aminosilsesquioxane
Aminosilsesquioxanes with amino groups and silsesquioxane structures address the low film formation rates and high-temperature requirements of conventional methods, enabling high-speed, high-quality silicon-containing film formation for semiconductor devices.
Patent Information
- Application Number
- JP2023043322
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-17
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional methods for forming silicon-containing films require high temperatures and have low film formation rates, limiting productivity in semiconductor device fabrication.
The use of aminosilsesquioxanes with specific cage-like structures as silicon precursors, particularly those with amino groups and silsesquioxane structures, allows for high deposition rates at low temperatures.
Aminosilsesquioxanes enable the formation of high-quality silicon-containing films at increased speeds and improved productivity, suitable for semiconductor devices.
Smart Images

Figure 2024132524000026 
Figure 2024132524000001 
Figure 2024132524000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to aminosilsesquioxanes, particularly aminosilsesquioxanes that are useful in forming silicon-containing films. [Background technology]
[0002] In the fabrication of semiconductor devices, silicon-containing thin films are fabricated into various forms of thin films, such as silicon films, silicon oxide films, silicon carbonitride films, and silicon oxynitride films, through various deposition processes, and are applied in various fields. Among them, silicon oxide films and silicon nitride films have excellent barrier properties and oxidation resistance, and therefore function as insulating films, intermetal dielectric materials, seed layers, spacers, hard masks, trench isolation, diffusion barriers, etch stop layers, and passivation layers in device fabrication.
[0003] In recent years, with the miniaturization of elements, the increase in aspect ratio, and the diversification of element materials, there is a demand for technology to deposit ultra-fine thin films with excellent electrical properties at low temperatures and high speeds. However, conventional deposition methods using silicon precursors require high deposition temperatures of 600°C or higher, and the deposition speed is slow, resulting in a decrease in productivity.
[0004] To solve this problem, Patent Document 1 proposes a method for forming a uniform silicon oxide film at a low temperature of less than 400°C by using bisdiethylaminosilane (BDEAS), an aminosilane compound, as a silicon source in an atomic layer deposition process. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 5329218 Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present disclosure is to provide a novel silicon precursor capable of forming a silicon-containing film at a low temperature and at a high film formation rate. [Means for solving the problem]
[0007] As a result of extensive investigations, the present inventors have found that the amino group (-N-R2, where R is an alkyl group) and the silsesquioxane structure (Si(-O-) 1.5 It has been found that the use of aminosilsesquioxanes having a specific cage structure as a silicon precursor can improve the film formation rate. In particular, it has been found that the use of aminosilsesquioxanes having a specific cage structure as a silicon precursor can improve the film formation rate, and this has led to the completion of the present disclosure.
[0008] An example of an embodiment of the present disclosure is as follows. [Section 1] Below formula (1): TIFF2024132524000001.tif41150[In formula (1), R 1 ~R 8 Six of these are hydrogen atoms. R 1 ~R 8 Each of the two is independently NR 9 R 10 is an amino group represented by R 9 and R 10 each independently represents an alkyl group having 1 to 4 carbon atoms.] The aminosilsesquioxane represented by the formula: [Section 2] Below formula (2): TIFF2024132524000002.tif51150 represents 1,3-bis(diethylamino)-pentacyclo[9.5.1.1 3,9 .1 5,15 .1 7,13 ]Octasiloxane, Below formula (3): TIFF2024132524000003.tif51150 represents 1,5-bis(diethylamino)-pentacyclo[9.5.1.13,9 .1 5,15 .1 7,13 ]octasiloxane, and Formula (4) below: TIFF2024132524000004.tif51150 represents 1,7-bis(diethylamino)-pentacyclo[9.5.1.1 3,9 .1 5,15 .1 7,13 Item 2. The aminosilsesquioxane according to item 1, which is at least one selected from the group consisting of octasiloxanes. [Section 3] Item 3. The aminosilsesquioxane according to item 1 or 2, wherein the aminosilsesquioxane is an isomeric mixture containing two or more isomeric structures. [Section 4] Item 4. A precursor of a silicon-containing film, comprising the aminosilsesquioxane according to any one of items 1 to 3. [Section 5] Item 5. The precursor