Cellulose nanofiber composition and production method thereof

A CNF composition with diol or diol derivative and water addresses storage and compatibility issues, enabling easy redispersion and improved reinforcing effects in resins and rubbers.

JP2024133092AActive Publication Date: 2024-10-01RENGO CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024109493
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-08-26
Filing Date
2024-07-08
Publication Date
2024-10-01
Estimated Expiration
2040-08-26

AI Technical Summary

Technical Problem

Existing methods for producing and storing cellulose nanofibers (CNF) face challenges such as high water content leading to increased load during transportation and storage, difficulty in redispersing after drying, and poor compatibility with hydrophobic resins and rubbers, resulting in weakened reinforcing effects.

Method used

A CNF composition containing a diol or diol derivative, along with water, is used to achieve low moisture content storage and easy redispersion, with the diol compound providing compatibility and ease of removal by evaporation.

Benefits of technology

The CNF composition allows for reduced transportation and storage loads, easy redispersion in various solvents, and improved compatibility with resins and rubbers, enhancing reinforcing effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133092000001_ABST
    Figure 2024133092000001_ABST
Patent Text Reader

Abstract

To provide a composition capable of storing a cellulose nanofiber in a dry state in which a moisture content is reduced significantly, capable of re-dispersing the cellulose nanofiber easily to a rubber or resin after storage thereof when adding the cellulose nanofiber, and after dispersion or addition, easily removing an unnecessary component for facilitating use of the cellulose nanofiber.SOLUTION: There is provided a cellulose nanofiber composition including: a diol compound which is formed of diol, a diol derivative or both thereof; and water.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composition in which cellulose nanofibers are easily redispersible. [Background technology]

[0002] A new material called nanocellulose, in which the fibers that make up plant-derived cellulose materials are broken down to a fiber diameter of less than 1 μm, is attracting attention. Of these, materials with fiber diameters of 3 to 100 nm have a large specific surface area and excellent properties as reinforcing fibers for resins, rubbers, etc. Such fine fibrous nanocellulose is called cellulose nanofiber (hereinafter abbreviated as "CNF"). To manufacture this CNF, cellulose materials such as pulp are finely defibrated in liquid, but since the cellulose material itself is a strong material, a large amount of energy is required for defibration even if you try to defibrate it as it is. Therefore, a technology has been proposed to chemically modify cellulose materials to make them easier to defibrate. The fine fibers obtained by chemically modifying and defibrating such cellulose, as well as the cellulose that is further regenerated from the cellulose, are collectively called CNF.

[0003] Usually, CNF is manufactured in the form of an aqueous suspension dispersed in water. If shipped in this state, the volume and mass of the water, which is the dispersion medium, is much larger than the CNF itself, and the load during transportation is too high. In addition, space is required for storage. Furthermore, it is difficult to use the CNF in combination with a hydrophobic resin if it is in the form of an aqueous suspension. For this reason, it is desirable to use a composition containing as little water as possible.

[0004] However, once this aqueous suspension is dried to reduce the water content to the point where it becomes solid, the individual CNF fibers strongly aggregate together, and there is a problem that they cannot easily be restored to their original dispersed state even if water is added after drying.

[0005] In response to this, Patent Document 1 considers a technology in which various polyhydroxy compounds, including carbohydrates such as sucrose, are added to an aqueous dispersion of microfibrillated cellulose produced according to the procedure described in Patent Document 2 as additives that substantially inhibit hydrogen bonding between cellulose fibers in the cellulose, thereby making it easier to redisperse the cellulose in water after drying.

[0006] Patent Document 3 describes a method for obtaining a dried product that is easily redispersible after drying, in which a hydroxy acid, a hydroxy salt, glycerin or a glycerin derivative is added as a redispersing agent to an aqueous dispersion of CNF to obtain a dried product.

[0007] Furthermore, Patent Document 4 describes a production method in which a water-soluble polymer is added to an aqueous dispersion of CNF and then dried to obtain a solid, in order to add CNF to a rubber composition while maintaining its dispersibility.

[0008] Furthermore, Patent Document 5 describes a polyurethane resin composition obtained by reacting a polyol composition in which cellulose is finely divided in a polyol with a polyisocyanate in order to produce the polyurethane resin composition. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Japanese Patent Application Publication No. 59-189141 [Patent Document 2] U.S. Patent No. 4,374,702 [Patent Document 3] Patent No. 6276740 [Patent Document 4] Re-listed 2017 / 061605 publication [Patent Document 5] JP 2013-194162 A Summary of the Invention [Problem to be solved by the invention]

[0010] However, Patent Document 1 does not specifically describe the size of the microfibrillated cellulose, and the left lower column on page 2 of Patent Document 1 states that Patent Document 2 is referred to for the manufacturing procedure. According to Patent Document 2, from line 55 of column 2, it is described that Orifice 3 must be small enough to apply sufficient shear force to the cellulose slurry, but must be larger than the diameter of the fiber. In other words, the diameter of Orifice 3 is roughly close to the diameter of the microfibrillated cellulose, and in line 57 of column 2 of Patent Document 2, it is described that the diameter is 1 / 64" to 1 / 4". 1 / 64" is converted to 0.40 mm. For this reason, the diameter of the microfibrillated cellulose described in Patent Document 1 is three or more orders of magnitude different from that of CNF, and as a result, the behavior of the water retention and the viscosity of the slurry is completely different, so even a person skilled in the art cannot derive from Patent Document 1 what kind of polyhydroxy compound is suitable for redispersing CNF.

[0011] In addition, the polyhydroxy compound described in Patent Document 1, the redispersing agent described in Patent Document 3, and the water-soluble polymer described in Patent Document 4 have poor volatility and are difficult to remove after use. They tend to remain in the resin or rubber, resulting in problems such as poor compatibility with the resin or rubber, reduced effects such as reinforcement provided by the addition of CNF, and changes in the physical properties of the resin or rubber.

