Method for manufacturing metal film deposition member, metal film deposition member, wavelength conversion member and light emitting device
The method of forming metal films on composite ceramic members with enhanced adhesion and controlled removal techniques addresses the challenge of precision, enhancing device performance by ensuring accurate film placement and adhesion.
Patent Information
- Application Number
- JP2024113982
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-06-05
AI Technical Summary
Existing methods struggle to form metal films with high precision on specific portions of surfaces, leading to inaccuracies and inefficiencies.
A method involving a composite ceramic member with a connecting member that has enhanced adhesion to noble metals, where a noble metal film is applied and selectively removed to achieve precise alignment with the ceramic member boundaries, utilizing sputtering and peeling techniques to control film thickness and adhesion.
Enables the formation of metal films with high precision, ensuring accurate boundaries and enhanced adhesion, reducing light leakage and improving the functionality of devices like light-emitting devices.
Smart Images

Figure 2024133271000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a metal film member, a metal film member, a wavelength conversion member, or a light emitting device. Regarding. [Background technology]
[0002] A technique is known in which a metal film is provided on a part of the surface for the purpose of light shielding, etc. In the present study, a method has been developed in which a metal light-shielding film is formed on the upper surface of the phosphor layer and then a part of the light-shielding film is removed. As shown. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent Publication No. 2013-232539 Summary of the Invention [Problem to be solved by the invention]
[0004] When a metal film is to be provided partially, the metal film must be formed with high precision in the required area. It is desirable to provide a metal film on a desired portion with high accuracy. . [Means for solving the problem]
[0005] The method for producing a metal film-formed member disclosed in the present specification includes: A composite ceramic member having a mix member and a connection member connected to the mix member. The composite ceramic member is provided with a connecting member having a stronger adhesive force with the precious metal than the ceramic member. and a step of providing a surface of the ceramic member and a surface of the connection member at least partially. providing a precious metal film on a surface region of the composite ceramic member; The noble metal film is formed in the region between the ceramic member and the connection member. and removing the precious metal film provided on the surface of the ceramic member by etching.
[0006] The metal deposition member disclosed in the present specification includes a ceramic member and the ceramic A connecting member that connects to the ceramic member, and a front portion along the boundary between the ceramic member and the connecting member. and a noble metal film formed on the surface of the connection member, The surface has a stronger adhesive force with the precious metal than the surface of the ceramic member.
[0007] The metal deposition member disclosed in the present specification is a ceramic member and the ceramic The surface area of a composite ceramic member is connected to a connecting member which has a stronger adhesive force with the precious metal than the member. providing a noble metal film on the surface region; and forming a ceramic layer of the noble metal film on the surface region. and removing the noble metal film provided on the surface of the member. A metal film forming portion in which the boundary of the precious metal film coincides with the boundary between the ceramic member and the connecting member. It is a material.
[0008] The present specification also provides a metal deposition member comprising a first ceramic member and the first A second ceramic member connected to the ceramic member, and a ceramic member and a ceramic member connected to the first ceramic member and the second ceramic member. A precious metal film is formed on the surface of the second ceramic member along the boundary with the ceramic member. and the second ceramic member has a surface roughness Rz of the surface on which the precious metal film is formed. is 0.10 μm or more.
[0009] The wavelength conversion member disclosed in the present specification includes a wavelength conversion portion having a phosphor, and a light reflecting portion connected to the wavelength converting portion, and along a boundary between the wavelength converting portion and the light reflecting portion, a light-shielding film formed on a surface of the light reflecting portion, the light-shielding film being a precious metal film; Across the boundary, the surface of the light reflecting portion is more likely to be a noble metal than the surface of the wavelength converting portion. The adhesion is strong.
[0010] The wavelength conversion member disclosed in the present specification includes a wavelength conversion portion and a ceramic-based material. A connection member that connects the wavelength conversion unit and a boundary between the wavelength conversion unit and the connection member are used as the material. and a light-shielding film formed on the surface of the connection member along the line The connecting member has a surface roughness Rz of 0.10 μm on the surface on which the precious metal film is formed. m or more.
[0011] The light emitting device disclosed in the present specification includes a light emitting element and a light emitting device in which the light emitting element is disposed. a wavelength conversion unit; a connection member connected to the wavelength conversion unit; and and a light-shielding film formed on the surface of the package, and the light-shielding film is directly or indirectly connected to the package. a wavelength conversion member, the light-shielding film being arranged along a boundary between the wavelength conversion portion and the connection member. a noble metal film formed on the surface of the connection member, The surface of the wavelength converting portion has a stronger adhesive strength with the noble metal than the surface of the wavelength converting portion.
[0012] The light emitting device disclosed in the present specification includes a light emitting element and a light emitting device in which the light emitting element is disposed. a package for converting the wavelength of the light emitted from the wavelength conversion element; and a connection part for connecting the wavelength conversion element to the package. and a light-shielding film formed on the surface of the connection member, a wavelength conversion member connected to the package, and the light-shielding film is A precious metal film is formed on the surface of the connection member along the boundary with the connection member, The surface of the connecting member on which the noble metal film is formed has a surface roughness Rz of 0.10 μm or more. Effect of the Invention
[0013] According to the present invention, a member having a metal film provided on its surface with high precision can be realized. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a perspective view of a metal deposition member according to an embodiment. [Diagram 2] FIG. 2 is a cross-sectional view of the metal film-formed member taken along line II-II in FIG. [Figure 3A] FIG. 3A is a cross-sectional view illustrating a method for producing a metal film member. [Figure 3B] FIG. 3B is a cross-sectional view illustrating the method for producing the metal film member. [Figure 3C] FIG. 3C is a cross-sectional view illustrating the method for producing the metal film member. [Figure 3D] FIG. 3D is a cross-sectional view illustrating the method for producing the metal film member. [Figure 4A] FIG. 4A is a TEM image of the produced metal-coated member. [Figure 4B] FIG. 4B is another TEM image of the produced metal-coated member. [Figure 4C] FIG. 4C is another TEM image of the produced metal-coated member. [Figure 4D] FIG. 4D is another TEM image of the produced metal-coated member. [Diagram 5] FIG. 5 is a perspective view of the light emitting device according to the embodiment. [Figure 6] FIG. 6 is a top view corresponding to FIG. [Figure 7] FIG. 7 is a cross-sectional view of the light emitting device taken along line VII-VII in FIG. [Figure 8]FIG. 8 is a perspective view for explaining the internal structure of the light emitting device according to the embodiment. [Figure 9] FIG. 9 is a top view corresponding to FIG. [Figure 10] FIG. 10 is a perspective view for explaining the internal structure of the light emitting device according to the embodiment. [Figure 11] FIG. 11 is a top view corresponding to FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] In this specification or claims, when referring to polygons such as triangles and quadrilaterals, Polygons and shapes that have been processed with rounded corners, chamfers, corner removal, rounding, etc. are also included. In addition, the shape where processing is applied not only to the corners (edges) but also to the middle part of the edge is also called In other words, the polygon is left as the base, but partial processing is performed. The shapes shown are within the interpretation of "polygon" as used herein and in the claims. It shall be so.
