Resin material for solid electrolyte, resin material composition for solid electrolyte, sheet material and battery
A resin material with a norbornene-derived and ethylene oxide structure stabilizes ionic conductivity in solid electrolytes, addressing conductivity issues and temperature variability, enhancing battery performance and reliability.
Patent Information
- Application Number
- JP2023127120
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-14
- Filing Date
- 2023-08-03
- Publication Date
- 2024-10-01
AI Technical Summary
Existing solid electrolytes exhibit lower ionic conductivity compared to liquid electrolytes, and their conductivity varies significantly with temperature, leading to instability in battery performance.
A resin material for solid electrolytes comprising a polyethylene oxide compound with a norbornene-derived structure in the main chain and an ethylene oxide structure in the side chain, which stabilizes ionic conductivity over a wide temperature range without the need for high-temperature treatment.
The resin material maintains excellent ionic conductivity and mechanical properties, improving battery charging/discharging characteristics and reliability by reducing interfacial resistance and preventing rapid conductivity changes.
Smart Images

Figure 2024132791000014 
Figure 2024132791000001 
Figure 2024132791000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin material for a solid electrolyte, a resin material composition for a solid electrolyte, a sheet material, and a battery. [Background technology]
[0002] For example, liquid electrolytes have been used in secondary batteries such as lithium ion secondary batteries, etc. However, the use of liquid electrolytes raises concerns about leakage from product containers, and improvements have been required to increase reliability.
[0003] In order to solve these problems, a method of using a solid electrolyte instead of a liquid electrolyte has been considered, but there is a problem that the ionic conductivity is lower than that of a liquid electrolyte.
[0004] In order to solve such problems, there have been attempts to use polyethylene oxide as a polymer for the electrolyte (see, for example, Patent Document 1).
[0005] However, when polyethylene oxide is used, although it shows a relatively high ionic conductivity in the high temperature range, there is a problem that the ionic conductivity drops rapidly when the temperature drops. Thus, when the temperature dependency of the ionic conductivity becomes large, there is a problem that the ionic conductivity changes rapidly within the operating temperature range of the battery. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2014 / 002858 Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide a resin material for solid electrolytes that exhibits stable and excellent ionic conductivity over a wide temperature range, and to provide a resin material composition for solid electrolytes, a sheet material, and a battery that contain the resin material for solid electrolytes. [Means for solving the problem]
[0008] Such an object can be achieved by the present invention described below in (1) to (13). (1) a polyethylene oxide compound as a first resin component; A resin material for a solid electrolyte, comprising: a second resin component having a norbornene-derived structure in its main chain and an ethylene oxide structure in its side chain.
[0009] (2) The resin material for a solid electrolyte according to the above (1), wherein the second resin component contains a monomer component represented by the following formula (NB):
[0010] [ka] (In formula (NB), R 1 is a hydrogen atom or a hydrocarbon group, and R 2 , R 3 and R 4 are each independently a hydrogen atom or an organic group having 1 to 3 carbon atoms, n is an integer of 1 or more, and a1 is 0, 1, or 2.
[0011] (3) The resin material for solid electrolytes according to the above (2), wherein n in the above formula (NB) is an integer of 2 or more and 6 or less.
[0012] (4) The resin material for solid electrolytes according to any one of (1) to (3) above, wherein the second resin component has a weight average molecular weight of 3,000 or more and 300,000 or less.
[0013] (5) The resin material for solid electrolytes according to any one of (1) to (3) above, wherein the second resin component has an average degree of polymerization of 10 or more and 1,350 or less.
[0014] (6) The resin material for solid electrolytes according to any one of (1) to (3) above, wherein the second resin component has a softening point of −30° C. or higher and 150° C. or lower.
[0015] (7) The resin material for a solid electrolyte according to any one of (1) to (3) above, wherein the first resin component has a weight average molecular weight of 500 or more and 100,000 or less.
[0016] (8) A resin material for solid electrolyte according to any one of (1) to (3), wherein, in the resin material for solid electrolyte, a content of the first resin component is X1 [mass%] and a content of the second resin component is X2 [mass%], the relationship of 0.10≦X2 / X1≦9.00 is satisfied.
[0017] (9) A resin material composition for a solid electrolyte, comprising the resin material for a solid electrolyte according to any one of (1) to (3) above and a lithium salt.
[0018] (10) The resin material composition for solid electrolytes according to the above (7), wherein the lithium salt is at least one selected from the group consisting of LiSCN, LiN(CN)2, LiClO4, LiBF4, LiAsF6, LiPF6, LiCF3SO3, Li(CF3SO2)2N, Li(CF3SO2)3C, LiSbF6, Li(FSO2)2N, LiC4F9SO3, LiN(SO2CF2CF3)2, LiPF3(CF2CF3)3, LiPF3(C2F5)3, LiPF3(CF3)3, LiCl, LiF, LiBr, LiI, LiB(C2O4)2, lithium difluoro(oxalate)borate and lithium bis(oxalate)borate.
[0019] (11) A resin material composition for a solid electrolyte according to the above (7), in which a ratio of the total number of oxygen atoms contained in the resin material for a solid electrolyte contained in the resin material composition for a solid electrolyte to the total number of lithium atoms contained in the lithium salt contained in the resin material composition for a solid electrolyte is 4.0 or more and 33.3 or less.
[0020] (12) A sheet material comprising a material containing the resin material for solid electrolytes according to any one of (1) to (3) above.
[0021] (13) a positive electrode layer; A negative electrode layer; a battery comprising an electrolyte layer located between the positive electrode layer and the negative electrode layer, A battery comprising the resin material for a solid electrolyte according to any one of (1) to (3) above. Effect of the Invention
[0022] According to the present invention, it is possible to provide a resin material for solid electrolytes that exhibits stable and excellent ionic conductivity over a wide temperature range, and to provide a resin material composition for solid electrolytes, a sheet material, and a battery that contain the resin material for solid electrolytes. [Brief description of the drawings]
[0023] [Figure 1] FIG. 1 is a longitudinal sectional view illustrating a schematic diagram of an example of an all-solid-state battery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] The present invention will now be described in detail with reference to the accompanying drawings. [1] Resin material for solid electrolyte The resin material for a solid electrolyte of the present invention is a resin material used for forming a solid electrolyte.
[0025] In the present invention, the solid electrolyte is a concept including all-solid electrolytes, semi-solid electrolytes, and gel electrolytes, and may contain a liquid component or an electrolytic solution in addition to a resin material for a solid electrolyte.
