Ionomer, resin sheet and glass laminate

The ionomer composition addresses the balance of transparency, elastic modulus, and odor issues in laminated glass interlayer films by using specific monomer contents and processing methods, resulting in improved performance and safety.

JP2024133195AActive Publication Date: 2024-10-01KURARAY EURO GMBH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024111651
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-05-31
Filing Date
2024-07-11
Publication Date
2024-10-01
Estimated Expiration
2040-05-22

AI Technical Summary

Technical Problem

Existing ionomers used in interlayer films for laminated glass lack a balanced combination of high transparency, high elastic modulus, low coloration, and reduced odor during molding, with some exhibiting strong odors that pose health risks to workers.

Method used

An ionomer composition comprising 0.05 to 1.0 mol% of (meth)acrylic acid ester units, 4.5 to 9.0 mol% of carboxylic acid units, and 0.65 to 3.0 mol% of carboxylic acid neutralized units, with specific monomer contents and processing methods to achieve transparency, high elastic modulus, and reduced odor.

Benefits of technology

The ionomer achieves excellent transparency, high elastic modulus, and low coloration while minimizing odor during molding, enhancing the performance and safety of laminated glass applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133195000001
    Figure 2024133195000001
  • Figure 2024133195000002
    Figure 2024133195000002
  • Figure 2024133195000003
    Figure 2024133195000003
Patent Text Reader

Abstract

To provide an ionomer which is excellent in transparency, maintains high elastic modulus at high temperature, is reduced in coloration, and is reduced in odor in molding.SOLUTION: An ionomer contains, based on the total monomer unit constituting a resin, 0.05 to 1.0 mol% of a (meth)acrylate unit, 4.5 to 9.0 mol% of a carboxylic acid unit, 0.65 to 3.0 mol% of a carboxylic acid neutralized compound unit, and an ethylene unit, and has a total content of the (meth)acrylate unit, the carboxylic acid unit and the carboxylic acid neutralized compound unit of 7.0 to 10 mol%.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an ionomer, and more particularly to an ionomer having excellent physical and optical properties, a resin sheet using the ionomer, and laminated glass using the resin sheet as an interlayer. [Background technology]

[0002] Ionomers, which are neutralized ethylene-unsaturated carboxylic acid copolymers, are used as interlayer films in laminated glass because of their excellent transparency and adhesion to glass (for example, Patent Document 1). In recent years, the performance requirements for laminated glass have increased, and ionomers are also required to maintain high transparency regardless of the manufacturing conditions of the laminated glass, maintain a high elastic modulus even at high temperatures and not reduce the strength of the laminated glass, and furthermore, to have less coloring and a good appearance.

[0003] For example, Patent Document 2 describes an ionomer in which 5 to 15 mass % of an α,β-unsaturated carboxylic acid derivative is introduced as a third component into an ethylene-unsaturated carboxylic acid copolymer, and this ionomer exhibits improved optical properties.

[0004] However, the ionomer of Patent Document 2 is still insufficient in terms of the well-balanced properties of transparency, high elastic modulus, and low coloration required for an ionomer for an interlayer film of laminated glass.In addition, the ionomer of Patent Document 2 generates a strong odor derived from the third component during molding, which causes a new problem in that the burden on workers is high. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] U.S. Patent No. 6,432,522 [Patent Document 2] Special Publication No. 2017-519083 Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made to solve the above-mentioned problems in the conventional art, and an object of the present invention is to provide an ionomer which has excellent transparency, maintains a high elastic modulus at high temperatures, is less discolored, and has a reduced odor during molding processing. [Means for solving the problem]

[0007] The present invention provides an ionomer which contains 0.05 to 1.0 mol % of (meth)acrylic acid ester units, 4.5 to 9.0 mol % of carboxylic acid units, 0.65 to 3.0 mol % of carboxylic acid neutralization product units, and ethylene units, based on all monomer units constituting the resin, and the total content of the (meth)acrylic acid ester units, carboxylic acid units, and carboxylic acid neutralization product units is 7.0 to 10 mol %.

[0008] In one embodiment, the ionomer has an MFR of 0.7 g / 10 min or more, measured under conditions of a measurement temperature of 190° C. and a load of 2.16 Kgf.

[0009] In one embodiment, the (meth)acrylic acid ester unit is at least one selected from the group consisting of methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, and isobutyl (meth)acrylate.

[0010] In one embodiment, the ionomer contains 6.5 to 10 mol % of (meth)acrylic acid ester units, It has a MFR of 90 to 400 g / 10 min, measured at a temperature of 190°C and a load of 2.16 kgf. It uses ethylene-(meth)acrylic acid ester copolymer as the raw material.

[0011] In one embodiment, the ionomer is A storage modulus of 30 MPa or more measured using a 0.8 mm thick resin sheet specimen at a measurement temperature of 50°C and a frequency of 1 Hz. A yellow index (YI) of 2.0 or less, measured using a resin sheet specimen having a thickness of 0.8 mm; and A haze of 5.0% or less measured using a laminated glass in which a 0.8 mm thick resin sheet test piece was placed between two glass plates, heated to 140°C, and then cooled slowly to 23°C at a rate of 0.1°C / min. It has the following.

[0012] The present invention also provides a resin composition containing any one of the above ionomers in an amount of 93 mass % or more.

[0013] The present invention also provides a resin sheet consisting essentially of any one of the above ionomers or the above resin composition.

[0014] The present invention also provides a laminated glass comprising two glass plates and the above-mentioned resin sheet as an interlayer disposed between the two glass plates. Effect of the Invention

[0015] According to the present invention, it is possible to provide an ionomer which has a good balance of transparency, high elastic modulus, and low coloration, and further has reduced odor during molding processing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] <Configuration> The ionomer of the present invention is a resin containing ethylene units, (meth)acrylic acid ester units (A), carboxylic acid units (B) and carboxylic acid neutralization product units (C). In one embodiment, the ionomer of the present invention is a resin composed of structural units (A), (B) and (C) and ethylene units.

[0017] Examples of monomers constituting the (meth)acrylic acid ester unit (A) include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, t-butyl (meth)acrylate, amyl (meth)acrylate, isoamyl (meth)acrylate, n-hexyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, pentadecyl (meth)acrylate, dodecyl (meth)acrylate, isobornyl (meth)acrylate, phenyl (meth)acrylate, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, glycidyl (meth)acrylate, and allyl (meth)acrylate. Among these, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, and t-butyl (meth)acrylate are preferred, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, and isobutyl (meth)acrylate are more preferred, methyl (meth)acrylate, n-butyl (meth)acrylate, and isobutyl (meth)acrylate are even more preferred, and methyl (meth)acrylate is the most preferred. Of the methacrylic acid esters and acrylic acid esters, the methacrylic acid esters are preferred because they are excellent in thermal decomposition resistance and low coloring. These (meth)acrylic acid esters can be used alone or in combination of two or more.

