Anti-stray light film
Patent Information
- Application Number
- JP2024027461
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-17
- Filing Date
- 2024-02-27
- Publication Date
- 2024-10-01
AI Technical Summary
【0007】 本発明によれば、可視光および近赤外光の各反射率が低減された迷光防止フィルムが提供される。
Smart Images

Figure 2024132916000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an anti-stray light film. [Background technology]
[0002] Stray light generated inside optical devices can cause flare or ghosting in images captured by cameras, and can also cause measurement errors in measuring instruments such as spectrophotometers. Anti-stray light films have been proposed that can reduce or prevent stray light by absorbing reflected light (for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 10-332907 [Patent Document 2] Special Publication No. 2021-509487 Summary of the Invention [Problem to be solved by the invention]
[0004] However, in each of the films disclosed in Patent Documents 1 and 2, there is room for improvement in terms of reducing the reflectance of each of visible light and near-infrared light.
[0005] The present invention provides an anti-stray light film with reduced reflectance for both visible light and near infrared light. [Means for solving the problem]
[0006] The present invention has the following aspects. [1] A stray light prevention film having a fine uneven structure formed on the surface of the stray light prevention film, in which the average spacing between convex portions is equal to or less than the wavelength of visible light, and having an 8-degree total reflectance of 550 nm visible light of 0.50% or less and an 8-degree total reflectance of 800 nm near-infrared light of 1.0% or less. [2] The stray light prevention film according to [1], having a 5-degree regular reflectance of 550 nm visible light of 0.10% or less and a 5-degree regular reflectance of 800 nm near-infrared light of 0.30% or less. [3] The stray light prevention film according to [1] or [2], further comprising an uneven structure having an arithmetic mean roughness Ra of 0.010 μm or more and less than 1.00 μm and a period Sm of 10 to 300 μm, wherein the fine uneven structure is formed on the uneven structure. [4] The stray light prevention film according to [3], wherein the period Sm of the uneven structure is 70 to 200 μm. [5] The stray light prevention film according to any one of [1] to [4], further comprising an adhesive layer on the opposite side to the surface on which the microrelief structure is formed, the adhesive layer being capable of blocking visible light and / or near-infrared light. [6] The stray light prevention film according to any one of [1] to [5], further comprising a film or sheet adhered via an adhesive layer to the opposite side of the surface on which the microrelief structure is formed, the film or sheet being capable of blocking visible light and / or near-infrared light. [7] The stray light prevention film according to any one of [1] to [6], further comprising an ink layer on the opposite side to the surface on which the fine uneven structure is formed, the ink layer being capable of blocking visible light and / or near-infrared light. [8] The stray light prevention film according to any one of [1] to [7], wherein the surface on which the fine uneven structure is formed has a contact angle with water of 30 degrees or less. [9] A method for preventing stray light, comprising installing the stray light prevention film according to any one of [1] to [8] inside an optical device. Effect of the Invention
[0007] According to the present invention, there is provided a stray light prevention film having reduced reflectance for both visible light and near infrared light. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a cross-sectional view illustrating an example of a stray light prevention film. [Diagram 2]FIG. 11 is a cross-sectional view illustrating another example of the stray light prevention film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The meanings of the terms are as follows: "Visible light" means light with a wavelength in the range of 400 nm to 780 nm. "Near infrared light" means light with a wavelength in the range of 800 to 2500 nm. The symbol "~" indicating a range of numerical values means that the numerical values before and after it are included as the lower limit and upper limit.
[0010] The anti-stray light film of the present invention has a fine uneven structure in which the average spacing between convex portions formed on its surface is equal to or less than the wavelength of visible light, and has an 8-degree total reflectance of 0.50% or less for visible light of 550 nm and an 8-degree total reflectance of 1.0% or less for near-infrared light of 800 nm. In this way, in the stray light prevention film of the present invention, the reflectance of each of visible light and near infrared light is reduced. The 8-degree total reflectance of 550 nm visible light is 0.50% or less, preferably 0.4% or less, more preferably 0.3% or less, and even more preferably 0.1% or less. The 8-degree total reflectance of 800 nm near infrared light is 1.0% or less, preferably 0.9% or less, more preferably 0.8% or less, and even more preferably 0.5% or less.
[0011] In a preferred embodiment of the stray light prevention film, the 5-degree regular reflectance of visible light of 550 nm is 0.20% or less, and the 5-degree regular reflectance of near-infrared light of 800 nm is 0.50% or less. The 5-degree regular reflectance of visible light of 550 nm is 0.20% or less, preferably 0.10% or less, more preferably 0.07% or less, and even more preferably 0.05% or less. The 5-degree regular reflectance of near-infrared light of 800 nm is 0.50% or less, preferably 0.30% or less, more preferably 0.20% or less, and even more preferably 0.10% or less.
