Aluminum electrolytic capacitor for cooling immersion liquid, sealing body, and cooling method of electronic apparatus

By employing a rubber member with a Hansen solubility parameter distance of 8.0 or more, aluminum electrolytic capacitors can withstand hydrocarbon refrigerants in liquid immersion cooling, addressing swelling issues and maintaining airtightness.

JP2024133015APending Publication Date: 2024-10-01NIPPON CHEMI CON CORP

Patent Information

Application Number
JP2024040110
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-14
Filing Date
2024-03-14
Publication Date
2024-10-01

Smart Images

  • Figure 2024133015000001_ABST
    Figure 2024133015000001_ABST
Patent Text Reader

Abstract

To provide an aluminum electrolytic capacitor which can be adopted to an immersion liquid cooling system using a hydrocarbon system cooling medium as a cooling liquid.SOLUTION: In an aluminum electrolytic capacitor for cooling an immersion liquid supplied for cooling a cooling liquid, the cooling liquid is a hydrocarbon system cooling medium, a sealing body of the aluminum electrolytic capacitor includes a rubber member in a region contacted to the cooling liquid when cooling the immersion liquid. The rubber member is formed by a rubber component or their vulcanization material containing a rubber component of which a Hansen solubility parameter distance from the cooling liquid is 8.0 or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an aluminum electrolytic capacitor that is subjected to liquid immersion cooling, a sealing body for the aluminum electrolytic capacitor, and a cooling method for an electronic device having the aluminum electrolytic capacitor. [Background technology]

[0002] There are two types of technologies for cooling electronic devices, such as supercomputers and server devices, that generate heat during operation: air-cooled systems that use air to cool the electronic devices, and liquid immersion cooling systems that immerse the electronic devices in a cooling liquid to cool them. Liquid immersion cooling systems use a liquid as a coolant that has a higher thermal conductivity than air, so they generally have a higher cooling efficiency than air-cooled systems and have been attracting attention in recent years as a technology that contributes to reducing power consumption.

[0003] Known coolants used in immersion cooling systems include fluorine-based insulating refrigerants such as 1,1,1,3,3,3-hexafluoroisopropyl methyl ether and 1,1,2,3,3,3-hexafluoropropyl methyl ether (Patent Document 1). Immersion cooling systems using fluorine-based insulating refrigerants have the advantage of being excellent in terms of maintenance, including inspection and repair of electronic devices. For this reason, fluorine-based insulating refrigerants are the refrigerants most widely used for immersion cooling systems today. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2022-169554 A Summary of the Invention [Problem to be solved by the invention]

[0005] As described above, although the fluorine-based insulating refrigerant is highly convenient, it is expensive, and therefore, replacement with cheaper cooling liquids other than the fluorine-based insulating refrigerant is being considered. As a promising cooling liquid to replace the fluorine-based insulating refrigerant, for example, a hydrocarbon-based refrigerant can be given.

[0006] Here, in electronic devices, aluminum electrolytic capacitors, which have a large capacitance and are inexpensive, are widely used. Aluminum electrolytic capacitors are formed by inserting a capacitor element into a metal case and sealing the opening of the metal case with a sealing body. The sealing body used in aluminum electrolytic capacitors is often made of rubber such as ethylene propylene rubber and butyl rubber, or has a rubber member made of rubber such as ethylene propylene rubber and butyl rubber. However, since these rubbers are easily affected by organic refrigerants, when an aluminum electrolytic capacitor having such a sealing body is subjected to liquid immersion cooling, the sealing body may expand, causing problems such as deterioration of the aluminum electrolytic capacitor. For this reason, aluminum electrolytic capacitors are considered to be capacitors that are difficult to apply to liquid immersion cooling systems, and in particular, no aluminum electrolytic capacitor that can withstand liquid immersion cooling using a hydrocarbon-based refrigerant has been known so far.

[0007] In view of the above, an object of the present disclosure is to provide an aluminum electrolytic capacitor that can be used in an immersion cooling system that uses a hydrocarbon-based refrigerant as the coolant. [Means for solving the problem]

[0008] As a result of extensive research aimed at solving the above problems, the present inventors have found that by applying a rubber component having a Hansen solubility parameter distance with respect to a coolant of a specific value or more to the rubber member of the sealing body, it is possible to provide an aluminum electrolytic capacitor that is highly stable against a coolant.

[0009] [1] An aluminum electrolytic capacitor for liquid immersion cooling that is cooled in a cooling liquid, The cooling liquid is a hydrocarbon refrigerant, a sealing body of the aluminum electrolytic capacitor having a rubber member in a region that comes into contact with the cooling liquid during immersion cooling, The rubber member is made of a rubber composition or a vulcanizate thereof, the rubber composition containing a rubber component having a Hansen solubility parameter distance with respect to the cooling liquid of 8.0 or more. [2] The aluminum electrolytic capacitor for liquid immersion cooling according to [1], wherein the rubber component is at least one selected from the group consisting of nitrile rubber, hydrogenated nitrile rubber, acrylic rubber, and fluororubber. [3] The aluminum electrolytic capacitor for liquid immersion cooling according to [1] or [2], wherein the rubber component contains more than 0% by weight and not more than 65% by weight of a rubber having a Hansen solubility parameter distance with the coolant of less than 8.0, based on the total amount of the rubber component. [4] The sealing body is used in the aluminum electrolytic capacitor for liquid immersion cooling according to any one of [1] to [3]. [5] A method for cooling an aluminum electrolytic capacitor, comprising the steps of: a liquid immersion cooling step of immersing the aluminum electrolytic capacitor in a cooling liquid to cool it, The cooling liquid is a hydrocarbon refrigerant, a sealing body of the aluminum electrolytic capacitor having a rubber member in a region that comes into contact with the cooling liquid during immersion cooling, The method for cooling an aluminum electrolytic capacitor, wherein the rubber member is made of a rubber composition or a vulcanizate thereof, which contains a rubber component having a Hansen solubility parameter distance with the coolant of 8.0 or more. [6] The aluminum electrolytic capacitor is mounted on an electronic device, The cooling method for an aluminum electrolytic capacitor according to [5], wherein the immersion cooling step is carried out by immersing a part or all of the electronic device in the cooling liquid. [7] A method for cooling an electronic device having an aluminum electrolytic capacitor, comprising the steps of: a liquid immersion cooling step of immersing a part or the whole of the electronic device in a cooling liquid to cool it, the liquid immersion cooling step is performed such that at least the aluminum electrolytic capacitor is immersed in the cooling liquid; The cooling liquid is a hydrocarbon refrigerant, a sealing body of the aluminum electrolytic capacitor having a rubber member in a region that comes into contact with the cooling liquid during immersion cooling, The method for cooling an electronic device, wherein the rubber member is made of a rubber composition or a vulcanizate thereof, which contains a rubber component having a Hansen solubility parameter distance with respect to the cooling liquid of 8.0 or more. [8] A method for producing an aluminum electrolytic capacitor for liquid immersion cooling, which is subjected to liquid immersion cooling in a hydrocarbon-based refrigerant and has a sealing body provided with a rubber member, comprising the steps of: a sealing step of sealing the capacitor element with the sealing body, In the sealing step, the sealing body is disposed so that the rubber member is located in a region that comes into contact with the hydrocarbon-based refrigerant during the immersion cooling; The method for producing an aluminum electrolytic capacitor for liquid immersion cooling, wherein the rubber member is made of a rubber composition or a vulcanizate thereof, which contains a rubber component having a Hansen solubility parameter distance with the hydrocarbon refrigerant of 8.0 or more. [9] The method for producing an aluminum electrolytic capacitor for liquid immersion cooling according to [8], wherein the rubber component is at least one selected from the group consisting of nitrile rubber, hydrogenated nitrile rubber, acrylic rubber, and fluororubber.

