Liquid crystal aligning agent, liquid crystal alignment film and production method of the same, and liquid crystal element and production method of the same
A liquid crystal aligning agent with specific polymer structures addresses impurity and mechanical stress issues in high-definition elements, ensuring stable voltage holding and improved transmittance.
Patent Information
- Application Number
- JP2023044278
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
AI Technical Summary
High-definition liquid crystal elements face issues with ionic impurities from insulating films eluting into the liquid crystal, leading to decreased voltage holding ratios and increased susceptibility to mechanical stress, particularly in high-transmittance and narrow-frame designs.
A liquid crystal aligning agent containing a polymer with specific partial structures, such as nitrogen-containing heterocyclic groups and polymerizable carbon-carbon double bonds, is used to form a film with enhanced impurity resistance and seal adhesion, improving mechanical strength and transmittance.
The solution results in a liquid crystal aligning film with improved impurity resistance and seal adhesion, maintaining voltage holding ratios and enhancing the mechanical stability of high-definition liquid crystal elements.
Smart Images

Figure 2024134142000001 
Figure 2024134142000002 
Figure 2024134142000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a liquid crystal aligning agent, a liquid crystal alignment film and a manufacturing method thereof, and a liquid crystal element and a manufacturing method thereof. [Background technology]
[0002] Conventionally, various driving methods have been developed for liquid crystal elements, which differ in electrode structure and physical properties of liquid crystal molecules used, and various liquid crystal elements are known, such as TN type, STN type, VA type, MVA type, in-plane switching type (IPS type), FFS type, optical compensation bend type (OCB type), and PSA type. These liquid crystal elements have a liquid crystal alignment film for aligning liquid crystal molecules. A liquid crystal alignment film is generally formed on a substrate by applying a liquid crystal alignment agent, which is a polymer component dissolved or dispersed in an organic solvent, to the substrate surface and preferably heating the applied liquid crystal alignment film.
[0003] In recent years, large-screen, high-definition liquid crystal televisions have become mainstream, and small display terminals such as smartphones and tablet PCs have become more widespread, further increasing the demand for high quality liquid crystal elements. In order to meet such demands for high quality, various liquid crystal alignment agents have been proposed (see, for example, Patent Document 1 and Patent Document 2). Patent Document 1 discloses that a liquid crystal alignment film is formed using a polymer obtained by reacting a diamine compound containing a diamine having a fluorene structure with a tetracarboxylic dianhydride. Patent Document 2 also discloses that a crosslinkable compound is contained in the liquid crystal alignment agent as a low molecular compound that improves the hardness of the liquid crystal alignment film, together with a polyimide or a polyimide precursor. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2002-155138 A [Patent Document 2] International Publication No. 2020 / 171128 Summary of the Invention [Problem to be solved by the invention]
[0005] As the definition of liquid crystal elements increases, the quality requirements become more stringent. For example, high-definition liquid crystal panels such as 4K and 8K often have an insulating film, but in liquid crystal panels with an insulating film, ionic impurities from the insulating film may dissolve into the liquid crystal through the liquid crystal alignment film. If ionic impurities dissolve into the liquid crystal, there is a concern that the quality of the liquid crystal element may decrease, such as by decreasing the voltage holding rate. Therefore, the liquid crystal alignment film is required to have the performance of suppressing the intrusion of impurities generated in the element into the liquid crystal and suppressing the decrease in the voltage holding rate caused by the impurities (hereinafter, also referred to as "impurity resistance"). In addition, in high-definition liquid crystal panels, the occupancy rate of the black matrix (BM) and thin film transistors (TFTs) increases. Therefore, the importance of improving the transmittance at the opening of the panel is increasing.
[0006] High-definition liquid crystal elements are required to have not only further improvements in impurity resistance and transmittance, but also excellent mechanical properties of the liquid crystal alignment film and adhesion to the substrate. For example, in mobile applications such as smartphones and tablet PCs, as well as large TVs and PC monitors, narrower frames are being sought from the viewpoint of design and miniaturization of display devices. One method for narrowing the frame is to form a liquid crystal alignment film on the entire substrate surface, and then apply a sealant to the liquid crystal alignment film to bond the substrates together. On the other hand, when the sealant is placed on the liquid crystal alignment film, force is easily applied to the part where the sealant is placed. For this reason, if the mechanical strength of the liquid crystal alignment film or the adhesion to the substrate is insufficient, the adhesion between the substrates (hereinafter also referred to as "sealing adhesion") will decrease, and there is a concern that the substrates will be easily peeled off due to the action of external forces, etc.
[0007] The present invention has been made in consideration of the above problems, and has as its main object to provide a liquid crystal alignment agent with which a liquid crystal alignment film having excellent impurity resistance and seal adhesion can be obtained, and a liquid crystal element having good transmittance can be obtained. [Means for solving the problem]
[0008] In order to further improve the quality of liquid crystal elements, the present inventors have conducted research and found that the above problems can be solved by improving the components of a liquid crystal alignment agent. Specifically, the present invention provides the following means.
[0009] [1] The following formula (1) [ka] (In formula (1), R 1 and R 2 are each independently a monovalent substituent. n1 and n2 are each independently 0 or 1. m1 is an integer of 0 to (n1×2+4). m2 is an integer of 0 to (n2×2+4). R 1 If there are multiple R 1 are the same or different, R 2 If there are multiple R 2 are the same or different. "*" represents a bond to a carbon atom.) and a partial structure (a2) shown below in the same molecule or in different molecules. Partial structure (a2): at least one selected from the group consisting of a nitrogen-containing heterocyclic structure, a partial structure represented by the following formula (2), and a partial structure represented by the following formula (3): [ka] (In formula (2), Y 1 A is a hydrogen atom or a monovalent group which is eliminated by heating and replaced with a hydrogen atom. 1 A is an alkanediyl group, a substituted or unsubstituted divalent alicyclic group, or a substituted or unsubstituted divalent aromatic ring group. 2 is an alkanediyl group. "*" represents a bond.) [ka] (In formula (3), Y 2 is a monovalent group that is eliminated by heating and replaced with a hydrogen atom. X3 R is a single bond or an alkanediyl group. 4 and R 5 are each independently a hydrogen atom or a monovalent hydrocarbon group. "*" represents a bond.)
[0010] [2] A polymer having a partial structure (a1) represented by the above formula (1) and -OE 1 (wherein E 1 is a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a monovalent leaving group.), a mercapto group, a protected mercapto group, an amino group, a protected amino group, an oxetanyl group, -Si(OR 11 ) r (R 12 ) 3-r (wherein R 11 and R 12 are each independently a monovalent hydrocarbon group having 1 to 10 carbon atoms, r is an integer of 1 to 3, and when r is 2 or 3, multiple R 11 are the same or different, and when r is 1, multiple R 12 are the same or different, and a compound having in one molecule a total of two or more of at least one type selected from the group consisting of polymerizable carbon-carbon double bond groups.
