Non-calcined aggregate and production method of non-calcined aggregate, flesh concrete, hydraulic hardened body
The non-fired aggregate composition with specified slag powder and cement ratios, combined with appropriate curing, effectively reduces CO2 emissions and enhances strength in hydraulic hardened bodies like concrete.
Patent Information
- Application Number
- JP2023044174
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2043-03-20
AI Technical Summary
Existing non-fired aggregates do not adequately address carbon dioxide emissions and strength requirements for hydraulic hardened bodies like concrete and mortar, with a need to reduce CO2 emissions and enhance strength.
A non-fired aggregate composition comprising 3.00% to 4.00% by weight of pulverized blast furnace slag powder and cement, with a ratio of cement to slag powder between 10 and 40, and a granulation process without firing, followed by curing methods like moist, sealed, or accelerated curing to enhance strength.
The method suppresses CO2 emissions and increases the strength of the non-fired aggregate and hydraulic hardened bodies, such as concrete, by optimizing the composition and curing process.
Smart Images

Figure 2024134072000001 
Figure 2024134072000002 
Figure 2024134072000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a non-calcined aggregate, a method for producing the non-calcined aggregate, fresh concrete, and a hydraulically hardened body. [Background technology]
[0002] In general, hydraulic hardened bodies such as concrete and mortar contain various aggregates depending on the desired properties of the hydraulic hardened body. For example, artificial aggregates can be produced by mixing various raw materials and firing them. Thus, when producing aggregates, a large amount of carbon dioxide (CO2, carbon dioxide gas) can be emitted by firing.
[0003] For example, Patent Document 1 describes a non-calcined artificial aggregate made by molding coal ash and cement as main components, with the coal ash having an average particle size of 12 μm or less. In Patent Document 1, no calcination is performed during the production of the aggregate because large-scale calcination equipment and complicated calcination temperature control are not required, and production and maintenance are easy, and as a result, CO2 emissions during aggregate production are suppressed.
[0004] Cement emits a large amount of CO2 during the production process due to the decarbonation of raw materials and the combustion during firing, and the aggregate in Patent Document 1 contains up to 50% of CO2. In recent years, in particular, there has been a demand for reducing CO2 emissions more than ever before, in response to growing interest in curbing climate change. However, Patent Document 1 does not mention or even consider the reduction of CO2 emissions. In addition to reducing CO2 emissions, aggregates are also required to have increased strength for use in hydraulic hardened bodies. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 9-12349 Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide a non-calcined aggregate that can reduce CO2 emissions and increase strength, a method for producing the non-calcined aggregate, and fresh concrete and a hydraulic hardened body that contain the non-calcined aggregate. [Means for solving the problem]
[0007] [1] An unfired aggregate comprising ground granulated blast furnace slag containing 3.00% by weight or more and 4.00% by weight or less of SO3 and cement, wherein the cement content ratio to the ground granulated blast furnace slag (cement weight / ground granulated blast furnace slag weight) is 10 or more and 40 or less. [2] The bone dry density of the unfired aggregate is 1.70 g / cm 3 The non-fired aggregate according to the above item [1]. [3] The non-calcined aggregate according to the above [1] or [2], wherein the average particle size of the ground granulated blast furnace slag is 12 μm or less. [4] Fresh concrete containing the non-calcined aggregate described in any one of [1] to [3] above. [5] A hydraulic hardened body comprising the uncalcined aggregate according to any one of [1] to [3] above. [6] A method for producing uncalcined aggregate, comprising: a granulation step of granulating uncalcined granules from a mixture containing ground granulated blast furnace slag containing 3.00% by weight or more and 4.00% by weight or less of SO3, cement, and water, without calcining the mixture; and a hardening step of hardening the uncalcined granules through moist curing, water retention curing, sealed curing, or accelerated curing, to obtain uncalcined aggregate in which the ratio of the cement to the ground granulated blast furnace slag (weight of cement / weight of ground granulated blast furnace slag) is 10 or more and 40 or less. Effect of the Invention
[0008] According to the present invention, it is possible to provide a non-calcined aggregate that can reduce CO2 emissions and increase strength, a method for producing the non-calcined aggregate, and fresh concrete and hydraulic hardened body that contain the non-calcined aggregate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, a detailed description will be given based on an embodiment.