[10] The method for producing an aluminum electrolytic capacitor for liquid immersion cooling according to [8] or [9], wherein the rubber component contains more than 0 wt% and not more than 65 wt% of a rubber having a Hansen solubility parameter distance with the hydrocarbon refrigerant of less than 8.0, based on a total amount of the rubber component. Effect of the Invention

[0010] According to the present disclosure, it is possible to provide an aluminum electrolytic capacitor that can be applied to a liquid immersion cooling system that uses a hydrocarbon-based refrigerant as the coolant. [Brief description of the drawings]

[0011] [Figure 1]1 is a schematic cross-sectional view of an aluminum electrolytic capacitor for liquid immersion cooling according to an embodiment of the present disclosure. FIG. [Diagram 2] 1 is a schematic cross-sectional view of an aluminum electrolytic capacitor for liquid immersion cooling according to an embodiment of the present disclosure. FIG. [Diagram 3] 1 is a schematic cross-sectional view of an aluminum electrolytic capacitor for liquid immersion cooling according to an embodiment of the present disclosure. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The following is a detailed description of the embodiments of the present disclosure. The following description of the components is an example (representative example) of the embodiments of the present disclosure, and the present disclosure is not limited to these contents as long as it does not exceed the gist of the disclosure.

[0013] 1. Aluminum electrolytic capacitors for liquid immersion cooling The first embodiment of the present disclosure is an aluminum electrolytic capacitor for liquid immersion cooling (hereinafter, may be simply referred to as "aluminum electrolytic capacitor") that is subjected to cooling in a cooling liquid. The sealing body of the aluminum electrolytic capacitor has a rubber member in an area that contacts the cooling liquid during liquid immersion cooling, and the rubber member is made of a rubber composition or a vulcanizate thereof that contains a rubber component having a Hansen solubility parameter distance of 8.0 or more with respect to the cooling liquid. In addition, when the aluminum electrolytic capacitor according to this embodiment is immersion cooled, a hydrocarbon-based refrigerant is used as the cooling liquid. Alternatively, a silicone oil-based refrigerant may be used as the cooling liquid instead of or together with the hydrocarbon-based refrigerant. In addition, in this disclosure, the "rubber member" refers to a rubber member made of the above rubber composition or a vulcanizate thereof, unless otherwise specified.

[0014] 1-1. Coolant The aluminum electrolytic capacitor according to the present embodiment is suitable as a capacitor to be mounted in an electronic device that is subjected to liquid immersion cooling using the above-mentioned coolant. By providing an aluminum electrolytic capacitor that is applicable to liquid immersion cooling using the above-mentioned coolant, the degree of freedom in the selection of the coolant is increased, and it becomes possible to replace the expensive fluorine-based insulating refrigerants that have been used up to now with inexpensive coolants such as hydrocarbon-based refrigerants.

[0015] Examples of the hydrocarbon refrigerant include petroleum hydrocarbons such as paraffinic mineral oil and naphthenic mineral oil, synthetic oils such as poly-α-olefins (PAOs) and artificial petroleum obtained by Fischer-Tropsch synthesis, and bio-oil. Among these, the hydrocarbon refrigerant is preferably one or more selected from synthetic oils, more preferably one or more selected from artificial petroleum, and even more preferably poly-α-olefins (PAOs) or artificial petroleum obtained by Fischer-Tropsch synthesis. In the present disclosure, "poly-α-olefins (PAOs)" refers to α-olefin polymers in which the terminal double bonds have been hydrogenated.

[0016] The petroleum-based hydrocarbons and synthetic petroleum are preferably a mixture of hydrocarbons having a carbon number of 15 to 50, and more preferably a mixture of hydrocarbons having a carbon number of 18 to 50. Each of the hydrocarbons may be any of linear, branched, and cyclic hydrocarbons, but is preferably a linear or branched hydrocarbon.

[0017] The poly-α-olefin is preferably a homopolymer or copolymer of an α-olefin having from 2 to 32 carbon atoms, more preferably a homopolymer or copolymer of an α-olefin having from 6 to 16 carbon atoms, even more preferably a homopolymer or copolymer of one or more α-olefins selected from the group consisting of α-octene, 1-decene, 1-dodecene, and 1-tetradecene, and particularly preferably a homopolymer of 1-decene.

[0018] The degree of polymerization of the poly-α-olefin is preferably 2 or more, more preferably 3 or more, and preferably 10 or less, more preferably 8 or less, and further preferably 5 or less. That is, preferred ranges of the degree of polymerization of the poly-α-olefin include, for example, ranges of 2 or more and 10 or less, 2 or more and 8 or less, and 3 or more and 5 or less.

[0019] The number of carbon atoms in the poly-α-olefin is preferably 10 or more, more preferably 20 or more, and even more preferably 30 or more, and is preferably 80 or less, more preferably 70 or less, and even more preferably 60 or less. That is, preferred ranges for the number of carbon atoms in the poly-α-olefin include, for example, ranges of 10 or more and 80 or less, 20 or more and 70 or less, and 30 or more and 60 or less.

[0020] The hydrocarbon refrigerant is preferably a fluorine-free hydrocarbon, and more preferably a petroleum-based hydrocarbon. In the present disclosure, the "fluorine-free hydrocarbon" may be a hydrocarbon that does not contain fluorine at all, or a hydrocarbon that unavoidably contains fluorine as an impurity.

[0021] Silicone oils include polysiloxanes such as polydimethylsiloxane and polymethylphenylsiloxane.

[0022] The coolant may be used alone or in any combination of two or more in any ratio.

[0023] The coolant is preferably insulating. In order not to impede wireless communication in the gigahertz band, the relative dielectric constant of the coolant is preferably 3.0 or less, and more preferably 2.5 or less.

[0024] 1-2.Aluminum electrolytic capacitors The aluminum electrolytic capacitor for immersion cooling according to this embodiment is not particularly limited in its structure, shape, constituent materials, and other configurations, as long as it has a sealing body described below, and can be the same as or similar to known aluminum electrolytic capacitors.

[0025] For example, the aluminum electrolytic capacitor may be any of a chip type, a lead type, a substrate-supporting type, and a screw terminal type. In addition, the capacitor element in an aluminum electrolytic capacitor is made up of anode foil and cathode foil that hold an electrolyte. The electrolytic solution may be wound with a separator interposed therebetween, the electrolytic solution may be replaced with a conductive polymer (i.e., a solid electrolytic capacitor element), or the electrolytic solution may be replaced with a hybrid electrolyte of an electrolytic solution and a conductive polymer. The electrolytic solution is not particularly limited, and examples thereof include glycol-based electrolytic solutions whose main solvent is glycol such as ethylene glycol and diethylene glycol; sulfolane-based electrolytic solutions; lactone-based electrolytic solutions; and aqueous electrolytic solutions.

[0026] An example of an aluminum electrolytic capacitor suitable for this embodiment is an aluminum electrolytic capacitor 10 as shown in Fig. 1, which includes a capacitor element 2, a metal case 4 that houses the capacitor element 2, and a sealing body 6 that seals the opening of the metal case 4, and the metal case 4 has a horizontal crimped portion 4a and a vertical crimped portion 4b. Such an aluminum electrolytic capacitor is manufactured by sequentially inserting the capacitor element and the sealing body into a cylindrical metal case with an opening and a bottom, and then crimping the side of the metal case (drawing process) and crimping the opening end of the metal case vertically (curling process). Such an aluminum electrolytic capacitor and its manufacturing method are disclosed, for example, in JP-A-2004-119907 and JP-A-2002-25870.