[0011] [3] A liquid crystal alignment film formed by using the liquid crystal aligning agent according to [1] or [2] above. [4] A liquid crystal element comprising the liquid crystal alignment film according to [3] above. [5] A method for producing a liquid crystal alignment film, comprising: forming a coating film using the liquid crystal alignment agent according to [1] or [2] above; and irradiating the coating film with light to impart liquid crystal alignment ability. [6] A process of forming a coating film on each conductive film of a pair of substrates having a conductive film by using the liquid crystal aligning agent according to [1] or [2] above; constructing a liquid crystal cell by disposing the pair of substrates on which the coating film is formed so that the coating film faces each other via a liquid crystal layer containing a photopolymerizable compound; and irradiating the liquid crystal cell with light while applying a voltage between the conductive films. A method for manufacturing a liquid crystal element comprising the steps of: Effect of the Invention
[0012] According to the liquid crystal aligning agent of the present invention, a liquid crystal alignment film having excellent impurity resistance and seal adhesion can be obtained. In addition, by forming a liquid crystal alignment film using the liquid crystal aligning agent of the present invention, a liquid crystal element having good transmittance can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Liquid crystal alignment agent The liquid crystal aligning agent of the present disclosure contains a polymer having a partial structure (a1) represented by the following formula (1). [ka] (In formula (1), R 1 and R 2 are each independently a monovalent substituent. n1 and n2 are each independently 0 or 1. m1 is an integer of 0 to (n1×2+4). m2 is an integer of 0 to (n2×2+4). R 1 If there are multiple R 1 are the same or different, R 2 If there are multiple R 2 are the same or different. "*" represents a bond to a carbon atom.)
[0014] In the present disclosure, specific embodiments of the liquid crystal aligning agent containing a polymer having the partial structure (a1) include the following first liquid crystal aligning agent and second liquid crystal aligning agent. First liquid crystal alignment agent: A liquid crystal alignment agent containing a polymer (hereinafter also referred to as "polymer (P1)") having a partial structure (a1) represented by the above formula (1) and a partial structure (a2) shown below in the same molecule or in different molecules. Partial structure (a2): at least one selected from the group consisting of a nitrogen-containing heterocyclic structure, a partial structure represented by the following formula (2), and a partial structure represented by the following formula (3): [ka] (In formula (2), Y 1A is a hydrogen atom or a monovalent group which is eliminated by heating and replaced with a hydrogen atom. 1 A is an alkanediyl group, a substituted or unsubstituted divalent alicyclic group, or a substituted or unsubstituted divalent aromatic ring group. 2 is an alkanediyl group. "*" represents a bond.) [ka] (In formula (3), Y 2 is a monovalent group that is eliminated by heating and replaced with a hydrogen atom. X 3 R is a single bond or an alkanediyl group. 4 and R 5 are each independently a hydrogen atom or a monovalent hydrocarbon group. "*" represents a bond.)
[0015] Second liquid crystal aligning agent: a polymer having a partial structure (a1) represented by the above formula (1) (hereinafter also referred to as "polymer (P2)") and -OE 1 (wherein E 1 is a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a monovalent leaving group.), a mercapto group, a protected mercapto group, an amino group, a protected amino group, an oxetanyl group, -Si(OR 11 ) r (R 12 ) 3-r (wherein R 11 and R 12 are each independently a monovalent hydrocarbon group having 1 to 10 carbon atoms, r is an integer of 1 to 3, and when r is 2 or 3, multiple R 11 are the same or different, and when r is 1, multiple R 12 are the same or different, and a compound having a total of two or more kinds selected from the group consisting of polymerizable carbon-carbon double bond groups in one molecule (hereinafter also referred to as "compound (A1)").
[0016] According to the above-mentioned first liquid crystal alignment agent and second liquid crystal alignment agent, a liquid crystal alignment film having excellent impurity resistance and seal adhesion can be obtained, and a liquid crystal element having good transmittance can be obtained. Hereinafter, each component contained in the first liquid crystal alignment agent and the second liquid crystal alignment agent, and other components that are optionally mixed as necessary will be described. Note that, unless otherwise specified, each component may be used alone or in combination of two or more.
[0017] Here, in this specification, the term "hydrocarbon group" includes chain-shaped hydrocarbon groups, alicyclic hydrocarbon groups, and aromatic hydrocarbon groups. The term "chain-shaped hydrocarbon group" means a straight-chain hydrocarbon group and a branched hydrocarbon group that do not include a cyclic structure in the main chain and are composed only of a chain structure. However, the chain-shaped hydrocarbon group may be saturated or unsaturated. The term "alicyclic hydrocarbon group" means a hydrocarbon group that includes only an alicyclic hydrocarbon structure as a ring structure and does not include an aromatic ring structure. However, the alicyclic hydrocarbon group does not necessarily have to be composed only of an alicyclic hydrocarbon structure, and also includes those that have a chain structure as a part of it. The term "aromatic hydrocarbon group" means a hydrocarbon group that includes an aromatic ring structure as a ring structure. However, the aromatic hydrocarbon group does not necessarily have to be composed only of an aromatic ring structure, and may include a chain structure or an alicyclic hydrocarbon structure as a part of it. The term "aromatic ring" includes aromatic hydrocarbon rings and aromatic heterocycles. The term "organic group" means an atomic group obtained by removing any hydrogen atom from a compound containing carbon (i.e., an organic compound).
[0018] The "main chain" of a polymer refers to the "trunk" portion of the polymer, which is the longest chain of atoms. It is permissible for this "trunk" portion to contain a ring structure. For example, "having a specific structure in the main chain" means that the specific structure constitutes a part of the main chain. A "side chain" refers to a portion branched off from the "trunk" portion of the polymer. "(Meth)acrylo" is a term that includes acrylo and methacrylo, and "(meth)acrylate" is a term that includes acrylate and methacrylate. A group that is eliminated by heating and replaced with a hydrogen atom is also called a "thermally eliminable group."
[0019] [First liquid crystal alignment agent] <Polymer (P1)> ·Substructure (a1) In the above formula (1), R 1 or R 2 Examples of the monovalent substituent represented by the formula (1) include an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, a halogen atom (e.g., a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, etc.), a halogenated alkyl group having 1 to 12 carbon atoms, a halogenated alkoxy group having 1 to 12 carbon atoms, a hydroxyl group, etc. The two bonds (*) in the formula (1) may be bonded to a carbon atom constituting the main chain of the polymer (P1), or may be bonded to a carbon atom constituting a side chain.