[0010] As a result of extensive research, the inventors have discovered that by using ground granulated blast furnace slag containing a predetermined amount of SO3 and setting the content ratio of ground granulated blast furnace slag to cement within a predetermined range, it is possible to reduce CO2 emissions during the production of non-calcined aggregate and to increase the strength of the non-calcined aggregate, and have completed the present invention based on this finding.
[0011] The non-calcined aggregate of the present invention contains ground granulated blast furnace slag containing 3.00% or more and 4.00% or less by weight of SO3 and cement, and the cement content ratio to the ground granulated blast furnace slag (cement weight / ground granulated blast furnace slag weight) is 10 or more and 40 or less.
[0012] The method for producing unsintered aggregate of the present invention includes a granulation step of granulating unsintered granules from a mixture containing ground granulated blast furnace slag containing 3.00% by weight or more and 4.00% by weight or less of SO3, cement, and water, without sintering, and a hardening step of hardening the unsintered granules through moist curing, water retention curing, sealed curing, or accelerated curing to obtain unsintered aggregate having a cement ratio to ground granulated blast furnace slag (cement weight / ground granulated blast furnace slag weight) of 10 or more and 40 or less.
[0013] First, the non-fired aggregate will be described.
[0014] The non-calcined aggregate of the embodiment contains ground granulated blast furnace slag and cement.
[0015] The ground granulated blast furnace slag that constitutes the non-calcined aggregate is a fine powder specified in JIS A 6206:2013 "ground granulated blast furnace slag for concrete". Granulated blast furnace slag is made by quenching molten blast furnace slag, which is produced at the same time as shear iron in a blast furnace, with water or air, and has a basicity of 1.60 or more. Ground granulated blast furnace slag is made by drying and pulverizing this granulated blast furnace slag, or by adding gypsum to it. By replacing part of the Portland cement with ground granulated blast furnace slag, it is possible to reduce carbon dioxide emissions during the cement manufacturing stage.
[0016] Furthermore, the ground granulated blast furnace slag contains 3.00% by weight or more and 4.00% by weight or less of SO3. If the amount of SO3 contained in the ground granulated blast furnace slag is within the above range, needle-shaped crystals of ettringite are generated in fresh concrete when non-calcined aggregate is produced, and the ettringite forms a hydrate skeleton, which contributes to increasing the strength of the non-calcined aggregate at an early age, thereby enabling the non-calcined aggregate to exhibit high strength.
[0017] In addition, by adding gypsum to ground granulated blast furnace slag, the amount of SO3 contained in the ground granulated blast furnace slag can be easily controlled.
[0018] The cement constituting the non-calcined aggregate is preferably Portland cement. Portland cement includes ordinary Portland cement (OPC), as well as high-early-strength, ultra-high-early-strength, moderate-heat, low-heat, sulfate-resistant, and other types, which are specified in JIS R 5210:2019. For the non-calcined aggregate, one or more of these various Portland cements may be used.
[0019] Regarding the ground granulated blast furnace slag and cement that constitute the non-calcined aggregate, the content ratio of cement to the ground granulated blast furnace slag (weight of cement / weight of ground granulated blast furnace slag) is not less than 10, and preferably not less than 20. When the content ratio (weight of cement / weight of ground granulated blast furnace slag) is not less than 10, it is possible to achieve an increase in the strength of the non-calcined aggregate due to ettringite resulting from the ground granulated blast furnace slag.
[0020] In addition, the content ratio (cement weight / ground granulated blast furnace slag weight) is not more than 40. When the content ratio is not more than 40, the cement content in the non-calcined aggregate can be reduced, so that the amount of CO2 emissions during the production of the non-calcined aggregate can be suppressed.
[0021] In this way, the main components of non-calcined aggregate, ground granulated blast furnace slag and cement, are contained in greater amounts than cement, so CO2 emissions during the production of non-calcined aggregate can be reduced. Also, although the cement content is less than that of ground granulated blast furnace slag, the inclusion of ground granulated blast furnace slag in non-calcined aggregate, which contains a certain amount of SO3, can increase the strength of the non-calcined aggregate.
