Fiber resin composite sheet, accessory, and vehicle interior material
The fiber resin composite sheet with a 4-methyl-1-pentene copolymer impregnated into a fiber aggregate addresses poor bendability and fuzz issues, ensuring flexibility and recovery while maintaining mechanical strength.
Patent Information
- Application Number
- JP2024026897
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-15
- Filing Date
- 2024-02-26
- Publication Date
- 2024-10-01
AI Technical Summary
Fiber-reinforced plastics with thermoplastic elastomers exhibit poor bendability and texture due to complete resin impregnation, leading to fuzz generation and poor mechanical properties, especially when cut.
A fiber resin composite sheet with a 4-methyl-1-pentene copolymer impregnated into a fiber aggregate, having a porosity of 36% or less, with specific molecular and viscoelastic properties to prevent fuzz and enhance flexibility and recovery.
The composite sheet minimizes fuzz on cuts, allows easy bending and recovery, and reduces wrinkles and dents over time, maintaining mechanical strength and flexibility.
Smart Images

Figure 2024132913000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a fiber-resin composite sheet, a piece of jewelry, and an interior material for an automobile. [Background technology]
[0002] Fiber-reinforced plastics are known. Fiber-reinforced plastics include fibers and a resin composition impregnated in the fibers. Molded products of fiber-reinforced plastics have excellent strength. In addition, molded products of fiber-reinforced plastics have a property of being difficult to bend.
[0003] On the other hand, depending on the application, such as daily necessities and automotive interior materials, fiber reinforced plastics may be required to have a property of being easily bent (easy bending). In addition, these applications may require a property of being easily restored after bending (bending recovery). Therefore, fiber resin composite sheets in which a thermoplastic resin is laminated to a woven fabric have been researched as fiber reinforced plastics that are easy to bend and restore to their original shape after bending.
[0004] As a bendable fiber resin composite sheet, Patent Document 1 describes a carbon fiber reinforced resin processed sheet in which a thermoplastic elastomer film or a rubber film is laminated on both sides of a carbon fiber fabric. Patent Document 2 describes a composite membrane material in which a polyurethane thermoplastic elastomer or soft polyvinyl chloride (soft PVC) is thermally laminated as a thermoplastic elastomer to a woven fabric of polyester fiber, carbon fiber, aramid fiber, or the like. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2016-179667 A [Patent Document 2] Patent Publication No. 2022-242085 Summary of the Invention [Problem to be solved by the invention]
[0006] In the fiber-resin composite sheet that mainly uses the thermoplastic elastomer, the thermoplastic elastomer has polarity, so it has good adhesion to the sizing agent on the carbon fiber surface, and can exhibit high mechanical strength. However, in particular in carbon fiber resin-processed sheets laminated with polyurethane-based thermoplastic elastomers, the resin is often only impregnated on the surface because the material becomes too hard and has poor bendability and feel if it is completely impregnated to the inside. This can cause the ends of the fibers to come out of the resin from the cut surface when the sheet is cut (generating fluff), which can cause itching, etc.
[0007] In view of the above problems, an object of the present invention is to provide a fiber-resin composite sheet which is less susceptible to fuzzing on the cut surfaces of the sheet. [Means for solving the problem]
[0008] One aspect of the present invention for solving the above problems relates to a fiber-resin composite sheet according to the following items [1] to [6]. [1] A fiber-resin composite sheet comprising a fiber assembly and a resin composition impregnated into the fiber assembly, The resin composition contains a 4-methyl-1-pentene copolymer (A) that satisfies the following requirement (Aa): When the porosity of the fiber-resin composite sheet is defined as a ratio of an area of an unimpregnated portion in which the fiber aggregate is not impregnated with the resin composition to an area of the fiber-resin composite sheet in a cross section cut in the thickness direction of the fiber-resin composite sheet, the porosity is 36% or less. Fiber-resin composite sheet. (Aa) The content of the structural unit (P) derived from 4-methyl-1-pentene is 65 mol% or more and less than 90 mol%, and the content of the structural unit (AQ) derived from a monomer selected from the group consisting of ethylene and linear or branched α-olefins having 3 to 20 carbon atoms (excluding 4-methyl-1-pentene) is more than 10 mol% and 35 mol% or less. [2] The structural unit (AQ) includes a structural unit derived from a monomer selected from the group consisting of ethylene and an α-olefin having 3 to 4 carbon atoms. The fiber-resin composite sheet according to [1]. [3] The porosity is 20% or less. The fiber-resin composite sheet according to [1] or [2]. [4] The 4-methyl-1-pentene copolymer (A) further satisfies the following requirement (Ab): The fiber-resin composite sheet according to any one of [1] to [3]. (Ab) No melting point (Tm) was observed by differential scanning calorimetry (DSC) [5] The 4-methyl-1-pentene copolymer (A) further satisfies the following requirements (Ac) and (Ad): The fiber-resin composite sheet according to [4]. (Ac) The peak temperature of the loss tangent tanδ obtained by dynamic viscoelasticity measurement in the temperature range of -40 to 150°C and at a frequency of 10 rad / s (1.6 Hz) is 15°C to 45°C. (Ad) The peak value of the loss tangent tanδ obtained by dynamic viscoelasticity measurement in the temperature range of -40 to 150°C and the frequency of 10 rad / s (1.6 Hz) is in the range of 1.0 to 5.0. [6] The fiber assembly contains carbon fibers. The fiber-resin composite sheet according to any one of [1] to [5].
[0009] Another aspect of the present invention for solving the above problem relates to the following accessory [7]. [7] An ornament comprising the fiber resin composite sheet according to any one of [1] to [6].
[0010] Another aspect of the present invention for solving the above problems relates to an automobile interior material as described below in [8]. [8] An automobile interior material comprising the fiber-resin composite sheet according to any one of [1] to [6]. Effect of the Invention
[0011] The fiber-resin composite sheet of the present invention is less susceptible to fuzzing on the cut surfaces of the sheet. [Brief description of the drawings]
[0012] [Figure 1] 1A, 1B, and 1C are images obtained by photographing cross sections of the sheets of Example 1, Example 2, and Comparative Example 1 near the center in the thickness direction with an SEM and trimming the images from the surface to the inside of the sheet, focusing on the void portion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, an example of a preferred embodiment of the present invention will be disclosed and described in detail.
[0014] The following description and examples are illustrative of embodiments and are not intended to limit the scope of the invention. In the present disclosure, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the lower and upper limits. In the present disclosure, in which numerical ranges are described in stages, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. In addition, in the numerical ranges described in this disclosure, the upper or lower limit value described in a certain numerical range may be replaced with a value shown in the Examples. In this disclosure, when a plurality of substances corresponding to each component are present in the composition, the amount of each component in the composition means the total amount of the plurality of substances present in the composition, unless otherwise specified. In the present disclosure, "mass %" and "weight %" are synonymous, and "parts by mass" and "parts by weight" are synonymous.
[0015] <Fiber-resin composite sheet> The fiber-resin composite sheet of the present invention will now be described.
[0016] The fiber resin composite sheet of the present invention includes a resin composition containing a 4-methyl-1-pentene copolymer (A) impregnated into a fiber assembly. In a cross section of the fiber resin composite sheet cut in the thickness direction, the ratio of the area of the unimpregnated portion where the fiber assembly is not impregnated with the resin composition to the area of the fiber resin composite sheet (porosity) is 36% or less. Here, the 4-methyl-1-pentene copolymer (A) has a content of structural units (P) derived from 4-methyl-1-pentene of 65 mol% or more and less than 90 mol%, and a content of structural units (AQ) derived from ethylene and linear or branched α-olefins having 3 to 20 carbon atoms (excluding 4-methyl-1-pentene) of more than 10 mol% and 35 mol% or less.
[0017] When the fiber-resin composite sheet contains the resin composition containing the 4-methyl-1-pentene copolymer (A) and has a porosity of 36% or less, fuzz is unlikely to be generated on the cut surface of the fiber-resin composite sheet, and therefore, even if the fiber-resin composite sheet is bent under load, cracks, wrinkles, bending marks and dents on the appearance tend to disappear over time.
[0018] The porosity is preferably 20% or less, more preferably 15% or less, and even more preferably 10% or less. The lower limit of the above ratio is not particularly limited, but can be 0% or more. A low porosity means that the resin composition is sufficiently impregnated into the center of the fiber assembly, or the resin is sufficiently impregnated around the fibers. If the resin is sufficiently impregnated around the fibers, the ends of the fibers cut short when cut are less likely to protrude from the resin (fuzzing is less likely to occur).
[0019] Furthermore, from the viewpoint of preventing wrinkles, folding marks and dents from occurring in the fiber-resin composite sheet even immediately after bending or releasing a load, the porosity may be 20% to 24%.
[0020] The porosity was calculated by the following measurement and analysis methods.
[0021] An arbitrary cross section of the fiber resin composite sheet is observed with a high-resolution scanning microscope (SEM). A secondary image is created by using an enlarged image obtained by observation at a magnification of 500 times, and trimming so that only the fiber resin composite sheet from the front surface to the back surface of the fiber aggregate / resin composition remains in the image. The obtained secondary image is loaded into image analysis software (ImageJ), and the commands: Process, Binary, Make Binary are executed to perform binarized image processing. At this time, the areas filled with the fiber aggregate and the resin composition are painted white, and the void areas are painted black. At this time, in order to paint the resin composition area white, the threshold is controlled with the commands: Image, Adjust, Threshold. Next, the area fraction of the void area (area fraction of the white area) excluding the fiber aggregate and the resin composition in the area of the observation field is calculated with the commands: Analyse, Analyze.
[0022] The magnification for observing the porosity may be changed depending on the type of fiber-resin composite sheet, and is determined so that the entire thickness of the sheet fits within the vertical direction of the observation field.