[0027] However, in manufacturing the aluminum electrolytic capacitor for liquid immersion cooling according to this embodiment, when inserting the sealing body into the metal case, the sealing body is positioned so that the rubber member of the sealing body is located in the area that will come into contact with the cooling liquid during liquid immersion cooling. In other words, the method for manufacturing the aluminum electrolytic capacitor for liquid immersion cooling according to this embodiment includes a sealing step of sealing the capacitor element with the sealing body, and in this sealing step, the sealing body is positioned so that the rubber member is located in the area that will come into contact with the cooling liquid during liquid immersion cooling. Then, the metal case is crimped as described above.

[0028] The method for producing the aluminum electrolytic capacitor for liquid immersion cooling according to the present embodiment may include a step of preparing a rubber member. The step of preparing a rubber member may be a step of molding a rubber composition described in detail below, or a step of molding a rubber composition described in detail below and then vulcanizing the rubber composition.

[0029] 1-3. Sealing body The sealing body of the aluminum electrolytic capacitor in this embodiment has a rubber member in a region that comes into contact with the cooling liquid during immersion cooling. The rubber member is made of a rubber composition or a vulcanizate thereof that contains a rubber component having a Hansen solubility parameter distance with the cooling liquid of 8.0 or more.

[0030] Conventionally, when aluminum electrolytic capacitors are subjected to immersion cooling, one of the reasons why it has been considered that the above-mentioned coolants cannot be used is that rubbers such as ethylene propylene rubber (EPDM) and butyl rubber are used as the material of the sealing body of the aluminum electrolytic capacitor. Since these rubbers are highly compatible with organic refrigerants, when the sealing body is immersed in the cooling liquid, the rubber forming the sealing body absorbs the cooling liquid and swells. When the rubber swells, the volume of the rubber expands and the metal case in which the capacitor element is housed may be deformed, or the cooling liquid may penetrate into the metal case, causing adverse effects on the capacitor element, conductive polymer, electrolyte, etc. housed in the metal case. That is, when conventional aluminum electrolytic capacitors are immersed in liquid cooling, depending on the type of cooling liquid, the metal case may be deformed, or airtightness may not be guaranteed, causing performance degradation and shortening of the lifespan.

[0031] Therefore, the inventors considered that in order to make it possible to apply an aluminum electrolytic capacitor to immersion cooling using a coolant such as a hydrocarbon, it would be necessary to make the sealant less susceptible to swelling due to the coolant. As a result, they focused on the Hansen solubility parameter (HSP) as an index for selecting the material for the sealant, and found that swelling of the sealant can be sufficiently suppressed by using a rubber composition or vulcanizate thereof that contains a rubber component with an HSP distance from the coolant of 8.0 or more as the rubber member disposed in the region of the sealant that comes into contact with the coolant.

[0032] HSP is a value that quantifies the solubility of one substance A in another substance B using a multidimensional vector. It is estimated that the shorter the HSP distance between two substances, the higher the solubility of substance A in substance B and the higher its compatibility with substance B.

[0033] HSP is calculated from the chemical structure using HSP analysis software such as HSPiP (Hansen Solubility Parameters in Practice, Ver.5.4.05). HSP is expressed by three components: δD (dispersion term), δP (polarization term), and δH (hydrogen bond term). The units of δD, δP, δH, and Ra are MPa. 1 / 2 The HSP distance between two compounds is the distance between two points when the values ​​of δD, δP, and δH are plotted on a three-dimensional orthogonal coordinate system, and can be calculated according to the following formula. In this disclosure, HSP is a value at 25°C. In this embodiment, the rubber component corresponds to substance B, and the coolant corresponds to substance A.

[0034] HSP distance (Ra)={4×(δD1-δD2) 2 +(δP1-δP2) 2 +(δH1-δH2) 2} 1 / 2 In the formula, δD1, δP1, and δH1 are δD, δP, and δH of substance A, respectively. In the formula, δD2, δP2, and δH2 are δD, δP, and δH of substance B, respectively.

[0035] In this embodiment, the HSP distance between the rubber component and the coolant is 8.0 or more, and is preferably 10.0 or more, more preferably 12.0 or more, even more preferably 15.0 or more, and particularly preferably 20.0 or more, in order to further suppress swelling of the sealing body. The upper limit of the HSP distance between the rubber component and the coolant is not particularly limited, but is preferably 50.0 or less or 40.0 or less. In other words, preferred ranges of the HSP distance between the rubber component and the coolant include, for example, 8.0 or more and 50.0 or less, 10.0 or more and 40.0 or less, 12.0 or more and 40.0 or less, 15.0 or more and 40.0 or less, and 20.0 or more and 40.0 or less.

[0036] If the HSP distance between the rubber component and the coolant is within the above range, swelling of the rubber member due to the coolant during immersion cooling can be suppressed, and problems such as deterioration of the performance and shortening of the life of the aluminum electrolytic capacitor, as well as deformation of the metal case can be avoided.

[0037] Note that "HSP distance between the rubber component and the coolant" means the HSP distance between the mixture and the coolant when the rubber component is a mixture of two or more types of rubber, means the HSP distance between the mixture and the rubber component when the coolant is a mixture of two or more types of refrigerants, and means the HSP distance between the mixture and the rubber component when the rubber component is the mixture and the coolant is the mixture. Therefore, as long as the HSP distance between the rubber component as a whole and the coolant is not less than the lower limit, the rubber component may contain rubber whose HSP distance between the coolant and the coolant is less than the lower limit.

[0038] The rubber component may be appropriately selected so that the HSP distance with the coolant falls within the above range, and the type is not particularly limited. However, rubber containing heteroatoms such as nitrogen atoms, oxygen atoms, chlorine atoms, sulfur atoms, and fluorine atoms in the main chain or side chain is preferred because it has a large HSP distance with the hydrocarbon refrigerant.

[0039] More specifically, in terms of a large HSP distance with the coolant, the rubber component preferably contains one or more types selected from the group consisting of nitrile rubber, hydrogenated nitrile rubber, acrylic rubber, fluororubber, chloroprene rubber, chlorosulfonated polyethylene rubber, urethane rubber, polysulfide rubber, and epichlorohydrin rubber, more preferably contains one or more types selected from the group consisting of nitrile rubber, hydrogenated nitrile rubber, acrylic rubber, and fluororubber, and even more preferably contains one or more types selected from the group consisting of nitrile rubber and acrylic rubber, or one or more types selected from the group consisting of nitrile rubber and fluororubber.

[0040] Nitrile rubber is a copolymer of acrylonitrile and butadiene and generally contains 15% to 60% by weight of acrylonitrile units. Nitrile rubber may also be copolymerized with other monomers such as ethylene, conjugated dienes, and vinyl compounds.

[0041] Hydrogenated nitrile rubber is a rubber obtained by hydrogenating nitrile rubber. The hydrogenation rate of the hydrogenated nitrile is not particularly limited, but is generally in the range of 70% to 100%.