according to item 4, wherein the silicon-containing film is formed by chemical vapor deposition. [Section 6] Item 6. The precursor according to item 4 or 5, wherein the silicon-containing film is formed by atomic layer deposition. [Section 7] Item 4. A composition for forming a silicon-containing film, comprising the aminosilsesquioxane according to any one of items 1 to 3. [Section 8] Item 8. The composition according to item 7, wherein the silicon-containing film is formed by chemical vapor deposition. [Section 9] Item 9. The composition according to item 7 or 8, wherein the silicon-containing film is formed by atomic layer deposition. [Section 10] Below formula (1) TIFF2024132524000005.tif41150[In formula (1), R 1 ~R 8 Six of these are hydrogen atoms. R 1 ~R 8 Each of the two is independently NR 9 R 10 is an amino group represented by R9 and R 10 each independently represents an alkyl group having 1 to 4 carbon atoms.] A method for producing an aminosilsesquioxane represented by the formula: (a) a synthesis step comprising reacting a starting silsesquioxane with a secondary amine to synthesize the aminosilsesquioxane; and (b) A purification step including distillation and / or sublimation. A method for producing aminosilsesquioxane, comprising: [Section 11] The secondary amine is represented by the following formula (5-2): HNR 9 R 10 (5-2) [In formula (5-2), R 9 and R 10 each independently represents an alkyl group having 1 to 4 carbon atoms.] Item 11. The method for producing an aminosilsesquioxane according to item 10, represented by the formula: [Section 12] Below formula (1): TIFF2024132524000006.tif41150[In formula (1), R 1 ~R 8 Six of these are hydrogen atoms. R 1 ~R 8 Each of the two is independently NR 9 R 10 is an amino group represented by R 9 and R 10 each independently represents an alkyl group having 1 to 4 carbon atoms.] The present invention relates to a method for producing a silicon-containing film, and more particularly to an aminosilsesquioxane represented by the formula: Effect of the Invention
[0009] The aminosilsesquioxanes disclosed herein can be used as silicon precursors with high film formation rates at low temperatures, thereby improving the productivity of silicon-containing films such as silicon oxide films. [Brief description of the drawings]
[0010] [Figure 1] The H-NMR chart of the isomer mixture of 1,3-bis(diethylamino)-pentacyclo[9.5.1.13,9.15,15.17,13]octasiloxane, 1,5-bis(diethylamino)-pentacyclo[9.5.1.13,9.15,15.17,13]octasiloxane, and 1,7-bis(diethylamino)-pentacyclo[9.5.1.13,9.15,15.17,13]octasiloxane obtained by the production method in Example 1 of the present disclosure is shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] <Aminosilsesquioxane> The aminosilsesquioxane in the present disclosure has the following formula (1): TIFF2024132524000007.tif41150[In formula (1), R 1 ~R 8 Six of these are hydrogen atoms. R 1 ~R 8 Each of the two is independently NR 9 R 10 is an amino group represented by R 9 and R 10 each independently represents an alkyl group having 1 to 4 carbon atoms.] It is expressed as:
[0012] By using the aminosilsesquioxane of the present disclosure as a silicon precursor, a high film formation rate can be achieved at low temperatures. In addition, by using the aminosilsesquioxane of the present disclosure as a silicon precursor, a high-quality film can be formed as a silicon-containing film (e.g., a silicon oxide film, a silicon nitride film). Therefore, by using the aminosilsesquioxane of the present disclosure, a film with excellent film properties can be formed at high speed, and a high-performance semiconductor device can be produced with high productivity.
[0013] R 1 ~R 8 Each of the groups is independently a hydrogen atom or NR 9 R 10 It is an amino group represented by the following formula:
[0014] R 1 ~R 8 Six of these are hydrogen atoms.
[0015] R 1 ~R 8 Each of the two is independently NR 9 R 10 is an amino group represented by R 9 and R 10 Each of NR is independently an alkyl group having 1 to 4 carbon atoms. 9 R 10 may be the same or different, for example, they are the same.
[0016] R 9 and R 10 Each of R is independently an alkyl group having 1 to 4 carbon atoms (e.g., methyl, ethyl, propyl, isopropyl, n-butyl, sec-butyl, isobutyl, or tert-butyl), and preferably an alkyl group having 1 to 3 carbon atoms (methyl, ethyl, propyl, or isopropyl). 9 and R 10 Each of R may independently be branched or linear, preferably linear. 9 and R 10 may be the same or different, for example, they are the same. 9 and R 10 NR 9 R 10 Examples of R include dimethylamino, diethylamino, dipropylamino, and diisopropylamino. 9 and R 10 Different NR 9 R 10 Examples include methylethylamino, methylpropylamino, methylisopropylamino, ethylpropylamino, and ethylisopropylamino.