[0023] The fiber-resin composite sheet of the present invention contains a resin composition containing a 4-methyl-1-pentene copolymer (A). The 4-methyl-1-pentene copolymer (A), other polymers (B) and other components that may be contained in the resin composition will be described below.
[0024] <4-methyl-1-pentene copolymer (A)> The 4-methyl-1-pentene copolymer (A) satisfies the following requirement (Aa). In addition, it is preferable that the copolymer further satisfies one or any of the following requirements (Ab) to (Ad).
[0025] The 4-methyl-1-pentene copolymer (A) that satisfies the following requirements enhances the stress relaxation property of the resin composition. Therefore, the 4-methyl-1-pentene copolymer (A) slowly flows the resin composition and returns it to its original shape after the fiber-resin composite sheet is folded or further loaded. As a result, the 4-methyl-1-pentene copolymer (A) causes wrinkles, folding marks, and dents that occur due to the folding or loading to disappear over time.
[0026] In addition, a resin composition containing a 4-methyl-1-pentene copolymer (A) that satisfies the following requirements easily penetrates into minute irregularities present on the surface of a fiber assembly, and therefore easily adheres to the fiber assembly even if the 4-methyl-1-pentene copolymer (A) does not have a polar site. Therefore, even if the porosity of the 4-methyl-1-pentene copolymer (A) is not 0% (a state in which the fiber assembly is completely impregnated with the resin composition), fluffing during cutting can be suppressed.
[0027] Requirement (Aa): The 4-methyl-1-pentene copolymer (A) has a content of structural units (P) derived from 4-methyl-1-pentene of 65 mol % or more and less than 90 mol %, and a content of structural units (AQ) derived from ethylene or a linear or branched α-olefin having 3 to 20 carbon atoms other than 4-methyl-1-pentene of more than 10 mol % and not more than 35 mol %.
[0028] The content of the structural unit (P) is 65 mol% or more and less than 90 mol%, and from the viewpoint of making it easier for wrinkles, bending marks, and dents caused by bending or loading to disappear over time, the content is preferably 68 mol% or more and less than 90 mol%, more preferably 68 mol% or more and less than 88 mol%, and particularly preferably 68 mol% or more and less than 80 mol%.
[0029] The content of the structural unit (AQ) (when there are two or more types of structural units (AQ), the total content of said two or more types) is more than 10 mol% and not more than 35 mol%, and from the viewpoint of making it easier to eliminate wrinkles, bending marks, and dents caused by bending or loading over time, it is preferably more than 10 mol% and not more than 32 mol%, more preferably more than 12 mol% and not more than 32 mol%, and particularly preferably more than 20 mol% and not more than 32 mol%.
[0030] As the linear or branched α-olefin having 3 to 20 carbon atoms other than ethylene and 4-methyl-1-pentene, which forms the structural unit (AQ), from the viewpoint of reducing the anisotropy of the tensile elongation at break and the anisotropy of the tear strength, ethylene, propylene, 1-butene, 1-hexene, 1-octene, 1-decene, 1-hexadecene, and 1-octadecene are preferred, ethylene and α-olefins having 3 to 4 carbon atoms, i.e., ethylene, propylene, and 1-butene, are more preferred, and propylene is particularly preferred. In other words, the structural unit (AQ) is preferably a structural unit derived from ethylene or an α-olefin having 3 to 4 carbon atoms, and particularly preferably a structural unit derived from propylene.
[0031] Furthermore, when ethylene or a linear or branched α-olefin having 3 to 20 carbon atoms is used as a monomer from which the structural unit (AQ) is derived, the flexibility and relaxivity of the resulting fiber resin composite sheet are improved.
[0032] The ethylene and linear or branched α-olefins from which the structural unit (AQ) is derived may be used alone or in combination of two or more kinds.
[0033] The 4-methyl-1-pentene copolymer (A) may contain other structural units besides the structural unit (P) derived from 4-methyl-1-pentene and the structural unit (AQ) derived from ethylene or a linear or branched α-olefin having 3 to 20 carbon atoms other than 4-methyl-1-pentene, within a range that does not impair the effects of the present invention. The content of the other structural units is, for example, 0 to 10 mol%.
[0034] Monomers from which the above-mentioned other structural units are derived include cyclic olefins, aromatic vinyl compounds, conjugated dienes, non-conjugated polyenes, functional vinyl compounds, hydroxyl group-containing olefins, halogenated olefins, and the like.
[0035] As the cyclic olefin, aromatic vinyl compound, conjugated diene, non-conjugated polyene, functional vinyl compound, hydroxyl group-containing olefin, and halogenated olefin, for example, the compounds described in paragraphs 0035 to 0041 of JP2013-169685A can be used.
[0036] As the monomers forming the other structural units, vinylcyclohexane and styrene are particularly preferred.
[0037] When the 4-methyl-1-pentene copolymer (A) contains the other structural units, it may contain only one type of the other structural units, or it may contain two or more types of the other structural units.
[0038] The content (mol%) of each structural unit in the 4-methyl-1-pentene copolymer (A) is determined under the conditions described in the examples described later. 13 This was measured using a C-NMR measurement method.
[0039] Requirements(Ab): In the measurement of the 4-methyl-1-pentene copolymer (A) by differential scanning calorimetry (DSC), the melting point (Tm) is not observed or is in the range of 100°C to 199°C.
[0040] It is preferable that the above melting point (Tm) of the 4-methyl-1-pentene copolymer (A) is not observed.
[0041] When the melting point (Tm) of the 4-methyl-1-pentene copolymer (A) is within the above range, the fiber-resin composite sheet becomes more flexible and is less susceptible to cracks or breakage when bent. When the melting point (Tm) of the 4-methyl-1-pentene copolymer (A) is not observed, the fiber-resin composite sheet is even less susceptible to cracks or breakage when bent.
[0042] Requirements(Ac): The 4-methyl-1-pentene polymer (A) has a peak temperature of loss tangent tanδ (hereinafter also referred to as "tanδ peak temperature") of 15°C to 45°C, determined by dynamic viscoelasticity measurement at a frequency of 10 rad / s (1.6 Hz) in a temperature range of -40 to 150°C.
[0043] The tan δ peak temperature of the 4-methyl-1-pentene polymer (A) is more preferably from 20°C to 45°C, and further preferably from 25°C to 45°C.
[0044] When the tan δ peak temperature of the 4-methyl-1-pentene polymer (A) is within the above range, the fiber-resin composite sheet has high room temperature relaxability, and therefore is likely to slowly return to its original shape after being bent or further loaded when used at room temperature, and wrinkles, bending marks and dents when used at room temperature are likely to disappear over time.
[0045] Requirements(Ad): The 4-methyl-1-pentene polymer (A) has a maximum value of loss tangent tanδ (hereinafter also referred to as "peak value of tanδ") of 1.0 to 5.0, which is obtained by performing dynamic viscoelasticity measurement in a temperature range of -40 to 150°C at a frequency of 10 rad / s (1.6 Hz).
[0046] The tan δ peak temperature of the 4-methyl-1-pentene polymer (A) is preferably 1.5 to 5.0, more preferably 2.0 to 4.0. When the tan δ peak temperature of the 4-methyl-1-pentene polymer (A) is within the above range, wrinkles, folding marks and dents in the fiber-resin composite sheet tend to disappear over time during use, particularly after a long period of time.
[0047] The 4-methyl-1-pentene copolymer (A) preferably satisfies one or more of the following requirements (Ae) to (Ah), more preferably satisfies two or more of the requirements (Ae) to (Ah), and particularly preferably satisfies all of the requirements (Ae) to (Ah).
[0048] Requirements(Ae): The intrinsic viscosity [η] of the 4-methyl-1-pentene copolymer (A) measured in a decalin solvent at 135°C is 0.5 to 4.0 dl / g.
[0049] The intrinsic viscosity [η] of the 4-methyl-1-pentene copolymer (A) is more preferably from 0.5 dl / g to 3.5 dl / g, and further preferably from 1.0 dl / g to 3.5 dl / g.
[0050] When the intrinsic viscosity [η] of the 4-methyl-1-pentene copolymer (A) is within the above range, the moldability of the fiber resin composite sheet is good.
[0051] The intrinsic viscosity [η] of the 4-methyl-1-pentene copolymer (A) is a value measured by the method described in the examples described later.
[0052] Requirements(Af): The molecular weight distribution (Mw / Mn) of the 4-methyl-1-pentene copolymer (A) is 1.0 to 3.5.
[0053] The Mw / Mn of the 4-methyl-1-pentene copolymer (A) is more preferably 1.1 to 3.0.
[0054] When the Mw / Mn of the 4-methyl-1-pentene copolymer (A) is within the above range, the fiber resin composite sheet is less likely to become sticky and tends to have a good appearance.
[0055] The weight average molecular weight (Mw) of the 4-methyl-1-pentene copolymer (A) is 1×10 4 ~2×10 6 Preferably, the concentration is 1×10 4 ~1×10 6 It is more preferable that:
[0056] The weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn) of the 4-methyl-1-pentene copolymer (A) are values calculated by the method described in the examples below.
[0057] Requirements (Ag): The density of the 4-methyl-1-pentene copolymer (A), measured in accordance with JIS K7112-2:2023 (density gradient tube method), is 830 kg / m from the viewpoint of handling. 3 ~860kg / m 3 is
[0058] The density of the 4-methyl-1-pentene copolymer (A) is 830 kg / m 3 ~850kg / m 3 It is more preferable that:
[0059] When the density of the 4-methyl-1-pentene copolymer (A) is within the above range, the fiber-resin composite sheet has good handleability.
[0060] Requirements (Ah): The melt flow rate (MFR) of the 4-methyl-1-pentene copolymer (A), measured in accordance with ASTM D1238 at 230°C under a load of 2.16 kg or at 260°C under a load of 5.0 kg, is preferably 0.1 g / 10 min to 100 g / 10 min, more preferably 0.5 g / 10 min to 50 g / 10 min, and even more preferably 0.5 g / 10 min to 30 g / 10 min, from the viewpoint of excellent fuzz resistance and excellent resistance to crease and wrinkle return of the fiber-resin composite sheet.
