All-solid-state lithium ion battery negative electrode material, preparation method, battery and application

By using phosphorus and carbon composite materials and sulfide solid electrolytes in all-solid-state lithium-ion batteries, the problem of insufficient battery conductivity is solved, and the battery performance with high cycle stability and high energy density is achieved, which is suitable for new energy applications.

CN119008922AInactive Publication Date: 2024-11-22CHINA UNIV OF PETROLEUM (EAST CHINA)

Patent Information

Application Number
CN202411278377.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing all-solid-state lithium-ion batteries have insufficient electronic conductivity and ion conductivity, resulting in energy density and safety that cannot meet the needs of new applications.

Method used

Phosphorus or phosphorus and carbon composite materials are used as negative electrode materials to prepare a uniform phosphorus-carbon composite structure through ball milling, combined with sulfide solid electrolyte, and use high voltage to promote lithiation fusion, reduce interface impedance, and improve conductivity.

Benefits of technology

The all-solid-state lithium-ion battery negative electrode material with high cycle stability and high energy density is suitable for green and environmentally friendly energy-saving vehicles and renewable energy storage systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008922A_ABST
    Figure CN119008922A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of all-solid-state lithium ion batteries, and discloses an all-solid-state lithium ion battery negative electrode material, a preparation method, a battery and application. The all-solid-state lithium ion battery negative electrode material is phosphorus or a phosphorus and carbon composite material. When the all-solid-state lithium ion battery negative electrode material is formed by compounding phosphorus and carbon, the carbon and phosphorus in the structure are uniformly mixed; the ratio of phosphorus to carbon is (5-9): (5-1). According to the invention, carbon and phosphorus are uniformly mixed through ball milling, graphite is utilized to make up for the defect of low electron conductivity of phosphorus, a conductive network structure is formed between phosphorus and graphite, and a solid electrolyte is combined, so that the battery has the characteristics of high electron conductivity and high ionic conductivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of all-solid-state lithium-ion batteries, and in particular relates to an all-solid-state lithium-ion battery negative electrode material, a preparation method, a battery and applications. Background Art

[0002] Conventional LIBs use organic liquid electrolytes (OLEs), which consist of lithium salts (e.g., lithium hexafluorophosphate (LiPF6)) dissolved in organic solvents (e.g., ethylene carbonate (EC) and dimethyl carbonate (DMC)). The high flammability of organic solvents (EC flash point 150°C and DMC flash point 18°C) presents a safety risk during battery operation. In addition, OLEs are depleted during charge / discharge cycles due to repeated breakdown and reformation of the solid electrolyte interphase (SEI) film. Therefore, conventional batteries with OLEs usually contain additional electrolytes to overcome depletion during extended cycles, which increases manufacturing costs. Based on the above limitations of OLEs, current LIB technology cannot meet the higher energy density and better safety required for existing and new applications. An ideal battery that meets these new demands would be made of a solid electrolyte (SSE), a lithium metal anode, and a high-voltage cathode, the so-called all-solid-state battery (ASSB). Most SSEs are non-flammable and have a wider operating temperature range, making them safer than liquid electrolytes in short-circuit situations. It is noteworthy that in ASSB, the battery structure model can be simplified by stacking the bipolar electrodes and solid electrolyte in alternating layers in a single battery shell, which reduces the number of battery shells required in liquid batteries.

[0003] Through the above analysis, the problems and defects of the existing technology are: the existing technology cannot make up for the low electronic conductivity of phosphorus, and the electronic conductivity and high ion conductivity of the battery prepared by the existing technology need to be improved. Summary of the invention

[0004] In order to overcome the problems existing in the related art, the embodiments disclosed in the present invention provide an all-solid-state lithium-ion battery negative electrode material, a preparation method, a battery and applications.

