Biodegradable polymer composition and method of producing the same

A biodegradable polymer composition using hemp waste as a carbon source addresses the environmental burden of plastic waste by providing improved mechanical properties and cost-effective production through microbial fermentation with specific bacteria strains.

JP2024133076AInactive Publication Date: 2024-10-01MOHARRAM VENTURES INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024104637
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2018-08-24
Filing Date
2024-06-28
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The environmental burden of plastic waste is increasing due to the slow degradation of conventional plastics, and there is a need for biodegradable plastics with improved mechanical properties and reduced production costs, as well as a need for sustainable use of hemp waste from the cannabis industry.

Method used

A biodegradable polymer composition comprising polyhydroxybutyrate, poly(3-hydroxybutyrate-co-3-hydroxyhexane), thermoplastic starch, compatibilizers such as sodium dihexylsulfosuccinate and maleic anhydride, and microcrystalline cellulose, produced using hemp waste as a carbon source through microbial fermentation by specific bacteria strains.

Benefits of technology

The composition offers improved mechanical properties and reduced production costs, with hemp waste being effectively utilized as a sustainable carbon source, enhancing the biodegradability and applicability of biodegradable plastics.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide a biodegradable polymer, in particular, a biodegradable polymer composition and a method of producing the biodegradable polymer using cannabis waste as a carbon source.SOLUTION: A biodegradable polymer composition according to the present invention comprises polyhydroxybutyrate and poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) blended with: thermoplastic starch; one or more compatibilizers selected from the group consisting of dihexyl sodium sulfosuccinate and maleic anhydride; and one or more additives selected from the group consisting of micro-crystalline cellulose and cellulose. Methods of producing a biodegradable polymer employs processed cannabis waste as a carbon source.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to biodegradable polymers, and in particular to biodegradable polymer compositions and methods for producing biodegradable polymers using Cannabis waste as a carbon source. [Background technology]

[0002] Plastics are light, durable, and versatile materials that are essential components of many industries, from construction to medicine, from consumer goods to packaging. Much of the production of plastic materials relies on non-renewable resources and is economically, environmentally, and long-term unsustainable. This problem is exacerbated by the time it takes many types of plastic to cause environmental damage. Typically, plastics used in consumer products such as plastic straws take about 200 years to degrade in the environment. More durable plastics, such as those used in fishing grounds, can take as long as 600 years to break down.

[0003] As a result, the burden of plastic waste on the environment is growing, and efforts to reduce plastic waste, such as banning single-use plastic items, including straws, are urgently needed. Other efforts, such as increasing plastic recycling programs, are limited by cost and the fact that most plastics can only be reused a limited number of times before their physical properties make them unsuitable for further use. Another option to address the problem of plastic waste accumulation in the environment is the production of plastics that decompose more quickly in the environment.

[0004] Biodegradable plastics can be broken down by microorganisms into single molecules such as water, carbon dioxide, and methane, and become biomass in a much shorter time than is required for typical plastics. Many biodegradable plastics can be produced from renewable resources rather than non-renewable petrochemical resources. However, biodegradable plastics are known to have many undesirable properties, such as being brittle or having poor thermal stability. Other known biodegradable plastics are prohibitively expensive to produce, which inhibits their widespread application.

[0005] Therefore, there is a need for new biodegradable plastics with improved mechanical properties. Furthermore, there is a need for new methods of producing biodegradable plastics from renewable raw materials in order to reduce production costs.

[0006] Cannabis waste and its disposal is expected to become a significant issue for the industry as various jurisdictions begin to legalize recreational use of cannabis. Producing one kilogram of cannabis for consumer use generates eight kilograms of waste. Current disposal methods for cannabis waste are highly regulated, including mixing the cannabis waste with chemicals and other waste materials. Summary of the Invention [Problem to be solved by the invention]

[0007] There is therefore a need to develop useful uses for the increasing amounts of hemp waste produced in this new industry. [Means for solving the problem]

[0008] The biodegradable polymer composition according to the present invention comprises poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) blended with polyhydroxybutyrate and one or more compatibilizers selected from the group consisting of thermoplastic starch, sodium dihexylsulfosuccinate and maleic anhydride, and one or more additives selected from the group consisting of microcrystalline cellulose and cellulose.