[0061] When the MFR of the 4-methyl-1-pentene copolymer (A) is within the above range, fuzz is unlikely to occur on the cut surface of the fiber-resin composite sheet, and even if the fiber-resin composite sheet is folded or subjected to a load, wrinkles, folding marks and dents are unlikely to occur in the appearance, and even if they do occur, they tend to disappear over time.
[0062] (Method for producing 4-methyl-1-pentene copolymer (A)) The method for producing the 4-methyl-1-pentene copolymer (A) is not particularly limited, but for example, it can be produced by polymerizing 4-methyl-1-pentene and the above-mentioned ethylene or a linear or branched α-olefin having 3 to 20 carbon atoms (excluding 4-methyl-1-pentene) in the presence of a suitable polymerization catalyst such as a magnesium-supported titanium catalyst or a metallocene catalyst.
[0063] Here, examples of polymerization catalysts that can be used include conventionally known catalysts, such as magnesium-supported titanium catalysts, metallocene catalysts described in International Publication No. 01 / 53369, International Publication No. 01 / 27124, JP-A-3-193796, JP-A-2-41303, International Publication No. 2011 / 055803, International Publication No. 2014 / 050817, etc. Polymerization can be appropriately selected from liquid phase polymerization methods including solution polymerization and suspension polymerization, and gas phase polymerization methods.
[0064] In the liquid phase polymerization method, an inert hydrocarbon solvent can be used as the solvent that constitutes the liquid phase.Examples of the inert hydrocarbon include aliphatic hydrocarbons including propane, butane, pentane, hexane, heptane, octane, decane, dodecane, and kerosene, alicyclic hydrocarbons including cyclopentane, cyclohexane, methyl-cyclopentane, and methyl-cyclohexane, aromatic hydrocarbons including benzene, toluene, and xylene, and halogenated hydrocarbons including ethylene chloride, chlorobenzene, dichloromethane, trichloromethane, and tetrachloromethane, and mixtures thereof.
[0065] Furthermore, in the liquid phase polymerization method, bulk polymerization can also be performed using a monomer corresponding to the structural unit (P) derived from the aforementioned 4-methyl-1-pentene (i.e., 4-methyl-1-pentene), or a monomer corresponding to the structural unit (AQ) derived from the aforementioned ethylene or a linear or branched α-olefin having 3 to 20 carbon atoms (excluding 4-methyl-1-pentene) (i.e., the aforementioned ethylene or a linear or branched α-olefin having 3 to 20 carbon atoms (4-methyl-1-pentene) itself as a solvent.
[0066] By stepwise copolymerizing the above 4-methyl-1-pentene with the above ethylene or a linear or branched α-olefin having 3 to 20 carbon atoms (excluding 4-methyl-1-pentene), it is possible to appropriately control the composition distribution of the structural units (P) derived from 4-methyl-1-pentene and the structural units (AQ) derived from ethylene or a linear or branched α-olefin having 3 to 20 carbon atoms (excluding 4-methyl-1-pentene) constituting the 4-methyl-1-pentene copolymer (A).
[0067] The polymerization temperature is preferably −50 to 200° C., more preferably 0 to 100° C., and further preferably 20 to 100° C. The polymerization pressure is preferably normal pressure to 10 MPa gauge pressure, and more preferably normal pressure to 5 MPa gauge pressure.
[0068] During polymerization, hydrogen may be added for the purpose of controlling the molecular weight and polymerization activity of the polymer produced. The amount of hydrogen added is appropriately about 0.001 to 100 NL per 1 kg of the total amount of the above-mentioned 4-methyl-1-pentene and the above-mentioned amount of ethylene or linear or branched α-olefin having 3 to 20 carbon atoms (excluding 4-methyl-1-pentene).
[0069] (4-methyl-1-pentene copolymer (A) content) The content of the 4-methyl-1-pentene copolymer (A) is preferably 30% by mass or more and 100% by mass or less, more preferably 50% by mass or more and 100% by mass or less, and even more preferably 60% by mass or more and 100% by mass or less, based on the total mass of the resin composition.
[0070] When the content of the 4-methyl-1-pentene copolymer (A) is within the above range, fuzz is less likely to occur from the cut surface of the fiber-resin composite sheet, and wrinkles, folding marks and dents when the fiber-resin composite sheet is folded or subjected to a load are more likely to disappear over time.
[0071] <Other polymers (B)> The fiber-resin composite sheet of the present invention may contain, in addition to the 4-methyl-1-pentene copolymer (A), other polymers (hereinafter referred to as "other polymers (B)") within the scope of not impairing the effects of the present invention. Examples of the other polymers (B) include thermoplastic polyolefin resins such as low-density polyethylene, medium-density polyethylene, high-density polyethylene, high-pressure low-density polyethylene, polypropylene, poly-1-butene, poly-4-methyl-1-pentene (excluding 4-methyl-1-pentene copolymers satisfying requirement (Aa)), poly-3-methyl-1-butene, ethylene-α-olefin copolymers, propylene-α-olefin copolymers, 1-butene-α-olefin copolymers, cyclic olefin copolymers, and chlorinated polyolefins; thermoplastic polyamide resins such as aliphatic polyamides (nylon 6, nylon 11, nylon 12, nylon 66, nylon 610, and nylon 612) and polyether block amide copolymers; thermoplastic polyester resins such as polyethylene terephthalate and polybutylene terephthalate; polystyrene, ABS resins, and ABS resins. Thermoplastic vinyl aromatic resins such as S resin; fluorine-based resins such as vinyl chloride resin, vinylidene chloride resin, acrylic resin, ethylene-vinyl acetate copolymer, ethylene-(meth)acrylate copolymer, ionomer, ethylene-vinyl alcohol copolymer, polyvinyl alcohol, polyvinyl fluoride resin, polytetrafluoroethylene, polyvinylidene fluoride, ETFE, polycarbonate, polyacetal, polyphenylene oxide, polyphenylene sulfide, polyimide, polyarylate, polysulfone, polyether sulfone, rosin-based resin, terpene-based resin, and thermoplastic elastomers such as petroleum resin olefin-based elastomer, styrene-based elastomer, acid-modified styrene-based elastomer, vinyl chloride-based elastomer, urethane-based elastomer, ester-based elastomer, amide-based elastomer, etc. These resins may be used alone or in combination of two or more.
[0072] The other polymer (B) is preferably a thermoplastic elastomer, more preferably an olefin-based elastomer (B-1) or a styrene-based elastomer (B-2), and even more preferably a styrene-based elastomer (B-2).
[0073] (Olefin elastomer (B-1)) A first embodiment of the olefin-based elastomer (B-1) includes a copolymer of ethylene or propylene with butadiene, hydrogenated butadiene, isoprene, hydrogenated isoprene isobutylene, or an α-olefin.
[0074] The form of copolymerization may be either block copolymerization or graft copolymerization, but a copolymer consisting of ethylene or propylene and an α-olefin may be a random copolymerization.
[0075] As the α-olefin, 1-butene, 1-octene, etc. are preferably used.
[0076] Examples of the olefin elastomer (B-1) include block copolymers of polyolefin blocks forming highly crystalline polymers such as polypropylene, which serve as the hard portion, and amorphous monomer copolymers, which serve as the soft portion. Specific examples include olefin (crystalline)-ethylene-butylene-olefin block copolymers and propylene-olefin (amorphous)-propylene block copolymers.
[0077] Specific examples of the first embodiment of the olefin-based elastomer (B-1) include those commercially available under the trade name: DYNARON (registered trademark) from JSR Corporation, trade names: TAFMER (registered trademark) and NOTIO (registered trademark) from Mitsui Chemicals, Inc., trade names: ENGAGE (registered trademark) and VERSIFY (registered trademark) from The Dow Chemical Company, and trade name: Vistamaxx (registered trademark) from ExxonMobil Chemical Corporation.
[0078] A second embodiment of the olefin elastomer (B-1) is a blend of one selected from the group consisting of polyethylene and polypropylene with one selected from the group consisting of ethylene-propylene copolymer, ethylene-propylene-diene copolymer, ethylene-butene copolymer, and hydrogenated styrene-butadiene. Such a blend is preferably one in which the partially or completely crosslinked ethylene-propylene copolymer, ethylene-propylene-diene copolymer, and ethylene-butene copolymer exist as islands in the phase selected from the group consisting of polyethylene and polypropylene by blending in the presence of a crosslinking agent.
[0079] Specific examples of the second embodiment of the olefin-based elastomer (B-1) include those commercially available under the trade name: Milastomer (registered trademark) from Mitsui Chemicals, Inc., the trade name: Esporex (registered trademark) from Sumitomo Chemical Co., Ltd., the trade names: Thermorun (registered trademark) and ZELAS (registered trademark) from Mitsubishi Chemical Corporation, and the trade name: Santoplene (registered trademark) from ExxonMobil Chemical Company.
[0080] The olefin elastomer (B-1) may be modified to have an acid anhydride group, a carboxyl group, an amino group, an imino group, an alkoxysilyl group, a silanol group, a silyl ether group, a hydroxyl group or an epoxy group.
[0081] (Styrene-based elastomer (B-2)) Examples of styrene-based elastomers (B-2) include block copolymers (SBS) of polystyrene blocks that form the hard portion (crystalline portion) and diene monomer blocks that form the soft portion, hydrogenated styrene-butadiene-styrene block copolymers (HSBR), styrene-ethylene-propylene-styrene block copolymers (SEPS), styrene-ethylene-butene-styrene block copolymers (SEBS), styrene-isoprene-styrene block copolymers (SIS), styrene-isobutylene-styrene copolymers (SIBS), and styrene-isobutylene copolymers (SIB).