[0005] The technical solution is as follows: an all-solid-state lithium-ion battery negative electrode material, the material being phosphorus or a phosphorus-carbon composite material;

[0006] When the material is composed of phosphorus and carbon, the carbon and phosphorus are evenly mixed inside the structure; the phosphorus-carbon ratio is (5-9): (5-1);

[0007] When the material is composed of phosphorus, the phosphorus is one or more of black phosphorus, red phosphorus and white phosphorus.

[0008] Furthermore, the carbon is one or more of graphite, hard carbon, soft carbon, and porous carbon.

[0009] Another object of the present invention is to provide an all-solid-state lithium-ion battery, which is assembled from the all-solid-state lithium-ion battery negative electrode material, has a first-cycle reversible specific capacity of 617.59-2223.09 mAh / g, a first coulombic efficiency of 70.36-85.8%, and a capacity retention rate of 57.64-81.62% after 50 cycles.

[0010] Another object of the present invention is to provide a method for preparing an all-solid-state lithium-ion battery, the method being used to prepare the all-solid-state lithium-ion battery, the method comprising the following steps:

[0011] S1, preparation of negative electrode material: carbon and phosphorus are compounded by ball milling, and a phosphorus / carbon composite structure is formed by ball milling at a speed of 300-500r / min;

[0012] S2, negative electrode material pretreatment: coating the electrode material with conductive carbon black and a binder, and assembling the battery negative electrode sheet;

[0013] S3, adding the coated battery negative electrode sheet to the solid electrolyte, applying pressure, and pressing it into an all-solid-state lithium-ion battery.

[0014] In step S1, the negative electrode material is prepared, including: using red phosphorus as the negative electrode material.

[0015] In step S2, the electrode material, conductive carbon black and binder are coated on the copper foil in a ratio of (80-99): (10-0): (10-1).

[0016] In step S3, the solid electrolyte used is Li6PS5X (X = Cl, Br, I), Li 11-x M 2-x P 1+x S 12 (M=Ge, Sn, Si), LiPS and PVDF-based solid electrolytes, or one or more solid electrolytes.

[0017] In step S3, pressure is used to promote the contact between the negative electrode sheet of the battery and the electrolyte particles to increase the ion / electron conductivity, and the pressure applied to the battery is 10-100 MPa.

[0018] Another object of the present invention is to provide an application of an all-solid-state lithium-ion battery in a green, environmentally friendly and energy-saving vehicle, wherein the green, environmentally friendly and energy-saving vehicle in the application is equipped with the all-solid-state lithium-ion battery.

[0019] Another object of the present invention is to provide an application of an all-solid-state lithium-ion battery in a renewable energy energy storage system, wherein the all-solid-state lithium-ion battery is installed in the renewable energy energy storage system.

[0020] In combination with all the above technical solutions, the beneficial effects of the present invention are as follows: the all-solid-state lithium-ion battery provided by the present invention uses phosphorus, phosphorus and carbon composite materials, the negative electrode material is phosphorus or phosphorus and carbon are uniformly mixed with high conductivity carbon materials, the electrode material obtained by ball milling is uniformly mixed with carbon, and a conductive network structure is formed inside the material. The present invention prepares the negative electrode material by ball milling, the process is simple, the cost is low, and it is suitable for large-scale production.

[0021] The present invention applies phosphorus to an all-solid-state lithium-ion battery with sulfide as electrolyte. Phosphorus is compounded with graphite to modify the problem of poor electronic conductivity of phosphorus. The ball-milled phosphorus and carbon are evenly mixed to form a conductive network structure. The PC and POC formed after ball milling covalently stabilize the two-dimensional interface between the negative electrode material and the electrolyte particles. By utilizing the characteristics of "soft phosphorus", the all-solid-state lithium-ion battery forms Li3P under high pressure, better realizes the lithium fusion between particles, avoids the micro-sized voids generated by volume expansion during the de-lithiation process, and reduces the interface impedance. By utilizing the pressure applied to the battery, the volume expansion of the negative electrode material during the lithium insertion / de-lithiation process is suppressed to a certain extent. In combination with the sulfide solid electrolyte, the ion / electronic conductivity of the all-solid-state lithium-ion battery is improved, and the all-solid-state lithium-ion battery negative electrode material with high cycle stability is prepared. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The accompanying drawings herein are incorporated in and constitute a part of the specification, illustrate embodiments consistent with the present disclosure, and together with the description, serve to explain the principles of the present disclosure;