[0009] In another embodiment, the biodegradable polymer composition comprises 5% to 70% by weight of polyhydroxybutyrate, 5% to 70% by weight of poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), 5% to 45% by weight of thermoplastic starch, 0.5% to 35% by weight of one or more compatibilizers, and 0.5% to 15% by weight of one or more additives.

[0010] In another embodiment, the biodegradable polymer composition comprises 10% to 30% by weight of polyhydroxybutyrate, 20% to 60% by weight of poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), 10% to 30% by weight of thermoplastic starch, 10% to 20% by weight of one or more compatibilizers, and 1% to 10% by weight of one or more additives.

[0011] In another embodiment, the biodegradable polymer composition comprises 20% by weight polyhydroxybutyrate, 40% by weight poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), 20% by weight thermoplastic starch, 15% by weight of one or more compatibilizers, and 5% by weight of one or more additives.

[0012] In another aspect of the present invention, there is provided a method for producing a biodegradable polymer using Cannabis waste as a carbon source, comprising the steps of: a) mechanically disrupting the Cannabis waste; b) heating the Cannabis waste in an inorganic acid solution at a temperature of at least 121° C. for 25 minutes to produce a Cannabis / acid solution; c) cooling, neutralizing and filtering the Cannabis / acid solution to produce a filtrate; d) mixing the filtrate with an inorganic salt medium in a ratio of 1:1 to 1:2 to produce a conditioned medium; e) culturing the conditioned medium with Bacillus subtilis, Cupriavidus necator, Bacillus cereus, Bacillus brevis, Caulobacter cresentus, Bacillus sphaericus, Bacillus coagulans, Bacillus sphaericus ... coagulans, Bacillus megaterium, Bacillus circulands, Bacillus licheniformis, Escherichia coli, Microlanatus phosphovorous, Rhizobium meliloti, Rhizobium viciae, Bredyrhizobium japonicum, Burkholderia cepacia, Burkholderia sacchari, Cupriavidus necactor, Neptunamonas antarctica Antarctica, Azotobacter vinelandii, Pseudomonas putida, Pseudomonas aeruginosa, Aeromonas caviae, Aeromonas hydrophilainoculating a starter culture of a microorganism selected from the group consisting of naturally occurring and genetically engineered strains of Lactobacillus hydrophila, Aeromonas punctate, Alcaligenes latus, Halomonas boliviensis, Lactobacillus rhamnosus, and Fermicutes bacterium, and culturing at least 30° C. for 48-72 hours to produce a culture; and f) extracting a biodegradable polymer from the culture.

[0013] In another embodiment, the step of extracting the biodegradable polymer from the culture comprises the following steps: a) filtering the culture through a membrane having a pore size of about 1 mm; b) separating the cells of the microorganism from the filtered culture; c) suspending the cells in a NaOH solution and incubating at a temperature of at least 30° C. for at least 1.5 hours to release the biodegradable polymer from the cells; d) separating the biodegradable polymer from the NaOH solution and resuspending it in water; e) separating the biodegradable polymer from the water and resuspending it in an ethanol solution; and f) separating the biodegradable polymer from the ethanol solution.

[0014] In another aspect of the invention, a method for producing a conditioned medium from Cannabis waste for use in the production of biodegradable polymers comprises the steps of: a) mechanically disrupting the Cannabis waste; b) heating the Cannabis waste in a mineral acid solution at a temperature of at least 121° C. for 25 minutes to produce a Cannabis / acid solution; c) cooling, neutralizing, and filtering the Cannabis / acid solution to produce a filtrate; and d) mixing the filtrate with a mineral salt medium in a ratio of 1:1 to 1:2 to produce a conditioned medium.

[0015] In another embodiment, the method further comprises agitating the treated Cannabis waste in water to decompose the Cannabis waste. The resulting mixture is filtered, and the filtrate is then heated and stirred in sodium hydroxide and hydrogen peroxide. The resulting slurry is filtered, the pH is neutralized, and a dry biomass is produced prior to heating the Cannabis waste in a mineral acid solution.

[0016] In another embodiment, the step of cooling, neutralizing, and filtering the hemp / acid solution includes adding cold deionized water to stop the reaction. The resulting mixture is centrifuged and the precipitate is washed with deionized water until a neutral pH is reached. The cellulose is hydrolyzed by acid hydrolysis in 0.5 M, 67% zinc chloride at 70° C., and the final product is diluted with sterile phosphate buffered saline.