[0012] In addition, the technology described in Patent Document 5 physically pulverizes cellulose directly in polyol instead of in water, making it difficult to sufficiently reduce the fiber diameter for cellulose nanofibers. In addition, instead of adding polyol to disperse CNF, this technology is carried out in a non-aqueous environment both before and after dispersion, and the underlying environment is different from that of the technology of the present application for dispersing CNF in an aqueous suspension.

[0013] Therefore, the object of this invention is to obtain a CNF composition which can be stored in a dry state with a significantly reduced moisture content, can be easily redispersed when added to resin or rubber after storage, and can be easily used by easily removing unnecessary components after dispersion or addition. [Means for solving the problem]

[0014] The present invention solves the above-mentioned problems by providing a CNF composition containing a diol compound consisting of a diol, a diol derivative, or both, water, and CNF.

[0015] The diol compound is considered to be suitable because of the strength of the affinity between the hydroxyl group contained therein and the CNF. A diol is a compound having two hydroxyl groups in a molecule, but a monool having one hydroxyl group has a low boiling point and high volatility, so it evaporates during drying. Even if a monool with a high boiling point is used, these monools are not compatible with water and cannot be used as a dispersant for CNF. On the other hand, a triol having three hydroxyl groups such as glycerin or a triol having more hydroxyl groups can ensure dispersibility, but the boiling point is too high, making it difficult to remove the composition after it is put into a resin or rubber. In contrast, a diol has an excellent balance between volatility and compatibility with water. A diol derivative is a compound in which one or both of the two hydroxyl groups of a diol are modified to give a functional group, and the compatibility with a resin or rubber can be adjusted by the functional group.

[0016] Even in the case of diol compounds, compounds with large molecular weights tend to be difficult to remove by evaporation, so the diol compounds used are selected taking into consideration the balance between volatility and compatibility with water when producing the CNF composition, and redispersibility and removal performance after addition when adding to resins or rubbers.

[0017] Furthermore, particularly when CNF is used as a reinforcing material in producing polyurethane, the CNF composition containing the diol compound, water, and CNF can be used as is, or the CNF composition can be redispersed in the diol compound and then used.

[0018] The CNF composition according to the present invention can have a water content of 10% by mass or less, and a mass mixing ratio of the CNF to the diol compound of 1:2 to 1:10.

[0019] A specific method for producing a CNF composition includes a procedure in which a diol, a diol derivative, or both are added to a water suspension containing dispersed CNFs, and then the water is evaporated to obtain the CNF composition.

[0020] Examples of the use of such a CNF composition include compounding the CNF composition with a resin or rubber to produce a molded product of the resin or rubber containing the CNF, etc. This molded product can be further heated to remove part or all of the diol compound contained therein.

[0021] Another method of using the CNF composition is to produce a polyurethane containing cellulose nanofibers by dispersing CNF in a polyol, and then reacting a polyol containing the diol compound contained in the CNF composition with a polyisocyanate to produce polyurethane. Here, the polyol may be only the diol compound contained in the CNF composition, or an additional polyol compound may be added. Alternatively, a urethane prepolymer obtained by reacting a polyol prepared separately in advance with an excess of polyisocyanate is mixed with the CNF composition, and the isocyanate group in the urethane prepolymer is reacted with the diol compound contained in the CNF composition to extend the chain of the urethane prepolymer, thereby producing a polyurethane containing the CNF composition. The cellulose nanofiber-containing polyurethane obtained in this way has improved strength compared to one not using the CNF composition. Effect of the Invention

[0022] The CNF composition containing the diol compound obtained by this invention can be easily returned to a dispersed state by adding water, even after the water content is reduced and the composition is solidified. It can also be dispersed in a polar solvent other than water, such as dimethylformamide. On the other hand, the CNF composition can be easily dispersed by adding it directly to a molten resin or a kneaded rubber master batch without adding water to the CNF composition. Furthermore, after the CNF composition is dispersed in a resin or rubber, the diol compound can be easily removed by evaporation through heating, and the physical property change of the resin or rubber after the addition can be suppressed while fully exerting the reinforcing effect. In addition, instead of removing the diol compound, the CNF contained in the CNF composition can be used as a material for improving the strength of polyurethane by using the diol compound as a part of the polyurethane material while keeping the CNF dispersed.

[0023] Furthermore, the CNF composition is lighter and has a smaller volume than a CNF dispersed in an aqueous suspension, which reduces the burden on storage and transportation of the CNF composition after its production. [Brief description of the drawings]

[0024] [Figure 1] Photograph of the CNF composition of Example 1 [Diagram 2] Graph showing the measurement results of strain and stress in Experimental Example 2 [Diagram 3] Graph showing the measurement results of strain and stress in Experimental Example 3 DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] The present invention is described in detail below. The present invention is a CNF composition containing a diol compound consisting of a diol, a diol derivative, or both, water, and CNF.

[0026] The CNF used in this invention may include not only cellulose whose molecular structure remains unchanged, but also cellulose whose molecular structure has been chemically modified in part, and cellulose that has been chemically modified and then regenerated into cellulose.

[0027] Examples of chemically modified cellulose include TEMPO-oxidized cellulose (TEMPO-oxidized cellulose), carboxymethyl cellulose (carboxymethyl cellulose), phosphoric acid ester cellulose, and cellulose treated with alkali and carbon disulfide to form xanthate groups (-OCSS). - M + Examples include xanthate cellulose, which has been introduced with cellulose phosphate. Chemically modifying cellulose materials made from materials such as pulp makes it easier to create nanofibers than defibrating the cellulose materials as is. CNF that has been chemically modified and defibrated in this way is called "chemically modified CNF." Of the chemically modified celluloses, cellulose phosphate and xanthate cellulose can be regenerated back to cellulose. CNF obtained by regenerating the molecular structure of chemically modified cellulose back to cellulose is called "regenerated CNF."

[0028] In the following description of this invention, the term CNF refers not only to CNFs obtained by simply defibrating cellulose materials, but also to the above-mentioned chemically modified CNFs and regenerated CNFs. In addition, regenerated CNFs may include not only CNFs in which hydroxyl groups have been once modified to other functional groups such as xanthate groups, but also CNFs in which some remain as other functional groups. Furthermore, these CNFs may be purified before use if necessary.