[0082] The styrene-based elastomer (B-2) may be used alone or in combination of two or more kinds.
[0083] A specific example of the hydrogenated styrene-butadiene-styrene block copolymer (HSBR) is one sold by JSR Corporation under the trade name Dynaron (registered trademark).
[0084] Styrene-ethylene-propylene-styrene block copolymer (SEPS) is obtained by hydrogenating styrene-isoprene-styrene block copolymer (SIS). Specific examples of SIS include those commercially available under the trade name JSR SIS (registered trademark) from JSR Corporation, under the trade name Hybra (registered trademark) from Kuraray Co., Ltd., and under the trade name Kraton D (registered trademark) from Shell Corporation.
[0085] Specific examples of styrene-ethylene-propylene-styrene block copolymers (SEPS) include those commercially available under the trade name: Septon (registered trademark) from Kuraray Co., Ltd., or under the trade name: Kraton (registered trademark) from Shell Corporation.
[0086] Specific examples of styrene-ethylene-butene-styrene block copolymers (SEBS) include those commercially available from Asahi Kasei Corporation under the trade name Tuftec (registered trademark) or from Shell Corporation under the trade name Kraton (registered trademark).
[0087] Specific examples of styrene-isobutylene copolymers (SIB) and styrene-isobutylene-styrene copolymers (SIBS) include those commercially available from Kaneka Corporation under the trade name SIBSTAR (registered trademark).
[0088] Furthermore, among the styrene-based elastomers (B-2), vinyl SIS (product name: Hybler, brand 5127) and vinyl SEPS (product name: Hybler, brand 7125) manufactured by Kuraray Co., Ltd., and SEBS (product name: SOE, brands: S1605, S1611, and L609) manufactured by Asahi Kasei Corporation, which have moderate compatibility with the 4-methyl-1-pentene copolymer (A), can also be preferably used from the viewpoints of compatibility, the temperature range showing the maximum value of the loss tangent, and the magnitude of the maximum value of the loss tangent.
[0089] (Content of other polymers (B)) The content of the other polymer (B) is not particularly limited, but is preferably 0.5% by mass or more, more preferably 1% by mass or more, even more preferably 2% by mass or more, even more preferably 3% by mass or more, and is preferably 65% by mass or less, more preferably 60% by mass or less, even more preferably 55% by mass or less, even more preferably 50% by mass or less, and particularly preferably 45% by mass or less, based on 100 parts by mass of the total of the above (A) and the other polymer (B). It is preferably 0.5% by mass to 65% by mass, more preferably 0.5% by mass to 60% by mass, even more preferably 1% by mass to 55% by mass, even more preferably 2% by mass to 50% by mass, and particularly preferably 3% by mass to 45% by mass.
[0090] When the content of the thermoplastic elastomer is within the above range, the flexibility at room temperature and the toughness at low temperatures are improved, so that the feel of the fiber-resin composite sheet of the present invention immediately after touching can be made more favorable.
[0091] <Other ingredients> In addition to the 4-methyl-1-pentene polymer (A) and the other polymer (B), the fiber-resin composite sheet of the present invention may contain components other than the 4-methyl-1-pentene polymer (A) and the other polymer (B) (hereinafter also referred to as "other components") depending on the application, within a range that does not impair the effects of the present invention.
[0092] Examples of such resin additives include pigments, dyes, fillers, lubricants, plasticizers, release agents, antioxidants, flame retardants, UV absorbers, antibacterial agents, surfactants, antistatic agents, weather stabilizers, heat stabilizers, antislip agents, antiblocking agents, foaming agents, crystallization aids, antifogging agents, (transparent) nucleating agents, antiaging agents, hydrochloric acid absorbers, impact modifiers, crosslinking agents, co-crosslinking agents, crosslinking aids, adhesives, softeners, processing aids, etc. These additives can be used alone or in appropriate combination of two or more.
[0093] Examples of pigments include inorganic pigments (titanium oxide, iron oxide, chromium oxide, cadmium sulfide, etc.) and organic pigments (azo lake type, thioindigo type, phthalocyanine type, anthraquinone type). Examples of dyes include azo type, anthraquinone type, triphenylmethane type, etc. The content of these pigments and dyes is not particularly limited, but is preferably 5% by mass or less, more preferably 0.1 to 3% by weight, in total, based on the total mass of the 4-methyl-1-pentene polymer (A).
[0094] Examples of fillers include glass fibers, carbon fibers, silica fibers, metal (stainless steel, aluminum, titanium, copper, etc.) fibers, carbon black, silica, glass beads, silicates (calcium silicate, talc, clay, etc.), metal oxides (iron oxide, titanium oxide, alumina, etc.), metal carbonates (calcium sulfate, barium sulfate), and various metal (magnesium, silicon, aluminum, titanium, copper, etc.) powders, mica, glass flakes, etc. These fillers may be used alone or in combination of two or more.
[0095] Examples of the lubricant include wax (such as carnauba wax), higher fatty acids (such as stearic acid), higher alcohols (such as stearyl alcohol), and higher fatty acid amides (such as stearic acid amide).
[0096] Examples of the plasticizer include aromatic carboxylates (dibutyl phthalate, etc.), aliphatic carboxylates (acetyl ricinoleate, etc.), aliphatic dialkoxylates (adipic acid-propylene glycol polyesters, etc.), aliphatic tricarboxylates (triethyl citrate, etc.), phosphate triesters (triphenyl phosphate, etc.), epoxy fatty acid esters (epoxybutyl stearate, etc.), and petroleum resins.
[0097] Examples of the release agent include lower (C1-4) alcohol esters of higher fatty acids (butyl stearate, etc.), polyhydric alcohol esters of fatty acids (C4-30) (hardened castor oil, etc.), glycol esters of fatty acids, and liquid paraffin.
[0098] Examples of the antioxidant include phenol-based (2,6-di-t-butyl-4-methyl-phenol, etc.), polycyclic phenol-based (2,2'-methylenebis(4-methyl-6-t-butylphenol, etc.), phosphorus-based (tetrakis(2,4-di-t-butylphenyl)-4,4-biphenylenediphosphonate, etc.), and amine-based (N,N-diisopropyl-p-phenylenediamine, etc.) antioxidants.
[0099] Examples of the flame retardant include organic flame retardants (nitrogen-containing, sulfur-containing, silicon-containing, phosphorus-containing, etc.) and inorganic flame retardants (antimony trioxide, magnesium hydroxide, zinc borate, red phosphorus, etc.).
[0100] Examples of the ultraviolet absorbing agent include benzotriazole-based, benzophenone-based, salicylic acid-based, and acrylate-based agents.
[0101] Examples of antibacterial agents include quaternary ammonium salts, pyridine compounds, organic acids, organic acid esters, halogenated phenols, and organic iodines.
[0102] The surfactants may be nonionic, anionic, cationic or amphoteric surfactants.
[0103] Examples of nonionic surfactants include polyethylene glycol-type nonionic surfactants such as higher alcohol ethylene oxide adducts, fatty acid ethylene oxide adducts, higher alkylamine ethylene oxide adducts, and polypropylene glycol ethylene oxide adducts, and polyhydric alcohol-type nonionic surfactants such as polyethylene oxide, fatty acid esters of glycerin, fatty acid esters of pentaerythritol, fatty acid esters of sorbitol or sorbitan, alkyl ethers of polyhydric alcohols, and fatty amides of alkanolamines. Examples of anionic surfactants include sulfate ester salts such as alkali metal salts of higher fatty acids, sulfonates such as alkylbenzene sulfonates, alkyl sulfonates, and paraffin sulfonates, and phosphate ester salts such as higher alcohol phosphate ester salts, and examples of cationic surfactants include quaternary ammonium salts such as alkyltrimethyl-ammonium salts. Examples of amphoteric surfactants include amino acid-type amphoteric surfactants such as higher alkylaminopropionates, and betaine-type amphoteric surfactants such as higher alkyldimethyl-betaines and higher alkyldihydroxyethyl betaines.
[0104] Examples of the antistatic agent include the above-mentioned surfactants, fatty acid esters, and polymeric antistatic agents. Examples of the fatty acid esters include esters of stearic acid and oleic acid, and examples of the polymeric antistatic agents include polyether ester amides.
[0105] The content of various additives such as the above-mentioned fillers, lubricants, plasticizers, mold release agents, antioxidants, flame retardants, UV absorbers, antibacterial agents, surfactants, and antistatic agents is not particularly limited depending on the application within a range that does not impair the object of the present invention, but is preferably 0.1 to 30 mass% in total based on the total mass of the 4-methyl-1-pentene polymer (A).
[0106] <Fiber assembly> The fiber aggregate is a sheet-like aggregate formed by a plurality of fibers being regularly or irregularly assembled. Examples of the fibers include carbon fibers, glass fibers, aramid fibers, alumina fibers, polyester fibers, polyurethane fibers, silicon carbide fibers, boron fibers, metal fibers, and cellulose fibers. The fibers can be used alone or in combination of two or more kinds.
[0107] The fibers are preferably carbon fibers, aramid fibers, polyester fibers, and cellulose fibers, and more preferably carbon fibers. Carbon fibers make it difficult for fuzz to occur from the cut surfaces of the fiber-resin composite sheet, make it difficult for wrinkles, folding marks, and dents to occur when the fiber-resin composite sheet is folded or loaded, and make the wrinkles, folding marks, and dents that do occur more likely to disappear over time, and further improve the design of the fiber-resin composite sheet.
[0108] Examples of carbon fibers (carbon fibers, CF) include pitch-based carbon fibers, polyacrylonitrile (PAN)-based carbon fibers, and rayon-based carbon fibers. Carbon fibers can be used alone or in combination of two or more kinds. As carbon fibers, PAN-based carbon fibers are preferable.