[0023] Figure 1 is a flow chart of a method for preparing an all-solid-state lithium-ion battery provided by an embodiment of the present invention;

[0024] Figure 2 It is a flow chart of a method for preparing an all-solid-state lithium-ion battery using sulfide as electrolyte provided by an embodiment of the present invention;

[0025] Figure 3 This is a flow chart of a method for preparing an all-solid-state lithium-ion battery using PVDF as a solid electrolyte provided by an embodiment of the present invention;

[0026] Figure 4 It is a scanned image of the all-solid-state lithium-ion battery negative electrode material provided by an embodiment of the present invention. DETAILED DESCRIPTION

[0027] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific implementation disclosed below.

[0028] The innovation of the present invention is that phosphorus is applied to all-solid-state lithium-ion batteries with sulfide as electrolyte. Phosphorus is compounded with graphite to modify the problem of poor electronic conductivity of phosphorus. The ball-milled phosphorus and carbon are evenly mixed to form a conductive network structure. The PC and POC formed after ball milling covalently stabilize the two-dimensional interface between the negative electrode material and the electrolyte particles. By utilizing the characteristics of "soft phosphorus", the all-solid-state lithium-ion battery forms Li3P under high pressure, better realizes the lithium fusion between particles, avoids the micro-sized voids caused by volume expansion during the delithiation process, and reduces the interface impedance. Combined with sulfide solid electrolyte, the ion / electronic conductivity of the all-solid-state lithium-ion battery is improved, and the all-solid-state lithium-ion battery negative electrode material with high cycle stability is prepared.

[0029] The present invention utilizes the advantages of high conductivity and adjustable pressure of all-solid-state lithium-ion batteries; the negative electrode material is ball-milled to uniformly mix carbon and phosphorus, and graphite is used to make up for the low electronic conductivity of phosphorus, forming a conductive network structure between phosphorus and graphite, and combined with a solid electrolyte, so that the battery has the characteristics of high electronic conductivity and high ionic conductivity.

[0030] Embodiment 1: The present invention provides a negative electrode material for an all-solid-state lithium-ion battery, wherein the negative electrode material is phosphorus or a phosphorus and carbon composite material.

[0031] When the material is composed of phosphorus and carbon, the carbon and phosphorus are evenly mixed inside the structure; the phosphorus-carbon ratio is (5-9): (5-1);

[0032] When the material is composed of phosphorus, the phosphorus is one or more of black phosphorus, red phosphorus and white phosphorus.

[0033] The carbon is one or more of graphite, hard carbon, soft carbon and porous carbon.

[0034] As a preferred embodiment, the negative electrode material is composed of a composite of phosphorus and carbon, and the carbon and phosphorus are evenly mixed inside the structure.

[0035] The phosphorus-carbon ratio of the all-solid-state lithium-ion battery negative electrode material is (5-9): (5-1).

[0036] The phosphorus is one or more of black phosphorus, red phosphorus and white phosphorus.

[0037] The carbon is one or more of graphite, hard carbon, soft carbon and porous carbon.

[0038] As another preferred method, an all-solid-state lithium-ion battery is prepared by using an all-solid-state lithium-ion battery negative electrode material.

[0039] like Figure 1 As shown, the preparation method of the all-solid-state lithium-ion battery comprises the following steps:

[0040] S1, preparation of negative electrode material: carbon and phosphorus are compounded by ball milling, and a phosphorus / carbon composite structure is formed by ball milling at a speed of 300-500r / min;

[0041] S2, negative electrode material pretreatment: coating the electrode material with conductive carbon black and a binder, and assembling the battery negative electrode sheet;

[0042] S3, adding the coated battery negative electrode sheet to the solid electrolyte, applying pressure, and pressing it into an all-solid-state lithium-ion battery.