[0029] In addition, the CNF preferably contains fine fibers having a fiber diameter of 3 nm to 100 nm as the main component. Here, "main component" means that 50% or more of the fibers present fall within the above fiber diameter condition. However, fine fibers having a fiber diameter outside the above range may be contained as long as it does not interfere with the production or use of the composition. The number average fiber diameter is preferably 20 nm or less. If the number average fiber diameter is too large, the surface area relative to the mass becomes small, and the dispersion by the diol compound may not work well. The number average fiber diameter of the CNF is preferably 3 nm or more. The present invention can be carried out even if the fiber diameter is smaller than this, but making it too fine requires a lot of energy and is not very practical in terms of work efficiency.

[0030] A diol compound is used as a dispersant for dispersing CNF in the CNF composition according to the present invention. It is possible to obtain the CNF composition according to the present invention even if a polar solvent other than the diol compound is contained. However, other polar solvents may evaporate during drying or storage, or may require additional steps to remove after use, or may not be removable at all. Therefore, care must be taken when selecting other polar solvents, and the lower the content in the CNF composition, the better.

[0031] The diol compound contained in the CNF composition according to the present invention is a diol, a diol derivative, or both. Here, a diol is a compound having two hydroxyl groups in the molecule. Also, a diol derivative is a compound in which one or both of the hydroxyl groups are modified to provide a functional group. The modification method here includes, for example, etherification and etherification. Specifically, alkyl ethers of diols and alkyl esters of diols are included.

[0032] Examples of the diol compound include diols such as diethylene glycol, triethylene glycol, dipropylene glycol, tripropylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, 1,6-hexylene glycol, and 3-methyl-1,3-butylene glycol, and diol derivatives such as dipropylene glycol monopropyl ether, diethylene glycol ethyl ether acetate, diethylene glycol monoethyl ether, tripropylene glycol methyl ether, and dipropylene glycol methyl ether acetate. These may be used alone or in combination. When CNF is added to a resin or rubber, an appropriate diol compound is selected depending on the compatibility with the resin or rubber. Among them, diethylene glycol, triethylene glycol, dipropylene glycol, tripropylene glycol, dipropylene glycol monopropyl ether, diethylene glycol ethyl ether acetate, 1,4-butylene glycol, and 1,6-hexylene glycol are particularly preferred because they have an excellent balance of residual rate when dried, evaporation performance after use, maintenance of dispersibility, and compatibility with resins and rubbers. As the diol compound having excellent properties, for example, a useful diol compound is one that has a viscosity recovery rate of 50% or more after redispersion, and has a residual rate of 50% or less when the diol compound is added to and mixed with a water suspension of CNF and heated at 105°C for 15 hours.

[0033] The mass mixing ratio of the CNF and the diol compound in the CNF composition is preferably 1:2 to 1:10. Although it depends on the type of the diol compound, if the amount of the CNF is more than 1:2, there is a small amount of the diol compound to maintain dispersibility, so that even if the CNF composition is to be redispersed in water or a diol compound, it may not be able to be dispersed well. On the other hand, if the amount of the diol compound is more than 1:10, the dispersion itself is sufficiently possible, but even if the ratio of the diol compound is increased beyond that, it does not contribute much to improving the redispersibility, and it may take a long time to evaporate after use. In addition, even if the water is removed, the mass of the CNF composition remains large due to the mass of the diol compound, and the advantage of using the CNF composition is reduced.

[0034] The water content of the CNF composition is preferably 10% by mass or less, and more preferably 7% by mass or less. Since water increases the mass and volume of the CNF composition during storage and transportation, it is desirable to have as little water as possible.

[0035] The procedure for producing the CNF composition is as follows: first, the diol compound is added to and mixed with a water suspension of CNF. The mixture is dried to evaporate the water, thereby reducing the water content, and the CNF composition is obtained. As a drying method, the mixture can be dried by leaving it at room temperature, but it is desirable to heat it to shorten the production time. The drying temperature is preferably 50°C or higher, and more preferably 60°C or higher. If the temperature is less than 50°C, the rate at which water evaporates from the mixture is too slow, and the production of the CNF composition takes too long. On the other hand, the drying temperature is preferably 110°C or lower, and more preferably 90°C or lower. If the temperature exceeds 110°C, the diol compound will also evaporate, making it difficult to redisperse the CNF. Although it depends on the selection of the diol compound, the evaporation of the diol compound can also be suppressed by setting the temperature at 90°C or lower. In addition, the drying method for obtaining the CNF composition can be known hot air drying, spray drying, vacuum drying, or the like.

[0036] The CNF composition can be stored and transported with a water content significantly reduced compared to the state of the aqueous suspension after defibrating the CNF. Since it is lightweight and has a small volume, the load during transportation is reduced. After that, the CNF composition can be added directly to resins or rubbers. In addition, the CNF can be easily used as a redispersion of CNF by mixing it in a polar solvent. Since the CNF is suitably dispersed in this redispersion, it can also be suitably used as a thickener, moisture retainer, emulsion stabilizing aid, etc. in cosmetics and paints.

[0037] Here, the polar solvent used to mix the CNF composition and redisperse the CNFs can be water or a solvent other than water, such as dimethylformamide, dimethylsulfoxide, or dimethylacetamide. However, when the diol compound is used as a polymer material, a polar solvent containing the diol compound may be used, or the diol compound itself may be used as the polar solvent.

[0038] The CNF composition can be added directly to thermoplastic resins, rubber, polyurethane, etc. to obtain the effect of CNF, such as strength improvement. Also, the effect of CNF, such as strength improvement, can be obtained by using a part of the compounds constituting the CNF composition as a material for a resin compound to produce a polymer and incorporating CNF in the polymer.