[0109] Examples of the aramid fiber include polyparaphenylene terephthalamide fiber and polymetaphenylene isophthalamide fiber. The aramid fiber can be used alone or in combination of two or more kinds.
[0110] Examples of polyester fibers include polyethylene terephthalate fibers, polybutylene terephthalate fibers, polytrimethylene terephthalate fibers, and polyethylene naphthalate fibers. The polyester fibers can be used alone or in combination of two or more types. Examples of polyurethane fibers include polyester-based polyurethane fibers and polyether-based polyurethane fibers. The polyurethane fibers can be used alone or in combination of two or more types.
[0111] Examples of cellulose fibers include hemp fibers, bamboo fibers, cotton fibers, wood fibers, kenaf fibers, hemp fibers, jute fibers, banana fibers, and coconut fibers. Examples of wood fibers include fibers obtained from wood pulp. Examples of wood include coniferous and broad-leaved trees. The cellulose fibers may be natural fibers or industrial fibers. The cellulose fibers may be cellulose nanofibers. The cellulose fibers may be used alone or in combination of two or more types.
[0112] In particular, since carbon fibers and polyester fibers obtained from synthetic polymers are continuously spun, there is no particular upper limit on the length of the fibers, but the length is preferably 25 mm or more and 5000 mm or less, more preferably 30 mm or more and 2000 mm or less, and even more preferably 50 mm or more and 1000 mm or less.
[0113] A fiber assembly can be obtained by forming a fiber material containing fibers into a sheet. Methods for forming a fiber material into a sheet include, for example, various weaving methods described below and methods for making paper such as washi paper. Washi paper can be made from fibers obtained from paper mulberry, mitsumata, gampi, etc.
[0114] Examples of the fiber assembly include woven fabrics, knitted fabrics, felts, nonwoven fabrics, and unidirectional materials. These may be used alone or in combination of two or more. The fiber assembly is preferably a woven fabric from the viewpoint of improving the touch.
[0115] Woven fabrics are formed by weaving fibers. Examples of weaving methods include plain weave, twill weave, tricot weave, satin weave, rib weave, twill weave, broken twill weave, herringbone weave, irregular satin weave, overlapped satin weave, honeycomb weave, pear weave, rinzu weave, tsuzure brocade weave, Bedford weave, pique weave, double weave, hollow weave, triple weave, and quadruple weave. Examples of weaving methods include weaving methods that draw special patterns on the fabric, such as jacquard weave. Plain weave or twill weave is preferred for carbon fibers, from the viewpoints of making it difficult for fuzz to occur from the cut surface of the fiber-resin composite sheet, making it difficult for wrinkles, folding marks, and dents to occur when the fiber-resin composite sheet is folded or loaded, and making it easier for the wrinkles, folding marks, and dents that have occurred to disappear over time.
[0116] Plain weaving, for example, is a method of weaving in which warp and weft threads alternately rise and fall.
[0117] Twill weaving is a weaving method in which a warp thread is passed, for example, over two or three weft threads and under one weft thread in sequence.
[0118] Satin weaving is a method of weaving in which the warp and weft threads are crossed so that, for example, one of the warp and weft threads skips over four or more of the other.
[0119] Rib weaving is, for example, a method of plain weaving the warp and weft threads so that one of the warp and weft threads crosses several of the other threads, or a method of using a mixture of thick and thin threads as the warp and weft threads.
[0120] Basket weaving is a method of weaving, for example, by arranging two or more warp threads and two or more weft threads into a plain weave. Broken twill weaving is a method of weaving, for example, by using three weft threads for one warp thread, so that the satin weave is irregularly arranged.
[0121] Herringbone weaving is, for example, a method of weaving warp and weft threads so that the continuous interlocking V-shapes or rectangles form a fishbone pattern. Irregular satin weaving is, for example, a method of weaving warp and weft threads so that the weaving points are irregularly arranged.
[0122] The overlapped satin weave is, for example, a method of overlapping two satin weaves so that the weaving points are offset, and a method of adding an additional weaving point at the point where the weaving points meet. The honeycomb weave is, for example, a method of stretching the floating parts of the warp and weft threads to create a grid pattern, thereby obtaining a honeycomb appearance with unevenness on the woven surface.
[0123] The matte weaving is a method of producing fine grain by, for example, irregularly setting the lengths and positions of the raised portions of the warp and weft threads.
[0124] For example, Rinzu weaving is a method of forming a pattern by a day and night weave consisting of a front satin and a back satin. Tsuzure Nishiki weaving is a method of forming a pattern by weaving together two or more colored threads as weft threads.
[0125] Bedford weaving, for example, is a method of forming a vertical rib pattern by using a double weave.
[0126] Pique weaving is a method of forming a horizontal rib pattern or a diamond pattern by double weaving, for example. Fastened double weaving is a method of overlapping two fabrics and forming a pattern across the upper fabric at a specific portion of the warp or weft to obtain a single fabric.
[0127] The hollow weave is a method of weaving the warp and weft threads into a hollow shape by separating the front and back fabrics without twisting them except at the ends (selvage parts). The triple weave is a method of changing the two layers of fabric in the above-mentioned double weave into three layers of fabric.
[0128] The quadruple weave is a method of changing the two pieces of fabric in the fastening double weave described above into four pieces of fabric.
[0129] Jacquard weaving is a method of weaving warp and weft threads randomly to create a desired pattern.
[0130] These may be used alone or in combination of two or more. The woven fabric may further be embroidered with a desired pattern (design). There is no particular limitation on the embroidery method, and any known method may be used.
[0131] The fiber assembly may be coated with an adhesive (also called a binder or a sealant) that prevents the fibers from fraying together, as long as the effect of the present invention is not impaired.
[0132] The fiber assembly has a thickness (average thickness) of, for example, 10 μm or more, preferably 50 μm or more, more preferably 100 μm or more. The fiber assembly has a thickness (average thickness) of, for example, 3000 μm or less, preferably 1000 μm or less, more preferably 500 μm or less, particularly preferably 350 μm or less.
[0133] The fiber aggregate has a basis weight of 5g / m 2 More than 700g / m 2 Preferably, it is 8 g / m or less. 2 More than 600g / m 2 It is more preferable that the fiber aggregate is Japanese paper. Furthermore, the basis weight is 8 g / m 2 More than 100g / m 2 In the case of Japanese paper, if the basis weight is within this range, it becomes easy to impregnate the paper with the resin composition, and the porosity tends to be small.
[0134] <Method of manufacturing fiber-resin composite sheet> The fiber-resin composite sheet according to the present invention is prepared by bonding a sheet or film of a resin composition containing the 4-methyl-1-pentene copolymer (A) and a fiber assembly together under heat and pressure by a known heat-pressing device.
[0135] The sheet or film of the resin composition containing the 4-methyl-1-pentene copolymer (A) can be produced by a known method without any particular limitation. For example, it can be obtained by molding with a general T-die extrusion molding machine and a mold printing molding machine. For example, a sheet is formed by molding with a single-screw extruder at a cylinder temperature of 170 to 250°C and a cast roll temperature of 0 to 70°C. The thickness of the sheet is usually 5 to 1000 μm, preferably 10 to 500 μm, more preferably 40 to 500 μm, further preferably 80 to 500 μm, and particularly preferably 120 to 300 μm, which is preferable because it is excellent in sheet productivity, does not cause pinholes during sheet molding, and provides sufficient strength. In addition, the sheet surface may be embossed, and may be stretched during or after sheet molding. Furthermore, the sheet obtained by molding may be annealed at a temperature below the melting point of the resin.
[0136] Examples of the thermocompression device for pressing and heating the sheet or film of the resin composition containing the 4-methyl-1-pentene copolymer (A) and the fiber assembly include an autoclave and a heat press.
[0137] The pressure bonding conditions and heating conditions are appropriately set according to the purpose and use. The pressure bonding pressure is, for example, 0.1 MPa or more, preferably 0.5 MPa or more. The pressure bonding pressure is, for example, 5.0 MPa or less, preferably 2.5 MPa or less. The heating temperature is, for example, 100°C or more, preferably 140°C or more, and, for example, 300°C or less, preferably 240°C or less. The pressure bonding time and heating time are, for example, 0.5 minutes or more, preferably 1 minute or more. The pressure bonding time and heating time are, for example, 30 minutes or less, preferably 10 minutes or less.
[0138] The environmental conditions for the bonding and heating may be a normal pressure environment or a reduced pressure environment. The reduced pressure environment includes a vacuum environment. A preferred environmental condition is a reduced pressure environment. Under a reduced pressure environment, the generation of bubbles in the fiber-resin composite sheet can be suppressed.
[0139] As a result, the resin composition containing the 4-methyl-1-pentene copolymer (A) is melted, and the fiber assembly is impregnated with the resin composition containing the thermoplastic 4-methyl-1-pentene copolymer (A). Thereafter, the resin composition containing the 4-methyl-1-pentene copolymer (A) is cooled to room temperature. As a result, a fiber-resin composite sheet is obtained.
[0140] In the above method, a sheet or film of the resin composition containing 4-methyl-1-pentene copolymer (A) can be placed on only one surface of the fiber assembly, and then pressed and heated. In this case, the resin composition containing 4-methyl-1-pentene copolymer (A) penetrates to a predetermined depth from one surface to the other surface in the thickness direction of the fiber assembly.
[0141] In this case, the resin composition containing 4-methyl-1-pentene copolymer (A) may reach from one surface to the other surface in the thickness direction of the fiber assembly, or may not reach from one surface to the other surface. The penetration depth of the resin composition containing 4-methyl-1-pentene copolymer (A) is appropriately set depending on the thickness of the sheet or film of the resin composition containing 4-methyl-1-pentene copolymer (A) and the heating conditions during compression bonding.
