Porous composite material capable of generating electrical arc in micro wave field, preparation method thereof, and usage thereof

A porous composite material generates an electric arc in a microwave field for high-temperature pyrolysis, addressing inefficiencies in current recycling methods by producing valuable chemical raw materials from plastics, rubber, and carbon fiber composites.

JP2024133574AInactive Publication Date: 2024-10-02CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024107304
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2018-10-29
Filing Date
2024-07-03
Publication Date
2024-10-02
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Current methods for recycling plastics, rubber, and carbon fiber composites are inefficient, costly, and environmentally harmful, and existing microwave pyrolysis technologies fail to achieve high temperatures and product selectivity.

Method used

A porous composite material composed of an inorganic porous framework and carbon material, capable of generating an electric arc in a microwave field, is used for rapid high-temperature pyrolysis of organic compounds, allowing for efficient recycling and resource recovery.

Benefits of technology

The porous composite material achieves rapid and efficient pyrolysis of plastics, rubber, and carbon fiber composites, producing valuable chemical raw materials and enabling effective recycling with minimal environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133574000001
    Figure 2024133574000001
  • Figure 2024133574000002
    Figure 2024133574000002
  • Figure 2024133574000003
    Figure 2024133574000003
Patent Text Reader

Abstract

To provide porous composite material capable of generating electric arc in a micro wave field, a preparation method thereof, and usage thereof.SOLUTION: Porous composite material including inorganic porous skeletons and carbon material supported on the inorganic porous skeleton, of which average pore diameter of the inorganic porous skeletons is 0.2 to 1000 μm, wherein the carbon material is selected from produced material through carbonization of graphene, carbon nano tube, graphite, carbon black, carbon fiber, carbon dot, carbon nano wire, carbonizable organic material or carbonizable mixture, and a group made of combinations of those.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

Detailed Description of the Invention

[0001] FIELD OF THEINVENTION The present invention relates to the fields of microwave heating, microwave high-temperature pyrolysis and waste resource utilization. In particular, the present invention relates to a porous composite material capable of generating an arc in a microwave field, a preparation method therefor and its use, and a method for pyrolyzing and / or recycling materials containing organic compounds.

[0002] [Background technology] More than 90% of chemical raw materials are derived from fossil energy sources such as petroleum, shale gas, and coal. However, fossil energy is non-renewable and generates CO2 during its use. Therefore, the development of environmentally friendly renewable energy has currently become one of the focuses in the energy sector. For a more sustainable economic and social development, it is urgent to replace fossil energy with renewable biomass energy. Among them, vegetable oils have been the subject of research due to their characteristics such as low price and large-scale cultivation. From 2012 to 2013, 462 million tons of major vegetable oils, including palm oil, rapeseed oil, sunflower oil, and soybean oil, were produced worldwide. In recent years, due to the rapid development of pyrolysis technology, pyrolysis technology has become one of the relatively efficient and mature biomass utilization technologies.

[0003] In another aspect, since the 1950s, humanity has produced 8.3 billion tons of plastic, of which 6.3 billion tons are waste. Of the 6.3 billion tons of waste plastic, 9% has been recycled, 12% has been incinerated, and the remaining 79% (about 5.5 billion tons) has been landfilled and accumulated in the natural environment. Humanity is still accelerating the rate of plastic production. Currently, the annual production of plastic has reached 400 million tons. It is estimated that there will be 12 billion tons of waste plastic in the world by 2050. More than 8 million tons of plastic are dumped into the ocean every year. If no restrictions are imposed, there will be more plastic trash in the ocean than fish by 2050. In recent years, top-tier international publications have been published one after another on the pollution of marine and river organisms and drinking water by plastic particles. The pollution of marine and river organisms and drinking water by plastic particles has aroused the interest of society as a whole in plastic pollution. In 2018, the United Nations Environment Programme focused for the first time on the problem of pollution by disposable plastics. In addition, the United Nations Environment Programme announced "Stop Plastic Pollution" as the theme for World Environment Day, calling for a "declaration of war" on plastic pollution around the world.

[0004] In order to solve the problem of plastic pollution, scientific researchers have made continuous efforts. Since 1970, many researches have been directed to the preparation of plastics that can be decomposed in natural environments. However, degradable plastics only have important applications in biomedicine, agricultural mulch films and garbage bags, etc., and when recycling is required, the presence of degradable plastics has a significant impact on the performance of recycled plastic articles. In addition, degradable plastics take a relatively long time to decompose in non-ideal natural environments, and therefore cannot effectively solve the problem of white pollution.

[0005] Currently, mechanical recycling is the only widely used technical solution for treating waste plastics. The main steps are the continuous removal of organic residues, washing, crushing, and melting and reprocessing. In the melting and reprocessing process, it is generally necessary to blend new materials to maintain performance. Different plastics react differently to the treatment process, which means that the technical solution of mechanical recycling is only applicable to a very small number of types of plastics. Currently, only polyethylene terephthalate (PET) and polyethylene (PE) are recycled, accounting for 9% and 37% of annual plastic production, respectively. Temperature-sensitive plastics, composites, and plastics that do not melt and flow at high temperatures (such as thermosetting plastics) cannot be treated in this way.

[0006] Chemical recycling, the preparation of waste plastics into small molecular hydrocarbons (gas, liquid oil or solid wax) by chemical or thermal conversion, is considered a technological solution that outperforms mechanical recycling. The products obtained can then be used as fuels or chemical feedstocks. However, this technological solution is not currently widely used, mainly due to its high cost. On the one hand, most chemical recycling processes require expensive catalysts. Also, the selectivity of the catalyst requires that the feedstock must be pure polymers, which requires time-consuming and labor-intensive sorting of the waste plastics. On the other hand, chemical recycling processes consume a lot of energy.

[0007] In addition, with the rapid development of the world economy, rubber materials are widely used in various industries, and the demand for rubber products is also increasing. The emergence of automobiles has brought great convenience to human production and life, and promoted the development of society. At the same time, it has also brought about a hidden danger that is difficult to ignore, namely the deterioration of environmental and resource problems. As the production of automobiles increases year by year, the consumption of resources and the amount of waste tires continue to increase. China has a vast territory and population and is a large country that uses tires. Waste tires occupy a lot of land resources and environmental space, and are not only not easy to compress and purify for the unknown time required for the decomposition of waste tires, but also difficult to biodegrade. Waste tires are called "black pollution" because they cause great harm to the environment and are difficult to process. There is an urgent need to reuse waste rubber resources.

[0008] According to another aspect, carbon fiber composite materials have excellent properties such as light weight, high strength, and good corrosion resistance. Carbon fiber composite materials are widely used in high-tech fields such as aerospace, new energy, automotive industry, and sporting goods. With the popularity of carbon fiber composite materials, the amount of carbon fiber composite waste generated is increasing day by day. A large amount of carbon fiber composite waste has attracted people's attention, which has a great impact on environmental protection and economic benefits. With the increasing interest in environmental protection and international situations, it has become the cause of the energy and resource crisis. In addition, the carbon fiber in carbon fiber composite materials is expensive and has excellent comprehensive performance, so the research of carbon fiber recycling technology is an important development trend in the future.

[0009] Current carbon fiber recycling technologies mainly include physical recycling and chemical recycling. The physical recycling method involves crushing and melting carbon fiber composite waste, which is the raw material for new materials. However, this method impairs the properties of various components of the composite material, in particular, carbon fibers cannot be obtained from it, and recyclability cannot be achieved. Chemical recycling is a method of recycling carbon fibers from carbon fiber composite waste using pyrolysis or organic solvent decomposition. Reuse by organic solvent decomposition can obtain clean carbon fibers. However, a large amount of organic solvent is used for recycling, which causes environmental pollution. Separation of used solvents (liquid separation, extraction, distillation, etc.) is complicated in operation and results in high recycling costs. In addition, this method is also selective in the type of matrix resin and the type of curing agent of carbon fiber reinforced resin composites, and is not suitable for all matrix resins. The most industrially feasible one disclosed in the prior art is the pyrolysis of carbon fiber composites. However, traditional heating methods generally have low efficiency and too high energy costs.

[0010] Printed circuit boards (PCBs) are essential components of almost all electronic information products and are widely used in various industrial fields such as electronic components and electrical control. As a substrate material in PCB manufacturing, copper clad laminates are mainly composed of three parts: substrate, copper foil and adhesive. The substrate is composed of polymer synthetic resin and reinforcing material. The adhesive is usually phenolic resin, epoxy resin, polyimide resin, cyanate ester resin, polyphenylene ether resin, etc. In the year 2000, the annual production of copper clad laminates reached 160,100 tons. In 2006, China's printed circuit board output surpassed Japan, becoming the world's most productive printed circuit board manufacturer. Up to now, about 40% of the world's PCBs are produced in China, but the amount of waste printed circuit boards (WPCBs) is also huge. Existing WPCB processing methods such as mechanical processing and acid dissolution mainly focus on recycling metals in circuit boards, but rarely involve effective recycling of non-metallic components in circuit boards, and moreover, most of these methods pose a great threat to environmental safety. Therefore, devising an efficient WPCB treatment method for cleaning is one of the key issues in current research.

[0011] Microwave refers to electromagnetic waves with wavelengths between infrared and ultra-high frequency (UHF) radio waves, with very strong penetrating ability, with wavelengths between 1m and 1mm, and corresponding frequencies between 300GHz and 300MHz. The magnetron of the microwave generator receives the output of a power source to generate microwaves. The microwaves are transmitted to the microwave heater through a waveguide. Then, the material to be heated is heated under the action of the microwave field. The microwave heating mode is quite different from normal heat transfer. The high frequency electric field periodically changes the applied electric field and direction at a rate of hundreds of millions per second. As a result, the polar molecules in the material vibrate at high frequencies due to the electric field as well as due to the friction and squeezing action between the molecules. The material is heated rapidly, which causes the internal and surface temperatures of the material to increase rapidly at the same time.

[0012] In recent years, microwave pyrolysis technology without catalysts has been developed. It can simultaneously process and pyrolyze waste plastics that are contaminated to a certain extent, such as the currently most commonly used polyethylene, polypropylene, polyester, polystyrene, and polyvinyl chloride, into chemical raw materials. In addition, microwave pyrolysis is also used to pyrolyze waste rubber into monomers and then repolymerize them for use. Therefore, it is expected that microwave pyrolysis technology will be the key to solving the problem of plastic pollution and reusing rubber resources.

[0013] Numerous patents, such as patent application CN102585860A, patent application CN103252226A, patent application CN106520176A, etc., disclose the technology of pyrolysis using this property of microwaves. However, they all use ordinary microwave-sensitive materials such as silicon carbide to generate heat in the microwave field and transfer heat to the material to be pyrolyzed, thereby achieving the pyrolysis purpose. Such methods cannot achieve high working temperatures, ideal efficiency and product composition. Therefore, it is still necessary to develop microwave heating materials that can rapidly generate high temperatures in the microwave field and transfer heat to the material. It is also still necessary to develop an efficient method for microwave high-temperature pyrolysis of waste plastics, waste rubber, biomass or vegetable oil. It is also still necessary to develop an efficient method for microwave high-temperature pyrolysis of carbon fiber composite materials and recycling of carbon fibers, as well as a method for microwave high-temperature pyrolysis of circuit boards to achieve effective resource recycling. The development of such materials and methods has great application prospects.

[0014] DISCLOSURE OF THEINVENTION In view of the problems of the prior art, the object of the present invention is to provide a porous composite material, as well as its preparation method and use. The porous composite material can generate an electric arc in a microwave field to rapidly generate high temperatures (e.g., within tens of seconds to several minutes) (especially above 1000°C). Thereby, effective microwave high-temperature heating or microwave pyrolysis of organic compound-containing materials (e.g., plastics such as polyethylene, polypropylene and polystyrene; rubber; vegetable oil; biomass; carbon fiber composites; circuit boards) is achieved, and the useful substances in the pyrolysis products are recycled as chemical raw materials or for application in other aspects. In addition, the porous composite material itself can withstand high temperatures and is suitable for industrial applications.

[0015] Another object of the present invention is to provide a method for producing a porous composite material that is simple and easy to implement and readily amenable to large scale production.

[0016] Another object of the present invention is to achieve efficient operation by using the porous composite material to perform microwave high-temperature heating or microwave pyrolysis of organic compound-containing materials. The pyrolysis products can achieve high added value, especially mainly light components (especially gas phase or small molecule gas).