[0016] This also applies to words that represent specific shapes, such as trapezoids, circles, and irregular shapes, not just polygons. The same is true for each edge that forms the shape. Even if the corners or middle parts are processed, the interpretation of the “side” includes the processed parts. In addition, "polygons" and "edges" that are not partially processed are distinguished from processed shapes. In such cases, the word "strict" shall be added, for example, "strict rectangle."
[0017] In addition, in the present specification or claims, the terms "up and down," "left and right," "front and back," "front and back," "front and back," and "back" are used interchangeably. These expressions only describe the relationship of relative position, orientation, direction, etc. For example, the top surface of a part may be aligned with the top surface of the finished product. Even if the component is mounted on the side, the top surface remains the same for that component.
[0018] In addition, in the present specification or claims, the following description will be used to refer to a certain component: When there are multiple things and you want to distinguish between them, you can put “first,” “second,” etc., in front of the component. In addition, the following points are sometimes distinguished in the present specification and the claims: In the case where the subject matter or viewpoint is different, the same notation is used between the present specification and the claims. may not refer to the
[0019] For example, objects that are distinguished by being labeled "first," "second," and "third" in this specification In the case where the claims are written only with respect to the "first" and "third" in the specification, In such cases, the claims may be distinguished by adding "first" and "second" for ease of reading. In this case, the subject matter described as "first" and "second" in the claims may be refers to the objects referred to as "first" and "third" in this specification.
[0020] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. The embodiments embody the technical ideas of the present invention, but do not limit the present invention. In the following description, the same names and symbols refer to the same or similar components. The drawings show the sizes of the components shown in the drawings. The sheath, positional relationship, etc. may be exaggerated for clarity of explanation.
[0021] <Embodiment> FIG. 1 is a perspective view showing an example of a metal film-formed member 1 according to an embodiment. 3A, 3B, 3C, and 3D are cross-sectional views of the metal deposition member 1 taken along line II. 4A to 4D are cross-sectional views for explaining a method for manufacturing the metal film-formed member 1. 1 is a TEM (Transmission Electron Microscope) image of a film-formed member 1.
[0022] FIG. 5 is a perspective view showing an example of the light emitting device 2 according to the embodiment. FIG. Fig. 7 is a cross-sectional view of the light emitting device 2 taken along line VII-VII in Fig. 6. FIG. 2 is a perspective view of the light emitting device 2 with the light blocking member 300 removed in order to explain the internal structure. FIG. 9 is a top view in the same state as FIG. 8. FIG. 10 is a top view in order to explain the internal structure. FIG. 2 is a perspective view of the light emitting device 2 from which a light-transmitting member 290 and a wavelength converting member 280 have been further removed. Fig. 11 is a top view in the same state as in Fig. 9.
[0023] First, the metal film member 1 according to the embodiment will be described, and then the metal film member according to the embodiment will be described. A light emitting device 2 formed by including the film-formed member 1 as a component will be described.
[0024] The metal film member 1 includes a composite ceramic member 110, a precious metal film 120, and a gold film. The metal film 130 and the black film 140 are included as components of the metal film member 1. It has at least a composite ceramic member 110 and a precious metal film 120 .
[0025] Each component of the metal deposition member 1 will be described. (Composite ceramic member 110) The composite ceramic member 110 includes, as its components, a ceramic member 111 and a connecting portion. The composite ceramic member 110 has a top surface, a bottom surface, and a side surface. The composite ceramic member 110 is formed in a flat plate shape. The member 110 is formed in a rectangular parallelepiped shape. Alternatively, the shape may be rectangular when viewed from below. Here, the rectangular shape includes a square.
[0026] On the upper surface of the composite ceramic member 110, the ceramic member 111 and the connecting member 112 The ceramic members 111 and 112 are continuous on the lower surface of the composite ceramic member 110. The composite ceramic member 110 and the connecting member 112 are continuous. The ceramic member 112 is exposed, but the ceramic member 111 is not exposed. At the side of the member 110, the ceramic member 111 and the connecting member 112 are not continuous. .
[0027] On the upper surface of the composite ceramic member 110, the ceramic member 111 is connected to a connecting member 112. The ceramic member 111 is surrounded by the lower surface of the composite ceramic member 110. The composite ceramic member 110 is surrounded by a connecting member 112. The ceramic member 111 is exposed in the region, and the ceramic member 111 is exposed on the lower surface of the composite ceramic member 110. The area where the material 111 is exposed has the same shape and size.
[0028] The ceramic member 111 has an upper surface, a lower surface, and a side surface. The ceramic member 11 is formed in a flat plate shape. The ceramic member 111 is formed in a rectangular parallelepiped shape. The ceramic member 111 is formed in a rectangular shape when viewed from above or below. The rectangle here includes a square. However, the shape does not have to be limited to a rectangle. For example, The illustrated ceramic member 111 has a shape similar to that of a rectangular shape when viewed from above and below. , formed in a rectangular shape.
[0029] The ceramic member 111 also has a connection region that is connected to the connection member 112. The ceramic member 111 has a connection region on its side. The entire surface of the ceramic member 111 is the connection region. The edge is included in the connection region. Also, the upper surface or the lower surface of the ceramic member 111 is the outer edge. , are not included in the connection region.
[0030] The entire upper or lower surface of the ceramic member 111 is not included in the connection region. As an example of a configuration in which the entire upper or lower surface is not included in the connection region, for example, a ceramic part The upper or lower surface of the member 111 has a shape protruding from the upper or lower surface of the connection member 112. There are cases where this is the case.
[0031] The ceramic member 111 is formed mainly of ceramic. Examples of ceramics include aluminum oxide, aluminum nitride, silicon oxide, and oxide. Examples of the oxides include yttrium oxide, zirconium oxide, and magnesium oxide. Thus, a ceramic member 111 is formed.
[0032] The connection member 112 has an upper surface, a lower surface, an outer surface, and an inner surface. 2 is formed in the shape of a flat plate with through holes. The outer edge of the member 112 is rectangular. Here, the rectangle includes a square. This shape is The shape is not limited to a rectangle, and may be, for example, a circle.
[0033] The connection member 112 has a connection region that connects to the ceramic member 111. The connection member 112 has a connection region on its inner surface. The connecting region is also defined by the intersection line between the upper surface and the inner surface of the connecting member 112 or the intersection line between the lower surface and the inner surface of the connecting member 112. The intersection line of the above is included in the connection area. It is not included in the connection region except for the line of intersection with .
