Starch-based doped hard carbon material as well as preparation method and application thereof

By combining esterified starch with phosphate and acid anhydride, the reaction temperature and conditions are controlled, and high-performance starch-based doped hard carbon materials are prepared, solving the problems of poor agglomeration and electrochemical performance when preparing hard carbon materials in starch are solved. , realizes the efficient electrochemical performance of sodium ion batteries.

CN118908183APending Publication Date: 2024-11-08WUHAN BISIDI BATTERY MATERIAL CO LTD

Patent Information

Application Number
CN202411206786.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the prior art, the use of starch to prepare hard carbon materials is prone to agglomeration problems, and the electrochemical performance is poor, making it difficult to meet the needs of sodium ion batteries.

Method used

The esterified starch, phosphate and acid anhydride are used as esterification agents to prepare starch-based doped hard carbon materials through esterification reaction, pre-carbonization and carbonization steps, control the esterification reaction temperature to avoid agglomeration, and use it during the carbonization process. Protect gases to improve material performance.

Benefits of technology

The specific capacity and charge and discharge efficiency of starch-based doped hard carbon materials are significantly improved, volume expansion is avoided, and the electrochemical performance of the material is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908183A_ABST
    Figure CN118908183A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of battery materials, and discloses a starch-based doped hard carbon material as well as a preparation method and application thereof. The preparation method comprises the following steps: mixing starch with an esterifying agent, carrying out esterification reaction to obtain esterified starch, then pre-carbonizing to obtain a pre-carbonized material, and carbonizing to obtain the starch-based doped hard carbon material, the esterifying agent comprises phosphate and anhydride. Through specific selection of the esterifying agent and mutual cooperation of phosphate and acid anhydride, the electrochemical performance of the prepared starch-based doped hard carbon material is obviously improved, for example, the specific capacity is high, and the charge-discharge efficiency is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of battery materials, and in particular relates to a starch-based doped hard carbon material and a preparation method and application thereof. Background Art

[0002] The raw materials required for sodium-ion batteries are abundant and have great market prospects. As one of the main materials for sodium-ion batteries, the negative electrode material greatly affects the electrochemical performance of the battery. Among them, hard carbon is common because it is the main negative electrode material for sodium-ion batteries. Common precursor materials for preparing hard carbon are mainly divided into four types: biomass precursors, sugar precursors, synthetic resin precursors, and asphalt precursors. Starch is a renewable and environmentally friendly biomass precursor, which is used to prepare hard carbon materials and has the significant advantage of low cost.

[0003] In the prior art, in the process of preparing hard carbon materials using starch, problems such as agglomeration or poor electrochemical performance (such as specific capacity) of the prepared hard carbon materials may easily occur.

[0004] Therefore, there is an urgent need to provide a new starch-based hard carbon material with good electrochemical properties. Summary of the invention

[0005] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a starch-based doped hard carbon material and a preparation method and application thereof.

[0006] A first aspect of the present invention provides a method for preparing a starch-doped hard carbon material.

[0007] Specifically, a method for preparing a starch-doped hard carbon material comprises the following steps:

[0008] Mix starch with an esterifying agent and carry out esterification reaction to obtain esterified starch.

[0009] Pre-carbonizing the esterified starch to obtain a pre-carbonized material;

[0010] Carbonizing the pre-carbonized material to obtain the starch-based doped hard carbon material;

[0011] Wherein, the esterification agent includes phosphate and acid anhydride.

[0012] A second aspect of the present invention provides a starch-based doped hard carbon material.

[0013] A starch-doped hard carbon material is prepared by the above preparation method.

[0014] A third aspect of the present invention provides an application of a starch-based doped hard carbon material.

[0015] A sodium ion battery comprises the above-mentioned starch-based doped hard carbon material.