[0017] Another object of the present invention is to provide a method for microwave high-temperature pyrolysis of circuit boards to achieve effective recycling of resources. The pyrolysis gas products can be gases with high recycling value, and the solid residue can easily realize separation of metal components and non-metal components. The solid residue can also easily realize efficient recovery of metals and glass fibers. This realizes clean and efficient recovery of all components of waste circuit boards.

[0018] The above objects of the present invention can be achieved by a porous composite material capable of generating an electric arc in a microwave field, the porous composite material comprising an inorganic porous framework and a carbon material supported on the inorganic porous framework.

[0019] Specifically, according to a first aspect of the present invention, there is provided a porous composite material capable of generating an electric arc in a microwave field, comprising an inorganic porous skeleton and a carbon material supported on the inorganic porous skeleton, the inorganic porous skeleton having an average pore size of 0.2 to 1000 μm.

[0020] Here, "supported" means that the carbon material is fixed to the surface and / or structure of the inorganic porous framework by specific binding forces, where surface means all interfaces of the porous framework that can be in contact with the gas phase, and "immobilized" means embedded or fixed inside the porous framework itself, rather than inside the pore channels.

[0021] An electric arc refers to a gas discharge phenomenon, which is a beam of high-temperature ionized gas and is also a type of plasma.

[0022] The carbon material may be at least one selected from the group consisting of graphene, carbon nanotubes, carbon nanofibers, graphite, carbon black, carbon fibers, carbon dots, carbon nanowires, products obtained by carbonization of carbonizable organic substances, and products after carbonization of mixtures of carbonizable organic substances; preferably from the group consisting of graphene, carbon nanotubes, products obtained by carbonization of carbonizable organic substances, and products after carbonization of mixtures of carbonizable organic substances.

[0023] Carbonization is a process in which organic matter is treated under certain temperature and atmospheric conditions to volatilize all or most of the hydrogen, oxygen, nitrogen, sulfur, etc. contained in the organic matter, thereby obtaining synthetic raw materials with a high carbon content.

[0024] Carbonizable organic matter refers to organic polymeric compounds including synthetic and natural organic polymeric compounds; The synthetic organic polymeric compound is preferably at least one selected from the group consisting of rubber or plastics, including thermosetting plastics and thermoplastics, more preferably epoxy resins, phenolic resins, furan resins, polystyrene, styrene-divinylbenzene copolymers, polyacrylonitrile, polyaniline, polypyrrole, polythiophene, styrene-butadiene rubber, and polyurethane rubber; The natural organic polymeric compound is preferably at least one selected from the group consisting of starch, viscose fiber, lignin and cellulose.

[0025] The mixture containing carbonizable organic matter refers to a mixture of carbonizable organic material with other metal-free organic materials and / or metal-free inorganic materials, preferably at least one selected from the group consisting of coal, natural pitch, petroleum pitch or coal tar pitch.

[0026] The proportion of the carbon material can be 0.001% to 99%, preferably 0.01% to 90%, and more preferably 0.1% to 80%, based on the total mass of the porous composite material.

[0027] The inorganic porous skeleton refers to an inorganic material having a porous structure. The average pore size of the inorganic porous skeleton is 0.2 to 1000 μm, preferably 0.2 to 500 μm, more preferably 0.5 to 500 μm, particularly preferably 0.5 to 250 μm, or 0.2 to 250 μm. The porosity of the inorganic porous skeleton may be 1% to 99.99%, preferably 10% to 99.9%, more preferably 30% to 99%.

[0028] Here, the average pore size is measured by a scanning electron microscope (SEM). First, the pore size of each pore is determined by the minimum distance between two intersections of a line passing through the center of each pore and the outline of the pore in the SEM photograph. Then, the average pore size is determined by the number average value of the pore size values ​​of all pores shown in the SEM photograph.

[0029] The porosity is determined with reference to GB / T 23561.4-2009.

[0030] The inorganic material may be one or more combinations of carbon, silicate, aluminate, borate, phosphate, germanate, titanate, oxide, nitride, carbide, boride, sulfide, silicide and halide, preferably one or more combinations of carbon, silicate, titanate, oxide, carbide, nitride and boride. Here, the oxide may be at least one selected from the group consisting of aluminum oxide, silicon oxide, zirconium oxide, magnesium oxide, cerium oxide and titanium oxide. Also, the nitride may be at least one selected from the group consisting of silicon nitride, boron nitride, zirconium nitride, hafnium nitride and tantalum nitride. The carbide may be at least one selected from the group consisting of silicon carbide, zirconium carbide, hafnium carbide and tantalum carbide. The boride may be at least one selected from the group consisting of zirconium boride, hafnium boride and tantalum boride. The inorganic material of the inorganic porous framework is more preferably at least one selected from the group consisting of carbon, silicate, aluminum oxide, magnesium oxide, zirconium oxide, silicon carbide, boron nitride, and potassium titanate.

[0031] Preferably, the inorganic porous skeleton is at least one of the following skeletons: a carbon skeleton obtained after carbonization of a polymer sponge, a porous skeleton composed of inorganic fibers, an inorganic sponge skeleton, a skeleton composed of inorganic particles, a ceramic porous skeleton obtained after baking a ceramic porous skeleton precursor, a ceramic fiber skeleton obtained after baking a ceramic fiber skeleton precursor; preferably a skeleton obtained after carbonization of a melamine sponge, a skeleton obtained after carbonization of a phenolic resin sponge, a porous skeleton of aluminum silicate fibers (such as aluminum silicate rock wool), a porous skeleton of mullite fibers, a porous skeleton of alumina fibers (such as alumina fiberboard), a porous skeleton of zirconia fibers, a porous skeleton of magnesium oxide fibers, a porous skeleton of boron nitride fibers, a porous skeleton of boron carbide fibers, a porous skeleton of silicon carbide fibers, a porous skeleton of potassium titanate fibers, and a ceramic fiber skeleton obtained after baking a ceramic fiber skeleton precursor.

[0032] The porous structure of the inorganic porous skeleton may be derived from the pore structure of the skeleton material itself, such as a sponge-like structural form, or the pore structure formed by filling with fibrous materials, such as fiber cotton, fiber felt, fiberboard, and other structural forms, or the pore structure formed by filling with granular materials, such as sand pile structural forms, or a combination of the above various forms. The porous structure of the inorganic porous skeleton is preferably derived from the pore structure formed by filling with fibrous materials. Particular attention should be paid to the porous skeleton composed of inorganic fibers as described above. The term "porous" therein refers to the pore structure in the skeleton formed by filling with fibrous materials, but does not mean that the fibers themselves are porous.

[0033] The porous composite material according to the invention is capable of generating a high temperature electric arc in a microwave field, for example in a microwave field of 900 w. The porous composite material is capable of generating an electric arc that can raise its temperature above 1000° C., and the porous composite material itself can withstand high temperatures up to 3000° C. This porous composite material according to the invention capable of generating an electric arc in a microwave field is an efficient microwave heating material.

[0034] <Preparation method> According to a second aspect of the present invention, there is provided a method for preparing a porous and composite material, the method comprising the steps of: Step (1): immersing an inorganic porous framework or an inorganic porous framework precursor into a solution or dispersion of a carbon material and / or a carbon material precursor such that the pores of the inorganic porous framework or the inorganic porous framework precursor are filled with the solution or dispersion; Step (2): A step of heating and drying the porous material obtained in step (1) to precipitate or solidify a carbon material or a carbon material precursor on the inorganic porous skeleton or the inorganic porous skeleton precursor, thereby supporting the carbon material or the carbon material precursor; Step (3): When at least one of a carbon material precursor and an inorganic porous skeleton precursor is used as a starting material, the following step is further carried out: heating the porous material obtained in step (2) under an inert gas atmosphere to convert the inorganic porous skeleton precursor into an inorganic porous skeleton, and / or reducing or carbonizing the carbon material precursor.

[0035] The solution or dispersion of the carbonaceous material or its precursor in step (1) may comprise a solvent selected from the following: benzene, toluene, xylene, trichlorobenzene, chloroform, cyclohexane, ethyl caproate, butyl acetate, carbon disulfide, ketones, acetone, cyclohexanone, tetrahydrofuran, dimethylformamide, water and alcohol; where the alcohol is preferably at least one selected from the group consisting of propanol, n-butanol, isobutanol, ethylene glycol, propylene glycol, 1,4-butanediol, isopropanol and ethanol.

[0036] The carbon material precursor for support used in the manufacturing method of the present invention is preferably a precursor that can be dissolved or dispersed in a human- and environmentally friendly solvent before being supported, and therefore the preparation process is "earth-friendly". The human- and environmentally friendly solvent is at least one selected from the group consisting of ethanol, water, and mixtures thereof. That is, the solvent in step a is more preferably a solvent containing water and / or ethanol, and even more preferably water and / or ethanol.

[0037] The solution or dispersion only needs to achieve sufficient dissolution or sufficient dispersion of the carbon material and / or carbon material precursor in the solvent. In general, the concentration may be 0.001 to 1 g / mL, preferably 0.002 to 0.8 g / mL, and more preferably 0.003 to 0.5 g / mL.

[0038] The heating and drying in step (2) can be carried out at a temperature of 50 to 250°C, preferably 60 to 200°C, more preferably 80 to 180°C, and is preferably performed by microwave heating. The microwave output may be 1 W to 100 KW, preferably 500 W to 10 KW. The microwave heating time can be 2 to 200 minutes, preferably 20 to 200 minutes.

[0039] The inorganic porous scaffold precursor is a porous material that can be converted into an inorganic porous scaffold and can be at least one selected from the group consisting of ceramic precursors, porous materials of carbonizable organic materials or porous materials of mixtures of carbonizable organic materials.

[0040] The carbon material precursor may be at least one of graphene oxide, modified carbon nanotubes, modified carbon nanofibers, modified graphite, modified carbon black, modified carbon fiber, and carbonizable organic matter or a mixture containing carbonizable organic matter. Modified carbon nanotubes, modified carbon nanofibers, modified graphite, modified carbon black, and modified carbon fiber refer to carbon materials that are pretreated to improve the dispersibility of these carbon materials in water or organic solvents and obtain a stable dispersion. For example, pretreatment with dispersants and surfactants, or pretreatment by grafting hydrophilic groups, etc. All of these pretreatment means are adopted as pretreatment means for improving dispersibility in the prior art. All of the above pretreated carbon materials are commercially available, including aqueous graphene dispersions, ethanol dispersions of graphene, aqueous graphene slurry, oil-based graphene slurry, aqueous dispersions of graphene oxide, ethanol dispersions of graphene oxide, N-methylpyrrolidone dispersions of graphene oxide, aqueous dispersions of graphene oxide, aqueous dispersions of carbon nanotubes, aqueous dispersions of carboxylated carbon nanotubes, ethanol dispersions of carbon nanotubes, dimethylformamide dispersions of carbon nanotubes, and N-methylpyrrolidone slurry of carbon nanotubes.

[0041] The heating temperature in step (3) may be 400 to 1800°C, preferably 600 to 1500°C, and more preferably 800 to 1200°C, and microwave heating is preferred. The microwave output may be 100 W to 100 KW, and preferably 700 W to 20 KW. The microwave heating time may be 0.5 to 200 minutes, and preferably 1 to 100 minutes.

[0042] In one embodiment, the preparation method comprises the steps of: a. preparing a solution or dispersion of a supporting carbon material or a carbon material precursor; b. a step of immersing an inorganic porous skeleton or an inorganic porous skeleton precursor in the solution or dispersion of step a, whereby the pores of the inorganic porous skeleton or inorganic porous skeleton precursor are filled with said solution or dispersion, in which the carbon material and / or carbon material precursor comprises 0.001% to 99.999%, preferably 0.01% to 99.99%, and more preferably 0.1% to 99.9% of the total mass of the inorganic porous skeleton material or inorganic porous skeleton material precursor and the carbon material and / or carbon material precursor; c. The porous material obtained in step b is taken out, then heated and dried to precipitate or solidify the carbon material or carbon material precursor and support it on the inorganic porous skeleton or inorganic porous skeleton precursor; the heating and drying temperature is 50-250°C, preferably 60-200°C, more preferably 80-180°C; When the starting materials are a carbon material and an inorganic porous framework, the method includes, after step c, a step of obtaining a porous composite material capable of generating an electric arc in a microwave field; Furthermore, when the starting material used comprises at least one of a carbon material precursor or an inorganic porous framework precursor, the following step d is carried out; d. heating the porous material obtained in step c under an inert gas atmosphere to convert the inorganic porous framework precursor into an inorganic porous framework and / or reduce or carbonize the carbon material precursor, thereby obtaining a porous composite material that can generate an electric arc in a microwave field; the heating temperature is 400-1800°C, preferably 600-1500°C, more preferably 800-1200°C.