[0018] The content of the (meth)acrylic acid ester unit (A) in the ionomer is 0.05 mol% or more and 1.0 mol% or less. The content of (A) in this range increases transparency and reduces odor during molding. The preferred lower limit of the content is preferably 0.07 mol% or more, more preferably 0.08 mol% or more, and even more preferably 0.09 mol% or more. The preferred upper limit of the content is preferably 0.9 mol% or less, more preferably 0.8 mol% or less, and even more preferably 0.6 mol% or less.

[0019] Examples of monomers constituting the carboxylic acid unit (B) include acrylic acid, methacrylic acid, itaconic acid, maleic anhydride, monomethyl maleate, monoethyl maleate, etc. Among these, acrylic acid, methacrylic acid, monomethyl maleate, and monoethyl maleate are more preferred, acrylic acid and methacrylic acid are even more preferred, and methacrylic acid is the most preferred. These carboxylic acid units can be used alone or in combination of two or more.

[0020] The content of the carboxylic acid unit (B) in the ionomer is 4.5 mol% or more and 9.0 mol% or less. When the content of (B) is within this range, it is possible to achieve both adhesion to glass and transparency. If the content is too low, the transparency decreases and the adhesion to glass also decreases. If the content is too high, the moldability decreases and coloring tends to occur. The preferred lower limit of the content is 5.0 mol% or more, more preferably 5.5 mol% or more, and even more preferably 5.8 mol% or more. The preferred upper limit of the content is 8.5 mol% or less, more preferably 8.0 mol% or less, and even more preferably 7.5 mol% or less.

[0021] The carboxylic acid neutralization unit (C) is preferably a neutralization unit of the carboxylic acid unit (B). The carboxylic acid neutralization product is a product in which the hydrogen ion of the carboxylic acid is replaced with a metal ion. Examples of the metal ion include ions of monovalent metals such as lithium, sodium, and potassium, and ions of polyvalent metals such as magnesium, calcium, zinc, aluminum, and titanium. Such metal ions do not need to be of one type, and two or more types can be used in combination. For example, one or more types of monovalent metal ions and one or more types of divalent metal ions may be used in combination.

[0022] The content of the carboxylic acid neutralization unit (C) in the ionomer is 0.65 mol% or more and 3.0 mol% or less. By having the content of (C) in this range, both transparency and molding processability can be achieved. If the content is too high, the melt viscosity during molding processing increases and coloring tends to occur. If the content is too low, the transparency decreases and the elastic modulus at 50°C decreases. The preferred lower limit of the content is 1.0 mol% or more, more preferably 1.5 mol% or more, and even more preferably 1.7 mol% or more. The preferred upper limit of the content is 2.7 mol% or less, more preferably 2.6 mol% or less, and even more preferably 2.5 mol% or less.

[0023] The ionomer of the present invention has a total content of (meth)acrylic acid ester units (A), carboxylic acid units (B) and carboxylic acid neutralization units (C) of 7.0 mol% or more and 10 mol% or less. When the total content of (A), (B) and (C) is within this range, the ionomer can have both high transparency and high elastic modulus at 50°C. The lower limit of the content is more preferably 7.5 mol% or more, even more preferably 8.0 mol% or more, and most preferably 8.5 mol% or more. The upper limit of the content is more preferably 9.9 mol% or less, and even more preferably 9.5 mol% or less.

[0024] <Manufacturing method> The method for producing the ionomer of the present invention includes a method in which ethylene and a (meth)acrylic acid ester are copolymerized at high temperature and high pressure to obtain an ethylene-(meth)acrylic acid ester copolymer (X), and then a part of the (meth)acrylic acid ester units are converted to (meth)acrylic acid units and neutralized (meth)acrylic acid units. A method for converting a part of the (meth)acrylic acid ester units to (meth)acrylic acid units and neutralized (meth)acrylic acid units includes, for example, a method in which a saponification reaction is carried out using sodium hydroxide to synthesize an ethylene-(meth)acrylic acid ester-neutralized (meth)acrylic acid copolymer, and then a part of the neutralized (meth)acrylic acid units are converted to (meth)acrylic acid using an acid.

[0025] The (meth)acrylic acid esters used as raw materials in the above-mentioned manufacturing method can be the above-mentioned (meth)acrylic acid esters. Among them, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate are preferred, and methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, and isobutyl (meth)acrylate are more preferred. Comparing methacrylic acid esters and acrylic acid esters, methacrylic acid esters are preferred because the resulting ionomer has excellent thermal decomposition resistance and low coloring properties. These (meth)acrylic acid esters can be used alone or in combination of two or more.

[0026] Specific examples of the ethylene-(meth)acrylic acid ester copolymer (X) include ethylene-methyl acrylate copolymer, ethylene-methyl methacrylate copolymer, ethylene-ethyl acrylate copolymer, ethylene-ethyl methacrylate copolymer, ethylene-n-propyl acrylate copolymer, ethylene-n-propyl methacrylate copolymer, ethylene-isopropyl acrylate copolymer, ethylene-isopropyl methacrylate copolymer, ethylene-n-butyl acrylate copolymer, ethylene-n-butyl methacrylate copolymer, ethylene-sec-butyl acrylate copolymer, ethylene-sec-butyl methacrylate copolymer, etc. These copolymers may be commercially available or may be synthesized with reference to US2013 / 0274424, JP2006-233059, or JP2007-84743.

[0027] The content of the (meth)acrylic acid ester unit in the ethylene-(meth)acrylic acid ester copolymer (X) is preferably 6.5 mol% or more and 10 mol% or less, more preferably 7.0 mol% or more and 9.5 mol% or less, and most preferably 7.5 mol% or more and 9.2 mol% or less. By adjusting the content to such a range, the contents of the (meth)acrylic acid ester unit, the carboxylic acid unit, and the carboxylic acid neutralization product unit of the obtained ionomer can be adjusted to an appropriate range.

[0028] The melt flow rate (MFR) of the ethylene-(meth)acrylic acid ester copolymer (X) measured under the conditions of 190°C and 2.16 kgf is preferably 90 g / 10 min or more and 400 g / 10 min or less, more preferably 100 g / 10 min or more and 350 g / 10 min or less, and most preferably 150 g / 10 min or more and 330 g / 10 min or less. By setting the MFR of the ethylene-(meth)acrylic acid ester copolymer (X) in such a range, the obtained ionomer can be made to have both moldability and strength. The MFR of the ethylene-(meth)acrylic acid ester copolymer (X) can be adjusted by the degree of polymerization and the ratio of (meth)acrylic acid ester units.

[0029] Ethylene-(meth)acrylic acid ester copolymer (X) was mixed with 1,2,4-trichlorobenzene as a solvent at a column temperature of 140°C and a column (TSKgel GMH HR From the viewpoint of achieving both the molding processability and strength of the obtained ionomer, the molecular weight in terms of polystyrene measured by three -H(20)HT in series is preferably 15,000 g / mol or more, more preferably 20,000 g / mol or more, even more preferably 25,000 g / mol or more, and particularly preferably 30,000 g / mol or more. The upper limit of the weight average molecular weight is preferably 200,000 g / mol or less, more preferably 100,000 g / mol or less, and even more preferably 50,000 g / mol or less. The lower limit of the number average molecular weight is preferably 3,000 g / mol or more, more preferably 5,000 g / mol or more, even more preferably 8,000 g / mol or more, even more preferably 10,000 g / mol or more, and particularly preferably 15,000 g / mol or more. The upper limit of the number average molecular weight is preferably 100,000 g / mol or less, more preferably 50,000 g / mol or less, and even more preferably 30,000 g / mol or less.