[0039] When the CNF composition is added to a thermoplastic resin such as polyolefin, the CNF composition is added to the molten resin and kneaded to obtain a resin molded product in which the CNF is suitably dispersed in the resin. Examples of the resin include polyolefins such as polyethylene, polypropylene, polyvinyl chloride, and polystyrene, polyesters such as polyethylene terephthalate and polytrimethylene terephthalate, and polyamides such as nylon 6 and nylon 12. The CNF composition may also be added to a resin that has been heated and melted to produce a master batch, which may then be molded by a general method.

[0040] When the CNF composition is added to rubber, the rubber may be, for example, natural rubber or a common synthetic rubber such as butadiene rubber, styrene-butadiene rubber, isoprene rubber, etc. However, since these rubbers tend to have low compatibility with diols, it is preferable to use the diol derivative, which is more hydrophobic than the diol, as the diol compound, since this makes it easier to redisperse the CNF in the rubber.

[0041] In the case where the diol compound contained in the CNF composition is used as a polymer material, for example, polyurethane is produced by polyaddition reaction with polyisocyanate. In that case, after obtaining the CNF composition, the diol compound and other polyols that are materials for the urethane reaction are added to the CNF composition, and the CNF is redispersed in these polyols and reacted with polyisocyanate to produce polyurethane. Alternatively, a urethane prepolymer obtained by reacting a polyol and an excess of polyisocyanate separately prepared in advance with the CNF composition may be mixed with the CNF composition, and the diol compound contained in the CNF composition may be reacted with the isocyanate group in the urethane prepolymer to extend the chain of the urethane prepolymer, thereby producing polyurethane in which the CNF is redispersed. This is preferable because it makes it easier to proceed with the urethane reaction in a state where the CNF is sufficiently dispersed. When a polyol containing the diol compound contained in the CNF composition is reacted with a polyisocyanate to produce polyurethane, the resulting polyurethane contains the CNFs dispersed in the CNF composition (cellulose nanofiber-containing polyurethane), and has improved strength compared to polyurethane that does not use the CNF composition. Here, the polyisocyanate is a compound having two or more isocyanate groups in the molecule, and examples of such compounds include tolylene diisocyanate and diphenylmethane diisocyanate. These may be used alone or in combination.

[0042] In addition, the CNF composition can be added to resins, rubbers, etc., to fully exert the effects of CNF, such as improving strength, and then the diol compound can be removed as necessary. If a high-temperature heating step is performed after the addition, the diol compound can be steamed depending on the temperature and time. However, the content of the diol compound can be further reduced by continuing the heating within a range that does not affect the appearance or physical properties of the resin or rubber. For example, after heating at 105°C for 15 hours, the content of the diol compound remaining in the CNF composition (dispersant residual rate) is preferably 50% or less, more preferably 30% or less, and most preferably 10% or less.

[0043] The heating temperature and time when the diol compound is heated to evaporate and remove it can be adjusted appropriately depending on the diol compound. Although it depends on the diol compound, it is preferably 50°C or higher, and 60°C or higher makes it easier to evaporate with many diol compounds. On the other hand, if the temperature is too high, there is a risk of fire, or the resin that should be left after evaporating the diol compound is more likely to be denatured. For this reason, it is preferable that the temperature is within a range in which the physical properties of the resin can be tolerated. Although it depends on the resin, it is preferably 200°C or lower, more preferably 150°C or lower, and if it is 120°C or lower, it can be used with many resins. In addition, if it is attempted to evaporate and remove it in a short time, a high temperature is required, which makes it easier to denature the resin, so it is preferable to take 1 hour or more, and more preferably 5 hours or more. On the other hand, heating for too long is disadvantageous in terms of work efficiency and also makes it easier to denature the resin, so it is preferable to take 48 hours or less, and more preferably 24 hours or less.

[0044] The redispersion of the CNF composition preferably has a viscosity restored to 50% or more of the original viscosity, more preferably 80% or more, and most preferably 100% of the original viscosity, when compared to the original aqueous suspension of CNF. This restoration rate is called the viscosity restoration rate. When the viscosity of the redispersion is restored to 50% or more, the CNF is suitably dispersed without agglomeration.

[0045] For dispersion to obtain a redispersed product, a general stirring device such as a rotary homogenizer, homomixer, or homodisper can be used, and a sufficiently dispersed state can be achieved without using a high-load stirring device such as a high-pressure homogenizer. EXAMPLES

[0046] The following describes specific examples of the present invention. First, we will explain the manufacturing procedure of xanthate-modified CNF, which is a chemically modified CNF obtained by defibrating chemically modified cellulose. The following materials were used. Kraft pulp (manufactured by Nippon Paper Industries Co., Ltd.: NBKP, α-cellulose content: 90% by mass, average degree of polymerization of α-cellulose: 1000) Hereinafter referred to as "NBKP".

[0047] <Alkaline treatment> NBKP was weighed out so that the pulp solids (pulp solids are the amount excluding the water content in the pulp; the same applies below) was 100 g. This was placed in a 3 L beaker, and 2500 g of an 8.5 mass% aqueous sodium hydroxide solution was added, and the mixture was stirred at room temperature for 3 hours to perform an alkali treatment. The pulp after this alkali treatment was subjected to solid-liquid separation using a centrifugal dehydrator (Kokusan Co., Ltd., H-110A, filter cloth 400 mesh) to obtain a dehydrated alkali cellulose. The sodium hydroxide content of this dehydrated alkali cellulose was 7.5 mass%, and the pulp solids content was 27.4 mass%.

[0048] <Xanthate treatment> The dehydrated alkali cellulose prepared above was weighed to a pulp solid content of 100 g and placed in an eggplant-shaped flask. 35 g of carbon disulfide (35% by mass relative to the pulp solid content) was added to the eggplant-shaped flask, and the sulfurization reaction was carried out at room temperature for 4.5 hours to perform a xanthate treatment, thereby obtaining xanthated cellulose.