[0043] In the production method of the present invention, when the carbon material supported on the inorganic porous skeleton is graphene, it is preferable to use an aqueous solution of graphene oxide in step (1) or step a.

[0044] When the carbon material supported on the inorganic porous skeleton is carbon nanotubes, it is preferable to use a dispersion of carbon nanotubes in step (1) or step a.

[0045] When thermosetting plastic is selected as the carbon material precursor for support, in step (1) or step a, a suitable curing system needs to be prepared according to the conventional curing agent of the thermosetting plastic selected in the prior art. In the curing system, any one or more additives selected from the following group can be added: curing accelerator, dye, pigment, colorant, antioxidant, stabilizer, plasticizer, lubricant, flow control agent or assistant, flame retardant, anti-dripping agent, anti-caking agent, adhesion promoter, conductive agent, polyvalent metal ion, impact control agent, release assistant, nucleating agent, etc. The amount of additives used may be a normal amount, and can be adjusted according to the actual conditions. When thermosetting plastic is selected as the carbon material precursor for support, after heating in step c, the thermosetting resin used as the carbon material precursor is cured and supported on the inorganic porous skeleton.

[0046] When a thermosetting plastic is selected as the supporting carbon material precursor, in step (1) or step a, a corresponding good solvent in the prior art is selected to dissolve the thermosetting plastic and its curing system to obtain the supporting carbon material precursor solution.

[0047] When selecting a thermoplastic material as the supporting carbon material precursor, the supporting carbon material precursor solution can be added with antioxidants, co-antioxidants, heat stabilizers, light stabilizers, ozone stabilizers, processing aids, plasticizers, softeners, antiblocking agents, foaming agents, dyes, pigments, waxes, extenders, organic acids, flame retardants, silane coupling agents and other additives commonly used in the prior art during plastic processing. The amount of additives used can be the conventional amount or can be adjusted according to the actual situation.

[0048] In the preparation method according to the invention, the pores of the inorganic porous framework can be filled with a solution or dispersion of the supporting carbon material or a precursor of the carbon material by squeezing several times or not at all.

[0049] In step (2) of the production method of the present invention, after the porous material obtained in step (1) is taken out, a measure may or may not be taken to remove excess solution or dispersion of the carbon material or carbon material precursor to be supported in the porous material obtained in step (1). The above measurement includes, but is not limited to, one or two of a squeezing operation and a centrifugation operation.

[0050] The heating in steps (2) and (3) of the preparation method according to the present invention may preferably be microwave heating, which is not only efficient but also can achieve uniform heating.

[0051] Specifically, in step (2), the microwave output may be from 1 W to 100 KW, and preferably from 500 W to 10 KW, and the microwave irradiation time is from 2 to 200 minutes, and preferably from 20 to 200 minutes.

[0052] In the step (3), the microwave output may be 100 W to 100 KW, preferably 700 W to 20 KW, and the microwave irradiation time is 0.5 to 200 minutes, preferably 1 to 100 minutes.

[0053] The heating in step (3) of the production method of the present invention must be carried out under an inert gas atmosphere, which is selected from inert gas atmospheres commonly used in the prior art, preferably nitrogen.

[0054] The apparatus used in the preparation methods according to the present invention is all common.

[0055] <Application Examples> The porous composite material according to the present invention unexpectedly exhibits excellent mechanical properties due to the combination of inorganic porous framework and carbon material. The porous composite material according to the present invention can generate an electric arc to rapidly generate high temperature in a microwave field, for example a 900w microwave field. The porous composite material according to the present invention can generate an electric arc that can increase the temperature of the porous composite material to more than 1000°C. This allows the porous composite material to be used in fields such as microwave high-temperature heating, biomass pyrolysis, vegetable oil treatment, waste polymer material pyrolysis, petrochemical pyrolysis, carbon fiber composite material recycling, garbage treatment, VOC waste gas treatment, COD wastewater treatment, and high-temperature catalysis. At the same time, the porous composite material itself is resistant to high temperatures, and its preparation process is simple and easy to carry out, which makes it easy to realize large-scale preparation.

[0056] Thus, according to a third aspect, the present invention provides the use of a porous composite material according to the present invention for microwave high-temperature heating, pyrolysis and recycling of substances containing organic compounds (e.g. organic matter, mixtures containing organic matter or composite materials containing organic matter), high-temperature catalysis and other fields, in particular for biomass pyrolysis, vegetable oil treatment, waste polymer material pyrolysis, petrochemical pyrolysis, carbon fiber composite material recycling, garbage treatment, VOC waste gas treatment or COD wastewater treatment.

[0057] In petrochemical manufacturing processes, petroleum fractional distillation products (including petroleum gas) are commonly used as feedstocks, and petrochemical pyrolysis means where temperatures are used rather than thermal cracking to break down the long-chain hydrocarbon molecules into a variety of short-chain gaseous hydrocarbons and small amounts of liquid hydrocarbons to provide organic chemical feedstocks.

[0058] The porous composite material according to the invention may be particularly suitable for pyrolyzing and / or recycling substances containing organic compounds.

[0059] Thus, according to a fourth aspect, the present invention provides a method for pyrolyzing and / or recycling a material comprising an organic compound. The material comprising an organic compound is contacted with a porous composite material according to the present invention under an inert atmosphere or under vacuum, and a microwave field is applied to said material comprising the organic compound and the porous composite material. The porous composite material generates an electric arc in the microwave field, thereby rapidly reaching a high temperature and pyrolyzing the material comprising the organic compound.

[0060] The organic compound-containing materials include organic materials, mixtures containing organic materials, and composite materials containing organic materials, which may be selected, for example, from the following: -Waste plastics; here, waste plastics refers to plastics and their mixtures that have been used for civilian, industrial and other purposes. Examples of waste plastics include, but are not limited to: Specifically, at least one of polyolefins, polyesters (such as at least one of polyethylene terephthalate, polybutylene terephthalate, and polyarylate, and mixtures thereof), polyamides, acrylonitrile-butadiene-styrene terpolymers, polycarbonates, polylactic acid, polyurethanes, polymethyl methacrylate, polyoxymethylene, polyoxymethylene ethers, and polyphenylene sulfides; preferably at least one of polyethylene and mixtures thereof (including, but not limited to, at least one of low density polyethylene, medium density polyethylene, high density polyethylene, and ultra-high molecular weight polyethylene), polypropylene and mixtures thereof, polyvinyl chloride and mixtures thereof, polyethylene terephthalate, polystyrene and mixtures thereof (including, but not limited to, normal polystyrene, expanded polystyrene, high impact polystyrene, and syndiotactic polystyrene), polyamides, acrylonitrile-butadiene-styrene terpolymers, polycarbonates, polylactic acid, polymethyl methacrylate, and polyoxymethylene; more preferably at least one of polyethylene, polypropylene, polyvinyl chloride, polyethylene terephthalate, polystyrene, polycarbonate, and polyamides. The waste plastics can be mixed together and directly processed without separation, thereby simplifying the processing procedure of the waste plastics, except that the waste plastics need to be processed according to type when there are special requirements for the decomposition products.

[0061] -Waste rubber; here, waste rubber refers to rubber and their mixtures for civilian, industrial and other purposes that have been used and finally discarded or replaced, preferably at least one of natural rubber, butadiene rubber, styrene butadiene rubber, nitrile rubber, isoprene rubber, ethylene propylene rubber, butyl rubber, neoprene, styrene-based block copolymer and silicone rubber, more preferably at least one of natural rubber, butadiene rubber, styrene butadiene rubber, isoprene rubber and ethylene propylene rubber. Waste rubbers are mixed together and directly processed without sorting, thereby simplifying the processing procedure of waste rubber; however, in the case where there are special requirements for decomposition products, waste rubber needs to be processed according to type.

[0062] -Biomass; where biomass refers to various animals, plants, and algae produced by photosynthesis that are primarily composed of cellulose, hemicellulose, and lignin, including, but not limited to, at least one of straw, bagasse, tree branches, leaves, wood chips, rice husks, rice stalks, straw, peanut shells, coconut shells, palm husks, walnut shells, macadamia nut shells, pistachio shells, wheat straw, corn stalks, and corn cobs.

[0063] -vegetable oil; here, in this specification, vegetable oil refers to oils and fats obtained from the fruits, seeds and germs of plants, and mixtures thereof.Oils and fats obtained from the fruits, seeds and germs of plants include, but are not limited to, at least one of palm oil, rapeseed oil, sunflower oil, soybean oil, peanut oil, linseed oil and castor oil, preferably at least one of palm oil, rapeseed oil, sunflower oil and soybean oil.

[0064] carbon fiber composites, where the carbon fiber composites are preferably carbon fiber reinforced polymer composites in the prior art, the polymer matrix composited with the carbon fibers includes, but is not limited to, at least one of polyethylene, polypropylene, nylon, phenolic resin and epoxy resin.

[0065] - circuit board; here the circuit board can be any of the various circuit boards produced in the current state of the art.

[0066] In the case of carbon fiber composites, a microwave field is applied to the carbon fiber composite and the porous composite in an inert atmosphere or vacuum, and the porous composite generates an electric arc in the microwave field, thereby rapidly reaching a high temperature to pyrolyze the polymer matrix in the carbon fiber composite, while the carbon fibers remain and are recycled.

[0067] In the case of a circuit board, the circuit board is in contact with the porous composite material, and a microwave field is applied to the circuit board and the porous composite material under an inert atmosphere or vacuum. The porous composite material generates an electric arc under microwaves and rapidly reaches a high temperature, thereby pyrolyzing organic materials such as polymeric synthetic resins in the circuit board, and obtaining a large amount of gas products, which are flammable gases with high calorific value, and solid residues. The solid residues include metal components with loose structure and easy separation, and non-metal components, mainly glass fiber mixtures.

[0068] The weight ratio of the substance containing an organic compound to the porous composite material may be 1:99 to 99:1, preferably 1:50 to 50:1, more preferably 1:30 to 30:1, more preferably 1:10 to 10:1.

[0069] The microwave power of the microwave field can be 1W to 100KW, more preferably 100W to 50KW, more preferably 200W to 50KW, more preferably 500W to 20KW, most preferably 700W to 20KW, especially for example 700W, 900W or 1500W. The duration of microwave irradiation can be 0.1 to 200 minutes, more preferably 0.5 to 150 minutes, most preferably 1 to 100 minutes. An electric arc is generated in the microwave field and can reach 700 to 3000°C, preferably 800 to 2500°C, more preferably 800 to 2000°C quickly. This causes the organic compounds in the organic compound-containing material to be pyrolyzed.

[0070] For example, the microwave output for pyrolysis of palm oil can be 200W to 80KW, preferably 300W to 50KW, and the microwave irradiation time can be 0.2 to 200 minutes, preferably 0.3 to 150 minutes. The microwave output for pyrolysis of rapeseed oil can be 100W to 50KW, preferably 200W to 30KW, and the microwave irradiation time can be 0.1 to 150 minutes, preferably 0.2 to 130 minutes. The microwave output for pyrolysis of sunflower oil can be 80W to 60KW, preferably 200W to 40KW, and the microwave irradiation time can be 0.3 to 120 minutes, preferably 0.4 to 100 minutes. The microwave output for pyrolysis of soybean oil can be 120W to 40KW, preferably 200W to 30KW, and the microwave irradiation time can be 0.2 to 100 minutes, preferably 0.5 to 90 minutes. The microwave power for pyrolyzing peanut oil can be 100W to 10KW, preferably 300W to 8KW, and the microwave irradiation time can be 0.3 to 100 minutes, preferably 0.5 to 90 minutes. The microwave power for pyrolyzing linseed oil can be 150W to 80KW, preferably 300W to 50KW, and the microwave irradiation time can be 0.1 to 80 minutes, preferably 0.3 to 70 minutes. The microwave power for pyrolyzing castor oil can be 200W to 50KW, preferably 300W to 40KW, and the microwave irradiation time can be 0.5 to 70 minutes, preferably 0.6 to 60 minutes. The microwave power for pyrolyzing straw can be 100W to 70KW, and the microwave irradiation time can be 0.2 to 150 minutes. The microwave power for pyrolyzing bagasse can be 80W-50KW, and the microwave irradiation time can be 0.2-120 minutes. The microwave power for pyrolyzing tree branches can be 120W-100KW, and the microwave irradiation time can be 0.5-200 minutes. The microwave power for pyrolyzing leaves can be 50W-40KW, and the microwave irradiation time can be 0.1-80 minutes. The microwave power for pyrolyzing wood chips can be 100W-10KW, and the microwave irradiation time can be 0.2-100 minutes.The microwave power for pyrolysis of rice husk can be 80W-80KW, and the microwave irradiation time can be 0.2-120 minutes. The microwave power for pyrolysis of rice stalk can be 100W-70KW, and the microwave irradiation time can be 0.2-100 minutes. The microwave power for pyrolysis of rice straw can be 50W-60KW, and the microwave irradiation time can be 0.2-60 minutes. The microwave power for pyrolysis of peanut shell can be 100W-50KW, and the microwave irradiation time can be 0.3-70 minutes. The microwave power for pyrolysis of coconut shell can be 200W-80KW, and the microwave irradiation time can be 0.5-150 minutes. The microwave power for pyrolysis of palm kernel husk can be 100W-50KW, and the microwave irradiation time can be 0.3-100 minutes. The microwave power for pyrolysis of corncob can be 80W-50KW, and the microwave irradiation time can be 0.2-70 minutes. The microwave power for pyrolysis of natural rubber can be 100W-50KW, and the microwave irradiation time can be 0.5-150 minutes. The microwave power for pyrolysis of butadiene rubber can be 120W-60KW, and the microwave irradiation time can be 0.5-120 minutes. The microwave power for pyrolysis of styrene butadiene rubber can be 150W-80KW, and the microwave irradiation time can be 0.6-200 minutes. The microwave power for pyrolysis of isoprene rubber can be 100W-60KW, and the microwave irradiation time can be 0.5-150 minutes. The microwave power for pyrolysis of ethylene propylene rubber can be 200W-70KW, and the microwave irradiation time can be 0.2-100 minutes.