[0030] The branching degree per 1000 carbon atoms of the ethylene-(meth)acrylic acid ester copolymer (X) is not particularly limited, but is preferably 5 to 30, and more preferably 6 to 20. The branching degree per 1000 carbon atoms is analyzed by dissolving the ethylene-(meth)acrylic acid ester copolymer in deuterated orthodichlorobenzene, 13 This can be done using the inverse gate decoupling method of C-NMR.

[0031] As a method for converting a part of the (meth)acrylic acid ester units of the ethylene-(meth)acrylic acid ester copolymer (X) into (meth)acrylic acid units and (meth)acrylic acid neutralized product units, a part of the (meth)acrylic acid ester units of the ethylene-(meth)acrylic acid ester copolymer (X) is subjected to a saponification reaction with an alkali to convert them into (meth)acrylic acid neutralized product units, and then a part of the (meth)acrylic acid neutralized product units is demetallized with an acid to convert them into (meth)acrylic acid units, thereby producing an ionomer having ethylene units, (meth)acrylic acid ester units, carboxylic acid units and carboxylic acid neutralized product units.

[0032] As another method, a part of the (meth)acrylic acid ester units of the ethylene-(meth)acrylic acid ester copolymer (X) is saponified with an alkali to convert them into neutralized (meth)acrylic acid units, and then all of the neutralized (meth)acrylic acid units are demetallized with an acid to convert them into (meth)acrylic acid units. A part of the units is then neutralized with an alkali metal or an alkaline earth metal to produce an ionomer having ethylene units, (meth)acrylic acid ester units, carboxylic acid units and neutralized carboxylic acid units.

[0033] Examples of the solvent when a part of the (meth)acrylic acid ester units of the ethylene-(meth)acrylic acid ester copolymer (X) is saponified with an alkali include ether solvents such as tetrahydrofuran and dioxane, halides such as chloroform and dichlorobenzene, ketones having 6 or more carbon atoms such as methyl butyl ketone, hydrocarbon compounds such as n-hexane and cyclohexane, mixed solvents of hydrocarbon compounds and alcohols such as methanol, ethanol, 1-propanol, 2-propanol, and 1-butanol, aromatic compounds such as benzene, toluene, xylene, and ethylbenzene, and mixed solvents of aromatic compounds and alcohols. The ethylene-(meth)acrylic acid ester copolymer (X) suitable for the present invention preferably contains (meth)acrylic acid ester units at a specific ratio, so that it is important to select an appropriate solvent and reaction conditions in order to produce the ionomer of the present invention.

[0034] The temperature when a part of the (meth)acrylic acid ester units of the ethylene-(meth)acrylic acid ester copolymer (X) is saponified with an alkali is preferably 50° C. or higher, more preferably 60° C. or higher, even more preferably 70° C. or higher, and most preferably 80° C. or higher, from the viewpoints of reactivity and the solubility of the ethylene-(meth)acrylic acid ester copolymer (X). There is no particular upper limit, but a temperature at which the ethylene-(meth)acrylic acid ester copolymer (X) does not decompose is preferred, for example, 300° C. or lower.

[0035] A part of the (meth)acrylic acid ester units of the ethylene-(meth)acrylic acid ester copolymer (X) is saponified with an alkali to convert it into a (meth)acrylic acid neutralized product unit, and then a part of the (meth)acrylic acid neutralized product units is demetallized with an acid to convert it into a (meth)acrylic acid unit. Known organic acids such as acetic acid, hydrochloric acid, nitric acid, sulfuric acid, etc. can be used as the type of acid used for demetallization with an acid. The same solvent as that used for the saponification reaction can be selected as the solvent for demetallization with an acid.

[0036] A part of the (meth)acrylic acid ester units of the ethylene-(meth)acrylic acid ester copolymer (X) is saponified with an alkali to convert it into a (meth)acrylic acid neutralized product unit, and then all of the (meth)acrylic acid neutralized product units are demetalized with an acid to convert it into a (meth)acrylic acid unit, and then a part of the (meth)acrylic acid units are neutralized with an alkali metal or an alkaline earth metal. The neutralizing agent used in this process is not particularly limited as long as it is an ionic compound containing the above-mentioned metal ion. Examples of the metal ion include alkali metal ions such as lithium, potassium, and sodium, alkaline earth metal ions such as magnesium and calcium, transition metal ions such as zinc, nickel, iron, and titanium, and aluminum ions. For example, examples of the neutralizing agent when the metal ion is a sodium cation include sodium hydroxide, sodium acetate, and sodium hydrogen carbonate. Polymers such as ionomers containing sodium carboxylate units can also be used as neutralizing agents.

[0037] The contents of (meth)acrylic acid ester units, carboxylic acid units, and carboxylic acid neutralization product units in the ionomer of the present invention can be analyzed by the following procedure. First, the constituent units in the ionomer are identified by pyrolysis gas chromatography, and then the contents of each can be evaluated using nuclear magnetic resonance spectroscopy (NMR) and elemental analysis. IR and Raman analysis can also be combined. Prior to these analyses, it is preferable to remove components other than the ionomer by reprecipitation or Soxhlet extraction.

[0038] The melting point of the ionomer of the present invention is preferably 50° C. or more and 200° C. or less, more preferably 60° C. or more and 180° C. or less, and even more preferably 80° C. or more and 150° C. or less. The melting point can be determined by the method described in JIS K7121:2012 using differential scanning calorimetry (DSC) with a cooling rate of −10° C. / min, a heating rate of 10° C. / min, and the pick-top temperature of the melting peak in the second heating.

[0039] The heat of fusion of the ionomer of the present invention is preferably 0 J / g or more and 25 J / g or less. It can be calculated by using differential scanning calorimetry (DSC) with reference to the method described in JIS K7122:2012, with a cooling rate of -10°C / min, a heating rate of 10°C / min, and the area of ​​the melting peak during the second heating.

[0040] The melt flow rate (MFR) of the ionomer of the present invention measured under the conditions of 190 ° C. and 2.16 kgf is preferably 0.3 g / 10 min or more, more preferably 0.7 g / 10 min or more, even more preferably 1.0 g / 10 min or more, even more preferably 1.5 g / 10 min or more, and particularly preferably 2.0 g / 10 min or more. There is no particular limit to the upper limit, but it is preferably 50 g / 10 min or less, more preferably 30 g / 10 min or less, even more preferably 10 g / 10 min or less, and particularly preferably 5 g / 10 min or less. When the MFR of the ionomer is in such a range, molding processing with suppressed deterioration due to heat is possible. The MFR of the ionomer can be adjusted by the molecular weight and the amount of (meth) acrylic acid ester unit (A), carboxylic acid unit (B) and carboxylic acid neutralization product unit (C).

