Electrostatic charge image developer, process cartridge, image forming apparatus, and image forming method
The electrostatic image developer with toner particles and a structured carrier maintains consistent glossiness and reduces fogging by employing specific viscoelastic properties and carrier design, addressing issues of inconsistent image quality under varying temperature and pressure.
Patent Information
- Application Number
- JP2023043908
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
AI Technical Summary
Existing electrostatic image developers exhibit significant differences in glossiness and are prone to image fogging when fixed under varying temperature and pressure conditions, leading to inconsistent image quality.
The developer uses toner particles with specific viscoelastic properties, characterized by loss tangents D1(90), D50(90), D1(150), and D50(150) within defined ranges, and a carrier with controlled magnetic powder content and specific gravity, along with a carrier structure comprising core particles, a first resin layer, and a second melamine resin layer, to maintain consistent glossiness and reduce fogging.
The solution results in an electrostatic image developer with minimal differences in glossiness and reduced image fogging across different fixing conditions, ensuring consistent image quality.
Smart Images

Figure 2024133900000007 
Figure 2024133900000008 
Figure 2024133900000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrostatic image developer, a process cartridge, an image forming apparatus, and an image forming method. [Background technology]
[0002] Patent Document 1 discloses a developer using a toner for developing electrostatic latent images, which contains toner particles containing a binder resin, the binder resin containing an amorphous resin and a crystalline resin, and which is obtained by performing a strain dispersion measurement of dynamic viscoelasticity under conditions of a temperature of 130° C., a frequency of 1 Hz, and a strain amplitude of 1.0 to 500%, and in which, when the integral value of the stress in a stress-strain curve at a strain amplitude of 100% is S130 and the slope of the major axis is θ130, the S130 is more than 0 Pa and 350,000 Pa or less, and the θ130 is more than 22° and less than 90°.
[0003] Patent Document 2 discloses a developer using a toner for developing electrostatic images, which contains at least a binder resin and a release agent, the binder resin containing at least a crystalline resin, and whose storage modulus, measured at a frequency of 1 Hz and at 150° C. while changing the strain from 0.01% to 1000%, satisfies a specific relationship.
[0004] Patent Document 3 discloses a developer using a toner for developing electrostatic latent images, which contains toner particles containing a binder resin, the binder resin containing an amorphous vinyl resin and a crystalline resin, and which is obtained by performing a strain dispersion measurement of dynamic viscoelasticity under conditions of a temperature of 130° C., a frequency of 1 Hz, and a strain amplitude of 1.0 to 500%, where S130 is the integral value of the stress in a stress-strain curve at a strain amplitude of 100%, and θ130 is the slope of the major axis, and S130 is more than 0 Pa and 350,000 Pa or less, and θ130 is 0° or more and less than 10°.
[0005] Patent Document 4 discloses a developer using a toner for developing electrostatic images, which contains toner base particles containing at least a binder resin and a release agent, and an external additive, wherein the binder resin contains at least a crystalline resin, and the peak top value of the loss tangent, tan δ6°C / min, when measured from 25°C to 100°C under conditions of a frequency of 1 Hz and a temperature rise rate of 6°C / min, and the peak top value of the loss tangent, tan δ3°C / min, when measured from 25°C to 100°C under conditions of a frequency of 1 Hz and a temperature rise rate of 3°C / min, satisfy a specific relationship.
[0006] Patent Document 5 describes a polymer film containing at least a binder resin, a colorant, and a release agent, in which the rate of change γG' of storage modulus G' is 50%<γG'<86%, and the rate of change γG" of loss modulus G" is greater than 50%, and the storage modulus G' in the range of 1 to 50% strain at a temperature of 150°C is 5×10 2 ~3.5×10 3 The binder resin is a toner for developing electrostatic images, the binder resin containing a non-crystalline resin and a crystalline resin.
[0007] Patent Documents 6 and 7 disclose a developer using a toner for developing electrostatic images, which is composed of toner particles containing a binder resin, and which is characterized in that, in an elasticity image of a cross section of the toner particle taken with an atomic force microscope (AFM), the binder resin has a domain-matrix structure composed of a high elasticity resin constituting the domains and a low elasticity resin constituting the matrix, the arithmetic mean value of the ratio (L / W) of the major axis L to the minor axis W of each domain is within the range of 1.5 to 5.0, 80% or more of the domains have a major axis L within the range of 60 to 500 nm, and 80% or more of the domains have a minor axis W within the range of 45 to 100 nm. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2020-042122 A [Patent Document 2] JP 2020-106685 A [Patent Document 3] JP 2020-042121 A [Patent Document 4] JP 2019-144368 A [Patent Document 5] JP 2013-160886 A [Patent Document 6] JP 2011-237793 A [Patent Document 7] JP 2011-237792 A Summary of the Invention [Problem to be solved by the invention]
[0009] In image formation using an electrostatic image developer containing a toner, for example, a toner image transferred to a recording medium is fixed to the recording medium by heating and pressurization. When an electrostatic image developer containing a toner that is easily melted by heating is used to obtain good fixability, the difference in glossiness between a fixed image fixed under high temperature and high pressure conditions and a fixed image fixed under low temperature and low pressure conditions may become large. In addition, when an electrostatic image developer containing a toner that is easily melted by heating is used, fogging may occur on the image.
[0010] The object of the present invention is to provide a carrier having a true specific gravity of 3.0 g / cm or less than 3.0 g / cm, in which any one of D1(90), D50(90), D1(150), and D50(150) is less than 0.5 or more than 2.5, the value of D50(150)-D1(150) is 1.5 or more, the value of 50(90)-D1(90) is 1.0 or more, and 3 Less than or equal to 4.0g / cm 3 The object of the present invention is to provide an electrostatic image developer in which the difference in gloss between an image fixed under low temperature and low pressure conditions and an image fixed under high temperature and high pressure conditions is small and image fog is suppressed, as compared with a case in which the content of magnetic powder in the carrier exceeds 80% by mass or less or 90% by mass or more. [Means for solving the problem]
[0011] The above problems are solved by the following means:
[0012] <1> a toner comprising toner particles containing a binder resin and an external additive, wherein, in a dynamic viscoelasticity measurement of the toner, when a loss tangent tanδ at a temperature of 90°C and a distortion of 1% is D1(90), a loss tangent tanδ at a temperature of 90°C and a distortion of 50% is D50(90), a loss tangent tanδ at a temperature of 150°C and a distortion of 1% is D1(150), and a loss tangent tanδ at a temperature of 150°C and a distortion of 50% is D50(150), D1(90), D50(90), D1(150), and D50(150) are each 0.5 or more and 2.5 or less, the value of D50(150)-D1(150) is less than 1.5, and the value of D50(90)-D1(90) is less than 1.0; True specific gravity is 3.0g / cm 3 More than 4.0g / cm 3 A career that is: An electrostatic image developer comprising:
[0013] <2> The true specific gravity of the carrier is dg / cm 3 the relationship between D1(90) and d satisfies any one of the following conditions 1 to 3: <1> Electrostatic image developer according to claim 1. Condition 1: 3.0≦d<3.4 and 1.4≦D1(90)≦2.5 Condition 2: 3.4≦d<3.8 and 1.1≦D1(90)<1.4 Condition 3: 3.8≦d≦4.0 and 0.5≦D1(90)<1.1 <3> The carrier includes a core particle having a magnetic powder dispersed in a resin, a first resin layer that covers the surface of the core particle, and a second resin layer that covers the outer peripheral surface of the first resin layer. <1> or <2> Electrostatic image developer according to claim 1. <4> The first resin layer contains a melamine resin. <3> Electrostatic image developer according to claim 1.
[0014] <5> The toner particles further contain resin particles. <1> ~ <4> 13. The electrostatic image developer according to claim 12, <6> The resin particles are crosslinked resin particles. <5> Electrostatic image developer according to claim 1. <7> The crosslinked resin particles are styrene (meth)acrylic resin particles. <6> Electrostatic image developer according to claim 1. <8> the number average molecular weight of the tetrahydrofuran soluble matter in the toner particles is 5,000 or more and 15,000 or less; <1> ~ <7> 13. The electrostatic image developer according to claim 12,
[0015] <9> a toner comprising toner particles containing a binder resin and an external additive, wherein, in a dynamic viscoelasticity measurement of the toner, when a loss tangent tanδ at a temperature of 90°C and a distortion of 1% is D1(90), a loss tangent tanδ at a temperature of 90°C and a distortion of 50% is D50(90), a loss tangent tanδ at a temperature of 150°C and a distortion of 1% is D1(150), and a loss tangent tanδ at a temperature of 150°C and a distortion of 50% is D50(150), D1(90), D50(90), D1(150), and D50(150) are each 0.5 or more and 2.5 or less, the value of D50(150)-D1(150) is less than 1.5, and the value of D50(90)-D1(90) is less than 1.0; A carrier including core particles in which a magnetic powder is dispersed in a resin, the content of the magnetic powder being more than 80% by mass and less than 90% by mass relative to the entire carrier; An electrostatic image developer comprising:
[0016] <10> <1> ~ <9> and a developing device that contains the electrostatic image developer according to any one of claims 1 to 5 and develops an electrostatic image formed on a surface of an image carrier into a toner image by using the electrostatic image developer, A process cartridge that is detachably attached to an image forming apparatus. <11> An image carrier; a charging device for charging the surface of the image carrier; an electrostatic image forming device for forming an electrostatic image on the charged surface of the image carrier; <1> ~ <9> a developing device that contains the electrostatic image developer according to any one of claims 1 to 5 and develops the electrostatic image formed on the surface of the image carrier into a toner image by the electrostatic image developer; a transfer device for transferring the toner image formed on the surface of the image carrier to a surface of a recording medium; a fixing device for fixing the toner image transferred onto the surface of the recording medium; An image forming apparatus comprising: <12> a charging step of charging the surface of the image carrier; an electrostatic image forming step of forming an electrostatic image on the charged surface of the image carrier; <1> ~ <9> a developing step of developing the electrostatic image formed on the surface of the image carrier into a toner image by using the electrostatic image developer according to any one of the above items; a transfer step of transferring the toner image formed on the surface of the image carrier onto a surface of a recording medium; a fixing step of fixing the toner image transferred onto the surface of the recording medium; The image forming method according to claim 1, Effect of the Invention
[0017] <1> or <5> According to the invention, any one of D1(90), D50(90), D1(150), and D50(150) is less than 0.5 or exceeds 2.5, the value of D50(150)-D1(150) is 1.5 or more, the value of 50(90)-D1(90) is 1.0 or more, or the true specific gravity of the carrier is 3.0 g / cm 3 Less than or equal to 4.0g / cm 3 The present invention provides an electrostatic image developer which has a smaller difference in gloss between an image fixed under low temperature and low pressure conditions and an image fixed under high temperature and high pressure conditions, and which suppresses image fogging, as compared with the case where the above-mentioned range is exceeded.
[0018] <2> According to the invention, there is provided an electrostatic image developer in which image fogging is suppressed compared to a case in which the relationship between D1(90) and d does not satisfy any of conditions 1 to 3. <3> or <4> According to the present invention, there is provided an electrostatic image developer in which image fogging is suppressed compared to when the carrier is composed of core particles and a second resin layer.
[0019] <6> According to the present invention, there is provided a toner for developing electrostatic images which has a smaller difference in gloss between an image fixed under low temperature and low pressure conditions and an image fixed under high temperature and high pressure conditions, as compared with a case in which the resin particles are non-crosslinked resin particles. <7> According to the invention, there is provided a toner for developing electrostatic images which has a smaller difference in gloss between an image fixed under low temperature and low pressure conditions and an image fixed under high temperature and high pressure conditions, as compared with a case in which the crosslinked resin particles are polyester resin particles. <8> According to the invention, an electrostatic image developer is provided in which the difference in gloss between an image fixed under low temperature and low pressure conditions and an image fixed under high temperature and high pressure conditions is smaller than when the number average molecular weight of the tetrahydrofuran soluble matter is less than 5,000 or exceeds 15,000.
[0020] <9> According to the invention, there is provided an electrostatic image developer in which the difference in gloss between an image fixed under low temperature and low pressure conditions and an image fixed under high temperature and high pressure conditions is smaller and image fog is suppressed, as compared with a case in which any of D1(90), D50(90), D1(150), and D50(150) is less than 0.5 or exceeds 2.5, the value of D50(150)-D1(150) is 1.5 or more, the value of 50(90)-D1(90) is 1.0 or more, or the content of magnetic powder in the carrier is less than 80% by mass or 90% by mass or more.
[0021] <10> , <11> or <12> According to the invention, any one of D1(90), D50(90), D1(150), and D50(150) is less than 0.5 or exceeds 2.5, the value of D50(150)-D1(150) is 1.5 or more, the value of D50(90)-D1(90) is 1.0 or more, and the true specific gravity of the carrier is 3.0 g / cm 3 Less than or equal to 4.0g / cm 3The present invention provides a process cartridge, an image forming apparatus, or an image forming method in which the difference in gloss between an image fixed under low temperature and low pressure conditions and an image fixed under high temperature and high pressure conditions is smaller and image fogging is suppressed, as compared to when the magnetic powder content in the carrier is less than 80% by mass or less or 90% by mass or more. [Brief description of the drawings]
[0022] [Figure 1] 1 is a schematic configuration diagram illustrating an example of an image forming apparatus according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram illustrating an example of a process cartridge that is detachably mounted to the image forming apparatus according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Hereinafter, an embodiment of the present invention will be described as an example. The description and examples are merely illustrative of the embodiment, and are not intended to limit the scope of the present invention. In the present specification, the upper or lower limit of one numerical range may be replaced with the upper or lower limit of another numerical range. In addition, in the present specification, the upper or lower limit of the numerical range may be replaced with a value shown in the examples. In this specification, (meth)acrylic means both acrylic and methacrylic.
[0024] In this specification, the term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved. Each component may contain multiple types of the corresponding substance. When referring to the amount of each component in a composition, if the composition contains multiple substances corresponding to each component, the amount refers to the total amount of those multiple substances present in the composition, unless otherwise specified.
[0025] [Electrostatic image developer] <First aspect> The electrostatic image developer (hereinafter also referred to as "developer") according to a first aspect is a toner including toner particles containing a binder resin, and in dynamic viscoelasticity measurement of the toner, when the loss tangent tanδ at a temperature of 90°C and a distortion of 1% is D1(90), the loss tangent tanδ at a temperature of 90°C and a distortion of 50% is D50(90), the loss tangent tanδ at a temperature of 150°C and a distortion of 1% is D1(150), and the loss tangent tanδ at a temperature of 150°C and a distortion of 50% is D50(150), D1(90), D50(90), D1(150), and D50(150) are each 0.5 to 2.5, the value of D50(150)-D1(150) is less than 1.5, and the value of D50(90)-D1(90) is less than 1.0; and 3 More than 4.0g / cm 3 and a carrier, Hereinafter, a toner having D1(90), D50(90), D1(150), and D50(150) inclusive is 0.5 or more and 2.5 or less, the value of D50(150)-D1(150) is less than 1.5, and the value of D50(90)-D1(90) is less than 1.0 will be referred to as a "specific toner", and a toner having a true specific gravity of 3.0 g / cm 3 More than 4.0g / cm 3 Hereinafter, the carrier in question is also referred to as the "first specific carrier."
[0026] The developer according to the first aspect has the above-mentioned constitution, so that the difference in glossiness between the fixed image under low temperature and low pressure conditions and the fixed image under high temperature and high pressure conditions is small, and image fogging is suppressed. The reason for this is presumed to be as follows. In the following, the difference in glossiness between the fixed image under low temperature and low pressure conditions and the fixed image under high temperature and high pressure conditions is also referred to as the "glossiness condition difference".
[0027] As described above, in order to obtain good fixing properties, it is considered to use a developer containing a toner that is easily melted by heating. On the other hand, when an image is formed using a developer containing a toner that is easily melted by heating, the gloss condition difference may become large. This is presumably because the deformation amount of toner particles at high temperature and high strain amount is larger than the deformation amount of toner particles at low temperature and low strain amount.
[0028] In addition, when an image is formed using a developer containing a toner that is easily melted by heating, fogging may occur on the image. For example, when a developer containing a toner and a carrier is stirred in a developing device, the external additive of the toner may be embedded in the toner particles due to the mechanical load from the carrier. In the toner in which the external additive is embedded in the toner particles, the chargeability of the toner itself decreases because the external additive has difficulty in retaining the charge, and the fluidity of the toner decreases because the fluidity improvement effect of the external additive cannot be obtained, which reduces the contact opportunity with the carrier and makes it difficult to be charged, which makes fogging more likely to occur. In addition, when a carrier with a low true specific gravity is used to reduce the mechanical load from the carrier, friction is less likely to occur when the toner and carrier come into contact, and charging due to friction is less likely to occur, which makes fogging more likely to occur.
[0029] In contrast, in the first embodiment, a specific toner is used, that is, a toner in which D1(90), D50(90), D1(150), and D50(150) are each 0.5 or more and 2.5 or less, the value of D50(150)-D1(150) is less than 1.5, and the value of D50(90)-D1(90) is less than 1.0. Here, a strain of 1% in dynamic viscoelasticity measurement means that a displacement of 1% is applied relative to the height of the sample (i.e., the gap). In other words, a strain of 1% is the application of a small amount of displacement, and corresponds to a case where the fixing device pressure is low in the toner fixing process. On the other hand, a strain of 50% corresponds to a case where the fixing device pressure is high in the toner fixing process. A temperature of 90°C and a strain of 1% correspond to fixing conditions at low temperature and low pressure, and a temperature of 150°C and a strain of 50% correspond to fixing conditions at high temperature and high pressure, and each loss tangent tan δ corresponds to the amount of toner deformation under each fixing condition. In the specific toner, the change in loss tangent relative to the change in the amount of distortion is small both at 90° C. and 150° C. Therefore, it is presumed that the toner has similar viscoelasticity at high temperature and high distortion and at low temperature and low distortion, so that even when an image is fixed under high temperature and high pressure conditions, a fixed image having a small difference in gloss compared to an image fixed under low temperature and low pressure conditions can be obtained.
[0030] In the first embodiment, a specific toner having D1(90), D50(90), D1(150), and D50(150) all being 0.5 or more and 2.5 or less, and a toner having a true specific gravity of 3.0 g / cm 3 More than 4.0g / cm 3 The toner having the appropriate viscoelasticity and the carrier having the appropriate low specific gravity are combined to suppress embedding of the external additive in the toner particles, and are also likely to cause triboelectric charging when the toner and the carrier come into contact with each other, which is believed to make it difficult for image fog to occur.
[0031] For the above reasons, it is presumed that in the first aspect, the difference in gloss condition is small and image fog is suppressed.
[0032] The loss tangent of the toner is determined as follows. Specifically, a measurement sample is prepared by molding the toner to be measured into a tablet shape at room temperature (25° C.) using a press molding machine. Then, using this measurement sample, dynamic viscoelasticity measurement is performed using a rheometer under the following conditions, and the loss tangent tanδ at a temperature of 90° C. or 150° C. and a strain of 1% or 50% is obtained from each of the obtained curves of the storage modulus and loss modulus, to obtain D1(90), D50(90), D1(150), and D50(150). -Measurement conditions- Measurement device: Rheometer ARES-G2 (manufactured by TA Instruments) Measurement jig: 8mm parallel plate Gap: Adjusted to 3mm Frequency: 1Hz
[0033] The method for obtaining the specific toner is not particularly limited. As a method for obtaining the specific toner, for example, a toner having a storage modulus G' of 1×10 in the range of 90° C. to 150° C. in dynamic viscoelasticity measurement at a temperature rise of 2° C. / min is 4 Pa or more 1×10 6 One method is to incorporate resin particles having a surface roughness of not more than 1 Pa evenly into both the region close to the surface and the region close to the center of the toner particle. The storage modulus G' in the range of 90°C to 150°C is 1×10 4 Pa or more 1×10 6 Resin particles having a viscosity of 0.1 Pa or less are also referred to as "specific resin particles". The reason why the specific toner can be easily obtained by dispersing the specific resin particles evenly in both the region close to the surface of the toner particle and the region close to the center of the toner particle is not clear, but is presumed to be as follows.