[0012] Hereinafter, some embodiments of the present invention will be described with reference to the drawings. However, the following description is for representative examples, and the present invention is not limited to the following description. The dimensional ratios in each drawing are for the convenience of explanation and may differ from the actual ones. In the following drawings, the same components are indicated by the same reference numerals, and the explanation of the overlapping components may be omitted.
[0013] The stray light prevention film 10A shown in Fig. 1 has a substrate 1, a fine concave-convex structure 3, and an adhesive layer 5. The fine concave-convex structure 3 is formed on a surface 1a of the substrate 1. The adhesive layer 5 is provided on a surface 1b of the substrate 1.
[0014] The material of the substrate 1 is not particularly limited as long as it transmits visible light, infrared light, and near infrared light. Examples of the substrate material include acrylic resins such as polymethyl methacrylate; polycarbonate resins; styrene resins such as polystyrene and methyl methacrylate-styrene copolymers; cellulose resins such as cellulose diacetate, cellulose triacetate, and cellulose acetate butyrate; polyester resins such as polyethylene terephthalate; polyamide resins; polyimide resins; polyethersulfone resins; polysulfone resins; polyolefin resins such as polypropylene, polymethylpentene, and alicyclic polyolefins; vinyl chloride resins such as polyvinyl chloride; polyvinyl acetal resins; polyether ketone resins; polyurethane resins; and glass. Among these, acrylic resins, polycarbonate resins, polyester resins, cellulose resins, and polyolefin resins are preferred because of their excellent transmittance of visible light and near infrared light.
[0015] The thickness of the substrate 1 is preferably 10 to 500 μm, more preferably 30 to 100 μm. When the thickness of the substrate 1 is equal to or greater than the lower limit of the above-mentioned numerical range, a stray light prevention film having excellent mechanical strength is easily obtained. When the thickness of the substrate 1 is equal to or less than the upper limit of the above-mentioned numerical range, a stray light prevention film having excellent formability to curved surfaces is easily obtained.
[0016] Examples of the method for producing the substrate include injection molding, extrusion molding, cast molding, etc. Among these, extrusion molding and cast molding are preferred because of their excellent productivity. The surface of the substrate may be subjected to a coating treatment, a corona treatment, a printing treatment, etc. for the purpose of improving properties such as adhesion, antistatic properties, scratch resistance, weather resistance, and design properties.
[0017] The stray light prevention film 10A has a fine uneven structure 3, a so-called moth-eye structure, in which the average interval between convex portions formed on the surface 1a of the substrate 1 is equal to or less than the wavelength of visible light. The fine uneven structure 3 imparts anti-reflection performance to the stray light prevention film 10A.
[0018] The fine concave-convex structure 3 is composed of a plurality of convex portions 13 and concave portions formed between the plurality of convex portions 13 . The average interval between adjacent convex portions 13 of the fine concave-convex structure is equal to or less than the wavelength of visible light. The average interval is preferably 20 nm to 400 nm, more preferably 80 nm to 250 nm. When the average interval between adjacent convex portions 13 of the fine concave-convex structure is equal to or more than the lower limit of the above-mentioned numerical range, the convex portions 13 are easily formed when the convex portions 13 are formed by transferring a plurality of pores of anodized porous alumina. When the average interval between adjacent convex portions 13 of the fine concave-convex structure is equal to or less than the upper limit of the above-mentioned numerical range, the voltage for increasing the pore interval can be suppressed when the convex portions 13 are formed by transferring a plurality of pores of anodized porous alumina, and the anodized porous alumina can be easily manufactured industrially. When the average interval between adjacent convex portions 13 of the fine concave-convex structure is equal to or less than 250 nm, the generation of unnecessary diffracted light can be suppressed. The average spacing between adjacent protrusions 13 is determined by measuring the spacing between adjacent protrusions 13 (the distance from the center of a protrusion 13 to the center of an adjacent protrusion 13) at 10 random points using an electron microscope and averaging these values.
[0019] The average height of the bumps 13 is preferably 100 nm to 500 nm, and more preferably 150 nm to 400 nm. When the average height of the bumps 13 is equal to or greater than the lower limit of the aforementioned numerical range, increases in the minimum reflectance and the reflectance of visible light and near-infrared light can be suppressed, resulting in excellent anti-reflection performance. When the average height of the bumps 13 is equal to or less than the upper limit of the aforementioned numerical range, the bumps 13 are easy to form, and the bumps 13 have excellent scratch resistance. The average height of the protrusions 13 is determined by measuring the vertical distance between the top of the protrusion 13 and the bottom of the adjacent recess at 10 random points using an electron microscope, and averaging these values.
[0020] The aspect ratio of the bumps 13 (average height of the bumps 13 / average distance between adjacent bumps 13) is preferably 0.8 to 5.0, more preferably 1.2 to 4.0, and even more preferably 1.5 to 3.0. When the aspect ratio of the bumps 13 is equal to or greater than the lower limit of the above-mentioned numerical range, the antireflection performance is excellent. When the aspect ratio of the bumps 13 is equal to or less than the upper limit of the above-mentioned numerical range, the bumps 13 are easy to form, and the bumps 13 have excellent scratch resistance.