[0042] Acrylic rubber is a rubber whose main component is an acrylic acid ester. "Mainly made of an acrylic acid ester" means that the content of acrylic acid ester units in the acrylic rubber is 50% by weight or more. In the present disclosure, "acrylic acid ester" may be "methacrylic acid ester". The acrylic rubber may be a copolymer of ethylene, vinyl acetate, and other monomers such as crosslinkable monomers. Examples of crosslinkable monomers include monomers having an epoxy group, a carboxyl group, a hydroxyl group, and the like, and diene monomers.

[0043] The fluororubber is a homopolymer or copolymer containing fluorine atoms in the main chain or side chain, and is obtained by polymerizing fluorine-containing monomers such as tetrafluoroethylene, hexafluoropropylene, vinylidene fluoride, etc. The fluororubber may also be a copolymer of fluorine-free monomers such as ethylene and propylene.

[0044] Chloroprene rubber is a diene-based rubber obtained by polymerizing chloroprene.

[0045] Chlorosulfonated polyethylene rubber is a rubber in which chlorine atoms and chlorosulfonyl groups (-SO2Cl) are bonded to the polyethylene main chain.

[0046] The urethane rubber is not particularly limited as long as it has a urethane bond in its molecular structure, but is preferably an ester-based urethane rubber.

[0047] Polysulfide rubber is a liquid polymer that has disulfide bonds (-SS-) in the main chain, a slightly branched structure, and a thiol group at the end. Polysulfide rubber can be cured with metal oxides, organic peroxides, etc.

[0048] Epichlorohydrin rubber is a general term for epichlorohydrin homopolymer (CO), copolymer of epichlorohydrin and ethylene oxide (ECO), copolymer of epichlorohydrin and allyl glycidyl ether (GCO), and copolymer of epichlorohydrin, ethylene oxide and allyl glycidyl ether (GECO).

[0049] The rubber component may be a single type of rubber, or may be a mixture of two or more types of rubber in any combination and ratio. When the rubber component is made of a single type of rubber, the single type of rubber is a rubber whose HSP distance with the coolant is equal to or greater than the above lower limit. When the rubber component is a mixture of two or more types of rubber, the mixture may contain two or more types of rubber whose HSP distance with the coolant is equal to or greater than the above lower limit, but may also contain any amount of rubber whose HSP distance with the coolant is less than the above lower limit, as long as the HSP distance between the mixture and the coolant is equal to or greater than the above lower limit. Examples of rubber whose HSP distance with the coolant is less than the above lower limit include butyl rubber and ethylene propylene rubber (EPDM).

[0050] The rubber component is preferably a mixture of a rubber having an HSP distance to the coolant that is equal to or greater than the above lower limit and a rubber having an HSP distance to the coolant that is less than the above lower limit. Rubbers with an HSP distance to the coolant that is less than the above-mentioned lower limit, such as EPDM rubber, tend to be less permeable to the electrolyte. Therefore, in an aluminum electrolytic capacitor containing an electrolyte, by combining a rubber whose HSP distance to the coolant is equal to or greater than the above-mentioned lower limit with a rubber whose HSP distance to the coolant is less than the above-mentioned lower limit, it is possible to both suppress the swelling of the sealing body and suppress the evaporation of the electrolyte through the sealing body, thereby making it possible to extend the life of the aluminum electrolytic capacitor.

[0051] The rubber component containing the rubber having an HSP distance with the coolant less than the lower limit and having an HSP distance with the coolant of equal to or greater than the lower limit is a mixture of rubber A having an HSP distance with the coolant of equal to or greater than the lower limit and rubber B having an HSP distance with the coolant less than the lower limit, and the content of rubber A relative to the total amount of the mixture (i.e., the total amount of the rubber components) is preferably 35% by weight or more, more preferably 40% by weight or more, even more preferably 50% by weight or more, and particularly preferably 60% by weight or more. In other words, the content of rubber B relative to the total amount of the mixture is preferably 65% ​​by weight or less, more preferably 60% by weight or less, even more preferably 50% by weight or less, and particularly preferably 40% by weight or less. The contents of rubber A and rubber B relative to the total amount of the mixture are usually more than 0% by weight and usually less than 100% by weight, respectively.

[0052] More specifically, a rubber component containing a rubber having an HSP distance with respect to the coolant that is less than the lower limit and having an HSP distance with respect to the coolant that is equal to or greater than the lower limit can be, for example, a mixture of nitrile rubber and butyl rubber, in which the content of nitrile rubber relative to the total amount of the mixture (i.e., the total amount of rubber components) is preferably 35% by weight or more, more preferably 40% by weight or more, even more preferably 50% by weight or more, and particularly preferably 60% by weight or more, as shown in the examples described below. At this time, the content of butyl rubber relative to the total amount of the mixture is preferably 65% ​​by weight or less, more preferably 60% by weight or less, even more preferably 50% by weight or less, and particularly preferably 40% by weight or less. The contents of nitrile rubber and butyl rubber relative to the total amount of the mixture are usually more than 0% by weight, and usually less than 100% by weight, respectively.

[0053] Alternatively, as an example of a rubber component containing a rubber whose HSP distance with the coolant is less than the lower limit and whose HSP distance with the coolant is equal to or greater than the lower limit, as shown in the examples described later, a mixture of nitrile rubber and ethylene propylene rubber (EPDM) in which the content of nitrile rubber relative to the total amount of the mixture (i.e., the total amount of rubber components) is preferably 35% by weight or more, more preferably 40% by weight or more, even more preferably 50% by weight or more, and particularly preferably 60% by weight or more can be mentioned. In this case, the content of ethylene propylene rubber (EPDM) relative to the total amount of the mixture is preferably 65% ​​by weight or less, more preferably 60% by weight or less, even more preferably 50% by weight or less, and particularly preferably 40% by weight or less. The contents of nitrile rubber and ethylene propylene rubber (EPDM) relative to the total amount of the mixture are usually more than 0% by weight and usually less than 100% by weight, respectively.

[0054] The rubber composition for forming the rubber member may contain other components as necessary in addition to the above-mentioned rubber components. Examples of other components include, but are not limited to, vulcanizing agents, fillers, and processing aids.

[0055] Examples of vulcanizing agents include sulfur; sulfur donors such as 4,4'-dithiodimorpholine and tetramethylthiuram disulfide; organic peroxides such as dicumyl peroxide and benzoyl peroxide; metal oxides such as zinc oxide; polyfunctional amine compounds such as hexamethylene diamine carbamate and 4,4'-diaminodiphenyl ether; and alkylphenol polymers such as alkylphenol-formaldehyde resins and halogenated alkylphenol-formaldehyde resins.

[0056] When the rubber composition contains a vulcanizing agent, the content of the vulcanizing agent in the rubber composition is not particularly limited, but is preferably 0.1 part by weight or more, more preferably 0.1 part by weight or more, based on 100 parts by weight of the rubber component. It is 0.5 parts by weight or more, more preferably 1 part by weight or more, and preferably 25 parts by weight or less, more preferably 20 parts by weight or less, and even more preferably 15 parts by weight or less. That is, when the rubber composition contains a vulcanizing agent, preferred ranges of the content of the vulcanizing agent per 100 parts by weight of the rubber component include, for example, 0.1 parts by weight or more and 25 parts by weight or less, 0.5 parts by weight or more and 20 parts by weight or less, and 1 part by weight or more and 15 parts by weight or less.

[0057] Preferred examples of the filler include inorganic fillers such as carbon black, clay, talc, calcium carbonate, and silica. The silica may be surface-treated with a silane coupling agent. Of these, the rubber composition preferably contains carbon black, which can increase the strength of the rubber member.