[0017] In another aspect of the present invention, there is provided a method for producing a biodegradable polymer, comprising the steps of: a) culturing Bacillus subtilis, Capricornis necator, Bacillus cereus, Bacillus brevis, Caulobacter crescentus, Bacillus sphaericus, Bacillus coagulans, Bacillus megaterium, Bacillus circulans, Bacillus licheniformis, Escherichia coli, Microlanthus cerevisiae, Bacillus niger ... · Phosphoborus, Rhizobium meliloti, Hairy vetch Rhizobium vikiae, Rhizobium japonicum, Burkholderia cepacia, Burkholderia sacchari, Capriavidus necator, Neptunamonas antarctica, Azotobacter vinelandii, Pseudomonas putida, Pseudomonas aeruginosa, Aeromonas caviae, Aeromonas hydrophila, Aeromonas punctata, Alkali The method includes the steps of inoculating a starter culture of a microorganism selected from the group consisting of Genes latus, Halomonas boliviensis, Lactobacillus rhamnosus, and natural and engineered strains of the phylum Firmicutes and culturing the culture at a temperature of at least 30° C. for 48 to 72 hours to produce a culture; b) filtering the culture through a membrane having a pore size of about 1 mm; c) isolating cells of the microorganism from the filtered culture; d) suspending the cells in a NaOH solution and incubating at a temperature of at least 30° C. for at least 1.5 hours to release a biodegradable polymer from the cells; e) separating the biodegradable polymer from the NaOH solution and resuspending it in water; f) separating the biodegradable polymer from the water and resuspending it in an ethanol solution; and g) separating the biodegradable polymer from the ethanol solution.

[0018] In another embodiment, the method comprises the steps of producing PHB using a conditioned medium produced from hemp waste and growing one or more microorganisms capable of producing PHB in a nutrient medium from a stock. Inoculating the conditioned medium with one or more microorganisms. Supplementing the conditioned medium with a limited nitrogen source and growing one or more microorganisms in the conditioned medium. Centrifuging the conditioned medium to separate cells of one or more microorganisms from the conditioned medium and drying the cells. Resuspending the dried cells in distilled water and adding sodium hydroxide to extract PHB from the cells. Adjusting the pH to 7.0 and centrifuging the mixture to separate PHB granules from the suspension and stop the reaction. Optionally, rinsing the granules with distilled water and centrifuging the mixture again. Adding mineral acid to separate the granules and centrifuging the mixture. Discarding the liquid phase and washing the product in an alkaline bath to purify the PHB. Optionally, rinsing the PHB with water and centrifuging. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The present invention relates to a biodegradable polymer composition and a method for making the same, comprising polyhydroxybutyrate (PHB) and poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (PHBHx) blended with thermoplastic starch (TPS), one or more compatibilizers, and one or more additives.

[0020] Either or both of the PHB and PHBHx used in the biodegradable polymer compositions described herein are preferably produced by microorganisms that are naturally occurring or genetically engineered to produce PHB and / or PHBHx. The PHBHx can be a random or non-random copolymer of PHB and HHx monomers. Preferably, the 3 hydroxyhexanoic acid units of the biosynthesized PHBHx copolymer remain in the amorphous phase of the semi-crystalline PHBHx.

[0021] Suitable microorganisms for the production of biodegradable polymers, including PHB and / or PHBHHx, include Bacillus subtilis, Caprifolius necator, Bacillus cereus, Bacillus brevis, Caulobacter crescentus, Bacillus sphaericus, Bacillus coagulans, Bacillus megaterium, Bacillus circulans, Bacillus licheniformis, Escherichia coli, Microlanatus phosphoborus, Rhizobium meliloti, Rhizobium vikiae, Rhizobium japonicum, Burkholderia cepacia, and B. cerevisiae. Cholderia saccharii, Capriavidus necator, Neptuna antarctica, Azotobacter vinelandii, Pseudomonas putida, Pseudomonas aeruginosa, Aeromonas caviae, Aeromonas hydrophila, Aeromonas punctata, Alcaligenes latus, Halomonas boliviensis, Lactobacillus rhamnosus, and genetically engineered strains of the phylum Firmicutes are used to produce PHB and PHBHx for the biodegradable polymer compositions described herein. Bacillus subtilis is a gram-positive bacterium and therefore does not contain the toxic lipid A present in gram-negative bacteria and is therefore preferred. Contamination of biodegradable polymers with lipid A is undesirable in certain applications such as food packaging, medical devices or packaging, hygienic packaging, and infant products.