[0041] The molecular weight can be measured by dissolving the ionomer in a mixed solvent of acetic acid and toluene under heating, converting the carboxylic acid neutralization units to carboxylic acid units. The carboxylic acid units are then esterified to methyl carboxylate with trimethylsilyldiazomethane. The resulting copolymer can then be dissolved in orthodichlorobenzene and the molecular weight can be measured using high-temperature SEC. A calibration curve is created using polystyrene as the standard substance, and the molecular weight calculated in terms of polystyrene.

[0042] The degree of branching per 1000 carbon atoms of the ionomer of the present invention is not particularly limited, but is preferably from 5 to 30, and more preferably from 6 to 20. Analysis of the degree of branching per 1000 carbon atoms can be carried out by the DDMAS method using solid-state NMR.

[0043] The storage modulus (E') at 50°C of the ionomer of the present invention measured by dynamic viscoelasticity measurement is preferably 20 MPa or more, more preferably 30 MPa or more, even more preferably 40 MPa or more, and most preferably 50 MPa or more. There is no particular upper limit to the storage modulus (E'), but it is preferably 1000 MPa or less. In the present invention, the storage modulus (E') is measured by the method described in the Examples.

[0044] <Resin composition> The ionomer of the present invention may contain an antiaging agent, an antioxidant, and a heat deterioration inhibitor as necessary. The blending amounts of such various additives can be appropriately determined within a range that does not impair the effects of the present invention, and the total amount is preferably 7 mass % or less, more preferably 5 mass % or less, and further preferably 4 mass % or less.

[0045] The resin composition contains the ionomer of the present invention in an amount of preferably 93% by mass or more, more preferably 95% by mass or more, and even more preferably 96% by mass or more.

[0046] The various additives may be added to the polymerization or polymer reaction system when producing the ionomer, or may be added during or after the resin separation step, or may be added during the production of a molded article such as a film.

[0047] Known materials can be used as the antiaging agent. Specifically, phenolic compounds such as hydroquinone, hydroquinone monomethyl ether, 2,5-di-t-butylphenol, 2,6-di(t-butyl)-4-methylphenol, and mono(or di, or tri)(α-methylbenzyl)phenol; bisphenolic compounds such as 2,2'-methylenebis(4-ethyl-6-t-butylphenol), 4,4'-butylidenebis(3-methyl-6-t-butylphenol), and 4,4'-thiobis(3-methyl-6-t-butylphenol); benzimidazole compounds such as 2-mercaptobenzimidazole and 2-mercaptomethylbenzimidazole; 6-ethoxy-1 Examples of compounds that can be used include amine-ketone compounds such as 2-dihydro-2,2,4-trimethylquinoline, reaction products of diphenylamine and acetone, and 2,2,4-trimethyl-1,2-dihydroquinoline polymers; aromatic secondary amine compounds such as N-phenyl-1-naphthylamine, alkylated diphenylamine, octylated diphenylamine, 4,4'-bis(α,α-dimethylbenzyl)diphenylamine, p-(p-toluenesulfonylamido)diphenylamine, and N,N'-diphenyl-p-phenylenediamine; and thiourea compounds such as 1,3-bis(dimethylaminopropyl)-2-thiourea and tributylthiourea.

[0048] The antioxidant is effective in preventing the oxidative deterioration of the resin by itself in the presence of oxygen. Examples of the antioxidant include phosphorus-based antioxidants, hindered phenol-based antioxidants, and thioether-based antioxidants. These antioxidants may be used alone or in combination of two or more. Among them, from the viewpoint of the effect of preventing the deterioration of optical properties due to coloring, phosphorus-based antioxidants and hindered phenol-based antioxidants are preferred, and the combined use of a phosphorus-based antioxidant and a hindered phenol-based antioxidant is more preferred.

[0049] When a phosphorus-based antioxidant and a hindered phenol-based antioxidant are used in combination, the mass ratio of the phosphorus-based antioxidant to the hindered phenol-based antioxidant is preferably from (1:5) to (2:1), and more preferably from (1:2) to (1:1).

[0050] Preferred examples of the phosphorus-based antioxidant include 2,2-methylenebis(4,6-di-t-butylphenyl)octylphosphite (manufactured by ADEKA CORPORATION; trade name: Adeka STAB HP-10), tris(2,4-di-t-butylphenyl)phosphite (manufactured by BASF; trade name: IRGAFOS168), and 3,9-bis(2,6-di-t-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane (manufactured by ADEKA CORPORATION; trade name: Adeka STAB PEP-36).

[0051] Preferred examples of the hindered phenol antioxidant include pentaerythrityl-tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate] (manufactured by BASF; trade name IRGANOX1010) and octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate (manufactured by BASF; trade name IRGANOX1076).

[0052] The heat deterioration inhibitor is capable of preventing the thermal deterioration of a resin by capturing polymer radicals that are generated when the resin is exposed to high heat in a substantially oxygen-free state.

[0053] Preferred examples of the heat deterioration inhibitor include 2-t-butyl-6-(3'-t-butyl-5'-methyl-hydroxybenzyl)-4-methylphenyl acrylate (manufactured by Sumitomo Chemical Co., Ltd.; product name: Sumilizer GM) and 2,4-di-t-amyl-6-(3',5'-di-t-amyl-2'-hydroxy-α-methylbenzyl)phenyl acrylate (manufactured by Sumitomo Chemical Co., Ltd.; product name: Sumilizer GS).

[0054] In the present invention, in addition to the above-mentioned antiaging agents, antioxidants, and heat deterioration inhibitors, various additives such as ultraviolet absorbers, light stabilizers, anti-sticking agents, lubricants, release agents, polymer processing aids, antistatic agents, flame retardants, dyes and pigments, organic dyes, matting agents, and fluorescent materials may be added to the ionomer as necessary. The amounts of such various additives can be appropriately determined within a range that does not impair the effects of the present invention, and the total amount is preferably 7% by mass or less, more preferably 5% by mass or less, and even more preferably 4% by mass or less.

[0055] The various additives may be added to the polymerization or polymer reaction system when producing the ionomer, or may be added during or after the resin separation step, or may be added during the production of a molded article such as a film.

[0056] An ultraviolet absorber is a compound capable of absorbing ultraviolet rays, and is said to have a main function of converting light energy into heat energy.

[0057] Examples of the ultraviolet absorbent include benzophenones, benzotriazoles, triazines, benzoates, salicylates, cyanoacrylates, oxalic anilides, malonic acid esters, formamidines, etc. These may be used alone or in combination of two or more.

[0058] Benzotriazoles are preferred as ultraviolet absorbers because they have a high effect of suppressing the deterioration of optical properties such as coloration caused by exposure to ultraviolet light. Preferred benzotriazoles include 2-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol (manufactured by BASF; product name TINUVIN329), 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol (manufactured by BASF; product name TINUVIN234), 2,2'-methylenebis[6-(2H-benzotriazol-2-yl)-4-t-octylphenol] (manufactured by ADEKA Corporation; LA-31), and 2-(5-octylthio-2H-benzotriazol-2-yl)-6-tert-butyl-4-methylphenol.