[0034] As mentioned above, the specific resin particles have a storage modulus G' of 1×10 4The specific resin particles are particles having a high elastic modulus at high temperatures. Therefore, it is presumed that the toner particles contain the specific resin particles, so that the loss tangent of the toner as a whole at high temperature and high strain is unlikely to be high, and the difference with the loss tangent of the toner as a whole at low temperature and low strain is small. In particular, it is presumed that by dispersing specific resin particles evenly in both the region close to the surface of the toner particle and the region close to the center of the toner particle, the loss tangent of the toner at both low temperature, low distortion and high temperature, high distortion is reduced, and the difference between the two is also reduced, making it easier to obtain a specific toner.
[0035] The storage modulus G' of the resin particles, as well as the loss tangent tan δ and the glass transition temperature Tg, which will be described later, are determined as follows. Specifically, a disk-shaped sample with a thickness of 2 mm and a diameter of 8 mm is prepared by applying pressure to the resin particles to be measured, and used as the measurement sample. When measuring the resin particles contained in the toner particles, the resin particles are removed from the toner particles before preparing the measurement sample. Examples of methods for removing the resin particles from the toner particles include a method in which the toner particles are immersed in a solvent that dissolves the binder resin but not the resin particles, and the binder resin is dissolved in the solvent to remove the resin particles. The obtained disk-shaped sample is sandwiched between parallel plates with a diameter of 8 mm, and the measurement temperature is raised from 10°C to 150°C at a rate of 2°C / min with a strain of 0.1 to 100%, to perform dynamic viscoelasticity measurement under the following conditions. The storage modulus G' and loss tangent tanδ are obtained from the curves of the storage modulus and loss modulus obtained by the measurement. The peak temperature of the loss tangent tanδ is defined as the glass transition temperature Tg. -Measurement conditions- Measurement device: Rheometer ARES-G2 (manufactured by TA Instruments) Gap: Adjusted to 3mm Frequency: 1Hz
[0036] The true specific gravity of the carrier is measured by the pycnometer method specified in JIS K0061:2001 "Method of measuring density and specific gravity of chemical products." The method for controlling the true specific gravity of the carrier is not particularly limited. For example, the true specific gravity of the carrier can be controlled by increasing or decreasing the amount of resin contained in the magnetic particles while containing the resin, by increasing or decreasing the coverage of the resin layer, or the like.
[0037] <Second aspect> The developer according to a second aspect has the specific toner and a carrier including core particles in which a magnetic powder is dispersed in a resin, and the content of the magnetic powder relative to the entire carrier is more than 80% by mass and less than 90% by mass. Hereinafter, a carrier that includes core particles in which magnetic powder is dispersed in a resin and in which the content of magnetic powder in the entire carrier is more than 80 mass % and less than 90 mass % is also referred to as a "second specific carrier". The developer according to the second aspect has the above-mentioned structure, and thus the gloss condition difference is small and image fog is suppressed. The reason for this is presumed to be as follows.
[0038] As described above, when an image is formed using a developer containing a toner that is easily melted by heating in order to obtain good fixing properties, not only does the difference in glossiness conditions become large, but fogging may also occur on the image. In contrast, in the second embodiment, a fixed image with a small gloss condition difference is obtained by using a specific toner. In addition, in the second embodiment, a specific toner in which D1(90), D50(90), D1(150), and D50(150) are all 0.5 or more and 2.5 or less is used in combination with a second specific carrier in which the magnetic powder content is more than 80% by mass and less than 90% by mass. The second specific carrier has a smaller specific gravity than a carrier in which the magnetic powder content is 90% by mass or more. Therefore, in addition to suppressing embedding of the external additive in the toner particles, it is presumed that the combination of a carrier with a moderately small specific gravity and a toner with moderate viscoelasticity makes it easier for frictional charging to occur when the toner and carrier come into contact, making it less likely for image fog to occur. For the above reasons, it is presumed that in the second embodiment, the difference in gloss condition is small and image fog is suppressed.
[0039] Hereinafter, a developer that corresponds to both the developer according to the first aspect and the developer according to the second aspect will be referred to as a “developer according to the present embodiment.” An example of the developer of the present invention may be a developer that corresponds to at least one of the developer according to the first aspect and the developer according to the second aspect. The toner and carrier contained in the developer according to this embodiment will be described in detail below.
[0040] <Toner> The toner according to the present embodiment includes toner particles and an external additive.
[0041] (Toner particles) The toner particles contain at least a binder resin, and may contain other components as necessary. The toner particles preferably further contain resin particles in addition to the binder resin. Furthermore, it is presumed that the toner particles contain resin particles, so that the amount of deformation of the toner fixed image due to the fixing pressure is suppressed, and a fixed image with a small difference in glossiness can be obtained.
[0042] The resin particles are preferably crosslinked resin particles. The term "crosslinked resin particles" as used herein refers to resin particles having a bridge structure between specific atoms in the polymer structure contained in the resin particles. By using crosslinked resin particles as the resin particles, the specific resin particles tend to have a storage modulus G' within the above range at temperatures of 90° C. or higher and 150° C. or lower, and the specific toner tends to be obtained.
[0043] The crosslinked resin particles are preferably styrene (meth)acrylic resin particles. When the crosslinked resin particles are styrene (meth)acrylic resin particles, the specific resin particles tend to have a storage modulus G' within the above range at 90° C. or higher and 150° C. or lower, and the specific toner tends to be obtained.
[0044] As described above, from the viewpoint of obtaining a specific toner, the toner particles preferably contain specific resin particles as the resin particles. Hereinafter, as an example of the toner particles contained in the specific toner, toner particles containing a binder resin and specific resin particles will be described. The toner particles are composed of, for example, a binder resin, specific resin particles, and, if necessary, a colorant, a release agent, and other additives.
[0045] -Binding resin- Examples of the binder resin include vinyl resins made of homopolymers of monomers such as styrenes (e.g., styrene, parachlorostyrene, α-methylstyrene, etc.), (meth)acrylic acid esters (e.g., methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, lauryl methacrylate, 2-ethylhexyl methacrylate, etc.), ethylenically unsaturated nitriles (e.g., acrylonitrile, methacrylonitrile, etc.), vinyl ethers (e.g., vinyl methyl ether, vinyl isobutyl ether, etc.), vinyl ketones (vinyl methyl ketone, vinyl ethyl ketone, vinyl isopropenyl ketone, etc.), and olefins (e.g., ethylene, propylene, butadiene, etc.), or copolymers of two or more of these monomers. Examples of the binder resin include non-vinyl resins such as epoxy resins, polyester resins, polyurethane resins, polyamide resins, cellulose resins, polyether resins, and modified rosin, mixtures of these with the vinyl resins, and graft polymers obtained by polymerizing vinyl monomers in the coexistence of these. These binder resins may be used alone or in combination of two or more kinds.
[0046] The binder resin preferably contains a polyester resin. By including a polyester resin as the binder resin, when styrene (meth)acrylic resin particles are used as the specific resin particles, the difference (SP value (S)-SP value (R)) between the solubility parameter SP value (S) of the specific resin particles described later and the solubility parameter SP value (R) of the binder resin tends to be within a preferred numerical range. This makes it easier for the specific resin particles to disperse in the toner particles, and as a result, the gloss condition difference is reduced. By having the difference (SP value (S)-SP value (R)) in the above range, the affinity between the binder resin and the specific resin particles is high, which prevents partial compatibility and a decrease in dispersibility, compared to when the difference is too small. Also, by having the difference (SP value (S)-SP value (R)) in the above range, the affinity between the binder resin and the specific resin particles is low, which prevents the specific resin particles from being encapsulated within the toner particles and being discharged to the surface of the toner particles or outside the toner particles, compared to when the difference is too large.
[0047] The binder resin preferably contains a crystalline resin and an amorphous resin. Here, the crystalline resin refers to a resin that has a clear endothermic peak rather than a stepwise change in endothermic amount in differential scanning calorimetry (DSC). On the other hand, an amorphous resin is one that, in thermal analysis measurement using differential scanning calorimetry (DSC), has only a step-like endothermic change rather than a clear endothermic peak, is a solid at room temperature, and becomes thermoplastic at a temperature equal to or higher than the glass transition temperature. Specifically, for example, a crystalline resin means a resin whose half-width of an endothermic peak is within 10°C when measured at a heating rate of 10°C / min, and an amorphous resin means a resin whose half-width exceeds 10°C or a resin in which no clear endothermic peak is observed.
[0048] The crystalline resin will now be described. The crystalline resin may be a crystalline polyester resin, a crystalline vinyl resin (e.g., polyal Examples of the crystalline resin include known crystalline resins such as xylene resins and long-chain alkyl (meth)acrylate resins. Among these, crystalline polyester resins are preferred from the viewpoints of the mechanical strength and low-temperature fixability of the toner.
[0049] Crystalline polyester resin The crystalline polyester resin may be, for example, a polycondensate of a polyvalent carboxylic acid and a polyhydric alcohol. The crystalline polyester resin may be a commercially available product or a synthesized product. Here, the crystalline polyester resin is preferably a polycondensate using a polymerizable monomer having a linear aliphatic group rather than a polymerizable monomer having an aromatic group, since the crystalline polyester resin can easily form a crystalline structure.
[0050] Examples of polyvalent carboxylic acids include aliphatic dicarboxylic acids (e.g., oxalic acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, 1,18-octadecanedicarboxylic acid, etc.), aromatic dicarboxylic acids (e.g., dibasic acids such as phthalic acid, isophthalic acid, terephthalic acid, naphthalene-2,6-dicarboxylic acid, etc.), anhydrides thereof, and lower alkyl esters thereof (e.g., having 1 to 5 carbon atoms). The polyvalent carboxylic acid may be a trivalent or higher carboxylic acid having a crosslinked or branched structure in combination with a dicarboxylic acid. Examples of the trivalent carboxylic acid include aromatic carboxylic acids (e.g., 1,2,3-benzenetricarboxylic acid, 1,2,4-benzenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, etc.), their anhydrides, and their lower alkyl esters (e.g., carbon number 1 to 5). As the polyvalent carboxylic acid, a dicarboxylic acid having a sulfonic acid group and a dicarboxylic acid having an ethylenic double bond may be used in combination with these dicarboxylic acids. The polyvalent carboxylic acids may be used alone or in combination of two or more kinds.
[0051] Examples of polyhydric alcohols include aliphatic diols (for example, straight-chain aliphatic diols having 7 to 20 carbon atoms in the main chain). Examples of aliphatic diols include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, and 1,14-eicosanedecanediol. Among these, 1,8-octanediol, 1,9-nonanediol, and 1,10-decanediol are preferred as aliphatic diols. The polyhydric alcohol may be a trihydric or higher alcohol having a crosslinked or branched structure in combination with the diol. Examples of the trihydric or higher alcohol include glycerin, trimethylolethane, trimethylolpropane, and pentaerythritol. The polyhydric alcohols may be used alone or in combination of two or more kinds.
[0052] Here, the polyhydric alcohol has an aliphatic diol content of 80 mol % or more, preferably 90 mol % or more.
[0053] The melting temperature of the crystalline polyester resin is preferably 50°C or higher and 100°C or lower, more preferably 55°C or higher and 90°C or lower, and even more preferably 60°C or higher and 85°C or lower. The melting temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC) based on the "melting peak temperature" described in the method for determining melting temperature in JIS K7121-1987 "Method for measuring transition temperature of plastics."
[0054] The weight average molecular weight (Mw) of the crystalline polyester resin is preferably 6,000 or more and 35,000 or less.
[0055] The crystalline polyester resin can be obtained by a known manufacturing method, for example, in the same manner as the amorphous polyester.
[0056] When the toner particles contain a crystalline resin, the content of the crystalline resin relative to the total binder resin is preferably 4% by mass or more and 50% by mass or less, more preferably 6% by mass or more and 30% by mass or less, and even more preferably 8% by mass or more and 20% by mass or less. By having the crystalline resin content in the above range, better fixability is easily obtained compared to when the content is less than the above range. Also, by having the crystalline resin content in the above range, compared to when the content is more than the above range, the glossiness of the fixed image fixed under high temperature and high pressure conditions is prevented from excessively increasing due to the relatively low elasticity crystalline resin being too much. As a result, the glossiness condition difference is reduced.
[0057] The amorphous resin will now be described. Examples of the amorphous resin include known amorphous resins such as amorphous polyester resin, amorphous vinyl resin (e.g., styrene-acrylic resin, etc.), epoxy resin, polycarbonate resin, polyurethane resin, etc. Among these, amorphous polyester resin and amorphous vinyl resin (particularly styrene-acrylic resin) are preferred, and amorphous polyester resin is more preferred.
[0058] Amorphous polyester resin The amorphous polyester resin may be, for example, a condensation polymer of a polyvalent carboxylic acid and a polyhydric alcohol. The amorphous polyester resin may be a commercially available product or a synthesized product.
[0059] Examples of polyvalent carboxylic acids include aliphatic dicarboxylic acids (e.g., oxalic acid, malonic acid, maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, succinic acid, alkenylsuccinic acid, adipic acid, sebacic acid, etc.), alicyclic dicarboxylic acids (e.g., cyclohexanedicarboxylic acid, etc.), aromatic dicarboxylic acids (e.g., terephthalic acid, isophthalic acid, phthalic acid, naphthalenedicarboxylic acid, etc.), anhydrides thereof, and lower alkyl esters thereof (e.g., having 1 to 5 carbon atoms). Among these, aromatic dicarboxylic acids are preferable as polyvalent carboxylic acids. The polyvalent carboxylic acid may be a trivalent or higher carboxylic acid having a crosslinked or branched structure in combination with a dicarboxylic acid. Examples of the trivalent or higher carboxylic acid include trimellitic acid, pyromellitic acid, anhydrides thereof, and lower (e.g., carbon number 1 to 5) alkyl esters thereof. The polyvalent carboxylic acids may be used alone or in combination of two or more kinds.
[0060] Examples of polyhydric alcohols include aliphatic diols (e.g., ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, butanediol, hexanediol, neopentyl glycol, etc.), alicyclic diols (e.g., cyclohexanediol, cyclohexanedimethanol, hydrogenated bisphenol A, etc.), and aromatic diols (e.g., ethylene oxide adducts of bisphenol A, propylene oxide adducts of bisphenol A, etc.). Among these, examples of polyhydric alcohols include aromatic diols and alicyclic diols, and more preferably aromatic diols. As the polyhydric alcohol, a polyhydric alcohol having a crosslinked or branched structure of three or more may be used in combination with the diol. Examples of the polyhydric alcohol having a trihydric or higher valence include glycerin, trimethylolpropane, and pentaerythritol. The polyhydric alcohols may be used alone or in combination of two or more kinds.
[0061] The glass transition temperature (Tg) of the amorphous polyester resin is preferably 50°C or higher and 80°C or lower, and more preferably 50°C or higher and 65°C or lower. The glass transition temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC), more specifically, from the "extrapolated glass transition onset temperature" described in the method for determining glass transition temperature in JIS K 7121-1987 "Method for measuring transition temperature of plastics."
[0062] The weight average molecular weight (Mw) of the amorphous polyester resin is preferably 5,000 or more and 1,000,000 or less, and more preferably 7,000 or more and 500,000 or less. The number average molecular weight (Mn) of the amorphous polyester resin is preferably 2,000 or more and 100,000 or less. The molecular weight distribution Mw / Mn of the amorphous polyester resin is preferably 1.5 or more and 100 or less, and more preferably 2 or more and 60 or less. The weight average molecular weight and number average molecular weight are measured by gel permeation chromatography (GPC). The molecular weight measurement by GPC is performed using a Tosoh GPC HLC-8120GPC as the measuring device, a Tosoh TSKgel SuperHM-M (15 cm) column, and THF solvent. The weight average molecular weight and number average molecular weight are calculated from the measurement results using a molecular weight calibration curve created with a monodisperse polystyrene standard sample.
[0063] The amorphous polyester resin can be obtained by a known manufacturing method, for example, by carrying out the reaction while removing water and alcohol generated during condensation by setting the polymerization temperature to 180° C. or higher and 230° C. or lower, and reducing the pressure in the reaction system as necessary. If the raw material monomer is not soluble or compatible at the reaction temperature, a high boiling point solvent may be added as a solubilizing agent to dissolve it. In this case, the polycondensation reaction is carried out while distilling off the solubilizing agent. If a monomer with poor compatibility is present, it is recommended that the monomer with poor compatibility is condensed in advance with the acid or alcohol to be polycondensed, and then polycondensed with the main component.
[0064] The binder resin preferably contains a polyester resin having an aliphatic dicarboxylic acid unit (i.e., a structural unit derived from an aliphatic dicarboxylic acid). When the polyester resin, which is the binder resin, has an aliphatic dicarboxylic acid unit, the flexibility of the binder resin is increased compared to when the binder resin has only an aromatic dicarboxylic acid unit, so that the specific resin particles can be dispersed in a state closer to uniformity, and the variation range of the loss tangent tanδ can be reduced.
[0065] In addition, the binder resin preferably contains an amorphous polyester resin having an aliphatic dicarboxylic acid unit and a crystalline polyester resin having an aliphatic dicarboxylic acid unit. When the binder resin contains an amorphous polyester resin and a crystalline polyester resin, the specific resin particles can be more uniformly dispersed by both of them having an aliphatic dicarboxylic acid unit.
[0066] In addition, examples of the aliphatic dicarboxylic acid include the dicarboxylic acid represented by the general formula "HOOC-(CH2) n In the above general formula, n is preferably 4 to 20, and more preferably 4 to 12.
[0067] The content of the binder resin is, for example, preferably from 40% by mass to 95% by mass, more preferably from 50% by mass to 90% by mass, and even more preferably from 60% by mass to 85% by mass, based on the total amount of the toner particles.
[0068] The ratio of the content of the crystalline resin to the content of the specific resin particles is preferably 0.2 or more and 10 or less, and more preferably 1 or more and 5 or less, assuming that the content of the specific resin particles is 1. By keeping the ratio of the crystalline resin content to the specific resin particle content within the above range, compared to when the ratio is less than 0.2, the amount of low-viscosity components in the toner at temperatures between 90°C and 150°C and the contribution of the specific resin particles, which are highly elastic components, is increased, thereby suppressing the decrease in the melting property of the toner and improving the fixing property. In addition, by keeping the ratio of the crystalline resin content to the specific resin particle content within the above range, the amount of reduced components is prevented from becoming excessive, which would result in an increase in the amount of deformation of the toner due to the heat and pressure applied by the fixing device, compared to when the ratio exceeds 10, and the difference in glossiness due to fixing conditions is reduced. The ratio of the content of the amorphous resin to the content of the specific resin particles is preferably 1.3 or more and 45 or less, and more preferably 3 or more and 15 or less, assuming that the content of the specific resin particles is 1.
[0069] -Specific resin particles- The specific resin particles have a storage modulus G' of 1 x 10 in the range of 90°C to 150°C in dynamic viscoelasticity measurement at a temperature rise of 2°C / min. 4 Pa or more 1×10 6 There are no particular limitations on the resin particles as long as they have a modulus of 0.1 Pa or less. The storage modulus G' of the specific resin particles in the range of 90°C to 150°C is 1×10 5 Pa or more 8×10 5 Pa or less, and 1×10 5 Pa or more 6×10 5 It is more preferable that the pressure is 0.1 Pa or less. By using resin particles having a storage modulus G' in the range of 90°C to 150°C in the above range, excessive increase in glossiness of the fixed image fixed under high temperature and high pressure conditions is suppressed compared to the case where resin particles having a lower storage modulus G' than the above range are used. This reduces the glossiness condition difference. In addition, by using resin particles having a storage modulus G' in the range of 90°C to 150°C in the above range, deterioration of fixability caused by the elasticity of the toner particles being too high is suppressed compared to the case where resin particles having a higher storage modulus G' than the above range are used, and good fixability is easily obtained.