[0026] The resin material for solid electrolytes of the present invention is characterized by comprising a polyethylene oxide compound as a first resin component, and a second resin component having a norbornene-derived structure in its main chain and an ethylene oxide structure in its side chain.
[0027] This makes it possible to provide a resin material for solid electrolytes that exhibits stable and excellent ion conductivity over a wide temperature range. Such excellent effects are believed to be obtained for the following reasons. In other words, by including a polyethylene oxide compound as the first resin component, it is possible to make the ion conductivity excellent in a relatively high temperature range, and by including a second resin component having an ethylene oxide structure in the side chain that has excellent affinity with the first resin component and a norbornene-derived structure in the main chain, it is possible to suppress crystallization that is likely to occur with an ethylene oxide structure alone, and it is possible to maintain excellent ion conductivity even in a relatively low temperature range. As a result, it is believed that it is possible to prevent a sudden change in ion conductivity over a wide temperature range and to exhibit stable and excellent ion conductivity. In addition, by including a second resin component having a rigid norbornene-derived structure in the main chain, it is possible to obtain good mechanical properties when molded into, for example, a film.
[0028] Furthermore, the solid electrolyte resin material can have excellent adhesion to inorganic materials (such as inorganic solid electrolytes, active materials, and current collectors, which will be described later).
[0029] In general, oxide-based inorganic solid electrolytes have high ionic conductivity but high interfacial resistance, and therefore require high-temperature treatment such as sintering to reduce the interfacial resistance. However, by combining the oxide-based inorganic solid electrolyte with the resin material for solid electrolytes of the present invention, the interfacial resistance can be reduced without high-temperature treatment such as sintering, and a flexible composite sheet having high ionic conductivity can be suitably formed.
[0030] Furthermore, unless high-temperature treatment such as sintering is performed on an oxide-based inorganic solid electrolyte, the interfacial resistance between the electrolyte and the electrode material increases, causing problems with charging and discharging, but by combining the electrolyte with the resin material for solid electrolyte of the present invention, the electrolyte can be suitably bonded to the electrode without high-temperature treatment such as sintering, and good charging and discharging characteristics can be obtained. As described above, the charging and discharging characteristics, reliability, etc. of a battery made of a material containing the resin material for solid electrolyte can be excellent.
[0031] [1-1] First resin component The resin material for a solid electrolyte of the present invention contains a polyethylene oxide compound as a first resin component.
[0032] In the present invention, the polyethylene oxide compound refers to polyethylene oxide and a compound in which at least one hydroxyl group of polyethylene oxide is etherified with an alkyl group having 1 to 6 carbon atoms.
[0033] That is, in the present invention, the polyethylene oxide compound refers to a compound represented by the following formula [V].
[0034] R 5 O(CH2CH2O) m R 6 [V] (In formula [V], R 5 and R 6 are each independently a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, and m is an integer of 2 or more.
[0035] In particular, R in the above formula [V] 5 and R 6 is preferably a hydrogen atom or a methyl group.
[0036] This allows the effects of the present invention to be more pronounced, as described above, and also improves the stability and ease of handling of the sheet when processed into a sheet material, as described below.
[0037] The weight average molecular weight of the first resin component is preferably 500 or more and 100,000 or less, more preferably 1,000 or more and 80,000 or less, and even more preferably 2,000 or more and 50,000 or less.
[0038] This allows the effects of the present invention to be more pronounced, as described above, and also improves the stability and ease of handling of the sheet when processed into a sheet material, as described below.
[0039] The content of the first resin component in the resin material for solid electrolytes of the present invention is preferably 8.0 mass% or more and 90.0 mass% or less, more preferably 20.0 mass% or more and 85.0 mass% or less, and even more preferably 40.0 mass% or more and 80.0 mass% or less.
[0040] This allows the effects of the present invention to be more pronounced, as described above, and also improves the stability and ease of handling of the sheet when processed into a sheet material, as described below.
[0041] [1-2] Second resin component The resin material for solid electrolytes of the present invention contains a second resin component having a norbornene-derived structure in the main chain and an ethylene oxide structure in the side chain.
[0042] The second resin component has a norbornene-derived structure in the main chain, and an example of the norbornene-derived structure is the structure represented by the following formula [II] as a monomer.
[0043] [ka] (At least one of R1, R2, R3, R4, R5, R6, R7, R8, R9, and R10 in formula [II] is a single bond (direct bond) or a divalent atom or atomic group bonded to the side chain, and the rest are monovalent atoms or atomic groups.)
[0044] The divalent atomic group may, for example, be a linear or branched alkylene group. The monovalent atom includes, for example, a hydrogen atom.
[0045] Examples of the monovalent atomic group include hydrocarbon groups such as alkyl groups, alkenyl groups, and alkynyl groups, and further include structures in which these are bonded to the divalent atom or divalent atomic group.
[0046] In particular, in the norbornene-derived structure, only one of R1 to R10 in the above formula [II] is a single bond bonded to the side chain, and the remaining nine are preferably hydrogen atoms.
[0047] This makes it possible to more significantly exhibit the effects of the present invention as described above. In addition, the synthesis of the monomer, which is the raw material of the second resin component, can be carried out in a higher yield, and the polymerization reaction of the monomer can also proceed more efficiently, thereby increasing the yield of the second resin component.
[0048] In this case, the single bond bonded to the side chain is preferably any one of R3 to R6 in the above formula [II].
[0049] This allows the effects of the present invention as described above to be more pronounced, and also allows the synthesis of the monomer, which is the raw material of the second resin component, to be carried out in a higher yield, and the polymerization reaction of the monomer to proceed more efficiently, thereby further increasing the yield of the second resin component.
[0050] When the second resin component contains a structure represented by the above formula [II] as a norbornene-derived structure, the second resin component may contain multiple different types of structures represented by the above formula [II] within the molecule.
[0051] The second resin component has an ethylene oxide structure in the side chain. The ethylene oxide structure may be one that exists alone (one that does not have a structure in which ethylene glycol molecules are condensed with each other) or one that has a repeating structure (one that has a structure in which ethylene glycol molecules are condensed with each other), but one that has a repeating structure (one that has a structure in which ethylene glycol molecules are condensed with each other) is preferable.
[0052] This makes it possible to increase the ionic conductivity of the solid electrolyte resin material.
[0053] In particular, the second resin component preferably contains a monomer component represented by the following formula (NB).
[0054] [ka] (In formula (NB), R 1 is a hydrogen atom or a hydrocarbon group, and R 2 , R 3 and R 4 are each independently a hydrogen atom or an organic group having 1 to 3 carbon atoms, n is an integer of 1 or more, and a1 is 0, 1, or 2.