[0020] From the viewpoint of obtaining a liquid crystal alignment film with higher seal adhesion and from the viewpoint of forming a film with high impurity resistance, it is preferable that the two bonds (*) in the above formula (1) are each bonded to an aromatic ring (preferably different aromatic rings). Specifically, it is preferable that the polymer (P1) contains, as a structure having the partial structure (a1) represented by the above formula (1), at least one partial structure selected from the group consisting of the partial structure represented by the following formula (1-1) and the partial structure represented by the following formula (1-2). [ka] (In formula (1-1) and formula (1-2), Ar 1 and Ar 2 are each independently a divalent aromatic ring group. 1 and X 2 are each independently a single bond, -O-, -S-, -CO-, -NR 8 -, -COO-, -CONR 8 -, -NR 8 CONR 9 -, -SO2-, -SO2-O-, an alkanediyl group having 1 to 10 carbon atoms, or an alkanediyl group having 2 to 10 carbon atoms in which any methylene group is -O-, -S-, -CO-, -NR 8 -, -COO-, -OCO-, -CONR 8 -, -NR 8 CO- or -NR 8 CONR9 - is a group replaced by R 6 and R 7 are each independently a single bond or a divalent aromatic ring group. 8 and R 9 are each independently a hydrogen atom or a monovalent organic group. 3 and Ar 4 are each independently a trivalent aromatic ring group. 1 , R 2 , n1, n2, m1 and m2 are defined as in the above formula (1). "*" represents a bond.)
[0021] In the above formula (1-1) and formula (1-2), Ar 1 Or Ar 2 The divalent aromatic ring group represented by is a group in which two hydrogen atoms have been removed from the ring portion of a substituted or unsubstituted aromatic ring. Examples of the aromatic ring include aromatic hydrocarbon rings such as a benzene ring, a naphthalene ring, and an anthracene ring; nitrogen-containing aromatic heterocycles such as a pyridine ring, a pyrazine ring, a pyrimidine ring, a pyridazine ring, and an imidazole ring; and sulfur-containing aromatic heterocycles such as a thiophene ring. When the aromatic ring has a substituent, examples of the substituent include an alkyl group having 1 to 5 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, a halogenated alkyl group having 1 to 5 carbon atoms, a halogenated alkoxy group having 1 to 5 carbon atoms, an alkoxyalkyl group having 1 to 5 carbon atoms, an alkoxyalkoxyalkyl group having 1 to 5 carbon atoms, a halogen atom, and a hydroxyl group.
[0022] Ar 1 and Ar 2 From the viewpoints of enhancing the effect of improving seal adhesion, of forming a film with high impurity resistance, and of easy availability of monomers, among these, is preferably a group in which two hydrogen atoms have been removed from the ring portion of a substituted or unsubstituted aromatic hydrocarbon ring, and more preferably a group in which two hydrogen atoms have been removed from the ring portion of a substituted or unsubstituted benzene ring.
[0023] X 1 Or X 2 Ga-NR 8 -,-CONR 8 -OR-NR8 CONR 9 - If R 8 or R 9 Examples of the monovalent organic group represented by the formula (I) include a monovalent hydrocarbon group having 1 to 10 carbon atoms and a monovalent thermally detachable group. 8 or R 9 When R is a monovalent hydrocarbon group having 1 to 10 carbon atoms, examples of the hydrocarbon group include an alkyl group having 1 to 10 carbon atoms, a monovalent alicyclic hydrocarbon group having 3 to 10 carbon atoms, and a monovalent aromatic hydrocarbon group having 5 to 10 carbon atoms. Among these, an alkyl group having 1 to 5 carbon atoms, a cyclohexyl group, or a phenyl group is preferred, and an alkyl group having 1 to 3 carbon atoms is more preferred. A monovalent thermally detachable group is a group which is detached by the application of heat and is replaced with a hydrogen atom. In terms of high detachability by heat, R 8 or R 9 The thermally detachable group represented by the following formula is preferably a tert-butoxycarbonyl group (Boc group).
[0024] X 1 and X 2 From the viewpoint of improving the seal adhesion, among the above, a single bond, -O- or -CONR 8 - is preferred, -O- or -CONR 8 - is more preferable. X 1 Ar in 1 The bond on the opposite side and X 2 Ar in 2 From the viewpoint of obtaining a liquid crystal alignment film having excellent impurity resistance and mechanical strength, it is preferable that the bond on the opposite side to the bond on the opposite side is bonded to an aromatic ring. 1 and Ar 2 Examples of the aromatic ring include the same aromatic rings as those exemplified in the description of 1.
[0025] Ar 3 Or Ar 4 The trivalent aromatic ring group represented by the formula (I) is a group in which three hydrogen atoms have been removed from the ring portion of a substituted or unsubstituted aromatic ring. Specific and preferred examples of the aromatic ring include Ar 1 and Ar 2 The divalent aromatic ring group in Ar3 and Ar 4 From the viewpoint of increasing the effect of improving seal adhesion and of easy availability of the monomer, among these, is preferably a group in which three hydrogen atoms have been removed from the ring portion of a substituted or unsubstituted aromatic hydrocarbon ring, and more preferably a group in which three hydrogen atoms have been removed from the ring portion of a substituted or unsubstituted benzene ring.
[0026] Specific examples of the partial structure containing the partial structure (a1) contained in the polymer (P1) include the partial structures represented by each of the following formulas (1-1) to (1-11). [ka] (In formulas (1-1) to (1-11), "*" represents a bond.)
[0027] From the viewpoint of ease of introduction into the partial structure (a1), the polymer (P1) preferably contains a structural unit derived from a monomer having the partial structure (a1). The content ratio of the structural unit derived from the monomer having the partial structure (a1) in the polymer (P1) is preferably 0.5 mol% or more, more preferably 1 mol% or more, and even more preferably 2 mol% or more, based on the total amount of the structural units constituting the polymer (P1). In addition, the content ratio of the structural unit derived from the monomer having the partial structure (a1) is preferably 40 mol% or less, more preferably 30 mol% or less, and even more preferably 25 mol% or less, based on the total amount of the structural units constituting the polymer (P1).
[0028] ·Partial structure (a2) (Nitrogen-containing heterocyclic structure) The partial structure (a2) has a specific nitrogen-containing structure. Since the polymer (P1) has the specific nitrogen-containing structure, in a liquid crystal element having a liquid crystal alignment film formed by the first liquid crystal alignment agent, impurities originating from an insulating film, etc. are adsorbed by the liquid crystal alignment film and kept within the film, thereby enhancing the effect of suppressing the intrusion of impurities into the liquid crystal layer, and it is considered that this can further suppress the decrease in voltage holding ratio caused by the generation of impurities.
[0029] When the polymer (P1) has a nitrogen-containing heterocyclic structure as the partial structure (a2), the nitrogen-containing heterocyclic ring in the nitrogen-containing heterocyclic structure may be an aromatic heterocyclic ring or a non-aromatic heterocyclic ring. The nitrogen-containing heterocyclic ring may be a single ring or a condensed ring. Specific examples of these include nitrogen-containing aromatic heterocyclic rings such as pyrrole ring, imidazole ring, pyrazole ring, triazole ring, pyridine ring, pyrimidine ring, pyridazine ring, quinoline ring, benzimidazole ring, carbazole ring, and pyrazine ring, as well as heterocyclic rings having a substituent (e.g., methyl group, ethyl group, etc.) on these rings. Examples of nitrogen-containing non-aromatic heterocyclic rings include piperidine ring, piperazine ring, morpholine ring, and hexamethyleneimine ring, as well as heterocyclic rings having a substituent (e.g., methyl group, ethyl group, etc.) introduced on these rings. A pyridine ring, a benzimidazole ring, a carbazole ring, a piperidine ring or a piperazine ring is preferred.