[0034] The entire upper or lower surface of the connection member 112 does not have to be included in the connection region. As an example of a configuration in which the entire upper or lower surface is not included in the connection region, for example, the upper surface of the connection member 112 may be When the upper or lower surface of the ceramic member 111 has a shape protruding from the upper or lower surface of the ceramic member 111, The answer is yes.
[0035] In addition, the adhesive strength between the connection member 112 and the precious metal is greater than that between the connection member 112 and the ceramic member 111. In addition, at least on the surface on which the precious metal film 120 is formed, the connecting member 112 is The adhesion to the noble metal is stronger than that to the ceramic member 111. The connecting member 112 is formed of a material or has a shape that is more likely to adhere to the noble metal than the connecting member 112. In other words, the fact that it is easy to peel off means that it is difficult to peel off.
[0036] The connecting member 112 is mainly made of ceramic. Examples of ceramics include aluminum oxide, aluminum nitride, silicon oxide, and oxide. Examples of the ceramic oxide include yttrium oxide, zirconium oxide, and magnesium oxide. For example, the connecting member 112 may be formed mainly of a metal. The adhesion strength of metals such as Al, Fe, and Ti to precious metals is stronger than that of ceramics. is also large.
[0037] The ceramic member 111 and the connection member 112 are integrally formed. The ceramic material is formed by integrally sintering the mixing member 111 and the connecting member 112. The lock member 111 and the connection member 112 are formed. For example, the sintered ceramic member 11 1 and the powder material forming the connection member 112 are integrally molded and sintered to form the connection member 112. For sintering, there are several methods, such as pressureless sintering, spark plasma sintering (SPS), hot press sintering, etc. The pressure-pressure sintering method (HP method) can be used.
[0038] In addition, the ceramic member 111 and the connection member 112 are formed using the same ceramic as the main material. In this case, the connection member 112 has a larger porosity than the ceramic member 111. However, the connecting member 112 is formed to include more voids. It depends on the sintering conditions (sintering temperature, sintering time, heating rate), the grain size of the material, the concentration of the sintering aid, etc. So it can be adjusted.
[0039] By increasing the porosity, the surface of the connection member 112 becomes uneven due to the voids. 120 adheres better to a surface with many projections and recesses than to a surface with few projections and recesses. This is because the precious metal penetrates into the unevenness and is then deposited. Therefore, by increasing the porosity, the adhesive strength with the precious metal can be increased.
[0040] (Precious metal film 120) The noble metal film 120 is a metal film formed mainly of a noble metal. The metal film formed only from a noble metal is a metal film formed only from a noble metal. The metal content of the product is 80% or more of the total. The noble metal film 120 may be made of an alloy containing P. The material may be one or more selected from the group consisting of precious metals, such as t, Au, Ag, and Rh. The film 120 may be formed solely from Pt.
[0041] The precious metal film 120 can be formed to a thickness in the range of 5 nm to 500 nm. The thickness may be more than 500 nm. Also, the thickness may be 1000 nm or less. It is preferred that a ferroelectric film is formed.
[0042] (Metal Film 130) The metal film 130 is a metal film formed mainly of metal. The main material is a metal different from the main material of the precious metal film 120. The metal film 130 is formed from a material that is not included in the material that forms the 0. The metal film 130 is made of a metal material selected from the group consisting of Ru, W, Al, Ti, and Ni. For example, the metal film 130 may be formed only from Ru. do.
[0043] The metal film 130 may be formed to a thickness in the range of 50 nm to 1000 nm. The thickness may be more than 1000 nm. It is preferable that the thickness is large.
[0044] (Black Film 140) The black film 140 is a black film. Note that the black color here means a film having a visible light reflectance of 30% or more. The color of the black film 140 is, for example, The black film 140 can be formed from only RuO2. The thickness of the film can be formed in the range of 100 nm or less. good.
[0045] Next, a method for producing the metal coating member 1 will be described. First, a composite ceramic member 110 is prepared. FIG. 3A shows the composite ceramic member 110. The composite ceramic member 110 is shown in an as-prepared state. The composite ceramic member 110 can be prepared by manufacturing the connecting member 112. Alternatively, instead of manufacturing the composite ceramic member 110, the composite ceramic member 110 may be prepared. You may prepare by reaching
[0046] The composite ceramic member 110 is formed by attaching the ceramic member to the connecting member 112 using, for example, an adhesive. As described above, the ceramic member 11 can be bonded to the ceramic member 11. The connecting member 112 can be integrally sintered to form the connecting member 112.
[0047] Next, a precious metal film 120 is provided on the composite ceramic member 110. FIG. The figure shows a state in which a precious metal film 120 is provided on a metal member 110. The precious metal film 120 is a composite The noble metal film 120 is formed on the surface of the ceramic member 110. The noble metal film 120 is provided on the upper or lower surface of the component 110. Not only the upper or lower surface of the member 110 but also, for example, the upper or lower surface to the side surface It may be provided over .
[0048] The precious metal film 120 is provided from the ceramic member 111 to the connection member 112. The noble metal film 120 is provided on the surface of the composite ceramic member 110. The precious metal film 120 is provided on a part of the entire surface of the composite ceramic member 110. The noble metal film 120 is formed on a part of the surface of the ceramic member 111 and on the connecting member 112. The surface area includes a portion of the surface of the substrate.
[0049] In addition, the precious metal film 120 has a connecting region where two regions having different adhesion strength to the precious metal are connected to each other. The noble metal film 120 is made of one or more metals selected from the group consisting of Pt, Au, Ag, and Rh. Two regions having different adhesion strengths to the precious metal above are provided in the continuous connecting region. The regions include regions with weak adhesion to the precious metal and regions with strong adhesion to the precious metal. In addition, since the ceramic member 111 and the connection member 112 have different adhesive strengths with the precious metal, Therefore, the region including the ceramic member 111 and the connection member 112 becomes a connection region.
[0050] The noble metal film 120 is formed on the surface of the composite ceramic member 110 by, for example, a sputtering method. It is also possible to form a film on the surface of the material by using a sputtering method or the like, so that the film has sufficient voids. When the precious metal film 120 is formed on the ceramic sintered body, the precious metal film 120 is formed on the uneven surface. The precious metal is deposited so as to fill the depressions according to their shape.
[0051] Next, a release film is provided on the precious metal film 120 provided on the composite ceramic member 110. FIG. 3C shows a state in which a release film is provided on the precious metal film 120. In the metal-coated member, the metal film 130 is a release film.