[0070] The specific resin particles preferably have a loss tangent tanδ of 0.01 to 2.5 in the range of 30° C. to 150° C. in dynamic viscoelasticity measurement at a temperature rise rate of 2° C. / min. The specific resin particles more preferably have a loss tangent tanδ of 0.01 to 1.0 in the range of 65° C. to 150° C., and even more preferably have a loss tangent tanδ of 0.01 to 0.5 in the range of 65° C. to 150° C. By setting the loss tangent tanδ of the specific resin particles in the above range in the range of 30° C. to 150° C., the toner particles are more likely to deform during fixing, and good fixing properties are more likely to be obtained, compared to when the temperature is lower than the above range. Furthermore, by setting the loss tangent tanδ of the specific resin particles in the above range in the range of 65° C. to 150° C., which is the temperature at which the toner particles are more likely to deform, the glossiness of the fixed image fixed under high temperature and high pressure conditions is suppressed from increasing excessively, compared to when the temperature is higher than the above range. This reduces the difference in glossiness conditions.
[0071] ·Crosslinked resin particles The specific resin particles are preferably crosslinked resin particles. Here, in order to include the specific resin particles in the toner particles, it is preferable that the specific resin particles have a high affinity with the binder resin.Specific methods for increasing the affinity include controlling the SP value and using a surfactant as a dispersant for the specific resin particles.However, when using specific resin particles having a high affinity with the binder resin, the specific resin particles are composed of organic polymers, unlike inorganic fillers, carbon black, metal particles, etc., and therefore tend to be compatible with the binder resin, and dispersibility may decrease. On the other hand, when specific resin particles having low affinity with the binder resin are used, they are difficult to be included in the toner particles and may be discharged onto the surface of the toner particles or outside the toner particles.
[0072] By using specific resin particles having an intermediate affinity between specific resin particles having a high affinity with the binder resin and specific resin particles having a low affinity, it is possible to include the specific resin particles in the toner particles to a certain extent, but regardless of the toner manufacturing method such as the emulsion aggregation method or the kneading and grinding method, when the specific resin particles come into contact with each other, they have a high affinity because they are made of the same type of material, and they may maintain a state of contact and be unevenly distributed, making it difficult to evenly distribute the specific resin particles in the toner particles. One of the reasons why the specific resin particles maintain a state of contact with each other is thought to be that the polymer chains of the polymer component that constitutes the specific resin particles become entangled when they come into contact. Therefore, by using crosslinked resin particles as the specific resin particles, it becomes possible to suppress entanglement of polymer chains, to prevent the polymer chains from remaining in contact with each other, and to distribute the polymer chains evenly throughout the toner particles.
[0073] Examples of the crosslinked resin particles include crosslinked resin particles crosslinked by ionic bonds (ionically crosslinked resin particles), crosslinked resin particles crosslinked by covalent bonds (covalently crosslinked resin particles), etc. Among these, the crosslinked resin particles are preferably crosslinked resin particles crosslinked by covalent bonds.
[0074] The types of resins used in the crosslinked resin particles include polyolefin resins (polyethylene, polypropylene, etc.), styrene resins (polystyrene, α-polymethylstyrene, etc.), (meth)acrylic resins (polymethyl methacrylate, polyacrylonitrile, etc.), epoxy resins, polyurethane resins, polyurea resins, polyamide resins, polycarbonate resins, polyether resins, polyester resins, and copolymer resins thereof. These resins may be used alone or in combination of two or more types, as necessary.
[0075] Of the above resins, the resin used for the crosslinked resin particles is preferably a styrene (meth)acrylic resin, which is a copolymer resin of a styrene-based resin and a (meth)acrylic resin. That is, the crosslinked resin particles are preferably styrene (meth)acrylic resin particles. The styrene (meth)acrylic resin may be, for example, a resin obtained by radical polymerization of the following styrene-based monomer and (meth)acrylic acid-based monomer.
[0076] Examples of styrene monomers include styrene, α-methylstyrene, vinylnaphthalene, alkyl-substituted styrenes having alkyl chains such as 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2-ethylstyrene, 3-ethylstyrene, and 4-ethylstyrene, halogen-substituted styrenes such as 2-chlorostyrene, 3-chlorostyrene, and 4-chlorostyrene, and fluorine-substituted styrenes such as 4-fluorostyrene and 2,5-difluorostyrene, etc. Among these, styrene and α-methylstyrene are preferred.
[0077] Examples of (meth)acrylic acid monomers include (meth)acrylic acid, n-methyl (meth)acrylate, n-ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, n-decyl (meth)acrylate, n-dodecyl (meth)acrylate, n-lauryl (meth)acrylate, n-tetradecyl (meth)acrylate, n-hexadecyl (meth)acrylate, n-octadecyl (meth)acrylate, isopropyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, isopentyl (meth)acrylate, amyl (meth)acrylate, Examples of such acrylates include neopentyl (meth)acrylate, isohexyl (meth)acrylate, isoheptyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, phenyl (meth)acrylate, biphenyl (meth)acrylate, diphenylethyl (meth)acrylate, t-butylphenyl (meth)acrylate, terphenyl (meth)acrylate, cyclohexyl (meth)acrylate, t-butylcyclohexyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, methoxyethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-carboxyethyl (meth)acrylate, (meth)acrylonitrile, and (meth)acrylamide. Among these, n-butyl (meth)acrylate and 2-carboxyethyl (meth)acrylate are preferred.
[0078] Examples of crosslinking agents for crosslinking the resin in the crosslinked resin particles include aromatic polyvinyl compounds such as divinylbenzene and divinylnaphthalene; polyvinyl esters of aromatic polyvalent carboxylic acids such as divinyl phthalate, divinyl isophthalate, divinyl terephthalate, divinyl homophthalate, divinyl trimesate, trivinyl trimesate, divinyl naphthalenedicarboxylate, and divinyl biphenylcarboxylate; divinyl esters of nitrogen-containing aromatic compounds such as divinyl pyridinedicarboxylate; vinyl esters of unsaturated heterocyclic compound carboxylic acids such as vinyl pyrromucate, vinyl furancarboxylate, vinyl pyrrole-2-carboxylate, and vinyl thiophenecarboxylate; butanediol diacrylate, butanediol dimethacrylate, hexanediol diacrylate, hexanediol dimethacrylate, octanediol diacrylate, octanediol dimethacrylate, nonanediol diacrylate, nonanediol dimethacrylate, decanediol diacrylate, decanedi ... (Meth)acrylic acid esters of linear polyhydric alcohols such as diol dimethacrylate, dodecane diol diacrylate, and dodecane diol dimethacrylate; (meth)acrylic acid esters of branched or substituted polyhydric alcohols such as neopentyl glycol dimethacrylate and 2-hydroxy, 1,3-diacryloxypropane; polyethylene glycol di(meth)acrylate, polypropylene polyethylene glycol di(meth)acrylates, divinyl succinate, divinyl fumarate, and maleic acid Examples of the crosslinking agent include polyvinyl esters of polyvalent carboxylic acids such as vinyl, divinyl maleate, divinyl diglycolate, vinyl itaconate, divinyl itaconate, divinyl acetonedicarboxylate, divinyl glutarate, divinyl 3,3'-thiodipropionate, divinyl trans-aconitate, trivinyl trans-aconitate, divinyl adipate, divinyl pimelate, divinyl suberate, divinyl azelaate, divinyl sebacate, divinyl dodecanedioate, and divinyl brassylate. The crosslinking agent may be used alone or in combination of two or more.
[0079] Among these, it is preferable to use a bifunctional alkyl acrylate having an alkylene chain with 6 or more carbon atoms as a crosslinking agent for crosslinking the resin. In other words, it is preferable that the crosslinked resin particles have a bifunctional alkyl acrylate as a constituent unit, and the alkylene chain in the bifunctional alkyl acrylate has 6 or more carbon atoms. The specific toner can be obtained more easily by using crosslinked resin particles having a bifunctional alkyl acrylate as a constituent unit and having 6 or more carbon atoms in the alkylene chain. In the specific toner, it is important to suppress the deformation amount of the toner particles to a certain range even under high pressure fixing conditions in order to suppress the gloss difference. If the difference in elasticity between the specific resin particles, which are crosslinked resin particles, and the binder resin is too large, it may be difficult to obtain the effect of suppressing the change in the loss tangent tan δ by the specific resin particles. For this reason, it is preferable to control the elasticity of the specific resin particles so that it does not become too high. If the crosslink density of the specific resin particles is high (i.e., the distance between the crosslinking points is short), the elasticity becomes too high, whereas if a bifunctional acrylate having a long alkylene chain is used as a crosslinking agent, the crosslink density becomes low (i.e., the distance between the crosslinking points is long), and the elasticity of the specific resin particles can be suppressed from becoming too high. As a result, the gloss difference can be further suppressed.
[0080] From the viewpoint of adjusting the crosslink density to an appropriate range, the number of carbon atoms in the alkylene chain in the bifunctional alkyl acrylate is preferably 6 or more, more preferably 6 to 12, and even more preferably 8 to 12. More specific examples of the bifunctional alkyl acrylate include 1,6-hexanediol acrylate, 1,6-hexanediol methacrylate, 1,8-octanediol diacrylate, 1,8-octanediol dimethacrylate, 1,9-nonanediol diacrylate, 1,9-nonanediol dimethacrylate, 1,10-decanediol diacrylate, 1,10-decanediol dimethacrylate, 1,12-dodecanediol diacrylate, and 1,12-dodecanediol dimethacrylate, and among these, 1,10-decanediol diacrylate and 1,10-decanediol dimethacrylate are preferred.
[0081] In addition, when the specific resin particles are polymers of a composition for forming specific resin particles containing a styrene-based monomer, a (meth)acrylic acid-based monomer, and a crosslinking agent, the amount of the crosslinking agent contained in the composition may be adjusted to control the viscoelasticity of the specific resin particles. For example, by increasing the amount of the crosslinking agent contained in the composition, resin particles having a high storage modulus G' are easily obtained. The content of the crosslinking agent in the composition for forming specific resin particles is, for example, preferably 0.3 parts by mass or more and 5.0 parts by mass or less, more preferably 0.5 parts by mass or more and 2.5 parts by mass or less, and even more preferably 1.0 parts by mass or more and 2.0 parts by mass or less, relative to 100 parts by mass of the total of the styrene-based monomer, the (meth)acrylic acid-based monomer, and the crosslinking agent.
[0082] The glass transition temperature Tg of the specific resin particles determined by dynamic viscoelasticity measurement is preferably 10° C. or more and 45° C. or less. When the glass transition temperature Tg of the specific resin particles is 10° C. or more and 45° C. or less, the toner has better fixing properties and reduces the difference in gloss between an image fixed under low temperature and low pressure conditions and an image fixed under high temperature and high pressure conditions. Furthermore, the glass transition temperature Tg of the specific resin particles is preferably 15°C or higher and 40°C or lower, and more preferably 20°C or higher and 35°C or lower. When the glass transition temperature Tg of the specific resin particles is within the above range, the difference with the Tg of the binder resin becomes large, and the resin particles are prevented from being easily unevenly distributed in the toner particles, and the specific resin particles are easily maintained in a nearly uniform dispersion state, and the effect of suppressing deformation due to pressure during fixing is easily obtained, and the gloss difference is small. Also, when the glass transition temperature Tg of the specific resin particles is within the above range, the deterioration of low-temperature fixing property caused by the deterioration of the melting property of the binder resin is suppressed, compared to when the Tg is too high.
[0083] The number average particle diameter of the specific resin particles is preferably 60 nm or more and 300 nm or less, more preferably 100 nm or more and 200 nm or less, and even more preferably 130 nm or more and 170 nm or less. By having the number-average particle diameter of the specific resin particles in the above range, the toner particles are more susceptible to the effect of the high elasticity of the specific resin particles, and the toner particles are less susceptible to the effect of the high elasticity of the specific resin particles, and good fixability is obtained. Also, by having the number-average particle diameter of the specific resin particles in the above range, the specific resin particles are more likely to be dispersed in a nearly uniform state within the toner particles, compared to when the number-average particle diameter is larger than the above range, and the toner is more likely to have similar viscoelasticity at high temperature and low temperature. This reduces the gloss condition difference.
[0084] The number average particle size of the specific resin particles is a value measured using a transmission electron microscope (TEM). As a transmission electron microscope, for example, JEM-1010 manufactured by JEOL Datum Co., Ltd. can be used. Hereinafter, a method for measuring the number average particle diameter of the specific resin particles will be specifically described. The toner particles are cut into pieces with a thickness of about 0.3 μm using a microtome. The cross sections of the toner particles are photographed at 4,500 times magnification using a transmission electron microscope, and the circular equivalent diameters of 1,000 resin particles dispersed in the toner particles are calculated from the individual cross-sectional areas, and the arithmetic average of these is taken as the number-average particle diameter. The number average particle diameter of the specific resin particles may be a value obtained by measuring a dispersion of the specific resin particles using a laser diffraction particle size distribution measuring device (for example, LA-700 manufactured by Horiba, Ltd.).
[0085] The specific resin particles are preferably contained evenly in both a region close to the surface of the toner particle (hereinafter also referred to as the "surface region") and a region close to the center of the toner particle (hereinafter also referred to as the "center region"). By containing the specific resin particles in both the surface region and the center region, the gloss condition difference is reduced compared to the case where the specific resin particles are contained only in either the surface region or the center region. For example, when the specific resin particles are contained only in the surface region, the deformation amount of the toner particles is small under low temperature and low pressure conditions due to the influence of viscoelasticity in the surface region, whereas the deformation amount of the toner particles is large under high temperature and high pressure conditions due to the influence of viscoelasticity in the center region. Therefore, the gloss condition difference may become large. Also, when the specific resin particles are contained only in the center region, the deformation amount of the toner particles is small under low temperature and low pressure conditions, and the dispersion state of the specific resin particles in the fixed image is poor (unevenly distributed), whereas the deformation amount of the toner particles is large under high temperature and high pressure conditions, and the dispersion state of the specific resin particles in the fixed image is likely to be good (close to uniform). When the dispersion state of the specific resin particles in the fixed image is poor, the part where the specific resin particles are present is easily deformed and becomes a convex part, whereas the part where the specific resin particles are not present is easily deformed and becomes a concave part, thereby reducing the gloss. When the dispersion state is good, the above-mentioned state is suppressed, and the gloss increases. Therefore, the gloss condition difference may become large. In contrast, when specific resin particles are contained in both the surface region and the central region, it is presumed that the gloss condition difference is reduced, unlike when the particles are contained only in the surface region or only in the central region.
[0086] The content of the specific resin particles is preferably from 2% by mass to 30% by mass, more preferably from 5% by mass to 25% by mass, and even more preferably from 8% by mass to 20% by mass, based on the total mass of the toner particles. By the content of the specific resin particles being within the above range, the toner tends to have a similar viscoelasticity at high temperature and low temperature, and the gloss condition difference is reduced, compared with the case where the content is less than the above range. Also, by the content of the specific resin particles being within the above range, the deterioration of fixability due to the toner particles having too high elasticity is suppressed, and good fixability is obtained, compared with the case where the content is more than the above range.
[0087] -Coloring agent- Examples of colorants include carbon black, chrome yellow, Hansa Yellow, benzidine yellow, threne yellow, quinoline yellow, pigment yellow, permanent orange GTR, pyrazolone orange, Balkan orange, watch young red, permanent red, brilliant carmine 3B, brilliant carmine 6B, DuPont oil red, pyrazolone red, lithol red, rhodamine B lake, lake red C, pigment red, rose bengal, aniline blue, ultramarine blue, and tetrahydrofuran. Examples of the dyes include various pigments such as phosphorus blue, chalcoil blue, methylene blue chloride, phthalocyanine blue, pigment blue, phthalocyanine green, and malachite green oxalate, and various dyes such as acridine-based, xanthene-based, azo-based, benzoquinone-based, azine-based, anthraquinone-based, thioindigo-based, dioxazine-based, thiazine-based, azomethine-based, indigo-based, phthalocyanine-based, aniline black-based, polymethine-based, triphenylmethane-based, diphenylmethane-based, and thiazole-based dyes. The colorant may be used alone or in combination of two or more kinds.
[0088] The colorant may be surface-treated as necessary, or may be used in combination with a dispersant. In addition, a plurality of types of colorants may be used in combination.
[0089] The content of the colorant is, for example, preferably from 1% by mass to 30% by mass, and more preferably from 3% by mass to 15% by mass, based on the total mass of the toner particles.
[0090] -Release agent- Examples of the release agent include hydrocarbon waxes, natural waxes such as carnauba wax, rice wax, and candelilla wax, synthetic or mineral / petroleum waxes such as montan wax, and ester waxes such as fatty acid esters and montan acid esters. The release agent is not limited to these.
[0091] The melting temperature of the release agent is preferably 50°C or higher and 110°C or lower, and more preferably 60°C or higher and 100°C or lower. The melting temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC) based on the "melting peak temperature" as described in the method for determining melting temperature in JIS K 7121-1987 "Method for measuring transition temperature of plastics."
[0092] The content of the release agent is, for example, preferably from 1% by mass to 20% by mass, and more preferably from 5% by mass to 15% by mass, based on the total amount of the toner particles.
[0093] -Other additives- Examples of other additives include well-known additives such as magnetic materials, charge control agents, inorganic powders, etc. These additives are contained in the toner particles as internal additives.
[0094] -Relationship between the composition of toner particles- Difference (SP value (S) - SP value (R)) The difference between the solubility parameter SP (S) of the specific resin particles and the solubility parameter SP (R) of the binder resin (SP (S)-SP (R)) is preferably -0.32 or more and -0.12 or less.
[0095] When the difference (SP value (S)-SP value (R)) is within the above range, the affinity between the binder resin constituting the majority of the toner particles and the specific resin particles is maintained at a moderate level, and the specific resin particles are more likely to disperse uniformly within the toner particles than when the difference is smaller than the above range. This makes it easier to obtain a toner having similar viscoelasticity at high temperature and high distortion and at low temperature and low distortion, reducing the difference in gloss conditions. In other words, compared to when the difference (SP value (S)-SP value (R)) is smaller than the above range, it is less likely that the affinity between the binder resin and the specific resin particles is too high, causing the specific resin particles to move easily within the toner particles, causing some of the specific resin particles to aggregate, and reducing the effect of the specific resin particles. In addition, when the difference (SP value (S) - SP value (R)) is within the above range, the increase in melt viscosity of the entire toner caused by excessive mixing and compatibility of the specific resin particles and the binder resin during toner melting is suppressed, compared to when the difference is greater than the above range. This has the advantage of suppressing the decrease in fixability caused by too high viscoelasticity, and obtaining good fixability. When the binder resin is a mixed resin, the solubility parameter of the resin having the largest content in the binder resin is defined as the SP value (R).
[0096] The difference (SP value (S) - SP value (R)) is more preferably -0.32 or more and -0.12 or less, and further preferably -0.29 or more and -0.18 or less.
[0097] The solubility parameter SP value (S) of the specific resin particles is preferably 9.00 or more and 9.15 or less, more preferably 9.03 or more and 9.12 or less, and even more preferably 9.06 or more and 9.10 or less.
[0098] Here, the solubility parameter SP value (S) of the specific resin particles and the solubility parameter SP value (R) of the binder resin (unit: (cal / cm 3 ) 1 / 2 ) is calculated by the Okitsu method. The Okitsu method is described in detail in the Journal of the Adhesion Society of Japan, Vol. 29, No. 5 (1993).
[0099] Viscoelasticity of components excluding specific resin particles (excluded components) The storage modulus G' of the toner particles excluding the specific resin particles in the range of 30°C to 50°C is 1 x 10 8 Pa or more, and the storage modulus G' is 1×10 5 Less than Pa The temperature at which the toner particle reaches the storage elastic modulus G' is preferably 65° C. or higher and 90° C. or lower. Hereinafter, the components excluding the specific resin particles from the toner particles are also referred to as "excluded components", and the storage elastic modulus G' is preferably 1×10 5The temperature at which the storage modulus G' of an excluded component satisfies the above condition is called the "specific elastic modulus reaching temperature". The storage modulus G' of an excluded component satisfies the above condition, and the elastic modulus is high at low temperatures and low at temperatures between 65°C and 90°C. Therefore, when the storage modulus G' of an excluded component satisfies the above condition, the storage modulus G' is 1×10 5 When the temperature reaches less than 1 Pa, the toner particles are more easily melted by heating than when the temperature exceeds 90° C., resulting in good fixability.