[0030] The nitrogen-containing heterocycle of the partial structure (a2) is preferably at least one selected from the group consisting of a pyridine ring, a pyrimidine ring, a pyrazine ring, a piperidine ring, a piperazine ring, a quinoline ring, and a benzimidazole ring. The nitrogen-containing heterocycle is preferably a pyridine ring because it exhibits strong basicity.
[0031] When the polymer (P1) has a nitrogen-containing heterocyclic structure as the partial structure (a2), the polymer (P1) may have the nitrogen-containing heterocyclic structure in its main chain, in its side chain, or in both its main chain and its side chain.
[0032] Specific examples of the nitrogen-containing heterocyclic structure include partial structures represented by the following formulae (2a-1) to (2a-10), in which "Boc" represents a tert-butoxycarbonyl group (the same applies below). [ka] (In formulas (2a-1) to (2a-10), "*" represents a bond.)
[0033] (Partial structure represented by the above formula (2)) In the above formula (2), Y 1 is a hydrogen atom or a thermally detachable group. Examples of the thermally detachable group include a carbamate-based detachable group, an amide-based detachable group, an imide-based detachable group, and a sulfonamide-based detachable group. Among these, a carbamate-based detachable group is preferred because of its high thermal detachability. Specific examples thereof include a tert-butoxycarbonyl group, a benzyloxycarbonyl group, a 1,1-dimethyl-2-haloethyloxycarbonyl group, an allyloxycarbonyl group, a 2-(trimethylsilyl)ethoxycarbonyl group, and a 9-fluorenylmethyloxycarbonyl group (F-moc group). Among these, a tert-butoxycarbonyl group (Boc group) is particularly preferred because of its excellent thermal detachability and the reduced amount of the deprotected portion remaining in the film.
[0034] A 1 Or A 2 The alkanediyl group represented by the formula (I) may be linear or branched. 1 Or A 2 The alkanediyl group represented by the formula (I) is preferably linear. 1 Or A 2 The number of carbon atoms of the alkanediyl group represented by the formula (I) is, for example, 1 to 10. 1 Or A 2 The alkanediyl group represented by the following formula (I) preferably has 1 to 6 carbon atoms, more preferably has 1 to 4 carbon atoms, and further preferably has 1 or 2 carbon atoms.
[0035] A 1 When A is a substituted or unsubstituted divalent alicyclic group, examples of the alicyclic group include a cyclopentanediyl group, a cyclohexanediyl group, and groups in which a substituent has been introduced into these groups. 1 When A is a substituted or unsubstituted divalent aromatic ring group, the aromatic ring group is preferably a phenylene group, a pyridinediyl group, or a group in which a substituent has been introduced into these groups.1 When is a substituted divalent alicyclic or aromatic group, the substituents are 1 Or Ar 2 Examples of the substituent that the divalent aromatic ring group represented by the following formula (I) may have include the same groups as those exemplified above.
[0036] When the polymer (P1) has a partial structure represented by the above formula (2) as the partial structure (a2), the polymer (P1) may have the partial structure represented by the above formula (2) in the main chain, in the side chain, or in both the main chain and the side chain. In order to obtain a liquid crystal alignment film having excellent impurity resistance, it is preferable that the partial structure represented by the above formula (2) is introduced into the main chain of the polymer (P1).
[0037] When the polymer (P1) has a partial structure represented by the above formula (2), specific examples of the partial structure of the polymer (P1) include partial structures represented by each of the following formulae (2b-1) to (2b-7), in which "F-moc" represents a 9-fluorenylmethyloxycarbonyl group (hereinafter the same). [ka] (In formulas (2b-1) to (2b-7), "*" represents a bond.)
[0038] In addition, when the polymer (P1) has a partial structure represented by the above formula (2b-7), the polymer (P1) corresponds to a polymer having a nitrogen-containing heterocyclic structure as the partial structure (a2) and the partial structure represented by the above formula (2).
[0039] (Partial structure represented by the above formula (3)) In the above formula (3), Y 2 is a thermally detachable group. Y in the above formula (2) 1 Examples of the groups include the same groups as those exemplified in the explanation of 1. A tert-butoxycarbonyl group (Boc group) is preferred because it is easily removable by heat and can reduce the amount of the deprotected portion remaining in the film.
[0040] X 3 The alkanediyl group represented by the following formula (I) preferably has 1 to 6 carbon atoms, more preferably has 1 to 4 carbon atoms, and further preferably has 1 or 2 carbon atoms. 3 The alkanediyl group represented by X may be linear or branched, but is preferably linear. 3 Among these, a single bond or an alkanediyl group having 1 to 4 carbon atoms is preferable, and a single bond, a methylene group or an ethylene group is more preferable.
[0041] R 4 or R 5 Examples of the monovalent hydrocarbon group represented by the formula (I) include a chain hydrocarbon group having 1 to 10 carbon atoms, an alicyclic hydrocarbon group having 3 to 12 carbon atoms, and an aromatic hydrocarbon group having 6 to 12 carbon atoms. 4 and R 5 is preferably a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, and more preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms.
[0042] When the polymer (P1) has a partial structure represented by the above formula (3), specific examples of the partial structure that the polymer (P1) has include partial structures represented by each of the following formulas (2c-1) to (2c-8). [ka] (In formulas (2c-1) to (2c-8), "*" represents a bond.)
[0043] From the viewpoint of ease of introduction of the partial structure (a2) into the main chain, the polymer (P1) preferably contains a structural unit derived from a monomer having the partial structure (a2). The content ratio of the structural unit derived from the monomer having the partial structure (a2) in the polymer (P1) is preferably 0.5 mol % or more, more preferably 1 mol % or more, and even more preferably 2 mol % or more, based on the total amount of the structural units constituting the polymer (P1). The content ratio of the structural unit derived from the monomer having the partial structure (a2) is preferably 50 mol % or less, more preferably 45 mol % or less, and even more preferably 40 mol % or less, based on the total amount of the structural units constituting the polymer (P1).
[0044] The polymer (P1) contains the partial structure (a1) and the partial structure (a2) in the same molecule or in different molecules. Specific examples of the first liquid crystal aligning agent containing the polymer (P1) include the following examples 1 and 2. [Mode 1] A mode in which the polymer (P1) contains a polymer having the partial structure (a1) and the partial structure (a2) in the same molecule (hereinafter also referred to as "first polymer (P11)"). [Embodiment 2] An embodiment in which the polymer (P1) includes a polymer having a partial structure (a1) (hereinafter also referred to as a "second polymer (P12)") and a polymer having a partial structure (a2) and different from the second polymer (hereinafter also referred to as a "third polymer (P13)"). Among these, embodiment 1 is preferred in that a liquid crystal alignment film having excellent impurity resistance and seal adhesion can be obtained with as few components as possible, and a liquid crystal device having good transmittance can be obtained.