[0022] The genetically modified microorganisms used in the methods described herein are genetically modified to express genes, including transgenes, necessary for the production of one or more biodegradable polymers. Preferably, the biodegradable polymer produced is PHB. Suitable genes include one or more of the phaA, phaB, phaC, phaJ, and phaP genes, which encode acetyl-CoA acetyltransferase, acetyl-CoA reductase, and PHB polymerase. Many microorganisms naturally express one or more of these genes. Some microorganisms may also express genes encoding one or more depolymerases that degrade one or more biodegradable polymers, including PHB. Preferably, the genetically engineered microorganisms used in the methods described herein express genes necessary for the production of PHB and do not express genes encoding depolymerases that can degrade PHB or any other desired biodegradable polymer produced by the selected microorganism.

[0023] For example, once synthesized and extracted by one of the methods described herein, PHB is blended with PHBHx, thermoplastic starch, one or more compatibilizers, and one or more additives. The thermoplastic starch used in the biodegradable plastic composition of the present invention is a plasticized natural polymer, preferably having low concentrations of ascorbic acid and citric acid, 30% glycerol as a plasticizer, and about 20% water by weight relative to the starch. The thermoplastic starch may be present in an amount up to 45% by weight of the biodegradable polymer composition.

[0024] Thermoplastic starch may be prepared by any suitable method for preparing plasticized natural polymers, such as mixing natural starch with a plasticizer and preparing the plasticizer in a twin-screw extruder at an elevated temperature of about 30° C. to about 200° C. Preferably, a mixture of water and glycerol is used as the plasticizer. Plasticization of the thermoplastic starch may be accomplished prior to mixing the thermoplastic starch into the biodegradable polymer composition, or by adding all the components (i.e., starch, glycerol, water, other components of the biodegradable polymer composition) at once to produce the final blend.

[0025] Compatibilizers may include one or more of dihexyl succinate, dihexyl sodium sulfosuccinate, maleic anhydride, methylene diphenyl isocyanate, and dioctyl fumarate or other polar monomer grafted polyolefins. Preferably, the sodium dihexyl sulfosuccinate and maleic anhydride are both present in an amount of 0.5 to 35% by weight.

[0026] The additives may include one or more of microcrystalline cellulose or cellulose. Preferably, the microcrystalline cellulose and the cellulose are both present in an amount of 0.5 to 35% by weight.

[0027] The time required for degradation of the biodegradable polymer composition may be selectively increased or decreased by manipulating the amount of thermoplastic starch, microcrystalline cellulose, and / or cellulose in the composition. As the relative amount of thermoplastic starch, microcrystalline cellulose, and / or cellulose increases, the time required for degradation of the composition decreases. Preferably, the relative amount of thermoplastic starch, but not the relative amount of microcrystalline cellulose or cellulose, is adjusted to selectively increase or decrease the degradation time of the composition. Furthermore, the time required for degradation of the biodegradable polymer composition may be selectively increased or decreased by manipulating the amount of PHBHx in the composition. As the relative amount of PHBHx increases, the time required for degradation of the composition increases.

[0028] Carbon sources used for the production of biodegradable polymers include hemp waste, leaves, fish solid waste, maple juice, pumpkin seeds, grape press or grape marc, or winemaking / brewing / distillery waste. Preferably, hemp waste materials are used as the carbon source for the production of PHB. Hemp waste consists of the roots, trimmings, leaves, stalks, and stems of the hemp plant, essentially all parts of the Cannabis sativa L. plant except the flower buds.

[0029] Cannabis waste is particularly suitable for use as a carbon source in the microbial production of PHB because Cannabis plants have a high biomass content, require only moderate water and fertilizer, and grow rapidly in most climates. Cannabis waste has a unique hierarchical pore structure and interconnected macropores compared to other potential carbon sources such as agricultural biomass, forest biomass, coal, petroleum residues, and bone. As a result, Cannabis waste has desirable properties for use as a carbon source, including its porosity, adsorption capacity, and degree of surface reactivity. Compared to other potential carbon sources, Cannabis waste has a high carbon concentration and low nitrogen, potassium, and phosphorus contents, which are suitable for the microbial production of PHB.