[0049] <Xanthate Substitution Degree Measurement> The average degree of xanthate substitution of the xanthated cellulose was measured by the Bredee method and found to be 0.312. The degree of xanthate substitution is a value relative to the degree of introduction of xanthate groups per glucose unit of cellulose. The procedure of the Bredee method was as follows. 1.5 g of xanthated cellulose was weighed into a 100 mL beaker, and 40 mL of saturated ammonium chloride aqueous solution (5 ° C.) was added. The sample was mixed well while crushing it with a glass rod, and after leaving it for 15 minutes, it was filtered with GFP filter paper (GS-25 manufactured by ADVANTEC Co., Ltd.) and thoroughly washed with saturated ammonium chloride aqueous solution. The sample was placed in a 500 mL tall beaker together with the GFP filter paper, and 50 mL of 0.5 M sodium hydroxide aqueous solution (5 ° C.) was added and stirred. After leaving it for 15 minutes, it was neutralized with 1.5 M acetic acid aqueous solution. Phenolphthalein indicator was used as the indicator. After neutralization, 250 mL of distilled water was added and stirred well, and 10 mL of 1.5 M acetic acid aqueous solution and 10 mL of 0.05 mol / L iodine aqueous solution were added by a volumetric pipette. This solution was titrated with 0.05 mol / L sodium thiosulfate aqueous solution. A 1% starch aqueous solution indicator was used as the indicator. The degree of xanthate substitution was calculated from the titration amount of sodium thiosulfate aqueous solution and the cellulose content in the sample using the following formula (1). The cellulose content in the xanthated cellulose was determined by adding water to the xanthated cellulose to disperse it, adding hydrochloric acid to perform a regeneration treatment, filtering the cellulose after the regeneration treatment, thoroughly washing it, and then drying it to measure the mass of only the cellulose.

[0050] Degree of xanthate substitution = (0.05 × 10 × 2 - 0.05 × sodium thiosulfate titration (mL)) ÷ 1000 ÷ (cellulose content in sample (g) / 162.1) ... (1)

[0051] <Defibrillation processing> The xanthated cellulose produced by the above xanthation treatment was weighed into a 5 L beaker with a handle so that the pulp solid content was 100 g, and distilled water was added and dispersed so that the pulp solid content concentration was 5% by mass. While centrifuging using the centrifuge, distilled water was added and thoroughly washed to remove impurities, alkali, unreacted carbon disulfide, etc. All of the washed xanthated cellulose was recovered, and distilled water was added to obtain 20 kg of an aqueous suspension having a cellulose concentration (hereinafter referred to as "cellulose concentration") of 0.5% by mass contained in the xanthated cellulose. This aqueous suspension was passed through a high-pressure homogenizer (manufactured by Sanwa Engineering Co., Ltd., model H20) five times at a flow rate of 2.5 L / min and a pressure of 40 MPa for fibrillation treatment to obtain xanthated CNF.

[0052] <Degree of fibrillation of CNF> Distilled water was added to the aqueous suspension of the xanthated CNF (cellulose concentration: 0.5% by mass) to dilute the cellulose concentration to 0.1% by mass. This diluted aqueous suspension was centrifuged at 12,000 G for 10 minutes using a centrifuge (manufactured by Beckman Coulter, Avanti J-25I) to precipitate unfibrillated matter. The supernatant was separated and transferred to an Erlenmeyer flask, and distilled water was added to the precipitated unfibrillated matter and centrifuged again to wash the unfibrillated matter. The unfibrillated matter was transferred to a crucible and dried to constant weight, and the mass of the unfibrillated matter was measured. The production rate of nanofibers generated from the following formula (2) based on the mass of the unfibrillated matter and the cellulose content in the xanthated cellulose was determined to be 99.0% by mass.

[0053] Production rate of nanofibers (% by mass) = (Cellulose content in xanthated cellulose - Mass of unfibrillated matter) ÷ (Cellulose content in xanthated cellulose) × 100......(2)

[0054] <Measurement of fiber diameter of CNF> The aqueous suspension of xanthated CNF diluted to a cellulose concentration of 0.1% by mass with water was placed in a centrifuge tube and centrifuged at 12,000 G for 10 minutes using the centrifuge, and the centrifuged supernatant was recovered. This centrifuged supernatant was further diluted and then stained, and dried on a support film to obtain a dried specimen. Trans A transmission electron microscope (TEM: manufactured by JEOL Ltd., JEM-1400) was used for observation at an acceleration voltage of 120 kV. Fifty nanofibers were selected from the 50,000-fold magnified image for observation, and the fiber diameters were measured. The average value was obtained, and the fiber diameters were found to be from 3.0 nm to 7.4 nm, with a number-average fiber diameter of 6.1 nm.

[0055] <Regeneration treatment and redispersion treatment> To 16.4 kg of the aqueous suspension of zanthated CNF (cellulose concentration 0.5% by mass) obtained by the above procedure, 360 ml of 1 M sulfuric acid aqueous solution (sulfuric acid amount 4.4 mmol / g-cellulose content) was added, and the mixture was stirred with an agitator for 1 hour for regeneration treatment. After the treatment, it was neutralized to pH 7 with 1 M sodium hydroxide aqueous solution to obtain a regenerated CNF aqueous suspension. When the average degree of zanthate substitution was measured, it was less than 0.001, which is the lower limit of measurement. Thus, it was confirmed that the zanthate groups were almost completely detached and returned to hydroxyl groups by the acid treatment.

[0056] The aqueous suspension of the regenerated CNF obtained above was centrifuged using the centrifuge while adding distilled water for sufficient washing. All of the washed regenerated CNF was collected, and distilled water was added to obtain 8 kg of an aqueous suspension with a CNF concentration of 1.0% by mass. This aqueous suspension was passed through the high-pressure homogenizer three times at a flow rate of 2.5 L / min and a pressure of 40 MPa for redispersion treatment. After the treatment, when the average fiber diameter of the redispersion of the regenerated CNF was calculated, the fiber diameters were from 3.0 nm to 7.4 nm, and the number-average fiber diameter was 6.0 nm.