[0100] The storage modulus G' of the excluded components at temperatures between 30°C and 50°C is 1×10 8 Pa or more, and 1×10 8 Pa or more 1×10 9 Pa or less is more preferable, and 2×10 8 Pa or more 6×10 8 It is more preferable that the pressure is 0.1 Pa or less. When the storage modulus G' of the excluded component at 30°C or higher and 50°C or lower is within the above range, the toner has better storage stability than when the storage modulus G' is lower than the above range, and better fixing properties are more likely to be obtained than when the storage modulus G' is higher than the above range.
[0101] The specific elastic modulus attainment temperature of the excluded components is preferably 65°C or higher and 90°C or lower, more preferably 68°C or higher and 80°C or lower, and even more preferably 70°C or higher and 75°C or lower. When the specific elastic modulus reaching temperature of the excluded component is within the above range, the storage stability of the toner is better than when the specific elastic modulus reaching temperature is lower than the above range, and better fixability is more easily obtained than when the specific elastic modulus reaching temperature is higher than the above range.
[0102] The loss tangent tan δ of the excluded component at the specific elastic modulus reaching temperature is preferably 0.8 or more and 1.6 or less, more preferably 0.9 or more and 1.5 or less, and even more preferably 1.0 or more and 1.4 or less. By setting the loss tangent tanδ of the excluded component at the specific elastic modulus reaching temperature within the above range, better fixability is obtained than when the loss tangent tanδ is lower than the above range. Also, by setting the loss tangent tanδ of the excluded component at the specific elastic modulus reaching temperature within the above range, the gloss condition difference is reduced compared to when the loss tangent tanδ is higher than the above range.
[0103] The storage modulus G' and loss tangent tan δ of the excluded component are determined as follows. Specifically, first, the resin particles are removed from the toner particles to extract only the removed components, and the removed components are molded into a tablet shape at 25° C. using a press molding machine to prepare a measurement sample. Examples of a method for removing the resin particles from the toner particles to extract only the removed components include a method in which the toner particles are immersed in a solvent that dissolves the binder resin but does not dissolve the resin particles, and the removed components are extracted and extracted. The obtained measurement sample is then sandwiched between parallel plates with a diameter of 8 mm, and the measurement temperature is raised from 30°C to 150°C at a rate of 2°C / min with a strain of 0.1 to 100%, to perform dynamic viscoelasticity measurement under the following conditions: The storage modulus G' and loss tangent tanδ are determined from the respective curves of the storage modulus and loss modulus obtained by the measurement. -Measurement conditions- Measurement device: Rheometer ARES-G2 (manufactured by TA Instruments) Measurement jig: 8mm parallel plate Gap: Adjusted to 3mm Frequency: 1Hz
[0104] Relationship between specific resin particles, toner particles, and excluded components In the range of 90°C to 150°C, the storage modulus of the specific resin particles is G'(p90-150), the storage modulus of the toner particles is G'(t90-150), and the storage modulus of the components excluding the specific resin particles from the toner particles is G'(r90-150). 50) is 1 x 10 4 Pa or more 1×10 6Pa or less, and logG'(t90-150)-logG'(r90-150) is preferably 1.0 or more and 4.0 or less. Furthermore, the value of logG'(t90-150)-logG'(r90-150) is more preferably 1.0 or more and 3.5 or less, further preferably 1.1 or more and 3.4 or less, and particularly preferably 1.2 or more and 3.3 or less. The value of logG'(t90-150)-logG'(r90-150) means the difference in viscoelasticity of toner particles depending on whether or not the specific resin particles are added. By dispersing and containing the specific resin particles in a nearly uniform state in the toner particles, the effect of the viscoelasticity of the specific resin particles on the viscoelasticity of the entire toner particles is suppressed, and by controlling the value of logG'(t90-150)-logG'(r90-150) to the above range, both good fixability and reduced gloss condition difference are achieved compared to when the value is smaller or larger than the above range.
[0105] -Characteristics of toner particles, etc.- The toner particles may be toner particles having a single layer structure, or may be toner particles having a so-called core-shell structure composed of a core portion (core particle) and a coating layer (shell layer) that coats the core portion. Here, the toner particles having a core-shell structure may be composed of, for example, a core portion containing a binder resin, specific resin particles, and, if necessary, other additives such as a colorant and a release agent, and a coating layer containing a binder resin and specific resin particles.
[0106] When the toner particles have a core-shell structure, it is preferable that the specific resin particles are contained in both the core particles and the shell layer. By containing the specific resin particles in both the core particles and the shell layer, the specific resin particles are contained in both the surface region and the central region of the toner particles, so that the gloss condition difference is further reduced.
[0107] The volume average particle size (D50v) of the toner particles is preferably from 2 μm to 10 μm, more preferably from 4 μm to 8 μm, and even more preferably from 4 μm to 6 μm.
[0108] The various average particle sizes and particle size distribution indexes of the toner particles are measured using a Coulter Multisizer II (manufactured by Beckman Coulter, Inc.), and the electrolyte is measured using an ISOTON-II (manufactured by Beckman Coulter, Inc.). For the measurement, 0.5 mg to 50 mg of the measurement sample is added to 2 ml of a 5% aqueous solution of a surfactant (preferably sodium alkylbenzene sulfonate) as a dispersant, and this is then added to 100 ml to 150 ml of the electrolyte. The electrolyte with the sample suspended in it is dispersed for 1 minute using an ultrasonic disperser, and the particle size distribution of particles with diameters in the range of 2 μm to 60 μm is measured using a Coulter Multisizer II with an aperture diameter of 100 μm. The number of particles sampled is 50,000. Based on the measured particle size distribution, cumulative distributions of volume and number are drawn for each divided particle size range (channel) from the smallest diameter side, and the particle size at 16% of the cumulative size is defined as the volume particle size D16v, the number particle size D16p, the particle size at 50% of the cumulative size as the volume average particle size D50v, the cumulative number average particle size D50p, and the particle size at 84% of the cumulative size as the volume particle size D84v and number particle size D84p. Using these, the volumetric particle size distribution index (GSDv) is (D84v / D16v) 1 / 2 The number size distribution index (GSDp) is (D84p / D16p) 1 / 2 It is calculated as:
[0109] The average circularity of the toner particles is preferably 0.94 or more and 1.00 or less, and more preferably 0.95 or more and 0.98 or less.
[0110] The average circularity of toner particles is calculated by (circular equivalent perimeter) / (perimeter) [(perimeter of a circle having the same projected area as the particle image) / (perimeter of the particle projected image)]. Specifically, it is a value measured by the following method. First, the toner particles to be measured are sucked and collected, flattened, and a still image of the particles is captured by instantaneous strobe light emission, and the particle image is analyzed by a flow-type particle image analyzer (FPIA-3000 manufactured by Sysmex Corporation). The number of samples to be taken in order to calculate the average circularity is 3,500. When the toner contains an external additive, the toner (developer) to be measured is dispersed in water containing a surfactant, and then ultrasonic treatment is performed to obtain toner particles from which the external additive has been removed.
[0111] Number average molecular weight of tetrahydrofuran solubles The number average molecular weight of the tetrahydrofuran soluble matter in the toner particles is preferably from 5000 to 15000. Hereinafter, the tetrahydrofuran soluble matter is also referred to as "THF soluble matter". By having the number average molecular weight of the THF soluble matter in the toner particles be 5000 or more and 15000 or less, the change in loss tangent with respect to the change in the amount of strain is small, and even if the toner has high viscoelasticity and the amount of deformation is suppressed, high fixability can be obtained. Specifically, by having the number average molecular weight of the THF soluble matter in the above range, the amount of deformation of the toner particles is increased under high-temperature and high-pressure fixing conditions due to the presence of a large amount of low-molecular-weight components in the toner particles, and the gloss difference is suppressed compared to when the number average molecular weight is too small. In addition, by having the number average molecular weight of the THF soluble matter in the above range, the amount of deformation of the toner particles is suppressed due to the presence of a large amount of high-molecular-weight components in the toner particles, and low-temperature fixability is suppressed compared to when the number average molecular weight is too large. It is more preferable that the number average molecular weight of the THF soluble matter is 7000 or more and 10000 or less.
[0112] The number average molecular weight of the THF-soluble portion of the toner particles is measured using two "HLC-8120GPC, SC-8020 (6.0 mm ID x 15 cm, manufactured by Tosoh Corporation)" and tetrahydrofuran (THF) as an eluent to prepare the THF-soluble portion of the toner particles. Specifically, 0.5 mg of toner particles to be measured is dissolved in 1 g of THF, and the solution is subjected to ultrasonic dispersion, and then the concentration is adjusted to 0.5% by mass. Measurements are performed using an RI detector under conditions of a sample concentration of 0.5% by mass, a flow rate of 0.6 ml / min, a sample injection amount of 10 μl, and a measurement temperature of 40°C. In addition, the calibration curve is prepared from 10 samples of "Polystyrene standard sample TSK standard" manufactured by Tosoh Corporation: "A-500", "F-1", "F-10", "F-80", "F-380", "A-2500", "F-4", "F-40", "F-128", and "F-700".
[0113] When obtaining toner particles from toner containing external additives, for example, the toner is dispersed in an aqueous solution of 0.2% by mass of polyoxyethylene (10) octylphenyl ether to a concentration of 10% by mass, and the external additives are liberated by applying ultrasonic vibration (frequency 20 kHz, output 30 W) for 60 minutes while maintaining a temperature of 30° C. or less. The toner particles are filtered and washed from the resulting dispersion to obtain toner particles from which the external additives have been removed.
[0114] (External additives) Examples of the external additive include inorganic particles, such as SiO2, TiO2, Al2O3, CuO, ZnO, SnO2, CeO2, Fe2O3, MgO, BaO, CaO, K2O, Na2O, ZrO2, CaO·SiO2, K2O·(TiO2)n, Al2O3·2SiO2, CaCO3, MgCO3, BaSO4, and MgSO4.
[0115] The surface of the inorganic particles as an external additive may be subjected to a hydrophobic treatment. The hydrophobic treatment may be performed, for example, by immersing the inorganic particles in a hydrophobic treatment agent. The hydrophobic treatment agent is not particularly limited, and examples thereof include silane coupling agents, silicone oils, titanate coupling agents, and aluminum coupling agents. These may be used alone or in combination of two or more. The amount of the hydrophobizing agent is usually, for example, 1 part by mass or more and 10 parts by mass or less per 100 parts by mass of the inorganic particles.
[0116] Examples of external additives include resin particles (resin particles such as polystyrene, polymethyl methacrylate (PMMA), and melamine resin), cleaning agents (for example, metal salts of higher fatty acids such as zinc stearate, and fluorine-based polymer particles).
[0117] The amount of the external additive added is, for example, preferably from 0.01% by mass to 5% by mass, and more preferably from 0.01% by mass to 2.0% by mass, based on the toner particles.
[0118] (Toner characteristics) - Viscoelasticity of toner - As described above, the toner according to the present embodiment is a specified toner, in other words, D1(90), D50(90), D1(150), and D50(150) are all 0.5 or more and 2.5 or less, the value of D50(150)-D1(150) is less than 1.5, and the value of D50(90)-D1(90) is less than 1.0.
[0119] D1(90) in the specific toner is 0.5 or more and 2.5 or less, preferably 0.5 or more and 2.0 or less, more preferably 0.6 or more and 1.8 or less, even more preferably 0.8 or more and 1.6 or less, and particularly preferably 1.0 or more and 1.5 or less. The D50(90) of the specific toner is from 0.5 to 2.5, preferably from 0.5 to 2.0, more preferably from 0.6 to 1.8, even more preferably from 0.8 to 1.6, and particularly preferably from 1.1 to 1.6. D1(150) in the specific toner is 0.5 or more and 2.5 or less, preferably 0.5 or more and 2.0 or less, more preferably 0.5 or more and 1.5 or less, even more preferably 0.55 or more and 1.0 or less, and particularly preferably 0.55 or more and 0.8 or less. The D50(150) of the specific toner is from 0.5 to 2.5, preferably from 0.8 to 2.2, more preferably from 1.0 to 2.0, even more preferably from 1.2 to 1.9, and particularly preferably from 1.4 to 1.7. When D1(90), D50(90), D1(150), and D50(150) are all within the above ranges, image fog is suppressed compared to when they are smaller or larger than the above ranges. Also, when D1(90), D50(90), D1(150), and D50(150) are all within the above ranges, better fixability is obtained compared to when they are smaller than the above ranges, and gloss condition differences are reduced compared to when they are larger than the above ranges.
[0120] The value of D50(150)-D1(150) in the specific toner is less than 1.5, preferably 1.2 or less, and more preferably 1.0 or less. When the value of D50(150)-D1(150) is within the above range, the gloss condition difference is reduced compared to when the value is greater than the above range. From the viewpoint of reducing the gloss condition difference, the smaller the value of D50(150)-D1(150), the more preferable. The lower limit of the value of D50(150)-D1(150) is not particularly limited.
[0121] The value of D50(90)-D1(90) in the specific toner is less than 1.0, preferably less than 0.5, more preferably 0.4 or less, and even more preferably 0.3 or less. By having the value of D50(90)-D1(90) in the above range, the gloss condition difference is reduced compared to when the value is greater than the above range. From the viewpoint of reducing the gloss condition difference, the smaller the value of D50(90)-D1(90), the more preferable. The lower limit of the value of D50(90)-D1(90) is not particularly limited.
[0122] The storage modulus G' of the toner in the range of 30°C to 50°C is 1×10 8 Pa or more, and the storage modulus G' is 1×10 5The temperature at which the storage elastic modulus G' reaches less than 1×10 Pa (i.e., the specific elastic modulus reaching temperature) is preferably 65° C. or higher and 90° C. or lower. A toner whose storage elastic modulus G' satisfies the above condition has a high elastic modulus at low temperatures and a low elastic modulus at temperatures from 65° C. to 90° C. Therefore, when the storage elastic modulus G' of a toner satisfies the above condition, the storage elastic modulus G' is 1×10 5 When the temperature reaches less than 1 Pa, the toner is more easily melted by heating than when the temperature exceeds 90° C., resulting in good fixability.
[0123] The storage modulus G' of the toner at 30°C to 50°C is 1×10 8 Pa or more, and 1×10 8 Pa or more 1×10 9 Pa is more preferable, and 2×10 8 Pa or more 6×10 8 It is more preferable that the pressure is 0.1 Pa or less. When the storage modulus G' of the toner at 30°C or higher and 50°C or lower is in the above range, the toner has better storage stability than when the storage modulus G' is lower than the above range, and better fixability is more likely to be obtained than when the storage modulus G' is higher than the above range.
[0124] The specific elastic modulus reaching temperature of the toner is preferably 65° C. or higher and 90° C. or lower, more preferably 70° C. or higher and 87° C. or lower, and even more preferably 75° C. or higher and 84° C. or lower. When the specific elastic modulus reaching temperature of the toner is within the above range, the toner has better storage stability than when it is lower than the above range, and better fixability is more likely to be obtained than when it is higher than the above range.
[0125] The storage elastic modulus G' and the specific elastic modulus reaching temperature of the toner are determined as follows. Specifically, the toner to be measured is molded into a tablet shape at room temperature (25°C) using a press molding machine to prepare a measurement sample. The obtained measurement sample is then sandwiched between parallel plates with a diameter of 8 mm, and the measurement temperature is raised from 30°C to 150°C at a rate of 2°C / min with a strain of 0.1 to 100%, to perform dynamic viscoelasticity measurement under the following conditions. The storage modulus G' is calculated from the curves of the storage modulus and loss modulus obtained by the measurement. -Measurement conditions- Measurement device: Rheometer ARES-G2 (manufactured by TA Instruments) Measurement jig: 8mm parallel plate Gap: Adjusted to 3mm Frequency: 1Hz
[0126] (Toner manufacturing method) Next, a method for producing the toner according to the present embodiment will be described. The toner according to the exemplary embodiment can be obtained by producing toner particles and then adding an external additive to the toner particles, if necessary.
[0127] The toner particles may be produced by any of a dry production method (e.g., a kneading and pulverizing method, etc.) and a wet production method (e.g., an aggregation-coalescence method, a suspension polymerization method, a dissolution suspension method, etc.). The method for producing the toner particles is not particularly limited, and a well-known production method is adopted. Among these, it is preferable to obtain toner particles by the aggregation and coalescence method.
[0128] Specifically, for example, when toner particles are produced by the aggregation and coalescence method, The toner particles are manufactured through a process including a step of preparing a resin particle dispersion in which resin particles to be the binder resin are dispersed, and a specific resin particle dispersion in which the specific resin particles are to be dispersed (resin particle dispersion preparation process), a step of aggregating the resin particles (or other particles, if necessary) in the resin particle dispersion (in a dispersion after mixing other particle dispersions, if necessary) to form aggregated particles (aggregated particle formation process), and a step of heating the aggregated particle dispersion in which the aggregated particles are dispersed, to fuse and coalesce the aggregated particles, thereby forming toner particles (fusion and coalescence process).
[0129] Each step will be described in detail below. In the following description, a method for obtaining toner particles containing a colorant and a release agent will be described, but the colorant and the release agent are used as necessary. Of course, additives other than the colorant and the release agent may be used.
[0130] -Resin particle dispersion preparation process- First, a resin particle dispersion in which resin particles serving as a binder resin are dispersed, as well as a colorant particle dispersion in which colorant particles are dispersed and a release agent particle dispersion in which release agent particles are dispersed are prepared.
[0131] Here, the resin particle dispersion liquid is prepared, for example, by dispersing resin particles in a dispersion medium with the aid of a surfactant.
[0132] The dispersion medium used in the resin particle dispersion liquid is, for example, an aqueous medium. Examples of the aqueous medium include water such as distilled water and ion-exchanged water, alcohols, etc. These may be used alone or in combination of two or more kinds.
[0133] Examples of the surfactant include anionic surfactants such as sulfate salts, sulfonates, phosphates, and soaps; cationic surfactants such as amine salts and quaternary ammonium salts; and nonionic surfactants such as polyethylene glycols, alkylphenol ethylene oxide adducts, and polyhydric alcohols. Among these, anionic surfactants and cationic surfactants are particularly preferred. The nonionic surfactants may be used in combination with anionic surfactants or cationic surfactants. The surfactant may be used alone or in combination of two or more kinds.
[0134] In the resin particle dispersion, examples of the method for dispersing the resin particles in the dispersion medium include general dispersion methods using, for example, a rotary shear type homogenizer, a ball mill having a media, a sand mill, a dyno mill, etc. Depending on the type of resin particles, the resin particles may be dispersed in the resin particle dispersion using, for example, a phase inversion emulsification method. The phase inversion emulsification method is a method in which the resin to be dispersed is dissolved in a hydrophobic organic solvent in which the resin is soluble, a base is added to the organic continuous phase (O phase) to neutralize it, and then an aqueous medium (W phase) is added to effect conversion of the resin from W / O to O / W (so-called phase inversion), resulting in a discontinuous phase, and the resin is dispersed in particulate form in the aqueous medium.
[0135] The volume average particle size of the resin particles dispersed in the resin particle dispersion is, for example, preferably from 0.01 μm to 1 μm, more preferably from 0.08 μm to 0.8 μm, and even more preferably from 0.1 μm to 0.6 μm. The volume average particle size of the resin particles is calculated by using the particle size distribution obtained by measurement using a laser diffraction particle size distribution measuring device (e.g., LA-700 manufactured by Horiba, Ltd.), subtracting the cumulative distribution for the volume from the small particle size side for the divided particle size range (channel), and calculating the cumulative distribution for all particles by 5. The particle size at which the particle size becomes 0% is measured as the volume average particle size D50v. The volume average particle sizes of particles in other dispersions are also measured in the same manner.
[0136] The content of the resin particles in the resin particle dispersion is, for example, preferably from 5% by mass to 50% by mass, and more preferably from 10% by mass to 40% by mass.