[0055] This allows the effects of the present invention to be more pronounced, as described above, and also improves the stability and ease of handling of the sheet when processed into a sheet material, as described below.
[0056] R in the above formula (NB) 1 may be a hydrogen atom or a hydrocarbon group, but is preferably an alkyl group having 1 to 4 carbon atoms, and more preferably a methyl group.
[0057] This allows the effects of the present invention to be more pronounced, as described above, and also improves the stability and ease of handling of the sheet when processed into a sheet material, as described below.
[0058] R in the above formula (NB) 2 , R3 and R 4 may each independently be a hydrogen atom or an organic group having 1 to 3 carbon atoms, and is preferably a hydrogen atom.
[0059] This allows the effects of the present invention to be more pronounced, as described above, and also improves the stability and ease of handling of the sheet when processed into a sheet material, as described below.
[0060] When the ethylene oxide structure constituting the side chain of the second resin component has a repeating structure (having a structure in which ethylene glycol molecules are condensed together), the number of ethylene glycol molecules in the ethylene oxide structure is preferably 2 to 6, more preferably 2 to 5, and even more preferably 2 to 3. More specifically, for example, when the second resin component contains a monomer component represented by the above formula (NB), n in the above formula (NB) may be an integer of 1 or more, but is preferably an integer of 2 to 6, more preferably an integer of 2 to 5, and even more preferably 2 or 3.
[0061] This allows the effects of the present invention to be more pronounced, as described above, and also improves the stability and ease of handling of the sheet when processed into a sheet material, as described below.
[0062] The second resin component may contain, in its molecule, a plurality of types of structures having different numbers of condensation of ethylene glycol molecules.
[0063] As described above, the second resin component preferably contains a monomer component represented by the above formula (NB). Among the monomer components represented by the above formula (NB), it is preferable that the second resin component contains a monomer component represented by the following formula [I].
[0064] [ka] (In formula [I], n is an integer of 1 or more, and R is a hydrogen atom or a hydrocarbon group.)
[0065] This allows the above-mentioned effects of the present invention to be more significantly exhibited, and also allows the ion conductivity of the solid electrolyte resin material to be made higher, and also allows the sheet to be more stable and easier to handle when processed into a sheet material as described below.
[0066] When the second resin component contains a monomer component represented by the above formula (NB), the second resin component may contain, in its molecule, multiple different types of monomer components represented by the above formula (NB).
[0067] The second resin component is required to have a norbornene-derived structure in the main chain, and may have a structure not derived from norbornene (e.g., a monomer component other than the above formula [II]) in addition to the norbornene-derived structure in the main chain.
[0068] In such a case, the proportion of monomer components having a norbornene-derived structure in all monomer components constituting the main chain of the second resin component is preferably 95.0 mol % or more, more preferably 98.0 mol % or more, and even more preferably 100 mol %.
[0069] The second resin component only needs to have an ethylene oxide structure in the side chain, and may have a structure other than the ethylene oxide structure in addition to the ethylene oxide structure in the side chain.
[0070] The proportion of the monomer component represented by the above formula [I] in all the monomer components constituting the second resin component is preferably 90.0 mol % or more, more preferably 95.0 mol % or more, and even more preferably 100 mol %.
[0071] The weight average molecular weight of the second resin component is preferably 3,000 or more and 300,000 or less, more preferably 4,000 or more and 250,000 or less, and even more preferably 5,000 or more and 200,000 or less.
[0072] This makes it possible to achieve a higher level of compatibility between the ionic conductivity of the solid electrolyte resin material and the stability and ease of handling of the sheet when processed into a sheet material as described below.
[0073] The average degree of polymerization of the second resin component is preferably 10 or more and 1,350 or less, more preferably 13 or more and 1,130 or less, and even more preferably 16 or more and 900 or less.
[0074] This makes it possible to achieve a higher level of compatibility between the ionic conductivity of the solid electrolyte resin material and the stability and ease of handling of the sheet when processed into a sheet material as described below.
[0075] The softening point of the second resin component is preferably -30°C or higher and 150°C or lower, more preferably -20°C or higher and 135°C or lower, and even more preferably -15°C or higher and 120°C or lower.
[0076] This makes it possible to achieve a higher level of compatibility between the ionic conductivity of the solid electrolyte resin material and the stability and ease of handling of the sheet when processed into a sheet material as described below.
[0077] The softening point can be determined using TMA / SS6100 under the conditions of a temperature rise rate of 3° C. / min and a compression load of 30 mN. In the examples described later, the softening point was determined under such conditions.
[0078] The content of the second resin component in the resin material for solid electrolyte of the present invention is preferably 9.0 mass% or more and 90.0 mass% or less, more preferably 15.0 mass% or more and 80.0 mass% or less, and even more preferably 20.0 mass% or more and 60.0 mass% or less.
[0079] This allows the effects of the present invention to be more pronounced, as described above, and also improves the stability and ease of handling of the sheet when processed into a sheet material, as described below.
[0080] In the resin material for solid electrolytes of the present invention, when the content of the first resin component is X1 [mass%] and the content of the second resin component is X2 [mass%], it is preferable to satisfy the relationship of 0.10≦X2 / X1≦9.00, more preferably to satisfy the relationship of 0.18≦X2 / X1≦4.00, and further preferably to satisfy the relationship of 0.25≦X2 / X1≦1.50.
[0081] This allows the effects of the present invention to be more pronounced, as described above, and also improves the stability and ease of handling of the sheet when processed into a sheet material, as described below.
[0082] [1-3] Other resin components The resin material for solid electrolytes of the present invention contains the first and second resin components described above, but may further contain other resin components. Hereinafter, such resin components are also referred to as "other resin components."
[0083] Examples of the other resin components include a resin material having a norbornene-derived structure in the main chain but not having an ethylene oxide structure in the side chain, a resin material having an ethylene oxide structure in the side chain but not having a norbornene-derived structure in the main chain, etc. Examples of the other resin components include PVDF (polyvinylidene fluoride), PTFE (polytetrafluoroethylene), PVF (polyvinyl fluoride), PVC (polyvinyl chloride), PVA (polyvinyl alcohol), polyvinyl acetate, polyethylene oxide, polyacrylic acid, polyacrylamide, polystyrene sulfonic acid, and derivatives thereof, etc., and particularly, polyethylene oxide, polyacrylic acid, polyacrylamide, and derivatives thereof, etc.