[0057] <Manufacturing procedure of CNF composition> Next, the manufacturing of the CNF composition will be described. As the diol compound, the following diols or diol derivatives were used. · Diethylene glycol (diol: manufactured by Nacalai Tesque, Inc.: diethylene glycol) · Triethylene glycol (diol: manufactured by Nacalai Tesque, Inc.: triethylene glycol) · Dipropylene glycol (diol: manufactured by Nacalai Tesque, Inc.: dipropylene glycol) Tripropylene glycol (Diol: Nacalai Tesque, Inc.: Tripropylene glycol) 1,3-Butylene glycol (diol: Kanto Chemical Co., Ltd.: 1,3-butanediol) ) 1,4-Butylene glycol (diol: Kanto Chemical Co., Ltd.: 1,4-butanediol) ) 1,6-Hexylene glycol (diol: Tokyo Chemical Industry Co., Ltd.: 1,6-hexanediol) Dipropylene glycol monopropyl ether (Diol derivative: Fujifilm Wako Pure Chemical Industries, Ltd.: Dipropylene glycol monopropyl ether) Diethylene glycol ethyl ether acetate (diol derivative: Tokyo Chemical Industry Co., Ltd.: diethylene glycol monoethyl ether acetate) Glycerin (polyol other than diol: Nacalai Tesque, Inc.: glycerin) Diglycerol (Polyol other than diol: Nacalai Tesque, Inc.: Diglycerol)

[0058] (Examples 1 to 7) To the regenerated CNF aqueous suspension, each of the diol compounds shown in Table 1 was added in an amount 10 times the amount of the regenerated CNF. 30 g of a mixture with a CNF concentration of 0.7 mass% and a diol compound concentration of 7.0 mass% was dried for the specified time shown in Table 1 using a hot air dryer at 60°C to obtain a CNF composition. A photograph of the CNF composition of Example 1 is shown in Figure 1.

[0059] <Calculation method for residual dispersant rate> In each example, about 0.2 to 0.4 g of a sample of the CNF composition was taken, 6 ml of methanol was added, and a dispersion treatment was performed for 5 minutes at 8000 rpm using a rotary homogenizer (AM-7, manufactured by Nippon Seiki Seisakusho Co., Ltd.). After the dispersion treatment, methanol was further added to make a total of 25 ml, and the content of the diol compound, which is a dispersant, was measured by gas chromatography analysis. The dispersant residual rate was calculated from the content of the dispersant relative to the total mass of the CNF composition. In addition, the mass of the dispersant and CNF was subtracted from the total mass of the CNF composition to calculate the amount of remaining moisture, and the moisture content after drying relative to the entire CNF composition was calculated. The results are shown in Tables 1 to 3. The gas chromatography analysis conditions were as follows: GC-17A manufactured by Shimadzu Corporation was used as the apparatus, and HP-WAX 25 m (inner diameter 0.32 μm) manufactured by Agilent was used as the column. The temperature conditions were 250 ° C for injection and 250 ° C for detector. The detector used was an FID, and the column heating conditions were t = 0 (40°C), t = 0.5 (40°C), t = 20.5 (240°C), and t = 24.5 (240°C).

[0060] <How to calculate viscosity recovery rate> Water was added to each of the CNF compositions so that the amount was the same as before drying, and the mixture was dispersed using the rotary homogenizer at 8000 rpm for 15 minutes to obtain a redispersion with a CNF concentration of 0.7% by mass. The redispersion was measured at 20°C, a rotation speed of 1 rpm (shear rate = 3.8 s) using an E-type viscometer manufactured by Toki Sangyo Co., Ltd. -1 ) and the viscosity was measured and compared with that of the original CNF aqueous suspension to determine the viscosity restoration rate. For example, the viscosity of the original CNF aqueous suspension in Example 1 was 448 mPa s, whereas the viscosity of the redispersion was exactly the same 448 mPa s, and the viscosity restoration rate was calculated to be 100%. Similarly, the results obtained in the other Examples, Reference Examples, and Comparative Examples are shown in Tables 1 to 4.

[0061] [Table 1]

[0062] In the CNF compositions dried at 60°C in Examples 1 to 9, 80% or more of the diol compound serving as a dispersant remained, and the viscosity recovery rates of the redispersions all showed high values.

[0063] (Reference examples 1~7) Mixtures with a CNF concentration of 0.7% by mass and a diol compound concentration of 7.0% by mass were prepared in the same manner as in Examples 1 to 7, and these mixtures were heated at 105°C for 15 hours. These mixtures are referred to as Reference Examples 1 to 7, and the dispersant residual rate and viscosity recovery rate are shown in Table 2. In Reference Example 1, the residual rate of the diol compound (dispersant) was only about 30%, but in the other Reference Examples, the diol compound was almost completely evaporated. This confirmed that these dispersants could be easily removed by heating after the CNF composition was used.

[0064] [Table 2]

[0065] (Consideration) From the above results, it was confirmed that for CNF compositions showing a preferable viscosity recovery rate of 50% or more, it is desirable that 50% or more of the diol compound acting as a dispersant remains. If no dispersant remains, the viscosity recovery rate was extremely low or redispersion was impossible in all cases.

[0066] (Comparative Examples 1 and 2) The results of Comparative Examples 1 and 2, in which glycerin, which has 3 hydroxyl groups in the molecule, and diglycerol, which has 4 hydroxyl groups, were used as dispersants, are shown in Table 3. These showed favorable values ​​in terms of dispersant residual rate and viscosity recovery rate when dried at 60°C, but even after heating at 105°C for 15 hours, a large amount of dispersant remained, and it was confirmed that the dispersant was difficult to remove.

[0067] [Table 3]

[0068] <Study on the effect of diol addition ratio> (Examples 8a to 8d) Water suspensions (30 g each) were prepared such that the CNF concentration was 0.7% by mass, and the content of triethylene glycol as the diol compound was 7.0% by mass (Example 8a), 3.5% by mass (Example 8b), 1.4% by mass (Example 8c), and 0.7% by mass (Example 8d), respectively, and the viscosities were measured. Next, each water suspension was dried at 60°C using a hot air dryer until the water content became 10% by mass or less. After drying, water was added to adjust the total mass to 30 g each, and the mixtures were mixed at 8000 rpm for 15 minutes using the rotary homogenizer to obtain redispersions. The viscosities of the respective redispersions were measured, and the viscosity recovery rates were calculated. The results are shown in Table 4.