[0016] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0017] (1) The preparation method of the present invention specifically selects an esterifying agent. Specifically, the esterifying agent of the present invention includes phosphate and acid anhydride. Phosphate not only serves as a part of the esterifying agent, but also plays a role of doping phosphorus, which is beneficial to improving the specific capacity of starch-based doped hard carbon materials; acid anhydride not only serves as an esterifying agent, but also helps to inhibit the volume expansion of starch-based doped hard carbon materials during the preparation process, and also has the effect of slightly improving the yield. Through the mutual coordination of phosphate and acid anhydride, the electrochemical properties of the prepared starch-based doped hard carbon material are significantly improved, such as high specific capacity and charge and discharge efficiency.

[0018] (2) Temperature control during the esterification process is helpful to avoid or reduce material agglomeration, thereby allowing the material to undergo a uniform esterification reaction and obtain uniformly esterified starch. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The charge and discharge curves of button batteries assembled from starch-doped hard carbon materials of Example 1 and Example 4 and starch-doped hard carbon materials of Comparative Examples 1-2;

[0020] Figure 2 These are actual pictures of the starch-doped hard carbon material of Example 1 and the starch-doped hard carbon material of Comparative Examples 1-2. DETAILED DESCRIPTION

[0021] The technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work belong to the scope of protection of the present application. In addition, it should be understood that the specific implementation methods described herein are only used to illustrate and explain the present application, and are not used to limit the present application.

[0022] In the description of the present application, the term "including" means "including but not limited to". Various embodiments of the present invention may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present invention; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0023] In this application, "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural.

[0024] In the present application, "at least one", "at least one" and other similar descriptions specifically refer to one or more, one or more; "multiple", "multiple" and other similar descriptions specifically refer to two or more, two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all represent: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or plural, respectively.

[0025] The present application provides a method for preparing a starch-doped hard carbon material, comprising the following steps:

[0026] Mix starch with an esterifying agent and carry out esterification reaction to obtain esterified starch.

[0027] Pre-carbonizing the esterified starch to obtain a pre-carbonized material;

[0028] Carbonizing the pre-carbonized material to obtain the starch-based doped hard carbon material;

[0029] Wherein, the esterification agent includes phosphate and acid anhydride.

[0030] In some embodiments of the present invention, the phosphate is selected from at least one of diammonium hydrogen phosphate, ammonium dihydrogen phosphate, calcium hydrogen phosphate, potassium dihydrogen phosphate, dipotassium hydrogen phosphate, sodium acid pyrophosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium phosphate, and sodium pyrophosphate.

[0031] In some embodiments of the present invention, the acid anhydride is selected from at least one of acetic anhydride, maleic anhydride, phthalic anhydride, boric anhydride, butyric anhydride and succinic anhydride.

[0032] In some embodiments of the present invention, the starch is dried before being mixed with the esterifying agent.

[0033] In some embodiments of the present invention, the starch is dried at a temperature of 110-150°C, for example, 120-140°C.

[0034] In some embodiments of the present invention, the starch is dried for 8-14 hours, for example, 8 hours, 10 hours, or 12 hours.

[0035] In some embodiments of the present invention, the starch is at least one of corn starch, potato starch, wheat starch, sweet potato starch, mung bean starch and tapioca starch.

[0036] In some embodiments of the present invention, the temperature of the esterification reaction is 65-100°C, for example, 65-85°C. Specifically, it can be 65°C, 75°C, 85°C, 90°C, 95°C, or 100°C.

[0037] In some embodiments of the present invention, the esterification reaction time is 2-6 hours, for example, 2-5 hours, specifically, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours.

[0038] In some embodiments of the present invention, the mass of the esterification agent is 6-15% of the mass of the starch, for example, 8-12%. Specifically, it can be 6%, 8%, 9%, 12%, or 15%.

[0039] In some embodiments of the present invention, in the esterification agent, the mass ratio of phosphate to anhydride is (3-5):5. Specifically, it can be 3:5, 10:15, or 5:5.

[0040] In some embodiments of the present invention, the esterification reaction is carried out under heating in a water bath.