[0043] The solid electrolyte used is Li6PS5X (X = Cl, Br, I), Li 11-x M 2-x P 1+x S 12 (M=Ge, Sn, Si), LiPS and PVDF based solid electrolytes. The selected Li6PS5X (X=Cl, Br, I) has the characteristics of high conductivity, good thermal stability and wide voltage window.

[0044] Pressure is used to promote contact between the negative electrode sheet of the battery and the electrolyte particles, increase ion / electron conductivity, and the pressure applied to the battery is 10-100MPa.

[0045] As another preferred method, taking sulfide solid electrolyte as an example, Figure 2 As shown, a solid-state lithium-ion battery using sulfide as electrolyte is prepared, and the preparation method includes:

[0046] S201, preparation of negative electrode material: carbon and phosphorus are compounded by ball milling, and a phosphorus / carbon composite structure is formed by ball milling at a high speed of 300-500r / min;

[0047] S202, pretreatment of negative electrode materials: coating the electrode materials with conductive carbon black and a binder, and assembling a negative electrode sheet of the battery;

[0048] S203, battery assembly: The coated battery negative electrode sheet is loaded into a polyetherketone mold, a sulfide solid electrolyte is added, pressure is applied, and it is pressed into a solid electrolyte membrane. Then, the negative electrode sheet is pressed on one side of the electrolyte membrane, and a piece of In-Li foil is stacked on the other side. Using stainless steel plugs as current collectors on both sides, pressure is applied on the two stainless steel plug molds to make the stainless steel plugs in close contact with the electrode negative electrode material. Finally, additional pressure is applied to the battery and maintained by a stainless steel frame, and finally an all-solid-state lithium-ion battery with sulfide as the electrolyte is obtained.

[0049] As another preferred method, taking PVDF-based solid electrolyte as an example, Figure 3 As shown, a fully solid-state lithium-ion battery with a PVDF-based solid electrolyte is prepared, and the preparation method includes:

[0050] S301, preparation of negative electrode material: carbon and phosphorus are compounded by ball milling, and a phosphorus / carbon composite structure is formed by ball milling at a high speed of 300-500r / min;

[0051] S302, pretreatment of negative electrode materials: coating the electrode materials with conductive carbon black and a binder, and assembling the negative electrode sheet of the battery;

[0052] S303, battery assembly: placing the coated battery negative electrode sheet into the negative electrode side of the battery, and sequentially adding PVDF-based solid electrolyte membrane, lithium sheet, gasket, spring, and positive electrode shell to apply pressure to seal.

[0053] Example 2, as another embodiment of the present invention, the present invention provides an all-solid-state lithium-ion battery negative electrode material, wherein the negative electrode material is a high-conductivity carbon material in which carbon and phosphorus are evenly mixed, wherein the phosphorus is mainly one or more of red phosphorus, black phosphorus, and white phosphorus; and the carbon is one or more of graphite, hard carbon, soft carbon, and porous carbon.

[0054] Specifically, the negative electrode material forms a conductive network structure between phosphorus and carbon through ball milling to make up for the low conductivity of phosphorus. At the same time, PC and POC covalent bonds are formed between phosphorus and carbon through ball milling to stabilize the two-dimensional interface between the negative electrode material and the solid electrolyte.

[0055] Example 3: The present invention applies single phosphorus to an all-solid-state lithium-ion battery using sulfide as electrolyte.