[0022] Furthermore, as described below, non-calcined aggregate is produced without calcination, which reduces the amount of CO2 emitted during production of non-calcined aggregate.
[0023] The bone dry density of unfired aggregate is 1.70 g / cm 3 The bone dry density of the non-fired aggregate is preferably 1.70 g / cm or more. 3 If the above ratio is met, the strength of the non-fired aggregate can be further increased.
[0024] The average particle size of the ground granulated blast furnace slag is preferably 12 μm or less, more preferably 10 μm or less. When the average particle size of the ground granulated blast furnace slag is 12 μm or less, the specific surface area of the ground granulated blast furnace slag increases, which facilitates the promotion of chemical reactions, thereby further increasing the strength of the non-calcined aggregate.
[0025] In addition, the specific surface area of ground granulated blast furnace slag is 5000 cm 2 / g or more 7000cm 2 When the Cd content is 1 / g or less, the strength of the non-fired aggregate can be further increased.
[0026] The non-calcined aggregate may further contain other additives, such as silica fume, fly ash, calcium carbonate, etc., within the scope of the effects of the present invention.
[0027] In addition, for fresh concrete containing the above non-calcined aggregate and hydraulic hardened body containing the above non-calcined aggregate, CO2 emissions during the production of the non-calcined aggregate can be reduced, so that CO2 emissions during the construction of a hydraulic hardened body obtained by hardening fresh concrete containing the non-calcined aggregate can be reduced. In addition, since the strength of the non-calcined aggregate is increased, the strength of the hydraulic hardened body containing the non-calcined aggregate can also be increased accordingly.
[0028] Next, a method for producing the non-fired aggregate will be described.
[0029] The method for producing the unsintered aggregate according to the embodiment includes a granulation step and a hardening step, and can produce the unsintered aggregate described above.
[0030] In the granulation process constituting the method for producing non-calcined aggregate, non-calcined granules are granulated from a kneaded material containing ground granulated blast furnace slag containing 3.00% by weight to 4.00% by weight of SO3, cement, and water, without sintering. In this way, in the granulation process, non-calcined granules are produced from the kneaded material without sintering. For example, non-calcined granules are produced from the kneaded material at room temperature (in an environment without temperature control).
[0031] In addition, when the non-sintered aggregate contains the above-mentioned other additives, the other additives are added to the kneaded material, so that the kneaded material also contains the other additives, thereby producing a non-sintered granulated material containing the other additives.
[0032] Although it depends on the granulation method, for example, the kneaded product in the granulation step contains 10.0 parts by weight to 20.0 parts by weight of water per 100 parts by weight of the ground granulated blast furnace slag and cement in total.
[0033] In the hardening step carried out after the granulation step, the non-calcined granules obtained in the granulation step are hardened by wet curing, water retention curing, sealed curing or accelerated curing to obtain non-calcined aggregate having the above content ratio (cement weight / ground granulated blast furnace slag weight) of 10 to 40. In the hardening step, the non-calcined granules are cured in a state of high moisture as in the above curing to promote the hydration reaction and produce non-calcined aggregate, thereby increasing the strength of the non-calcined aggregate. In the hardening step, only one of the above curing steps may be carried out, or two or more of them may be carried out.
[0034] When the content ratio is 10 or more, the strength of the non-calcined aggregate can be increased. Therefore, the content ratio is preferably 20 or more. Also, when the content ratio is 40 or less, the cement content in the non-calcined aggregate can be reduced, so that the amount of CO2 emissions during the production of the non-calcined aggregate can be reduced.
[0035] In this way, the content of ground granulated blast furnace slag and cement that make up the non-calcined aggregate is higher in ground granulated blast furnace slag than in cement, so CO2 emissions during the production of non-calcined aggregate can be reduced. Also, although the cement content is lower than that of ground granulated blast furnace slag, the inclusion of ground granulated blast furnace slag in the non-calcined aggregate, which contains a certain amount of SO3, can increase the strength of the non-calcined aggregate.
[0036] Furthermore, in the manufacturing method of non-calcined aggregate, no calcination is performed in the entire manufacturing process including the granulation process, which reduces the amount of CO2 emissions in the manufacturing method of non-calcined aggregate.