[0041] In some embodiments of the present invention, the starch and the esterifying agent are placed in a stirred reactor and heated to perform an esterification reaction to obtain esterified starch; during the esterification reaction, the stirred reactor is first stirred at a linear speed of 5.5-7.5 m / s, and when the real-time monitoring temperature in the stirred reactor reaches above 80°C, the linear speed is adjusted to 1.5-2.5 m / s; when the real-time monitoring temperature drops below 70°C, the stirring is continued at a linear speed of 5.5-7.5 m / s, and the cycle is repeated. By regulating the linear speed of the reaction stirrer, the stability of the esterification reaction is controlled to prevent the agglomeration of the material.

[0042] The temperature control during the esterification reaction is beneficial to avoid or reduce material agglomeration, thereby allowing the material to undergo a uniform esterification reaction and obtaining uniformly esterified starch.

[0043] In some embodiments of the present invention, the pre-carbonization temperature is 550-700°C, for example, 650-700°C.

[0044] In some embodiments of the present invention, the pre-carbonization time is 1-3 hours, for example, 2-3 hours.

[0045] In some embodiments of the present invention, the carbonization temperature is 1200-1500°C, for example, 1300-1400°C.

[0046] In some embodiments of the present invention, the carbonization time is 2-4 hours, for example, 2-3 hours.

[0047] In some embodiments of the present invention, the carbonization is performed under a protective gas atmosphere. The protective gas is, for example, nitrogen or a rare gas. The rare gas may be argon or helium.

[0048] In some embodiments of the present invention, a coating agent is added during the carbonization process, so that carbonization and coating can be performed simultaneously. In other embodiments of the present invention, after the carbonization is completed, the carbonized material is mixed with a coating agent and coated to obtain the starch-doped hard carbon material.

[0049] In the above embodiment, the coating agent includes coated asphalt, and the softening point of the coated asphalt is petroleum asphalt with a temperature of 220-280° C. The mass of the coating agent is 4-8% of the mass of the pre-carbonized material, for example, 4-5%, and more specifically, for example, 4%, 5%, or 8%.

[0050] In some embodiments of the present invention, when the coating treatment is performed after carbonization, the coating treatment temperature is 1200-1500° C. and the time is 1-3 hours.

[0051] A second aspect of the present invention provides a starch-based doped hard carbon material.

[0052] A starch-doped hard carbon material is prepared by the above preparation method.

[0053] A third aspect of the present invention provides an application of a starch-based doped hard carbon material.

[0054] A sodium ion battery comprises the above-mentioned starch-based doped hard carbon material.

[0055] The technical scheme and technical effects of the present application are described in detail below through specific embodiments and comparative examples. The following embodiments are only some embodiments of the present application and do not specifically limit the present application.

[0056] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.

[0057] Example 1: Preparation of starch-based hard carbon material

[0058] A method for preparing a starch-doped hard carbon material comprises the following steps:

[0059] (1) uniformly mixing an esterifying agent with corn starch to obtain a mixed material, wherein the mass of the esterifying agent is 15% of the mass of the corn starch, and the esterifying agent is composed of maleic anhydride and diammonium hydrogen phosphate in a mass ratio of 3:2;

[0060] (2) Under the condition of water bath heating, the mixed material is subjected to esterification reaction at 90° C. for 2 h to obtain esterified starch;

[0061] (3) pre-carbonizing the esterified starch at 700° C. for 2 h under a nitrogen atmosphere to obtain a pre-carbonized material;

[0062] (4) The pre-carbonized material is mixed with a coating agent (the coating agent is petroleum asphalt with a softening point of 250°C), the coating agent being 5% of the mass of the pre-carbonized material, and the mixture is heated to 1300°C for high-temperature carbonization treatment for 2 hours in a nitrogen atmosphere to obtain a starch-based doped hard carbon material.