[0056] Specifically, one or more of red phosphorus, black phosphorus, and white phosphorus are used in all-solid-state lithium-ion batteries. Compared with silicon, phosphorus has lower hardness and modulus, and is softer. During the delithiation process, the electrolyte-free silicon negative electrode produces micro-sized voids due to volume expansion. Phosphorus is relatively "soft" and can be well lithium-fused with electrolyte particles during the cycle process under high pressure, avoiding micro-sized voids caused by volume expansion during the delithiation process, and reducing the electrochemical reaction impedance of the "solid-solid" contact between the electrode material and the electrolyte in the all-solid-state lithium-ion battery. Graphite and phosphorus are used to increase electronic conductivity, establish a conductive network structure inside the electrode material, make up for the low electronic conductivity of phosphorus, and improve the battery cycle stability.

[0057] The present invention uses ball milling to compound phosphorus and carbon, and modifies the phosphorus negative electrode to form a two-dimensional interface between the PC and POC covalent bonds to stabilize the negative electrode material and the electrolyte particles. At the same time, after ball milling, phosphorus and carbon are mixed to form a conductive network structure, and carbon is used to make up for the disadvantage of low electronic conductivity of phosphorus and increase the electronic conductivity of the negative electrode material; high voltage is used to suppress the volume expansion of phosphorus during the cycle; solid electrolytes are used to enhance the ion conductivity of the material; using the characteristics of "soft phosphorus", the all-solid-state lithium-ion battery forms Li3P under high pressure, better realizes the lithium fusion between particles, avoids the micro-sized voids generated by volume expansion during the de-lithiation process, reduces the interface impedance, and enhances the reaction kinetics. By applying a certain pressure to the battery, the high electrochemical reaction impedance caused by the "solid-solid" contact between the electrode material and the electrolyte in the all-solid-state lithium-ion battery is reduced.

[0058] The present invention is further described below with experimental methods.

[0059] Experimental methods: The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, etc. used in the following examples are all commercially available unless otherwise specified.

[0060] Microscopic morphology test: Scanning electron microscope images were obtained using a German Zeiss Gemini 500 scanning electron microscope;

[0061] Electrical performance test: The present invention conducted multiple performance tests such as half-cell reversible capacity and first efficiency on the all-solid-state lithium-ion battery negative electrode materials prepared in the above-mentioned embodiments and comparative examples.

[0062] Test method: The electrochemical performance test was performed using a LAND CT2001 A tester (LAND Electronics Co., Ltd., Wuhan City). The test cycle was set to 50 cycles. Specifically, the voltage range was -0.61-1.828 V (the comparison was -0.61-0.88) and the current was 0.1 mA / cm 2The first cycle reversible capacity (mAh / g) and first coulombic efficiency were tested at a current density of 0.5 mA / cm 2 The cycle was performed at a current density of .

[0063] Experimental example 1.

[0064] like Figure 4 As shown, this experimental example 1 provides an all-solid-state lithium-ion battery, specifically:

[0065] Material preparation: graphite and phosphorus are compounded by ball milling in a ratio of 5:5, and a phosphorus / graphite composite structure is formed by ball milling at a rotation speed of 400 r / min; wherein the phosphorus is a mixture of one or more of red phosphorus, white phosphorus, and black phosphorus;

[0066] Material pretreatment: coating the prepared electrode material and binder on copper foil in a ratio of 99:1;

[0067] Battery assembly: Place the coated electrode sheet into a polyetherketone mold, add the sulfide solid electrolyte Li6PS5Cl, apply 4t pressure to press it into a solid electrolyte membrane and make the electrode material in close contact with the solid electrolyte, and use 2t pressure to press a piece of In-Li foil on the other side. Use stainless steel plugs as current collectors on both sides, and apply pressure on the two stainless steel plug molds to make the stainless steel plugs in close contact with the electrode material. Finally, apply an additional 100MPa of pressure to the battery and maintain it with a stainless steel frame. After the first cycle of charge and discharge testing, the first efficiency was 70.36%, the first cycle reversible specific capacity was 617.59mAh / g, and the capacity retention rate was 74.32% after 50 cycles.

[0068] Experimental example 2.