[0017] The aminosilsesquioxane may be at least one selected from the group consisting of 1,3-position amino group modified products, 1.5-position amino group modified products, and 1,7-position amino group modified products. The aminosilsesquioxane may be a mixture of two or more isomers, for example, a mixture of 1,3-position amino group modified products, 1.5-position amino group modified products, and 1,7-position amino group modified products. Specific examples of aminosilsesquioxane include: Below formula (2): TIFF2024132524000008.tif51150 represents 1,3-bis(diethylamino)-pentacyclo[9.5.1.1 3,9 .1 5,15 .1 7,13 ]Octasiloxane, Below formula (3): TIFF2024132524000009.tif51150 represents 1,5-bis(diethylamino)-pentacyclo[9.5.1.1 3,9 .1 5,15 .1 7,13 ]octasiloxane, and Below formula (4): TIFF2024132524000010.tif51150 represents 1,7-bis(diethylamino)-pentacyclo[9.5.1.1 3,9 .1 5,15 .1 7,13 ]octasiloxane, for example, a mixture of these three isomers.
[0018] <Method of producing aminosilsesquioxane> The method for producing an aminosilsesquioxane represented by formula (1) in the present disclosure includes the following steps: (a) a synthesis step of reacting a raw material silsesquioxane with a secondary amine to synthesize an aminosilsesquioxane; and (b) Purification by distillation and / or sublimation may include:
[0019] [Synthesis step (a)] In the synthesis step (a), a raw material silsesquioxane is reacted with a secondary amine to synthesize an aminosilsesquioxane.
[0020] The raw material silsesquioxane is represented by the following formula (5-1): Below formula (5-1): The cage hydrosilsesquioxane (pentacyclo[9.5.1.1 3,9 .1 5,15 .1 7,13 ]octasiloxane).
[0021] Secondary amines are represented by the following formula (5-2): HNR 9 R 10 (5-2) [In formula (5-2), R 9 and R 10 each independently represents an alkyl group having 1 to 4 carbon atoms.] In this case, R 9 and R 10 The aspect is as described above.
[0022] The synthesis step (a) in the present disclosure may be carried out in the presence of a catalyst. The catalyst may be a known catalyst that can be used in the amination reaction of known hydrosilsesquioxanes. The catalyst may be a transition metal catalyst, for example, a Ru, Re, Pd, Pt, Au, Ir, Rh, Mn, Zn, Cu, Ni, Fe or Y-based catalyst. The simple substance, complex (e.g., carbonyl catalyst), oxide, halide, salt, etc. of these metals may be used as a catalyst. These may be used alone or in combination of two or more kinds. Specific examples of the catalyst include triruthenium dodecacarbonyl, chlorotris(triphenylphosphine)rhodium(I), dicobalt octacarbonyl, etc.
[0023] Examples of the solvent that can be used in the present disclosure include hydrocarbons such as hexane, cyclohexane, heptane, nonane, and decane; halogenated hydrocarbons such as dichloroethane, dichloromethane, and chloroform; aromatic hydrocarbons such as benzene, toluene, xylene, chlorobenzene, and trichlorobenzene; ethers such as diethyl ether, tetrahydrofuran (THF), and ethylene glycol dimethyl ether, and mixtures thereof. Ethers such as diethyl ether, tetrahydrofuran (THF), and ethylene glycol dimethyl ether, or hydrocarbons such as hexane, cyclohexane, and heptane are preferred. The amount of the solvent used is usually 0.1 to 50 times the mass of the raw material silsesquioxane.
[0024] In order to avoid hydrolysis of the raw material silsesquioxane, etc., it is desirable to carry out the reaction system in the synthesis step (a) under anhydrous conditions, and the water content in all raw materials used is set to 0 to 5000 mass ppm, preferably 0 to 500 mass ppm, based on the mass of all raw materials. It is also desirable to use a reaction apparatus that has been dried by heating, reducing pressure, or replacing with an inert gas such as nitrogen or argon.