[0063] Example 2: Preparation of starch-based hard carbon materials

[0064] A method for preparing a starch-doped hard carbon material comprises the following steps:

[0065] (1) uniformly mixing an esterifying agent and corn starch to obtain a mixed material, wherein the mass of the esterifying agent is 15% of the mass of the corn starch, and the esterifying agent is composed of succinic anhydride and sodium pyrophosphate in a mass ratio of 5:3;

[0066] (2) Under the condition of water bath heating, the mixed material is subjected to esterification reaction at 90° C. for 2 h to obtain esterified starch;

[0067] (3) pre-carbonizing the esterified starch at 700° C. for 2 h under a nitrogen atmosphere to obtain a pre-carbonized material;

[0068] (4) The pre-carbonized material is mixed with a coating agent (the coating agent is petroleum asphalt with a softening point of 250°C), the coating agent being 5% of the mass of the pre-carbonized material, and the mixture is heated to 1300°C for high-temperature carbonization treatment for 2 hours in a nitrogen atmosphere to obtain a starch-based doped hard carbon material.

[0069] Example 3: Preparation of starch-based hard carbon materials

[0070] A method for preparing a starch-doped hard carbon material comprises the following steps:

[0071] (1) uniformly mixing an esterifying agent with corn starch to obtain a mixed material, wherein the mass of the esterifying agent is 15% of the mass of the corn starch, and the esterifying agent is composed of acetic anhydride and calcium hydrogen phosphate in a mass ratio of 5:5;

[0072] (2) Under the condition of water bath heating, the mixed material is subjected to esterification reaction at 90° C. for 2 h to obtain esterified starch;

[0073] (3) pre-carbonizing the esterified starch at 700° C. for 2 h under a nitrogen atmosphere to obtain a pre-carbonized material;

[0074] (4) The pre-carbonized material is mixed with a coating agent (the coating agent is petroleum asphalt with a softening point of 250°C), the coating agent being 5% of the mass of the pre-carbonized material, and the mixture is heated to 1300°C for high-temperature carbonization treatment for 2 hours in a nitrogen atmosphere to obtain a starch-based doped hard carbon material.

[0075] Example 4

[0076] Step (3) and step (4) of Example 4 are the same as those of Example 1. The only difference between Example 4 and Example 1 is step (1) and step (2). The specific contents of step (1) and step (2) of Example 4 are as follows:

[0077] The esterification agent and corn starch are placed in a stirred reactor and heated to carry out an esterification reaction for 2 hours to obtain esterified starch; during the esterification reaction, the stirred reactor is first stirred at a linear speed of 6.5 m / s, and when the real-time monitoring temperature in the stirred reactor reaches above 80°C, the linear speed is adjusted to 2.0 m / s; when the real-time monitoring temperature drops below 70°C, the stirring is continued at a linear speed of 6.5 m / s, and this cycle is repeated;

[0078] The mass of the esterifying agent is 15% of the mass of the corn starch, and the esterifying agent is composed of maleic anhydride and diammonium hydrogen phosphate in a mass ratio of 3:2.

[0079] Example 5

[0080] Compared with Example 1, the only difference in Example 5 is that no coating agent is added in step (4), and the rest of the process is the same as Example 1.

[0081] Example 6

[0082] A method for preparing a starch-doped hard carbon material comprises the following steps:

[0083] (1) uniformly mixing an esterifying agent with corn starch to obtain a mixed material, wherein the mass of the esterifying agent is 15% of the mass of the corn starch, and the esterifying agent is composed of maleic anhydride and diammonium hydrogen phosphate in a mass ratio of 3:2;

[0084] (2) Under the condition of water bath heating, the mixed material is subjected to esterification reaction at 90° C. for 2 h to obtain esterified starch;

[0085] (3) pre-carbonizing the esterified starch at 700° C. for 2 h under a nitrogen atmosphere to obtain a pre-carbonized material;

[0086] (4) The pre-carbonized material is heated to 1300° C. for high-temperature carbonization treatment for 2 h in a nitrogen atmosphere to obtain a carbonized material;

[0087] (5) The carbonized material is mixed with a coating agent (the coating agent is petroleum asphalt with a softening point of 250°C), the coating agent is 5% of the mass of the pre-carbonized material, and the temperature is raised to 1300°C under a nitrogen atmosphere for high-temperature coating treatment for 2 hours to obtain a starch-based doped hard carbon material.

[0088] Example 7

[0089] Compared with Example 1, the only difference in Example 7 is that the mass of the esterification agent in step (1) is 6% of the mass of the corn starch, and the rest of the process is the same as Example 1.