[0071] The microwave field can be generated by a variety of microwave devices in the prior art, such as a domestic microwave oven, industrialized microwave devices (such as microwave pyrolysis reactors), etc.

[0072] The inert atmosphere is an inert gas atmosphere commonly used in the prior art, such as nitrogen, helium, neon, argon, krypton, or xenon, preferably nitrogen.

[0073] The organic compound-containing material and the porous composite material can be contacted in various ways. When the organic compound-containing material is a solid, such as waste plastic, the material can be placed on the porous composite material, placed in the cavity formed by the porous composite material, or covered by the porous composite material, etc., and preferably the solid material (e.g., a circuit board) is crushed and then contacted with the porous composite material. When the organic compound-containing material is a liquid, such as vegetable oil, one useful mode is batch mode, i.e., vegetable oil is added to the porous composite material first. In that case, the porous composite material automatically absorbs the vegetable oil into the pores. Then, microwave pyrolysis is performed. Another useful mode is continuous mode. That is, during microwave pyrolysis, a pump (such as a peristaltic pump) is used to continuously add vegetable oil to the surface of the porous material through a quartz pipe. The above pumping speed only needs to ensure the residence time of the mixture of vegetable oil and porous composite material in the microwave field. When the organic compound-containing material is a mixture of solid and liquid, the above-mentioned contact mode mixing form can be adopted correspondingly.

[0074] In the method of the present invention, the equipment used to place or transport the organic compound-containing material and the porous composite material can be microwave transparent and can withstand high temperatures of over 1200°C, and the equipment can be various containers or pipes such as quartz crucibles, quartz reactors, quartz tubes, alumina crucibles, alumina reactors, alumina tubes, etc.

[0075] The organic compound-containing material in the method of the present invention is gasified after pyrolysis. The gas obtained after pyrolysis can be collected for subsequent processing or recycling, for example, after separation, the gas is used as fuel for subsequent reactions and production, or as chemical industrial raw materials. The residue after pyrolysis is discarded as waste, or for carbon fiber composite materials, the residue after pyrolysis is mainly carbon fiber, which can be recovered and reused after removing impurities, or for circuit boards, the solid residue obtained from the pyrolysis of the circuit board can be treated to separate the metal and non-metal components therein and recycled respectively. The above separation of the solid residue can adopt various separation methods and devices in the prior art.

[0076] Gas collection is a common method in the prior art and can be carried out using a gas collection device, preferably under an inert atmosphere. For example, when a domestic microwave oven is used as the microwave oven, a quartz crucible filled with a substance consisting of an organic compound and a porous composite material is placed in a vacuum bag and sealed in a nitrogen-protected glove box. After reacting under microwaves, the crucible is opened across the vacuum bag and a syringe is pushed into the vacuum bag for sampling. When an industrial microwave oven (such as a microwave pyrolysis reactor) with a gas inlet and a gas exhaust is used, the gas collection mode is such that purging with nitrogen is carried out during the reaction process, and sampling and collection by a gas collection bag are carried out at the gas exhaust.

[0077] The method of the present invention utilizes a porous composite material to generate an electric arc in a microwave field, which rapidly generates high temperatures to pyrolyze materials including organic compounds. The pyrolysis products can be used as chemical raw materials for recycling, or valuable residues such as carbon fibers or metals left after pyrolysis can be recycled, especially complete recycling of waste circuit boards can be achieved. The method is efficient and the product composition has high added value.

[0078] [Example] The present invention will be further described with reference to the following examples, but the scope of the present invention is not limited to these examples.

[0079] The experimental data in the examples were measured using the following instruments and measurement methods: 1. Determination of the mass percentage of carbon material supported in a porous composite material: 1) When an inorganic porous framework material was used as the starting material, the weight of the inorganic porous framework material was measured first, and then the weight of the resulting porous composite material was measured. The difference between the two weights was taken as the weight of the supporting carbon material, and the mass percentage of the carbon material supported in the porous composite material was calculated.

[0080] 2) When an inorganic porous skeleton precursor was used as the starting material, two samples of the inorganic porous skeleton precursor of the same weight were used. One of them was used in the examples of the present invention, and the other was used in the reference example in which only steps c and d of the above preparation method were carried out. After the experiment was completed, the weight of the porous composite material obtained in the examples was weighed, and the final weight of the sample obtained in the reference example was weighed. The difference between the two weights was taken as the weight of the supported carbon material, and the mass percentage of the carbon material supported in the porous composite material was calculated. 2. In the following examples and comparative examples, unless otherwise specified, the chromatographic analysis of the pyrolyzed gas was carried out using an Agilent 6890N gas chromatograph manufactured by Agilent (USA). The Agilent 6890N gas chromatograph used was equipped with an FID detector, an HP-PLOT AL2O3 capillary column (50 m x 0.53 mm x 15 μm) as a chromatographic column, He as a carrier gas, a linear velocity of 41 cm / s, an inlet temperature of 200°C, a detector temperature of 250°C, a split ratio of 15:1, an injected sample volume of 0.25 ml (gas), and a temperature rise program, with the initial temperature being maintained at 55°C for 3 minutes, then increased to 120°C at 4°C / min and maintained for 4 minutes, and then further increased to 170°C at 20°C / min and maintained for 10 minutes. 3. The average pore size of the inorganic porous scaffolds and porous composite materials was determined as follows. The pore size of each pore was determined by the minimum distance between two intersection points of lines passing through the center of each pore and the outline of the pore in a scanning electron microscope (SEM) photograph. The average pore size was then determined by averaging the pore size values ​​of all pores shown in the SEM photograph. The SEM used was a Hitachi S-4800 (Hitachi, Japan) with a magnification of 200x. 4. The porosity was determined with reference to GB / T 23561.4-2009.

[0081] All starting materials used in the examples were commercially available.

[0082] <Preparation of porous composite materials> [Example 1] (1) 500 ml of an aqueous dispersion of graphene oxide (JCGO-95-1-2.6-W, 10 mg / ml, Nanjing Ji Cang Nano Tech Co, LTD.) was weighed into a beaker; (2) 2 g of a porous scaffold made of phenolic resin (phenolic foam, average pore size 300 μm, porosity 99%, Choshu Smithers-Oesis Floral Foam Co., Ltd.) was immersed in an aqueous dispersion of graphene oxide. As a result, the dispersion fully penetrated into the pore channels of the porous scaffold; (3) The soaked porous material was taken out and placed on a stainless steel tray, which was then placed in an oven at 180°C and heated for 1 hour, thereby drying and pre-reducing the material; (4) The dried porous material was placed in a domestic microwave oven (700w, M1-L213B model, Midea) and microwaved at high power for 2 min to reduce the pre-reduced graphene oxide to graphene and carbonize the phenolic resin skeleton to a carbon skeleton (average pore size 200 μm, porosity 99%). This resulted in a porous composite with graphene supported on a carbon porous skeleton that can generate an electric arc in a microwave field. Graphene constituted 10% of the total mass of the porous composite.

[0083] [Example 2] (1) 500 ml of a dispersion of carbon nanotubes (XFWDM, 100 mg / ml, Nanjing XFNANO Materials Tech Co, Ltd.) was measured and placed in a beaker; (2) 2 g of a porous scaffold made of phenolic resin (phenolic foam, average pore size 200 μm, porosity 99%, Choshu Smithers-Oesis Floral Foam Co., Ltd.) was immersed in the dispersion of carbon nanotubes. As a result, the dispersion of carbon nanotubes was fully absorbed into the pore channels of the porous scaffold; (3) The soaked porous material was removed and placed on a stainless steel tray, which was placed in an oven at 80°C and heated for 5 hours, thereby drying the material; (4) The dried porous material was placed in a tubular furnace and carbonized at 800 °C for 1 h under a nitrogen atmosphere, resulting in a porous composite material with carbon nanotubes supported on a carbon porous skeleton (average pore size of the carbon skeleton was 140 μm, porosity was 99%) that could generate an electric arc in a microwave field. The carbon nanotubes comprised 30% of the total mass of the porous composite material.

[0084] [Example 3] (1) 500 ml of a dispersion of carbon nanotubes (XFWDM, 100 mg / ml, Nanjing XFNANO Materials Tech Co, Ltd.) was weighed out and placed into a beaker; (2) 5 g of fibrous cotton-like porous scaffold composed of silicate (average pore size 150 μm, porosity 90%, Shandong Luyang Energy-Saving Materials Co., Ltd.) was immersed in the carbon nanotube dispersion and squeezed several times to ensure that the dispersion was fully introduced into the pore channels of the porous scaffold; (3) The soaked porous material was removed, placed on a stainless steel tray, and placed in an oven at 150°C for 2 hours and dried to obtain a porous composite material with carbon nanotubes supported on a silicate fiber porous scaffold that can generate electric arcs in a microwave field. The carbon nanotubes comprised 10% of the total mass of the porous composite material.

[0085] [Example 4] (1) Weigh out 30 g of powdered phenolic resin (2123, Xinxiang Bomafengfan Industry Co, Ltd.) and 3.6 g of hexamethylenetetramine hardener, put them into a beaker, pour in 500 ml of ethanol, and stir with a magnetic stirrer for 1 hour until all the components are dissolved; (2) 5 g of fibrous cotton-like porous scaffold made of silicate (average pore size 150 μm, porosity 90% Shandong Luyang Energy-saving Materials Co, Ltd.) was immersed in the compounded solution and squeezed several times, so that the solution was fully penetrated into the pore channels of the porous scaffold; (3) The soaked porous material was removed and placed on a stainless steel tray, then placed in a furnace at 180°C and heated for 2 hours to dry the material, remove the solvent, and cure the phenolic resin; (4) The dried and hardened porous material was placed in a tubular furnace and carbonized at 1000 °C for 1 h under nitrogen atmosphere to carbonize the phenolic resin and obtain a porous composite material with phenolic resin carbonized supported on a silicate fiber porous framework that can generate an electric arc in a microwave field. The carbon material constituted 5% of the total mass of the porous composite material.

[0086] [Example 5] (1) 50 g of liquid phenolic resin (2152, Jining Baiyi Chemicals) was weighed out and placed in a beaker, and 500 ml of ethanol was poured in and stirred with a magnetic stirrer for 1 hour to dissolve; (2) 8 g of a plate-shaped porous scaffold made of alumina (average pore size 100 μm, porosity 85%, Shandong Luyang Energy-Saving Materials Co., Ltd.) was immersed in the blended solution. As a result, the solution fully penetrated into the pore channels of the porous scaffold; (3) The soaked porous material was removed and placed on a stainless steel tray, then placed in a furnace at 180°C and heated for 2 hours to dry the material, remove the solvent, and cure the phenolic resin; (4) The dried and hardened porous material was placed in a tubular furnace and carbonized at 900 °C for 1 h under nitrogen atmosphere to carbonize the phenolic resin and obtain a porous composite material with phenolic resin carbide supported on an alumina fiber porous skeleton that can generate an electric arc in a microwave field. The carbon material constituted 6% of the total mass of the porous composite material.