[0030] Cannabis waste is first processed for use in the production of PHB by mechanical disruption in the following manner: Raw hemp waste may be treated by shredding, grinding, pressing, or other suitable mechanical disruption means to increase the surface area available for removal of cellulose and fatty acids. Fatty acids are then separated from the processed hemp waste to provide a carbon source for the synthesis of PHB. EXAMPLES

[0031] [Prepared medium 1] The treated hemp waste is mixed with 1% sulfuric acid solution at a ratio of 10 g per 100 mL of acid solution. The solution is heated at 121° C. for 25 minutes, preferably in an autoclave, and then cooled to room temperature. The solution is then neutralized with 2 M NaOH solution and filtered through a sieve to remove larger particles of vegetable waste. The solution is then centrifuged at 1500 g for 20 minutes and the supernatant is filtered through a membrane with a pore size of about 1 mm. The resulting filtrate, i.e., hemp waste hydrolysate, can be used immediately or stored at 4° C. until required.

[0032] Prepare medium 1 by mixing the filtrate with 2X mineral salts medium (0.9 g (NH4)2S04, 0.3 g KH2P04, 1.32 g Na2HP04, 0.06 g MgS04·7H20, 300 uL of trace element solution (0.97 g FeCl3, 0.78 g CaCl2, 0.0156 g CuS04·5H20, 0.326 g NiCl2·6H20 in 100 mL of 0.1 M HC1) in a 1:1 ratio. Immediately autoclave the medium at 121°C for 10 minutes. EXAMPLES

[0033] [Extract 1] Synthesis and extraction of biodegradable polymers may be performed by the following method: A suitable microorganism is grown in nutrient medium from a stock that has been shaken at 150 revolutions per minute for 72 hours at 30°C to produce a starter culture. After 72 hours, the starter culture is inoculated at 1 / 10 (v / v) into Prepared Medium 1 and shaken at 150 rpm for 72 hours at 30°C to produce a culture.

[0034] The culture is then filtered through a membrane with a pore size of approximately 1 mm to remove insoluble plant material. The microbial cells are then separated from the filtered culture by centrifugation at 1500 g for 20 minutes. After removing the supernatant, the cells are washed by resuspending the cells in mineral salts medium, repeating the centrifugation and removing the supernatant again.

[0035] The cells were then resuspended in 150 mL of 0.2 M NaOH solution, the solution was vortexed vigorously to homogenize, and then incubated at 30° C. for 1.5 h, which lyses the cells and releases the biodegradable polymer into the NaOH solution. The biodegradable polymer is then separated from the NaOH solution by centrifugation at 1500 g for 20 min and removal of the supernatant.

[0036] The biodegradable polymer is resuspended in 150 mL of Milli-Q water and then separated from the water by centrifugation at 1500 g for 20 min. The supernatant is removed to remove impurities. The biodegradable polymer is then resuspended in 150 mL of 1% ethanol solution and separated from the ethanol solution by centrifugation at 1500 g for 20 min. The supernatant is again discarded to remove further impurities. EXAMPLES

[0037] [Prepared medium 2] Add 5 g of mill waste to 300 mL of deionized water and sonicate at room temperature. Filter through Whatman No. 1 filter paper and vigorously stir with 100 mL of a solution of sodium hydroxide (5%, w / v) and hydrogen peroxide (1.1%, v / v) for 90 min at 55 °C. Filter the slurry, neutralize the pH, and dry at 50 °C. Add 5 g of dried biomass to 100 mL of 6 M sulfuric acid, vigorously stir for 30 min, and quench the reaction by adding 500 mL of cold deionized water. Centrifuge at 10,000 rpm for 10 min and wash with deionized water until a neutral pH is reached. Acid hydrolysis with 67% zinc chloride at 0.5 M and 70 °C obtains single monomers from cellulose, which ideally results in a soluble sugar yield of >80%. The final glucose product is then diluted in 1 L of sterile phosphate buffered saline pH 7.0, thereby producing Conditioned Medium 2 (final concentrations: 8 g / L NaCl, 0.2 g / L KCl, 1.44 g / L Na2HP04, 0.24 g / L K2HP04). EXAMPLES

[0038] [Extract 2] The synthesis and extraction of PHB for use in the biodegradable polymer compositions of the present invention may be carried out by the following method: A suitable Bacillus species is grown in nutrient medium from stock overnight with shaking at 120 rpm at 37°C. 8A density of cells / mL may be added at 1 / 10 v / v in conditioned medium 2 supplemented with a limited nitrogen source such as Com Steep Liquor (CSL) or ammonium salts at a concentration equivalent to 0.05% NH4C1 and grown at 37° C. with shaking at 120 rpm for 72 hours. The cells are then centrifuged at 6500 g for 10 minutes and dried at 50° C.