[0084] However, the proportion of other resin components in the resin material for solid electrolytes of the present invention is preferably 20 mass % or less, more preferably 10 mass % or less, and even more preferably 5 mass % or less.
[0085] [2] Resin material composition for solid electrolyte Next, the resin material composition for solid electrolytes of the present invention will be described.
[0086] The resin material composition for solid electrolytes of the present invention is characterized by containing the above-mentioned resin material for solid electrolytes of the present invention and a lithium salt.
[0087] This makes it possible to provide a resin material composition for solid electrolytes that contains a resin material for solid electrolytes that exhibits stable and excellent ion conductivity over a wide temperature range, thereby forming a solid electrolyte that exhibits stable and excellent ion conductivity over a wide temperature range.
[0088] When the resin component constituting the resin material for solid electrolytes of the present invention has a lithium salt structure in the molecule, the resin material composition for solid electrolytes of the present invention contains a lithium salt other than the resin component.
[0089] The content of the resin material for solid electrolytes of the present invention in the resin material composition for solid electrolytes of the present invention is not particularly limited, but the ratio of the resin material for solid electrolytes of the present invention to the total solid content of the resin material composition for solid electrolytes of the present invention is preferably 45 mass % or more and 90 mass % or less, more preferably 50 mass % or more and 88 mass % or less, and even more preferably 55 mass % or more and 85 mass % or less.
[0090] This makes it possible to provide a solid electrolyte formed using the resin material composition for a solid electrolyte with superior ionic conductivity.
[0091] The lithium salt contained in the resin material composition for solid electrolytes of the present invention is not particularly limited, but is preferably at least one selected from the group consisting of LiSCN, LiN(CN)2, LiClO4, LiBF4, LiAsF6, LiPF6, LiCF3SO3, Li(CF3SO2)2N, Li(CF3SO2)3C, LiSbF6, Li(FSO2)2N, LiC4F9SO3, LiN(SO2CF2CF3)2, LiPF3(CF2CF3)3, LiPF3(C2F5)3, LiPF3(CF3)3, LiCl, LiF, LiBr, LiI, LiB(C2O4)2, lithium difluoro(oxalate)borate, and lithium bis(oxalate)borate, and is more preferably Li(CF3SO2)2N.
[0092] This makes it possible to provide a solid electrolyte formed using the resin material composition for a solid electrolyte with superior ionic conductivity.
[0093] The content of the lithium salt in the resin material composition for solid electrolytes of the present invention is not particularly limited, but the ratio of the lithium salt to the total solid content of the resin material composition for solid electrolytes of the present invention is preferably 5 mass % or more and 55 mass % or less, more preferably 10 mass % or more and 50 mass % or less, and even more preferably 15 mass % or more and 45 mass % or less.
[0094] This makes it possible to provide a solid electrolyte formed using the resin material composition for a solid electrolyte with superior ionic conductivity.
[0095] The content ratio of the resin material for solid electrolytes of the present invention and the lithium salt in the resin material composition for solid electrolytes of the present invention is not particularly limited, but the ratio of the total number of oxygen atoms contained in the resin material for solid electrolytes of the present invention contained in the resin material composition for solid electrolytes of the present invention to the total number of lithium atoms contained in the lithium salt contained in the resin material composition for solid electrolytes of the present invention is preferably 4.0 or more and 33.3 or less, more preferably 4.5 or more and 25.0 or less, and even more preferably 5.0 or more and 20.0 or less.
[0096] This makes it possible to provide a solid electrolyte formed using the resin material composition for a solid electrolyte with superior ionic conductivity.
[0097] The resin material composition for solid electrolytes of the present invention may further contain, for example, an active material such as a positive electrode active material or a negative electrode active material.
[0098] Examples of the positive electrode active material include LiCoO2, LiNiO2, LiMn2O4, Li2Mn2O3, and LiCr. 0.5 Mn 0.5 Examples of the positive electrode active material include fluorides such as LiFeF3, LiBH4, Li4BN3H, and the like. 10 boron complex compounds such as boron fluoride complexes, iodine complex compounds such as polyvinylpyridine-iodine complexes, and nonmetallic compounds such as sulfur can also be used.
[0099] Examples of negative electrode active materials include Nb2O5, V2O5, TiO2, In2O3, ZnO, SnO2, NiO, ITO, AZO, GZO, ATO, FTO, and Li4Ti5O. 12 Examples of the negative electrode active material include metals and alloys such as Li, Al, Si, Si-Mn, Si-Co, Si-Ni, Sn, Zn, Sb, Bi, In, and Au, carbon materials such as graphite and hard carbon, LiC 24 Alternatively, a material in which lithium ions are inserted between layers of a carbon material such as LiC6 may be used.
[0100] When the resin material composition for a solid electrolyte of the present invention contains a positive electrode active material, the resin material composition for a solid electrolyte can be suitably used for forming a positive electrode layer of a battery as described below, and when the resin material composition for a solid electrolyte of the present invention contains a negative electrode active material, the resin material composition for a solid electrolyte can be suitably used for forming a negative electrode layer of a battery as described below.
[0101] The resin material composition for solid electrolytes of the present invention may further contain, for example, an inorganic solid electrolyte.
[0102] Examples of inorganic solid electrolytes include LiLaZrO-based compounds, LiLaZrNbO-based compounds, LiLaZrTaO-based compounds, LiLaTaO-based compounds, LiLaTiO-based compounds, LiAlGePO-based compounds, LiAlTiPO-based compounds, LiPO-based compounds, LiSiO-based compounds, LiBO-based compounds, LiPS-based compounds, and LiPSCl-based compounds.
[0103] When the resin material composition for solid electrolytes of the present invention contains an inorganic solid electrolyte, the proportion of the inorganic solid electrolyte in the total solid content of the resin material composition for solid electrolytes of the present invention is preferably 10 mass % or more and 95 mass % or less, more preferably 15 mass % or more and 90 mass % or less, and even more preferably 20 mass % or more and 85 mass % or less.
[0104] This can provide the resin material composition for solid electrolytes with better strength and ion conductivity.
[0105] The resin material composition for solid electrolytes of the present invention may further contain, for example, a non-aqueous solvent used in the electrolyte solution.