[0142] In other words, the resin composition containing the 4-methyl-1-pentene copolymer (A) may be impregnated from one surface in the thickness direction of the fiber assembly to a predetermined depth, i.e., the surface on the other side in the thickness direction of the fiber assembly does not have to be completely impregnated with the resin composition containing the 4-methyl-1-pentene copolymer (A).
[0143] In the above method, a sheet or film of a resin composition containing 4-methyl-1-pentene copolymer (A) can be placed on both sides of the fiber assembly, and then pressed and heated. In this case, the resin composition containing 4-methyl-1-pentene copolymer (A) penetrates to a predetermined depth from one surface to the other surface in the thickness direction of the fiber assembly. At the same time, the resin composition containing 4-methyl-1-pentene copolymer (A) penetrates to a predetermined depth from the other surface to one surface in the thickness direction of the fiber assembly.
[0144] In this case, the resin composition containing the 4-methyl-1-pentene copolymer (A) may or may not be entirely impregnated into the fiber assembly in the thickness direction.
[0145] In other words, the resin composition containing the 4-methyl-1-pentene copolymer (A) may be impregnated to a predetermined depth from each of the surfaces on one side and the other side in the thickness direction of the fiber assembly. That is, the fiber assembly may have an area in the thickness direction inside that is not completely impregnated with the resin composition containing the 4-methyl-1-pentene copolymer (A).
[0146] Preferably, a sheet or film of a resin composition containing the 4-methyl-1-pentene copolymer (A) is pressed and heated on both sides of the fiber assembly.
[0147] From the viewpoints of improving the restorability when the fiber resin composite sheet is folded and preventing wrinkles, folding marks and dents from occurring when the fiber resin composite sheet is folded or loaded, it is preferable that a region that is not impregnated with the resin composition containing 4-methyl-1-pentene copolymer (A) is formed inside the fiber assembly in the thickness direction or on the other surface side. The impregnation state of the resin composition containing 4-methyl-1-pentene copolymer (A) is confirmed and determined, for example, by observing the cross section of the fiber resin composite sheet with a scanning electron microscope (SEM).
[0148] In addition, when pressure is applied, a release film can be placed on the outside of the sheet or film of the resin composition containing the 4-methyl-1-pentene copolymer (A). This can improve workability and provide a fiber resin composite sheet with excellent appearance. Furthermore, the surface shape of the release film can be processed as desired. For example, the surface of the release film can be embossed. This can improve the appearance of the fiber resin composite sheet.
[0149] The fiber resin composite sheet described in the present invention is cured as necessary. The curing temperature is, for example, 40° C. or higher, preferably 80° C. or higher. The curing temperature is, for example, 140° C. or lower, preferably 120° C. or lower. The curing time is, for example, 30 minutes or longer, preferably 1 hour or longer. The curing time is, for example, 7 days or shorter, preferably 3 days or shorter.
[0150] In addition, the fiber-resin composite sheet according to the present invention may have a coating layer on the surface thereof to the extent that the functions of fluff resistance, flex recovery, crease resistance, and wrinkle recovery are not impaired. The coating layer can prevent the resin composition containing the 4-methyl-1-pentene copolymer (A) from swelling due to human sebum during use and from abrasion deterioration due to rubbing.
[0151] <Shapes and uses of fiber-resin composite sheets> The thickness of the fiber-resin composite sheet varies depending on its intended use, but for example, the lower limit of the thickness is 15 μm or more, preferably 30 μm or more, more preferably 40 μm or more, even more preferably 80 μm or more, and particularly preferably 120 μm or more. The upper limit of the thickness is, for example, 5000 μm or less, preferably 1000 μm or less, more preferably 500 μm or less, even more preferably 300 μm or less, and particularly preferably 250 μm or less.
[0152] The surface of the fiber-resin composite sheet may be covered with a coating layer. The surface of the fiber-resin composite sheet or the surface of the coating layer may be embossed or textured to impart design properties.
[0153] The fiber resin composite sheet may be molded into various shapes, or may be attached to the surface of another molded body, or may be sewn together by overlapping sheets, or may be fused with heat, ultrasonic waves, or the like to form a tube or a bag. It is preferably used in various industrial fields. Examples of the industrial fields include the field of accessories such as daily necessities, the field of vehicles such as automotive interior materials, the field of furniture, the field of sports, the field of robots, the field of office supplies, the field of architecture, the field of health care, and the field of electricity. The fiber resin composite sheet is preferably used in the field of accessories. Examples of accessories include bags, shoes, wallets, and business card holders. EXAMPLES
[0154] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples as long as it does not depart from the gist of the present invention.
[0155] [Measurement methods for various physical properties] The methods used to measure various physical properties of the polymers obtained in the examples are shown below.
[0156] (1) Composition 13 The composition of the polymer was determined by C-NMR measurement. 13 The measurement conditions for C-NMR are as follows: ~Conditions~ Measurement equipment: Nuclear magnetic resonance equipment (ECP500 type, manufactured by JEOL Ltd.) Observation kernel: 13 C(125MHz) Sequence: Single pulse proton decoupling Pulse width: 4.7μsec (45° pulse) Repeat time: 5.5 seconds Number of times: 10,000 or more Solvent: orthodichlorobenzene / deuterated benzene (volume ratio: 80 / 20) mixed solvent Sample concentration: 55mg / 0.6mL Measurement temperature: 120℃ Chemical shift reference value: 27.50 ppm
[0157] (2) Intrinsic viscosity [η] Approximately 20 mg of 4-methyl-1-pentene copolymer (A) was dissolved in 25 ml of decalin, and the specific viscosity η was measured using an Ubbelohde viscometer in an oil bath at 135°C. sp The decalin solution was diluted with 5 ml of decalin, and the specific viscosity η was measured in the same manner as above. sp This dilution procedure was repeated two more times, and the value of ηsp / C when the concentration (C) was extrapolated to 0 was calculated as the intrinsic viscosity [η] (unit: dl / g) (see Equation 1 below). [η]=lim(η sp / C) (C→0)...Formula 1
[0158] (3) Weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn) Liquid chromatograph: Waters ALC / GPC 150-C plus type (integrated differential refractometer detector type), 2 Tosoh Corporation GMH6-HT and 2 GMH6-HTL columns were connected in series, and gel permeation chromatography (GPC) was performed at a flow rate of 1.0 ml / min and 140° C. using o-dichlorobenzene as the mobile phase medium. The weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn) were determined by analyzing the obtained chromatogram using a calibration curve using a standard polystyrene sample by a known method.
[0159] (4) Density The density was determined in accordance with JIS K7112 (density gradient tube method).
[0160] (5) Melting point (Tm) Using a differential scanning calorimetry (DSC), the following method was measured in accordance with JIS K7121. Approximately 5 mg of 4-methyl-1-pentene copolymer (A) was sealed at room temperature in an aluminum pan for measurement of a differential scanning calorimeter (DSC220C type) manufactured by Seiko Instruments Inc., and heated from room temperature to 260°C at a rate of 10°C / min. In order to completely melt the 4-methyl-1-pentene copolymer (A), it was held at 260°C for 5 minutes, and then cooled to -50°C at a rate of 10°C / min. After holding at -50°C for 5 minutes, it was heated a second time to 260°C at a rate of 10°C / min, and the temperature at which a peak was observed in this second heating was taken as the melting point (Tm) of the polymer. If no clear peak was detected, it was considered that there was no melting point, and if multiple peaks were detected, the peak detected on the highest temperature side was adopted.
[0161] (6) Melt flow rate (MFR) The melt flow rate (MFR) of the 4-methyl-1-pentene copolymer (A) was measured in accordance with ASTM D1238 at 230°C under a load of 2.16 kg and at 260°C under a load of 5.0 kg. The MFR of other polymers (B) (i.e., polymers B-1 and B-2 below) was measured under different measurement conditions at 230°C under a load of 2.16 kg.
[0162] (7) tan δ peak temperature, tan δ peak value In the measurement of dynamic viscoelasticity, a 3 mm thick pressed sheet was used as the measurement sample, and a 45 mm x 10 mm x 3 mm strip was cut out as required for the dynamic viscoelasticity measurement. Using an ANTON Paar MCR301, the temperature dependence of dynamic viscoelasticity was measured from -40 to 150°C at a frequency of 10 rad / s, and the temperature (tan δ peak temperature) at which the loss tangent (tan δ) due to the glass transition temperature reached its peak value (maximum value) in the range of 0 to 40°C, and the value of the loss tangent (tan δ) at that time (tan δ peak value) were measured.
[0163] [Preparing materials] <Synthesis of 4-methyl-1-pentene copolymer (A)> Synthesis of 4-methyl-1-pentene copolymer (A-1) A 1.5-liter stainless steel autoclave equipped with an agitator and thoroughly purged with nitrogen was charged with 300 ml of normal hexane (dried over activated alumina in a dry nitrogen atmosphere) and 450 ml of 4-methyl-1-pentene at 23° C. 0.75 ml of a 1.0 mmol / ml toluene solution of triisobutylaluminum (TIBAL) was charged into the autoclave and the agitator was turned on.
[0164] Next, the autoclave was heated to an internal temperature of 60°C, and pressurized with propylene so that the total pressure was 0.40MPa (gauge pressure). Then, 0.34ml of a toluene solution containing 1mmol of methyl-aluminoxane in terms of Al and 0.01mmol of diphenylmethylene (1-ethyl-3-t-butyl-cyclopentadienyl) (2,7-di-t-butyl-fluorenyl) zirconium dichloride, which had been prepared in advance, was pressed into the autoclave with nitrogen to start polymerization. During the polymerization reaction, the temperature was adjusted so that the internal temperature of the autoclave was 60°C. 60 minutes after the start of polymerization, 5ml of methanol was pressed into the autoclave with nitrogen to stop the polymerization, and the autoclave was depressurized to atmospheric pressure. Acetone was poured into the reaction solution while stirring.