[0059] Examples of triazine ultraviolet absorbers include 2,4,6-tris(2-hydroxy-4-hexyloxy-3-methylphenyl)-1,3,5-triazine (LA-F70, manufactured by ADEKA CORPORATION) and its analogues, hydroxyphenyltriazine ultraviolet absorbers (TINUVIN477 and TINUVIN460, manufactured by BASF), and 2,4-diphenyl-6-(2-hydroxy-4-hexyloxyphenyl)-1,3,5-triazine.

[0060] Light stabilizers are compounds that are said to have the function of capturing radicals generated mainly by oxidation due to light. Suitable light stabilizers include hindered amines such as compounds having a 2,2,6,6-tetraalkylpiperidine skeleton.

[0061] The anti-sticking agent is preferably a salt or ester of a fatty acid, an ester of a polyhydric alcohol, an inorganic salt, an inorganic oxide, or a particulate resin.Specific examples include calcium stearate, calcium carbonate, calcium sulfate, magnesium sulfate, barium sulfate, silicon dioxide (manufactured by Evonik under the trade name Aerosil), and particulate acrylic resin.

[0062] Examples of the lubricant include stearic acid, behenic acid, stearamide acid, methylene bisstearamide, hydroxystearic acid triglyceride, paraffin wax, ketone wax, octyl alcohol, and hardened oil.

[0063] Examples of the release agent include higher alcohols such as cetyl alcohol and stearyl alcohol; and higher fatty acid esters of glycerin such as stearate monoglyceride and stearate diglyceride.

[0064] As the polymer processing aid, polymer particles having a particle size of 0.05 to 0.5 μm, which can be produced by emulsion polymerization, are usually used. The polymer particles may be single-layer particles made of a polymer with a single composition ratio and a single intrinsic viscosity, or may be multi-layer particles made of two or more polymers with different composition ratios or intrinsic viscosities. Among these, preferred are particles with a two-layer structure having a polymer layer with a low intrinsic viscosity in the inner layer and a polymer layer with a high intrinsic viscosity of 5 dl / g or more in the outer layer. The polymer processing aid preferably has an intrinsic viscosity of 3 to 6 dl / g. If the intrinsic viscosity is too small, the effect of improving moldability tends to be low. If the intrinsic viscosity is too large, the moldability of the copolymer tends to decrease.

[0065] As the organic dye, a compound having a function of converting ultraviolet light into visible light is preferably used.

[0066] Examples of fluorescent substances include fluorescent pigments, fluorescent dyes, fluorescent white dyes, fluorescent brighteners, and fluorescent bleaches.

[0067] The ionomer of the present invention and the resin composition containing the ionomer of the present invention can be made into a form such as pellets to improve the convenience during storage, transportation, or molding. When molding into pellets, it is possible to obtain them by cutting strands obtained by melt extrusion. The resin temperature during melt extrusion is preferably 150°C or higher, more preferably 170°C or higher. In addition, the resin temperature during extrusion is preferably 250°C or lower, more preferably 230°C or lower. In this case, the health of workers can be ensured by using the resin of the present invention, which has little odor. The ionomer of the present invention and the resin composition containing the ionomer of the present invention are useful as an interlayer film for laminated glass.

[0068] <Resin sheet> The resin sheet of the present invention may be composed of only a layer (x) containing the ionomer or a resin composition thereof, or may be a multilayer film containing at least one layer (x). The multilayer film is not particularly limited, but examples thereof include a two-layer film in which a layer (x) and another layer are laminated, and a film in which another layer is disposed between two layers (x).

[0069] The other layers may include layers containing known resins. Examples of the resins include polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyurethane, polytetrafluoroethylene, acrylic resins, polyamide, polyacetal, polycarbonate, and polyesters, such as polyethylene terephthalate, polybutylene terephthalate, cyclic polyolefins, polyphenylene sulfide, polytetrafluoroethylene, polysulfone, polyethersulfone, polyarylate, liquid crystal polymers, polyimides, and thermoplastic elastomers. In addition, the other layers may also contain additives such as plasticizers, antioxidants, ultraviolet absorbers, light stabilizers, blocking inhibitors, pigments, dyes, heat-shielding materials (e.g., inorganic heat-shielding fine particles or organic heat-shielding materials having infrared absorbing ability), and functional inorganic compounds, as necessary.

[0070] The method for producing the resin sheet of the present invention is not particularly limited, and for example, the ionomer of the present invention or a resin composition containing the ionomer of the present invention is uniformly kneaded, and then the layer (x) is formed by a known film forming method such as an extrusion method, a calendar method, a press method, a solution casting method, a melt casting method, or an inflation method. The layer (x) may be used alone as a resin sheet. If necessary, the layer (x) may be laminated with other layers by press molding or the like to form a laminated resin sheet, or the layer (x) and other layers may be molded by a co-extrusion method to form a laminated resin sheet.

[0071] Among known film-forming methods, a method of producing a resin sheet using an extruder is particularly suitable. The resin temperature during extrusion is preferably 150°C or higher, more preferably 170°C or higher. The resin temperature during extrusion is preferably 250°C or lower, more preferably 230°C or lower. If the resin temperature becomes too high, the resin used will decompose, and there is concern about deterioration of the resin. Conversely, if the temperature is too low, the discharge from the extruder will not be stable, which will cause mechanical trouble. In order to efficiently remove the volatile substances, it is preferable to remove the volatile substances by reducing the pressure from the vent port of the extruder. Even if the volatile substances are efficiently removed, there is a possibility that odor will be generated at the T-die or the like, significantly worsening the working environment. By using the ionomer of the present invention, it is possible to form a film without worsening the working environment during film formation.

[0072] In addition, it is preferable that the resin sheet of the present invention has a surface formed with a concave-convex structure by a conventionally known method such as melt fracture or embossing. The shape of the melt fracture and embossing can be a conventionally known one. When a concave-convex structure is formed on the surface of the resin sheet of the present invention, it is preferable because it has excellent bubble releasing properties when the resin sheet is thermocompression bonded to a substrate such as glass.

[0073] The lower limit of the thickness of the resin sheet of the present invention is, in order of preference (the first lower limit is preferred, and the last lower limit is most preferred), 0.1 mm, 0.2 mm, 0.3 mm, 0.4 mm, 0.5 mm, 0.6 mm, 0.7 mm, and 0.75 mm. The upper limit is, in order of preference (the first upper limit is preferred, and the last upper limit is most preferred), 5 mm, 4 mm, 2 mm, 1.6 mm, 1.2 mm, 1.1 mm, 1 mm, and 0.79 mm. The thickness of the resin sheet is measured by a conventional method, for example, using a contact or non-contact thickness meter. The resin sheet may be in a rolled state or in the form of individual sheets.

[0074] The resin sheet of the present invention has the morphology, storage modulus (E') and haze described above with respect to the melt-kneaded product of the resin composition of the present invention.