[0045] In addition, when the polymer (P1) is composed of multiple types of polymers, the ratio of the structural unit derived from the monomer having the partial structure (a1) in the polymer (P1) and the ratio of the structural unit derived from the monomer having the partial structure (a2) represent the total ratio of the multiple types of polymers. For example, when the first liquid crystal alignment agent contains the second polymer (P12) and the second polymer (P13) as the polymer (P1), the total of the ratio of the structural unit derived from the monomer having the partial structure (a1) in the second polymer (P12) and the ratio of the structural unit derived from the monomer having the partial structure (a1) in the third polymer (P13) is the ratio of the structural unit derived from the monomer having the partial structure (a1) in the polymer (P1).
[0046] The main skeleton of the polymer (P1) is not particularly limited. Examples of the main skeleton of the polymer (P1) include polyamic acid, polyamic acid ester, polyimide, polyamine, polyenamine, polyurea, polyorganosiloxane, polyester, polyamide, polyamideimide, polybenzoxazole precursor, polybenzoxazole, cellulose derivative, polyacetal, and addition polymer. The addition polymer is a polymer obtained by polymerizing (addition polymerization) a monomer having a polymerizable unsaturated carbon-carbon bond, and examples thereof include (meth)acrylic polymers, styrene polymers, maleimide polymers, and styrene-maleimide copolymers. The polyenamine is a polymer having a carbon-carbon double bond adjacent to the amino group of a polyamine, and examples thereof include polyenaminoketone, polyenaminoester, polyenaminonitrile, and polyenaminosulfonyl.
[0047] From the viewpoints of affinity with liquid crystal molecules, mechanical strength, liquid crystal alignment, and ease of introduction of the partial structure (a1) and the partial structure (a2), the polymer (P1) is preferably a polymer containing a structural unit derived from a diamine compound. Specific examples of such a polymer (P1) include polyamic acid, polyamic acid ester, polyimide, polyamide, polyenamine, polyamideimide, etc. Among them, the polymer (P1) is preferably at least one selected from the group consisting of polyamic acid, polyamic acid ester, and polyimide.
[0048] The method for producing the polyamic acid, polyamic acid ester, and polyimide as the polymer (P1) is not particularly limited, and they can be produced by appropriately combining standard methods in organic chemistry. Specific examples of the method for producing the polymer (P1) include: [I] a method of reacting a tetracarboxylic dianhydride with a diamine compound containing a diamine having a partial structure (a1) (hereinafter also referred to as a "first specific diamine") and a diamine having a partial structure (a2) (hereinafter also referred to as a "second specific diamine"); [II] a method of reacting a tetracarboxylic dianhydride having a partial structure (a1) (hereinafter also referred to as a "specific acid dianhydride") with a diamine compound containing a second specific diamine; a method of combining the method [I] and the method [II], etc. The details of the polyamic acid, polyamic acid ester, and polyimide as the polymer (P1) will be described below.
[0049] (Polyamic acid) Tetracarboxylic acid dianhydride Examples of the specific acid dianhydride that can be used in the synthesis of the polyamic acid (hereinafter also referred to as "polyamic acid (P1)") as the polymer (P1) include a tetracarboxylic acid dianhydride having a partial structure represented by the above formula (1-1) and a tetracarboxylic acid dianhydride having a partial structure represented by the above formula (1-2). Specific examples of the specific acid dianhydride include compounds represented by the following formulas (t1-1) to (t1-4). [ka]
[0050] In synthesizing the polyamic acid (P1), a tetracarboxylic dianhydride not having the partial structure (a1) (hereinafter also referred to as "other acid dianhydride") may be used alone or together with the specific acid dianhydride. Examples of the other acid dianhydride include aliphatic tetracarboxylic dianhydrides and aromatic tetracarboxylic dianhydrides. The aliphatic tetracarboxylic dianhydrides include linear tetracarboxylic dianhydrides and alicyclic tetracarboxylic dianhydrides.
[0051] Specific examples of the chain tetracarboxylic dianhydride include butane tetracarboxylic dianhydride, etc. Specific examples of the alicyclic tetracarboxylic dianhydride include 1,2,3,4-cyclobutane tetracarboxylic dianhydride, 1,3-dimethyl-1,2,3,4-cyclobutane tetracarboxylic dianhydride, 2,3,5-tricarboxycyclopentylacetic dianhydride, 5-(2,5-dioxotetrahydrofuran-3-yl)-3a,4,5,9b-tetrahydronaphtho[1,2-c]furan-1,3-dione, 5-(2,5-dioxotetrahydrofuran-3-yl)-8-methyl-3a,4,5,9b-tetrahydronaphtho[1,2-c]furan-1,3-dione, 3-oxabicyclo [3.2.1]octane-2,4-dione-6-spiro-3'-(tetrahydrofuran-2',5'-dione), 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, 3,5,6-tricarboxy-2-carboxymethylnorbornane-2:3,5:6-dianhydride, bicyclo[3.3.0]octane-2,4,6,8-tetracarboxylic acid 2:4,6:8-dianhydride, bicyclo[2.2.1]heptane-2,3,5,6-tetracarboxylic acid 2:3,5:6-dianhydride, 4,9-dioxatricyclo[5.3.1.0 2,6 ]undecane-3,5,8,10-tetraone, 1,2,4,5-cyclohexanetetracarboxylic dianhydride, bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride, ethylenediaminetetraacetic dianhydride, cyclopentanetetracarboxylic dianhydride, and the like.
[0052] Examples of aromatic tetracarboxylic dianhydrides include pyromellitic dianhydride, 4,4'-(hexafluoroisopropylidene)diphthalic anhydride, p-phenylene bis(trimellitic monoester anhydride), ethylene glycol bis(anhydrotrimellitate), 1,3-propylene glycol bis(anhydrotrimellitate), 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 4,4'-biphthalic dianhydride, etc. In addition to the above, tetracarboxylic dianhydrides described in JP-A-2010-97188 can be used as the tetracarboxylic dianhydride used in the synthesis of polyamic acid (P1).
[0053] When the organic film formed by the first liquid crystal alignment agent is given liquid crystal alignment ability by photo-alignment treatment, it is preferable to use a substituted cyclobutane tetracarboxylic dianhydride in the synthesis of the polymer (P1) in order to increase the photoreactivity of the organic film. Specific examples of the substituted cyclobutane tetracarboxylic dianhydride include the compounds represented by the following formulae (t2-1) to (t2-6). [ka]
[0054] When a specific acid dianhydride is used in the synthesis of polyamic acid (P1), the ratio of the specific acid dianhydride used is preferably 1 mol% or more, more preferably 2 mol% or more, and even more preferably 5 mol% or more, based on the total amount of tetracarboxylic dianhydride used in the synthesis of polyamic acid (P1). The ratio of the specific acid dianhydride used is preferably 50 mol% or less, more preferably 40 mol% or less, and even more preferably 30 mol% or less, based on the total amount of tetracarboxylic dianhydride used in the synthesis of polyamic acid (P1). Note that, for polyamic acid, polyamic acid ester, and polyimide, the blending ratio of monomers used in the synthesis of the polymer is the same as the ratio of monomer units constituting the resulting polymer.