[0137] In addition, for example, a colorant particle dispersion and a release agent particle dispersion are also prepared in the same manner as the resin particle dispersion. That is, the volume average particle size, dispersion medium, dispersion method, and particle content of the particles in the resin particle dispersion are the same for the colorant particles dispersed in the colorant particle dispersion and the release agent particles dispersed in the release agent particle dispersion.
[0138] Preparation of specific resin particle dispersion The specific resin particle dispersion can be prepared by any known method, such as emulsion polymerization, melt kneading using a Banbury mixer or kneader, suspension polymerization, spray drying, etc., with emulsion polymerization being preferred.
[0139] From the viewpoint of setting the storage modulus G' and loss tangent tan δ of the specific resin particles within a preferred range, it is preferable to use a styrene-based monomer and a (meth)acrylic acid-based monomer as the monomers and polymerize them in the presence of a crosslinking agent. In the production of the specific resin particles, it is preferable to carry out emulsion polymerization a number of times. The method for producing the specific resin particles will be described in more detail below.
[0140] The method for preparing the specific resin particle dispersion liquid includes the steps of: A step of obtaining an emulsion containing a monomer, a crosslinking agent, a surfactant, and water (an emulsion preparation step); a step of adding a polymerization initiator to the emulsion and polymerizing the monomers by heating (first emulsion polymerization step); a step of adding an emulsion containing a monomer and a crosslinking agent to the reaction solution after the first emulsion polymerization step and polymerizing the monomer by heating (second emulsion polymerization step); It is preferred that the compound contains
[0141] (Emulsion preparation process) This is a process for obtaining an emulsion containing a monomer, a crosslinking agent, a surfactant, and water. It is preferable to obtain an emulsion by emulsifying a monomer, a crosslinking agent, a surfactant, and water using an emulsifier. Examples of emulsifiers include rotary mixers equipped with propeller-type, anchor-type, paddle-type, or turbine-type stirring blades, static mixers such as static mixers, rotor-stator type emulsifiers such as homogenizers and Clearmix, mill-type emulsifiers equipped with a grinding function, high-pressure emulsifiers such as Manton-Gaulin pressure emulsifiers, high-pressure nozzle type emulsifiers that generate cavitation under high pressure, high-pressure collision type emulsifiers such as microfluidizers that apply shear force by colliding liquids together under high pressure, ultrasonic emulsifiers that generate cavitation using ultrasound, and membrane emulsifiers that perform uniform emulsification through fine pores.
[0142] As the monomer, it is preferable to use a styrene-based monomer and a (meth)acrylic acid-based monomer. As the crosslinking agent, those already mentioned are applicable.
[0143] Examples of the surfactant include anionic surfactants such as sulfate salts, sulfonates, phosphates, and soaps; cationic surfactants such as amine salts and quaternary ammonium salts; and nonionic surfactants such as polyethylene glycols, alkylphenol ethylene oxide adducts, and polyhydric alcohols. The nonionic surfactants may be used in combination with anionic surfactants or cationic surfactants. Among these, anionic surfactants are preferred. The surfactants may be used alone or in combination with two or more.
[0144] The emulsion may contain a chain transfer agent. There is no particular limitation on the chain transfer agent, but a compound having a thiol component can be used. Specifically, alkyl mercaptans such as hexyl mercaptan, heptyl mercaptan, octyl mercaptan, nonyl mercaptan, decyl mercaptan, and dodecyl mercaptan are preferred.
[0145] From the viewpoint of setting the storage modulus G' and loss tangent tanδ of the specific resin particles within a preferred range, the mass ratio of the styrene-based monomer and the (meth)acrylic acid-based monomer in the emulsion (styrene-based monomer / (meth)acrylic acid-based monomer) is preferably 0.2 or more and 1.1 or less. In order to set the storage modulus G' and loss tangent tan δ of the specific resin particles within preferred ranges, the content of the crosslinking agent in the entire emulsion is preferably 0.5% by mass or more and 3% by mass or less.
[0146] (First emulsion polymerization step) This is a process in which a polymerization initiator is added to the emulsion and then heated to polymerize the monomers. During polymerization, it is preferable to stir the emulsion (reaction solution) containing the polymerization initiator with a stirrer. The agitator may be a rotary agitator equipped with a propeller-type, anchor-type, paddle-type, or turbine-type agitator blade. As the polymerization initiator, ammonium persulfate is preferably used. In addition, when a polymerization initiator is used, the viscoelasticity of the obtained specific resin particles may be controlled by adjusting the amount of the polymerization initiator added. For example, by reducing the amount of the polymerization initiator added, resin particles having a high storage modulus G' are easily obtained.
[0147] (Second emulsion polymerization step) This is a step in which an emulsion containing a monomer is added to the reaction solution after the first emulsion polymerization step, and the monomer is polymerized by heating. During the polymerization, it is preferable to stir the reaction solution in the same manner as in the first emulsion polymerization step. In this step, the viscoelasticity of the specific resin particles obtained may be controlled by adjusting the time taken to add the emulsion containing the monomer. For example, by increasing the time taken to add the emulsion containing the monomer, resin particles having a high storage modulus G' are more likely to be obtained. The time taken to add the emulsion containing the monomer may be, for example, in the range of 2 hours to 5 hours. In addition, in this process, the viscoelasticity of the specific resin particles obtained may be controlled by adjusting the temperature when the reaction solution is stirred. For example, by lowering the temperature when the reaction solution is stirred, resin particles with a high storage modulus G' are easily obtained. The temperature when the reaction solution is stirred may be, for example, in the range of 55°C or more and 75°C or less. The emulsion containing the monomer is preferably obtained by emulsifying the monomer, a surfactant, and water using an emulsifier.
[0148] -Agglomerated particle formation process- Next, the colorant particle dispersion, the release agent particle dispersion, and the specific resin particle dispersion are mixed with the resin particle dispersion. Then, in the mixed dispersion, the resin particles, the colorant particles, the release agent particles, and the specific resin particles are hetero-aggregated to form aggregated particles containing the resin particles, the colorant particles, the release agent particles, and the specific resin particles and having a diameter close to the diameter of the target toner particles.
[0149] Specifically, for example, an aggregating agent is added to the mixed dispersion, the pH of the mixed dispersion is adjusted to be acidic (e.g., pH 2 or more and 5 or less), a dispersion stabilizer is added as necessary, and then the mixed dispersion is heated to a temperature of the glass transition temperature of the resin particles (specifically, for example, a temperature of the glass transition temperature of the resin particles -30°C or more and the glass transition temperature -10°C or less), and the particles dispersed in the mixed dispersion are aggregated to form aggregated particles. In the aggregated particle formation process, for example, the above-mentioned aggregating agent may be added to the mixed dispersion at room temperature (e.g., 25°C) while stirring the mixed dispersion with a rotary shear homogenizer, the pH of the mixed dispersion may be adjusted to an acidic state (e.g., pH 2 or more and 5 or less), and a dispersion stabilizer may be added as necessary, followed by the above-mentioned heating.
[0150] In this step, the temperature of the mixed dispersion liquid when the aggregating agent is added may be adjusted to control the dispersion state of the specific resin particles in the toner particles obtained. For example, the dispersibility of the specific resin particles is improved by lowering the temperature of the mixed dispersion liquid. The temperature of the mixed dispersion liquid may be, for example, in the range of 5°C to 40°C. In this step, the stirring speed after the addition of the aggregating agent may be adjusted to control the dispersion state of the specific resin particles in the toner particles obtained. For example, by increasing the stirring speed after the addition of the aggregating agent, the dispersibility of the specific resin particles becomes good.
[0151] Examples of the flocculant include a surfactant having a polarity opposite to that of the surfactant used as the dispersant added to the mixed dispersion, an inorganic metal salt, and a divalent or higher metal complex. In particular, when a metal complex is used as the flocculant, the amount of surfactant used is reduced and the charging characteristics are improved. If necessary, an additive that forms a complex or a similar bond with the metal ions of the flocculant may be used, and a chelating agent is preferably used as this additive.
[0152] Examples of inorganic metal salts include metal salts such as calcium chloride, calcium nitrate, barium chloride, magnesium chloride, zinc chloride, aluminum chloride, and aluminum sulfate, as well as inorganic metal salt polymers such as polyaluminum chloride, polyaluminum hydroxide, and calcium polysulfide. The chelating agent may be a water-soluble chelating agent, for example, oxycarboxylic acid such as tartaric acid, citric acid, gluconic acid, iminodiacetic acid (IDA), nitrilotriacetic acid (NTA), ethylenediaminetetraacetic acid (EDTA), etc. The amount of the chelating agent added is, for example, preferably 0.01 parts by mass or more and 5.0 parts by mass or less, and more preferably 0.1 parts by mass or more and less than 3.0 parts by mass, relative to 100 parts by mass of the resin particles.
[0153] -Fusion / unification process- Next, the aggregated particle dispersion liquid in which the aggregated particles are dispersed is heated, for example, to a temperature equal to or higher than the glass transition temperature of the resin particles (for example, a temperature 10 to 30° C. higher than the glass transition temperature of the resin particles) to fuse and coalesce the aggregated particles, thereby forming toner particles.
[0154] Through the above steps, toner particles are obtained. Note that, after obtaining an aggregated particle dispersion liquid in which the aggregated particles are dispersed, the toner particles may be manufactured through a process of further mixing the aggregated particle dispersion liquid, a resin particle dispersion liquid in which resin particles are dispersed, and a specific resin particle dispersion liquid in which specific resin particles are dispersed, and aggregating the aggregated particles so that the resin particles and the specific resin particles are further attached to the surfaces of the aggregated particles to form second aggregated particles, and a process of heating the second aggregated particle dispersion liquid in which the second aggregated particles are dispersed, to fuse and coalesce the second aggregated particles to form toner particles having a core / shell structure.
[0155] In the step of forming the second aggregated particles, the addition of the resin particle dispersion and the specific resin particle dispersion and the adhesion of the resin particles and the specific resin particles to the surfaces of the aggregated particles may be repeated multiple times, whereby toner particles in which the specific resin particles are evenly contained in both the surface region and the center region of the toner particles are obtained.
[0156] After the fusion and coalescence process, the toner particles formed in the solution are subjected to a known washing process, solid-liquid separation process, and drying process to obtain toner particles in a dried state. In the washing step, it is preferable to carry out sufficient replacement washing with ion-exchanged water from the viewpoint of electrostatic charge. In addition, the solid-liquid separation step is not particularly limited, but it is preferable to carry out suction filtration, pressure filtration, etc. from the viewpoint of productivity. In addition, in the drying step, there is no particular limit to the method, but it is preferable to carry out freeze drying, air flow drying, fluidized drying, vibration type fluidized drying, etc. from the viewpoint of productivity.
[0157] The toner according to the present embodiment is produced, for example, by adding an external additive to the obtained toner particles in a dry state and mixing them. The mixing may be performed, for example, by using a V blender, a Henschel mixer, a Loedige mixer, etc. Furthermore, if necessary, coarse particles of the toner may be removed using a vibration sieve, an air sieve, etc.
[0158] <Career> The form of the first specific carrier is not particularly limited, and examples thereof include a carrier having a core particle and a resin layer covering the surface of the core particle. The core particle is not particularly limited, and known magnetic particles used as the core material of carriers are applied.Specific examples of the core particle include magnetic metal particles such as iron, nickel, cobalt, etc.; magnetic oxide particles such as ferrite, magnetite, etc.; resin-impregnated magnetic particles in which porous magnetic powder is impregnated with resin; magnetic powder-dispersed resin particles in which magnetic powder is dispersed in resin; etc.The core particle is preferably a magnetic powder-dispersed resin particle in view of easy control of true specific gravity within the above range. The second specific carrier includes a core particle that is a magnetic powder-dispersed resin particle in which a magnetic powder is dispersed in a resin. The second specific carrier may have the above-mentioned core particle and a resin layer that covers the surface of the core particle. Hereinafter, as an example of the carrier used in the present embodiment, a carrier having core particles that are magnetic powder-dispersed resin particles and a resin layer that covers the surface of the core particle will be described.
[0159] (Core particle) The core particle, which is a magnetic powder-dispersed resin particle, contains magnetic powder and resin.
[0160] The magnetic powder is not particularly limited, and any conventionally known magnetic powder may be used.Specific examples include γ-iron oxide, ferrite, magnetite, etc., and ferrite and magnetite are preferably used because of their excellent stability, and magnetite is preferred because of their low cost.
[0161] An example of the ferrite is ferrite particles represented by the following structural formula: Structural formula: (MO) X (Fe2O3) Y (In the structural formula, M represents at least one metal element selected from Cu, Zn, Fe, Mg, Mn, Ca, Li, Ti, Ni, Sn, Sr, Al, Ba, Co, and Mo. In addition, X and Y represent a molar ratio, and X+Y=100 is satisfied.)
[0162] As the ferrite, among the structures represented by the above structural formula, examples of the structure in which M is represented by a plurality of metal elements include iron-based oxides such as Mn-Zn-based ferrite, Ni-Zn-based ferrite, Mn-Mg-based ferrite, Li-based ferrite, and Cu-Zn-based ferrite.
[0163] From the viewpoint of increasing the filling rate of the magnetic powder in the core particle and making it easier to control the specific gravity of the core particle, the volume average particle size of the magnetic powder is preferably 0.01 μm or more and 1 μm or less, more preferably 0.03 μm or more and 0.5 μm or less, and particularly preferably 0.05 μm or more and 0.35 μm or less. The volume average particle diameters of the magnetic powder, core particles, core material having a thin film layer formed on the surface of the core particles, and carrier in this embodiment are values measured by a laser diffraction particle size distribution measuring device LA-700 (manufactured by Horiba, Ltd.) Specifically, the particle size distribution obtained by the measuring device is divided into particle size ranges (channels), and the particle diameter at which the cumulative volume distribution is subtracted from the small particle size side to reach 50% of the cumulative volume is defined as the volume average particle diameter.
[0164] A suitable method for removing the resin coating layer from the carrier is to dissolve the resin coating layer with an organic solvent and separate the core particles or core material. More specifically, the method for removing the resin coating layer from the carrier may be, for example, the following method. Put 20 g of carrier into 100 mL of toluene. Apply ultrasonic waves at 40 kHz for 30 seconds. Separate the core particles or core material from the resin solution using any filter paper according to the particle size. Pour 20 mL of toluene over the core particles or core material remaining on the filter paper to wash it. Next, collect the core particles or core material remaining on the filter paper. Place the collected core particles or core material in 100 mL of toluene in the same way and apply ultrasonic waves at 40 kHz for 30 seconds. Filter in the same way, wash with 20 mL of toluene, and collect. Repeat this process 10 times in total. Finally, dry the collected core particles or core material.
[0165] The content of the magnetic powder in the core particles is set to more than 80% by mass and less than 90% by mass with respect to the entire carrier, or the true specific gravity of the entire carrier is set to 3.0 g / cm 3 More than 4.0g / cm 3 From the viewpoint of the above, the content is preferably more than 80% by mass and not more than 95% by mass, more preferably more than 80% by mass and not more than 90% by mass, and particularly preferably 82% by mass or more and not more than 85% by mass.
[0166] The resin constituting the core particles may be either a thermoplastic resin or a thermosetting resin, such as a vinyl resin, a polyester resin, an epoxy resin, a phenol resin, a urea resin, a polyurethane resin, a polyimide resin, a cellulose resin, a silicone resin, an acrylic resin, or a polyether resin. The resin may be one type or a mixture of two or more types.
[0167] The phenolic resin may be, for example, one obtained by reacting a phenol with formaldehyde. Core particles containing a phenolic resin as a resin may be obtained, for example, by reacting ferromagnetic iron compound particles, non-magnetic iron compound particles, phenols, and aldehydes in an aqueous medium in the presence of a basic catalyst. Examples of phenols include phenol itself, as well as compounds having a phenolic hydroxyl group, such as alkylphenols such as m-cresol, p-tert-butylphenol, o-propylphenol, resorcinol, and bisphenol A, and halogenated phenols in which the benzene nucleus or alkyl group is partially or entirely substituted with a chlorine atom or bromine atom. Of these, phenol is particularly preferred. Examples of the aldehydes include formaldehyde and paraformaldehyde. The molar ratio of the aldehydes to the phenols is preferably 1 to 2, and particularly preferably 1.1 to 1.6. If the molar ratio of the aldehydes to the phenols is less than 1, it is difficult to produce spherical composite particles, or even if they are produced, the strength of the produced particles tends to be weak because the curing of the resin is difficult to proceed, while if the molar ratio of the aldehydes to the phenols is greater than 2, the amount of unreacted aldehydes remaining in the aqueous medium after the reaction tends to increase. The basic catalyst used in this embodiment is one that is commonly used in the production of resol resins, such as aqueous ammonia, hexamethylenetetramine, and alkylamines such as dimethylamine, diethyltriamine, and polyethyleneimine. The molar ratio of these basic catalysts to phenols is preferably 0.02 or more and 0.3 or less. When the phenols and aldehydes are reacted in the presence of a basic catalyst, the amount of the ferromagnetic iron compound particles and non-magnetic iron compound particles to be coexisted is preferably 0.5 to 200 times by weight relative to the amount of the phenols, and more preferably 4 to 100 times, taking into consideration the strength of the resulting spherical composite particles.
[0168] Preferred examples of the vinyl resin include vinyl ether resins and N-vinyl resins. Among these vinyl resins, vinyl ether resins are preferred from the viewpoint of binding properties.
[0169] In particular, from the viewpoint of achieving both suppression of carrier deformation and charge retention performance, it is preferable that the resin in the core particle contains a phenol resin, it is more preferable that the phenol resin be contained in an amount of 50 mass% or more based on the total mass of the resin in the core particle, and it is particularly preferable that the phenol resin be contained in an amount of 80 mass% or more based on the total mass of the resin in the core particle.
[0170] The core particles may further contain other components depending on the purpose, such as a charge control agent and fluorine-containing particles.
[0171] The method for producing the core particles is not particularly limited, and examples thereof include a melt kneading method (JP Patent Publication No. 59-24416, JP Patent Publication No. 8-3679, etc.) in which the magnetic powder and resin are melt-kneaded using a Banbury mixer, kneader, etc., cooled, pulverized, and classified; a suspension polymerization method (JP Patent Publication No. 5-100493, etc.) in which monomer units of a binder resin and magnetic powder are dispersed in a solvent to prepare a suspension, and this suspension is polymerized; and a spray drying method in which magnetic powder is mixed and dispersed in a resin solution, and then spray-dried. The above melt kneading method, suspension polymerization method, and spray drying method all include a step of preparing magnetic powder in advance by some means, mixing this magnetic powder with resin, a resin monomer solution, or a resin solution, and dispersing the magnetic powder in the resin.
[0172] The magnetic force of the core particles is preferably 50 emu / g or more, more preferably 60 emu / g or more, in terms of saturation magnetization in a magnetic field of 3,000 oersteds. The saturation magnetization is measured using a vibrating sample magnetic measuring device VSMP10-15 (manufactured by Toei Kogyo Co., Ltd.). The measurement sample is packed in a cell with an inner diameter of 7 mm and a height of 5 mm and set in the device. The measurement is performed by applying a magnetic field and sweeping up to a maximum of 3,000 oersteds. The applied magnetic field is then reduced, and a hysteresis curve is prepared on a recording paper. The saturation magnetization, residual magnetization, and retentivity are determined from the data of the curve.
[0173] The volume resistivity of the core particle is 1×10 5 Ω cm or more 1×10 9 Ω cm or less is preferable, and 1×10 7 Ω cm or more 1×10 9 Ω·cm or less is more preferable. The volume resistivity (Ω·cm) of the core particles is measured as follows: 2 The object to be measured is placed flat on the surface of the circular jig on which the electrode plate is arranged, with a thickness of 1 mm to 3 mm, to form a layer. 2The layer is sandwiched between two electrode plates. In order to eliminate any gaps between the objects being measured, a 4 kg load is placed on the electrode plate placed on the layer, and then the thickness of the layer (cm) is measured. The top and bottom electrodes of the layer are connected to an electrometer and a high-voltage power supply generator. An electric field of 10 3.8 A high voltage is applied so that the resistance is V / cm, and the current value (A) that flows is read. The measurement environment is a temperature of 20°C and a relative humidity of 50%. The formula for calculating the volumetric electrical resistivity (Ω cm) of the measurement object is as shown below. R=E×20 / (I-I0) / L In the above formula, R is the volume resistivity (Ω cm) of the object to be measured, E is the applied voltage (V), I is the current value (A), I0 is the current value (A) at an applied voltage of 0 V, and L is the layer thickness (cm). The coefficient 20 is the area of the electrode plate (cm 2 )
[0174] From the viewpoint of suppressing embedding of external additives in the toner and ensuring the fluidity of the carrier, the volume average particle diameter of the core particles is preferably 25 μm or more and 40 μm or less, more preferably 25 μm or more and 38 μm or less, and particularly preferably 28 μm or more and 36 μm or less.