[0058] When the rubber composition contains a filler, the content of the filler in the rubber composition is not particularly limited, but is preferably 10 parts by weight or more, more preferably 20 parts by weight or more, and even more preferably 30 parts by weight or more, and is preferably 250 parts by weight or less, more preferably 200 parts by weight or less, and even more preferably 150 parts by weight or less, relative to 100 parts by weight of the rubber component. That is, when the rubber composition contains a filler, preferred ranges of the content of the filler relative to 100 parts by weight of the rubber component include, for example, 10 parts by weight or more and 250 parts by weight or less, 20 parts by weight or more and 200 parts by weight or less, and 30 parts by weight or more and 150 parts by weight or less.

[0059] As the processing aid, a known rubber processing aid can be used. Known rubber processing aids include fatty acids having 12 to 30 carbon atoms, such as ricinoleic acid, stearic acid, palmitic acid, and lauric acid; salts of fatty acids having 12 to 30 carbon atoms, such as barium stearate, calcium stearate, and zinc stearate; and esters of fatty acids having 12 to 30 carbon atoms, such as ricinoleic acid esters, stearic acid esters, palmitic acid esters, and lauric acid esters. Among these, the rubber composition preferably contains stearic acid, in that it can improve the dispersibility of each component in the composition and the flowability of the rubber component to improve molding processability.

[0060] When the rubber composition contains a processing aid, the content of the processing aid in the rubber composition is not particularly limited, but is preferably 0.1 parts by weight or more, more preferably 0.3 parts by weight or more, and even more preferably 0.5 parts by weight or more, and is preferably 20 parts by weight or less, more preferably 10 parts by weight or less, and even more preferably 5 parts by weight or less, relative to 100 parts by weight of the rubber component. That is, when the rubber composition contains a processing aid, preferred ranges of the content of the processing aid relative to 100 parts by weight of the rubber component include, for example, 0.1 parts by weight or more and 20 parts by weight or less, 0.3 parts by weight or more and 10 parts by weight or less, and 0.5 parts by weight or more and 5 parts by weight or less.

[0061] A rubber member is disposed in at least a part of the sealing body. This rubber member is a part that is responsible for the airtightness of the exterior body such as a metal case and the lead terminals, and is disposed in a region that is exposed to the outside of the aluminum electrolytic capacitor and that comes into contact with the cooling liquid during immersion cooling. If the rubber member disposed in the region that comes into contact with the cooling liquid during immersion cooling is formed from the above rubber composition or its vulcanizate, the adverse effects of the cooling liquid can be reduced, so that the constituent materials of the other parts are not particularly limited. In addition, the specific form of the rubber member is not particularly limited as long as it is disposed in the region of the sealing body that comes into contact with the cooling liquid during immersion cooling, and may be the sealing body itself, or may be a layer or a partial structure that constitutes the sealing body. Below, preferred forms of the sealing body will be described with several examples, but the sealing body in this embodiment is not limited to the following examples.

[0062] Fig. 1 shows a schematic cross-sectional view of an aluminum electrolytic capacitor 10 according to this embodiment. In Fig. 1, a sealing body 6 is disposed between a vertical crimped portion 4b of a metal case 4 and a capacitor element 2. In this aluminum electrolytic capacitor 10, The vertical crimping portion 4b of the housing 4 ensures airtightness of the aluminum electrolytic capacitor 10.

[0063] 1, not only is the entire area of ​​sealing body 6 that comes into contact with the cooling liquid during immersion cooling formed of rubber member 6a, but the entire sealing body is also formed of rubber member 6a. This prevents sealing body 6 from swelling, thereby preventing deformation of metal case 4 and ensuring the airtightness of aluminum electrolytic capacitor 10.

[0064] 2 is a schematic cross-sectional view of another aluminum electrolytic capacitor 10 according to the present embodiment. In FIG. 2, sealing body 6 is disposed in the same position as in FIG.

[0065] In FIG. 2, the sealing body 6 is formed by coating or laminating a layer made of the above-mentioned rubber composition or its vulcanizate on the surface of the sealing body main body 6b opposite to the surface facing the capacitor element 2. This layer made of the rubber composition or its vulcanizate corresponds to the rubber member 6a. The sealing body main body 6b is formed of a rubber other than the above-mentioned rubber component or its vulcanizate, and the sealing body main body 6b is covered with the rubber member 6a, so that contact with the cooling liquid during liquid immersion cooling can be avoided. This suppresses swelling of the sealing body 6, and ensures the airtightness of the aluminum electrolytic capacitor 10. For this reason, the sealing body main body 6b may be formed of ethylene propylene rubber (EPDM) and butyl rubber or its vulcanizate. In addition, when the aluminum electrolytic capacitor 10 contains an electrolytic solution, it is also preferable that the sealing body main body 6b is formed of a rubber or its vulcanizate that is highly resistant to the electrolytic solution.

[0066] 2, the layer (rubber member 6a) made of the rubber composition or its vulcanizate is formed over the entire surface of sealing body main body 6b opposite the surface facing capacitor element 2, but it is not necessary to cover this entire surface as long as sealing body main body 6b is prevented from coming into contact with the cooling liquid during immersion cooling. In other words, as long as the layer made of the rubber composition or its vulcanizate is formed on at least the area surrounded by metal case edge portion 4c of the surface of sealing body main body 6b opposite the surface facing capacitor element 2, swelling of sealing body 6 can be suppressed, and as a result, deformation of metal case 4 and deterioration of airtightness of aluminum electrolytic capacitor 10 can be suppressed.

[0067] 3 is a schematic cross-sectional view of another aluminum electrolytic capacitor 10 according to the present embodiment. In FIG. 3, sealing body 6 is disposed between vertical crimped portion 4b and horizontal crimped portion 4a of metal case 4.

[0068] In Fig. 3, the sealing body 6 is a rubber-clad laminate having a rubber member 6a and a substrate 6c. The sealing body 6 may be the same as a known rubber-clad sealing laminate, except that the rubber layer is the rubber member 6a. Therefore, the substrate 6c may be a resin-based substrate such as a hard resin plate or a bakelite plate. When the aluminum electrolytic capacitor 10 contains an electrolyte, the substrate 6c is preferably formed of a material that is highly resistant to the electrolyte.

[0069] 3, substrate 6c does not come into contact with the cooling liquid during immersion cooling, which prevents sealing body 6 from swelling, thereby preventing metal case 4 from deforming, and ensuring the airtightness of aluminum electrolytic capacitor 10.

[0070] In addition, the sealing body may be a sealing body main body made of a material that does not easily swell with the coolant, such as metal or resin, and a rubber member is formed on the portion of the sealing body that receives pressure from the edge of the metal case. Alternatively, the sealing body may be a sealing body main body made of a material that does not easily swell with the coolant, and a rubber member is disposed on the boundary between the sealing body and the lead wire. In such an embodiment, the rubber member does not easily swell with the coolant, so deformation of the metal case 4 and a decrease in the airtightness of the aluminum electrolytic capacitor 10 can be suppressed.

[0071] The above-mentioned sealing body structures can be appropriately combined as long as the effects of the present disclosure are not impaired. For example, the position of the sealing body 6 in FIG. 1 or 2 can be the position of the sealing body 6 shown in FIG.

[0072] 1 to 3, the seal 6 shown in Fig. 1 is more preferable because it can be manufactured from a single rubber composition, which increases manufacturing efficiency and reduces manufacturing costs. Also, the seal 6 shown in Fig. 1 and Fig. 2 is more preferable because it allows the use of a rubber seal as the seal for the aluminum electrolytic capacitor.