[0106] Examples of the non-aqueous solvent include cyclic carbonates such as propylene carbonate (PC), ethylene carbonate (EC), and vinylene carbonate (VC); chain carbonates such as diethyl carbonate (DEC), dimethyl carbonate (DMC), and methyl ethyl carbonate (MEC); cyclic ethers such as tetrahydrofuran (THF), 2-methyl tetrahydrofuran (2MeTHF), and dioxolane (DOX); chain ethers such as dimethoxy ethane (DME) and diethoxy ethane (DEE); γ-butyrolactone (GBL), acetonitrile (AN), and sulfolane (SL). These non-aqueous solvents can be used alone or in combination.
[0107] When the resin material composition for solid electrolytes of the present invention contains a non-aqueous solvent, the proportion of the plasticizer in the total solid content of the resin material composition for solid electrolytes of the present invention is preferably 0.1 mass % or more and 90 mass % or less, more preferably 1 mass % or more and 85 mass % or less, and even more preferably 5 mass % or more and 80 mass % or less.
[0108] This can improve the ease of handling of the resin material composition for solid electrolytes, the ion conductivity, and the interface formation with the composite.
[0109] The resin material composition for solid electrolytes of the present invention may further contain a liquid component that is liquid at 25°C, for example.
[0110] This improves the ease of handling of the resin material composition for solid electrolytes, and allows the formation of a solid electrolyte to be more suitably carried out.
[0111] Examples of the liquid component include alcohols such as methanol, ethanol, isopropanol, butanol, octanol, and benzyl alcohol; esters such as ethyl acetate, butyl acetate, ethyl lactate, γ-butyrolactone, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, butyl butyrate, and methyl benzoate; dioxane, 1,2-dimethoxyethane, tetrahydrofuran (THF), ethylene glycol monobutyl ether, propylene glycol monomethyl ether, ethylene diglycol monomethyl ether, ethylene diglycol ethyl ether, and the like. ethers such as dimethyl ether; amides such as N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, diisobutyl ketone (DIBK), cyclohexanone; nitriles such as acetonitrile; aromatic hydrocarbons such as benzene, toluene, xylene, trimethylbenzene (mesitylene, hemimelitene, pseudocumene), ethylbenzene, tetralin, and derivatives thereof (for example, compounds in which the hydrogen atoms of these compounds are substituted with other atoms or atomic groups (functional groups, etc.)), and the like. One or more selected from these can be used in combination.
[0112] When the resin material composition for solid electrolytes of the present invention contains the liquid component, the proportion of the liquid component in the resin material composition for solid electrolytes of the present invention is preferably 0.001% by mass or more and 10% by mass or less, and more preferably 0.005% by mass or more and 5% by mass or less.
[0113] This makes it possible to more suitably remove liquid components during the formation of the solid electrolyte while improving the ease of handling of the resin material composition for solid electrolytes, thereby improving the productivity of the solid electrolyte.
[0114] The resin material composition for solid electrolytes of the present invention may contain components other than the above-mentioned components. Hereinafter, such components are also referred to as "other components".
[0115] Examples of other components include adhesion aids, leveling agents, antifoaming agents, colorants, antioxidants, flame retardants, inorganic fillers such as silica, medium-chain normal alkanes such as paraffin and petrolatum, natural materials such as rosin, pine resin, and Canada balsam, and glymes such as butyl glyme and tetraglyme.
[0116] However, the proportion of other components in the resin material composition for solid electrolytes of the present invention is preferably 10 mass % or less, more preferably 5 mass % or less, and even more preferably 3 mass % or less.
[0117] [3] Sheet material Next, the sheet material of the present invention will be described.
[0118] The sheet material of the present invention is characterized in that it is made of a material containing the above-mentioned resin material for solid electrolytes of the present invention.
[0119] This makes it possible to provide a sheet material containing a resin material for a solid electrolyte that exhibits stable and excellent ion conductivity over a wide temperature range. In addition, by using such a sheet material, a layered (sheet-shaped) solid electrolyte can be suitably formed. As a result, it can be suitably applied to the manufacture of a battery as described below. More specifically, when the sheet material does not contain an active material, it can be suitably used to form a solid electrolyte layer of a battery, when the sheet material contains a positive electrode active material, it can be suitably used to form a positive electrode layer of a battery, and when the sheet material contains a negative electrode active material, it can be suitably used to form a negative electrode layer of a battery.
[0120] The content of the resin material for solid electrolyte of the present invention in the sheet material of the present invention is preferably 45 mass% or more and 90 mass% or less, more preferably 50 mass% or more and 88 mass% or less, and even more preferably 55 mass% or more and 85 mass% or less.
[0121] This makes it possible to provide a solid electrolyte formed using the resin material composition for a solid electrolyte with superior ionic conductivity.
[0122] The sheet material of the present invention may contain components other than the resin material for solid electrolyte of the present invention. Examples of such components include the components described in the resin material composition for solid electrolytes.
[0123] The thickness of the sheet material of the present invention is not particularly limited, but is preferably from 5 μm to 5000 μm, and more preferably from 10 μm to 1000 μm.
[0124] This makes it easier for the sheet material itself to maintain its mechanical strength in a more suitable manner, making it easier to handle the sheet material during the battery manufacturing process and the like.
[0125] The sheet material of the present invention may be produced by any method, but can be suitably produced, for example, by the following method.
[0126] That is, a composition containing the constituent materials of the sheet material or precursors thereof can be formed into a sheet to obtain the sheet material.
[0127] Examples of the precursor of the constituent material of the sheet material that can be contained in the composition include oligomers and prepolymers that correspond to the resin components that constitute the resin material for solid electrolyte of the present invention described above.
[0128] The sheet material can be produced using the above-mentioned resin material composition for solid electrolytes. When a composition containing a liquid component is used to manufacture a sheet material, for example, an excess amount of the liquid component may be used when preparing the composition, and a portion of the liquid component may be removed before forming the composition into a sheet to form a slurry.
[0129] When a sheet material is produced using a composition containing a liquid component, for example, a layer is formed using various coating methods such as cast coating, and then the liquid component is removed from the layer, thereby making it possible to obtain a suitable sheet material.
[0130] In addition, a part of the liquid component used in the manufacturing process may remain in the sheet material, and in such a case, the liquid component may be removed during the manufacturing process of the battery.
[0131] [4]Battery Next, the battery of the present invention will be described.
[0132] The battery of the present invention is a battery comprising a positive electrode layer, a negative electrode layer, and an electrolyte layer located between the positive electrode layer and the negative electrode layer, and is characterized in that it contains the above-mentioned resin material for solid electrolyte of the present invention.
[0133] This makes it possible to provide a battery containing a solid electrolyte resin material that exhibits stable and excellent ionic conductivity over a wide temperature range, thereby providing a battery that exhibits stable and excellent charge / discharge characteristics over a wide temperature range and has excellent reliability.