[0021] Examples of the shape of the convex portion include a cone shape, a pyramid shape, a bell shape, and a cylinder shape. These shapes of the convex portion 13 may be used alone or in combination of two or more. Among these shapes of the convex portion 13, a shape in which the cross-sectional area of the convex portion 13 in a direction perpendicular to the height direction increases continuously from the apex in the depth direction is preferred, since it is possible to continuously increase the refractive index from the air to the surface of the material forming the fine uneven structure, thereby achieving anti-reflection performance that combines low reflectance and low wavelength dependency, and a cone shape, a pyramid shape, and a bell shape are more preferred. The convex portion may be one in which a plurality of fine convex portions are united to form one convex portion.
[0022] Examples of methods for forming the fine uneven structure include the following methods A1 to A3. Method A1: A method in which a microrelief structure is formed directly on the surface of a substrate by injection molding or press molding using a mold having an inverted structure of the microrelief structure on its surface. Method A2: A method in which an active energy ray-curable composition is sandwiched between a mold having an inverted structure of a microrelief structure and a substrate, the active energy ray-curable composition is cured to form a cured resin layer, and then the cured resin layer and the mold are separated. Method A3: A method in which an active energy ray-curable composition is sandwiched between a mold having an inverted structure of a fine relief structure and a substrate, the fine relief structure of the mold is transferred to the active energy ray-curable composition, the mold is then separated, and the active energy ray-curable composition is cured to form a cured resin layer. Among the methods for producing a fine concave-convex structure, methods A2 and A3 are preferred, and method A2 is more preferred, because they are excellent in transferability of the fine concave-convex structure and have a high degree of freedom in surface composition.
[0023] Examples of the mold include a mold having a microrelief structure formed on its surface by lithography, a mold having a microrelief structure formed on its surface by laser processing, a mold having anodized porous alumina with multiple pores formed on its surface, and a replica mold replicated from a mother mold having a microrelief structure by electroforming or the like. Among these molds, a mold having anodized porous alumina with multiple pores formed on its surface is preferred because it has excellent antireflection performance and is easy to form a large-area microrelief structure at low cost.
[0024] Examples of the lithography method include electron beam lithography and laser interference lithography. Examples of methods for producing a mold having an inverted microrelief structure on its surface by lithography include a method in which a photoresist film is applied to the surface of a substrate, and the photoresist film is exposed to an ultraviolet laser, an electron beam, an X-ray, or the like, and then developed to obtain a mold having a microrelief structure on its surface consisting of a resist pattern; and a method in which the substrate is selectively etched by dry etching or the like through the resist pattern, and the resist pattern is removed to obtain a mold having a microrelief structure formed directly on the surface of the substrate.
[0025] Examples of methods for manufacturing a mold having anodized porous alumina with a plurality of pores formed on its surface include a method in which aluminum is anodized at a predetermined voltage using an electrolyte such as oxalic acid, sulfuric acid, or phosphoric acid.
[0026] As a method for producing a mold having anodized porous alumina formed on the surface, for example, there is a method in which aluminum is anodized at a predetermined voltage using oxalic acid, sulfuric acid, phosphoric acid or the like as an electrolyte. According to a method of anodizing aluminum at a predetermined voltage using an electrolyte such as oxalic acid, sulfuric acid, or phosphoric acid, it is possible to form pores in high purity aluminum that are not rectangular in cross section but triangular or bell-shaped by combining anodizing and pore size expansion treatment. Furthermore, it is possible to make the angle of the innermost part of the pores sharp by appropriately adjusting the time, number of times, conditions, etc. of anodizing and pore size expansion treatment. An example of a method for producing a mold having anodized porous alumina formed on its surface is the method described in JP 2015-129706 A.
[0027] Examples of the shape of the mold include a flat plate, a belt, a roll, etc. Among these mold shapes, the belt and roll are preferred because they allow the fine concave-convex structure to be transferred continuously and are excellent in productivity of the substrate.
[0028] The fine unevenness is preferably made of a cured resin layer, since it is possible to form the fine unevenness more easily. The cured resin layer is a layer made of a cured product of an active energy ray-curable composition.
[0029] The active energy ray-curable composition is a composition that undergoes a polymerization reaction and is cured when irradiated with active energy rays. Examples of active energy rays include visible light, ultraviolet light, electron beams, plasma, heat rays (infrared rays, etc.), etc. Among these active energy rays, ultraviolet light and electron beams are preferred, and ultraviolet light is more preferred, since they provide excellent curing properties for the active energy ray-curable composition.
[0030] The active energy ray-curable composition preferably contains a polymerizable compound, a polymerization initiator, and, if necessary, other additives.