[0052] The release film is provided on the surface region. The release film is provided with a noble metal film 120. The region is provided from the ceramic member 111 to the connection member 112. The release film is provided on the connection region. The release film is formed by, for example, sputtering. The peeling film can be formed on the surface of the precious metal film 120 by the method. The film is formed using a metal different from the noble metal used in 120 .
[0053] Next, a black film 140 is provided on the release film. FIG. 3D shows a state where the black film 140 is provided on the release film. The black film 140 is formed on at least the composite ceramic member 110. On the precious metal film 120 and the peeling film provided in the area having a high adhesive strength with the precious metal, The black film 140 is formed on the surface of the release film by, for example, a sputtering method. It is possible.
[0054] Next, the ceramic member 1 is removed from the composite ceramic member 110 on which the precious metal film 120 is formed. The noble metal film 120 formed on the surface of the substrate 11 is removed. Accordingly, the release film and the black film 140 provided on the surface of the ceramic member 111 are also removed. will be done.
[0055] In addition, the noble metal film 120 formed on the composite ceramic member 110 is a ceramic member The ceramic member 111 and the connecting member 112 are connected to each other by a contact hole 114. The precious metal film 120 is removed. In addition, the precious metal film 12 provided on the composite ceramic member 110 is 0, the precious metal film 120 provided on the surface of the connection member 112 is not removed. A release film is provided on the precious metal film 120 provided on the surface of the connection member 112. Among the precious metal films 120 provided in the connection region of the composite ceramic member 110, Only the noble metal film 120 provided in the area where the adhesion to the metal is weak is removed.
[0056] The precious metal film 120 is removed by utilizing the difference in adhesion. The precious metal film 120 formed on the ceramic member 1 is a composite ceramic member having a precious metal film 120 formed thereon. The metal film 120 can be removed by vibrating the metal film 110. The ceramic member 111 can be removed by subjecting it to ultrasonic vibration or thermal shock.
[0057] Since the ceramic member 111 has a small adhesive strength with the precious metal, the composite ceramic member 110 When the precious metal film 120 is formed on the surface of the substrate, the precious metal is not sufficiently adhered to the substrate. The connecting member 112 has a strong adhesive force with the precious metal, so that the precious metal is not easily bonded to the composite ceramic member 110. When the metal film 120 is formed, it is in a state of sufficient adhesion to the precious metal. Therefore, the surface of the ceramic member 111 is not subjected to external forces such as vibration or ultrasonic vibration. Only the exposed noble metal film 120 is removed.
[0058] 4A and 4D are TEM images of the manufactured metal deposition member 1. 4A and 4C are scattered electron images, and FIGS. 4B and 4D are transmitted electron images.
[0059] In the metal-coated member 1 from which this image was obtained, the composite ceramic member 110 is made of a main material. A ceramic member 111 made of aluminum oxide and a ceramic member 112 made of aluminum oxide as the main material It is an integral sintered body formed from the connection member 112. The porosity of the connection member 112 is 10 %. The sintering conditions were adjusted to obtain a composite ceramic member 110 having a porosity of about 1.0. The thickness of the precious metal film 120 is 0.4 mm. The black film 140 was made of RuO2. The thickness of each film was set to 200 nm. The deposition rate was adjusted accordingly.
[0060] The TEM images of FIG. 4A and FIG. 4B show the vicinity of the boundary between the ceramic member 111 and the connection member 112. This is a result of analyzing the vicinity of the surface on which the noble metal film 120 is provided. The left side is the ceramic member 111, and the right side is the connection member 112. The connection member 112 has multiple While many voids are observed in the ceramic member 111, no voids are observed in the ceramic member 112. The connection member 112 has unevenness due to voids formed therein. The connection member 112 has a precious metal film 120, a release film, and , a black film 140 is formed.
[0061] As can be seen from the images of FIGS. 4A and 4B, the noble metal film 120 has an uneven surface. The ceramic member 11 is provided in the area where the projections and recesses are formed, and is removed from the area where the projections and recesses are not formed. A noble metal film 120 is formed on the surface of the connection member 112 along the boundary between the connection member 112 and the substrate 112. Furthermore, the area where the noble metal film 120 is provided and the area where the noble metal film 120 is not provided are different in surface area. The boundary between the area with and without bumps on the surface of the precious metal film 1 is clearly distinguishable. 20 coincides with the boundary between the ceramic member 111 and the connection member 112. The noble metal film 120 can be removed with high precision only from the ceramic member 111 .
[0062] On the surface on which the precious metal film 120 is provided, the ceramic member 111 and the connection member 112 The degree of unevenness varies. The surface roughness Rz (maximum height) of the surface is 0.05 μm or less. The surface roughness Rz of the surface on which the precious metal film 120 is provided is 0.10 μm or more. The difference in the surface roughness creates a difference in the adhesion to the precious metal, and the area where the precious metal film is to be formed is Can be controlled.
[0063] According to this manufacturing method, the region where the noble metal film 120 is provided and the region where the noble metal film 120 is not provided are different from each other. The boundary between the ceramic member 111 and the connection member 112 is set within 1000 nm from the boundary between the ceramic member 111 and the connection member 112. Alternatively, the region where the noble metal film 120 is provided and the region where the noble metal film 120 is provided may be different. The boundary between the ceramic member 111 and the connecting member 112 and the region where the ceramic member 111 and the connecting member 112 are not exposed is set to within 100 nm. Alternatively, the region where the noble metal film 120 is provided and the region where the noble metal film 120 is provided may be different from each other. The boundary between the ceramic member 111 and the connecting member 112 and the non-connected region is 50 n Alternatively, the region where the noble metal film 120 is provided and the region where the noble metal film 120 is provided may be provided within a range of 100 mm. The boundary between the ceramic member 111 and the connecting member 112 and the region not covered with the ceramic member 111 are They can be located in the same qualitative position.
[0064] Here, the boundary of the precious metal film 120 and the boundary between the ceramic member 111 and the connection member 112 are The degree of agreement between the two can be said to be highly accurate, but it cannot be said with certainty that there is no discrepancy at all. In light of this, the term "substantially the same position" is used herein. From D, it appears to match, and it is clear that the accuracy is high, but it is difficult to accurately measure the accuracy of the match. It is difficult to quantify. Here, "matching" means being in substantially the same position. "
[0065] The TEM images of FIGS. 4C and 4D are the results of analyzing the area where the noble metal film 120 is provided. The left end of FIG. 4C is the ceramic member 111 and the connection member 11 in FIG. 4A. 4C, the layers of the precious metal film 120, the release film, and the black film 140 are Although the noble metal film 120, the release film, and the black film 14 are not clearly visible in FIG. 4D, Each layer of 0 can be recognized.