[0039] The dry cell mass is measured, and PHB can be extracted by sodium hydroxide extraction and selective lysis. The cells are resuspended in distilled water and sodium hydroxide extraction is performed by adding NaOH (0.2N NaOH, 30°C, 1-5 hours). The reaction is stopped by adjusting the pH to 7.0 with HCl. Centrifuge at 2500g for 20 minutes. The PHB granules are gently rinsed with distilled water, centrifuged again, and air-dried.

[0040] Selective dissolution is achieved by adding a mineral acid, such as sulfuric acid, to the mixture, so that the granules separate in a solid phase while the undesired material separates in a liquid phase. These phases can be further separated by centrifugation at 5000 g. The unwanted supernatant (liquid phase) is discarded while the solid phase proceeds during processing. Although the mineral acid successfully isolates the PHB from the mixture, the purity is preferably improved before use. This is achieved by washing the product in an alkaline bath, such as NaOH (pH 10). After washing, the yield and purity obtained are high (>97%). Commercially available bleach can be used to decolorize the product. After a final centrifugation and water rinse, the PHB product is ready for use.

[0041] To measure PHB production, the pellet is centrifuged and washed with alcohol. The pellet is dissolved in chloroform and transferred to a pre-weighed clean serum tube. The chloroform is evaporated, the tube is weighed, and the amount of PHB is calculated. This method can produce a yield of 2-5 g / L of PHB from a cell mass of 7-9 g / L. This growth method can also be applied to large-scale production of PHB using Bacillus species, as it requires a small volume of culture medium and a short time. Alternatively, a similarly engineered Capriavidus necator strain can be used instead. EXAMPLES

[0042] [Extract 3] In another embodiment, PHB may be synthesized and extracted by the following method. PHB may be produced using Capriavidus necator as the microorganism and hemp waste as the carbon source according to the following method. Capriavidus necator is Alcaligenes eutrophus H16 (Capriavidus necator was previously known as Alcaligenes eutrophus). A. euthrophus H16 is cultivated in nitrogen-limited mineral salts medium containing 1% (v / v) hemp oil and 0.05% (w / v) NH4Cl at 30°C for 72 hours. Kanamycin (50 mg / L) is added to maintain the broad-host-range plasmid inserted in A. euthrophus H16. After growth, the cells are harvested, washed twice with distilled water, and lyophilized. PHB is extracted using hot chloroform in a Soxhlet apparatus and purified by methanol reprecipitation.

[0043] PHB may be produced by the method of extraction 3 at a rate of about 0.0128 grams of PHB per gram of hemp oil per hour. EXAMPLES

[0044] [Extract 4] In another embodiment, PHB may be synthesized and extracted using Capriavidus necator as a microorganism and Cannabis waste as a carbon source by the following method: Optionally, a surfactant, gum arabic, may be added to the reaction medium to enhance the ability of Capriavidus necator to interact / utilize Cannabis oil, since Cannabis oil is non-toxic and does not inhibit the growth of Capriavidus necator. Capriavidus necator may be grown in minimal medium containing 2% fructose and 0.1% NH4Cl (16 g / L), NaH2P04 (4 g / L), Na2HP0 (4.6 g / L), K2S04 (0.45 g / L), MgS04 (0.39 g / L), CaCl2 (62 mg / L), and 1 ml / L of trace element solution (15 g / L FeS04·7H20, 2.4 g / L MnS04·H20, 2.4 g / L ZnS04·7H20, and 0.48 g / L CuS04·5H20 dissolved in 0.1 M hydrochloric acid). Cells from the minimal medium are used to inoculate each fermenter to reach an OD600 of 0.1. Each reaction vessel contains 400 mL of emulsified hemp oil medium. In minimal medium containing 0.1% NH4Cl, approximately 2% hemp oil is used. To prepare the medium, use a 10x solution of gum arabic in water and stir rapidly. Centrifuge at 10,500g to separate insoluble particles. Mix water, clear gum arabic liquid, and hemp oil with sodium phosphate (4.0 g / L) and K2S04 (0.45 g / L). Emulsify the mixture by homogenization or sonication. The amount of water added before emulsification depends on the specific equipment used to make the emulsion. After emulsification, the mixture is autoclaved and cooled, followed by addition of MgSO4 (0.39 g / L), CaCl2 (62 mg / L), trace elements (15 g / L FeSO4·7H20, 2.4 g / L MnSO4·H20, 2.4 g / L ZnSO4·7H20, and 0.48 g / L CuSO4·5H20 dissolved in 0.1 M hydrochloric acid), and gentamicin (10 pg / mL). Each reaction vessel is maintained at 30 °C with a pH of 6.8 (controlled with 2 M NaOH) and agitated at a speed of 500-900 rpm with a dissolved oxygen concentration of 40% for 72 h. Preferably, a fed-batch culture technique is used to maintain excess carbon in order to increase PHB production.