[0031] Examples of the polymerizable compound include monomers, oligomers, reactive polymers, etc., each of which contains at least one of a radical polymerizable bond and a cationic polymerizable bond in the molecule. The polymerizable compound may be used alone or in combination of two or more kinds.
[0032] Examples of the monomer having a radical polymerizable bond include monofunctional monomers having a (meth)acryloyl group, a vinyl group, etc., and polyfunctional monomers having a (meth)acryloyl group, a vinyl group, etc. The monomer having a radical polymerizable bond may be used alone or in combination of two or more kinds. (Meth)acrylic is a general term for acrylic and methacrylic.
[0033] Examples of the monomer having a cationic polymerizable bond include a monomer having an epoxy group, an oxetanyl group, an oxazolyl group, a vinyloxy group, etc. The monomer having a cationic polymerizable bond may be used alone or in combination of two or more kinds.
[0034] Examples of oligomers or reactive polymers containing at least one of radically polymerizable bonds and cationic polymerizable bonds in the molecule include unsaturated polyester compounds such as condensates of unsaturated dicarboxylic acids and polyhydric alcohols; polyester (meth)acrylates; polyether (meth)acrylates; polyol (meth)acrylates; epoxy (meth)acrylates; urethane (meth)acrylates; cationic polymerization type epoxy compounds; homopolymers or copolymers of monomers having the above radically polymerizable bonds in their side chains, etc. The oligomers or reactive polymers containing at least one of radically polymerizable bonds and cationic polymerizable bonds in the molecule may be used alone or in combination of two or more.
[0035] Examples of the polymerization initiator include a photopolymerization initiator, an electron beam polymerization initiator, and a thermal polymerization initiator. These polymerization initiators may be used alone or in combination of two or more. The other additives are not particularly limited, but examples thereof include non-reactive polymers, antioxidants, release agents, lubricants, plasticizers, antistatic agents, light stabilizers, flame retardants, flame retardant assistants, polymerization inhibitors, ultraviolet absorbers, fillers, silane coupling agents, reinforcing agents, inorganic fillers, and impact resistance modifiers. The other additives may be used alone or in combination of two or more.
[0036] When imparting water repellency to the surface of the fine unevenness structure, it is preferable to use a fluorine-containing compound or a silicone-based compound as an active energy ray curable composition capable of forming a hydrophobic material. To impart water repellency means to make the contact angle between the fine unevenness structure and water 120 degrees or more. If the surface is water repellent, when the surface is used in a photographing device or a measuring device, even if fogging occurs due to temperature change or in a high humidity environment, the surface can be dried quickly to suppress a decrease in detection sensitivity and visibility.
[0037] When imparting hydrophilicity to the surface of the fine unevenness structure, it is preferable to use a combination of a polyfunctional (meth)acrylate having tetrafunctional or more and a hydrophilic (meth)acrylate having difunctional or more as an active energy ray curable composition capable of forming a hydrophilic material. The term "hydrophilicity" refers to making the contact angle between the fine unevenness structure and water 30 degrees or less. If the material is hydrophilic, when the material is used in a photographic device or a measuring device, fogging due to temperature changes or in a high humidity environment can be suppressed, and a decrease in detection sensitivity and visibility can be suppressed.
[0038] The composition of the active energy ray-curable composition is not particularly limited. For example, the compositions described in JP-A-2013-175733 and JP-A-2015-129947 can be used as reference.
[0039] Examples of a method for sandwiching the active energy ray-curable composition between a mold and a substrate include a method in which the active energy ray-curable composition is placed between the mold and the substrate, and the mold and the substrate are pressed together to inject the active energy ray-curable composition into the fine uneven structure of the mold.
[0040] (Adhesive layer) As in the stray light prevention film 10A shown in FIG. 1, the stray light prevention film according to the preferred embodiment may further have an adhesive layer on the opposite side to the surface on which the fine uneven structure is formed. The adhesive layer has a function of imparting adhesiveness to the stray light prevention film. The adhesive layer can be formed, for example, by curing an adhesive composition. A preferred adhesive composition includes an acrylic resin. The acrylic resin is not particularly limited, and various acrylic resins can be used. In order to apply the stray light prevention film to a curved surface, the adhesive composition may be capable of being cured in stages two or more times, that is, may exhibit multi-stage curing properties.
[0041] The adhesive layer may contain a colorant to block visible light and / or near infrared light. If visible light and / or near infrared light can be blocked, the reflectance of visible light and near infrared light can be further reduced.
[0042] The colorant may be any coloring material such as a pigment or a dye, but a pigment can be preferably used. Specifically, for example, black coloring materials include carbon black (furnace black, channel black, acetylene black, thermal black, lamp black, pine smoke, etc.), graphite, copper oxide, manganese dioxide, aniline black, perylene black, titanium black, cyanine black, activated carbon, ferrite (non-magnetic ferrite, magnetic ferrite, etc.), magnetite, chromium oxide, iron oxide, molybdenum disulfide, chromium complex, composite oxide black pigment, anthraquinone organic black pigment, etc. Among them, carbon black is preferable from the viewpoint of cost and availability. The black coloring materials can be used alone or in combination of two or more.