[0037] In order to increase the strength of the non-sintered granules and maintain the structure of the non-sintered granules during the curing, air curing may be performed before the curing in the hardening step or between the curing steps if the curing is performed multiple times.
[0038] From the viewpoint of further increasing the strength of the non-calcined aggregate, the average particle size of the ground granulated blast furnace slag in the non-calcined aggregate is preferably 12 μm or less, and more preferably 10 μm or less.
[0039] The method of the granulation step can be appropriately selected depending on the desired properties of the non-calcined aggregate and the manufacturing conditions of the non-calcined aggregate. For example, when the non-calcined granulated material is granulated from the kneaded material by rolling granulation using a rolling granulator such as a pan pelletizer or a rolling granulator in which the kneaded material is placed in a container excluding the balls from a ball mill and the container is rotated, maintenance of the equipment used, such as post-treatment of the container and the rolling granulator after granulation, is easy. Furthermore, when the non-calcined granulated material is granulated from the kneaded material by rolling granulation using a pan-type granulator such as a pan pelletizer, the non-calcined granulated material can be granulated with higher accuracy.
[0040] In addition, when accelerated curing is performed in the hardening step, from the viewpoint of increasing the strength of the unfired aggregate at an early age, the accelerated curing is preferably steam curing in which water vapor is supplied. In this case, the temperature of the steam curing is preferably 40°C or higher and 100°C or lower, and the time is preferably 13 hours or longer.
[0041] According to the embodiment described above, by using ground granulated blast furnace slag containing a predetermined amount of SO3 and setting the content ratio of ground granulated blast furnace slag to cement within a predetermined range, it is possible to reduce CO2 emissions during the production of non-calcined aggregate and to increase the strength of the non-calcined aggregate.
[0042] Although the embodiments have been described above, the present invention is not limited to the above embodiments, but includes all aspects included in the concept and scope of the claims of the present disclosure, and can be modified in various ways within the scope of the present disclosure. EXAMPLES
[0043] Next, examples and comparative examples will be described, but the present invention is not limited to these examples.
[0044] (Examples 1-1 to 1-5) Fine Cerament 6000A (density 2.91 g / cm) is used as fine powder of blast furnace slag. 3 ) was used, and Portland cement (density 3.16 g / cm 3) was used to granulate the kneaded material having the composition shown in Table 1 at room temperature without firing it, using a rolling granulator. The unsintered granulated material was then hardened by curing in air for 2 days and then curing in water for 5 days, to obtain unsintered aggregate having the composition shown in Table 1.
[0045] (Comparative Example 1-1) An unsintered aggregate was obtained in the same manner as in Example 1-1 above, except that no cement was used.
[0046] (Comparative Example 1-2) An unfired aggregate was obtained in the same manner as in Example 1-1 above, except that the content ratio (cement weight / ground granulated blast furnace slag weight) was set to less than 10.
[0047] (Examples 2-1 to 2-4) Fine Cerament 6000A (density 2.91 g / cm) is used as fine powder of blast furnace slag. 3 ) was used, and Portland cement (density 3.16 g / cm 3 ) was used to granulate the kneaded material having the composition shown in Table 2 at room temperature without firing it, using a rolling granulator. Next, the kneaded material was cured in air for 2 days, then cured in water for 5 days, then cured in sealed water for 2 days, and then cured in water for 5 days. The unsintered granulated material was hardened to obtain unsintered aggregate having the composition shown in Table 2.
[0048] (Comparative Example 2-1) An unsintered aggregate was obtained in the same manner as in Example 2-1 above, except that no cement was used.
[0049] (Examples 3-1 to 3-3) Fine Cerament 6000A (density 2.91 g / cm) is used as fine powder of blast furnace slag. 3 ) was used, and Portland cement (density 3.16 g / cm 3) was used to granulate the kneaded material having the composition shown in Table 3 at room temperature without firing it, using a rolling granulator. Next, the unsintered granulated material was hardened by sealing and curing for two days, followed by underwater curing for five days, to obtain unsintered aggregate having the composition shown in Table 3.
[0050] (Comparative Example 3-1) An unsintered aggregate was obtained in the same manner as in Example 3-1 above, except that no cement was used.