[0069] Material preparation: Graphite and phosphorus are compounded by ball milling in a ratio of 4:6, and a phosphorus / graphite composite structure is formed by ball milling at a rotation speed of 400 r / min; wherein the phosphorus is a mixture of one or more of red phosphorus, white phosphorus, and black phosphorus;

[0070] Material pretreatment: coating the prepared electrode material and binder on copper foil in a ratio of 99:1;

[0071] Battery assembly: Place the coated electrode sheet into a polyetherketone mold, add the sulfide solid electrolyte Li6PS5Cl, apply 4t pressure to press it into a solid electrolyte membrane and make the electrode material in close contact with the solid electrolyte, and use 2t pressure to press a piece of In-Li foil on the other side. Use stainless steel plugs as current collectors on both sides, and apply pressure on the two stainless steel plug molds to make the stainless steel plugs in close contact with the electrode material. Finally, apply an additional 100MPa of pressure to the battery and maintain it with a stainless steel frame. After the first cycle of charge and discharge testing, the first efficiency was 76.17%, the first cycle reversible specific capacity was 944.6mAh / g, and the capacity retention rate was 78.46% after 50 cycles.

[0072] Experimental example 3.

[0073] Material preparation: graphite and phosphorus are compounded by ball milling in a ratio of 3:7, and a phosphorus / graphite composite structure is formed by ball milling at a rotation speed of 400 r / min; wherein the phosphorus is a mixture of one or more of red phosphorus, white phosphorus, and black phosphorus;

[0074] Material pretreatment: coating the prepared electrode material and binder on copper foil in a ratio of 99:1;

[0075] Battery assembly: Place the coated electrode sheet into a polyetherketone mold, add the sulfide solid electrolyte Li6PS5Cl, apply 4t pressure to press it into a solid electrolyte membrane and make the electrode material in close contact with the solid electrolyte, and use 2t pressure to press a piece of In-Li foil on the other side. Use stainless steel plugs as current collectors on both sides, and apply pressure on the two stainless steel plug molds to make the stainless steel plugs in close contact with the electrode material. Finally, apply an additional 100MPa of pressure to the battery and maintain it with a stainless steel frame. After the first cycle of charge and discharge testing, the first efficiency was 85.33%, the first cycle reversible specific capacity was 1443.01mAh / g, and the capacity retention rate was 81.62% after 50 cycles of testing.

[0076] Experimental example 4.

[0077] Material preparation: graphite and phosphorus are compounded by ball milling in a ratio of 2:8, and a phosphorus / graphite composite structure is formed by ball milling at a rotation speed of 400 r / min; wherein the phosphorus is a mixture of one or more of red phosphorus, white phosphorus, and black phosphorus;

[0078] Material pretreatment: coating the prepared electrode material and binder on copper foil in a ratio of 99:1;

[0079] Battery assembly: Place the coated electrode sheet into a polyetherketone mold, add the sulfide solid electrolyte Li6PS5Cl, apply 4t pressure to press it into a solid electrolyte membrane and make the electrode material in close contact with the solid electrolyte, and use 2t pressure to press a piece of In-Li foil on the other side. Use stainless steel plugs as current collectors on both sides, and apply pressure on the two stainless steel plug molds to make the stainless steel plugs in close contact with the electrode material. Finally, apply an additional 100MPa of pressure to the battery and maintain it with a stainless steel frame. After the first cycle of charge and discharge testing, the first efficiency was 84.37%, the first cycle reversible specific capacity was 1532.89mAh / g, and the capacity retention rate was 76.47% after 50 cycles of testing.

[0080] Experimental example 5.