[0043] In addition to the above, additives may be added to the colored layer as necessary, such as antioxidants, light stabilizers, plasticizers, softeners, fillers, and flame retardants.
[0044] (Micro-relief structure formed on a relief structure) The stray light prevention film according to a preferred embodiment may further have a concave-convex structure having an arithmetic mean roughness Ra of 0.010 μm or more and less than 1.00 μm and a period Sm of 10 to 300 μm. By forming a fine concave-convex structure on the concave-convex structure, the reflectance of visible light and near-infrared light can be further reduced.
[0045] The stray light prevention film 10B shown in Fig. 2 has a substrate 1, a concave-convex structure 2, a fine concave-convex structure 4, and an adhesive layer 5. The concave-convex structure 2 is formed on a surface 1a of the substrate 1, and the fine concave-convex structure 4 is formed on the concave-convex structure 2.
[0046] The arithmetic mean roughness Ra of the uneven structure 2 is 0.010 μm or more and less than 1.00 μm, preferably 0.050 to 0.90 μm, and more preferably 0.10 to 0.80 μm. When the arithmetic mean roughness Ra is equal to or more than the lower limit of the above-mentioned numerical range, the gloss is extremely reduced and reflection can be suppressed. Thus, stray light can be prevented. When the arithmetic mean roughness Ra is equal to or less than the upper limit of the above-mentioned numerical range, the uneven structure formed by curing the active energy ray-curable composition can be easily released from the mold, improving productivity. Moreover, unnecessary scattering can be suppressed and reflection is also reduced. Thus, stray light can be prevented. The arithmetic mean roughness Ra is a value measured according to JIS B 0601:2001 (ISO 4287:1997).
[0047] The period Sm of the uneven structure 2 is 10 to 300 μm, preferably 70 to 200 μm, and more preferably 80 to 150 μm. When the period Sm is equal to or greater than the lower limit of the above-mentioned numerical range, the gloss is extremely reduced and reflection can be suppressed. Thus, stray light can be prevented. When the period Sm is equal to or less than the upper limit of the above-mentioned numerical range, the uneven structure formed by curing the active energy ray-curable composition can be easily released from the mold, improving productivity. Moreover, excessive scattering can be suppressed and reflection is also reduced. Thus, stray light can be prevented. The period is a value measured according to JIS B 0601:2001 (ISO 4287:1997).
[0048] Methods for forming the concave-convex structure 2 and the fine concave-convex structure 3 include the same methods as the above-mentioned methods A1 to A3, except that a stamper having an inverted structure of the fine concave-convex structure formed on the concave-convex structure is used as a mold. The stamper can be manufactured, for example, by blasting the surface to be processed of an aluminum base material and then anodizing the treated surface. For details of the blasting and anodizing for manufacturing the stamper, see, for example, International Publication No. WO 2013 / 099935.
[0049] The arithmetic mean roughness Ra of the uneven structure 2 can be adjusted by the blasting conditions such as the distance r from the tip of the discharge nozzle to the surface of the aluminum base material to be blasted, the discharge pressure at which the abrasive is discharged, etc. Specifically, the arithmetic mean roughness Ra tends to increase when the distance r and / or the discharge pressure is increased, and the arithmetic mean roughness Ra tends to decrease when the distance r and / or the discharge pressure is decreased.
[0050] The period Sm of the uneven structure 2 can be adjusted by the density at which the abrasive is discharged onto the aluminum substrate in the blasting process, and the discharge density of the abrasive can be adjusted by the moving speed of the discharge nozzle, the supply amount of the abrasive, etc. Specifically, the period Sm tends to increase when the blasting operation pitch is made loose, and the period Sm tends to decrease when the blasting operation pitch is made tight. In addition, the period Sm tends to increase when the particle diameter of the abrasive is increased, and the period Sm tends to decrease when the particle diameter is decreased.
[0051] (Ink layer) The stray light prevention film according to the preferred embodiment may further have an ink layer on the opposite side of the surface on which the fine relief structure is formed. If the ink layer can block visible light and / or near infrared light, the reflectance of visible light and near infrared light can be further reduced.
[0052] The ink layer is a layer containing a resin ink. The ink layer may be a single layer or a multi-layer structure. In one example, a plurality of ink layers of different colors may be formed on the back surface of the substrate to form a printed image such as a photograph, a picture, a letter, a number, etc.
[0053] The resin ink contains a resin, a colorant, and a solvent. The resin ink may further contain additives as necessary. Resin inks can be roughly divided into oil-based and water-soluble inks. The resin ink used in the present invention may be either oil-based or water-soluble, but oil-based inks are preferred in terms of excellent compatibility with substrates. As the oil-based ink or water-soluble ink, a known ink used for forming a printed image can be used. In addition, a commercially available product can be used. An example of each component contained in the oil-based ink and water-soluble ink will be described in detail below.