[0069]

Table 4

[0070] From the above results, it was confirmed that when the addition amount of the diol compound was 2 times or more with respect to CNF, the viscosity recovery rate showed good results of 50% or more.

[0071] <Resin kneading of CNF composition> (Experimental Example 1) A water suspension (32 g) containing 0.5% by mass of recycled CNF and 5.0% by mass of dipropylene glycol (DPG) as the diol compound was prepared. This water suspension was dried at 60°C for 12 hours using a hot air dryer to obtain a CNF composition with a dried weight of 1.83 g.

[0072] 1.83 g of this CNF composition and 15 g of polypropylene resin (Wintech WFX4M manufactured by Nippon Polypropylene Co., Ltd.) were kneaded at 180°C for 5 minutes using a tabletop small kneader (DSM Xplore MC15M manufactured by Xplore Instruments) to obtain a kneaded resin. The DPG content before kneading was 9.5% by mass.

[0073] A portion (112.6 mg) was taken from the kneaded resin, immersed in 1.5 mL of toluene, allowed to stand at 80 °C for 2 hours to dissolve the polypropylene resin. This solution was dropped into a vial containing 5 mL of methanol to dissolve DPG in methanol, and then further methanol was added to make up to 10 mL. Next, this methanol solution was subjected to gas chromatographic analysis to quantify the dissolved DPG. The analysis conditions of the gas chromatograph were the same as those in the above-mentioned "method for calculating the dispersant residual rate". As a result, the content of DPG contained in the kneaded resin was 1.3% by mass, which was sufficiently reduced from 9.5% by mass before kneading. Thus, it was confirmed that when the CNF composition was introduced into the heat-melted resin, the amount of the diol compound used for maintaining the dispersibility of CNF evaporated during kneading and the amount remaining in the resin was small.

[0074] <Rubber Kneading of CNF Composition> (Experimental Example 2) 300 g of a masterbatch prepared by drying natural rubber latex (manufactured by Revertex Co., Ltd., HA NR LATEX, solid content 60% by mass, ammonia 0.7% by mass) was kneaded using a two-roll mill heated to 50 °C (manufactured by Nippon Roll Manufacturing Co., Ltd., φ200 mm × L500 mm mixing roll machine). Then, 1.5 g of stearic acid (manufactured by Nacalai Tesque, Inc.) and 18 g of zinc oxide (manufactured by Nacalai Tesque, Inc.) were added and kneaded to obtain a kneaded product. Next, 90.32 g of a CNF composition (15.0 g of CNF, 75.0 g of diethylene glycol ethyl ether acetate, 0.32 g of moisture) prepared by mixing and drying diethylene glycol ethyl ether acetate as a diol compound and recycled CNF was added to the above kneaded product and further kneaded. Thereafter, 10.5 g of sulfur (manufactured by Nacalai Tesque, Inc.) and 2.1 g of a vulcanization accelerator (Sunceler NS-G manufactured by Sanshin Chemical Industry Co., Ltd.) were added and mixed to produce a compound sheet with a thickness of 2 mm or more.

[0075] Using the obtained compound sheet, the 90% vulcanization time (Tc90) was measured with a vulcanization determination machine (manufactured by Orientech Co., Ltd., Curemeter V type, measurement temperature 150 °C, measurement time 20 minutes). At this time, Tc90 was 6 minutes. This compound sheet was placed in a mold, Based on the measured value of Tc90, a vulcanized rubber sheet with a thickness of 2 mm was obtained by compression molding at 150 °C for 6 minutes. As described above, it was confirmed that a rubber sheet can be produced by adding the CNF composition to the rubber.

[0076] From the obtained rubber sheet, dumbbell-shaped No. 3 test pieces specified in JIS K 6251 were punched out. For this test piece, a tensile test (grip width: 50 mm, speed: 500 mm / min, conforming to JIS K6251) was performed using a tensile testing machine (Shimadzu Corporation Precision Universal Testing Machine AG-1000D). Also, among the above procedures, a rubber sheet prepared by the same procedure except that only diethylene glycol ethyl ether acetate not containing recycled CNF was added instead of the CNF composition was used as a blank.

[0077] The results of the tensile tests of this test piece and the blank are shown in Figure 2 and Table 5. As a result, compared with the blank, the rubber sheet added with recycled CNF had a 68.8% improvement in stress (M30%) at an elongation (= strain) of 30%, a 46.2% improvement at an elongation of 100% (M100%), and a 26.8% improvement at an elongation of 300% (M300%). From this, it was confirmed that the strength of the rubber sheet was improved by the dispersed recycled CNF.

[0078]

Table 5

[0079] <Synthesis of Polyurethane with CNF Composition> (Experimental Example 3) 1,4-butylene glycol was used as a diol compound, and was added in an amount 10 times that of the regenerated CNF to prepare a regenerated CNF aqueous suspension with a CNF concentration of 0.8% by mass and a diol concentration of 8.0% by mass. 200 g of this regenerated CNF aqueous suspension was dried at 60°C for 18 hours using a hot air dryer to obtain a CNF composition (regenerated CNF: 9.3% by mass, 1,4-butylene glycol: 86.8% by mass, water content: 4.0%).

[0080] To 10.8 g of this CNF composition, 89.2 g of polytetramethylene glycol (PTMG), a polyol used as a raw material for the urethane reaction, was added, and the mixture was dispersed for 10 minutes at 10,000 rpm using a rotary homogenizer (AM-7) to obtain a regenerated CNF polyol dispersion (regenerated CNF: 1.0 mass%, 1,4-butylene glycol: 9.4 mass%, PTMG: 89.1 mass%, water content 0.5%).