[0055] When a substituted cyclobutane tetracarboxylic dianhydride is used in the synthesis of polyamic acid (P1), the proportion of the substituted cyclobutane tetracarboxylic dianhydride used in the synthesis of polyamic acid (P1) is preferably 10 mol % or more, more preferably 30 mol % or more, and even more preferably 50 mol % or more, based on the total amount of tetracarboxylic dianhydride used in the synthesis of polyamic acid (P1), from the viewpoint of sufficiently increasing the photoreactivity of the coating film.
[0056] Diamine Compounds As the first specific diamine that can be used in the synthesis of the polyamic acid (P1), a diamine having a partial structure represented by the above formula (1-1) can be preferably used. A preferred example of the first specific diamine is a compound represented by the following formula (D1). [ka] (In formula (D1), R 1 , R 2 , n1, n2, m1 and m2 are the same as those in formula (1). 1 , Ar 2 , X 1 and X 2 R has the same meaning as in formula (1-1) above. 6 and R 7 are each independently a single bond or a divalent aromatic ring group. 6 If is a single bond, X 1 is a single bond or an alkanediyl group having 1 to 10 carbon atoms, R 7 If is a single bond, X 2 is a single bond or an alkanediyl group having 1 to 10 carbon atoms.
[0057] Further specific examples of the first specific diamine include compounds represented by each of the following formulas (d1-1) to (d1-20). [ka] [ka]
[0058] The second specific diamine that can be used in the synthesis of the polyamic acid (P1) is preferably a compound having at least one selected from the group consisting of a nitrogen-containing heterocyclic structure, a partial structure represented by the above formula (2) and a partial structure represented by the above formula (3), and two primary diamines. Specific examples of the second specific diamine include the compounds represented by the following formulas (d2-1) to (d2-31). [ka] [ka]
[0059] In the synthesis of the polyamic acid (P1), a diamine having neither the partial structure (a1) nor the partial structure (a2) (hereinafter also referred to as "other diamines") may be used. As the other diamines, known diamines may be used, for example, aliphatic diamines, aromatic diamines, diaminoorganosiloxanes, etc. The aliphatic diamines include linear diamines and alicyclic diamines.
[0060] Specific examples of other diamines include chain diamines such as m-xylylenediamine, 1,3-propanediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, 1,3-bis(aminomethyl)cyclohexane, etc.; alicyclic diamines such as 1,4-diaminocyclohexane, 4,4'-methylenebis(cyclohexylamine), etc.; Examples of aromatic diamines include dodecanoxydiaminobenzene, tetradecanoxydiaminobenzene, pentadecanoxydiaminobenzene, hexadecananoxydiaminobenzene, octadecanoxydiaminobenzene, cholestanyloxydiaminobenzene, cholesteryloxydiaminobenzene, cholestanyl diaminobenzoate, cholesteryl diaminobenzoate, lanostannyl diaminobenzoate, 3,6-bis(4-aminobenzoyloxy)cholestane, 3,6-bis(4-aminophenoxy)cholestane, 1 ,1-bis(4-((aminophenyl)methyl)phenyl)-4-butylcyclohexane, 1,1-bis(4-((aminophenyl)methyl)phenyl)-4-heptylcyclohexane, 1,1-bis(4-((aminophenoxy)methyl)phenyl)-4-heptylcyclohexane, 1,1-bis(4-((aminophenyl)methyl)phenyl)-4-(4-heptylcyclohexyl)cyclohexane, N-(2,4-diaminophenyl)-4-(4-heptylcyclohexyl)benzamide, and the following formula (E-1): [ka] (In formula (E-1), X I and X II are each independently a single bond, -O-, *-COO-, or *-OCO- (wherein "*" represents a bond to the diaminophenyl group). I R is an alkanediyl group having 1 to 3 carbon atoms. II R is a single bond or an alkanediyl group having 1 to 3 carbon atoms. III is an alkyl group, an alkoxy group, a fluoroalkyl group or a fluoroalkoxy group having 1 to 20 carbon atoms. a is 0 or 1. b is an integer of 0 to 3. c is an integer of 0 to 2. d is 0 or 1, provided that 1≦a+b+c≦3. Directing group-containing diamines such as compounds represented by the formula: p-phenylenediamine, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylamine, 4,4'-diaminodiphenyl sulfide, 4-aminophenyl-4'-aminobenzoate, 4,4'-diaminoazobenzene, 1,2-bis(4-aminophenoxy)ethane, 1,2-bis(4-aminophenoxy)ethane, 1,3-bis(4-aminophenoxy)propane, 1,5-bis(4-aminophenoxy)pentane, 1,6-bis(4-aminophenoxy)hexane, 1,7-bis(4-aminophenoxy)heptane, bis[2-(4-aminophenyl)ethyl]hexanedioic acid, N,N-bis(4-aminophenyl)methylamine, 4,4'-(2,2'-oxybis(ethane-2,1-diyl)bis(oxy))dianiline, 1,5-diaminonaphthalene, 2,2'-dimethyl -4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 4,4'-diaminodiphenyl ether, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2-bis(4-aminophenyl)hexafluoropropane, 4,4'-(p-phenylenediisopropylidene)bisaniline, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, N,N'-bis(4-aminophenyl)-benzidine, N,N'-bis(4-aminophenyl)-N,N'-dimethylbenzidine, 3,5-diaminobenzoic acid, 1-(4-aminophenoxy)-2-(4-(4'-aminophenyl)phenoxy)ethane, etc.; Examples of diaminoorganosiloxanes include 1,3-bis(3-aminopropyl)-tetramethyldisiloxane, and the like. In addition, the diamines described in JP-A-2010-97188 can also be used.
[0061] In the above formula (E-1), "-X I -(R I -X II ) dThe divalent group represented by "-" is preferably an alkanediyl group having 1 to 3 carbon atoms, *-O-, *-COO-, or *-O-C2H4-O- (wherein the bond marked with "*" is bonded to a diaminophenyl group). III The two amino groups in the diaminophenyl group are preferably in the 2,4- or 3,5-position relative to the other group.
[0062] Specific examples of the compound represented by formula (E-1) above include the compounds represented by formulas (E-1-1) to (E-1-4) below. [ka]
[0063] When the first specific diamine is used in the synthesis of the polyamic acid (P1), the proportion of the first specific diamine used is preferably 1 mol% or more, more preferably 2 mol% or more, and even more preferably 5 mol% or more, based on the total amount of the diamine compounds used in the synthesis of the polyamic acid (P1). By setting the proportion of the first specific diamine used in the above range, it is preferable that a liquid crystal alignment film having an excellent balance of impurity resistance, mechanical strength, and transmittance can be obtained. In addition, the proportion of the first specific diamine used is preferably 50 mol% or less, more preferably 40 mol% or less, based on the total amount of the diamine compounds used in the synthesis of the polyamic acid (P1), from the viewpoint of obtaining a liquid crystal alignment film having better impurity resistance by using the second specific diamine and from the viewpoint of the solubility of the polymer.