[0075] The resin sheet of the present invention is preferably colorless as much as possible, and has a YI of preferably 2.0 or less, more preferably 1.8 or less, even more preferably 1.5 or less, and most preferably 1.0 or less, when the film thickness is 0.8 mm. The lower limit is 0.

[0076] The resin sheet of the present invention preferably has a low water content. For example, the water content is preferably 1% by mass or less, more preferably 0.5% by mass or less, further preferably 0.02% by mass or less, and most preferably 0.01% by mass or less.

[0077] <Laminated glass> The resin sheet of the present invention is preferably used as an interlayer film for laminated glass. In this case, the glass to be laminated with the interlayer film of the resin sheet of the present invention may be, for example, inorganic glass such as float glass plate, tempered glass plate, polished glass plate, figured glass plate, wired glass plate, heat absorbing glass plate, or conventionally known organic glass such as polymethyl methacrylate or polycarbonate, without any restrictions. These may be either colorless or colored. These may be used alone or in combination of two or more. The thickness of the glass is preferably 100 mm or less.

[0078] The laminated glass obtained by sandwiching the resin sheet of the present invention between two pieces of glass can be produced by a conventionally known method. For example, a method using a vacuum laminator, a method using a vacuum bag, a method using a vacuum ring, a method using a nip roll, etc. In addition, a method in which the glass sheets are temporarily pressed together by the above method, and then put into an autoclave for main bonding can also be mentioned.

[0079] When using a vacuum laminator, for example, 1×10 -6 ~3×10 -2 The inorganic glass plate, the intermediate film, the adhesive resin layer and the organic glass plate are laminated under a reduced pressure of 100 MPa at 60 to 200° C., particularly at 80 to 160° C. A method using a vacuum bag or a vacuum ring is described in, for example, European Patent No. 1235683, and a vacuum pressure of about 2×10 -2 It is laminated at 100 to 160°C under a pressure of MPa.

[0080] The manufacturing method using nip rolls includes a method in which the interlayer is degassed with rolls at a temperature below the flow initiation temperature, and then pressure-bonded at a temperature close to the flow initiation temperature. Specifically, for example, the interlayer is heated to 30 to 70°C with an infrared heater or the like, degassed with rolls, and then heated to 50 to 120°C, and then pressure-bonded with rolls.

[0081] When the laminated glass is subjected to pressure bonding using the above-mentioned method and then placed in an autoclave for further pressure bonding, the operating conditions for the autoclave step are appropriately selected depending on the thickness and configuration of the laminated glass. For example, it is preferable to treat the laminated glass under a pressure of 0.5 to 1.5 MPa at 100 to 160°C for 0.5 to 3 hours.

[0082] The laminated glass of the present invention has excellent transparency. For example, when the thickness of the interlayer is 0.8 mm, the haze of the laminated glass is preferably 1% or less, more preferably 0.8% or less, and even more preferably 0.5% or less. The lower limit is not particularly specified, but is 0.01%. In the present invention, the haze is measured using a haze meter HZ-1 (manufactured by Suga Test Instruments Co., Ltd.) in accordance with JIS K7136:2000.

[0083] It is particularly preferable that the laminated glass of the present invention has excellent transparency even after being heated to 140° C. and then slowly cooled from 140° C. to 23° C. at a rate of 0.1° C. / min. For example, the haze of a laminated glass having an interlayer thickness of 0.8 mm after slow cooling is preferably 5.0% or less, more preferably 4.5% or less, even more preferably 4.0% or less, and most preferably 3.0% or less. There is no particular lower limit, but it is 0.01%.

[0084] The laminated glass of the present invention is preferably colorless, and as colorless as possible. For example, in a laminated glass having an interlayer thickness of 0.8 mm, YI is preferably 2.0 or less, more preferably 1.8 or less, even more preferably 1.5 or less, and most preferably 1.0 or less. The lower limit is 0.

[0085] The adhesive strength between the glass and the interlayer film of the laminated glass of the present invention is preferably high. For example, the value evaluated by the compression shear strength test described in WO1999-058334 is preferably 15 MPa or more, more preferably 20 MPa or more, and most preferably 25 MPa or more. There is no particular upper limit, but it is 100 MPa or less.

[0086] As described above, the ionomer of the present invention and the resin sheet obtained by molding the resin composition containing the ionomer of the present invention are useful as an interlayer film for laminated glass. The interlayer film for laminated glass is particularly preferable as an interlayer film for laminated glass for structural materials, since it has excellent adhesion to substrates such as glass, transparency, and self-supporting property. In addition, it is also suitable as an interlayer film for laminated glass in various applications such as automobile front glass, automobile side glass, automobile sunroof, automobile rear glass, glass for head-up display, other moving bodies such as automobiles, laminates for exterior walls and roofs, panels, doors, windows, walls, roofs, sunroofs, sound insulation walls, display windows, balconies, handrail walls, and other buildings, partition glass members for conference rooms, solar cells, etc., but is not limited to these applications. EXAMPLES

[0087] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0088] [Analysis of resins obtained in the examples and comparative examples] The contents of (meth)acrylic acid ester units, carboxylic acid units and carboxylic acid neutralization product units were analyzed as follows.

[0089] The ionomer or the resin composition containing the ionomer obtained by the method described below was dissolved in a mixed solvent of dehydrated toluene / dehydrated acetic acid (75 / 25% by mass), reacted at 100°C for 2 hours, and then reprecipitated in a mixed solvent of acetone / water (80 / 20% by mass) to convert the carboxylic acid neutralized product into a carboxylic acid. The resin obtained was thoroughly washed with water and then dried. The components of the polymerization units of the resin obtained were analyzed by pyrolysis GC-MS (1). Next, the acid value of the resin obtained was measured in accordance with JIS K0070-1992 (2). The resin obtained was also analyzed by pyrolysis GC-MS (1) to determine the acid value of the resin obtained. ... 1H-NMR (400 MHz, JEOL Ltd.) measurements were performed (3). In addition, the ionomer or the resin composition containing the ionomer was pretreated by microwave decomposition with nitric acid, and then the type and amount of metal ions in the carboxylic acid neutralization product were identified by ICP emission spectrometry (Thermo Fisher Scientific iCAP6500Duo) (4). The type and structure of the (meth)acrylic acid ester unit and the carboxylic acid unit were identified from (1), and based on this information, the ratio of ethylene / (meth)acrylic acid ester unit / (total of carboxylic acid unit and carboxylic acid neutralization product unit) was calculated from the information in (2) and (3). Furthermore, the ratio of ethylene / (meth)acrylic acid ester unit / carboxylic acid unit / carboxylic acid neutralization product unit was calculated from the information in (4).

[0090] [Melt flow rate (MFR)] In accordance with JIS K7210, the amount of resin extruded per 10 minutes from a die of a specified diameter installed at the bottom of the cylinder was measured under conditions of 190°C and a load of 2.16 kgf for the molten resin in the cylinder.