[0025] An example of the reaction between the starting silsesquioxane and the secondary amine (5-2) is shown below. Formula (6): TIFF2024132524000012.tif51150[where, R 9 and R 10 is as stated above.]
[0026] In step (a), either a method in which the raw material silsesquioxane is first dissolved in an organic solvent and the secondary amine (5-2) is added thereto, or a method in which the secondary amine (5-2) is dissolved in an organic solvent and the raw material silsesquioxane is added thereto can be used in this reaction.
[0027] The amount of the secondary amine (5-2) used in step (a) is usually 1.5 mol or more, preferably 2.0 mol or more, per 1.0 mol of the raw material silsesquioxane. The amount of the secondary amine (5-2) used in step (a) is usually 3.0 mol or less, preferably 2.5 mol or less, per 1.0 mol of the raw material silsesquioxane.
[0028] When a catalyst is used, the amount of the catalyst is usually 0.0001 mol or more, preferably 0.0005 mol or more, per 1.0 mol of the raw material silsesquioxane. The amount of the catalyst is 0.1 mol or less, preferably 0.01 mol or less, per 1.0 mol of the raw material silsesquioxane.
[0029] The reaction temperature may be 20° C. or higher, and preferably 50° C. or higher. The reaction temperature may be 200° C. or lower, and preferably 100° C. or lower.
[0030] The reaction time may be 10 minutes or more, or 30 minutes or more. The reaction time may be 48 hours or less, or 24 hours or less.
[0031] In step (a), a post-treatment step including a filtration step or a purification step or both may be carried out after the reaction is completed. The purification step may include a distillation step or a sublimation step or both. If a solid such as a by-product salt is present in the reaction liquid after the reaction is completed, filtration may be carried out to remove the solid from the crude product in the reactor. When a filtration step is carried out, it is desirable to carry out the filtration step under a dry inert gas, for example, under nitrogen or argon, in order to suppress decomposition of the aminosilsesquioxane. The filtration temperature is not uniquely determined, but can be applied from 10°C to the boiling point of the solvent used. It is preferable to carry out the filtration temperature in the range of 20°C to 65°C. The present production method can be applied whether or not a post-treatment step is carried out.
[0032] [Purification step (b)] In step (b), the aminosilsesquioxane is purified by an operation including distillation and / or sublimation (distillation or sublimation or both), for example, vacuum distillation. The organic solvent can be easily removed, and the target aminosilsesquioxane can be purified with a sufficiently high purity. The product obtained in the reaction step (a) may also contain by-products such as mono-substituted and tri-substituted products, but the target aminosilsesquioxane can be obtained by distillation and / or sublimation. The aminosilsesquioxane after distillation and / or sublimation may contain isomers, and the isomers may be separated using a means such as chromatography.
[0033] Step (b) may include other purification steps in addition to distillation and / or sublimation. The other purification steps may include, for example, precipitation removal of non-target substances such as metal catalysts and by-product salts, which are then removed by filtration or the like. Examples of precipitating agents include N,N,N',N'-tetramethyl-thioperoxydicarbonic diamide (also known as tetramethylthiuram disulfide), thiophenol, and the like. When filtration is performed, it may be performed under a dry inert gas, for example, under nitrogen or argon, in order to suppress decomposition of the aminosilsesquioxane. The filtration temperature is not uniquely determined, but can be applied from 10°C to the boiling point of the solvent used. It is preferable to perform the filtration at a temperature in the range of 20°C to 65°C. The other purification steps may be performed after the synthesis step and before the distillation and / or sublimation step. The present production method can be applied whether or not the other purification steps are performed.