[0090] Comparative Example 1

[0091] Compared with Example 1, the difference of Comparative Example 1 is that an equal amount of maleic anhydride is used in the esterification agent instead of diammonium hydrogen phosphate, and the rest of the process is the same as Example 1.

[0092] Comparative Example 2

[0093] Compared with Example 1, the difference of Comparative Example 2 is that an equal amount of diammonium hydrogen phosphate is used in the esterification agent instead of maleic anhydride, and the rest of the process is the same as Example 1.

[0094] Product effect testing

[0095] The starch-doped hard carbon material prepared in the above Examples 1-7 and the starch-doped hard carbon material prepared in Comparative Examples 1-2 were mixed with conductive carbon Super-P and PVDF (polyvinylidene fluoride) in a mass ratio of 92:3:3, and then N-methylpyrrolidone (NMP) was used as a solvent. After uniform mixing, the mixture was coated on aluminum foil and dried in a vacuum oven at 102°C. After rolling, the electrode was cut into a circular electrode sheet with a diameter of 8 mm, with a sodium sheet as the negative electrode, an electrolyte of NaPF6 lipid electrolyte of model NP-001, and a diaphragm of glass fiber. The button cell was assembled in a glove box filled with argon. The charge and discharge performance of the prepared sodium ion battery was tested. The battery test adopted the Xinwei battery testing system. The test method adopted constant current and constant voltage discharge and constant current charging. The charge and discharge test was carried out at a current density of 0.1C, the discharge cut-off voltage was 0V, and the charge cut-off voltage was 2.5V. The results are shown below (charge and discharge efficiency = charge specific capacity / discharge specific capacity*100%).

[0096] Table 1

[0097] Charge specific capacity (mAh / g) Discharge specific capacity (mAh / g) Charge and discharge efficiency (%) Example 1 324.40 376.29 86.21 Example 2 323.01 371.14 87.03 Example 3 323.00 367.34 87.93 Example 4 331.90 383.38 86.57 Example 5 317.91 365.41 87.00 Example 6 326.31 378.97 86.10 Example 7 312.94 372.85 83.93 Comparative Example 1 302.41 349.43 86.54 Comparative Example 2 251.53 303.34 82.92

[0098] As can be seen from Table 1, the button cell assembled from the starch-doped hard carbon material prepared in the embodiment of the present invention has a higher specific charge and discharge capacity. Compared with Example 1, in Comparative Example 1-2, maleic anhydride and diammonium hydrogen phosphate were not used simultaneously, resulting in a significant decrease in the electrochemical performance of the hard carbon material, indicating that in the present invention, the esterification agent including both phosphate and anhydride helps to significantly improve the electrochemical performance of the hard carbon material.

[0099] Figure 1 The charge and discharge curves of button batteries assembled from starch-doped hard carbon materials of Example 1 and Example 4 and starch-doped hard carbon materials of Comparative Examples 1-2; Figure 1 It can be seen that the specific capacity of Example 1 and Example 4 is significantly improved compared with Comparative Examples 1-2.

[0100] Figure 2 The starch-doped hard carbon material of Example 1 and the starch-doped hard carbon material of Comparative Examples 1-2 are shown in FIG. Figure 2 (Figure "a" in Figure 2 corresponds to the starch-based doped hard carbon material of Example 1, Figure "b" corresponds to the starch-based hard carbon material of Comparative Example 1, and Figure "c" corresponds to the starch-based hard carbon material of Comparative Example 2) It can be seen that the starch-based doped hard carbon material prepared in Example 1 did not undergo volume expansion, while the starch-based hard carbon material prepared in Comparative Examples 1-2 had significant volume expansion. This indicates that the esterification agent of the present invention has a significant effect of inhibiting the volume expansion during the preparation of hard carbon materials.

Claims

1. A method for preparing a starch-doped hard carbon material, characterized in that: The following steps are involved: Mixing starch with an esterifying agent and performing an esterification reaction to obtain esterified starch; Pre-carbonizing the esterified starch to obtain a pre-carbonized material; Carbonizing the pre-carbonized material to obtain the starch-based doped hard carbon material; Wherein, the esterification agent includes phosphate and acid anhydride.