[0091] [Odor] 50 g of the ionomer or the resin composition containing the ionomer obtained by the method described below was melt-kneaded at 220°C and 100 rpm in a Labo Plastomill (manufactured by Toyo Seiki). The inlet of the Labo Plastomill was left open, and the odor was compared from a position 50 mm away directly above it. The odor was measured using a portable odor sensor (model: XP-329m, manufactured by Shin Cosmos Electric Co., Ltd.) for 30 seconds starting 5 minutes after the start of melt-kneading, and the average values ​​of the maximum and minimum odor values ​​for the 30 seconds were compared. The higher the odor value, the stronger the odor. An odor value of 700 or more was evaluated as "B", and an odor value of less than 700 was evaluated as "A".

[0092] [Independent in high temperature environment] A melt-kneaded product of an ionomer or a resin composition containing an ionomer obtained by the method described below was subjected to heating at 210°C and a pressure of 50 kgf / cm 2The sheet was compression molded at a pressure of 1000 MPa for 5 minutes to obtain a resin sheet having a thickness of 0.8 mm. A test piece having a length of 40 mm and a width of 5 mm was cut out from the sheet, and the storage modulus (E') was measured at a measurement temperature of 50°C and a frequency of 1 Hz using a dynamic viscoelasticity measuring device manufactured by UBM Co., Ltd. The value was used as an index of the self-supporting property of the resin sheet in a high-temperature environment. When the storage modulus was 30 MPa or more, it was evaluated as "A", and when it was less than 30 MPa, it was evaluated as "B".

[0093] [Colorability] A melt-kneaded product of an ionomer or a resin composition containing an ionomer obtained by the method described below was subjected to heating at 210°C and a pressure of 50 kgf / cm 2 The resin sheet was compression molded at a pressure of 0.05 for 5 minutes to obtain a resin sheet having a thickness of 0.8 mm. The sheet was measured in accordance with JIS Z8722 using a colorimeter "ZE-2000" (product name) manufactured by Nippon Denshoku Industries Co., Ltd. The yellowness value calculated in accordance with JIS K7373 based on the obtained value was taken as the yellow index (YI). The measured YI was rated as "A" when it was 2.0 or less, "B" when it was more than 2.0 and less than 3.0, and "C" when it was 3.0 or more.

[0094] [Transparency] A melt-kneaded product of an ionomer or a resin composition containing an ionomer obtained by the method described below was subjected to heating at 210°C and a pressure of 50 kgf / cm 2 The resin sheet was compressed at a pressure of 100° C. for 5 minutes to obtain a resin sheet having a thickness of 0.8 mm. The resin sheet obtained was sandwiched between two float glass sheets having a thickness of 2.7 mm, and a vacuum laminator (1522N manufactured by Nisshinbo Mechatronics Inc.) was used to reduce the pressure inside the vacuum laminator at 100° C. for 1 minute, and the vacuum degree and temperature were maintained while pressing at 30 kPa for 5 minutes to obtain a temporary bonded body. The temporary bonded body obtained was placed in an autoclave and treated at 140° C. and 1.2 MPa for 30 minutes to obtain a laminated glass.

[0095] The laminated glass obtained by the above method was heated to 140°C, and then slowly cooled to 23°C at a rate of 0.1°C / min. The haze of the laminated glass after the slow cooling operation was measured using a haze meter HZ-1 (manufactured by Suga Test Instruments Co., Ltd.) in accordance with JIS K7136:2000. The measured haze was evaluated as "A" when it was 5.0% or less, "B" when it was more than 5.0% and less than 10%, and "C" when it was 10% or more.

[0096] Table 1 summarizes the ethylene-(meth)acrylic acid ester copolymers (X) used as raw materials for producing the ionomers of the present examples and comparative examples. These ethylene-(meth)acrylic acid ester copolymers (X) can be synthesized by the high-temperature, high-pressure radical polymerization method described in US2013 / 0274424, JP2006-233059, or JP2007-84743. For example, "Acryft" (registered trademark) WD301F manufactured by Sumitomo Chemical Co., Ltd. can be used as EMMA1, and "Rexpearl" (registered trademark) A4250 manufactured by Japan Polyethylene Corporation can be used as EEA1.

[0097] [Table 1]

[0098] [Example 1] 233 parts by mass of toluene was added to 100 parts by mass of EMMA4 in Table 1, and dissolved under a pressure of 0.02 MPa at 60° C. 96 parts by mass of a methanol solution of sodium hydroxide (20% by mass) was added to the resulting solution, and the methyl methacrylate units were saponified at 100° C. for 2 hours to convert them to sodium methacrylate units.

[0099] To this solution, 44 parts by mass of concentrated hydrochloric acid (36% by mass) was added, and a part of the sodium methacrylate units was converted to methacrylic acid at 100° C. for 2 hours. The obtained solution was reprecipitated in a mixed solvent of acetone / water (80 / 20% by mass) to obtain ionomer 1. The obtained ionomer 1 was then analyzed and its properties were evaluated. The analysis results of ionomer 1 are shown in Table 2. The MFR measurement results and odor evaluation results of ionomer 1, the self-supporting property of the resin sheet at high temperatures, and the evaluation results of the transparency and colorability of the laminated glass are shown in Table 3.

[0100] [Example 2] Ionomer 2 was obtained in the same manner as in Example 1, except that EMMA5 in Table 1 was used and 100 parts by mass of a methanol solution of sodium hydroxide and 46 parts by mass of concentrated hydrochloric acid were added. The analysis results and evaluation results of the obtained ionomer 2 are shown in Tables 2 and 3.

[0101] [Example 3] Ionomer 3 was obtained in the same manner as in Example 1, except that EMMA5 in Table 1 was used, 95 parts by mass of a methanol solution of sodium hydroxide (16 mass%) was added, the methyl methacrylate units were saponified at 100° C. for 10 hours, and 33 parts by mass of concentrated hydrochloric acid was added. The analysis results and evaluation results of the obtained ionomer 3 are shown in Tables 2 and 3.

[0102] [Example 4] Ionomer 4 was obtained in the same manner as in Example 1, except that EMMA6 in Table 1 was used and 112 parts by mass of a methanol solution of sodium hydroxide and 51 parts by mass of concentrated hydrochloric acid were added. The analysis results and evaluation results of the obtained ionomer 4 are shown in Tables 2 and 3.

[0103] [Example 5] Ionomer 5 was obtained in the same manner as in Example 1, except that EEA2 in Table 1 was used and 100 parts by mass of a methanol solution of sodium hydroxide and 43 parts by mass of concentrated hydrochloric acid were added. The analysis results and evaluation results of the obtained ionomer 5 are shown in Tables 2 and 3.

[0104] [Example 6] Ionomer 6 was obtained in the same manner as in Example 1, except that EEA1 in Table 1 was used and 100 parts by mass of a methanol solution of sodium hydroxide and 46 parts by mass of concentrated hydrochloric acid were added. The analysis results and evaluation results of the obtained ionomer 6 are shown in Tables 2 and 3.