[0045] PHB may be produced by the method of extraction 4 at a rate of about 0.2415 grams of PHB per gram of hemp oil. EXAMPLES

[0046] [Extract 5] In another embodiment, PHB may be synthesized and extracted using genetically engineered strains of Capriavidus necator and E. coli, and optionally Aeromonas hydrophila carrying phbA and phbB genes as microorganisms and Cannabis waste by the following method: Cannabis waste is first crushed and placed in water at about 2% (w / v) and at a temperature of about 30° C. The Cannabis-water mixture is inoculated with a mixed culture of Capriavidus necator and E. coli, and optionally A. hydrophila and fertilizer, such as rice bran extract, are added at 0.1%. The reaction medium is then stirred and grown for 20 hours. After the initial growth period, the reaction medium is stirred for an additional 15 hours, but no further fertilizer is added to induce nitrogen deficiency conditions and promote the production of PHB.

[0047] Extraction of PHB is achieved by adding an inorganic acid such as sulfuric acid to the reaction medium after about 35 hours. The PHB granules are separated by centrifugation at 5000 g. The unwanted supernatant (liquid phase) is discarded while the solid phase proceeds during processing. The inorganic acid isolates PHB from the mixture. The purity of the compound can be improved by washing in an alkaline bath such as NaOH (pH 10) followed by a final centrifugation and rinsing with water. This method results in high yields and purity of PHB (>97%). In some cases, the product can be decolorized using commercially available bleach. EXAMPLES

[0048] [Prepared medium 3] In another embodiment, PHB can be synthesized and extracted using Pseudomonas putida GPpl04 as the microorganism and hemp waste as the carbon source as follows: P. putida is grown overnight in LB medium containing 50 mg / L kanamycin at 30°C with shaking at 200 rpm. The phosphate buffered saline solution for culturing this strain is composed of 9.0 g / L Na2HP04·12H20, 1.5 g / L KH2PO4, 1.0 g / L (NH4)2S04, 0.4 g / L MgS04·7H20, and pH 7.0. EXAMPLES

[0049] [Extract 6] Density 1.5×10 8 Add 1 / 10 v / v to 1 L of prepared medium 3 and grow at 30 °C with shaking at 200 rpm for 72 h. PHB may be extracted using sodium hypochlorite as follows: Add 100 mL of sodium hypochlorite (30%) to 8 g of biomass and incubate at 37 °C for 90 min. Centrifuge the pellet and wash with alcohol. Dissolve the pellet in chloroform and, if necessary, transfer to a clean, pre-weighed serum tube. Allow the chloroform to evaporate, weigh the tube and calculate the amount of PHB.

[0050] Although the present invention has been described with reference to exemplary embodiments, those skilled in the art will recognize that various modifications can be made and equivalents can be substituted for elements thereof without departing from the scope of the invention as set forth in the claims. That is, it is not intended that the invention be limited to the specific embodiments disclosed herein.

Claims

1. 1. A biodegradable polymer comprising: 5% to 70% by weight of polyhydroxybutyrate; 5% to 70% by weight of poly(3-hydroxybutyrate-co-3-hydroxyhexanoate); 5% to 45% by weight of thermoplastic starch; 0.5% to 35% by weight of one or more compatibilizers; and 0.5% to 15% by weight of one or more additives.