[0073] Furthermore, the sealing body of the aluminum electrolytic capacitor may be a sealing body with a protective material attached to the surface facing the capacitor element. The protective material is a member for protecting the sealing body from the electrolyte. The shape of the protective material is not particularly limited as long as it can prevent contact between the sealing body and the electrolyte, and can be, for example, a membrane-like, foil-like, film-like, sheet-like, or plate-like member. The material for forming the protective material is not particularly limited as long as it is a material with high resistance to the electrolyte, and for example, a known insulating material such as a phenol resin can be used.

[0074] 1-4.Evaluation Whether an aluminum electrolytic capacitor can be applied to immersion cooling using the above-mentioned coolant can be evaluated by observing the change in hardness of a test piece formed of the same material as the above-mentioned rubber member by immersing the test piece in the coolant. This is because there is a correlation between the degree of swelling of the rubber member and the change in hardness. More specifically, based on the fact that the hardness of the rubber member decreases as the rubber member swells and causes volume expansion and structural changes (e.g., crosslink scission), it can be determined that the smaller the change in hardness of the rubber member, the more defects caused by the expansion of the rubber member are suppressed.

[0075] The change in hardness of the rubber part before and after immersion in the coolant is evaluated by calculating the hardness change rate of a dumbbell-shaped test piece (type 3) made of the same material as the rubber part. The hardness change rate of the dumbbell-shaped test piece is calculated by the following steps (1) to (4). (1) The hardness of three dumbbell-shaped test pieces is measured, and the median of the measured values ​​is determined as the hardness before immersion. (2) Immerse the three dumbbell-shaped test pieces from (1) in the cooling liquid and heat them at 85°C for 168 hours. (3) Measure the hardness of the three dumbbell-shaped test pieces removed from the cooling liquid, and determine the median of the measured values ​​as the hardness after immersion. (4) The hardness change rate is calculated by applying the hardness before immersion and the hardness after immersion to the following formula (I).

[0076]

number

[0077] The hardness of the dumbbell-shaped test piece is measured using a type A durometer in accordance with JIS K 6253-3:2012 "Vulcanized rubber and thermoplastic rubber - Determination of hardness - Part 3: Durometer hardness" (established on March 21, 2012).

[0078] It is evaluated that the greater the rate of change in hardness obtained as described above is in the negative direction, the greater the decrease in hardness of the rubber member due to immersion in the coolant.

[0079] The hardness change rate is preferably -20% or more, more preferably -15% or more, even more preferably -10% or more, and particularly preferably -5% or more. The upper limit of the hardness change rate is preferably 10% or less, more preferably 5% or less. That is, preferred ranges of the hardness change rate include, for example, -20% or more and 10% or less, -15% or more and 10% or less, -10% or more and 5% or less, and -5% or more and 5% or less.

[0080] If the hardness change rate is within the above range, the rubber member is unlikely to swell due to the coolant, and is therefore highly suitable for immersion cooling of aluminum electrolytic capacitors.

[0081] 2. Cooling methods for aluminum electrolytic capacitors A second embodiment of the present disclosure is a cooling method for an aluminum electrolytic capacitor according to the first embodiment of the present disclosure, which includes an immersion cooling step of immersing the aluminum electrolytic capacitor in a cooling liquid to cool it. The cooling liquid is a hydrocarbon-based refrigerant, and is the same as the cooling liquid described in the description of the first embodiment of the present disclosure.

[0082] In the present embodiment, the aluminum electrolytic capacitor may be mounted on an electronic device. When the aluminum electrolytic capacitor is mounted on an electronic device, the liquid immersion cooling process is performed by immersing the aluminum electrolytic capacitor together with the electronic device in the cooling liquid. In this case, the liquid immersion cooling process may be performed by immersing at least a part of the electronic device to which the aluminum electrolytic capacitor is attached in the cooling liquid to cool the aluminum electrolytic capacitor. Therefore, the liquid immersion cooling process may be a process of immersing the entire electronic device in the cooling liquid to cool it, or a process of immersing a part to which the aluminum electrolytic capacitor is attached in the cooling liquid to cool it. An example of a part to which the aluminum electrolytic capacitor is attached is a substrate such as a printed circuit board. When the aluminum electrolytic capacitor is mounted on an electronic device, the liquid immersion cooling process can cool not only the aluminum electrolytic capacitor but also the entire electronic device or the entire part to which the aluminum electrolytic capacitor is attached.

[0083] The electronic device to be cooled by the immersion cooling process is not particularly limited as long as it has the aluminum electrolytic capacitor according to the first embodiment of the present disclosure, and examples thereof include supercomputers, servers, and communication devices having a printed circuit board with an aluminum electrolytic capacitor attached thereto.

[0084] In the immersion cooling process, the aluminum electrolytic capacitor or electronic device is immersed in a cooling liquid, and the heat generated by these operations is transferred to the cooling liquid, thereby cooling (dissipating heat). The specific method for performing the immersion cooling process is not particularly limited as long as the above-mentioned cooling liquid is used, and the process can be performed by a known immersion cooling system. Known immersion cooling systems include a single-phase immersion cooling system that uses the cooling liquid in a liquid state, and a two-phase immersion cooling system that uses the phase change of the cooling liquid.

[0085] The cooling method according to the present embodiment can prevent the aluminum electrolytic capacitor from losing its airtightness due to swelling of the sealing body during immersion cooling, and can prevent the metal case from deforming. This makes it possible to immerse the aluminum electrolytic capacitor and an electronic device equipped with the aluminum electrolytic capacitor by using a hydrocarbon-based refrigerant as the coolant.

[0086] 3. Cooling methods for electronic devices A third embodiment of the present disclosure is a method for cooling an electronic device having an aluminum electrolytic capacitor according to the first embodiment of the present disclosure, and includes a liquid immersion cooling step of immersing a part or the whole of the electronic device in a cooling liquid to cool it. The cooling liquid is a hydrocarbon-based refrigerant, and is the same as the cooling liquid described in the description of the first embodiment of the present disclosure. The electronic device is also a method for cooling an electronic device having an aluminum electrolytic capacitor according to the first embodiment of the present disclosure. This has the same meaning as the electronic device described in the second embodiment.

[0087] In the liquid immersion cooling process, the electronic device is immersed in the cooling liquid so that at least the aluminum electrolytic capacitor is immersed in the cooling liquid. In other words, the liquid immersion cooling process may be a process of immersing the entire electronic device in the cooling liquid to cool it, or a process of immersing a part to which an aluminum electrolytic capacitor is attached in the cooling liquid to cool it. An example of a part to which an aluminum electrolytic capacitor is attached is a substrate such as a printed circuit board. The liquid immersion cooling process can cool the entire electronic device or the entire part to which an aluminum electrolytic capacitor is attached.

[0088] In the immersion cooling process, an electronic device is immersed in a cooling liquid, and heat generated during operation is transferred to the cooling liquid, thereby cooling (dissipating heat). The specific method for performing the immersion cooling process is not particularly limited as long as the above-mentioned cooling liquid is used, and the process can be performed by a known immersion cooling system. Known immersion cooling systems include a single-phase immersion cooling system that uses the cooling liquid in a liquid state, and a two-phase immersion cooling system that uses a phase change of the cooling liquid.