[0134] Hereinafter, among batteries, a representative description will be given of an all-solid-state battery as a secondary battery in particular.
[0135] FIG. 1 is a vertical cross-sectional view illustrating a schematic diagram of an example of an all-solid-state battery. As shown in FIG. 1, the all-solid-state battery 10 includes a positive electrode layer 11, a negative electrode layer 12, and a solid electrolyte layer 13 interposed between the positive electrode layer 11 and the negative electrode layer 12.
[0136] The positive electrode layer 11 and the negative electrode layer 12 are each layered, particularly sheet-shaped, and contain a solid electrolyte and an electrode active material, and the solid electrolyte layer 13 is layered, particularly sheet-shaped, and contains a solid electrolyte.
[0137] At least one of the positive electrode layer 11, the negative electrode layer 12, and the solid electrolyte layer 13 contains the solid electrolyte resin material of the present invention as a solid electrolyte.
[0138] In particular, it is preferable that at least the solid electrolyte layer 13 contains the resin material for a solid electrolyte of the present invention, and it is more preferable that both the positive electrode layer 11 and the solid electrolyte layer 13 contain the resin material for a solid electrolyte of the present invention.
[0139] The active material contained in the positive electrode layer 11, i.e., the positive electrode active material, is usually an inorganic material. More specifically, the positive electrode active material is, for example, LiCoO2, LiNiO2, LiMn2O4, Li2Mn2O3, LiCr 0.5 Mn 0.5 Examples of the positive electrode active material include fluorides such as LiFeF3, LiBH4, Li4BN3H, and the like. 10 boron complex compounds such as boron fluoride complexes, iodine complex compounds such as polyvinylpyridine-iodine complexes, and nonmetallic compounds such as sulfur can also be used.
[0140] The active material contained in the negative electrode layer 12, i.e., the negative electrode active material, is usually an inorganic material. More specifically, examples of the negative electrode active material include Nb2O5, V2O5, TiO2, In2O3, ZnO, SnO2, NiO, ITO, AZO, GZO, ATO, FTO, and Li4Ti5O 12 Examples of the negative electrode active material include metals and alloys such as Li, Al, Si, Si-Mn, Si-Co, Si-Ni, Sn, Zn, Sb, Bi, In, and Au, carbon materials such as graphite and hard carbon, LiC 24 Alternatively, a material in which lithium ions are inserted between layers of a carbon material such as LiC6 may be used.
[0141] The resin material for solid electrolytes of the present invention has excellent ionic conductivity by itself and also has excellent adhesion to inorganic materials. Therefore, the resin material for solid electrolytes of the present invention can have excellent adhesion to the active material as described above that comes into contact with the resin material for solid electrolytes, and can effectively prevent unintended poor adhesion, peeling, and the like between them. As a result, the ionic conductivity of the entire all-solid-state battery 10 can be stably excellent for a long period of time.
[0142] In addition, a current collector (not shown) may be provided on the surface of the positive electrode layer 11 opposite to the surface facing the solid electrolyte layer 13, and on the surface of the negative electrode layer 12 opposite to the surface facing the solid electrolyte layer 13.
[0143] The current collector is usually made of an inorganic material as described below. When the portion in contact with the current collector made of such an inorganic material, i.e., the positive electrode layer 11 or the negative electrode layer 12, is made of a material containing the resin material for a solid electrolyte of the present invention, the adhesion between the portion and the current collector can be excellent, and the reliability of the all-solid-state battery 10 can be improved.
[0144] The current collector is a conductor provided to transfer electrons to and from the positive electrode layer 11 and the negative electrode layer 12. The current collector is usually made of a material that has a sufficiently small electrical resistance and whose electrical conductivity characteristics and mechanical structure do not change substantially due to charging and discharging. Specifically, for example, Al, Ti, Pt, Au, Cu, etc. are preferably used, and alloy materials such as stainless steel are also preferably used depending on the application. The shape of the current collector is not particularly limited, and examples thereof include a foil, a plate, a mesh, and the like.
[0145] The all-solid-state battery 10 may be used for any purpose. Examples of electronic devices to which the all-solid-state battery 10 is applied as a power source include mobile phones, smartphones, tablet terminals, video cameras, calculators, electronic game devices, personal computers, digital cameras, and the like. The all-solid-state battery 10 may also be applied to, for example, moving objects such as automobiles. More specifically, the all-solid-state battery 10 can be suitably applied to, for example, storage batteries for electric vehicles, plug-in hybrid vehicles, hybrid vehicles, fuel cell vehicles, and the like. The all-solid-state battery 10 can also be applied to, for example, household power sources, industrial power sources, solar power storage batteries, and the like.
[0146] Although a preferred embodiment of the present invention has been described above, the present invention is not limited to the above, and modifications and improvements within the scope of the present invention that can achieve the object of the present invention are included in the present invention.
[0147] For example, the present invention is not limited to being applied to the all-solid-state battery described above. More specifically, for example, the battery of the present invention may be a battery other than an all-solid-state battery, such as a fuel cell or a redox flow battery. EXAMPLES
[0148] The present invention will be described in detail below based on examples, but the present invention is not limited thereto.
[0149] [5] Manufacturing the second resin component (Production Example 1) First, 91.37 g (404.00 mmol) of the compound represented by the following formula [III] was dissolved in a mixed solvent of 228.86 g of toluene and 276.51 g of ethyl acetate, and the solution was filled into a reaction vessel.
[0150] [ka]
[0151] The solution was sparged with nitrogen for 30 minutes to remove oxygen and then heated to 50° C. Once the solution reached 50° C., a solution of 0.784 g (1.62 mmol) of (η6-toluene)Ni(C6F5)2 in 258.43 g of toluene (prepared in the glove box) was added to the reaction vessel via syringe. The mixture was stirred at 50° C. for 3.0 hours, after which 0.73 g (40.40 mmol) of a 30 wt % aqueous solution of H2O2 was added.
[0152] Next, the above reaction mixture was treated with 21.24 g (353.7 mmol) of acetic acid and 41.38 g (1216.5 mmol) of 30 wt % H2O2 aqueous solution to remove Ni residues, and then washed with water and isopropyl alcohol (IPA).
[0153] The solvent was then removed by evaporation using a rotary evaporator to obtain a polymerization reaction product. The polymerization reaction product was dissolved in the same mass of acetone, and then added to a 14-fold excess amount of heptane and stirred to remove unreacted monomers.