[0087] [Example 6] (1) Weigh out 30 g of water-soluble starch (pharmaceutical grade, product number: S104454, Shanghai Aladdin Biochemical Technology Co., Ltd.) and place it in a beaker, pour in 500 ml of deionized water, and stir with a magnetic rotor for 1 hour to dissolve; (2) 8 g of a fibrous mat-like porous scaffold made of alumina (average pore size 100 μm, porosity 85%, Shandong Luyang Energy-Saving Materials Co., Ltd.) was immersed in the blended solution. As a result, the solution fully penetrated into the pore channels of the porous scaffold; (3) The soaked porous material was taken out and placed into a microwave pyrolysis reactor (XOLJ-2000N, Nanjing Atpio Instrument Manufacturing Co, Ltd.), microwave treated at a power of 10 KW for 2 minutes, and the porous material was dried; (4) The dried porous material was placed in a tubular furnace and carbonized at 1200 °C for 1 h under nitrogen atmosphere to carbonize the water-soluble starch and obtain a porous composite material supported on an alumina fiber porous framework that can generate an electric arc in a microwave field. The carbon material constituted 0.1% of the total mass of the porous composite material.

[0088] [Example 7] (1) 50 g of water-soluble starch (pharmaceutical grade, product number: S104454, Shanghai Aladdin Biochemical Technology Co., Ltd.) was weighed out and placed in a beaker, and 500 ml of deionized water was poured in and stirred with a magnetic rotor for 1 hour to dissolve; (2) 8 g of a fibrous floss-like porous scaffold made of alumina (average pore size 100 μm, porosity 85%, Shandong Luyang Energy-Saving Materials Co., Ltd.) was immersed in the blended solution and squeezed several times, so that the solution fully penetrated into the pore channels of the porous scaffold; (3) The soaked porous material was taken out and placed into a microwave pyrolysis reactor (XOLJ-2000N, Nanjing Atpio Instrument Manufacturing Co, Ltd.), and treated by microwave at a power of 500 W for 2 hours, and the porous material was dried; (4) The dried porous material was placed in a tubular furnace and carbonized at 1000 °C for 1 h under nitrogen atmosphere to carbonize the starch, resulting in a porous composite material supported on an alumina fiber porous framework that can generate an electric arc in a microwave field. The carbon material constituted 0.2% of the total mass of the porous composite material.

[0089] [Example 8] (1) 2 kg of liquid phenolic resin (2152, Jining Baiyi Chemicals) was weighed and placed in a beaker, and 4 L of ethanol was poured in and stirred with a magnetic stirrer for 1 hour to dissolve; (2) 2 g of a porous scaffold made of phenolic resin (phenolic foam, average pore size 500 μm, porosity 99%, Choshu Smithers-Oesis Floral Foam Co., Ltd.) was immersed in the blended solution. As a result, the solution sufficiently penetrated into the pore channels of the porous scaffold; (3) The soaked porous material was removed and placed on a stainless steel tray, which was placed in an oven at 150°C and heated for 2 hours, thereby drying the material; (4) The dried porous material was placed in a microwave pyrolysis reactor (XOLJ-2000N, Nanjing Atpio Instrument Manufacturing Co, Ltd.) and microwave-treated under nitrogen atmosphere for 100 minutes at a power of 20KW, and an electric arc could be generated in the microwave field to obtain a porous composite material with phenolic resin carbide supported on a carbon porous skeleton (the carbon skeleton has an average pore size of 350μm and a porosity of 99%). The carbon material supported on the inorganic carbon skeleton constituted 80% of the total mass of the porous composite material.

[0090] [Example 9] (1) Weigh out 0.3 g of liquid phenolic resin (2152, Jining Baiyi Chemicals) and place it in a beaker, pour in 100 ml of ethanol, and stir with a magnetic stirrer for 1 hour to dissolve; (2) 300 g of activated alumina (average pore size 0.05 μm, porosity 30%, Shandong Ocean Chemical Industry Co., Ltd.) was immersed in the blended solution, so that the solution was fully absorbed into the pore channels of the activated alumina; (3) The soaked porous material was removed and placed on a stainless steel tray, which was placed in an oven at 150°C and heated for 2 hours, thereby drying the material; (4) The dried porous material was placed in a tubular furnace and carbonized at 1000 °C for 1 h under nitrogen atmosphere to carbonize the phenolic resin and obtain a porous composite material with phenolic resin carbonized supported on activated alumina (porous framework) that can generate an electric arc in a microwave field. The carbon material constituted 0.05% of the total mass of the porous composite material.

[0091] [Example 10] (1) Weigh out 30 g of powdered phenolic resin (2123, Xinxiang Bomafengfan Industry Co, Ltd.) and 3.6 g of hexamethylenetetramine curing agent, put them into a beaker, pour in 500 ml of ethanol, and stir with a magnetic rotor for 1 hour until dissolved; (2) 8 g of a fiberboard-shaped porous scaffold made of magnesium oxide (average pore size 100 μm, porosity 80%, Jinan Huolong Thermal Ceramics Co, Ltd.) was immersed in the compounded solution, so that the solution fully penetrated into the pore channels of the porous scaffold; (3) The soaked porous material was removed and placed on a stainless steel tray, then placed in a furnace at 180°C and heated for 2 hours to dry the material, remove the solvent, and cure the phenolic resin; (4) The dried and hardened porous material was placed in a tubular furnace and carbonized at 1000 °C for 1 h under nitrogen atmosphere to carbonize the phenolic resin and obtain a porous composite material with phenolic resin carbonized on a magnesium oxide fiber porous framework that can generate an electric arc in a microwave field. The carbon material constituted 3% of the total mass of the porous composite material.

[0092] [Example 11] (1) Weigh out 100 g of water-soluble starch (pharmaceutical grade, Shanghai Aladdin Biochemical Technology Co., Ltd.) and place it in a beaker, pour in 500 ml of deionized water, and stir with a magnetic rotor for 1 hour to dissolve; (2) 8 g of a fiberboard-shaped porous scaffold made of zirconia (average pore size 150 μm, porosity 80%) was immersed in the compounded solution (Jinan Huolong Thermal Ceramics Co, Ltd.). As a result, the solution was fully absorbed into the pore channels of the porous scaffold; (3) The soaked porous material was taken out and placed into a microwave pyrolysis reactor (XOLJ-2000N, Nanjing Atpio Instrument Manufacturing Co, Ltd.), and treated by microwave at a power of 3KW for 20 minutes, and the porous material was dried; (4) The dried porous material was placed in a tubular furnace and carbonized at 900 °C for 2 h under nitrogen atmosphere to carbonize the starch, resulting in a porous composite material with starch carbide supported on a zirconia fiber porous framework that can generate an electric arc in a microwave field. The carbon material constituted 0.5% of the total mass of the porous composite material.

[0093] [Example 12] (1) 50 g of liquid phenolic resin (2152, Jining Baiyi Chemicals) was weighed out and placed in a beaker, and 500 ml of ethanol was poured in and stirred with a magnetic stirrer for 1 hour to dissolve; (2) 8 g of a fiberboard-like porous scaffold made of boron nitride (average pore size 100 μm, porosity 80%, Jinan Huolong Thermal Ceramics Co, Ltd.) was immersed in the prepared solution, so that the solution fully penetrated into the pore channels of the porous scaffold; (3) The soaked porous material was removed and placed on a stainless steel tray, then placed in a furnace at 180°C and heated for 2 hours to dry the material, remove the solvent, and cure the phenolic resin; (4) The dried and hardened porous material was placed in a tubular furnace and carbonized at 900 °C for 1 h under nitrogen atmosphere to carbonize the phenolic resin and obtain a porous composite material with phenolic resin carbide supported on a boron nitride fiber porous skeleton that can generate an electric arc in a microwave field. The carbon material constituted 5% of the total mass of the porous composite material.

[0094] [Example 13] (1) Weigh out 100 g of liquid phenolic resin (2152, Jining Baiyi Chemicals) and place it in a beaker, pour in 500 ml of ethanol, and stir with a magnetic stirrer for 1 hour to dissolve; (2) 8 g of a fiberboard-shaped porous scaffold made of silicon carbide (average pore size 100 μm, porosity 80%) was immersed in the compounded solution (Jinan Huolong Thermal Ceramics Co, Ltd.). As a result, the solution was fully penetrated into the pore channels of the porous scaffold; (3) The soaked porous material was removed and placed on a stainless steel tray, then placed in a furnace at 180°C and heated for 2 hours to dry the material, remove the solvent, and cure the phenolic resin; (4) The dried and hardened porous material was placed in a tubular furnace and carbonized at 800 °C for 1 h under nitrogen atmosphere to carbonize the phenolic resin and obtain a porous composite material with phenolic resin char supported on a silicon carbide fiber porous skeleton that can generate an electric arc in a microwave field. The carbon material constituted 10% of the total mass of the porous composite material.

[0095] [Example 14] (1) Weigh out 100 g of liquid phenolic resin (2152, Jining Baiyi Chemicals) and place it in a beaker, pour in 500 ml of ethanol, and stir with a magnetic stirrer for 1 hour to dissolve; (2) 8 g of a fiberboard-shaped porous scaffold made of potassium titanate (average pore size 100 μm, porosity 80%) was immersed in the compounded solution (Jinan Huolong Thermal Ceramics Co, Ltd.). As a result, the solution was fully penetrated into the pore channels of the porous scaffold; (3) The soaked porous material was removed and placed on a stainless steel tray, then placed in a furnace at 180°C and heated for 2 hours to dry the material, remove the solvent, and cure the phenolic resin; (4) The dried and hardened porous material was placed in a tubular furnace and carbonized at 800 °C for 1 h under a nitrogen atmosphere to carbonize the phenolic resin, obtaining a porous composite material with phenolic resin carbide supported on a potassium titanate fiber porous framework capable of generating an electric arc in a microwave field. The carbon material constituted 10% of the total mass of the porous composite material.

[0096] <Microwave pyrolysis of waste plastics>: [Example 15] 0.5 g each of beverage bottle body (PET), beverage bottle cap (HDPE), greenhouse membrane (LLDPE), PP pellets, PP lunchbox fragment, packaging polystyrene (PS) foam, acrylonitrile-butadiene-styrene terpolymer tray (ABS), nylon pipe fragment (PA6) and transparent water cup (PC) and 0.5 g each of polyvinyl chloride (PVC) hose were cut with scissors or weighed, placed on 1 g of the porous composite material obtained in Example 1, and then protected with nitrogen and pyrolyzed by high-power microwaves in a household microwave oven (700w) for 30 seconds. After a short microwave treatment of 30 seconds in a household microwave oven (700w) using the porous composite material obtained in Example 1, all materials were pyrolyzed and gasified. There was almost no residue, and only a small amount of black material remained on the polyvinyl chloride (PVC) hose. Violent arcing phenomena were observed throughout the entire process. The porous composite material generated an electric arc in the microwave field, which rapidly generated high temperatures and transferred heat to the material, causing it to rapidly pyrolyze.

[0097] Using the samples obtained in Examples 2 to 14, experiments similar to the above steps were carried out, and similar experimental phenomena and results were obtained. All the porous composite materials obtained in Examples 2 to 14 were able to generate electric arcs in a microwave field, which could rapidly generate high temperatures and transfer heat to the materials to rapidly pyrolyze the materials.

[0098] [Example 16] 50g of beverage bottle cap (HDPE), 50g of PP lunch box fragment, 50g of acrylonitrile-butadiene-styrene terpolymer tray (ABS), 50g of nylon tube fragment (PA6), 50g of transparent water cup (PC), 3g of packaging foam (PS), 10g of house film (LLDPE), 50g of beverage bottle body (PET), 50g of disposable transparent plastic cup (PS) fragment, and 50g of polyvinyl chloride (PVC) hose fragment were cut with scissors and placed in a cavity composed of 30g of the porous composite material obtained in Example 1, and then treated with a microwave pyrolysis reactor (XOLJ-2000N, Nanjing Atopio Equipment Manufacturing Co., Ltd.) for 5 minutes at a power of 1500W after protecting with nitrogen. In addition, in the polyvinyl chloride hose, almost no residue was found in all materials, and only a small amount of black material remained.

[0099] The placement of the material to be pyrolyzed in the cavity made of the porous composite material that generates an electric arc in the microwave was specifically performed as follows: First, a part of the porous composite material was placed on the bottom and periphery of the quartz reactor to form a cavity with an upper opening; Second, the material was placed in the cavity; Finally, the top of the material was covered with the remaining porous composite material.