[0051] [Table 1]
[0052] [Table 2]
[0053] [Table 3]
[0054] The unsintered aggregates obtained in the above Examples and Comparative Examples were subjected to the following measurements. The results are shown in Tables 4 to 6.
[0055] [1] Crushing strength The crushing strength of the unfired aggregate was measured according to JIS Z 8841 Granulated materials - Strength test method.
[0056] [2] Absolute dry density Bone dry density of unfired aggregate d d (g / cm 3) was calculated by the following formula (1). First, to measure the volume of the non-calcined aggregate, the sample (non-calcined aggregate) was immersed in water for 10 minutes, and then the water film was wiped off with a rag, and the mass of the sample was measured and recorded as the surface dry mass m2 (g). Next, the sample was placed in a pycnometer, which was filled with water, and the air bubbles were removed, the lid was placed, and the mass of the pycnometer m3 (g) was measured. Next, the sample after the volume measurement was dried at 105°C until it reached a constant weight, and the mass was measured and recorded as the bone dry mass m4 (g). In addition, water was placed in the pycnometer, and the air bubbles were removed, the lid was placed, and the mass of the pycnometer m1 (g) was measured. The following formula (1) is based on JIS A 1135.
[0057] d d =m4×ρ w / (m1+m2-m3) Equation (1)
[0058] m1: Total mass of the pycnometer filled with water (g) m2: Mass of the surface-dry state of the absorbed non-calcined aggregate (surface dry mass) (g) m3: Mass of the pycnometer filled with surface-dried sample and water (g) m4: Mass of unfired aggregate after drying at 105℃ (bone dry mass) (g) ρ w : Density of water at test temperature (g / cm 3 )
[0059] [3] Water absorption rate The water absorption rate Q (%) of the non-fired aggregate was calculated by the following formula (2).
[0060] Q=(m2-m4) / m4×100 Formula (2)
[0061] [Table 4]
[0062] [Table 5]
[0063] [Table 6]
[0064] As described above, in the above examples, the strength of the non-calcined aggregate was improved and the CO2 emissions during the production of the non-calcined aggregate were suppressed by using ground granulated blast furnace slag containing a predetermined amount of SO3 and setting the content ratio of the ground granulated blast furnace slag to cement within a predetermined range. On the other hand, in the above comparative examples, the content ratio of the ground granulated blast furnace slag to cement was outside the predetermined range, so the strength of the non-calcined aggregate could not be improved and the CO2 emissions during the production of the non-calcined aggregate could not be suppressed. In particular, in comparative example 1-1, the strength of the non-calcined granulated material was very low, so the non-calcined granulated material was damaged during underwater curing.
Claims
1. SO 3 % or more and 4.00% or less by weight of ground granulated blast furnace slag, and cement, wherein the content ratio of the cement to the ground granulated blast furnace slag (weight of cement / weight of ground granulated blast furnace slag) is 10 or more and 40 or less.
2. The bone dry density of the unfired aggregate is 1.70 g / cm 3 The non-fired aggregate according to claim 1 .
3. The non-fired aggregate according to claim 1, wherein the average particle size of the ground granulated blast furnace slag is 12 μm or less.
4. Fresh concrete comprising the non-calcined aggregate according to any one of claims 1 to 3.
5. A hydraulically hardened body comprising the uncalcined aggregate according to any one of claims 1 to 3.
6. SO 3 A granulation process for granulating a non-sintered granulated material from a kneaded material containing ground granulated blast furnace slag containing 3.00% by weight or more and 4.00% by weight or less, cement, and water without firing the kneaded material; a hardening step of hardening the non-calcined granules by wet curing, water retention curing, sealed curing or accelerated curing to obtain non-calcined aggregate having a content ratio of the cement to the ground granulated blast furnace slag (cement weight / ground granulated blast furnace slag weight) of 10 or more and 40 or less; A method for producing an unfired aggregate comprising the steps of:
Citation Information
Patent Citations
Method for preparing functional permeable material from multi-source solid waste
CN114085054A
Use of coal ash
JP1991141139A
Artificial aggregate and its production
JP1997012349A
Low-alkalinity and high-strength cement composition
JP2000072519A
Sulfate-resisting cement