[0066] As can be seen from the images of FIGS. 4C and 4D, the surface of the precious metal film 120 is uneven. The void is not inserted into the cavity, but is inserted into the cavity itself. Rather, the unevenness of the surface is a factor that increases the adhesive strength with the precious metal film 120. In other words, any method other than providing voids can be used to provide unevenness on the surface. In this case, it can be said that it is possible to increase the adhesive strength with the noble metal film 120.
[0067] The above describes the metal film member 1 and the manufacturing method thereof. Even if the ceramic member 111 is not heated, the precious metal film 120 formed on the surface of the ceramic member 111 can be removed. Therefore, the ceramic member 11 can be formed without a step of providing a release film. It is possible to carry out a step of removing the precious metal film 120 provided on the surface of the substrate 1. By providing the metal film 120, it becomes easier to remove the metal film 120. Therefore, the step of providing the black film 140 may be omitted.
[0068] The metal film member 1 can be used as an optical member, for example. When used as a component, the precious metal film 120 can be used as a light-shielding film. For example, when the ceramic member 111 is used as a light emission region, light leakage from the connection member 112 As a countermeasure against this, it is possible to provide a light-shielding film. This is not limited to this.
[0069] (Light emitting device) Next, a light emitting device 2 having a metal film member 1 as one of its components will be described. In the device 2, the metal film member 1 is used as a wavelength conversion member 280, which is an example of an optical member. .
[0070] The light emitting device 2 includes, as its components, a base 210, a light emitting element 220, a submount 230, Light reflecting member 240, protective element 250, temperature measuring element 260, wiring 270, wavelength conversion member 2 The light emitting device 2 includes a light-transmitting member 80, a light-transmitting member 290, and a light-shielding member 300. As an element, it has at least a light emitting element 220 and an optical member.
[0071] The light emitting device 2 also includes one or more light emitting elements 220. and the same number of light reflecting members 240 as the number of light emitting elements 220. Also, the device has one or more protection elements 250. Also, the device has one or more temperature measuring elements 26. 0. Also, it has one or more wirings 270.
[0072] Next, each component of the light emitting device 2 will be described. (base 210) The base 210 has a concave shape that is recessed from the top surface to the bottom surface. The base 210 has a top surface 211 and a bottom surface 212. , a lower surface 213 , a number of inner surfaces 214 , and one or more outer surfaces 215 . In addition, when viewed from above, a frame is formed by one or more inner surfaces 214 intersecting with the upper surface 211. The recess of the base 210 is surrounded by this frame.
[0073] In addition, the base 210 has one or more step portions 216 on the inside of the frame. The step portion 216 is composed only of an upper surface and a side surface that intersects with the upper surface and extends downward. The one or more inner surfaces 214 include a side surface that intersects with the upper surface 211 of the base portion 210 and a step portion 21 6 aspects and.
[0074] The base 210 may be formed primarily of ceramic. As the material, aluminum nitride, silicon nitride, aluminum oxide, and silicon carbide can be used. It should be noted that the main material is not limited to ceramic, and other insulating materials may also be used. Good too.
[0075] In addition, one or more metal films are provided on the bottom surface 212 of the base 210. The upper surface 211 of the semiconductor device 210 is provided with one or more metal films. The one or more metal films to be formed include a metal film electrically connected to the metal film provided on the upper surface 211. A membrane is included.
[0076] (Light emitting element 220) The light emitting element 220 is a semiconductor laser element. However, it does not have to be a semiconductor laser element. For example, light-emitting diodes (LEDs) and organic light-emitting diodes (OLEDs) Any element that can be used as the light emitting element 220 of the light emitting device 2 can be used. In the present embodiment, a semiconductor laser element 20 is employed as a light emitting element 220.
[0077] The semiconductor laser element 20 shown in the figure has a rectangular outer shape when viewed from above. The side surface intersecting with one of the two short sides is the emitting surface of the light emitted from the semiconductor laser element 20. The upper and lower surfaces of the semiconductor laser element 20 are larger in area than the light emitting end surface. stomach.
[0078] The light (laser light) emitted from the semiconductor laser element 20 has a spreading property. An elliptical far-field pattern (hereinafter referred to as "FFP") in a plane parallel to the end face. Here, FFP refers to the shape and light emitted from the light source at a position away from the light output facet. The intensity distribution is shown.
[0079] The light emitted from the semiconductor laser element 20 is distributed along an active region in a plane parallel to the light emission end face. An ellipse with the layer direction of multiple semiconductor layers as its minor axis and the stacking direction perpendicular to that as its major axis. The layer direction corresponding to the short axis is the horizontal direction of the FFP, and the stacking direction corresponding to the long axis is the The direction is called the vertical direction of the FFP.
[0080] Based on the light intensity distribution of the FFP of the semiconductor laser element 20, 1 / e 2 The light having the intensity above this level is called the main part of the light. The angle corresponding to the full width at half maximum of the fabric is called the divergence angle. The spread angle of the FFP in the horizontal direction is called the horizontal spread angle. This is called the bevel angle.
[0081] The light emitting element 220 has a peak emission wavelength of 320n Use a wavelength in the range of 430 nm to 530 nm, typically in the range of 430 nm to 480 nm. Such a semiconductor laser element 20 can be a semiconductor laser including a nitride semiconductor. Examples of nitride semiconductors include GaN, InGaN, and Al GaN can be used. However, the light emitted from the light emitting element 220 is not limited to this. It's good.
[0082] (Submount 230) The submount 230 is configured in a rectangular parallelepiped shape and has a bottom surface, a top surface, and side surfaces. The submount 230 has the smallest width in the vertical direction. The shape is not limited to a rectangular parallelepiped. The submount 230 may be made of, for example, silicon nitride, aluminum nitride, or silicon carbide. It is to be noted that other materials may be used. A metal film is provided on the surface.
[0083] (Light reflecting member 240) The light reflecting member 240 has a light reflecting surface 241 that reflects light. The light reflecting surface may include, for example, A surface is provided that has a light reflectance of 90% or more for the peak wavelength of the irradiated light. The light reflectance can be up to or less than 100%.
[0084] The light reflecting member 240 has a plurality of light reflecting surfaces 241. Each of them is flat and inclined with respect to the bottom surface, and the inclination angle with respect to the bottom surface is different from each other. The two light reflecting surfaces 241 are each oriented in a direction perpendicular to the bottom surface. The arrangement relationship between the two light reflecting surfaces 241 is neither perpendicular nor parallel. The shape of the light reflecting surface 241 is not limited to a flat shape. For example, the shape may be curved.
[0085] The light reflecting member 240 may be made of glass, metal, or the like as the main material forming its outer shape. The main material should be heat-resistant, such as quartz or BK7 (borosilicate glass). The material for the light reflecting surface may be glass, metal such as aluminum, or silicon. For example, metals such as Ag and Al, Ta2O5 / SiO2, TiO2 / SiO2, Nb2O5 It can be formed using a dielectric multilayer film such as SiO2.