[0105] [Example 7] Ionomer 7 was obtained in the same manner as in Example 1, except that EMA in Table 1 was used and 112 parts by mass of a methanol solution of sodium hydroxide and 51 parts by mass of concentrated hydrochloric acid were added. The analysis results and evaluation results of the obtained Ionomer 7 are shown in Tables 2 and 3.

[0106] [Example 8] Ionomer 18 was obtained in the same manner as in Example 1, except that EMMA7 in Table 1 was used and 100 parts by mass of a methanol solution of sodium hydroxide and 46 parts by mass of concentrated hydrochloric acid were added. The analysis results and evaluation results of the obtained ionomer 18 are shown in Tables 2 and 3.

[0107] [Comparative Example 1] Ionomer 8 was obtained in the same manner as in Example 1, except that EMMA1 in Table 1 was used and 40 parts by mass of a methanol solution of sodium hydroxide and 18 parts by mass of concentrated hydrochloric acid were added. The analysis results and evaluation results of the obtained ionomer 8 are shown in Tables 2 and 3.

[0108] [Comparative Example 2] Ionomer 9 was obtained in the same manner as in Example 1, except that EMMA2 in Table 1 was used and 72 parts by mass of a methanol solution of sodium hydroxide and 33 parts by mass of concentrated hydrochloric acid were added. The analysis results and evaluation results of the obtained ionomer 9 are shown in Tables 2 and 3.

[0109] [Comparative Example 3] Ionomer 10 was obtained in the same manner as in Example 1, except that 80 parts by mass of a methanol solution of sodium hydroxide and 37 parts by mass of concentrated hydrochloric acid were added using EMMA3 in Table 1. The analysis results and evaluation results of the obtained ionomer 10 are shown in Tables 2 and 3.

[0110] [Comparative Example 4] Ionomer 11 was obtained in the same manner as in Example 1, except that EMMA4 in Table 1 was used and 78 parts by mass of acetic acid was added instead of concentrated hydrochloric acid. The analysis results and evaluation results of the obtained ionomer 11 are shown in Tables 2 and 3.

[0111] [Comparative Example 5] Ionomer 12 was obtained in the same manner as in Example 1, except that EMMA5 in Table 1 was used, 100 parts by mass of a methanol solution of sodium hydroxide was added, the methyl methacrylate units were saponified at 120° C. for 10 hours, and 46 parts by mass of concentrated hydrochloric acid was added, and the analytical results and evaluation results of the obtained ionomer 12 are shown in Tables 2 and 3.

[0112] [Comparative Example 6] Ionomer 13 was obtained in the same manner as in Example 3, except that EMMA5 in Table 1 was used, the reaction time of the saponification reaction was set to 3 hours, and 39 parts by mass of concentrated hydrochloric acid was added. The analysis results and evaluation results of the obtained ionomer 13 are shown in Tables 2 and 3.

[0113] [Comparative Example 7] Ionomer 14 was obtained in the same manner as in Example 4, except that EMMA6 in Table 1 was used and 47 parts by mass of concentrated hydrochloric acid was added. The analysis results and evaluation results of the obtained ionomer 14 are shown in Tables 2 and 3.

[0114] [Comparative Example 8] Ionomer 15 was obtained in the same manner as in Example 1, except that EMA in Table 1 was used, 106 parts by mass of a methanol solution of sodium hydroxide, the reaction time of the saponification reaction was set to 3 hours, and 49 parts by mass of concentrated hydrochloric acid was added. The analysis results and evaluation results of the obtained ionomer 15 are shown in Tables 2 and 3.

[0115] [Comparative Example 9] An ethylene / methacrylic acid ionomer having a methacrylic acid unit content of 6.3 mol % and a sodium methacrylate unit content of 1.8 mol % and an MFR of 2.7 g / 10 min was used as ionomer 16. The analysis and evaluation results of ionomer 16 are shown in Tables 2 and 3.

[0116] [Comparative Example 10] An ethylene / n-butyl methacrylate / methacrylic acid ionomer having a methacrylic acid unit content of 6.0 mol%, a sodium methacrylate unit content of 2.1 mol%, and a n-butyl methacrylate unit content of 3.0 mol%, and an MFR of 3.5 g / 10 min, was used as ionomer 17. The analysis and evaluation results of ionomer 17 are shown in Tables 2 and 3.

[0117] [Table 2]

[0118] [Table 3]

[0119] From the above results, the ionomers of the Examples, which satisfied all of the prescribed constituent requirements of the present invention, were excellent in terms of transparency, high modulus, and low coloration in a well-balanced manner, and also had reduced odor during molding processing. In contrast, the ionomers of the Comparative Examples, which did not satisfy any of the constituent requirements, were inferior in any of the performances among transparency, high modulus, low coloration, and odor.

Claims

1. An ionomer comprising, based on all monomer units constituting the resin, 0.05 to 1.0 mol % of (meth)acrylic acid ester units, 4.5 to 9.0 mol % of carboxylic acid units, 0.65 to 3.0 mol % of carboxylic acid neutralization product units, and ethylene units, and the total content of the (meth)acrylic acid ester units, carboxylic acid units, and carboxylic acid neutralization product units is 7.0 to 10 mol %.

2. 2. The ionomer according to claim 1, which has an MFR of 0.7 g / 10 min or more, measured under conditions of a measurement temperature of 190° C. and a load of 2.16 kgf.

3. The ionomer according to claim 1 or 2, wherein the (meth)acrylic acid ester unit is at least one selected from the group consisting of methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, and isobutyl (meth)acrylate.

4. Contains 6.5 to 10 mol % of (meth)acrylic acid ester units; It has an MFR of 90 to 400 g / 10 min measured at a temperature of 190° C. and a load of 2.16 kgf. Uses ethylene-(meth)acrylic acid ester copolymer as raw material. The ionomer according to any one of claims 1 to 3.

5. A storage modulus of 30 MPa or more measured using a resin sheet-like test piece having a thickness of 0.8 mm under the conditions of a measurement temperature of 50° C. and a frequency of 1 Hz; A yellow index (YI) of 2.0 or less, measured using a resin sheet specimen having a thickness of 0.8 mm; and A haze of 5.0% or less measured using a laminated glass in which a resin sheet-like test piece having a thickness of 0.8 mm was placed between two glass plates, heated to 140° C., and then cooled slowly to 23° C. at a rate of 0.1° C. / min. The ionomer according to any one of claims 1 to 4, having the formula:

6. A resin composition comprising the ionomer according to any one of claims 1 to 5 in an amount of 93% by mass or more.

7. A resin sheet consisting essentially of the ionomer according to any one of claims 1 to 5 or the resin composition according to claim 6.

8. A laminated glass comprising two glass plates and the resin sheet according to claim 7 disposed between the two glass plates as an interlayer film.

Citation Information

Patent Citations

  • JP1973045577A

  • Laminate

    JP1980109658A

  • Oxygen absorber, laminated body using it and packing vessel

    JP2005087991A

  • ionomer film or sheet and solar cell modules containing the same

    JP2011507278A

  • Multilayer interlayer and glass laminate

    WO2017196707A1