[0054] Oil-based inks: Resins contained in oil-based inks include thermoplastic resins such as acrylic resins, maleic acid resins, rosin resins, epoxy resins, silicone resins, butyral resins, etc. Colorants contained in oil-based inks include dyes such as azo-based metal complexes and phthalocyanines, and pigments such as carbon black and organic pigments. The solvent contained in the oil-based ink is an organic solvent such as ketone, alcohol, ethyl acetate, etc. In particular, alcohol having a penetrating property is preferable, and it is possible to reduce the difference in refractive index at the interface with the light-transmitting substrate 12. Examples of additives contained in oil-based inks include a conductivity imparting agent, a plasticizer, an antioxidant, and an ultraviolet absorbing agent.
[0055] Water-soluble inks: The resin contained in the water-soluble ink may be, for example, an acrylic block copolymer. Examples of colorants contained in the water-soluble ink include dyes such as anionic azo dyes and phthalocyanine; and pigments such as carbon black and organic pigments. The solvent contained in the water-soluble ink is water. The water may also contain glycerin or glycol, which acts as an anti-drying agent, or alcohol or glycol ether, which acts as a penetrating agent. In particular, if the water contains a penetrating agent, the refractive index difference at the interface with the substrate can be reduced. Additives contained in water-soluble inks include, for example, pH adjusters such as alcohol amines and sodium hydroxide; chelating agents such as EDTA; surfactants such as nonionic surfactants, cationic surfactants, and anionic surfactants; and antibacterial and antifungal agents.
[0056] The printing method of the ink layer is not particularly limited, and a known method can be adopted. For example, it includes plateless printing such as inkjet printing, thermal transfer (ink ribbon) printing, and laser printer printing; stencil printing such as screen printing; lithographic printing such as offset printing; relief printing such as letterpress printing and flexographic printing; and intaglio printing such as gravure printing. In addition, the ink layer may be formed using a seal or stamp, or may be formed by simple drawing.
[0057] (film, sheet) The stray light prevention film according to the preferred embodiment may further have a film or sheet attached via an adhesive layer to the opposite side of the surface on which the fine unevenness structure is formed. If the film or sheet can block visible light and / or near infrared light, the reflectance of visible light and near infrared light can be further reduced. In order to block visible light and / or near infrared light, the film or sheet preferably contains the same colorant as the adhesive layer.
[0058] The material of the film and sheet is not particularly limited, but examples include acrylic resins such as polymethyl methacrylate; polycarbonate resins; styrene resins such as polystyrene and methyl methacrylate-styrene copolymers; cellulose resins such as cellulose diacetate, cellulose triacetate, and cellulose acetate butyrate; polyester resins such as polyethylene terephthalate; polyamide resins; polyimide resins; polyethersulfone resins; polysulfone resins; polyolefin resins such as polypropylene, polymethylpentene, and alicyclic polyolefins; vinyl chloride resins such as polyvinyl chloride; polyvinyl acetal resins; polyether ketone resins; and polyurethane resins.
[0059] Although the embodiments have been described above by showing several example embodiments, the present invention is not limited to the example embodiments disclosed in this specification, and can be appropriately modified and implemented without departing from the gist of the invention. The embodiments disclosed in this specification can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the gist of the invention. EXAMPLES
[0060] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following description.
[0061] <Measurement method> (Measurement of arithmetic mean roughness Ra and period Sm) The arithmetic mean roughness Ra and period Sm of the rough uneven structure on the stray light prevention film were obtained in accordance with JIS B 0601:2001 (ISO 4287:1997). A stylus roughness meter ("SUPERCOM1400LCD" manufactured by Tokyo Seimitsu Co., Ltd.) was used for the measurement.
[0062] (Dimensions of the micro-relief structure of the anti-reflection layer including the moth-eye structure) Platinum was evaporated onto the longitudinal section or surface of the antireflection layer containing the moth-eye structure on which the transfer surface was formed, and the transfer surface of the antireflection layer containing the moth-eye structure was observed using a scanning electron microscope (manufactured by JEOL Ltd., "JSM-7400F") at an acceleration voltage of 3.00 kV. From the obtained image, the period and height of the convexities originating from the fine unevenness structure of the mold formed on the transfer surface were measured at 10 points, and the average value was calculated.
[0063] (reflectance) The spectrophotometer (Shimadzu Corporation, "UV-2450") was used to measure the regular reflectance of the surface (fine relief structure surface) of the antireflection layer containing the moth-eye structure at an incident angle of 5 degrees and in the wavelength range of 380 nm to 900 nm. The spectrophotometer (Hitachi High-Tech Corporation, "UH-4150") was used to measure the total reflectance of the surface (fine relief structure surface) of the antireflection layer containing the moth-eye structure at an incident angle of 8 degrees and in the wavelength range of 380 nm to 900 nm.