[0086] (Protection element 250) The protective element 250 is a protection element that protects against damage caused by excessive current flowing through a specific element such as a light-emitting element. The protective element 250 is, for example, a ceramic made of Si. A core diode can be used.
[0087] (Temperature measuring element 260) The temperature measuring element 260 is an element used as a temperature sensor for measuring the surrounding temperature. The temperature measuring element 260 may be, for example, a thermistor.
[0088] (Wiring 270) The wiring 270 is used for electrical connection between the two components. The wiring 270 may be: For example, a metal wire can be used.
[0089] (Wavelength conversion member 280) The wavelength conversion member 280 is one form of the metal film member 1. The wavelength conversion member 280 is It has a wavelength conversion portion 281 , a light reflection portion 282 , and a light blocking film 283 .
[0090] The wavelength converting portion 281 of the wavelength converting member 280 is a ceramic of the metal deposition member 1. The light reflecting portion 282 in the wavelength conversion member 280 corresponds to the metal film member 111. The light-shielding film 283 in the wavelength conversion member 280 corresponds to the connection member 112 in the The wavelength conversion portion 281 corresponds to the precious metal film 120 in the film-formed member 1. 82 and the light-shielding film 283, the ceramic member 111, the connection member 112, and The same applies as for the noble metal film 120 .
[0091] The wavelength conversion member 280 is formed by providing a light-shielding film 283 on the surface of a base material. The light reflecting portion 281 and the light reflecting portion 282 are integrally formed to form the base material of the wavelength conversion member 280. The base material of the wavelength conversion member 280 is the composite ceramic portion of the metal film member 1. Therefore, the base material of the wavelength conversion member 280 is also a composite ceramic part. The same can be said about the material 110. In addition, the wavelength conversion member 280 further includes , a metal film 130 , or a black film 140 .
[0092] The wavelength conversion member 280 converts the incident light into light of a different wavelength and emits the converted light. In addition, the wavelength conversion member 280 emits a part of the incident light. The wavelength conversion member 80 may convert all the incident light into light of different wavelengths. In this case, The light incident on 80 does not exit from the wavelength conversion member 280 .
[0093] The wavelength conversion section 281 converts the light incident thereon into light of a different wavelength. The wavelength conversion portion 281 can be formed by using ceramics as a main material and by containing a phosphor. In order to prevent the wavelength conversion portion 281 from being deformed or discolored due to heat, the wavelength conversion portion 281 is fused. It is preferable to use a material with a melting point of 1300°C to 2500°C as the main material.
[0094] For example, the wavelength conversion unit 281 is formed by sintering a phosphor and a light-transmitting material such as aluminum oxide. The content of the phosphor is 0.05 parts by volume relative to the total volume of the ceramic. % to 50% by volume. Alternatively, the wavelength conversion section 281 may be made of ceramics made of only phosphor. The phosphor single crystal has low adhesion to the noble metal.
[0095] The phosphor used was cerium-activated yttrium aluminum garnet (Y AG), cerium-activated lutetium aluminum garnet (LAG), Nitrogen-containing calcium aluminosilicate (CaO-Al) activated with rhodium and / or chromium 2O3-SiO2), europium activated silicate ((Sr,Ba)2SiO4), Examples of such phosphors include α-sialon phosphors and β-sialon phosphors. The YAG phosphor is a phosphor that can emit white light in combination with blue excitation light. It is preferable to use
[0096] The light reflecting portion 282 reflects the light irradiated from the wavelength converting portion 281 toward the light reflecting portion 282. The inner surface of the light reflecting portion 282 contacts the side surface of the wavelength converting portion 281. The wavelength conversion unit 282 converts light incident on the wavelength conversion unit 281 or light converted by the wavelength conversion unit 281. The converted light is reflected by the inner surface of the light reflecting portion 282 .
[0097] The light reflecting portion 282 can be formed by using ceramics as the main material. However, metals and composites of ceramics and metals may also be used. An example of the ceramic material is alumina (Al2O3).
[0098] In addition, the light reflecting portion 282 is made of a material with high thermal conductivity that can dissipate heat generated by the wavelength converting portion 281. The light reflecting portion 282, which is mainly made of a material with high thermal conductivity, It has a heat dissipation function to exhaust heat in the conversion part 281, and from this viewpoint, instead of the light reflection part 282 It can also be considered a heat dissipation material. Alumina (Al2O3) is a ceramic with high thermal conductivity. It is a material.
[0099] The wavelength conversion member 280 has a wavelength conversion portion 281 and a light reflecting portion 282 that form a base material thereof. Light is irradiated during operation of the device 2. Therefore, the base material of the wavelength conversion member 280 is irradiated with light. It is preferable to use an inorganic material, which is less likely to decompose, as the main material. It doesn't have to be.
[0100] (Translucent member 290) The light-transmitting member 290 has a lower surface, an upper surface, and a side surface. It has a light-transmitting property that transmits light. Here, light-transmitting property means that the light transmittance is 80% or more. The light-transmitting member 290 has a base material formed in a rectangular parallelepiped flat plate shape. The shape is not limited to a rectangular parallelepiped.
[0101] The base material of the light-transmitting member 290 can be formed by using sapphire as the main material. The fiber is a material with relatively high transmittance and strength. Other than fiber, for example, quartz, silicon carbide, or glass may also be used.
[0102] (Light blocking member 300) The light blocking member 300 is made of a resin having light blocking properties. It exhibits the property of not transmitting light, blocking light, absorbing light, and reflecting light. For example, a filler such as a light diffusing material and / or a light absorbing material may be added to the resin. It can be formed by containing
[0103] The resin for forming the light blocking member 300 may be an epoxy resin, a silicone resin, an acrylate resin, or the like. resin, urethane resin, phenolic resin, BT resin, etc. The filler may be a dark color pigment such as carbon black.
[0104] Next, a light emitting device 2 manufactured using these components will be described. First, two light reflecting members 240 are disposed on the bottom surface 212 of the base 210. The members 240 are disposed on different metal films, and their lower surfaces are in contact with the bottom surface 21 of the base 210. 2. The two light reflecting members 240 are arranged symmetrically with respect to the point SP. (See FIG. 11). In addition, the upper ends of the light reflecting surfaces 241 of the two light reflecting members 240 are aligned in a top view. , parallel or perpendicular to the inner surface 214 or the outer surface 215 of the base 210 .
[0105] Next, a protection element 250 and a temperature measuring element 260 are disposed on the bottom surface 212 of the base 210. The protective element 250 is a metal film on which one of the two light reflecting members 240 is disposed. The temperature measuring element 260 is disposed on the metal plate 210 on which the two light reflecting members 240 are disposed. The metal film is disposed on and bonded to a different metal film.