[0175] (Resin layer) The resin layer is a layer that covers the surface of the core particle and contains a resin. The resin layer may be a layer that covers at least a part of the surface of the magnetic particle. The resin layer may be a single layer or two or more layers. The resin layer preferably includes a first resin layer that covers the surface of the core particle and a second resin layer that covers the outer peripheral surface of the first resin layer. The second resin layer is a layer that includes a resin different from the resin included in the first resin layer. When the resin layer includes the first resin layer and the second resin layer, fogging of the image is suppressed. The reason for this is presumed to be that when the resin layer includes the first resin layer and the second resin layer, the charge stability of the carrier is improved. Specifically, for example, local charge leakage occurs in the carrier under high temperature and high humidity conditions, which may cause the charge of the carrier to become unstable and fogging to occur easily. In a carrier in which the resin layer includes the first resin layer and the second resin layer, it is presumed that the local charge leakage is less likely to occur, thereby suppressing fogging. The resin layer may include a resin layer other than the first resin layer and the second resin layer. The first resin layer is preferably a layer provided in contact with the core particle. The second resin layer is preferably the outermost layer. The resin layer is preferably a layer consisting of the first resin layer and the second resin layer. Hereinafter, the first resin layer is also referred to as a thin film layer, and the second resin layer is also referred to as a resin coating layer. The thin film layer and the resin coating layer will be described below. When there is only one resin layer, the resin layer may be the same as the resin coating layer described below.
[0176] -Thin film layer- The thin film layer is a layer provided between the core particle and the resin coating layer. There are no particular limitations on the thin film layer as long as it is a layer containing a resin different from that of the resin coating layer. Examples of the resin constituting the thin film layer include a melamine resin, a urethane resin, a urea resin, an epoxy resin, and a polyester resin. From the viewpoint of suppressing fogging of an image, the thin film layer preferably contains at least one selected from the group consisting of a melamine resin, a urethane resin, and a urea resin, and more preferably contains a melamine resin. It is presumed that the thin film layer contains a melamine resin, and the melamine resin contained in the thin film layer functions as a chargeability imparting agent, making it easier for the toner to be charged, thereby suppressing fogging.
[0177] The thin film layer may contain components other than the resin. Examples of the other components include charge control agents such as amine compounds and carboxylic acid compounds; conductive agents such as carbon black and tin oxide; etc. The content of the resin in the entire thin film layer is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more.
[0178] Methods for forming the thin film layer on the surface of the core particles include, for example, a wet method and a dry method. The wet method is a method that uses a solvent to dissolve or disperse the resin that constitutes the resin coating layer. On the other hand, the dry method is a method that does not use the above solvent. Examples of the wet manufacturing method include a dipping method in which core particles are dipped in a resin liquid for forming a thin film layer to coat them, etc. Examples of the dry manufacturing method include a method in which a mixture of core particles and a resin for forming a thin film layer is heated in a dry state to form a thin film layer. For example, when a thin film layer containing a melamine resin is formed on the surface of a core particle, a wet manufacturing method is preferably used. Specifically, the core particles are added to a solution containing melamine, formalin, and a solvent, and the solution is stirred and heated to obtain a core particle having a thin film layer containing a melamine resin. The solvent may be ion-exchanged water or the like.
[0179] From the viewpoints of charge retention and carrier resistance, the average thickness of the thin film layer is preferably from 0.05 μm to 1.50 μm, more preferably from 0.10 μm to 1.00 μm, and particularly preferably from 0.10 μm to 0.60 μm. The average thickness of the thin film layer and the average thickness of the resin coating layer described below are determined by the following method. The carrier is embedded in epoxy resin and cut with a microtome to prepare a carrier cross section. The SEM images of the carrier cross section taken with a scanning electron microscope (SEM) are imported into an image processing analyzer and subjected to image analysis. Ten locations per carrier particle are randomly selected to measure the thickness (μm) of the thin film layer and the resin coating layer, and then measurements are taken for 100 carriers, and the arithmetic mean of all measurements is calculated. These are regarded as the average thickness (μm) of the thin film layer and the average thickness (μm) of the resin coating layer, respectively.
[0180] The volume average particle size of the core material having a thin film layer formed on the core particle is preferably 25 μm or more and 40 μm or less, more preferably 25 μm or more and 38 μm or less, and particularly preferably 28 μm or more and 36 μm or less, from the viewpoint of suppressing embedding of external additives in the toner and ensuring the fluidity of the carrier. The content of the magnetic powder in the entire core material in which a thin film layer is formed on the core particles is set to be more than 80% by mass and less than 90% by mass in the entire carrier, or the true specific gravity of the entire carrier is set to 3.0 g / cm 3 More than 4.0g / cm 3 From the viewpoint of the above, the content is preferably more than 80% by mass and not more than 90% by mass, more preferably 82% by mass or more and 87% by mass or less, and particularly preferably 83% by mass or more and 85% by mass or less.
[0181] -Resin coating layer- The resin coating layer is a layer provided on the outer peripheral surface of the thin film layer. There are no particular limitations on the resin coating layer as long as it is a layer containing a resin different from the resin of the thin film layer. Examples of resins that make up the resin coating layer include styrene-acrylic acid copolymers; polyolefin resins such as polyethylene and polypropylene; polyvinyl or polyvinylidene resins such as polystyrene, acrylic resin, polyacrylonitrile, polyvinyl acetate, polyvinyl alcohol, polyvinyl butyral, polyvinyl chloride, polyvinyl carbazole, polyvinyl ether, and polyvinyl ketone; vinyl chloride-vinyl acetate copolymers; straight silicone resins or modified products thereof consisting of organosiloxane bonds; fluororesins such as polytetrafluoroethylene, polyvinyl fluoride, polyvinylidene fluoride, and polychlorotrifluoroethylene; polyesters; polyurethanes; polycarbonates; amino resins such as urea-formaldehyde resins; and epoxy resins. In particular, from the viewpoints of electrostatic charge and controllability of external additive adhesion, it is preferable that the resin constituting the resin coating layer contains an acrylic resin, it is more preferable that the acrylic resin is contained in an amount of 50 mass% or more based on the total mass of the resin in the resin coating layer, and it is particularly preferable that the acrylic resin is contained in an amount of 80 mass% or more based on the total mass of the resin in the resin coating layer.
[0182] From the viewpoint of suppressing charge fluctuations due to temperature and humidity, the resin coating layer preferably contains an acrylic resin having an alicyclic structure. As a polymerization component of the acrylic resin having an alicyclic structure, a lower alkyl ester of (meth)acrylic acid (for example, an alkyl (meth)acrylate ester having an alkyl group with 1 to 9 carbon atoms) is preferable, and specific examples thereof include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate. These monomers may be used alone or in combination of two or more. The acrylic resin having an alicyclic structure preferably contains cyclohexyl (meth)acrylate as a polymerization component. The content of the monomer unit derived from cyclohexyl (meth)acrylate contained in the acrylic resin having an alicyclic structure is preferably 75% by mass or more and 100% by mass or less, more preferably 85% by mass or more and 100% by mass or less, and even more preferably 95% by mass or more and 100% by mass or less, based on the total mass of the acrylic resin having an alicyclic structure.
[0183] The weight average molecular weight of the resin contained in the resin coating layer is preferably less than 300,000, more preferably less than 250,000, even more preferably from 5,000 to less than 250,000, and particularly preferably from 10,000 to 200,000. When within the above range, the resin is well wetted to the core material, and a resin coating layer with a uniform thickness can be obtained.
[0184] The resin coating layer may contain conductive particles for the purpose of controlling electrostatic charge and resistance. Examples of the conductive particles include carbon black, metals such as gold, silver, and copper, carbon black, titanium oxide, zinc oxide, tin oxide, barium sulfate, aluminum borate, and potassium titanate.
[0185] Methods for forming the resin coating layer on the outer peripheral surface of the thin film layer include, for example, a wet manufacturing method and a dry manufacturing method. The wet manufacturing method is a manufacturing method that uses a solvent that dissolves or disperses the resin that constitutes the resin coating layer. On the other hand, the dry manufacturing method is a manufacturing method that does not use the above-mentioned solvent.
[0186] Examples of the wet manufacturing method include a dipping method in which a core particle on which a thin film layer has been formed is dipped in a resin liquid for forming a resin coating layer to coat it; a spraying method in which a resin liquid for forming a resin coating layer is sprayed on the outer peripheral surface of the thin film layer; a fluidized bed method in which a core particle on which a thin film layer has been formed is fluidized in a fluidized bed and a resin liquid for forming a resin coating layer is sprayed on it; a kneader coater method in which a core particle on which a thin film layer has been formed is mixed with a resin liquid for forming a resin coating layer in a kneader coater and the solvent is removed; etc. These manufacturing methods may be repeated or combined. The resin liquid for forming the resin coating layer used in the wet manufacturing method is prepared by dissolving or dispersing the resin and other components in a solvent. The solvent is not particularly limited, and examples of the solvent that can be used include aromatic hydrocarbons such as toluene and xylene, ketones such as acetone and methyl ethyl ketone, and ethers such as tetrahydrofuran and dioxane.
[0187] The dry manufacturing method may be, for example, a method in which a mixture of core particles on which a thin film layer is formed and a resin for forming a resin coating layer is heated in a dry state to form a resin coating layer. Specifically, for example, the core particles on which a thin film layer is formed and the resin for forming a resin coating layer are mixed in a gas phase and heated and melted to form a resin coating layer.
[0188] From the viewpoint of suppressing resistance changes due to temperature and humidity, the average thickness of the resin coating layer is preferably 0.6 μm or more and 1.4 μm or less, more preferably 0.8 μm or more and 1.2 μm or less, and particularly preferably 0.8 μm or more and 1.1 μm or less.
[0189] (Carrier characteristics) From the viewpoint of suppressing embedding of external additives in the toner and ensuring the fluidity of the carrier, the volume average particle size of the carrier is preferably from 25 to 40 μm, more preferably from 26 to 38 μm, and particularly preferably from 28 to 37 μm.
[0190] From the viewpoint of suppressing embedding of external additives in the toner, the average circularity of the carrier is preferably 0.95 to 1.00, more preferably 0.96 to 0.98, and even more preferably 0.96 to 0.97. The average circularity of the carrier is determined by dispersing 0.03 g of the carrier in a 25% by mass aqueous solution of ethylene glycol, measuring in the LPF measurement mode using an FPIA3000 (manufactured by Sysmex Corporation) as a measuring device, and performing shape analysis after cutting out particles with particle sizes of less than 10 μm and more than 50 μm.
[0191] In the first embodiment, the true specific gravity of the carrier is 3.0 g / cm 3 More than 4.0g / cm3 Less than or equal to 3.2 g / cm 3 More than 3.9g / cm 3 It is preferable that the density is 3.4 g / cm or less. 3 More than 3.6g / cm 3 In the second embodiment, the true specific gravity of the carrier is preferably 3.0 g / cm or less. 3 More than 4.0g / cm 3 It is preferable that the density is 3.2 g / cm or less. 3 More than 3.9g / cm 3 More preferably, it is 3.4 g / cm or less. 3 More than 3.6g / cm 3 It is even more preferable that: By having the true specific gravity of the carrier in the above range, the embedding of the external additive in the toner is suppressed compared to when the true specific gravity is greater than the above range, and image fogging caused by the embedding of the external additive is suppressed. Also, by having the true specific gravity of the carrier in the above range, the fluidity of the carrier is ensured compared to when the true specific gravity is less than the above range, and frictional charging with the toner is stabilized, which is advantageous in that image fogging is suppressed.
[0192] The true specific gravity of the carrier is dg / cm 3 In this case, the relationship between D1(90) of the toner and the true specific gravity d of the carrier preferably satisfies any one of the following conditions 1 to 3, from the viewpoint of suppressing image fog. Condition 1: 3.0≦d<3.4 and 1.4≦D1(90)≦2.5 Condition 2: 3.4≦d<3.8 and 1.1≦D1(90)<1.4 Condition 3: 3.8≦d≦4.0 and 0.5≦D1(90)<1.1
[0193] Although it is not clear why fog is suppressed when the relationship between D1(90) and d satisfies any one of Conditions 1 to 3, it is presumed as follows. Specifically, when a carrier with a low specific gravity is used, it is preferable to combine it with a toner with high surface viscosity, i.e., a large D1(90), in order to facilitate charging due to friction when the toner and carrier come into contact. On the other hand, when a carrier with a high specific gravity is used within the above range, not only is triboelectric charging likely to occur even when combined with a toner with a small D1(90), but combining it with a toner with a small D1(90) also suppresses the embedding of external additives. From the above, it is presumed that when the relationship between D1(90) and d satisfies any one of conditions 1 to 3, frictional charging is likely to occur, and the embedding of the external additive is suppressed, thereby suppressing image fog.
[0194] The relationship between D1(90) and d more preferably satisfies any one of the following conditions 4 to 6, and further more preferably satisfies any one of the following conditions 7 to 9. Condition 4: 3.0≦d<3.4 and 1.45≦D1(90)≦2.00 Condition 5: 3.4≦d<3.8 and 1.15≦D1(90)<1.30 Condition 6: 3.8≦d≦4.0 and 0.55≦D1(90)<1.05 Condition 7: 3.0≦d<3.4 and 1.50≦D1(90)≦1.80 Condition 8: 3.4≦d<3.8 and 1.20≦D1(90)<1.28 Condition 9: 3.8≦d≦4.0 and 0.55≦D1(90)<1.00
[0195] In the second embodiment, the content of the magnetic powder in the entire carrier is more than 80% by mass and less than 90% by mass, preferably 82% by mass to 87% by mass, and more preferably 84% by mass to 86% by mass. In the first embodiment, the content of the magnetic powder in the entire carrier is also preferably more than 80% by mass and less than 90% by mass, more preferably 82% by mass to 87% by mass, and even more preferably 84% by mass to 86% by mass. By having the magnetic powder content in the above range, the specific gravity of the entire carrier is smaller than when the content is higher than the above range, the embedding of the external additive in the toner is suppressed, and image fogging caused by the embedding of the external additive is suppressed. Also, by having the magnetic powder content in the above range, the magnetization of the carrier is higher than when the content is lower than the above range, which has the advantage of making the density of the developer on the magnetic roll of the developing device uniform and suppressing image fogging.
[0196] <Mixing ratio of toner and carrier> The mixture ratio (mass ratio) of the toner and the carrier in the developer contained in the developing device is, for example, in the range of 1 part by mass or more and 30 parts by mass or less of the toner per 100 parts by mass of the carrier.
[0197] <Process cartridge, image forming apparatus, and image forming method> A process cartridge, an image forming apparatus, and an image forming method using the above-mentioned developer will be described below.
[0198] The process cartridge according to this embodiment includes a process cartridge that contains the above-mentioned developer as an initial filling developer, is equipped with a developing device that uses the developer to develop an electrostatic charge image formed on the surface of an image carrier into a toner image, and is detachably attached to an image forming apparatus. An example of an image forming apparatus according to this embodiment includes an image forming apparatus including an image carrier, a charging device that charges the surface of the image carrier, an electrostatic image forming device that forms an electrostatic image on the surface of the charged image carrier, a developing device that contains the above-mentioned developer as an initial filling developer and uses the developer to develop the electrostatic image formed on the surface of the image carrier into a toner image, a transfer device that transfers the toner image formed on the surface of the image carrier to the surface of a recording medium, and a fixing device that fixes the toner image transferred to the surface of the recording medium. The image forming method according to this embodiment includes an image forming method having a charging step of charging the surface of an image carrier, an electrostatic image forming step of forming an electrostatic image on the charged surface of the image carrier, a developing step of developing the electrostatic image formed on the surface of the image carrier as a toner image using the initial filling developer, which is the aforementioned developer contained in a developing device, a transfer step of transferring the toner image formed on the surface of the image carrier to the surface of a recording medium, and a fixing step of fixing the toner image transferred to the surface of the recording medium.
[0199] The image forming apparatus according to the present embodiment may be any of known image forming apparatuses, such as a direct transfer type apparatus in which a toner image formed on the surface of an image holder is directly transferred to a recording medium; an intermediate transfer type apparatus in which a toner image formed on the surface of an image holder is primarily transferred to the surface of an intermediate transfer body, and the toner image transferred to the surface of the intermediate transfer body is then secondarily transferred to the surface of a recording medium; an apparatus equipped with a cleaning device that cleans the surface of the image holder before charging after the transfer of the toner image; and an apparatus equipped with a static elimination device that irradiates the surface of the image holder with static elimination light to eliminate static electricity before charging after the transfer of the toner image. In the case of an intermediate transfer type device, the transfer device is configured to have, for example, an intermediate transfer body onto whose surface a toner image is transferred, a primary transfer device which primarily transfers the toner image formed on the surface of the image carrier onto the surface of the intermediate transfer body, and a secondary transfer device which secondarily transfers the toner image transferred onto the surface of the intermediate transfer body onto the surface of a recording medium.
[0200] An example of an image forming apparatus according to the present embodiment will be described below, but the present invention is not limited to this. Note that only the main parts shown in the drawings will be described, and descriptions of the rest will be omitted.
[0201] The image forming apparatus shown in Fig. 1 includes first to fourth electrophotographic image forming units 10Y, 10M, 10C, and 10K that output images of the respective colors of yellow (Y), magenta (M), cyan (C), and black (K) based on color-separated image data. These image forming units (hereinafter sometimes simply referred to as "units") 10Y, 10M, 10C, and 10K are arranged in parallel at predetermined distances from each other in the horizontal direction. These units 10Y, 10M, 10C, and 10K may be process cartridges that are detachable from the image forming apparatus.
[0202] Above each of the units 10Y, 10M, 10C, and 10K in the drawing, an intermediate transfer belt 20 is provided as an intermediate transfer body extending through each unit. The intermediate transfer belt 20 is provided wound around a drive roll 22 and a support roll 24 that are arranged from left to right in the drawing at a distance from each other and contact the inner surface of the intermediate transfer belt 20, and is adapted to run in a direction from the first unit 10Y to the fourth unit 10K. Note that a force is applied to the support roll 24 in a direction away from the drive roll 22 by a spring or the like (not shown), and tension is applied to the intermediate transfer belt 20 wound around them. In addition, an intermediate transfer body cleaning device 30 is provided on the image carrier side of the intermediate transfer belt 20, facing the drive roll 22. Further, the developing devices 4Y, 4M, 4C, and 4K of the units 10Y, 10M, 10C, and 10K are supplied with toner including four colors of toner, yellow, magenta, cyan, and black, contained in toner cartridges 8Y, 8M, 8C, and 8K, respectively.
[0203] Since the first to fourth units 10Y, 10M, 10C, and 10K have the same configuration, the first unit 10Y that forms a yellow image and is disposed upstream in the direction in which the intermediate transfer belt travels will be described here as a representative example. Note that by assigning reference numerals of magenta (M), cyan (C), and black (K) instead of yellow (Y) to parts equivalent to those of the first unit 10Y, descriptions of the second to fourth units 10M, 10C, and 10K will be omitted.
