved.

[0108] It can be seen from Examples 1-3 and 2-8 to 2-13 that when the electrolyte includes FEC and a cyclic compound containing a sulfur-oxygen double bond at the same time, the synergistic effect of FEC and the sulfur-oxygen double bond compound with the compound of formula (I) in the film formation process can make the lithium ion battery have a higher capacity retention rate and initial efficiency, indicating that the lithium ion battery has good cycle stability and charge and discharge efficiency.

[0109] Table 3

[0110]

[0111] The length of the separator beyond the positive electrode sheet and the thickness of the separator usually affect the cycle stability, charge and discharge efficiency and thermal shock performance of the lithium-ion battery. It can be seen from Examples 1-3 and 3-1 to 3-5 that when the values ​​of a and b / a are within the range of the present application, the lithium-ion battery has a higher cycle capacity retention rate, first efficiency and thermal shock temperature, indicating that the lithium-ion battery has good cycle stability and charge and discharge efficiency while having good thermal shock performance.

[0112] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.

Claims

1. An electrochemical device comprising a negative electrode sheet and an electrolyte, wherein: The negative electrode plate includes a negative electrode material layer, the negative electrode material layer includes silicon element, and based on the total mass of the negative electrode material layer, the mass percentage of the silicon element is 20% to 50%; The electrolyte comprises a compound of formula (I) and ethylene carbonate: wherein R1 is selected from a fluorine atom, an alkyl group of C1 to C6 which is at least partially substituted with fluorine, a C6 to C 10 aryl, C1 to C6 oxygen-containing alkyl at least partially substituted with fluorine, C6 to C 10 An oxygen-containing aromatic group, wherein the O atom in R1 is not directly connected to the S atom; R2 and R3 are each independently selected from unsubstituted or partially fluorinated C1 to C5 alkyl, unsubstituted or partially fluorinated C6 to C 10 The aromatic group, R2 and R3 may be connected to form a ring; Based on the total mass of the electrolyte, the mass percentage of the ethylene carbonate is 5% to 40%.

2. The electrochemical device according to claim 1, wherein: The compound of formula (I) comprises at least one of the following compounds:

3. The electrochemical device according to claim 1, wherein Based on the total mass of the electrolyte, the mass percentage of the ethylene carbonate is 10% to 30%.

4. The electrochemical device according to claim 1, wherein Based on the total mass of the electrolyte, the mass percentage of the compound of formula (I) is 3% to 50%.

5. The electrochemical device according to claim 1, wherein Based on the total mass of the electrolyte, the mass percentage of the compound of formula (I) is 10% to 40%.

6. The electrochemical device according to claim 1, wherein The electrolyte further comprises fluoroethylene carbonate, and the mass percentage of the fluoroethylene carbonate is 5% to 30% based on the total mass of the electrolyte.

7. The electrochemical device according to claim 1, wherein: The electrolyte further comprises fluoroethylene carbonate, and the mass percentage of the fluoroethylene carbonate is 10% to 30% based on the total mass of the electrolyte.

8. The electrochemical device according to claim 1, wherein The electrolyte includes a cyclic compound containing a sulfur-oxygen double bond, and the cyclic compound containing a sulfur-oxygen double bond includes at least one of 1,3-propane sultone, 1,4-butane sultone or 2,4-butane sultone; Based on the total mass of the electrolyte, the mass percentage of the cyclic compound containing sulfur-oxygen double bonds is 0.1% to 5%.

9. The electrochemical device according to any one of claims 1 to 8, wherein: The electrochemical device comprises an isolation membrane and a positive electrode sheet. Along the extension direction of the electrode ear of the electrochemical device, the length of the isolation membrane beyond the positive electrode sheet is a μm, the thickness of the isolation membrane is b μm, 0.0008≤b / a≤0.009, 1000≤a≤5000. 10 . An electronic device comprising the electrochemical device according to claim 1 .

Citation Information

Cited By

  • Electrochemical apparatus and electronic apparatus

    WO2025256216A1

  • Non-aqueous electrolyte and lithium secondary battery comprising same

    WO2026142212A1

  • Electrolyte and electrochemical device

    WO2026183659A1