[0106] Next, two submounts 230 are placed on the bottom surface 212 of the base 210. The mounts 230 are disposed on different metal films, and their lower surfaces are aligned with the bottom surface of the base 210. 212. In addition, each of the two submounts 230 has a light reflecting member 240. The submount 230 and the light reflecting member 240 are disposed on the metal film. They may be disposed on different metal films.
[0107] The light emitting device 220 is then placed on the submount 230. In the embodiment, the semiconductor laser element 20 is mounted on a submount 230. The laser elements 20 are mounted on the upper surfaces of different submounts 230, and their lower surfaces are bonded to each other. The two semiconductor laser elements 20 are arranged symmetrically with respect to the point SP. That is, the two semiconductor laser elements 20 are symmetrical to each other and the two light reflecting members 240 are symmetrical to each other. In the following explanation, this point SP will be called the symmetric point. .
[0108] The two semiconductor laser elements 20 have their emission end faces extending to the inner surface 214 of the base portion 210 when viewed from above. Therefore, the upper end of the light reflecting surface 241 is not parallel or perpendicular to the outer surface 215. In other words, the semiconductor laser element 20 is arranged so that the inner side of the base portion 210 is not aligned vertically. The light emitting end surface is inclined with respect to the surface 214 and the outer surface 215, or the upper end of the light reflecting surface 241. are arranged so that
[0109] Instead of disposing the semiconductor laser element 20 at an angle, the light reflecting member 240 is disposed at an angle. That is, the semiconductor laser element 20 may be disposed on the inner surface 214 of the base portion 210. Alternatively, the light reflecting member 240 may be arranged parallel or perpendicular to the outer surface 215. The devices may be arranged so that
[0110] The light emitted from the output end face of each of the two semiconductor laser elements 20 is divided into corresponding light The light is irradiated onto the reflecting member 240. The corresponding light reflecting member 240 is disposed on the same metal film. The light reflecting member 240 is configured so that at least a major portion of the light is irradiated onto the light reflecting surface 241. The semiconductor laser element 20 is disposed as shown in FIG.
[0111] In addition, between the corresponding semiconductor laser element 20 and the light reflecting member 240, the light reflecting member 240 The semiconductor laser element 20 is located farther from the symmetrical point than the semiconductor laser element 21. The light emitted from the light emitting element 20 travels in a direction approaching the symmetric point. At least one of them is disposed in a position close to the temperature measuring element 260. The temperature of the element 220 can be measured well.
[0112] The submount 230 on which the light emitting element 220 is disposed is a light emitting element 22 The submount 230 serves as a heat dissipation member that dissipates heat generated from the In order to function as a heat dissipation member, it is necessary to form the light emitting element 220 from a material having a higher thermal conductivity than the light emitting element 220. Also, if the material has a higher thermal conductivity than the bottom surface of the base, a higher heat dissipation effect can be obtained. It is possible.
[0113] In addition, the submount 230 supports the light emission of the semiconductor laser element 20 in the light emitting device 2. For example, the light passing through the optical axis can be aligned horizontally with the bottom surface 212. When it is desired to irradiate a predetermined position on the light reflecting surface 241, the submount is used as an adjustment member.
[0114] Next, the light emitting element 220, the protection element 250, and the temperature measuring element 260 are electrically connected. For electrical connection, a plurality of wirings 270 are bonded to the bottom surface 212 of the base 210. As a result, the metal film on the upper surface 211 of the base 210 is used. These elements can be electrically connected to an external power source.
[0115] Next, the light-transmitting member 290 is placed on the upper surface of the base 210. The lower surface of the light-transmitting member 290 is joined to the base 210. The light-transmitting member 290 is bonded to the base portion 210, whereby the semiconductor laser element 2 In this manner, in the light emitting device 2, the light-transmitting member 290 is a lid. This closed space is formed in an airtight sealed state. By hermetically sealing the semiconductor laser element 20, organic matter and the like are prevented from collecting on the light emitting end face of the semiconductor laser element 20. This can prevent the above from happening.
[0116] In addition, a wavelength conversion member 280 is disposed on the upper surface of the light-transmitting member 290. 280 is joined to the light-transmitting member 290. When the light-transmitting member 290 is joined to the base portion 210, In this case, the wavelength conversion member 280 is already bonded to the light-transmitting member 290. 290 is bonded to the base 210, and then the wavelength conversion member 280 is bonded to the light-transmitting member 290. Good too.
[0117] A major portion of the light emitted by the light emitting element 220 enters the light-transmitting member 290. The optical member 290 is transparent to the light emitted by the light emitting element 220. The main part of the light is incident on the wavelength conversion member 280. The main part of the light passes through the light-transmitting member 290 and enters the wavelength conversion portion 281 of the light-transmitting member 290. After passing through the wavelength conversion member 280 , the light is incident on the wavelength conversion member 280 .
[0118] The wavelength conversion member 280 has a light entrance area on its lower surface where the main part of the light is incident, and In addition, in the wavelength conversion member 280, the wavelength conversion portion 281 is a light incident portion. The light from the light emitting element 220 or the wavelength-converted light is reflected by the wavelength conversion unit 28. The light is emitted from the upper surface of the wavelength conversion portion 281 to the outside of the light emitting device 2. This serves as the light extraction surface of the device 2.
[0119] The light-shielding film 283 is provided on the upper surface side of the wavelength conversion member 280. The light-shielding film 283 is provided on the light-extraction surface side of the optical device 2. The light-shielding film 283 is provided on the upper surface of the light-reflecting portion 282. The boundary of the light-shielding film 283 is a wavelength conversion portion 281 that is a light extraction surface and a light reflection portion 282. The light shielding film 283 formed with high precision by the precious metal film 120 is It is possible to suppress leakage of light from other than the wavelength conversion portion 281, which is the surface, and to achieve excellent light emission quality. The device 2 can be realized.
[0120] For example, when the light emitting device 2 or the wavelength conversion member 280 is mass-produced, ceramic is used as the main material. The shape of the wavelength conversion portion 281 varies. In comparison with the method of providing a light-shielding film in a region, the method of the embodiment is free from such shape variations. The effect on the accuracy of the light-shielding film can be reduced.
[0121] Moreover, the light-shielding film 283 is preferably formed to a thickness in the range of 50 nm to 500 nm. By forming the film in this range, the film can function as a light-shielding film sufficiently with an appropriate amount of precious metal. It can be achieved in minutes.
[0122] In the case of the wavelength conversion member 280 in which the black film 140 is further provided on the light-shielding film 283, The light emitting device 2 absorbs light, such as return light, traveling from the outside of the light emitting device 2 toward the light emitting device 2. In other words, such light is reflected by the light-shielding film 283 and the metal film 130. By providing the black film 140, reflection of return light and the like can be suppressed.