[0081] 45 ml of dimethylformamide (DMF) was added to 5.0 g of the regenerated CNF polyol dispersion, and the above-mentioned rotary homogenizer was used to perform dispersion treatment at 3000 rpm for 5 minutes to obtain a DMF dispersion. Then, this DMF dispersion was placed in a centrifuge tube, and centrifuged at 1100 G for 10 minutes using the above-mentioned centrifuge. After removing the supernatant from the centrifuged product, 50 ml of DMF was added to the sediment and centrifuged again. After removing the supernatant from the centrifuged product again, a solvent was added to the sediment and centrifuged again using acetone as a solvent, followed by distilled water as a solvent to wash the precipitated residue. This residue was treated as an undispersed matter in the regenerated CNF polyol dispersion, and the weight was measured after drying for 8 hours at 105 ° C. using a hot air dryer, and the regeneration of the entire regenerated CNF polyol dispersion was confirmed. The ratio of undispersed CNF to the amount of virgin CNF was calculated, which was 11%, confirming that 89% of the regenerated CNF was uniformly dispersed in the regenerated CNF polyol dispersion.

[0082] 0.5 g of 1,4-butylene glycol was added to 96.3 g of the above-mentioned recycled CNF polyol dispersion so that the mass ratio of PTMG to 1,4-butylene glycol was 9:1, and the mixture was stirred for 30 minutes at 80° C. using a three-one motor. 57.2 g of diphenylmethane diisocyanate was added to this mixture and stirred for 5 minutes, then transferred to a preheated stainless steel tray and reacted for 24 hours at 110° C. using a hot air dryer to obtain 136 g of synthetic polyurethane with recycled CNF dispersed therein.

[0083] The obtained synthetic polyurethane was melted at 220°C for 10 minutes using a tabletop test press SA-302 manufactured by Tester Sangyo Co., Ltd., and then processed into a film having a thickness of 300 μm by applying a pressure of 7 MPa and hot pressing for 5 minutes. A tensile test was performed on a test piece punched out from this film into a dumbbell shape No. 8 as specified in JIS K 7311, with a measurement length of 25 mm and a tensile speed of 100 mm / min. On the other hand, a blank film without the addition of recycled CNF was made from polyurethane synthesized with the same amounts of PTMG and 1,4-butylene glycol, but without using the recycled CNF aqueous dispersion.

[0084] The results of the tensile tests of this test piece and the blank are shown in Figure 3 and Table 6. Compared to the blank, the polyurethane with added recycled CNF had a 9.7% increase in stress at 100% elongation (strain) (M100%). Also, the stress at 200% elongation (strain) (M200%) increased by 9.8%. This confirmed that the strength of the synthetic polyurethane was improved by the dispersed recycled CNF.

[0085] [Table 6]

Claims

1. A regenerated cellulose nanofiber composition is obtained by adding a diol, a diol derivative, or a diol compound consisting of both as a dispersant to a regenerated cellulose nanofiber aqueous suspension containing regenerated cellulose nanofibers having a number average fiber diameter of 3 nm to 20 nm, and then evaporating a portion of the water to obtain a regenerated cellulose nanofiber composition; A method for producing a regenerated cellulose nanofiber composition, wherein the regenerated cellulose nanofiber has a viscosity recovery rate of 50% or more when redispersed compared to the original aqueous suspension of the cellulose nanofiber.

2. A method for producing regenerated cellulose nanofibers as described in claim 1, wherein the regenerated cellulose nanofibers are obtained by regenerating xanthated cellulose nanofibers to a degree of xanthate substitution of less than 0.

001.

3. A method for producing a molded resin or rubber containing regenerated cellulose nanofibers, comprising mixing a regenerated cellulose nanofiber composition containing a diol compound consisting of a diol, a diol derivative, or both, water, and regenerated cellulose nanofibers having a number average fiber diameter of 3 nm or more and 20 nm or less, the regenerated cellulose nanofiber composition having a viscosity recovery rate of 50% or more when redispersed compared to the original aqueous suspension of cellulose nanofibers, with molten resin or kneaded rubber.

4. A method for producing a resin or rubber molded article, comprising heating the resin or rubber molded article produced by the method according to claim 3 to remove a part or all of the diol compound.

5. A method for producing a polyurethane containing regenerated cellulose nanofibers, the method comprising: mixing a regenerated cellulose nanofiber composition containing a diol compound consisting of a diol, a diol derivative, or both, water, and regenerated cellulose nanofibers having a number average fiber diameter of 3 nm or more and 20 nm or less, the regenerated cellulose nanofiber composition having a viscosity recovery rate of 50% or more when redispersed compared to the original aqueous suspension of cellulose nanofibers, with a polyol; dispersing the regenerated cellulose nanofibers in the polyol; and reacting the polyol containing the diol compound contained in the regenerated cellulose nanofiber composition with a polyisocyanate to produce a polyurethane.

6. A polyol is reacted with an excess of polyisocyanate to obtain a urethane prepolymer, The urethane prepolymer; A regenerated cellulose nanofiber composition containing a diol compound consisting of a diol, a diol derivative, or both, water, and regenerated cellulose nanofibers having a number average fiber diameter of 3 nm to 20 nm, the regenerated cellulose nanofiber composition having a viscosity recovery rate of 50% or more when redispersed compared to the original aqueous suspension of the cellulose nanofibers; Mix the following: A method for producing polyurethane containing regenerated cellulose nanofibers, comprising reacting an isocyanate group in the urethane prepolymer with the diol compound contained in the regenerated cellulose nanofiber composition to produce polyurethane by chain-extending the urethane prepolymer.

Citation Information

Patent Citations

  • Moisture-curable urethane composition, covering material, and civil engineering construction structure

    JP2015067664A

  • Gel-like sheet composition and method for producing the same

    JP2018002668A

  • Acetylated pulp composition containing ethylene glycol derivative, resin composition containing microfibrillated acetylated pulp, and method for producing the same

    JP2018115292A

  • Redispersible microfibrillated cellulose

    JP1984189141A

  • Manufacture of semiconductor device

    JP1987076740A