[0034] <Method of manufacturing silicon-containing film> The aminosilsesquioxane according to the present disclosure can be used as an intermediate for forming a silicon-containing film on a substrate by chemical vapor deposition, particularly atomic deposition. More specifically, the method for forming a silicon-containing film according to the present disclosure includes the steps of: (c) providing a substrate with a cage-shaped silsesquioxane composition having an amino group, i.e., a compound represented by the following formula (1): TIFF2024132524000013.tif41150[In formula (1), R 1 ~R 8Six of these are hydrogen atoms. R 1 ~R 8 Each of the two is independently NR 9 R 10 is an amino group represented by R 9 and R 10 each independently represents an alkyl group having 1 to 4 carbon atoms.] to adsorb the aminosilsesquioxane onto the substrate; (d) purging unadsorbed aminosilsesquioxane and by-products; (e) injecting a reactive gas into the substrate on which the aminosilsesquioxane is adsorbed, thereby decomposing the aminosilsesquioxane to form an atomic layer; and (f) purging unreacted reaction gas and by-products; It may be a chemical vapor deposition method (particularly an atomic layer deposition method), including
[0035] The temperature of the substrate may be 100° C. or more, 150° C. or more, 200° C. or more, or 250° C. or more. The temperature of the substrate may be 800° C. or less, 700° C. or less, 600° C. or less, 500° C. or less, or 450° C. or less, and is preferably 700° C. or less.
[0036] The pressure during gas injection in steps (c) and (e) may be 0.05 Torr or more, 0.1 Torr or more, or 0.15 Torr or more. The pressure during gas injection in steps (c) and (e) may be 100 Torr or less, 50 Torr or less, or 25 Torr or less, preferably 50 Torr or less. The composition may contain an inert gas such as nitrogen or argon as a carrier gas.
[0037] In the step (e), when a silicon oxide film having a Si-O bond is formed, one or more gases selected from oxygen, ozone, and nitrogen monoxide can be used as the reactive gas. When a silicon nitride film having a Si-N bond is formed, one or more gases selected from nitrogen, ammonia, nitrous oxide, nitrogen monoxide, and nitrogen dioxide can be used.
[0038] The formation of the silicon-containing film is desirably carried out after replacing the atmosphere with an inert gas such as nitrogen or argon, that is, it is preferable to carry out the above step (c) after replacing the atmosphere inside the reaction system with an inert gas. EXAMPLES
[0039] The present disclosure will now be described in detail with reference to examples.
[0040] [Example 1: 1,3-bis(diethylamino)-pentacyclo[9.5.1.1 3,9 .1 5,15 .1 7,13 ]Octasilosiloxane, 1,5-bis(diethylamino)-pentacyclo[9.5.1.1 3,9 .1 5,15 .1 7,13 ]octasiloxane, and 1,7-bis(diethylamino)-pentacyclo[9.5.1.1 3,9 .1 5,15 .1 7,13 ]Synthesis of octasiloxane composition] After replacing with nitrogen, add pentacyclo[9.5.1.1] to a 500 mL flask equipped with a thermometer, a condenser, and a motor stirrer. 3,9 .1 5,15 .1 7,13 ]30.8 g (0.072 mol) of octasiloxane, 0.89 g (0.0014 mol) of triruthenium dodecacarbonyl, and 83.0 g of toluene were added, and the temperature was maintained at 90°C using an oil bath. While stirring, 12.3 g (0.17 mol) of diethylamine was added dropwise using a 50 mL dropping funnel over 3 hours, yielding 125.7 g of a toluene solution containing 19.7 g (0.0035 mol, calculated from GC analysis) of the desired aminosilsesquioxane.
[0041] To the obtained toluene solution containing the target aminosilsesquioxane, 2.0 g (0.0084 mol) of tetramethylthiuram disulfide and 167.2 g of toluene were added, and the mixture was stirred for 3 hours while maintaining the temperature at 70° C. using an oil bath. The toluene was removed by vacuum distillation at an internal temperature of 48° C., and solid matter, mainly a complex formed by the reaction of triruthenium dodecacarbonyl and tetramethylthiuram disulfide, was removed by vacuum filtration and hexane washing in a nitrogen-substituted glove box, yielding 94.3 g of a hexane solution containing the target aminosilsesquioxane composition.
[0042] The hexane was removed from the resulting hexane solution containing the target aminosilsesquioxane composition by vacuum distillation at an internal temperature of 46° C. The target aminosilsesquioxane was obtained in high purity by further sublimation using a sublimation apparatus at an oil bath temperature of 95° C. and 0.3 Torr.
[0043] GC analysis after sublimation confirmed that 8.0 g (yield 19%) of aminosilsesquioxane was obtained with a purity of 78 area %. The resulting aminosilsesquioxane composition was 1 The compound was identified by H-NMR and GC-MS. 1 H-NMR assignments are as follows: 1 The H-NMR chart is shown in Figure 1.