[0081] Material preparation: graphite and phosphorus are compounded by ball milling in a ratio of 1:9, and a phosphorus / graphite composite structure is formed by ball milling at a rotation speed of 400 r / min; wherein the phosphorus is a mixture of one or more of red phosphorus, white phosphorus, and black phosphorus;

[0082] Material pretreatment: coating the prepared electrode material and binder on copper foil in a ratio of 99:1;

[0083] Battery assembly: Place the coated electrode sheet into a polyetherketone mold, add the sulfide solid electrolyte Li6PS5Cl, apply 4t pressure to press it into a solid electrolyte membrane and make the electrode material in close contact with the solid electrolyte, and use 2t pressure to press a piece of In-Li foil on the other side. Use stainless steel plugs as current collectors on both sides, and apply pressure on the two stainless steel plug molds to make the stainless steel plugs in close contact with the electrode material. Finally, an additional 100MPa of pressure is applied to the battery and maintained by a stainless steel frame. After the first cycle of charge and discharge testing, the first efficiency is 85.43%, the first cycle reversible specific capacity is 1839.8mAh / g, and the capacity retention rate after 50 cycles is 70.82%.

[0084] Experimental example 6.

[0085] Material preparation: Red phosphorus is used as the negative electrode material;

[0086] Material pretreatment: phosphorus, conductive carbon black and binder are coated on copper foil in a ratio of 80:10:10;

[0087] Battery assembly: Place the coated electrode sheet into a polyetherketone mold, add the sulfide solid electrolyte Li6PS5Cl, apply 4t pressure to press it into a solid electrolyte membrane and make the electrode material in close contact with the solid electrolyte, and use 2t pressure to press a piece of In-Li foil on the other side. Use stainless steel plugs as current collectors on both sides, and the pressure applied by the two stainless steel plug molds makes the stainless steel plugs in close contact with the electrode material. Finally, apply additional pressure to the battery and maintain it with a stainless steel frame. After the first cycle of charge and discharge testing, the first efficiency was 85.8%, the first cycle reversible specific capacity was 2223.09mAh / g, and the capacity retention rate after 50 cycles was 57.64%.

[0088] Comparative example 1.

[0089] Comparative Example 1 is a silicon-based lithium-ion battery negative electrode material using micron silicon as the negative electrode.

[0090] Material preparation: Use micron silicon as negative electrode material;

[0091] Material pretreatment: Micron silicon and adhesive are coated on copper foil in a ratio of 99:1;

[0092] Battery assembly: Place the coated electrode sheet into a polyetherketone mold, add the sulfide solid electrolyte Li6PS5Cl, apply 4t pressure to press it into a solid electrolyte membrane and make the electrode material in close contact with the solid electrolyte, and use 2t pressure to press a piece of In-Li foil on the other side. Use stainless steel plugs as current collectors on both sides, and apply pressure on the two stainless steel plug molds to make the stainless steel plugs in close contact with the electrode material. Finally, apply an additional 100MPa of pressure to the battery and maintain it with a stainless steel frame. After the first cycle of charge and discharge testing, the first efficiency was 76.47%, the first cycle reversible specific capacity was 2151.32mAh / g, and the capacity retention rate was 44.01% after 50 cycles.

[0093] The electrochemical performance test results are summarized in Table 1 below: In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not detailed or recorded in a certain embodiment, please refer to the relevant description of other embodiments.

[0094] Table 1 Electrochemical performance test results

[0095]

[0096]

[0097] This all-solid-state lithium-ion battery uses phosphorus as the main negative electrode material, and is composited with one or more of graphite, hard carbon, soft carbon, and porous carbon. It has a high energy density and can provide stable energy output during use. It is suitable for energy storage systems of renewable energy sources such as solar energy and wind energy. With the widespread application of renewable energy, the demand for solid-state batteries in energy storage systems will gradually increase. Studies have shown that during the charge and discharge process of the silicon negative electrode, tiny voids appear between the electrolyte particles and the negative electrode material due to volume expansion, while phosphorus is "softer" and undergoes plastic deformation and volume expansion during the charge and discharge process, avoiding the formation of such tiny voids. Phosphorus is applied to all-solid-state lithium-ion batteries, and the "softer" mechanical properties of phosphorus are utilized to avoid the problem of tiny-sized voids caused by volume expansion during the charge and discharge cycle of silicon negative electrode all-solid-state lithium-ion batteries, reduce interface impedance, and promote interface ion and electron transmission.