[0064] <Example 1> (Mold manufacturing) An aluminum ingot with a purity of 99.99% was cut to an outer diameter of 200 mm, an inner diameter of 155 mm, and a length of 350 mm to prepare a cylindrical aluminum base material without rolling marks. The obtained aluminum base material was anodized for 10 minutes in a 0.3 M oxalic acid aqueous solution at a DC voltage of 40 V and a temperature of 16 ° C. The obtained aluminum base material was immersed in a 5 mass % phosphoric acid aqueous solution at 30 ° C. for 8 minutes to perform a pore diameter expansion treatment (pore diameter expansion treatment step). Thereafter, the aluminum base material was anodized for 30 seconds in a 0.3 M oxalic acid aqueous solution at a DC voltage of 40 V and a temperature of 16 ° C. (oxide film growth step). This pore diameter expansion treatment step and oxide film growth step were repeated a total of four times, and finally, the pore diameter expansion treatment step was performed to obtain a roll-shaped mold on the surface of which anodized alumina having approximately conical pores with an average interval of 100 nm and a depth of 200 nm was formed.
[0065] (Preparation of active energy ray-curable composition) 25 parts by mass of dipentaerythritol hexaacrylate, 25 parts by mass of pentaerythritol triacrylate, 25 parts by mass of polyethylene glycol diacrylate, and 25 parts by mass of an ethylene oxide modified compound of dipentaerythritol hexaacrylate were mixed. Furthermore, 1 part by mass of a first photopolymerization initiator (trade name "Irgacure 184", manufactured by BASF) and 0.5 parts by mass of a second photopolymerization initiator (trade name "Irgacure 819", manufactured by BASF) were added and mixed to prepare an active energy ray curable composition.
[0066] (Production of anti-reflective layer containing moth-eye structure) The obtained roll-shaped mold was rotated, and a cellulose triacetate substrate (product name "TD80UL", manufactured by Fujifilm Corporation, thickness 80 μm) was run along the outer peripheral surface of the mold in the rotation direction of the mold, while an active energy ray curable composition was supplied between the outer peripheral surface of the mold and the running substrate, and the active energy ray curable composition was cured by irradiating with ultraviolet rays. The obtained cured product was peeled off from the mold to produce an antireflection layer including a moth-eye structure. The back surface of the substrate on which the antireflection layer including a moth-eye structure was formed was attached to a black acrylic plate via a transparent adhesive layer (OCA), and the reflectance was measured. (Table 2, Example 1-(1)).
[0067] (Manufacture of anti-stray light film) The anti-reflection layer containing the moth-eye structure was attached to a black polyester film "Lumirror R#25-X36" via an adhesive layer to obtain a stray light prevention film. When the surface of the obtained stray light prevention film was observed with a scanning electron microscope, fine convex portions with a period of 100 nm and a height of 190 nm were formed. The reflectance was also measured. (Table 2, Example 1-(2)).
[0068] <Example 2> (Stamper manufacturing) A cylindrical aluminum substrate without rolling marks was prepared by cutting an aluminum ingot with a purity of 99.99% to an outer diameter of 200 mm, an inner diameter of 155 mm, and a length of 350 mm. Next, the aluminum substrate was blasted using glass beads (Potters Ballotini Co., Ltd., "J220", particle size range 45-75 μm) as a spherical abrasive without sharp edges under the conditions of a discharge pressure of 0.05 MPa, an operation pitch of 2.5 mm, a moving speed of the discharge nozzle of 20 m / min, and a distance of 500 mm from the tip of the discharge nozzle to the surface of the aluminum substrate to be blasted. The blasted aluminum substrate was then anodized for 10 minutes in a 0.3 M oxalic acid solution at a DC voltage of 40 V and a temperature of 16°C. The aluminum substrate was then immersed in a 5% by mass phosphoric acid solution at 30°C for 8 minutes to perform a pore size expansion treatment (pore size expansion treatment process). Thereafter, the aluminum substrate was anodized in a 0.3 M oxalic acid aqueous solution at a DC voltage of 40 V and a temperature of 16° C. for 30 seconds (oxide film growth step). This pore size expansion treatment step and oxide film growth step were repeated a total of four times, and finally, a pore size expansion treatment step was performed to obtain a roll-shaped stamper.
[0069] (Preparation of active energy ray-curable composition) An active energy ray-curable composition having the same composition as in Example 1 was prepared by the same method.
[0070] (Production of anti-reflective layer containing moth-eye structure) An antireflection layer including a moth-eye structure was produced in the same manner as in Example 1, except that the roll-shaped stamper of Example 2 was used. The back surface of the substrate on which the antireflection layer including the moth-eye structure was formed was attached to a black acrylic plate via a transparent adhesive layer (OCA), and the reflectance was measured (Table 2, Example 2-(1)).