[0154] The product obtained in the above step was dried in a vacuum at 60° C. for 16 hours to isolate 59 g (yield: 60%) of a second resin component represented by the following formula [IV].
[0155] [ka]
[0156] The second resin component obtained as described above had a weight average molecular weight of 150,000, an average degree of polymerization of 370, and a softening point of 105°C.
[0157] (Manufacturing Examples 2 and 3) The second resin components were produced in the same manner as in Production Example 1, except that the reaction conditions were changed so that the weight average molecular weight and softening point conditions were as shown in Table 1.
[0158] (Manufacturing Examples 4 and 5) A second resin component was produced in the same manner as in Production Example 1, except that a compound represented by the following formula [VI] was used instead of the compound represented by the above formula [III], and the reaction conditions were adjusted so that the weight average molecular weight and softening point conditions were as shown in Table 1.
[0159] [ka]
[0160] The second resin components produced in Production Examples 4 and 5 are both represented by the following formula [VII].
[0161] [ka]
[0162] The conditions for each of the second resin components produced in Production Examples 1 to 5 are summarized in Table 1.
[0163] [Table 1]
[0164] [6] Manufacturing of resin materials for solid electrolytes (Example A1) As the first resin component, polyethylene oxide dimethyl ether having a weight average molecular weight of 2,000 (R in the above formula [V]) 5 , R 6In the above, a compound in which each of the groups represented by the formula (I) is a methyl group and the second resin component produced in Production Example 1 were prepared, and these were mixed in a mass ratio of 50:50 to obtain a resin material for a solid electrolyte.
[0165] (Examples A2 to A8) A resin material for a solid electrolyte was produced in the same manner as in Example A1, except that the type of the second resin component was as shown in Table 2 and the mixing ratio of the first resin component and the second resin component was as shown in Table 2.
[0166] (Example A9) As the first resin component, polyethylene oxide dimethyl ether having a weight average molecular weight of 5,000 (R 5 is a methyl group, R 6 A resin material for a solid electrolyte was produced in the same manner as in Example A8, except that a compound in which R is a hydroxyl group was used.
[0167] (Example A10) As the first resin component, polyethylene oxide dimethyl ether having a weight average molecular weight of 8,000 (R in the above formula [V]) 5 , R 6 A resin material for a solid electrolyte was produced in the same manner as in Example A8, except that a compound in which each of the groups represented by the formula (I) was used (wherein each of the groups represented by the formula (I) was a hydroxyl group).
[0168] (Comparative Example A1) Polyethylene oxide dimethyl ether having a weight average molecular weight of 2,000 (R in the above formula [V]) 5 , R 6 In this comparative example, a compound in which each of the first and second resin components is a methyl group was prepared and used as the resin material for the solid electrolyte. That is, the resin material for the solid electrolyte in this comparative example is composed of only the first resin component and does not contain the second resin component.
[0169] (Comparative example A2) The second resin component produced in the above-mentioned Production Example 1 was prepared and used as a resin material for a solid electrolyte in this comparative example. That is, the resin material for a solid electrolyte in this comparative example is composed only of the second resin component and does not contain the first resin component.
[0170] (Comparative example A3) Polyethylene oxide dimethyl ether having a weight average molecular weight of 5,000 (R in the above formula [V]) 5 is a methyl group, R 6 In this comparative example, a compound in which R is a hydroxyl group was prepared and used as a resin material for a solid electrolyte. That is, the resin material for a solid electrolyte in this comparative example is composed of only the first resin component and does not contain the second resin component.
[0171] (Comparative example A4) Polyethylene oxide dimethyl ether having a weight average molecular weight of 8,000 (R in the above formula [V]) 5 , R 6 In this comparative example, a compound in which each of the first and second resin components is a hydroxyl group was prepared and used as a resin material for a solid electrolyte. That is, the resin material for a solid electrolyte in this comparative example is composed of only the first resin component and does not contain the second resin component.
[0172] Table 2 shows the conditions of the resin materials for the solid electrolyte in Examples A1 to A10 and Comparative Examples A1 to A4.
[0173] [Table 2]
[0174] [7] Production of resin material composition for solid electrolyte Example B1 100 parts by mass of the resin material for solid electrolyte obtained in Example A1, 19 parts by mass of Li(CF3SO2)2N(LiTFSI) as a lithium salt, and acetone as a solvent were mixed to obtain a transparent liquid. The liquid was then vacuum dried at 60°C for 1 hour to remove the acetone, and a resin material composition for solid electrolyte was obtained.
[0175] (Examples B2 to B10) A resin material composition for a solid electrolyte was produced in the same manner as in Example B1 except that the resin material for a solid electrolyte obtained in Example A1 was replaced with the resin materials for a solid electrolyte obtained in Examples A2 to A10, and the ratio of the resin material for a solid electrolyte to the lithium salt was set as shown in Table 3.
[0176] (Comparative Examples B1 to B5) A solid electrolyte resin material composition was produced in the same manner as in Example B1, except that the type of solid electrolyte resin material and the ratio of the solid electrolyte resin material to the lithium salt were as shown in Table 3.
[0177] [8] Evaluation [8-1] Ionic conductivity evaluation
[0178] Using each of the solid electrolyte resin material compositions of Examples B1 to B10 and Comparative Examples B1 to B5, the ionic conductivity was evaluated as follows.
[0179] That is, for those rated as ◯ or △ in the evaluation of [8-3] described below, the resin material composition for solid electrolyte obtained in [7] above was formed into a sheet by vacuum pressing at 0.8 MPa and 100° C. for 5 minutes, and then vacuum dried at 60° C. for 15 hours to remove moisture, thereby obtaining a sample sheet. All of the sample sheets obtained in this manner had a residual solvent content of 0.1 mass % or less and a moisture content of 500 ppm or less.
[0180] Using the obtained sample sheet, the ionic conductivity was measured by an AC impedance method at temperatures of 60° C., 45° C., and 30° C. The measurement frequency range was 1 Hz to 50 kHz, and the measurement voltage was 0.5 V.
[0181] On the other hand, for those evaluated as × in the [8-3] described below, the ionic conductivity was measured in the same manner as above using the resin material composition for solid electrolyte obtained in [7] above instead of the sample sheet without forming the sample into a sheet by vacuum pressing or removing the moisture by vacuum drying.
[0182] [8-2] Shape retention evaluation Each of the solid electrolyte resin material compositions of Examples B1 to B10 and Comparative Examples B1 to B5 was attached to a glass plate, and the glass plate was held vertically and left to stand for 24 hours. After 24 hours had passed, it was confirmed whether the solid electrolyte resin material composition deformed under its own weight.