[0165] The obtained powdery polymer containing the solvent was dried at 100° C. under reduced pressure for 12 hours to obtain 36.9 g of 4-methyl-1-pentene copolymer (A-1). The measurement results of various physical properties are shown in Table 1.
[0166] Synthesis of 4-methyl-1-pentene copolymer (A-2) According to the polymerization method described in Comparative Example 9 of WO 2006 / 054613, a 4-methyl-1-pentene polymer was obtained by changing the ratio of 4-methyl-1-pentene, other α-olefins (mass mixture of 1-hexadecene, 1-octadecene, etc.), and hydrogen. The measurement results of the seed physical properties are shown in Table 1.
[0167] [Table 1]
[0168] <Other polymers (B)> (B-1): Styrene-vinylisoprene-styrene copolymer "Hybra 7311F" (manufactured by Kuraray Co., Ltd.) (B-2): Ester-based polyurethane sheet "Higress DUS601" (manufactured by Seedom Co., Ltd.) (B-3): Polypropylene "J13B" (Prime Polymer Co., Ltd.)
[0169] <Fiber assembly> (C-1): Carbon fiber fabric (twill weave), manufactured by Formosa Plastics, Carbon Fabric EC3CX, Average thickness: 250 μm (C-2): Carbon fiber fabric, manufactured by Teijin Limited, Tenax (registered trademark) Dry Reinforcement fabric Average thickness: 250 μm (C-3): Cellulose fiber fabric (twill weave, made of flax), manufactured by Bcomp, ampliTex (registered trademark), No. 5040 Weight 300g / m 2 , average thickness 900μm (C-4): Cellulose fiber fabric (plain weave, made from hemp), HEMP SHOW Weight 520g / m 2 , average thickness 850μm (C-5): Cellulose fiber aggregate (washi paper), made in Gokayama Washi Village Weight 65g / m 2 , average thickness 200μm (C-6): Polyester fiber / polyurethane fiber fabric, Kawada Knit Co., Ltd., TRINOCOOL CF TC-8686 Weight 240g / m 2 , average thickness 500μm
[0170] [Preparation of fiber-resin composite sheet] <Example 1> 4-Methyl-1-pentene copolymer (A-1) was used, and a single screw extruder (cylinder inner diameter D: 50 mm, full flight screw, L / D: 32 mm when the effective screw length is L, carbon dioxide supply position: 17.5 D from the screw supply side), T-die (die width: 320 mm, lip opening: 0.5-1.8 mm), cooling roll (outer diameter 50 mm, mirror-finished steel with hard chrome plating surface treatment, water-cooled), T-die, cooling roll, and take-off machine were used, and the components were melted and kneaded under the conditions of a temperature of 220°C in each part of the cylinder and a screw rotation speed of 26 rpm, and extruded into a sheet from the T-die at a resin temperature of 195°C at the cylinder head to an extrusion rate of 4.5 kg / hour.
[0171] The extruded sheet was cooled with a cooling roll (water passing through the roll at 15°C) and taken up using a take-up machine (take-up speed 2.3 m / min) to obtain a sheet having a width of approximately 310 mm and a thickness of 180 μm containing 4-methyl-1-pentene polymer (A-1).
[0172] The obtained (A-1) sheet was sandwiched between both sides of C-1, a 500 μm thick Teflon (registered trademark) sheet was laid as a release sheet, and the sheet was sandwiched between SUS plates. The sample was preheated for 5 minutes using a heat press machine (Toyo Seiki Co., Ltd., heating and cooling two-stage press) set at 230° C., and then pressed at 10 MPa for 3 minutes to impregnate the fiber aggregate (C-1) with the resin composition (sheet). Then, it was cooled for 3 minutes at 5 MPa using a press machine (Toyo Seiki Co., Ltd.) set at 23° C. to obtain a fiber resin composite sheet of Example 1.
[0173] <Example 2> The sheets containing the 4-methyl-1-pentene copolymer (A-1) prepared in Example 1 were placed on both sides of the fiber assembly (C-1), and the fiber assembly (C-1) was impregnated with the resin composition by changing the heat pressing conditions in various ways between a heating temperature of 190 to 230°C and a pressure condition of 5 to 10 MPa using the same method as in Example 1, to obtain a fiber resin composite sheet of Example 2. At this time, when a sheet with a high porosity was prepared, the pressing temperature was set near the lower limit and the pressure condition was lowered.
[0174] <Example 3> A sheet containing the 4-methyl-1-pentene copolymer (A-1) prepared in Example 1 was placed on one side of a fiber aggregate (C-2), and the fiber aggregate (C-1) was impregnated with the resin composition using a method similar to that used in Example 2, with various changes being made to the conditions during heat pressing, to obtain a fiber resin composite sheet of Example 3.
[0175] <Examples 4 to 6> A sheet containing the 4-methyl-1-pentene copolymer (A-1) prepared in Example 1 was placed on both sides of a fiber assembly (C-2), and the fiber assembly (C-2) was impregnated with the resin composition using the same method as in Example 2 while changing various conditions during heat pressing, thereby obtaining fiber resin composite sheets of Examples 4 to 6.
[0176] <Example 7> A sheet containing the 4-methyl-1-pentene copolymer (A-1) prepared in Example 1 was placed on both sides of a fiber aggregate (C-1), and the fiber aggregate (C-1) was impregnated with the resin composition using a method similar to that used in Example 2, with various changes being made to the conditions during the heat press, to obtain a fiber resin composite sheet of Example 7.
[0177] <Example 8> A sheet containing the 4-methyl-1-pentene copolymer (A-1) prepared in Example 1 was placed on one side of a fiber aggregate (C-2), and the fiber aggregate (C-2) was impregnated with the resin composition using a method similar to that used in Example 2, with various changes being made to the conditions during the heat press, to obtain a fiber resin composite sheet of Example 8.
[0178] <Example 9> A sheet containing the 4-methyl-1-pentene copolymer (A-1) prepared in Example 1 was placed on one side of a fiber aggregate (C-1), and the fiber aggregate (C-1) was impregnated with the resin composition using a method similar to that used in Example 2, with various changes being made to the conditions during the heat press, to obtain a fiber resin composite sheet of Example 9.
[0179] <Example 10, Comparative Example 5> A sheet containing the 4-methyl-1-pentene copolymer (A-1) prepared in Example 1 was placed on both sides of a fiber aggregate (C-2), and the fiber aggregate (C-2) was impregnated with the resin composition using a method similar to that used in Example 2 while changing various conditions during heat pressing, thereby obtaining fiber resin composite sheets of Example 10 and Comparative Example 5.
[0180] <Example 11> Using 60 parts by mass of 4-methyl-1-pentene copolymer (A-1) and 40 parts by mass of other copolymer (B-1), a resin sheet containing 4-methyl-1-pentene copolymer (A-1) was obtained using a T-die molding machine having a single screw extruder similar to that in Example 1. The thickness of the sheet was 200 μm.
[0181] The obtained sheet was placed on one side of a fiber aggregate (C-1), and the resin composition was impregnated into the fiber aggregate (C-1) using a method similar to that of Example 2, but with various changes to the conditions during heat pressing, to obtain a fiber resin composite sheet of Example 11.
[0182] <Example 12> Using 60 parts by mass of 4-methyl-1-pentene copolymer (A-1) and 40 parts by mass of other copolymer (B-1), a resin sheet containing 4-methyl-1-pentene copolymer (A-1) was obtained using a T-die molding machine having a single screw extruder similar to that in Example 11. The thickness of the sheet was 200 μm.
[0183] The obtained sheets were placed on both sides of a fiber aggregate (C-1), and the resin composition was impregnated into the fiber aggregate (C-1) using a method similar to that used in Example 2, with various changes being made to the conditions during heat pressing, to obtain a fiber resin composite sheet of Example 12.
[0184] <Comparative Example 1> The 4-methyl-1-pentene copolymer (A-2) was used, and the same single-screw extruder as in Example 1 was used, and the mixture was put into the hopper. The components were melted and kneaded under the conditions of a temperature of 280°C in each part of the cylinder and a screw rotation speed of 20 rpm, and extruded into a sheet from a T-die at a resin temperature of 255°C in the cylinder head and an extrusion rate of 5 kg / hour. The extruded sheet was cooled with a cooling roll (water passing temperature inside the roll: 40°C) and taken up with a take-up machine (take-up speed: 2.3 m / min), to obtain a sheet of 4-methyl-1-pentene polymer (A-2) with a sheet width of about 300 mm. The thickness of the sheet was 170 μm.
[0185] The obtained sheet was placed on one side of the fiber assembly (C-1), a 500 μm thick Teflon (registered trademark) sheet was laid as a release sheet, and the sheet was sandwiched between SUS plates. The sample was preheated for 5 minutes using a heat press (Toyo Seiki Co., Ltd., heating and cooling two-stage press) set at 260°C, and then pressed at 5 MPa for 3 minutes to impregnate the fiber assembly (C-1) with the resin composition (sheet). Then, the sample was cooled for 2 minutes at 5 MPa using a press (Toyo Seiki Co., Ltd.) set at 23°C to obtain a fiber resin composite sheet of Comparative Example 1.
[0186] <Comparative Example 2> Using an autoclave heating device owned by The MOT Company, one side of a carbon fiber aggregate (C-1) was impregnated with a thermosetting urethane raw material (ester, isocyanate), and the thermosetting urethane raw material was impregnated into the fiber aggregate (C-1) by autoclave pressure treatment, thereby obtaining a sheet for Comparative Example 2.
[0187] <Comparative Example 3> A commercially available tote bag (product name: Large tote bag) manufactured by Hide kasuga 1896 Co., Ltd. was disassembled to take out a flat carbon fiber resin sheet (the resin was found to be ester polyurethane (B-2) by IR spectrum measurement, and the carbon fiber was found to be twill). The obtained sheet was used as the sheet of Comparative Example 3.