2. (i) the one or more compatibilizers are selected from the group consisting of dihexyl succinate, sodium dihexyl sulfosuccinate, maleic anhydride, methylene diphenyl isocyanate, and dioctyl fumarate; and 2. The biodegradable polymer of claim 1, wherein (ii) the one or more additives are selected from the group consisting of microcrystalline cellulose and cellulose.

3. 10. The biodegradable polymer of claim 1, wherein the thermoplastic starch is a plasticized natural polymer comprising about 30% by weight glycerol and about 20% by weight water.

4. 4. The biodegradable polymer of claim 3, comprising from 20% to 60% by weight of poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), from 10% to 30% by weight of thermoplastic starch, from 10% to 20% by weight of one or more compatibilizers, and from 1% to 10% by weight of one or more additives.

5. 4. The biodegradable polymer of claim 3, comprising 20% ​​by weight polyhydroxybutyrate, 40% by weight poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), 20% by weight thermoplastic starch, 15% by weight of one or more compatibilizers, and 5% by weight of one or more additives.

6. 2. The method for producing a biodegradable polymer according to claim 1, wherein a Cannabis waste is used as a carbon source, the method comprising the steps of: a) heating the hemp waste in a mineral acid solution at a temperature of at least 121° C. for 25 minutes to produce a hemp / acid solution; b) filtering the cannabis / acid solution to produce a filtrate; c) mixing the filtrate with a mineral salts medium in a ratio of 1:1 to 1:2 to produce a conditioned medium; and d) The prepared medium is cultured using a culture medium selected from the group consisting of Bacillus subtilis, Cupriavidus necator, Bacillus cereus, Bacillus brevis, Caulobacter crescentus, Bacillus sphaericus, Bacillus coagulans, Bacillus megaterium, Bacillus circulans, Bacillus cereus ... circulands, Bacillus licheniformis, Escherichia coli, Microlanatus phosphovorous, Rhizobium meliloti, Rhizobium viciae, Bredyrhizobium japonicum, Burkholderia cepacia, Burkholderia saccharii sacchari, Cupriavidus necator, Neptunamonas Antarctica, Azotobacter vinelandii, Pseudomonas putida, Pseudomonas aeruginosa, Aeromonas caviae, Aeromonas hydrophila, Aeromonas punctate, Alcaligenes latus latus, Halomonas boliviensis, Lactobacillus rhamnosus, and Fermicutesinoculating a starter culture of a microorganism selected from the group consisting of naturally occurring and genetically engineered strains of Propionibacterium bacterium and culturing at least 30° C. for 48-72 hours to produce a culture; A method comprising:

7. In addition, the following: a. filtering the culture to separate the microbial cells; b. suspending the cells in a NaOH solution and incubating at a temperature of at least 30° C. for at least 1.5 hours to release the biodegradable polymer from the cells; c. Separating the biodegradable polymer from the NaOH solution and resuspending it in water; d. separating the biodegradable polymer from the water and resuspending it in an ethanol solution; and e. separating the biodegradable polymer from the ethanol solution; Extracting the biodegradable polymer from the culture, The method according to claim 6.

8. 7. The method of claim 6, wherein the microorganism is a genetically engineered strain of Bacillus subtilis expressing one or more genes encoding acetyl-CoA acetyltransferase, acetyl-CoA reductase, and polyhydroxybutyrate polymerase.

9. 9. The method of claim 8, wherein the one or more genes are selected from the group consisting of phaA, phaB, phaC, phaJ, and phaP.

10. The method of claim 6, wherein the microorganism is a metabolically engineered strain of E. coli.

11. The method of claim 10, wherein the biodegradable polymer comprises poly(3-hydroxybutyrate-co-3-hydroxyhexanoate).

12. The method of claim 10, wherein the biodegradable polymer comprises poly(glycolate-co-lactate-co-3-hydroxybutyrate-co-4-hydroxybutyrate).

13. The method of claim 6, wherein the microorganism is a genetically modified E. coli strain.

14. The method of claim 13, wherein the biodegradable polymer comprises prolyl-4-hydroxylase.

15. The method of claim 13, wherein the biodegradable polymer comprises poly(3-hydroxybutyrate-co-3-hydroxyhexanoate).

16. 2. Use of Cannabis waste as a carbon source for the production of the biodegradable polymer according to claim 1.

17. 17. The use according to claim 16, wherein the Cannabis waste comprises one or more of the roots, trimmings, leaves, stalks and stems of the Cannabis plant.