[0100] Using the samples obtained in Examples 2 to 14, experiments similar to those described above were carried out, and similar experimental phenomena and results were obtained. All the porous composite materials obtained in Examples 2 to 14 were capable of generating electric arcs in microwaves, which could rapidly generate high temperatures and transfer them to the materials to rapidly pyrolyze the materials.

[0101] [Comparative Example 1] 0.5g of beverage bottle cap (HDPE) fragments, 0.5g of PP lunchbox fragments, 0.5g of PET bottle body fragments, PS foam and 0.5g of PVC hose were placed on 1g of silicon carbide powder (98.5%, Sinopharm Chemical Reagent Beijing Co, Ltd.), respectively, and after protecting with nitrogen, they were subjected to high-power microwave treatment in a household microwave oven (700w) for 30 seconds. There were no sparks in all materials during the microwave process. After the microwave treatment, the HDPE bottle cap, PP lunchbox fragments, PET fragments, PS foam and PVC hose were all unchanged, and only the bottom of the quartz crucible was slightly warmed.

[0102] [Comparative Example 2] 0.5g of beverage bottle cap (HDPE) fragments were placed on 1g of activated carbon powder (AR, ≥200 mesh, item no. C112223, Shanghai Aladdin Bio-Chem Technology Co, LTD.) and protected with nitrogen, then high-power microwaved in a domestic microwave oven (700w) for 30 seconds. During the microwave process, electric arcs appeared occasionally. After microwave treatment, the HDPE bottle cap melted but did not disappear completely. The weight loss of the HDPE was found to be 25% after weighing.

[0103] [Example 17] The other parameters and procedures were the same as in Example 15, except for the following: Using 1 g of the sample obtained in Example 1, 0.5 g of HDPE, 0.5 g of PP, and 0.5 g of LLDPE were pyrolyzed at 700 W output for 30 seconds (or at high output for 30 seconds using a household microwave oven (700 W)) in a microwave pyrolysis reactor (XOLJ-2000N, Nanjing Atpio Instrument Manufacturing Co, Ltd.), and the resulting gas was analyzed by chromatography. The main components detected are shown in Table 1-1.

[0104] Using 1 g of the sample obtained in Example 1, 0.5 g of PET was pyrolyzed at 700 W for 30 seconds (or at high power in a household microwave oven (700 W) for 30 seconds) in a microwave pyrolysis reactor (XOLJ-2000N, Nanjing Atpio Instrument Manufacturing Co, Ltd.), and the resulting gas was analyzed by chromatography. The main components detected are shown in Table 1-2.

[0105] Using 1 g of the sample obtained in Example 1, 0.5 g of PS was pyrolyzed at 700 W for 30 seconds (or at high power for 30 seconds using a household microwave oven (700 W)) in a microwave pyrolysis reactor (XOLJ-2000N, Nanjing Atpio Instrument Manufacturing Co, Ltd.), and the resulting gas was analyzed by chromatography. The main components detected are shown in Tables 1-3.

[0106] Using 1 g of the sample obtained in Example 1, 0.5 g of PVC was pyrolyzed at high power for 30 seconds in a household microwave oven (700 W), and the resulting gas was subjected to chromatographic analysis. The main components detected are shown in Tables 1-4.

[0107] [Table 1-1]

[0108] [Table 1-2]

[0109] [Table 1-3]

[0110] [Table 1-4]

[0111] [Example 18] The other parameters and procedures were the same as in Example 15, except for the following: 30 g of the sample obtained in Example 6 was pyrolyzed for 10 minutes using a microwave pyrolysis reactor with 50 g of HDPE, 50 g of PP, and 50 g of LLDPE at an output of 1500 W, and the resulting gas was subjected to chromatographic analysis. The main components detected are shown in Table 2-1.

[0112] 30g of the sample obtained in Example 6 was used to pyrolyze 50g of PET using a microwave pyrolysis reactor at a power of 1500W for 20 minutes, and then the resulting gas was subjected to chromatographic analysis. The main components detected are shown in Table 2-2.

[0113] Using 30 g of the sample obtained in Example 6, 3 g of PS was pyrolyzed in a microwave pyrolysis reactor at a power of 1500 W for 40 minutes, and the resulting gas was subjected to chromatographic analysis. The main components detected are shown in Table 2-3.

[0114] 30 g of the sample obtained in Example 6 was used to pyrolyze 50 g of a disposable transparent plastic cup (PS) fragment using a microwave pyrolysis reactor at a power of 1500 W for 15 minutes, and then the resulting gas was subjected to chromatographic analysis. The main components detected are shown in Tables 2-4.

[0115] 30g of the sample obtained in Example 6 was used to pyrolyze 50g of PVC hose fragments using a microwave pyrolysis reactor at a power of 1500W for 15 minutes, and then the resulting gas was subjected to chromatographic analysis. The main components detected are shown in Tables 2-5.

[0116] [Table 2-1]

[0117] [Table 2-2]

[0118] [Table 2-3]

[0119] [Table 2-4]

[0120] [Table 2-5]

[0121] [Comparative Example 3] (1) 50 g of liquid phenolic resin (2152, Jining Baiyi Chemicals) was weighed out and placed in a beaker, and 500 ml of ethanol was poured in and stirred with a magnetic stirrer for 1 hour to dissolve; (2) 8 g of a fiberboard-shaped porous scaffold made of alumina (average pore size 100 nm, Pu-Yuan Nanotechnology limited company, Hefei, China) was immersed in the formulation solution so that the solution could fully enter the pore channels of the porous scaffold; (3) The soaked porous material was removed and placed on a stainless steel tray, which was then placed in a furnace at 180°C and heated for 2 hours to remove the solvent and cure the phenolic resin; (4) The dried and hardened porous body was placed in a tubular furnace and carbonized in a nitrogen atmosphere at 900°C for 1 hour to carbonize the phenolic resin.

[0122] 0.5 g of a beverage bottle cap (HDPE) fragment was placed on 1 g of the material obtained in step (4), and then, after protecting with nitrogen, it was subjected to high-power microwave treatment in a domestic microwave oven (700 w) for 30 seconds. During the microwave treatment, there were no sparks, and the HDPE bottle cap was unchanged after the microwave treatment. It was found that when the pore size of the inorganic porous framework was small, a porous composite material capable of generating an electric arc in the microwave field to achieve effective pyrolysis was not obtained.

[0123] <Microwave pyrolysis of vegetable oil>: [Example 19] 0.5 g each of palm oil, rapeseed oil, sunflower oil, and soybean oil was placed on 1 g of the porous composite material obtained in Example 1, and the oil was automatically absorbed into the porous composite material. After protecting it with nitrogen, high-power microwave pyrolysis was performed for 30 seconds in a household microwave oven (700w) (or pyrolysis for 30 minutes at a power of 700W using a microwave pyrolysis reactor (XOLJ-2000N, Nanjing Atpio Instrument Manufacturing Co, Ltd.)), and then weighed to confirm that there was almost no material residue in the porous composite material. After a short time of 30 seconds of microwave (700w) treatment using the porous composite material obtained in Example 1, all the materials were pyrolyzed and gasified, and a violent arc discharge phenomenon was observed. The porous composite material generated an electric arc in the microwave field, which rapidly generated high temperatures and transferred heat to the material to rapidly pyrolyze the material. The gas obtained after pyrolysis was subjected to chromatographic analysis, and the main components detected are shown in Table 3-1.

[0124] [Table 3-1]

[0125] [Example 20] Palm oil, rapeseed oil, sunflower oil, and soybean oil were placed in a beaker of 100 g each, and 30 g of the porous composite material obtained in Example 1 was placed in a quartz reactor purged with nitrogen at 500 ml / min for 10 minutes, and the flow rate was adjusted to 100 ml / min. Then, a microwave pyrolysis reactor (XOLJ-2000N, Nanjing Atopio Industrial Co., Ltd.) was started with an output of 1500 W, and the above vegetable oil was continuously added to the surface of the porous composite material in the quartz reactor through a quartz capillary tube at a rate of about 2 g / min using a peristaltic pump (LongerPump BT100-2J precision peristaltic pump), and continuously pyrolyzed in the gas. After the operation was completed, almost no material remained.

[0126] When the porous and composite materials obtained in Examples 2 to 14 were used to carry out experiments similar to those described above, similar experimental phenomena and results were obtained.

[0127] [Comparative Example 4] 0.5g of palm oil was dropped onto 1g of silicon carbide powder (98.5%, Sinopharm Chemical Reagent Beijing Co, Ltd.), and after nitrogen protection, it was subjected to high-power microwave treatment in a household microwave oven (700w) for 30 seconds. There was no spark during the microwave treatment, and only the bottom of the quartz crucible was slightly warmed. After the microwave treatment, weight measurement showed that the mass of the palm oil did not change obviously.

[0128] [Example 21] The other parameters and procedures were the same as in Example 19, except for the following: 30 g of the sample obtained in Example 6 was used to pyrolyze 100 g each of palm oil, rapeseed oil, sunflower oil, and soybean oil using a microwave pyrolysis reactor with a power of 1500 W and a feed rate of 2 g / min. The resulting gas was analyzed by chromatography. The main components detected are shown in Table 3-2.

[0129] [Table 3-2]

[0130] <Microwave pyrolysis of biomass> [Example 22] 0.5 g each of straw, bagasse, tree branches, leaves, wood chips, rice husks, rice straw, peanut shells, coconut shells, coconut shells, and corn cobs were placed on 1 g of the porous composite material obtained in Example 1, protected with nitrogen, and then pyrolyzed by high-power microwaves in a household microwave oven (700 w) for 30 seconds. After a short microwave treatment of 30 seconds in a household microwave oven (700 w) using the porous composite material obtained in Example 1, all the materials were pyrolyzed and gasified, and only black matter remained. During this process, an active arc discharge phenomenon was observed. The porous composite material generated an electric arc in the microwave, which rapidly generated high temperatures and transferred heat to the material, causing it to pyrolyze rapidly.

[0131] 50 g of each of straw, bagasse, tree branches, leaves, wood chips, rice husk, rice straw, peanut shell, coconut shell, palm seed husk, corn husk, and corn cob were placed in a cavity composed of 30 g of the porous composite material obtained in Example 1, protected with nitrogen, and then treated for 5 minutes at a power of 1500 W using a microwave pyrolysis reactor (XOLJ-2000N, Nanjing Atpio Instrument Manufacturing Co, Ltd.). For all materials, only black matter remained.

[0132] The placement of the material to be pyrolyzed in the cavity formed by the porous composite material was specifically performed as follows: first, a part of the porous composite material was placed on the bottom and periphery of the quartz reactor to form a cavity with an upper opening; then, the material was placed in the cavity; finally, the top of the material was covered with the remaining porous composite material.

[0133] Using the samples obtained in Examples 2 to 14, experiments similar to those described above were carried out, and similar experimental phenomena and results were obtained.

[0134] [Comparative Example 5] 0.5g of rice husk was placed on 1g of silicon carbide powder (98.5%, Sinopharm Chemical Reagent Beijing Co, Ltd.) and, after nitrogen protection, was subjected to high-power microwave treatment in a household microwave oven (700w) for 30 seconds. There were no sparks during the microwave process. After the microwave treatment, the rice husk was unchanged, and only the bottom of the quartz crucible was slightly warmed.

[0135] [Example 23] The other parameters and procedures were the same as those in Example 22, except for the following: 1 g of the sample obtained in Example 1 was used to pyrolyze 0.5 g of straw and rice husk, respectively, using a household microwave oven (700 W) at high power for 30 seconds. The resulting gas was then subjected to chromatographic analysis. The main components detected other than CO and CO2 are shown in Table 4-1.

[0136] 30 g of the sample obtained in Example 6 was used to pyrolyze 50 g of straw and rice husk, respectively, using a microwave pyrolysis reactor with a power output of 1500 W for 15 minutes. The resulting gas was then subjected to chromatographic analysis. The main components detected other than CO and CO2 are shown in Table 4-2.

[0137] [Table 4-1]

[0138] [Table 4-2]

[0139] <Microwave pyrolysis of waste rubber> [Example 24] 0.5g of each of the automobile tire (Hankook) fragments, styrene-butadiene rubber (Beijing Rubber Products Factory), and ethylene-propylene rubber (Beijing Rubber Products Factory) samples were placed on 1g of the porous composite material obtained in Example 1, and after protecting them with nitrogen, they were pyrolyzed by high-power microwaves in a household microwave oven (700w) for 30 seconds. After a short microwave treatment of 30 seconds in a household microwave oven (700w) using the porous composite material obtained in Example 1, all the materials were pyrolyzed and gasified; only a black substance crushed into one pinch remained for the automobile tire fragments; no residue remained for the styrene-butadiene rubber and ethylene-propylene rubber samples. During this process, a vigorous arc discharge phenomenon was observed. The porous composite material generated an electric arc in the microwave, which rapidly generated high temperatures and transferred heat to the materials, causing the materials to pyrolyze rapidly.