[0188] <Comparative Example 4> A carbon fiber resin-processed sheet was taken out by dismantling the outer skin from a commercially available ski boot (product name ONE BOOTS) manufactured by RONIX Japan (the resin was found to be ether-based polyurethane by IR spectrum measurement, and the carbon fiber was found to be Carbitex CX6 twill weave by product information). The obtained sheet was used as the sheet of Comparative Example 4.
[0189] <Comparative Example 6> The other copolymer (B-3) was used, and the same single screw extruder as in Example 1 was used, and the mixture was put into the hopper. The components were melted and kneaded under the conditions of a temperature of 220°C in each part of the cylinder and a screw rotation speed of 20 rpm, and extruded into a sheet from a T-die at a resin temperature of 215°C in the cylinder head and an extrusion rate of 4 kg / hour. The extruded sheet was cooled with a cooling roll (water passing temperature inside the roll: 20°C) and taken up with a take-up machine (take-up speed: 2.3 m / min) to obtain a sheet of the other copolymer (B-3) with a sheet width of about 200 mm. The thickness of the sheet was 160 μm.
[0190] The obtained sheet was placed on one side of the fiber assembly (C-1), a 500 μm thick Teflon (registered trademark) sheet was laid as a release sheet, and the sheet was sandwiched between SUS plates. The sample was preheated for 3 minutes using a heat press (Toyo Seiki Co., Ltd., heating and cooling two-stage press) set at 220°C, and then pressed at 5 MPa for 2 minutes to impregnate the fiber assembly (C-1) with the resin composition (sheet). Then, the sample was cooled at 5 MPa for 2 minutes using a press (Toyo Seiki Co., Ltd.) set at 23°C to obtain a fiber resin composite sheet of Comparative Example 6.
[0191] <Example 13> Using 60 parts by mass of 4-methyl-1-pentene copolymer (A-1) and 40 parts by mass of other copolymer (B-1), a resin sheet containing 4-methyl-1-pentene copolymer (A-1) was obtained using a T-die molding machine having a single screw extruder similar to that in Example 11. The thickness of the sheet was 300 μm.
[0192] The obtained sheets were placed on both sides of a fiber aggregate (C-3), and the resin composition was impregnated into the fiber aggregate (C-3) using a method similar to that used in Example 2, with various changes being made to the conditions during heat pressing, to obtain a fiber resin composite sheet of Example 12.
[0193] <Examples 14 to 16> Using 60 parts by mass of 4-methyl-1-pentene copolymer (A-1) and 40 parts by mass of other copolymer (B-1), a resin sheet containing 4-methyl-1-pentene copolymer (A-1) was obtained using a T-die molding machine having a single screw extruder similar to that in Example 11. The thickness of the sheet was 300 μm.
[0194] The obtained sheets were placed on one side of each of the fiber assemblies (C-4) to (C-6), and the fiber assemblies were impregnated with the resin composition using a method similar to that of Example 2 while varying the conditions during heat pressing, thereby obtaining fiber resin composite sheets of Examples 14 to 16.
[0195] <Comparative Example 7> A sheet containing the 4-methyl-1-pentene copolymer (A-1) prepared in Example 1 was placed on one side of a fiber aggregate (C-3), and the resin composition was impregnated into the fiber aggregate (C-3) using a method similar to that of Example 2 while changing various conditions during heat pressing, thereby obtaining a fiber resin composite sheet of Comparative Example 7.
[0196] [Evaluation of fiber-resin composite sheets] The prepared fiber-resin composite sheets were evaluated according to the following criteria.
[0197] <Porosity (%)> An arbitrary cross section of the test piece for measurement was observed with a high-resolution scanning electron microscope (SEM) in such a way that it included the surface vicinity to the internal structure. A secondary image was created by trimming an enlarged image obtained by observation at a magnification of 500 times so that only the fiber resin composite sheet from the front surface to the back surface of the fiber aggregate / resin composition remained in the image. The obtained secondary image was loaded into an image analysis software (ImageJ), and the commands: Process, Binary, Make Binary were executed to perform binarized image processing. At this time, the area filled with the fiber aggregate and the resin composition was painted white, and the void area was painted black. At this time, in order to paint the resin composition part white, the threshold was controlled with the commands: Image, Adjust, Threshold. Next, the area fraction of the void part (area fraction of the white area) excluding the fiber aggregate and the resin composition part in the area of the observation field of view was calculated with the commands: Analyse, Analyze. The average value of the area fraction of the void part at any three points was taken as the porosity of the test piece for measurement.
[0198] In addition, for Examples 13 to 16 and Comparative Example 7, the porosity was measured in the same manner, except that the magnification of the SEM observation was optimized for each resin sheet.
[0199] <Fluff> A sheet sample of 152 mm × 100 mm was cut into 15 mm widths with a cutter. Six such samples were made and visually inspected for the presence or absence of dry fibers protruding from the end faces. ×: Dry fibers were sticking out. △: Dry fibers were slightly protruding. O: The dry eye bar did not protrude.
[0200] <Wrinkles, fold marks, dents> A sheet sample of 152 mm x 100 mm was cut into 15 mm widths with a cutter. The sheet was folded 180°, a 2 kg weight was placed on the sheet, and the sheet was left for 10 minutes, after which the weight was removed. The appearance of the sheet was observed immediately after removing the weight and 60 minutes later, and wrinkles, fold marks, and dents were visually confirmed. (i) 60 minutes after removing the weight ×: Cracks were generated at the folded portion of the surface of the sheet, and folding marks were also observed. △: Wrinkles, fold marks and dents were observed on the surface of the sheet. ◯: There were no wrinkles on the surface of the sheet, but folding marks and dents were observed. ◎: No wrinkles, fold marks or dents were found on the surface of the sheet. (ii) Immediately after removing the weight ×: Cracks were generated at the folded portion of the surface of the sheet, and folding marks were also observed. △: Wrinkles, fold marks and dents were observed on the surface of the sheet. ○: There were no wrinkles or fold marks on the surface of the sheet, but dents were observed. ◎: The sheet quickly returned to its original shape immediately after removal, and no wrinkles, fold marks or dents were observed on the surface of the sheet.
[0201] Tables 2 to 4 show the types of 4-methyl-1-pentene copolymers, types of other polymers and their ratios, types and shapes of fiber assemblies used in the preparation of fiber resin composite sheets in the Examples and Comparative Examples, and the evaluation results.
[0202] [Table 2]
[0203] [Table 3]
[0204] [Table 4]
[0205] 1A, 1B, and 1C are images taken by SEM observation of cross sections near the center in the thickness direction of the sheets of Example 1, Example 2, and Comparative Example 1, respectively. White circles indicate fibers, gray areas indicate impregnated resin composition, and black areas indicate voids. From Figs. 1A to 1C, it can be seen that in Example 1, the fiber aggregate is completely impregnated with the resin composition and there are no voids, whereas in Example 2 voids are generated and in Comparative Example 1 the voids are larger.
[0206] From Tables 2 to 4, it can be seen that a fiber resin composite sheet obtained by impregnating a fiber assembly with a resin composition containing a 4-methyl-1-pentene copolymer (A) satisfying condition (A-1) is less likely to generate fuzz on the cut surfaces of the sheet. [Industrial Applicability]
[0207] The fiber-resin composite sheet of the present invention is flexible, even though the fibers are impregnated with resin, and is easy to restore from bending, and is less likely to produce fuzz on the cut surfaces. The fiber-resin composite sheet of the present invention can provide a novel material that can be used in the above-mentioned wide variety of fields.
Claims
1. A fiber resin composite sheet comprising a fiber assembly and a resin composition impregnated into the fiber assembly, The resin composition contains a 4-methyl-1-pentene copolymer (A) that satisfies the following requirement (A-a): When the porosity of the fiber-resin composite sheet is defined as a ratio of an area of an unimpregnated portion of the fiber aggregate in which the resin composition is not impregnated to an area of the fiber-resin composite sheet in a cross section cut in a thickness direction of the fiber-resin composite sheet, the porosity is 36% or less. Fiber-resin composite sheet. (A-a) The content of structural units (P) derived from 4-methyl-1-pentene is 65 mol% or more and less than 90 mol%, and the content of structural units (AQ) derived from a monomer selected from the group consisting of ethylene and linear or branched α-olefins having 3 to 20 carbon atoms (excluding 4-methyl-1-pentene) is more than 10 mol% and not more than 35 mol%.
2. The structural unit (AQ) includes a structural unit derived from a monomer selected from the group consisting of ethylene and an α-olefin having 3 to 4 carbon atoms.
2. The fiber-resin composite sheet of claim 1.
3. The porosity is 20% or less. The fiber-resin composite sheet according to claim 1 or 2.
4. The 4-methyl-1-pentene copolymer (A) further satisfies the following requirement (A-b): The fiber-resin composite sheet according to claim 1 or 2. (A-b) No melting point (Tm) is observed when measured by differential scanning calorimetry (DSC)
5. The 4-methyl-1-pentene copolymer (A) further satisfies the following requirements (Ac) and (Ad): The fiber-resin composite sheet according to claim 4. (Ac) The peak temperature of the loss tangent tan δ determined by dynamic viscoelasticity measurement in the temperature range of −40 to 150° C. and at a frequency of 10 rad / s (1.6 Hz) is 15° C. to 45° C. (Ad) The peak value of the loss tangent tan δ determined by dynamic viscoelasticity measurement in the temperature range of -40 to 150°C and at a frequency of 10 rad / s (1.6 Hz) is in the range of 1.0 to 5.
0.
6. The fiber assembly includes carbon fibers. The fiber-resin composite sheet according to claim 1 or 2.
7. 3. An ornament comprising the fiber resin composite sheet according to claim 1 or 2.
8. An automobile interior material comprising the fiber resin composite sheet according to claim 1 or 2.
Citation Information