[0204] The first unit 10Y has a photoconductor 1Y that acts as an image carrier. Around the photoconductor 1Y, a charging roll (an example of a charging device) 2Y that charges the surface of the photoconductor 1Y to a predetermined potential, an exposure device (an example of an electrostatic image forming device) 3 that exposes the charged surface to a laser beam 3Y based on a color-separated image signal to form an electrostatic image, a developing device 4Y that supplies charged toner to the electrostatic image to develop it, a primary transfer roll 5Y (an example of a primary transfer device) that transfers the developed toner image onto an intermediate transfer belt 20, and a photoconductor cleaning device (an example of a cleaning device) 6Y that removes toner remaining on the surface of the photoconductor 1Y after the primary transfer are arranged in this order. The primary transfer roll 5Y is disposed inside the intermediate transfer belt 20 and is provided at a position facing the photoconductor 1Y. Furthermore, a bias power supply (not shown) that applies a primary transfer bias is connected to each of the primary transfer rolls 5Y, 5M, 5C, and 5K. Each bias power supply varies the transfer bias applied to each primary transfer roll under the control of a control unit (not shown).
[0205] Hereinafter, an operation of forming a yellow image in first unit 10Y will be described. First, prior to operation, the surface of the photoconductor 1Y is charged to a potential of −600V to −800V by the charging roll 2Y. The photoconductor 1Y has a conductivity (for example, a volume resistivity at 20° C. of 1×10 -6 The photosensitive layer is formed by laminating a photosensitive layer on a substrate having a resistivity of Ωcm or less. This photosensitive layer is usually highly resistive (the resistance of ordinary resins), but when irradiated with a laser beam 3Y, the resistivity of the portion irradiated with the laser beam changes. A laser beam 3Y is output to the charged surface of the photoreceptor 1Y via an exposure device 3 in accordance with image data for yellow sent from a control unit (not shown). The laser beam 3Y is irradiated onto the photosensitive layer on the surface of the photoreceptor 1Y, and an electrostatic charge image of a yellow image pattern is formed on the surface of the photoreceptor 1Y.
[0206] An electrostatic image is an image formed on the surface of the photoconductor 1Y by electrostatic charging. The laser beam 3Y reduces the resistivity of the irradiated parts of the photosensitive layer, causing the charged charges on the surface of the photoconductor 1Y to flow, while the charges remain in the parts not irradiated by the laser beam 3Y. This is a so-called negative latent image. The electrostatic image formed on the photoconductor 1Y is rotated to a predetermined developing position as the photoconductor 1Y travels. Then, at this developing position, the electrostatic image on the photoconductor 1Y is made visible as a toner image (developed image) by the developing device 4Y.
[0207] The developing device 4Y contains an electrostatic image developer including at least yellow toner and a carrier, for example. The yellow toner is triboelectrically charged by being stirred inside the developing device 4Y, and is held on a developer roll (an example of a developer holder) with a charge of the same polarity (negative polarity) as the charge on the photoconductor 1Y. As the surface of the photoconductor 1Y passes through the developing device 4Y, the yellow toner electrostatically adheres to the discharged latent image portion on the surface of the photoconductor 1Y, and the latent image is developed with the yellow toner. The photoconductor 1Y on which the yellow toner image has been formed continues to travel at a predetermined speed, and the toner image developed on the photoconductor 1Y is transported to a predetermined primary transfer position.
[0208] When the yellow toner image on the photoconductor 1Y is transported to the primary transfer position, a primary transfer bias is applied to the primary transfer roll 5Y, and an electrostatic force from the photoconductor 1Y toward the primary transfer roll 5Y acts on the toner image, and the toner image on the photoconductor 1Y is transferred onto the intermediate transfer belt 20. The transfer bias applied at this time has a polarity (+) opposite to the polarity (-) of the toner, and in the first unit 10Y, for example, it is controlled to +10 μA by a control unit (not shown). On the other hand, the toner remaining on the photoconductor 1Y is removed and collected by the photoconductor cleaning device 6Y.
[0209] Further, the primary transfer bias applied to the primary transfer rolls 5M, 5C, and 5K subsequent to the second unit 10M is also controlled in accordance with the first unit. In this manner, the intermediate transfer belt 20 onto which the yellow toner image has been transferred by the first unit 10Y is conveyed successively through the second to fourth units 10M, 10C, and 10K, where the toner images of the respective colors are transferred in a superimposed manner.
[0210] The intermediate transfer belt 20 onto which the four color toner images have been transferred in multiple layers through the first to fourth units reaches a secondary transfer section that is composed of the intermediate transfer belt 20, a support roll 24 that contacts the inner surface of the intermediate transfer belt, and a secondary transfer roll (an example of a secondary transfer device) 26 arranged on the image carrying surface side of the intermediate transfer belt 20. Meanwhile, a recording paper (an example of a recording medium) P is fed at a predetermined timing into the gap between the secondary transfer roll 26 and the intermediate transfer belt 20 via a supply mechanism, and a secondary transfer bias is applied to the support roll 24. The transfer bias applied at this time has a (-) polarity that is the same as the (-) polarity of the toner, and an electrostatic force from the intermediate transfer belt 20 toward the recording paper P acts on the toner image, so that the toner image on the intermediate transfer belt 20 is transferred onto the recording paper P. The secondary transfer bias at this time is determined according to the resistance detected by a resistance detection means (not shown) that detects the resistance of the secondary transfer section, and is voltage controlled.
[0211] Thereafter, the recording paper P is sent to a pressure contact portion (nip portion) of a pair of fixing rolls in the fixing device 28, where the toner image is fixed onto the recording paper P, forming a fixed image.
[0212] The recording paper P onto which the toner image is transferred can be, for example, plain paper used in electrophotographic copying machines, printers, etc. In addition to the recording paper P, other examples of the recording medium include overhead projector sheets, etc. To further improve the smoothness of the image surface after fixing, it is preferable that the surface of the recording paper P is also smooth. For example, coated paper in which the surface of ordinary paper is coated with resin or the like, art paper for printing, etc. are preferably used.
[0213] After the color image has been fixed, the recording paper P is conveyed toward the discharge section, and the series of color image forming operations is completed.
[0214] FIG. 2 is a schematic diagram showing the process cartridge according to the present embodiment. The process cartridge 200 shown in FIG. 2 is configured by, for example, a housing 117 having a mounting rail 116 and an opening 118 for exposure, which integrally holds a photoconductor 107 (an example of an image carrier), a charging roll 108 (an example of a charging device) provided around the photoconductor 107, a developing device 111 (an example of a developing device), and a photoconductor cleaning device 113 (an example of a cleaning device), which are combined and held together into a cartridge. In FIG. 2, 109 denotes an exposure device (an example of an electrostatic image forming device), 112 denotes a transfer device (an example of a transfer device), 115 denotes a fixing device (an example of a fixing device), and 300 denotes recording paper (an example of a recording medium).
[0215] In addition, the process cartridge according to this embodiment is not limited to the above configuration, and may be configured to include a developing device and, as necessary, at least one other means selected from an image carrier, a charging device, an electrostatic image forming device, and a transfer device. EXAMPLES
[0216] Examples will be described below, but the present invention is not limited to these examples. In the following description, unless otherwise specified, all "parts" and "%" are based on mass.
[0217] [Preparation of specific resin particle dispersion] <Preparation of specific resin particle dispersion 1> Styrene: 47.9 parts n-Butyl acrylate: 51.8 parts 2-Carboxyethyl acrylate: 0.3 parts Anionic surfactant (Dow Chemical Company, Dowfax2A1): 0.8 parts 1,10-Decanediol diacrylate: 1.65 parts The above raw materials were mixed and dissolved, and 60 parts of ion-exchanged water was added thereto, followed by dispersion and emulsification in a flask to prepare an emulsion. Next, 1.3 parts of an anionic surfactant (Dowfax2A1, manufactured by The Dow Chemical Company) The resulting material was dissolved in 90 parts of ion-exchanged water, 1 part of the emulsion was added thereto, and then 10 parts of ion-exchanged water in which 5.4 parts of ammonium persulfate had been dissolved was added. The remainder of the emulsion was then added over a period of 180 minutes, and the atmosphere in the flask was replaced with nitrogen.The solution in the flask was then heated to 65°C in an oil bath while stirring, and emulsion polymerization was continued for 500 minutes, after which a specific resin particle dispersion 1 was obtained with a solids content adjusted to 24.5% by mass. The results obtained by the above-mentioned methods for the resin particles contained in the obtained specific resin particle dispersion 1 are as follows. Glass transition temperature Tg determined from dynamic viscoelasticity measurement: 32.1℃ Minimum storage modulus G'(p90-150): 2.6×10 5 Pa Maximum value of storage modulus G'(p90-150): 5.1×10 5 Pa Minimum loss tangent tanδ in the range of 30°C to 150°C: 0.028 Maximum loss tangent tanδ in the range of 30°C to 150°C: 2.35 Minimum loss tangent tanδ in the range of 65°C to 150°C: 0.028 Maximum loss tangent tanδ in the range of 65°C to 150°C: 0.203 Number average particle size: 153 nm SP value (S): 9.07
[0218] [Toner Preparation] <Preparation of amorphous resin particle dispersion 1> Terephthalic acid: 28 parts Fumaric acid: 164 parts Adipic acid: 10 parts Bisphenol A ethylene oxide 2 mole adduct: 26 parts Bisphenol A propylene oxide 2 mole adduct: 542 parts The above materials were charged into a reaction vessel equipped with a stirrer, a nitrogen inlet tube, a temperature sensor, and a distillation column, the temperature was raised to 190°C over 1 hour, and 1.2 parts of dibutyltin oxide was added per 100 parts of the above materials. The temperature was raised to 240°C over 6 hours while distilling off the generated water, and the dehydration condensation reaction was continued for 3 hours while maintaining the temperature at 240°C, after which the reaction product was cooled.
[0219] The reactant was transferred to a Cavitron CD1010 (Eurotech) at a rate of 100 g per minute while remaining in a molten state. At the same time, ammonia water with a concentration of 0.37% by mass was transferred to the Cavitron CD1010 at a rate of 0.1 liters per minute while being heated to 120°C in a heat exchanger. The rotor rotation speed was 60 Hz, and the pressure was 5 kg / cm. 2 The Cavitron CD1010 was operated under the conditions above to obtain a resin particle dispersion in which resin particles of an amorphous polyester resin having a volume average particle size of 169 nm were dispersed. Ion-exchanged water was added to the resin particle dispersion to adjust the solid content to 20 mass %, thereby obtaining amorphous resin particle dispersion 1. The SP value (R) of the obtained amorphous polyester resin was 9.41.
[0220] <Preparation of Crystalline Resin Particle Dispersion> 1,10-dodecanedioic acid: 225 parts 1,6-Hexanediol: 143 parts The above materials were charged into a reaction vessel equipped with a stirrer, a nitrogen inlet tube, a temperature sensor, and a distillation column, the temperature was raised to 160°C over 1 hour, and 0.8 parts by mass of dibutyltin oxide was added. The temperature was raised to 180°C over 6 hours while distilling off the generated water, and the dehydration condensation reaction was continued for 5 hours while maintaining the temperature at 180°C. Thereafter, the temperature was gradually raised to 230°C under reduced pressure, and stirring was performed for 2 hours while maintaining the temperature at 230°C. The reactant was then cooled. After cooling, solid-liquid separation was performed, and the solid was dried to obtain a crystalline polyester resin.
[0221] Crystalline polyester resin: 100 parts Methyl ethyl ketone: 40 parts Isopropyl alcohol: 30 parts 10% ammonia solution: 6 parts The above materials were added to a 3-liter jacketed reaction tank (manufactured by Tokyo Rikakikai Co., Ltd.: BJ-30N) equipped with a condenser, a thermometer, a water dropping device, and an anchor blade, and the resin was dissolved while stirring and mixing at 100 rpm while maintaining the temperature at 80°C in a water circulation type thermostatic bath. Thereafter, the water circulation type thermostatic bath was set to 50°C, and a total of 400 parts of ion-exchanged water kept at 50°C was dropped at a rate of 7 parts by mass / min to cause phase inversion, thereby obtaining an emulsion. 576 parts by mass of the obtained emulsion and 500 parts by mass of ion-exchanged water were placed in a 2-liter eggplant flask, and set in an evaporator (manufactured by Tokyo Rikakikai Co., Ltd.) equipped with a vacuum control unit via a trap ball. The eggplant flask was rotated and heated in a hot water bath at 60°C, and the pressure was reduced to 7 kPa while paying attention to bumping, and the solvent was removed. The volume average particle size D50v of the resin particles in this dispersion was 185 nm. Thereafter, ion-exchanged water was added to obtain a crystalline resin particle dispersion liquid with a solid content concentration of 22.1% by mass.
[0222] <Preparation of Colorant Dispersion> Cyan pigment (Dainichi Seikagaku Co., Ltd., Pigment Blue 15:3 (copper phthalocyanine)): 98 parts Anionic surfactant (Tayca Power, manufactured by Tayca Corporation): 2 parts Ion-exchanged water: 420 parts The above ingredients were mixed and dissolved, and dispersed for 10 minutes using a homogenizer (IKA Ultra Turrax), to obtain a colorant dispersion having a median particle size of 164 nm and a solid content of 21.1% by mass.
[0223] <Preparation of release agent dispersion> Synthetic wax (Nippon Seiro Co., Ltd., FNP92, melting temperature Tw: 92℃): 50 parts Anionic surfactant (Tayca Power, manufactured by Tayca Corporation): 1 part Ion-exchanged water: 200 parts The above materials were mixed and heated to 130°C, dispersed using a homogenizer (IKA Ultra Turrax T50), and then dispersed using a Manton-Gaulin high pressure homogenizer (Gaulin) to obtain a release agent dispersion (solid content 20% by mass) in which release agent particles were dispersed. The volume average particle size of the release agent particles was 214 nm.
[0224] <Preparation of Toner 1> ·Amorphous resin particle dispersion 1: 169 parts ·Specified resin particle dispersion liquid 1: 33 parts ·Crystalline resin particle dispersion: 53 parts Release agent dispersion: 25 parts Colorant dispersion: 33 parts Anionic surfactant (Dow Chemical Company, Dowfax2A1): 4.8 parts The above raw materials, the liquid temperature of which had been adjusted to 10° C., were placed in a 3 L cylindrical stainless steel container, and dispersed and mixed for 2 minutes while applying shear force at 4000 rpm using a homogenizer (IKA Ultra Turrax T50). Next, 1.75 parts of a 10% aqueous solution of aluminum sulfate in nitric acid was gradually added dropwise as a flocculant, and the homogenizer was rotated at 10,000 rpm for 10 minutes to disperse and mix, thereby obtaining a raw dispersion liquid.
[0225] The raw material dispersion was then transferred to a polymerization kettle equipped with a stirrer using two paddle stirrers and a thermometer, and the stirring speed was set to 550 rpm and heating was started with a mantle heater to promote the growth of aggregated particles at 40°C. At this time, the pH of the raw material dispersion was controlled in the range of 2.2 to 3.5 with 0.3 M nitric acid and 1 M sodium hydroxide aqueous solution. The pH was maintained in the above range for about 2 hours to form aggregated particles. Next, a dispersion liquid obtained by mixing 1:21 parts of amorphous resin particle dispersion liquid and 1:8 parts of specific resin particle dispersion liquid was added, and the mixture was held for 60 minutes to allow the binder resin and specific resin particles to adhere to the surfaces of the aggregated particles.The temperature was further increased to 53°C, and then 1:21 parts of amorphous resin particle dispersion liquid was added, and the mixture was held for 60 minutes to allow the binder resin particles to adhere to the surfaces of the aggregated particles.
[0226] The aggregated particles were adjusted while checking the particle size and morphology with an optical microscope and a Multisizer 3. Thereafter, the pH was adjusted to 7.8 using a 5% aqueous sodium hydroxide solution, and maintained for 15 minutes. Thereafter, in order to fuse the aggregated particles, the pH was increased to 8.0, and the temperature was increased to 85° C. After confirming with an optical microscope that the aggregated particles had fused, heating was stopped after 2 hours, and the mixture was cooled at a temperature decreasing rate of 1.0° C. / min. Thereafter, the mixture was sieved through a 20 μm mesh, repeatedly washed with water, and then dried in a vacuum dryer to obtain toner particles 1 having a volume average particle size of 5.3 μm.
[0227] 100 parts of the obtained toner particles and 0.7 parts of dimethyl silicone oil-treated silica particles (RY200 manufactured by Nippon Aerosil Co., Ltd.) were mixed in a Henschel mixer to obtain toner 1.
[0228] <Preparation of Toner 2> Toner 2 was obtained in the same manner as Toner 1, except that specific resin particle dispersion 1 was used in an amount such that the content of specific resin particles relative to the total toner particles was the value shown in Table 1, and the pH during fusion of the aggregated particles was changed from 8.0 to 6.0.
[0229] <Preparation of Toner 3> Toner 3 was obtained in the same manner as Toner 1, except that the specific resin particle dispersion 1 was used in an amount such that the content of the specific resin particles relative to the total amount of the toner particles was the value shown in Table 1.
[0230] <Preparation of Toner 4> Toner 4 was obtained in the same manner as Toner 1, except that the pH during fusion of the aggregated particles was changed from 8.0 to 6.5, the temperature after heating was changed from 85°C to 75°C, and 5.2 parts of anionic surfactant (Dowfax2A1, manufactured by The Dow Chemical Company) was added when the temperature reached 75°C.
[0231] <Preparation of Toner C1> ·Amorphous resin particle dispersion 1: 169 parts ·Specified resin particle dispersion 1: 41 parts ·Crystalline resin particle dispersion: 53 parts Release agent dispersion: 25 parts Colorant dispersion: 33 parts Anionic surfactant (Dow Chemical Company, Dowfax2A1): 4.8 parts The above raw materials, the liquid temperature of which had been adjusted to 30° C., were placed in a 3 L cylindrical stainless steel container, and dispersed and mixed for 2 minutes while applying shear force at 4000 rpm using a homogenizer (IKA Ultra Turrax T50). Next, 1.75 parts of a 10% aqueous solution of aluminum sulfate in nitric acid was gradually added dropwise as a flocculant, and the mixture was dispersed and mixed for 3 minutes at a homogenizer speed of 4000 rpm to obtain a raw dispersion liquid.
[0232] The raw material dispersion was then transferred to a polymerization kettle equipped with a stirrer using two paddle stirrers and a thermometer, and the stirring speed was set to 550 rpm and heating was started with a mantle heater to promote the growth of aggregated particles at 40°C. At this time, the pH of the raw material dispersion was controlled in the range of 2.2 to 3.5 with 0.3 M nitric acid and 1 M sodium hydroxide aqueous solution. The pH was maintained in the above range for about 2 hours to form aggregated particles. Next, 1:42 parts of the amorphous resin particle dispersion liquid was further added and held for 60 minutes to allow the resin particles of the binder resin to adhere to the surfaces of the aggregated particles.
[0233] The aggregated particles were adjusted while checking the particle size and morphology with an optical microscope and a Multisizer 3. Thereafter, the pH was adjusted to 7.8 using a 5% aqueous sodium hydroxide solution, and maintained for 15 minutes. Thereafter, in order to fuse the aggregated particles, the pH was increased to 8.0, and the temperature was increased to 85° C. After confirming that the aggregated particles had fused using an optical microscope, heating was stopped after 2 hours, and the mixture was cooled at a temperature drop rate of 1.0° C. / min. Thereafter, the mixture was sieved through a 20 μm mesh, repeatedly washed with water, and then dried in a vacuum dryer to obtain toner particles C1.
[0234] 100 parts of the obtained toner particles and 0.7 parts of dimethyl silicone oil-treated silica particles (RY200 manufactured by Nippon Aerosil Co., Ltd.) were mixed in a Henschel mixer to obtain toner C1.
[0235] Table 1 shows the content of the specific resin particles in the entire toner particles in the obtained toner ("Particle content (%)" in the table). Table 1 also shows the ratio of the crystalline resin content to the specific resin particle content in the obtained toner ("Crystalline content ratio vs. particles" in the table) and the ratio of the amorphous resin content to the specific resin particle content ("Amorphous content ratio vs. particles" in the table). Table 1 also shows the volume average particle size of the toner particles in the obtained toner.