[0064] When the second specific diamine is used in the synthesis of the polyamic acid (P1), the proportion of the second specific diamine used is preferably 1 mol% or more, more preferably 2 mol% or more, and even more preferably 5 mol% or more, based on the total amount of the diamine compounds used in the synthesis of the polyamic acid (P1). By setting the proportion of the second specific diamine used in the above range, it is preferable that a liquid crystal alignment film having excellent impurity resistance can be obtained. In addition, the proportion of the second specific diamine used is preferably 90 mol% or less, more preferably 85 mol% or less, based on the total amount of the diamine compounds used in the synthesis of the polyamic acid (P1).
[0065] Synthesis of polyamic acid The polyamic acid (P1) can be obtained by reacting the above-mentioned tetracarboxylic dianhydride with a diamine compound, optionally together with a molecular weight modifier. The ratio of the tetracarboxylic dianhydride and the diamine compound used in the synthesis reaction of the polyamic acid (P1) is preferably such that the acid anhydride group of the tetracarboxylic dianhydride is 0.2 to 2 equivalents, more preferably 0.3 to 1.2 equivalents, per equivalent of the amino group of the diamine compound.
[0066] Examples of the molecular weight regulator include acid monoanhydrides such as maleic anhydride, phthalic anhydride, and itaconic anhydride, monoamine compounds such as aniline, cyclohexylamine, and n-butylamine, and monoisocyanate compounds such as phenyl isocyanate and naphthyl isocyanate. The proportion of the molecular weight regulator used is preferably 20 parts by mass or less, and more preferably 10 parts by mass or less, relative to 100 parts by mass of the total of the tetracarboxylic dianhydride and diamine compounds used.
[0067] The synthesis reaction of the polyamic acid (P1) is preferably carried out in an organic solvent. The reaction temperature is preferably from −20° C. to 150° C., more preferably from 0 to 100° C. The reaction time is preferably from 0.1 to 24 hours, more preferably from 0.5 to 12 hours.
[0068] Examples of organic solvents used in the reaction include aprotic polar solvents, phenolic solvents, alcohols, ketones, esters, ethers, halogenated hydrocarbons, and hydrocarbons. Of these organic solvents, it is preferable to use one or more selected from the group consisting of aprotic polar solvents and phenolic solvents (organic solvents of group 1), or a mixture of one or more selected from the organic solvents of group 1 and one or more selected from the group consisting of alcohols, ketones, esters, ethers, halogenated hydrocarbons, and hydrocarbons (organic solvents of group 2). In the latter case, the proportion of the organic solvents of group 2 used is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less, based on the total amount of the organic solvents of group 1 and group 2.
[0069] Particularly preferred organic solvents are one or more selected from the group consisting of N-methyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, dimethylsulfoxide, γ-butyrolactone, tetramethylurea, hexamethylphosphortriamide, m-cresol, xylenol and halogenated phenols, or a mixture of one or more of these with other organic solvents in the above ratio range. The amount (x) of the organic solvent used is preferably an amount such that the total amount (y) of the tetracarboxylic dianhydride and the diamine compound is 0.1 to 50 mass% relative to the total amount (x+y) of the reaction solution.
[0070] In this manner, a reaction solution in which the polyamic acid (P1) is dissolved is obtained. This reaction solution may be used as it is for the preparation of a liquid crystal alignment agent, or the polyamic acid (P1) contained in the reaction solution may be isolated and then used for the preparation of a liquid crystal alignment agent, or the isolated polyamic acid (P1) may be purified and then used for the preparation of a liquid crystal alignment agent. When the polyamic acid (P) is dehydrated and cyclized to form a polyimide, the reaction solution may be used as it is for the dehydration and cyclization reaction, or the polyamic acid (P) contained in the reaction solution may be isolated and then used for the dehydration and cyclization reaction, or the isolated polyamic acid (P) may be purified and then used for the dehydration and cyclization reaction. The isolation and purification of the polyamic acid (P) can be carried out according to a known method.
[0071] (Polyamic acid ester) The polyamic acid ester as the polymer (P1) can be obtained, for example, by a method such as [I] reacting the polyamic acid (P1) obtained by the above synthesis reaction with an esterifying agent, [II] reacting a tetracarboxylic acid diester with a diamine compound, or [III] reacting a tetracarboxylic acid diester dihalide with a diamine compound.
[0072] In this specification, the term "tetracarboxylic acid diester" refers to a compound in which two of the four carboxy groups in a tetracarboxylic acid are esterified and the remaining two are carboxy groups. The term "tetracarboxylic acid diester dihalide" refers to a compound in which two of the four carboxy groups in a tetracarboxylic acid are esterified and the remaining two are halogenated.
[0073] Examples of the esterification agent used in the method [I] include hydroxyl group-containing compounds, acetal compounds, halides, epoxy group-containing compounds, etc. Specific examples of these include hydroxyl group-containing compounds such as alcohols, such as methanol, ethanol, and propanol, and phenols, such as phenol and cresol; acetal compounds such as N,N-dimethylformamide diethyl acetal and N,N-diethylformamide diethyl acetal; halides such as methyl bromide, ethyl bromide, stearyl bromide, methyl chloride, stearyl chloride, and 1,1,1-trifluoro-2-iodoethane; and epoxy group-containing compounds such as propylene oxide.
[0074] The tetracarboxylic acid diester used in the method [II] can be obtained, for example, by ring-opening the tetracarboxylic acid dianhydride exemplified in the explanation of the synthesis of the polyamic acid (P1) with an alcohol such as methanol, ethanol, etc. The tetracarboxylic acid derivative used in the method [II] may be only a tetracarboxylic acid diester, or may be used in combination with a tetracarboxylic acid dianhydride.
[0075] The reaction of the method [III] is preferably carried out in an organic solvent in the presence of a suitable dehydration catalyst. Examples of the organic solvent include those exemplified as those used in the synthesis of the polyamic acid (P1). Examples of the dehydration catalyst include 4-(4,6-dimethoxy-1,3,5-triazin-2-yl)-4-methylmorpholinium halide, carbonylimidazole, and phosphorus-based condensing agents. The reaction temperature is preferably -20 to 150°C, more preferably 0 to 100°C. The reaction time is preferably 0.1 to 24 hours, more preferably 0.5 to 12 hours.
[0076] The tetracarboxylic acid diester dihalide used in the method [III] can be obtained, for example, by reacting the tetracarboxylic acid diester obtained as described above with a suitable chlorinating agent such as thionyl chloride. The tetracarboxylic acid derivative used in the method [III] may be only the tetracarboxylic acid diester dihalide, or may be used in combination with a tetracarboxylic acid dianhydride.
[0077] The reaction in the method [III] is preferably carried out in an organic solvent in the presence of a suitable base. Examples of the organic solvent include those exemplified as those used in the synthesis of the polyamic acid (P1). Examples of the base that can be preferably used include tertiary amines such as pyridine and triethylamine; and alkali metals such as sodium hydride, potassium hydride, sodium hydroxide, potassium hydroxide, sodium, and potassium. The reaction temperature is preferably -20 to 150°C, more preferably 0 to 100°C. The reaction time is preferably 0.1 to 24 hours, more preferably 0.5 to 12 hours.