[0089] The cooling method according to the present embodiment can prevent the aluminum electrolytic capacitor from losing its airtightness due to swelling of the sealing body during immersion cooling, and can prevent the metal case from deforming. This makes it possible to immerse an electronic device equipped with an aluminum electrolytic capacitor in the immersion cooling by using a hydrocarbon-based refrigerant as the coolant. EXAMPLES

[0090] The present disclosure will be described in more detail below with reference to examples. However, the present disclosure is not limited to the description of the following examples as long as it does not depart from the gist of the disclosure. In this disclosure, "room temperature" means a temperature in the range of 15°C or higher and 35°C or lower.

[0091] Example 1 100 parts by weight of acrylonitrile butadiene rubber, 50 parts by weight of carbon black, 1 part by weight of stearic acid, and 5 parts by weight of dicumyl peroxide were kneaded, and the resulting composition was vulcanized at 170°C for 10 minutes to obtain a sheet with a thickness of 2 mm. This sheet was punched out into a dumbbell shape to prepare a dumbbell-shaped test piece (size 3).

[0092] The HSP of acrylonitrile butadiene rubber and Fischer-Tropsch distillate heavy oil (a mixture of branched and linear hydrocarbons with carbon numbers of 18 to 50) which is a hydrocarbon refrigerant was calculated using the HSP analysis software "HSPiP (Ver.5.4.05)". The HSP calculation values ​​of acrylonitrile butadiene rubber and hydrocarbon refrigerants, as well as the HSP distance between acrylonitrile butadiene rubber and hydrocarbon refrigerants obtained from these calculation values ​​are shown in Table 1.

[0093] In addition, the hardness change of the dumbbell-shaped test pieces caused by immersion in a hydrocarbon refrigerant was evaluated according to the method described below. The results are shown in Table 1.

[0094] [Evaluation of change in hardness due to immersion] (Immersion test) Three dumbbell-shaped test pieces were immersed in the test refrigerant contained in a test tube. The test tube was heated in an oven set at 85°C for 168 hours. The test tube was removed from the oven and left at room temperature for 30 minutes to cool. After cooling, the dumbbell-shaped test pieces were removed from the test refrigerant, and the test refrigerant adhering to the dumbbell-shaped test pieces was wiped off.

[0095] (Calculation of hardness change rate) Using a durometer (Telok Corporation's "GX-01A"; Type A), JIS K In accordance with 6253-3:2012 "Vulcanized and thermoplastic rubber - Determination of hardness - Part 3: Durometer hardness" (established on March 21, 2012), the hardness of the three dumbbell-shaped test pieces was measured before the immersion test, and the median value of each measurement was determined as the hardness of the dumbbell-shaped test pieces before the immersion test. The hardness of the dumbbell-shaped test pieces after the immersion test was calculated in the same manner. The hardness change rate of the dumbbell-shaped test pieces was calculated by applying these calculation results to the above formula (I). The results are shown in Table 1.

[0096] Example 2 A dumbbell-shaped test piece (Type 3) was prepared in the same manner as in Example 1, except that 100 parts by weight of acrylonitrile butadiene rubber was changed to 100 parts by weight of ethylene-vinyl acetate-acrylic acid ester copolymer, and 5 parts by weight of dicumyl peroxide was changed to 1 part by weight of hexamethylenediamine carbamate.

[0097] The calculation of HSP and HSP distance, and the evaluation of hardness change were performed in the same manner as in Example 1. The results are shown in Table 1.

[0098] Example 3 A dumbbell-shaped test piece (No. 3) was prepared in the same manner as in Example 1, except that 100 parts by weight of the acrylonitrile butadiene rubber was changed to 100 parts by weight of vinylidene fluoride-hexafluoropropylene copolymer.

[0099] The calculation of HSP and HSP distance, and the evaluation of hardness change were performed in the same manner as in Example 1. The results are shown in Table 1.

[0100] Example 4 A dumbbell-shaped test piece (Type 3) was prepared in the same manner as in Example 1, except that 100 parts by weight of acrylonitrile butadiene rubber was changed to 100 parts by weight of hydrogenated acrylonitrile butadiene rubber, and the amount of dicumyl peroxide was changed to 10 parts by weight.

[0101] The calculation of HSP and HSP distance, and the evaluation of hardness change were performed in the same manner as in Example 1. The results are shown in Table 1.

[0102] Comparative Example 1 A dumbbell-shaped test piece (No. 3) was prepared in the same manner as in Example 1, except that 100 parts by weight of acrylonitrile butadiene rubber was changed to 100 parts by weight of ethylene propylene rubber (EPDM).

[0103] The calculation of HSP and HSP distance, and the evaluation of hardness change were performed in the same manner as in Example 1. The results are shown in Table 1.

[0104] Comparative Example 2 Dumbbell-shaped test pieces (Type 3) were prepared in the same manner as in Example 1, except that 100 parts by weight of acrylonitrile butadiene rubber was changed to 100 parts by weight of butyl rubber, 5 parts by weight of dicumyl peroxide was changed to 10 parts by weight of alkylphenol formaldehyde resin, and the vulcanization conditions were changed to 170°C for 40 minutes.

[0105] In the same manner as in Example 1, the HSP and HSP distance were calculated, and the hardness change was evaluated. The results are shown in Table 1.

[0106] Example 5 20 parts by weight of butyl rubber, 80 parts by weight of nitrile rubber, 50 parts by weight of carbon black, 1 part by weight of stearic acid, and 12 parts by weight of alkylphenol-formaldehyde resin were kneaded, and the resulting composition was vulcanized at 170°C for 40 minutes to obtain a sheet with a thickness of 2 mm. This sheet was punched out into a dumbbell shape to prepare a dumbbell-shaped test piece (type 3).

[0107] The calculation of HSP and HSP distance, and the evaluation of hardness change were performed in the same manner as in Example 1. The results are shown in Table 1.

[0108] Example 6 A dumbbell-shaped test piece (Type 3) was prepared in the same manner as in Example 5, except that the rubber component consisting of a mixture of 20 parts by weight of butyl rubber and 80 parts by weight of nitrile rubber was changed to a rubber component consisting of a mixture of 40 parts by weight of butyl rubber and 60 parts by weight of nitrile rubber.

[0109] The calculation of HSP and HSP distance, and the evaluation of hardness change were performed in the same manner as in Example 1. The results are shown in Table 1.

[0110] Example 7 A dumbbell-shaped test piece (Type 3) was prepared in the same manner as in Example 5, except that the rubber component consisting of a mixture of 20 parts by weight of butyl rubber and 80 parts by weight of nitrile rubber was changed to a rubber component consisting of a mixture of 50 parts by weight of butyl rubber and 50 parts by weight of nitrile rubber.

[0111] The calculation of HSP and HSP distance, and the evaluation of hardness change were performed in the same manner as in Example 1. The results are shown in Table 1.

[0112] Example 8 A dumbbell-shaped test piece (Type 3) was prepared in the same manner as in Example 5, except that the rubber component consisting of a mixture of 20 parts by weight of butyl rubber and 80 parts by weight of nitrile rubber was changed to a rubber component consisting of a mixture of 60 parts by weight of butyl rubber and 40 parts by weight of nitrile rubber.

[0113] Example 9 A dumbbell-shaped test piece (Type 3) was prepared in the same manner as in Example 5, except that the rubber component consisting of a mixture of 20 parts by weight of butyl rubber and 80 parts by weight of nitrile rubber was changed to a rubber component consisting of a mixture of 65 parts by weight of butyl rubber and 35 parts by weight of nitrile rubber.

[0114] The calculation of HSP and HSP distance, and the evaluation of hardness change were performed in the same manner as in Example 1. The results are shown in Table 1.