[0098] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principles of the present invention should be covered within the protection scope of the present invention.

Claims

1. An all-solid-state lithium-ion battery negative electrode material, characterized in that: The material is phosphorus or a composite material of phosphorus and carbon; When the material is composed of phosphorus and carbon, the carbon and phosphorus are evenly mixed inside the structure; the phosphorus-carbon ratio is (5-9): (5-1); When the material is composed of phosphorus, the phosphorus is one or more of black phosphorus, red phosphorus and white phosphorus.

2. The all-solid-state lithium-ion battery negative electrode material according to claim 1, characterized in that: The carbon is one or more of graphite, hard carbon, soft carbon and porous carbon.

3. An all-solid-state lithium-ion battery, characterized in that: The battery is assembled from the all-solid-state lithium-ion battery negative electrode material according to any one of claims 1 to 2, has a first-cycle reversible specific capacity of 617.59-2223.09 mAh / g, a first coulombic efficiency of 70.36-85.8%, and a capacity retention rate of 57.64-81.62% after 50 cycles.

4. A method for preparing an all-solid-state lithium-ion battery, characterized in that: The preparation method is used to prepare the all-solid-state lithium-ion battery according to claim 3, and the method comprises the following steps: S1, preparation of negative electrode material: carbon and phosphorus are compounded by ball milling, and a phosphorus / carbon composite structure is formed by ball milling at a speed of 300-500r / min; S2, negative electrode material pretreatment: coating the electrode material with conductive carbon black and a binder, and assembling the battery negative electrode sheet; S3, adding the coated battery negative electrode sheet to the solid electrolyte, applying pressure, and pressing it into an all-solid-state lithium-ion battery.

5. The method for preparing an all-solid-state lithium-ion battery according to claim 4, characterized in that: In step S1, the negative electrode material is prepared, including: using red phosphorus as the negative electrode material.

6. The method for preparing an all-solid-state lithium-ion battery according to claim 4, characterized in that: In step S2, the electrode material, conductive carbon black and binder are coated on the copper foil in a ratio of (80-99): (10-0): (10-1).

7. The method for preparing an all-solid-state lithium-ion battery according to claim 4, characterized in that: In step S3, the solid electrolyte used is Li6PS5X (X = Cl, Br, I), Li 11-x M 2-x P 1+x S 12 (M=Ge, Sn, Si), LiPS and PVDF-based solid electrolytes, or one or more solid electrolytes.

8. The method for preparing an all-solid-state lithium-ion battery according to claim 4, characterized in that: In step S3, pressure is used to promote the contact between the negative electrode sheet of the battery and the electrolyte particles to increase the ion / electron conductivity, and the pressure applied to the battery is 10-100 MPa.

9. An application of an all-solid-state lithium-ion battery in a green, environmentally friendly and energy-saving vehicle, characterized in that: The green, environmentally friendly and energy-saving vehicle in this application is equipped with the all-solid-state lithium-ion battery described in claim 3.

10. An application of an all-solid-state lithium-ion battery in a renewable energy storage system, characterized in that: The all-solid-state lithium-ion battery according to claim 3 is installed in the renewable energy storage system.

Citation Information

Patent Citations

  • Phosphorus / carbon composite negative electrode material of lithium ion battery and preparation method thereof

    CN101604752A

  • Synthesis of solid-state lithium battery as well as preparation methods of graphite composite negative plate and LiFePO4 composite positive plate

    CN108232120A

  • Anode material and method for producing the same

    CN112563477A

  • High-energy-density negative electrode material, preparation method and application thereof

    CN114335466A

  • Preparation method of silver phosphide-carbon material compound and solid-state lithium ion battery containing silver phosphide-carbon material compound

    CN114361459A

Cited By

  • Phosphorus-based negative electrode material and preparation method and application thereof

    CN120674484A