[0140] In the cavity of 30 g of the porous composite material obtained in Example 1 that was arced in the microwave, 50 g of a fragment of an automobile tire (Hankook), a styrene-butadiene rubber (Beijing Rubber Products Factory), and an ethylene-propylene rubber (Beijing Rubber Products Factory) sample were placed, respectively, and treated for 5 minutes at a power of 1500 W using a microwave pyrolysis reactor (XOLJ-2000N, Nanjing Atpio Instrument Manufacturing Co, Ltd.) after nitrogen protection. After a short microwave treatment of 30 seconds in a household microwave oven (700w), all the materials were pyrolyzed and gasified; for the fragment of the automobile tire, only a black material crushed in one pinch remained; for the styrene-butadiene rubber and ethylene-propylene rubber samples, no residue remained.

[0141] The placement of the material to be pyrolyzed in the cavity constituted by the porous composite material was in particular operated as follows: first, a part of the porous composite material was placed at the bottom and periphery of the quartz reactor to form a cavity with an upper opening, then the material was placed in the cavity, and finally, the top of the material was covered with the remaining porous composite material.

[0142] When the porous and composite materials obtained in Examples 2 to 14 were used to carry out experiments similar to those described above, similar experimental phenomena and results were obtained.

[0143] [Comparative Example 6] 0.5g of styrene-butadiene rubber sample was placed on 1g of silicon carbide powder (98.5%, Sinopharm Chemical Reagent Beijing Co, Ltd.) and protected with nitrogen, then treated by high-power microwaves in a domestic microwave oven (700w) for 30 seconds. There were no sparks during the microwave treatment process. After microwave treatment, the styrene-butadiene rubber sample was unchanged, and only the bottom of the quartz crucible was slightly warm.

[0144] [Example 25] 0.5g of each of automobile tire (Hankook) fragments, styrene butadiene rubber (Beijing Rubber Products Factory), and ethylene propylene rubber (Beijing Rubber Products Factory) samples were placed on 1g of the porous composite material obtained in Example 1, and after nitrogen protection, they were pyrolyzed by high-power microwaves in a household microwave oven (700w) for 30 seconds and then chromatographic analysis was performed. The main components other than CO and CO2 are shown in Tables 5-1, 5-2, and 5-3.

[0145] Using the same process as above, 30 g of the sample obtained in Example 6 was used, and 50 g samples of automobile tire (Hankook), styrene-butadiene rubber (Beijing Rubber Products Factory), and ethylene-propylene rubber (Beijing Rubber Products Factory) were pyrolyzed for 15 minutes at a power of 1500 W using a microwave pyrolysis reactor, and the resulting gas was subjected to chromatographic analysis. The main components other than CO and CO2 are shown in Tables 5-4, 5-5, and 5-6.

[0146] [Table 5-1]

[0147] [Table 5-2]

[0148] [Table 5-3]

[0149] [Table 5-4]

[0150] [Table 5-5]

[0151] [Table 5-6]

[0152] <Microwave pyrolysis of carbon fiber composites>: [Example 26] 2 g of carbon fiber reinforced epoxy resin composite material (Choshu Kata Fiber Composite Materials Co., Ltd.) was placed on 1 g of the porous composite material obtained in Example 1, and pyrolysis was performed for 40 seconds using high-power microwaves in a household microwave oven (700 w). When the carbon fiber composite material was removed and weighed, weight loss was observed, and the carbon fibers could be easily peeled off. During the microwave treatment, a vigorous arc discharge phenomenon was observed. The porous composite material generated an electric arc in the microwave, which rapidly generated high temperatures and transferred heat to the material, causing it to rapidly pyrolyze.

[0153] In a cavity made of 30 g of the porous composite material that generates an arc in microwaves obtained in Example 1, 50 g of carbon fiber reinforced epoxy resin composite material (Choshu Kata Fiber Composite Material Co., Ltd.) was placed, and after nitrogen protection, it was treated with 1500 W of electricity for 5 minutes using a microwave pyrolysis reactor (XOLJ-2000N, Nanjing Atpio Instrument Manufacturing Co, Ltd.). When the carbon fiber composite material was taken out and weighed, weight loss was observed, and the carbon fiber could be easily peeled off from the nonwoven fabric.

[0154] The placement of the material to be pyrolyzed in the cavity made of the porous composite material that generates an electric arc in microwaves was specifically performed as follows: First, a part of the porous composite material that generates an electric arc in microwaves was placed at the bottom and periphery of the quartz reactor to form a cavity with an upper opening. Then, the material was placed in the cavity. Finally, the top of the material was covered with the remaining porous composite material.

[0155] Using the samples obtained in Examples 2 to 14, experiments similar to those described above were carried out, and similar experimental phenomena and results were obtained. All the porous composite materials obtained in Examples 2 to 14 were capable of generating electric arcs in microwaves, which could rapidly generate high temperatures and transfer them to the materials to rapidly pyrolyze the materials.

[0156] [Comparative Example 7] 2g of carbon fiber reinforced epoxy resin composite (Changzhou Huatan Fiber Composite Co, Ltd.) was placed on 1g of silicon carbide powder (98.5%, Sinopharm Chemical Reagent Beijing Co, Ltd.), and after nitrogen protection, it was high-power microwaved in a household microwave oven (700w) for 30 seconds. There were no sparks during the microwave treatment process. After microwave treatment, the material did not change, and only the bottom of the quartz crucible was slightly warmed.

[0157] [Example 27] 2 g of carbon fiber reinforced epoxy resin composite material (Choshu Kata Fiber Composite Materials Co., Ltd.) was placed on 1 g of the porous composite material obtained in Example 1 in which an arc was generated by microwaves, and pyrolysis was carried out for 40 seconds using high-power microwaves in a household microwave oven (700W). The carbon fiber composite material was then removed. After weighing, a weight loss of 36% was observed, and the carbon fiber could be easily peeled off from the nonwoven fabric. The collected gas was subjected to chromatographic analysis, and the main components detected are shown in Table 6.

[0158] In a cavity made of 30 g of the porous composite material obtained in Example 6 in which an arc was generated in a microwave, 30 g of carbon fiber reinforced polypropylene composite material (Choshu Kata Fiber Composite Materials Co., Ltd.) was placed, and after nitrogen protection, it was treated for 5 minutes at an output of 1500 W using a microwave pyrolysis reactor (XOLJ-2000N, Nanjing Atpio Instrument Manufacturing Co, Ltd.). After weighing, a weight loss of 38% was observed, and the carbon fiber could be easily peeled off from the nonwoven fabric. The collected gas was subjected to chromatographic analysis, and the main components detected are shown in Table 6.

[0159] 50 g of carbon fiber reinforced nylon composite material (Choshu Kata Fiber Composite Materials Co., Ltd.) was placed in a cavity consisting of 30 g of the porous composite material that generates an arc in microwaves obtained in Example 7, and after nitrogen protection, it was treated for 10 minutes at an output of 2000 W using a microwave pyrolysis reactor (XOLJ-2000N, Nanjing Thermal Appliance Manufacturing Co., Ltd.). After weighing, a weight loss of 39% was observed, and the carbon fiber could be easily peeled off from the nonwoven fabric. The collected gas was subjected to chromatographic analysis, and the main components detected are shown in Table 6.

[0160] The placement of the material in the cavity made of the porous composite material with microwave electric arc generation was specifically performed as follows: First, a part of the porous composite material with microwave electric arc generation was placed on the bottom and periphery of the quartz reactor to form a cavity with an upper opening; Second, the material was placed in the cavity; Finally, the top of the material was covered with the remaining porous composite material.

[0161] [Table 6]

[0162] <Microwave pyrolysis of circuit boards>: In the following examples, the collected gases were chromatographically analyzed as follows: The gas products collected after pyrolysis were analyzed using a refined gas analyzer (HP Agilent 7890 A, consisting of three channels including one FID and two TCDs (thermal conductivity detectors)) according to the ASTM D1945-14 method. Hydrocarbons were analyzed on the FID channel. One TCD using nitrogen carrier gas was used to determine hydrogen content because there was a slight difference in conductivity between hydrogen and helium carrier gas. The other TCD using helium as carrier gas was used for the detection of CO, CO2, N2, and O2. For quantitative analysis, the response factor was determined by using RGA (refined gas analysis) calibration gas standards.

[0163] [Example 28] In a cavity formed of 50 g of the porous composite material obtained in Example 1, a waste circuit board (the waste circuit board has an area of ​​about 1 cm 2 The porous composite material was pre-shattered into irregular pieces of 10g (10 ...

[0164] The main components of the pyrolysis gas products are shown in Table 7-1. The mass of the solid residue after the reaction was completed was 30% of that before pyrolysis, including metal components that have a loose structure and are easy to separate, and nonmetallic components mainly consisting of glass fiber mixtures. After simple crushing, the metal and nonmetallic parts (mainly glass fibers) in it could be separated and recovered.

[0165] The placement of the circuit board to be pyrolyzed in the cavity made of the porous composite material was specifically performed as follows: First, a part of the porous composite material was placed inside the quartz reactor, and the porous composite materials were placed in order to form a hollow cavity with an opening at the top. Then, the waste circuit board was placed in the cavity. Finally, the top of the material was covered with the remaining porous composite material.

[0166] Using the samples obtained in Examples 2-14, experiments similar to the above steps were carried out, and similar experimental phenomena and results were obtained. The mass of the solid residue after the reaction was completed was about 28-35% of that before pyrolysis. All the porous composite materials obtained in Examples 2-14 were able to generate an electric arc in the microwave field, which could rapidly generate high temperatures and transfer them to the material to rapidly pyrolyze the material.

[0167] [Comparative Example 8] 10 g of waste circuit boards and 50 g of silicon carbide powder (98.5%, Sinopharm Chemical Reagent Beijing Co, Ltd.) were mixed uniformly and then placed in a quartz reaction tank, which was then placed in a microwave reactor (MKX-R1C1B, Qingdao Makewave Instrument Manufacturing Co, Ltd.) and protected with nitrogen, after which it was treated in the microwave pyrolysis reactor for 5 minutes at a power of 900 W. There were no sparks during the microwave treatment, the waste circuit boards did not change after the microwave treatment, and only the bottom of the quartz reaction tank was slightly warmed.

[0168] [Example 29] The other parameters and procedures were the same as in Example 28, except for the following: 10 waste circuit boards and 30 g of the multi-layer composite material obtained in Example 6, which had been subjected to electric arc generation in microwaves, were mixed uniformly and placed in a quartz reaction tank, and then the whole was placed in a microwave pyrolysis reactor, protected with nitrogen, and then treated in the microwave pyrolysis reactor for 10 minutes at an output of 1,200 W. The porous composite material generated an electric arc in the microwave, which rapidly generated high temperatures, which were transferred to the material to rapidly pyrolyze the material. The collected gas components were subjected to gas chromatography analysis. The main components of the pyrolysis gas products are shown in Table 7-2. The mass of the solid residue after the reaction was completed was 32% of that before pyrolysis. In addition, the metal and the substrate had a loose structure, and the metal and nonmetallic parts could be separated and collected by simple crushing.

[0169] [Example 30] The other parameters and procedures were the same as in Example 28, except for the following: 15 g of the porous composite material obtained in Example 2, which had been subjected to arc generation in microwaves, and 10 g of waste circuit boards were mixed uniformly and placed in a quartz reaction vessel, and then the whole was placed in a microwave pyrolysis reactor, protected with nitrogen, and then treated in the microwave pyrolysis reactor at an output of 900 W for 20 minutes. The porous composite material generated an electric arc in the microwave, which rapidly generated high temperatures, which were then transferred to the material to rapidly pyrolyze the material. The collected gas components were subjected to gas chromatography analysis. The main components of the pyrolysis gas products are shown in Table 7-3. The mass of the solid residue after the reaction was completed was 30% of that before pyrolysis. In addition, the metal and the substrate had a loose structure, and the metal and nonmetallic parts could be separated and collected by simple crushing.