[0115] Example 10 65 parts by weight of ethylene propylene rubber (EPDM), 35 parts by weight of nitrile rubber, 50 parts by weight of carbon black, 1 part by weight of stearic acid, and 5 parts by weight of dicumyl peroxide were kneaded, and the resulting composition was vulcanized at 170°C for 10 minutes to obtain a sheet with a thickness of 2 mm. This sheet was punched out into a dumbbell shape to prepare a dumbbell-shaped test piece (type 3).

[0116] The calculation of HSP and HSP distance, and the evaluation of hardness change were performed in the same manner as in Example 1. The results are shown in Table 1.

[0117] Example 11 65 parts by weight of ethylene propylene rubber (EPDM), 35 parts by weight of acrylic rubber, 50 parts by weight of carbon black, 1 part by weight of stearic acid, and 5 parts by weight of dicumyl peroxide were kneaded, and the resulting composition was vulcanized at 170°C for 10 minutes to obtain a sheet with a thickness of 2 mm. This sheet was punched out into a dumbbell shape to prepare a dumbbell-shaped test piece (type 3).

[0118] The calculation of HSP and HSP distance, and the evaluation of hardness change were performed in the same manner as in Example 1. The results are shown in Table 1.

[0119] [Examples 12 to 15] The dumbbell-shaped test pieces (Type 3) prepared in each of Examples 1 to 4 were subjected to immersion tests in the same manner as in Example 1, except that the test refrigerant and the hydrocarbon-based refrigerant, poly-α-olefin (poly(1-decene)), were used.

[0120] Moreover, the HSP and the HSP distance were calculated, and the hardness change was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0121] [Comparative Examples 3 and 4] The dumbbell-shaped test pieces (Type 3) prepared in each of Comparative Examples 1 and 2 were subjected to immersion tests in the same manner as in Example 1, except that a hydrocarbon-based refrigerant, poly-α-olefin (poly(1-decene)), was used as the test refrigerant.

[0122] Moreover, the HSP and the HSP distance were calculated, and the hardness change was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0123] [Table 1]

[0124] From Table 1, it was confirmed that when the HSP distance between the rubber component and the coolant was less than 8.0 (Comparative Examples 1 to 4), the hardness change rate of the dumbbell-shaped test piece was -24% or less. This shows that the rubber member formed of the vulcanizate of the rubber composition containing such a rubber component swells with the coolant and the hardness is significantly reduced. On the other hand, when the HSP distance between the rubber component and the coolant is 8.0 or more (Examples 1 to 15), it was confirmed that the change in hardness of the dumbbell-shaped test piece was small regardless of the type of rubber component and the type of coolant. This shows that a rubber member formed of a vulcanizate of a rubber composition containing a rubber component having an HSP distance between the rubber component and the coolant of 8.0 or more is less likely to swell in the coolant and can maintain its hardness even after immersion in the coolant.

[0125] From the above, even in an aluminum electrolytic capacitor having a rubber member in an area that comes into contact with the coolant during immersion cooling, if the material forming the rubber member is a rubber composition or a vulcanizate thereof that contains a rubber component having an HSP distance with the coolant of 8.0 or more, swelling of the rubber member is less likely to occur, and the aluminum electrolytic capacitor can be applied to a liquid immersion cooling system that uses a hydrocarbon refrigerant as the coolant. [Explanation of symbols]

[0126] 2. Capacitor elements 4 Metal case 4a Side crimping part 4b Vertical crimping part 4c Metal case edge 6 Sealing body 6a Rubber material 6b Sealing body 6c Board 10. Aluminum electrolytic capacitors

Claims

1. An aluminum electrolytic capacitor for liquid immersion cooling that is cooled in a cooling liquid, The cooling liquid is a hydrocarbon refrigerant, a sealing body of the aluminum electrolytic capacitor having a rubber member in a region that comes into contact with the cooling liquid during immersion cooling, The aluminum electrolytic capacitor for liquid immersion cooling, wherein the rubber member is made of a rubber composition or a vulcanizate thereof, the rubber composition containing a rubber component having a Hansen solubility parameter distance with the cooling liquid of 8.0 or more.

2. 2. The aluminum electrolytic capacitor for liquid immersion cooling according to claim 1, wherein the rubber component is at least one selected from the group consisting of nitrile rubber, hydrogenated nitrile rubber, acrylic rubber, and fluororubber.

3. 2. The aluminum electrolytic capacitor for liquid immersion cooling according to claim 1, wherein the rubber component contains more than 0% by weight and not more than 65% by weight of a rubber having a Hansen solubility parameter distance with the coolant of less than 8.0, based on a total amount of the rubber component.

4. The sealing body is used in the aluminum electrolytic capacitor for liquid immersion cooling according to any one of claims 1 to 3.

5. A method for cooling an aluminum electrolytic capacitor, comprising the steps of: a liquid immersion cooling step of immersing the aluminum electrolytic capacitor in a cooling liquid to cool it, The cooling liquid is a hydrocarbon refrigerant, a sealing body of the aluminum electrolytic capacitor having a rubber member in a region that comes into contact with the cooling liquid during immersion cooling, The method for cooling an aluminum electrolytic capacitor, wherein the rubber member is made of a rubber composition or a vulcanizate thereof, which contains a rubber component having a Hansen solubility parameter distance with the coolant of 8.0 or more.

6. The aluminum electrolytic capacitor is mounted on an electronic device, 6. The cooling method for an aluminum electrolytic capacitor according to claim 5, wherein the liquid immersion cooling step is performed by immersing a part or an entirety of the electronic device in the cooling liquid.

7. A method for cooling an electronic device having an aluminum electrolytic capacitor, comprising the steps of: a liquid immersion cooling step of immersing a part or the whole of the electronic device in a cooling liquid to cool it, the immersion cooling step is performed such that at least the aluminum electrolytic capacitor is immersed in the cooling liquid; The cooling liquid is a hydrocarbon refrigerant, a sealing body of the aluminum electrolytic capacitor having a rubber member in a region that comes into contact with the cooling liquid during immersion cooling, The method for cooling an electronic device, wherein the rubber member is made of a rubber composition or a vulcanizate thereof, the rubber composition containing a rubber component having a Hansen solubility parameter distance with respect to the cooling liquid of 8.0 or more.

8. A method for producing an aluminum electrolytic capacitor for liquid immersion cooling, which is subjected to liquid immersion cooling in a hydrocarbon-based refrigerant and has a sealing body provided with a rubber member, comprising the steps of: a sealing step of sealing the capacitor element with the sealing body, In the sealing step, the sealing body is disposed so that the rubber member is located in an area that comes into contact with the hydrocarbon-based refrigerant during the immersion cooling; The rubber member is made of a rubber composition or a vulcanizate thereof, the rubber composition including a rubber component having a Hansen solubility parameter distance with the hydrocarbon refrigerant of 8.0 or more.

9. 9. The method for producing an aluminum electrolytic capacitor for liquid immersion cooling according to claim 8, wherein the rubber component is at least one selected from the group consisting of nitrile rubber, hydrogenated nitrile rubber, acrylic rubber, and fluororubber.

10. 10. The method for producing an aluminum electrolytic capacitor for liquid immersion cooling according to claim 8, wherein the rubber component contains more than 0 wt% and 65 wt% or less of a rubber having a Hansen solubility parameter distance with the hydrocarbon refrigerant of less than 8.0, based on a total amount of the rubber component.

Citation Information

Patent Citations

  • Liquid immersion cooling device

    JP2022169554A

Cited By

  • Capacitor capable of being used for immersion cooling and method for manufacturing the same

    WO2025205515A1