[0044] 1 H-NMR(400MHz,CDCl3):δ0.95-1.09(m,12H,[ CH 3-CH2-N]),δ2.82-2.98(m,8H,[CH3- CH 2-N]), δ3.80-4.77(m, 6H, [Si- H ])
[0045] the above 1 The results of H-NMR and GC-MS showed that the obtained aminosilsesquioxane composition was a compound represented by the following formula: TIFF2024132524000014.tif4139 represents 1,3-bis(diethylamino)-pentacyclo[9.5.1.1 3,9 .1 5,15 .1 7,13 ]octasiloxane and the following formula: TIFF2024132524000015.tif4145 represents 1,5-bis(diethylamino)-pentacyclo[9.5.1.1 3,9 .1 5,15 .1 7,13 ]octasiloxane and the following formula: TIFF2024132524000016.tif4637 represents 1,7-bis(diethylamino)-pentacyclo[9.5.1.1 3,9 .1 5,15 .1 7,13 ] and was identified as a composition with octasiloxane.
[0046] [Example 2: 1,3-bis(diethylamino)-pentacyclo[9.5.1.1 3,9 .1 5,15 .1 7,13 ]Octasilosiloxane, 1,5-bis(diethylamino)-pentacyclo[9.5.1.1 3,9 .1 5,15 .1 7,13 ]octasiloxane and 1,7-bis(diethylamino)-pentacyclo[9.5.1.1 3,9 .1 5,15 .1 7,13 ]Formation of silicon-containing films using octasiloxane compositions] A silicon substrate was placed in a vacuum apparatus and heated to 250 to 700°C. The silsesquioxane composition containing the aminosilsesquioxane and carrier gas obtained in Example 1 was adsorbed onto the heated silicon substrate. Then, argon gas was introduced to purge the unadsorbed aminosilsesquioxane and by-products from within the apparatus. Thereafter, ozone was injected as a reactive gas at a pressure of 0.05 to 100 Torr to form an atomic layer of silicon oxide derived from the silsesquioxane composition deposited on the substrate. Then, argon gas was introduced to purge the unreacted ozone and by-products. The above cycle was repeated to obtain a silicon oxide film.
[0047] [Comparative Example 1: Formation of silicon-containing film using 2-dimethylamino-2,4,6,8-tetramethylcyclotetrasiloxane] A silicon substrate was placed in a vacuum apparatus and heated to a predetermined temperature of 100 to 750°C. A siloxane composition containing 2-dimethylamino-2,4,6,8-tetramethylcyclotetrasiloxane and a carrier gas was injected at a pressure of 0.05 to 100 Torr and adsorbed onto the heated silicon substrate. Then, argon gas was introduced to purge the unadsorbed aminosiloxane composition and by-products from the apparatus. Then, ozone was injected as a reactive gas at a pressure of 0.05 to 100 Torr to form an atomic layer of silicon oxide derived from 2-dimethylamino-2,4,6,8-tetramethylcyclotetrasiloxane deposited on the substrate. Then, argon gas was introduced to purge the unreacted ozone gas and by-products. The above cycle was repeated to obtain a silicon oxide film.
[0048] [Comparative Example 2: Formation of silicon-containing film using bis(diethylaminosilane)] A silicon substrate was placed in a vacuum apparatus and heated to a predetermined temperature of 100 to 750°C. An aminosilane composition containing bisdiethylaminosilane and a carrier gas was injected at a pressure of 0.05 to 100 Torr and adsorbed onto the heated silicon substrate. Then, argon gas was introduced to purge the unadsorbed aminosilane composition and by-products from the apparatus. Then, ozone was injected as a reactive gas at a pressure of 0.05 to 100 Torr to form an atomic layer of silicon oxide derived from bisdiethylaminosilane deposited on the substrate. Then, argon gas was introduced to purge the unreacted ozone gas and by-products. The above cycle was repeated to obtain a silicon oxide film.
[0049] Comparative Example 3: Formation of silicon-containing film using octamethylsilsesquioxane A silicon substrate was placed in a vacuum chamber and heated to a predetermined temperature of 100 to 750° C. An attempt was made to inject a silsesquioxane composition containing octamethylsilsesquioxane and a carrier gas at a pressure of 0.05 to 100 Torr. However, under these conditions, the silsesquioxane composition was unable to be used for ALD film formation.