[0123] In addition, if the heat generated by the wavelength conversion is concentrated in a specific location, the light from the wavelength conversion unit 281 may be reduced. Since the conversion efficiency is likely to decrease, it is better for the distribution of light incident on the wavelength conversion unit 281 to be diffused. For example, the light intensity of the laser light emitted from each of the two semiconductor laser elements 20 is For example, the light reflecting surface 241 of the light reflecting member 240 may be Such control is possible by adjusting
[0124] The upper surface of the light-transmitting member 290 is larger than the lower surface of the wavelength conversion member 280. In the top view, the upper surface of the light-transmitting member 290 surrounds the lower surface of the wavelength conversion member 280. Alternatively, It surrounds the wavelength converting member 280 .
[0125] Next, the light-shielding member 300 is formed inside the frame formed by the upper surface 211 of the base 210. The member 300 is formed so as to fill the gap between the base 210 and the wavelength conversion member 280. The light blocking member 300 is formed, for example, by pouring a thermosetting resin and curing it with heat. By providing the light blocking member 300, leakage of light is suppressed.
[0126] The light blocking member 300 is formed by an inner surface 214 that intersects with the upper surface 211 of the base 210 and a step of the base 210. The upper surface of the light-transmitting member 216, the side surface of the light-transmitting member 290, the upper surface of the light-transmitting member 290, and the wavelength conversion portion The wavelength conversion member 280 is in contact with the side surface of the member 280, and does not reach the top surface of the member 280. Even if it reaches the upper surface of the light reflecting portion 282, it does not reach the upper surface of the wavelength converting portion 281. However, the light shielding member 300 can shield the boundary between the wavelength conversion portion 281 and the light reflection portion 282 with high accuracy. It is difficult to realize light from the light-extracting surface, so by combining it with the light-shielding film 283, The leakage can be suppressed with high precision.
[0127] As explained above, the present invention having the technical features disclosed in the specification is For example, the present invention is not limited to the structure described in the embodiment. The present invention can also be applied to devices having elements, and the like, and the like that differ from the disclosed structure. The existence of a problem is not a reason for not being able to apply the present invention. From the viewpoint of the minimum components for performing the above-mentioned operation, the device disclosed in the embodiment has It can be said that some of the components are not essential.
[0128] This means that the devices and the like disclosed in the embodiments of this specification are In addition to the viewpoint of disclosure of a reasonable configuration assuming one form of use, While the application of the invention is not limited to the exemplary forms of use, There are also aspects that work more effectively when applied to different usage patterns.
[0129] In view of this, the present invention (claims) discloses the following in one embodiment. It may not be necessary to include all of the elements described in the claims. Some components of the device disclosed in the embodiment are not described in the following. In this case, the components are not limited to those disclosed in the present embodiment, and may be replaced, omitted, The freedom of design by those skilled in the art, such as modification of the shape and change of materials, is recognized, and a patent claim is made. It is claimed that the invention described in the claims applies. [Industrial Applicability]
[0130] The metal film member and the light emitting device described in the embodiment can be used in an in-vehicle headlight. In other words, the vehicle headlight can be said to be one application form to which the present invention can be applied. The present invention is not limited to this, but may be applied to lighting, projectors, head-mounted displays, and the like. The present invention can also be used as a light source for backlighting of other displays. The uses of the metal film member are not limited to these, and it can be used in a wide variety of applications. . [Explanation of symbols]
[0131] 1 Metal deposition materials 110 Composite ceramic components 111 Ceramic components 112 Connection member 120 Precious metal film 130 Metal Film 140 Black Film 2. Light-emitting device 210 base 211 Top surface 212 Bottom 213 Bottom surface 214 Inner surface 215 External surface 216 Step 220 Light emitting element 230 Submount 240 Light reflecting material 241 Light reflective surface 250 Protection element 260 Temperature measuring element 270 Wiring 280 Wavelength conversion material 281 Wavelength conversion unit 282 Light reflecting part 283 Light-shielding film 290 Translucent material 300 Light-shielding material
Claims
1. A first ceramic member; a second ceramic member connected to the first ceramic member; a precious metal film formed on a surface of the second ceramic member along a boundary between the first ceramic member and the second ceramic member; The second ceramic member is a metal film-formed member having a surface roughness Rz of 0.10 μm or more on which the precious metal film is formed.
2. 2. The metal coated member according to claim 1, wherein the first ceramic member and the second ceramic member are integrally sintered to form an integrated sintered body.
3. The metal coated member according to claim 1 or 2, wherein the second ceramic member has a larger porosity than the first ceramic member.
4. 4. The metal deposited member according to claim 1, wherein the precious metal film contains one or more precious metals selected from the group consisting of Pt, Au, Ag, and Rh.
5. A wavelength conversion unit; A connection member made mainly of ceramic and connected to the wavelength conversion unit; a light-shielding film formed on a surface of the connection member along a boundary between the wavelength conversion unit and the connection member, the light-shielding film is a precious metal film, The connection member is a wavelength conversion member, the surface on which the noble metal film is formed having a surface roughness Rz of 0.10 μm or more.
6. The wavelength conversion member according to claim 5 , wherein the wavelength conversion portion is made of a sintered ceramic or a single crystal of a phosphor.
7. The wavelength conversion member according to claim 5 , wherein the noble metal film contains one or more noble metals selected from the group consisting of Pt, Au, Ag, and Rh.
8. A light-emitting element; a package in which the light emitting element is disposed; a wavelength converting member having a wavelength converting portion, a connection member made mainly of ceramic and connected to the wavelength converting portion, and a light-shielding film formed on a surface of the connection member, the wavelength converting member being directly or indirectly connected to the package; Equipped with the light-shielding film is a precious metal film formed on a surface of the connection member along a boundary between the wavelength conversion unit and the connection member, The connecting member has a surface on which the precious metal film is formed having a surface roughness Rz of 0.10 μm or more.
9. The light emitting device according to claim 8 , wherein the wavelength conversion portion is made of a sintered ceramic or a single crystal of a phosphor.
10. 10. The light emitting device according to claim 8, wherein the noble metal film contains one or more noble metals selected from the group consisting of Pt, Au, Ag, and Rh.
Citation Information
Patent Citations
Communication optimizing method for parallel program
JP1995073150A
Hard carbon film, and its depositing method
JP2006161075A
Conductive pattern forming method by direct irradiation of electromagnetic wave, and resin structure having conductive pattern
JP2016529713A
Optical component, light-emitting device using optical component, and method for manufacturing optical component
JP2019053130A
Semiconductor light-emitting device and manufacturing method of the same
JP2013232539A