[0183] Those which deformed under their own weight were rated as "X", and those which did not deform under their own weight were rated as "O".
[0184] [8-3] Evaluation of self-supporting film properties For the resin material compositions for solid electrolytes that were evaluated as "good" in [8-2] above, a vacuum press was performed at 0.8 MPa and 100°C for 5 minutes, and then the compositions were vacuum dried at 60°C for 15 hours to remove moisture, thereby attempting to manufacture a film-shaped molded product. Here, the samples in which a film-like molded product was not obtained were evaluated as "x".
[0185] The film-like molded articles obtained were curved to fit the outer periphery of a rod having a diameter of 13 mm.
[0186] Here, samples in which cracks or irreversible deformation occurred were rated as "△", and samples in which cracks or irreversible deformation did not occur were rated as "◯".
[0187] These results are summarized in Table 3 together with the configurations of the solid electrolyte resin material compositions of Examples B1 to B10 and Comparative Examples B1 to B5. In Table 3, with regard to the ratio of the solid electrolyte resin material and the lithium salt in the solid electrolyte resin material composition, the ratio of the total number of oxygen atoms contained in the solid electrolyte resin material contained in the solid electrolyte resin material composition to the total number of lithium atoms contained in the lithium salt contained in the solid electrolyte resin material composition is shown as "[O] / [Li]", and the ratio by mass of the content of the solid electrolyte resin material to the content of the lithium salt in the solid electrolyte resin material composition is shown as "mass ratio".
[0188] [Table 3]
[0189] As is clear from Table 3, it was confirmed that each of the Examples B1 to B10 exhibited stable and excellent ion conductivity over a wide temperature range compared to the Comparative Examples B1 to B5. It was also confirmed that the Examples B1 to B6, B9, and B10 had particularly excellent shape retention, and the Examples B1 to B6 had particularly excellent free-standing film properties.
[0190] In addition, the weight average molecular weight of the first resin component was within a range of 1,000 to 50,000, the weight average molecular weight of the second resin component was within a range of 3,000 to 200,000, the average degree of polymerization of the second resin component was within a range of 10 to 900, the softening point of the second resin component was within a range of -30°C to 150°C, and the content of the first resin component in the resin material for solid electrolyte was X1 [mass%], and the content of the second resin component was X2 [mass%], and the value of X2 / X1 was within a range of 0.10 to 9.00. A resin material for solid electrolyte and a resin material composition for solid electrolyte were produced in the same manner as in the above-mentioned Examples, and evaluation was performed in the same manner as above, and excellent results were obtained as above.
[0191] In addition, resin material compositions for solid electrolytes were produced in the same manner as in the above Examples, except that the ratio of the total number of oxygen atoms contained in the resin material for solid electrolytes contained in the resin material composition for solid electrolytes to the total number of lithium atoms contained in the lithium salt contained in the resin material composition for solid electrolytes was variously changed within the range of 4.0 to 33.3, and evaluations were performed in the same manner as above, and excellent results were obtained as above. [Explanation of symbols]
[0192] 10: All-solid-state battery 11: Positive electrode layer 12: Negative electrode layer 13: Solid electrolyte layer
Claims
1. A polyethylene oxide compound as a first resin component; a second resin component having a norbornene-derived structure in its main chain and an ethylene oxide structure in its side chain.
2. The resin material for a solid electrolyte according to claim 1 , wherein the second resin component contains a monomer component represented by the following formula (NB): 【Chemistry 1】 (In formula (NB), R 1 is a hydrogen atom or a hydrocarbon group, R 2 , R 3 and R 4 are each independently a hydrogen atom or an organic group having 1 to 3 carbon atoms, n is an integer of 1 or more, 1 is 0, 1 or 2.)
3. 3. The resin material for a solid electrolyte according to claim 2, wherein n in the formula (NB) is an integer of 2 or more and 6 or less.
4. 4. The resin material for a solid electrolyte according to claim 1, wherein the second resin component has a weight average molecular weight of 3,000 or more and 300,000 or less.
5. 4. The resin material for a solid electrolyte according to claim 1, wherein the average degree of polymerization of the second resin component is 10 or more and 1,350 or less.
6. 4. The resin material for a solid electrolyte according to claim 1, wherein the second resin component has a softening point of -30° C. or more and 150° C. or less.
7. 4. The resin material for a solid electrolyte according to claim 1, wherein the first resin component has a weight average molecular weight of 500 or more and 100,000 or less.
8. 4. The resin material for solid electrolyte according to claim 1, wherein, when a content of the first resin component in the resin material for solid electrolyte is X1 [mass%] and a content of the second resin component in the resin material for solid electrolyte is X2 [mass%], a relationship of 0.10≦X2 / X1≦9.00 is satisfied.
9. A resin material composition for a solid electrolyte, comprising the resin material for a solid electrolyte according to claim 1 and a lithium salt.
10. The lithium salt is LiSCN, LiN(CN) 2 , LiClO 4 , LiBF 4 , LiAsF 6 , LiPF 6 , LiCF 3 SO 3 , Li(CF 3 SO 2 ) 2 N, Li(CF 3 SO 2 ) 3 C, LiSbF 6 , Li(FSO 2 ) 2 N, LiC 4 F 9 SO 3 , LiN(SO 2 CF 2 CF 3 ) 2 , LiPF 3 (CF 2 CF 3 ) 3 , LiPF 3 (C 2 F 5 ) 3 , LiPF 3 (CF 3 ) 3 , LiCl, LiF, LiBr, LiI, LiB(C 2 O 4 ) 2 10. The resin material composition for solid electrolytes according to claim 9, wherein the compound is at least one selected from the group consisting of lithium difluoro(oxalato)borate and lithium bis(oxalato)borate.
11. 10. A resin material composition for a solid electrolyte according to claim 9, wherein a ratio of a total number of oxygen atoms contained in the resin material for a solid electrolyte contained in the resin material composition for a solid electrolyte to a total number of lithium atoms contained in the lithium salt contained in the resin material composition for a solid electrolyte is 4.0 or more and 33.3 or less.
12. A sheet material comprising a material containing the resin material for a solid electrolyte according to claim 1 .
13. A positive electrode layer; A negative electrode layer; a battery comprising an electrolyte layer located between the positive electrode layer and the negative electrode layer, A battery comprising the resin material for a solid electrolyte according to any one of claims 1 to 3.
Citation Information
Patent Citations
All-solid-state battery
WO2014002858A1