2. The preparation method according to claim 1, characterized in that: The phosphate is selected from at least one of diammonium hydrogen phosphate, ammonium dihydrogen phosphate, calcium hydrogen phosphate, potassium dihydrogen phosphate, dipotassium hydrogen phosphate, sodium acid pyrophosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium phosphate, and sodium pyrophosphate; And / or, the acid anhydride is selected from at least one of acetic anhydride, maleic anhydride, phthalic anhydride, boric anhydride, butyric anhydride and succinic anhydride; And / or, before mixing the starch with the esterifying agent, the starch is dried first.

3. The preparation method according to claim 2, characterized in that: The starch is dried at a temperature of 110-150°C; And / or, the starch is dried for 4-14 hours; And / or, the starch is at least one of corn starch, potato starch, wheat starch, sweet potato starch, mung bean starch and tapioca starch; And / or, the temperature of the esterification reaction is 65-100°C; And / or, the esterification reaction time is 2-6 hours.

4. The preparation method according to claim 1, characterized in that: The mass of the esterifying agent is 6-15% of the mass of the starch; and / or, in the esterifying agent, the mass ratio of phosphate to anhydride is (3-5):5; And / or, the esterification reaction is carried out under heating in a water bath.

5. The preparation method according to claim 1, characterized in that: The starch and the esterification agent are placed in a stirred reactor and heated to carry out an esterification reaction to obtain esterified starch; during the esterification reaction, the stirred reactor is first stirred at a linear speed of 5.5-7.5 m / s, and when the real-time monitoring temperature in the stirred reactor reaches above 80° C., the linear speed is adjusted to 1.5-2.5 m / s; when the real-time monitoring temperature drops below 70° C., the stirring is continued at a linear speed of 5.5-7.5 m / s, and this cycle is repeated.

6. The preparation method according to claim 1, characterized in that: The pre-carbonization temperature is 550-700°C; And / or, the pre-carbonization time is 1-3 hours; And / or, the pre-carbonization is carried out under a protective gas atmosphere, wherein the protective gas is one or more of nitrogen, argon or helium; And / or, the carbonization temperature is 1200-1500°C; And / or, the carbonization time is 2-4 hours; And / or, the carbonization is performed under a protective gas atmosphere, wherein the protective gas is one or more of nitrogen, argon or helium.

7. The preparation method according to claim 6, characterized in that: During the carbonization process, a coating agent is also added; Alternatively, after the carbonization is completed, the carbonized material is mixed with a coating agent and subjected to coating treatment to obtain the starch-based doped hard carbon material.

8. The preparation method according to claim 7, characterized in that: The coating agent includes coated asphalt, and the softening point of the coated asphalt is petroleum asphalt with a temperature of 220-280°C; And / or, the mass of the coating agent is 4%-8% of the mass of the pre-carbonized material; And / or, the coating treatment is carried out at a temperature of 1200-1500° C. and for a time of 1-3 hours.

9. A starch-doped hard carbon material, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 8.

10. A sodium ion battery, characterized in that: Including the starch-doped hard carbon material as described in claim 9.

Citation Information

Patent Citations

  • Preparation method of hard carbon-soft carbon-fast ion conductor composite material

    CN115520851A

  • Preparation method of starch-based hard carbon negative electrode material, negative electrode material and sodium ion battery

    CN115536002A

  • Hard carbon negative electrode material, preparation method thereof and secondary battery

    CN115838165A

  • Positive electrode active material composition, positive electrode plate, battery and electric device

    CN116868376A

  • Negative electrode material for sodium secondary battery, electrode for sodium secondary battery, and sodium secondary battery

    JP2013168241A

Cited By

  • Starch-based hard carbon and preparation method thereof, negative electrode plate, sodium ion battery and power-related equipment

    CN119683605A

  • Preparation method of sodium ion battery negative electrode material

    CN120504319A