[0050] The specific deposition method is shown in Table 1. Table 2 summarizes the deposition rates at each temperature for Example 2 and Comparative Examples 1, 2, and 3. The layer thicknesses were measured with an ellipsometer. [Table 1] [Table 2]
[0051] As shown in Table 2, at a substrate temperature of 300°C, 1,3-bis(diethylamino)-pentacyclo[9.5.1.1 3,9 .1 5,15 .1 7,13 ]Octasilosiloxane, 1,5-bis(diethylamino)-pentacyclo[9.5.1.1 3,9 .1 5,15 .1 7,13 ]octasiloxane and 1,7-bis(diethylamino)-pentacyclo[9.5.1.1 3,9 .1 5,15 .1 7,13 The octasiloxane composition can be deposited at a higher deposition rate than the 2-dimethylamino-2,4,6,8-tetramethylcyclotetrasiloxane, bisdiethylaminosilane, and octamethylsilsesquioxane shown in the comparative examples. [Industrial Applicability]
[0052] By using the chemical vapor deposition method of the present disclosure, for example, atomic deposition, it is possible to form an extremely thin silicon oxide film free of atomic defects that can be used for semiconductor substrates with high aspect ratio structures, nanowires, etc. The aminosilsesquioxane of the present disclosure has good film quality and is particularly useful for atomic deposition, which forms films at a higher speed.
Claims
1. Below formula (1): [In formula (1), R 1 ~R 8 Six of these are hydrogen atoms. R 1 ~R 8 Each of the two is independently NR 9 R 10 is an amino group represented by R 9 and R 10 are each independently an alkyl group having 1 to 4 carbon atoms. The aminosilsesquioxane represented by the formula:
2. Below formula (2): 1,3-bis(diethylamino)-pentacyclo[9.5.1.1 3,9 .1 5,15 .1 7,13 ]Octasiloxane, Below formula (3): 1,5-bis(diethylamino)-pentacyclo[9.5.1.1 3,9 .1 5,15 .1 7,13 ]octasiloxane, and Below formula (4): 1,7-bis(diethylamino)-pentacyclo[9.5.1.1 3,9 .1 5,15 .1 7,13 2. The aminosilsesquioxane according to claim 1, which is at least one selected from the group consisting of octasiloxanes.
3. 3. The aminosilsesquioxane according to claim 1, wherein the aminosilsesquioxane is an isomeric mixture comprising two or more isomeric structures.
4. A precursor of a silicon-containing film comprising the aminosilsesquioxane of claim 1 or 2.
5. The precursor of claim 4 , wherein the silicon-containing film is formed by chemical vapor deposition.
6. 5. The precursor of claim 4, wherein the silicon-containing film is formed by atomic layer deposition.
7. A composition for forming a silicon-containing film, comprising the aminosilsesquioxane according to claim 1 or 2.
8. The composition of claim 7 , wherein the silicon-containing film is formed by chemical vapor deposition.
9. The composition of claim 7 , wherein the silicon-containing film is formed by atomic layer deposition.
10. Below formula (1): [In formula (1), R 1 ~R 8 Six of these are hydrogen atoms. R 1 ~R 8 Each of the two is independently NR 9 R 10 is an amino group represented by R 9 and R 10 are each independently an alkyl group having 1 to 4 carbon atoms. A method for producing an aminosilsesquioxane represented by the formula: (a) a synthesis step comprising reacting a starting silsesquioxane with a secondary amine to synthesize the aminosilsesquioxane; and (b) a purification step including distillation and / or sublimation A method for producing aminosilsesquioxane, comprising:
11. The secondary amine is represented by the following formula (5-2): HNR 9 R 10 (5-2) [In formula (5-2), R 9 and R 10 are each independently an alkyl group having 1 to 4 carbon atoms. The method for producing the aminosilsesquioxane according to claim 10, represented by the formula:
12. Below formula (1): [In formula (1), R 1 ~R 8 Six of these are hydrogen atoms. R 1 ~R 8 Each of the two is independently NR 9 R 10 is an amino group represented by R 9 and R 10 are each independently an alkyl group having 1 to 4 carbon atoms. The present invention relates to a method for producing a silicon-containing film, and more particularly to an aminosilsesquioxane represented by the formula:
Citation Information
Patent Citations
Production of ultralow carbon* 80 kg*mm2 high tensile steel plate
JP1978029218A