[0236] Table 1 also shows the results of the storage modulus G' of the excluded components in the range of 30°C or higher and 50°C or lower ("30-50°C G' (Pa)" in the table), the temperature at which the specific elastic modulus is reached ("Attained temperature (°C)" in the table), and the loss tangent tanδ at the specific elastic modulus reaching temperature ("Attained temperature tanδ" in the table), all determined using the methods described above. Table 2 also shows the results of determining, by the above-mentioned method, for the obtained toner, D1(90), D50(90), D1(150), D50(150), D50(150)-D1(150) values ("Difference (150)" in the table), D50(90)-D1(90) value ("Difference (90)" in the table), number average molecular weight of the THF-soluble matter in the toner particles ("Mn" in the table), storage modulus G' in the range of 30°C or higher and 50°C or lower ("30-50 G'(Pa)" in the table), specific elastic modulus attainment temperature ("Attainment temperature (°C)" in the table), logG'(t90-150)-logG'(r90-150) value ("Viscoelastic difference" in the table), and difference (SP value(S)-SP value(R)) ("SP value difference" in the table).
[0237] [Table 1]
[0238] [Table 2]
[0239] [Creating the carrier] <Preparation of core particles> Magnetite powder (volume average particle size: 0.2 μm), phenol, 36 mass% formalin, ion-exchanged water, and 26 mass% aqueous ammonia solution were mixed in the amounts shown in Table 3, heated to 85°C with stirring, and reacted and cured for 4 hours. Thereafter, the mixture was cooled, filtered, and washed with ion-exchanged water to obtain core particles.
[0240] [Table 3]
[0241] <Formation of thin film layer> (Preparation of core materials 1 to 6 and C1) Melamine and 36% by mass formalin were mixed in the amounts shown in Table 4, and the mixture was heated to 60° C. at a rate of 1° C. / minute with stirring, and then heated at 60° C. for 1 hour to obtain a melamine solution. Separately, a core particle dispersion liquid prepared by mixing 60 parts of ion-exchanged water and 400 parts of the core particles shown in Table 4 was heated to 85° C., the melamine solution was added, and stirring was continued at 85° C. for 2 hours. Next, the mixture was cooled, filtered, and washed with ion-exchanged water to obtain a core material having a thin film layer formed on the surface of the core particle. Table 4 also shows the volume average particle size ("Particle size" in the table), true specific gravity, average thickness of the thin film layer ("Film thickness" in the table), and magnetic powder content in the entire core material ("Magnetic powder ratio" in the table). In the table, "-" means that no additive was added.
[0242] [Table 4]
[0243] <Preparation of Coating Agent> Cyclohexyl methacrylate (weight average molecular weight: 50,000): 36 parts Carbon black (Cabot VXC72): 4 parts Toluene: 300 parts The above components and glass beads (particle size: 1 mm, same amount as toluene) were placed in a sand mill manufactured by Kansai Paint Co., Ltd. and stirred at a rotation speed of 1200 rpm for 30 minutes to prepare a coating agent with a solid content of 11 mass %.
[0244] <Preparation of carrier> 2000 g of the core material shown in Table 5 was placed in a vacuum degassing type 5 L kneader, and the coating agent was further added in the amount shown in Table 5. While stirring, the mixture was reduced in pressure to -200 mmHg at 60°C and mixed for 15 minutes, then the temperature was raised and the pressure was reduced, and the mixture was stirred and dried for 30 minutes at a temperature of 94°C and a gauge pressure of -720 mmHg. The mixture was then sieved through a 75 μm mesh sieve to obtain a carrier in which a resin coating layer was formed on the core material. Table 5 also shows the volume average particle size ("Particle size" in the table), true specific gravity, average thickness of the resin coating layer ("Film thickness" in the table), average circularity, and magnetic powder content relative to the entire carrier ("Magnetic powder ratio" in the table).
[0245] [Table 5]
[0246] [Preparation of developer] A developer was obtained by mixing 8 parts of the toner shown in Table 6 with 100 parts of the carrier shown in Table 6. For the obtained developer, the applicable conditions among the above conditions 1 to 3 ("Conditions 1 to 3" in the table), the applicable conditions among the above conditions 4 to 6 ("Conditions 4 to 6" in the table), and the applicable conditions among the above conditions 7 to 9 ("Conditions 7 to 9" in the table) are also shown in Table 6. Note that "none" in the table indicates that none of the conditions apply.
[0247] [Developer evaluation] <Gloss Difference> The developer obtained was filled into the developing unit of a color copier ApeosPortIV C3370 (manufactured by Fujifilm Business Innovation Co., Ltd.) from which the fixing unit had been removed, and the toner loading amount was adjusted to 0.45 mg / cm 2The unfixed image was output by adjusting the image density so that the image density was adjusted to the following value. The recording medium used was A4 size OS coated W paper (127 gsm basis weight) manufactured by Fujifilm Business Innovation Co., Ltd. The output image was a 50 mm x 50 mm image with a 100% image density.
[0248] The fixing evaluation device used was an ApeosPortIV C3370 manufactured by FUJIFILM Business Innovation Co., Ltd., whose fixing unit had been removed and modified so that the nip pressure and fixing temperature could be changed. The process speed was 175 mm / sec. Under these conditions, the unfixed image was fixed under low temperature and low pressure conditions (specifically, the temperature of the fixing unit was 120 degrees and the nip pressure was 1.6 kgf / cm 2 ) and high temperature and pressure conditions (specifically, the fixing unit temperature was 180 degrees and the nip pressure was 6.0 kgf / cm 2 The image was fixed under two conditions, and a fixed image was obtained. The gloss of the fixed image was measured at 60° gloss using a BYK Micro Trigloss glossmeter, and the gloss difference between the fixed image under low temperature and low pressure conditions and the fixed image under high temperature and high pressure conditions (i.e., gloss condition difference) was calculated. The results are shown in Table 6. In addition, when the gloss difference is less than 5, it is difficult to visually recognize the gloss difference, when the gloss difference is 5 or more but less than 10, the gloss difference is visually noticeable but is slight, when the gloss difference is 10 or more but less than 15, the gloss difference is visible but within the acceptable range, and when the gloss difference is 15 or more, the gloss difference is large and outside the acceptable range.
[0249] <Focus> Fog evaluation was carried out using an image forming apparatus (DC VII C7773). Specifically, 100,000 sheets of an image consisting of 24 characters (4 characters per line, 6 lines) of A to Z, with font: MS Gothic, size: 14 points, were printed on A4 size recording medium paper under conditions of 23°C and 15% RH. After that, the image forming apparatus was moved to an environment of 28°C and 85% RH, and 20 sheets of A4 full solid (image density 100%) were printed. Next, 10 images of 1 point size single-color black lines were printed on A4 size recording medium paper, 15 cm long and 5 cm apart, and the obtained images were evaluated according to the following criteria. The results are shown in Table 6. G1: Lines are printed without any problems G2: Variation in line thickness is evident under a 25x magnifying glass. G3: Faint toner fogging is observed around the lines under a 25x magnifying glass. G4: Faint toner fogging is visually confirmed around the lines. G5: Toner is scattered around the lines, causing the lines to bleed.
[0250] [Table 6]
[0251] From the above results, it is understood that the developer of this embodiment has a small difference in gloss between an image fixed under low temperature and low pressure conditions and an image fixed under high temperature and high pressure conditions, and also suppresses image fog.
[0252] The present embodiment includes the following aspects. (((1))) a toner comprising toner particles containing a binder resin and an external additive, wherein, in a dynamic viscoelasticity measurement of the toner, when a loss tangent tanδ at a temperature of 90°C and a distortion of 1% is D1(90), a loss tangent tanδ at a temperature of 90°C and a distortion of 50% is D50(90), a loss tangent tanδ at a temperature of 150°C and a distortion of 1% is D1(150), and a loss tangent tanδ at a temperature of 150°C and a distortion of 50% is D50(150), D1(90), D50(90), D1(150), and D50(150) are each 0.5 or more and 2.5 or less, the value of D50(150)-D1(150) is less than 1.5, and the value of D50(90)-D1(90) is less than 1.0; True specific gravity is 3.0g / cm 3 More than 4.0g / cm 3 A career that is: An electrostatic image developer comprising:
[0253] (((2))) The true specific gravity of the carrier is dg / cm 3 The electrostatic image developer according to (((1))), wherein the relationship between D1(90) and d satisfies any one of the following conditions 1 to 3: Condition 1: 3.0≦d<3.4 and 1.4≦D1(90)≦2.5 Condition 2: 3.4≦d<3.8 and 1.1≦D1(90)<1.4 Condition 3: 3.8≦d≦4.0 and 0.5≦D1(90)<1.1 (((3))) The electrostatic image developer according to (((1))) or (((2))), wherein the carrier includes core particles in which a magnetic powder is dispersed in a resin, a first resin layer that coats the surfaces of the core particles, and a second resin layer that coats the outer peripheral surface of the first resin layer. (((4))) The electrostatic image developer according to (((3))), wherein the first resin layer contains a melamine resin.
[0254] (((5))) The electrostatic image developer according to any one of (((1))) to (((4))), wherein the toner particles further contain resin particles. (((6))) The electrostatic image developer according to (((5))), wherein the resin particles are crosslinked resin particles. (((7))) The electrostatic image developer according to (((6))), wherein the crosslinked resin particles are styrene (meth)acrylic resin particles. (((8))) The electrostatic image developer according to any one of (((1))) to (((7))), wherein the number average molecular weight of a tetrahydrofuran-soluble portion in the toner particles is 5,000 or more and 15,000 or less.
[0255] (((9))) a toner comprising toner particles containing a binder resin and an external additive, wherein, in a dynamic viscoelasticity measurement of the toner, when a loss tangent tanδ at a temperature of 90°C and a distortion of 1% is D1(90), a loss tangent tanδ at a temperature of 90°C and a distortion of 50% is D50(90), a loss tangent tanδ at a temperature of 150°C and a distortion of 1% is D1(150), and a loss tangent tanδ at a temperature of 150°C and a distortion of 50% is D50(150), D1(90), D50(90), D1(150), and D50(150) are each 0.5 or more and 2.5 or less, the value of D50(150)-D1(150) is less than 1.5, and the value of D50(90)-D1(90) is less than 1.0; A carrier including core particles in which a magnetic powder is dispersed in a resin, the content of the magnetic powder being more than 80% by mass and less than 90% by mass relative to the entire carrier; An electrostatic image developer comprising:
[0256] (((10))) a developing device that contains the electrostatic image developer according to any one of (((1))) to (((9))) and develops an electrostatic image formed on a surface of an image carrier into a toner image by using the electrostatic image developer, A process cartridge that is detachably attached to an image forming apparatus. (((11))) An image carrier; a charging device for charging the surface of the image carrier; an electrostatic image forming device for forming an electrostatic image on the charged surface of the image carrier; a developing device that contains the electrostatic image developer according to any one of (((1))) to (((9))) and develops the electrostatic image formed on the surface of the image carrier into a toner image by the electrostatic image developer; a transfer device for transferring the toner image formed on the surface of the image carrier to a surface of a recording medium; a fixing device for fixing the toner image transferred onto the surface of the recording medium; An image forming apparatus comprising: (((12))) a charging step of charging the surface of the image carrier; an electrostatic image forming step of forming an electrostatic image on the charged surface of the image carrier; a developing step of developing the electrostatic image formed on the surface of the image carrier into a toner image by using the electrostatic image developer according to any one of (((1))) to (((9))); a transfer step of transferring the toner image formed on the surface of the image carrier onto a surface of a recording medium; a fixing step of fixing the toner image transferred onto the surface of the recording medium; The image forming method according to claim 1,
[0257] According to the invention related to (((1))) or (((5))), any one of D1(90), D50(90), D1(150), and D50(150) is less than 0.5 or exceeds 2.5, the value of D50(150)-D1(150) is 1.5 or more, the value of 50(90)-D1(90) is 1.0 or more, or the true specific gravity of the carrier is 3.0 g / cm 3 Less than or equal to 4.0g / cm 3 The present invention provides an electrostatic image developer which has a smaller difference in gloss between an image fixed under low temperature and low pressure conditions and an image fixed under high temperature and high pressure conditions, and which suppresses image fogging, as compared with the case where the above-mentioned range is exceeded.
[0258] According to the invention related to (((2))), an electrostatic image developer is provided in which image fog is suppressed compared to the case in which the relationship between D1(90) and d does not satisfy any of conditions 1 to 3. According to the invention related to (((3))) or (((4))), there is provided an electrostatic image developer in which image fogging is suppressed compared to when the carrier is composed of core particles and a second resin layer.
[0259] According to the invention related to (((6))), there is provided a toner for developing electrostatic images in which the difference in gloss between an image fixed under low temperature and low pressure conditions and an image fixed under high temperature and high pressure conditions is smaller than when the resin particles are non-crosslinked resin particles. According to the invention related to (((7))), there is provided a toner for developing electrostatic images in which the difference in gloss between an image fixed under low temperature and low pressure conditions and an image fixed under high temperature and high pressure conditions is smaller than when the crosslinked resin particles are polyester resin particles. According to the invention related to (((8))), there is provided an electrostatic image developer in which the difference in gloss between an image fixed under low temperature and low pressure conditions and an image fixed under high temperature and high pressure conditions is smaller than when the number average molecular weight of the tetrahydrofuran soluble matter is less than 5,000 or exceeds 15,000.
[0260] The invention related to (((9))) provides an electrostatic image developer in which the difference in gloss between an image fixed under low temperature and low pressure conditions and an image fixed under high temperature and high pressure conditions is smaller and image fog is suppressed, as compared with a case in which any of D1(90), D50(90), D1(150), and D50(150) is less than 0.5 or exceeds 2.5, the value of D50(150)-D1(150) is 1.5 or more, the value of 50(90)-D1(90) is 1.0 or more, or the content of magnetic powder in the carrier is less than 80% by mass or 90% by mass or more.
[0261] According to the invention related to (((10))), (((11))), or (((12))), any one of D1(90), D50(90), D1(150), and D50(150) is less than 0.5 or exceeds 2.5, the value of D50(150)-D1(150) is 1.5 or more, the value of D50(90)-D1(90) is 1.0 or more, and the true specific gravity of the carrier is 3.0 g / cm 3 Less than or equal to 4.0g / cm 3The present invention provides a process cartridge, an image forming apparatus, or an image forming method in which the difference in gloss between an image fixed under low temperature and low pressure conditions and an image fixed under high temperature and high pressure conditions is smaller and image fogging is suppressed, as compared to when the magnetic powder content in the carrier is less than 80% by mass or less or 90% by mass or more. [Explanation of symbols]
[0262] 1Y, 1M, 1C, 1K Photoconductor (an example of an image carrier) 2Y, 2M, 2C, 2K Charging roll (example of charging device) 3 Exposure device (an example of an electrostatic image forming device) 3Y, 3M, 3C, 3K laser beam 4Y, 4M, 4C, 4K developing device 5Y, 5M, 5C, 5K Primary transfer roll (part of transfer device) 6Y, 6M, 6C, 6K Photoconductor cleaning device (example of cleaning device) 8Y, 8M, 8C, 8K toner cartridges 10Y, 10M, 10C, 10K Image forming units 20 Intermediate transfer belt (part of the transfer device) 22 Driving Roll 24 Support roll 26 Secondary transfer roll (part of the transfer device) 28 Fixing device 30 Intermediate transfer body cleaning device 107 Photoconductor (an example of an image carrier) 108 Charging roll (an example of a charging device) 109 Exposure device (an example of an electrostatic image forming device) 111 Developing device (an example of a developing device) 112 Transcription device (an example of a transcription device) 113 Photoconductor cleaning device (an example of a cleaning device) 115 Fixing device (an example of a fixing device) 116 Mounting Rail 117 Cabinet 118 Exposure Aperture 200 Process Cartridge 300 Recording paper (an example of a recording medium) P Recording paper (an example of a recording medium)
Claims
1. a toner comprising toner particles containing a binder resin and an external additive, wherein, in a dynamic viscoelasticity measurement of the toner, when a loss tangent tan δ at a temperature of 90° C. and a distortion of 1% is D1(90), a loss tangent tan δ at a temperature of 90° C. and a distortion of 50% is D50(90), a loss tangent tan δ at a temperature of 150° C. and a distortion of 1% is D1(150), and a loss tangent tan δ at a temperature of 150° C. and a distortion of 50% is D50(150), D1(90), D50(90), D1(150), and D50(150) are each 0.5 to 2.5, the value of D50(150)-D1(150) is less than 1.5, and the value of D50(90)-D1(90) is less than 1.0; True specific gravity is 3.0 g / cm 3 4.0g / cm or more 3 A career that is: An electrostatic image developer comprising:
2. The true specific gravity of the carrier is dg / cm 3 2. The electrostatic image developer according to claim 1, wherein the relationship between D1(90) and d satisfies any one of the following conditions 1 to 3: Condition 1: 3.0≦d<3.4 and 1.4≦D1(90)≦2.5 Condition 2: 3.4≦d<3.8 and 1.1≦D1(90)<1.4 Condition 3: 3.8≦d≦4.0 and 0.5≦D1(90)<1.1
3. 2. The electrostatic image developer according to claim 1, wherein the carrier includes a core particle having a magnetic powder dispersed in a resin, a first resin layer that covers a surface of the core particle, and a second resin layer that covers an outer peripheral surface of the first resin layer.
4. 4. The electrostatic image developer according to claim 3, wherein the first resin layer contains a melamine resin.
5. 2. The electrostatic image developer according to claim 1, wherein said toner particles further contain resin particles.
6. 6. The electrostatic image developer according to claim 5, wherein said resin particles are crosslinked resin particles.
7. 7. The electrostatic image developer according to claim 6, wherein said crosslinked resin particles are styrene (meth)acrylic resin particles.
8. 2. The electrostatic image developer according to claim 1, wherein the number average molecular weight of the tetrahydrofuran soluble portion in the toner particles is 5,000 or more and 15,000 or less.
9. a toner comprising toner particles containing a binder resin and an external additive, wherein, in a dynamic viscoelasticity measurement of the toner, when a loss tangent tan δ at a temperature of 90° C. and a distortion of 1% is D1(90), a loss tangent tan δ at a temperature of 90° C. and a distortion of 50% is D50(90), a loss tangent tan δ at a temperature of 150° C. and a distortion of 1% is D1(150), and a loss tangent tan δ at a temperature of 150° C. and a distortion of 50% is D50(150), D1(90), D50(90), D1(150), and D50(150) are each 0.5 to 2.5, the value of D50(150)-D1(150) is less than 1.5, and the value of D50(90)-D1(90) is less than 1.0; a carrier including core particles in which a magnetic powder is dispersed in a resin, the content of the magnetic powder being more than 80% by mass and less than 90% by mass relative to the entire carrier; An electrostatic image developer comprising:
10. a developing device that contains the electrostatic image developer according to any one of claims 1 to 9 and develops an electrostatic image formed on a surface of an image carrier into a toner image by using the electrostatic image developer; A process cartridge that is detachably attached to an image forming apparatus.
11. An image carrier; a charging device for charging the surface of the image carrier; an electrostatic image forming device for forming an electrostatic image on the charged surface of the image carrier; a developing device that contains the electrostatic image developer according to any one of claims 1 to 9 and develops the electrostatic image formed on the surface of the image carrier into a toner image by the electrostatic image developer; a transfer device for transferring the toner image formed on the surface of the image carrier to a surface of a recording medium; a fixing device for fixing the toner image transferred onto the surface of the recording medium; An image forming apparatus comprising:
12. a charging step of charging the surface of the image carrier; an electrostatic image forming step of forming an electrostatic image on the charged surface of the image carrier; a developing step of developing the electrostatic image formed on the surface of the image carrier into a toner image by using the electrostatic image developer according to any one of claims 1 to 9; a transfer step of transferring the toner image formed on the surface of the image carrier onto a surface of a recording medium; a fixing step of fixing the toner image transferred onto the surface of the recording medium; The image forming method according to claim 1,
Citation Information
Patent Citations
Toner for electrostatic charge image development and production method of the same
JP2011237792A
Image-forming method
JP2011237793A
Toner for developing electrostatic charge image and developer
JP2013160886A
Electrostatic charge image developing toner
JP2019144368A
Electrostatic latent image development toner and method of evaluating fixability of the same
JP2020042121A