[0071] (Manufacture of anti-stray light film) A stray light prevention film was produced in the same manner as in Example 1, except that the antireflection layer including the moth-eye structure according to Example 2 was used. When the surface of the stray light prevention film was observed with a scanning electron microscope, fine convex portions with a period of 100 nm and a height of 190 nm were formed. The surface of the stray light prevention film was also measured with a stylus roughness meter, and the results were recorded as the arithmetic mean roughness Ra and period Sm. The reflectance was also measured (Table 2, Example 2-(2)).
[0072] <Examples 3 and 4> An antireflection layer and an anti-stray light film including a moth-eye structure were manufactured in the same manner as in Example 2, except that the blasting conditions during the manufacture of the stamper were changed as shown in Table 1. Regarding the abrasives shown in Table 1, J90 is glass beads manufactured by Potters Ballotini Co., Ltd., and has a particle size range of 125 to 180 μm. J100 is glass beads manufactured by Potters Ballotini Co., Ltd., and has a particle size range of 106 to 150 μm. As for the reflectance, it was found from the results of Examples 1 and 2 that there was no significant difference in the measured value between the case where the back surface of the substrate on which the anti-reflection layer including the moth-eye structure was formed was attached to a black acrylic plate via a transparent adhesive layer (OCA) and the case where the substrate was used as a stray light prevention film. Therefore, in Examples 3 and 4, the measurement was performed only when the back surface of the substrate on which the anti-reflection layer including the moth-eye structure was formed was attached to a black acrylic plate via a transparent adhesive layer (OCA).
[0073] [Table 1]
[0074] <Comparative Example 1> The subject of the analysis was Shibuya Optical Products Co., Ltd.'s light-blocking, anti-reflection black film SNR-T50.
[0075] <Comparative Example 2> The subject of the analysis was Shibuya Optical Products Co., Ltd.'s light-blocking, anti-reflective black film SBIR-S.
[0076] <Result> Table 2 shows the measurement results for the 8-degree total reflectance of 550 nm visible light, the 8-degree total reflectance of 800 nm near-infrared light, the 5-degree specular reflectance of 550 nm visible light, and the 5-degree specular reflectance of 800 nm near-infrared light for each example.
[0077] [Table 2]
[0078] In the stray light prevention films of Examples 1 to 4, the 5-degree regular reflectance and the 8-degree total reflectance at 550 nm and 800 nm were good. In contrast, in the films of Comparative Examples 1 and 2, the 5-degree regular reflectance and the 8-degree total reflectance at 550 nm and 800 nm were high. [Industrial Applicability]
[0079] According to the present invention, a stray light prevention film having reduced reflectance for visible light and near infrared light is provided. By installing the stray light prevention film of the present invention inside an optical device, stray light can be effectively reduced or prevented, and the occurrence of flare and ghosting can be prevented. [Explanation of symbols]
[0080] 1 Base material 2 Uneven structure 3 Fine uneven structure 4 Fine uneven structure 5 Adhesive layer 10. Stray light prevention film 13 Convex
Claims
1. A stray light prevention film, The stray light prevention film has a fine uneven structure formed on a surface thereof, the average interval between the convex portions being equal to or less than the wavelength of visible light, The 8-degree total reflectance of visible light at 550 nm is 0.50% or less, and A stray light prevention film having an 8-degree total reflectance of 1.0% or less for near-infrared light of 800 nm.
2. The 5-degree regular reflectance of visible light of 550 nm is 0.10% or less, and 2. The stray light prevention film according to claim 1, having a 5-degree regular reflectance of near-infrared light of 800 nm of 0.30% or less.
3. The uneven structure further has an arithmetic mean roughness Ra of 0.010 μm or more and less than 1.00 μm and a period Sm of 10 to 300 μm, The stray light prevention film according to claim 1 or 2, wherein the fine concave-convex structure is formed on the concave-convex structure.
4. The stray light prevention film according to claim 3, wherein the period Sm of the uneven structure is 70 to 200 μm.
5. Further, the adhesive layer is provided on the opposite side of the surface on which the microrelief structure is formed, The stray light prevention film according to claim 1 or 2, wherein the adhesive layer is capable of blocking visible light and / or near infrared light.
6. The present invention further includes a film or sheet adhered via an adhesive layer to the opposite side of the surface on which the microrelief structure is formed, The stray light prevention film according to claim 1 or 2, wherein the film or sheet is capable of blocking visible light and / or near-infrared light.
7. Further, the ink layer is provided on the opposite side to the surface on which the fine uneven structure is formed, The stray light prevention film according to claim 1 or 2, wherein the ink layer is capable of blocking visible light and / or near infrared light.
8. The stray light prevention film according to claim 1 or 2, wherein the surface on which the fine uneven structure is formed has a contact angle with water of 30 degrees or less.
9. A method for preventing stray light, comprising installing the stray light prevention film according to claim 1 or 2 inside an optical device.
Citation Information
Patent Citations
Stray light preventing film
JP1998332907A
Stray Light Absorption Film