[0170] [Example 31] The other parameters and procedures were the same as in Example 28, except for the following: 60g of the porous composite material obtained in Example 11, which had been subjected to arc generation in microwaves, and 2g of waste circuit boards were mixed uniformly and placed in a quartz reaction vessel, and then the whole was placed in a microwave pyrolysis reactor. After nitrogen protection, the whole was treated in the microwave pyrolysis reactor at an output of 900W for 5 minutes. The porous composite material generated an electric arc in the microwave, which rapidly generated high temperatures, which were then transferred to the material to rapidly pyrolyze the material. The collected gas components were subjected to gas chromatography analysis. The main components of the pyrolysis gas products are shown in Table 7-4. The mass of the solid residue after the reaction was completed was 30% of that before pyrolysis. In addition, the metal and the substrate had a loose structure, and the metal and nonmetallic parts could be separated and collected by simple crushing.

[0171] [Example 32] The other parameters and procedures were the same as in Example 28, except for the following: 5 g of the multilayer composite material in the electric arc generated by microwaves obtained in Example 8 and 20 g of waste circuit boards were mixed uniformly and placed in a quartz reaction tank, and then the whole was placed in a microwave pyrolysis reactor, protected with nitrogen, and then treated in the microwave pyrolysis reactor at an output of 1000 W for 30 minutes. The porous composite material generated an electric arc in the microwave, which rapidly generated high temperatures, which were transferred to the material to rapidly pyrolyze the material. The collected gas components were subjected to gas chromatography analysis. The main components of the pyrolysis gas products are shown in Table 7-5. The mass of the solid residue after the reaction was completed was 31% of that before pyrolysis. In addition, the metal and the substrate had a loose structure, and the metal and nonmetallic parts could be separated and collected by simple crushing.

[0172] [Table 7-1]

[0173] [Table 7-2]

[0174] [Table 7-3]

[0175] [Table 7-4]

[0176] [Table 7-5]

[0177] The data in the table also shows that the pyrolysis products contain a relatively high percentage of hydrogen and therefore can be collected and used as a fuel.

Claims

1. 1. A porous composite material capable of generating an arc in a microwave field, the porous composite material comprising an inorganic porous framework and a carbon material supported on the inorganic porous framework, The inorganic porous skeleton has an average pore size of 0.2 to 1000 μm; The inorganic porous framework is an inorganic material having a porous structure, the inorganic material being selected from the group consisting of carbon, silicate, aluminate, borate, phosphate, germanate, titanate, oxide, nitride, carbide, boride, sulfide, silicide, halide, and combinations thereof; The inorganic porous skeleton has at least one skeleton selected from the group consisting of a skeleton after carbonization of a melamine sponge, a skeleton after carbonization of a phenolic resin sponge, a porous skeleton composed of inorganic fibers, a skeleton composed of filled inorganic particles, and a ceramic fiber skeleton obtained after firing a ceramic fiber skeleton precursor; The carbon material is selected from the group consisting of graphene, carbon nanotubes, graphite, carbon black, carbon fibers, carbon dots, carbon nanowires, products obtained by carbonizing a carbonizable organic substance or a mixture containing a carbonizable organic substance, and combinations thereof. Porous composite material.

2. the inorganic porous skeleton has an average pore size of 0.2 to 500 μm, and / or The porosity of the inorganic porous framework is 1% to 99.99%; The porous composite material according to claim 1 .

3. The ratio of the carbon material is 0.001% to 99% based on the total mass of the porous composite material; The porous and composite material according to claim 1 or 2.

4. The porous composite material is heated to a temperature of more than 1000° C. by electric arcs generated by the porous composite material in a microwave field. The porous and composite material according to any one of claims 1 to 3.

5. The carbon material is selected from the group consisting of graphene, carbon nanofibers, carbon nanotubes, products obtained by carbonizing a carbonizable organic substance or a mixture containing a carbonizable organic substance, and combinations thereof. The porous and composite material according to any one of claims 1 to 4.

6. The carbonizable organic matter is selected from synthetic organic polymer compounds and natural organic polymer compounds. The porous composite material according to claim 1 .

7. the synthetic organic polymer compound is a rubber or a plastic; The plastics include thermosetting plastics and thermoplastics; The natural organic polymer compound is at least one selected from the group consisting of starch, viscose fiber, lignin and cellulose; The porous composite material according to claim 6 .

8. The synthetic organic polymer compound is selected from the group consisting of epoxy resins, phenolic resins, furan resins, polystyrene, styrene-divinylbenzene copolymers, polyacrylonitrile, polyaniline, polypyrrole, polythiophene, styrene-butadiene rubber, polyurethane rubber, and combinations thereof; The porous composite material according to claim 7 .

9. The mixture containing a carbonizable organic material is a mixture of a carbonizable organic material with other metal-free organic materials and / or metal-free inorganic materials; The porous composite material according to claim 1 .

10. The mixture containing carbonizable organic matter is selected from the group consisting of coal, natural pitch, petroleum pitch or coal tar pitch, and combinations thereof; The porous composite material according to claim 9 .

11. the oxide is selected from the group consisting of aluminum oxide, silicon oxide, zirconium oxide, magnesium oxide, cerium oxide, titanium oxide, and combinations thereof; the nitride is selected from the group consisting of silicon nitride, boron nitride, zirconium nitride, hafnium nitride, tantalum nitride, and combinations thereof; the carbide is selected from the group consisting of silicon carbide, zirconium carbide, hafnium carbide, tantalum carbide, and combinations thereof; and the boride is selected from the group consisting of zirconium boride, hafnium boride, tantalum boride, and combinations thereof. The porous and composite material according to any one of claims 1 to 10.

12. The inorganic porous skeleton is at least one of a skeleton after carbonization of a melamine sponge, a skeleton after carbonization of a phenolic resin sponge, a porous skeleton of an aluminum silicate fiber, a porous skeleton of a mullite fiber, a porous skeleton of an alumina fiber, a porous skeleton of a zirconia fiber, a porous skeleton of a magnesium oxide fiber, a porous skeleton of a boron nitride fiber, a porous skeleton of a boron carbide fiber, a porous skeleton of a silicon carbide fiber, a porous skeleton of a potassium titanate fiber, and a ceramic fiber skeleton obtained after firing a ceramic fiber skeleton precursor.

12. The porous and composite material according to claim 1 .

13. A method for preparing the porous and composite material according to any one of claims 1 to 12, comprising the steps of: Step (1): immersing an inorganic porous skeleton or an inorganic porous skeleton precursor in a solution or dispersion of a carbon material and / or a carbon material precursor to fill pores of the inorganic porous skeleton or inorganic porous skeleton precursor with the solution or dispersion; Step (2): A step of heating and drying the porous material obtained in step (1) to precipitate or solidify a carbon material or a carbon material precursor on the inorganic porous skeleton or the inorganic porous skeleton precursor, thereby supporting the carbon material or the carbon material precursor; Step (3): when at least one of a carbon material precursor or an inorganic porous skeleton precursor is used as a starting material, heating the porous material obtained in step (2) under an inert gas atmosphere to convert the inorganic porous skeleton precursor into an inorganic porous skeleton and / or reduce or carbonize the carbon material precursor; Including, A preparation method comprising the steps of:

14. The solution or dispersion of the carbon material or carbon material precursor in step (1) comprises a solvent selected from the group consisting of benzene, toluene, xylene, trichlorobenzene, chloroform, cyclohexane, ethyl caproate, butyl acetate, carbon disulfide, ketones, acetone, cyclohexanone, tetrahydrofuran, dimethylformamide, water, and alcohol, and combinations thereof; and / or The concentration of the solution or dispersion in step (1) is 0.001 to 1 g / mL; and / or In step (1), the carbon material and / or carbon precursor material is contained in an amount of 0.001% to 99.999% of the total mass of the inorganic porous framework material or inorganic porous framework material precursor and the carbon material and / or carbon material precursor; 14. The method according to claim 13 .

15. The solvent of the solution or dispersion of the carbon material or carbon material precursor in the step (1) is water and / or ethanol.

15. The method according to claim 14 .

16. The heating and drying in step (2) is carried out at 50 to 250° C.; 16. The process according to any one of claims 13 to 15.

17. The heating and drying in step (2) is carried out by heating with microwaves, The microwave output is 1 W to 100 kW. The microwave heating time is 2 to 200 minutes.

17. The method of claim 16.

18. The inorganic porous scaffold precursor is selected from the group consisting of a ceramic precursor, a porous material of a carbonizable organic material, or a porous material of a mixture containing a carbonizable organic material, and combinations thereof; and / or The carbon material precursor is selected from the group consisting of graphene oxide, modified carbon nanotubes, modified carbon nanofibers, modified graphite, modified carbon black, modified carbon fiber, carbonizable organics or mixtures containing carbonizable organics, and combinations thereof; and / or The heating in the step (3) is carried out at a temperature of 400 to 1800° C.; 18. The process according to any one of claims 13 to 17.

19. The heating in the step (3) is heating by microwaves, The microwave output is 100 W to 100 KW. The microwave heating time is preferably 0.5 to 200 minutes.

20. The method of claim 18 .

20. Use of the porous composite material according to any one of claims 1 to 12 in the fields of high-temperature heating, pyrolysis and reuse of materials containing organic compounds by microwaves, or in the fields of high-temperature catalysis such as biomass pyrolysis, vegetable oil processing, waste polymer material pyrolysis, petrochemical pyrolysis, carbon fiber composite material recycling, food waste processing, VOC exhaust gas processing or COD sewage processing.

21. 1. A method for pyrolyzing and / or recycling organic compound-containing materials, comprising: Contacting the organic compound-containing material with the porous and composite material according to any one of claims 1 to 12, A microwave field is applied to the organic compound-containing material and the porous composite material under an inert atmosphere or vacuum, and the porous composite material generates an electric arc in the microwave field, rapidly reaches a high temperature, and thermally decomposes the organic compound contained in the organic compound-containing material.

1. A method for pyrolyzing and / or recycling organic compound-containing materials, comprising:

22. The organic compound-containing material is an organic substance, a mixture containing an organic substance, or a composite material containing an organic substance.

22. A method for pyrolyzing and / or recycling organic compound-containing materials according to claim 21.

23. The method of claim 21, wherein the organic compound-containing material is selected from the group consisting of: (i) Waste plastics, or at least one selected from the group consisting of polyolefins, polyesters, polyamides, acrylonitrile-butadiene-styrene terpolymers, polycarbonates, polylactic acid, polyurethanes, polymethyl methacrylate, polyoxymethylene, polyphenylene ethers, and polyphenylene sulfides; or at least one selected from the group consisting of polyethylene, polypropylene, polyvinyl chloride, polyethylene terephthalate, polystyrene, polyamides, acrylonitrile-butadiene-styrene terpolymers, polycarbonates, polylactic acid, polymethyl methacrylate, and polyoxymethylene; or at least one selected from the group consisting of polyethylene, polypropylene, polyvinyl chloride, polyethylene terephthalate, polystyrene, polycarbonates, and polyamides; (ii) Waste rubber, or at least one selected from the group consisting of natural rubber, butadiene rubber, styrene butadiene rubber, nitrile rubber, isoprene rubber, ethylene propylene rubber, butyl rubber, neoprene, styrene-based block copolymers, and silicone rubber; or at least one selected from the group consisting of natural rubber, butadiene rubber, styrene butadiene rubber, isoprene rubber, and ethylene propylene rubber; (iii) biomass or at least one selected from the group consisting of straw, bagasse, tree branches, leaves, wood chips, rice husks, rice stalks, rice straw, peanut shells, coconut shells, palm husks, walnut shells, macadamia nut shells, pistachio shells, wheat straw, corn stalks, and corn cobs; (iv) a vegetable oil, or at least one selected from the group consisting of palm oil, rapeseed oil, sunflower oil, soybean oil, peanut oil, linseed oil and castor oil; or at least one selected from the group consisting of palm oil, rapeseed oil, sunflower oil and soybean oil; (v) carbon fiber composites containing a polymer matrix selected from the group consisting of polyethylene, polypropylene, nylon, phenolic resins and epoxy resins; and, (vi) A circuit board.

24. The weight ratio of the organic compound-containing material to the porous composite material is 1:99 to 99:1; and / or The microwave power of the microwave field is between 1 W and 100 KW; and / or The microwave irradiation time is 0.1 to 200 minutes.

22. The method of claim 21.

25. the organic compound-containing material is a carbon fiber composite material, pyrolyzing the polymer matrix in the carbon fiber composite and then recycling the remaining carbon fibers; 22. The method of claim 21.

26. the organic compound-containing material is a circuit board, Treating the solid residue obtained by pyrolyzing the circuit board to separate and recycle the metallic and non-metallic components therein; and / or collecting gas products resulting from pyrolysis of the circuit board; 22. The method of claim 21.

27. The hydrogen contained in the pyrolysis product is collected.

27. The method of claim 26.