[0078] The polyamic acid ester contained in the liquid crystal aligning agent may have only an amic acid ester structure, or may be a partially esterified product in which an amic acid structure and an amic acid ester structure coexist. The reaction solution in which the polyamic acid ester is dissolved may be used for preparing the liquid crystal aligning agent as it is, or the polyamic acid ester contained in the reaction solution may be isolated and then used for preparing the liquid crystal aligning agent, or the isolated polyamic acid ester may be purified and then used for preparing the liquid crystal aligning agent. The isolation and purification of the polyamic acid ester may be performed according to a known method.
[0079] (Polyimide) The polyimide as the polymer (P1) can be obtained, for example, by subjecting the polyamic acid (P1) synthesized as described above to dehydration ring closure to form an imidized product.
[0080] The polyimide may be a complete imidation product in which all amic acid structures of the polyamic acid precursor are dehydrated and cyclically closed, or a partial imidation product in which only a part of the amic acid structures are dehydrated and cyclically closed, so that amic acid structures and imide ring structures coexist. The polyimide used in the reaction preferably has an imidization rate of 20% or more, more preferably 30 to 99%. This imidization rate is the ratio of the number of imide ring structures to the total number of amic acid structures and imide ring structures of the polyimide, expressed as a percentage. Here, some of the imide rings may be isoimide rings.
[0081] The dehydration and ring-closing of the polyamic acid is preferably carried out by heating the polyamic acid, or by dissolving the polyamic acid in an organic solvent, adding a dehydrating agent and a dehydration and ring-closing catalyst to the solution, and heating as necessary.
[0082] In the method of adding a dehydrating agent and a dehydration ring-closing catalyst to a solution of a polyamic acid, for example, an acid anhydride such as acetic anhydride, propionic anhydride, or trifluoroacetic anhydride can be used as the dehydrating agent. The amount of the dehydrating agent used is preferably 0.01 to 20 moles per mole of the amic acid structure of the polyamic acid. The amount of the dehydration ring-closing catalyst used is preferably 0.01 to 10 moles per mole of the dehydrating agent used. Examples of the organic solvent used in the dehydration ring-closing reaction include the organic solvents exemplified as those used in the synthesis of polyamic acid. The reaction temperature of the dehydration ring-closing reaction is preferably 0 to 180°C, more preferably 10 to 150°C. The reaction time is preferably 1.0 to 120 hours, more preferably 2.0 to 30 hours.
[0083] In this way, a reaction solution containing polyimide is obtained. This reaction solution may be used as it is for the preparation of a liquid crystal alignment agent, or may be used for the preparation of a liquid crystal alignment agent after removing the dehydrating agent and the dehydration ring-closing catalyst from the reaction solution, or may be used for the preparation of a liquid crystal alignment agent after isolating the polyimide, or may be used for the preparation of a liquid crystal alignment agent after purifying the isolated polyimide. These purification operations can be performed according to a known method. In addition, polyimide can also be obtained by imidizing a polyamic acid ester.
[0084] The polyamic acid, polyamic acid ester, and polyimide thus obtained as polymer (P1) preferably have a solution viscosity of 20 to 1,800 mPa·s, and more preferably 50 to 1,500 mPa·s, when made into a 15% by mass solution. The solution viscosity (mPa·s) of the polymer is a value measured at 25°C using an E-type rotational viscometer for a 15% by mass polymer solution prepared using a good solvent for the polymer (e.g., γ-butyrolactone, N-methyl-2-pyrrolidone, etc.).
[0085] The polystyrene-equivalent weight average molecular weight (Mw) of the polyamic acid, polyamic acid ester, and polyimide as the polymer (P1), measured by gel permeation chromatography (GPC), is preferably 1,000 to 500,000, and more preferably 2,000 to 300,000. The molecular weight distribution (Mw / Mn) of the polyamic acid, polyamic acid ester, and polyimide as the polymer (P1), expressed as the ratio of Mw to the polystyrene-equivalent number average molecular weight (Mn) measured by GPC, is preferably 8 or less, and more preferably 7 or less. When the Mw and Mw / Mn of the polyamic acid, polyamic acid ester, and polyimide as the polymer (P1) are within the above ranges, good liquid crystal alignment properties of the liquid crystal element can be ensured.
[0086] The content of the polymer (P1) in the first liquid crystal alignment agent is preferably 40 mass% or more, more preferably 50 mass% or more, and even more preferably 60 mass% or more, based on the total amount of solids contained in the liquid crystal alignment agent (i.e., the total mass of components other than the solvent of the liquid crystal alignment agent).
[0087] <Other ingredients> The first liquid crystal alignment agent may further contain components other than the polymer (P1) (hereinafter, also referred to as "other components"). Examples of the other components include a polymer different from the polymer (P) (hereinafter, also referred to as "polymer (Q)"), a crosslinking agent, a solvent, etc.
[0088] Polymer (Q) The polymer (Q) is a polymer having neither the partial structure (a1) nor the partial structure (a2). The main skeleton of the polymer (Q) is not particularly limited. Examples of the polymer (Q) include polyamic acid, polyamic acid ester, polyimide, polyorganosiloxane, polyester, polyenamine, polyurea, polyamide, polyamideimide, polybenzoxazole precursor, polybenzoxazole, cellulose derivative, polyacetal, and addition polymer. Among these, the polymer (Q) is preferably at least one selected from the group consisting of polyamic acid, polyamic acid ester, polyimide, polyorganosiloxane, and addition polymer, in that it shows good liquid crystal alignment property when used in combination with the polymer (P1).
[0089] When the polymer (Q) is contained in the liquid crystal alignment agent, the content of the polymer (Q) is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 5% by mass or more, based on the total amount of the polymer (P1) and the polymer (Q). The content of the polymer (Q) is preferably 95% by mass or less, more preferably 80% by mass or less, based on the total amount of the polymer (P1) and the polymer (Q).
[0090] Crosslinking agent The first liquid crystal alignment agent contains -OE 1 (wherein E 1is a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a monovalent leaving group.), a mercapto group, a protected mercapto group, an amino group, a protected amino group, an oxiranyl group, an oxetanyl group, -Si(OR 11 ) r (R 12 ) 3-r (wherein R 11 and R 12 are each independently a monovalent hydrocarbon group having 1 to 10 carbon atoms, r is an integer of 1 to 3, and when r is 2 or 3, multiple R 11 are the same or different, and when r is 1, multiple R 12 are the same or different.) and a compound having at least one group selected from the group consisting of a polymerizable carbon-carbon double bond group (hereinafter also referred to as "crosslinkable group F1") (hereinafter also referred to as "compound (A)"). It is considered that the film density of the liquid crystal alignment film can be increased by using the polymer (P1) and compound (A) in combination. This further improves the resistance to impurities derived from panel components and the like, and also improves the mechanical strength of the liquid crystal alignment film, thereby making it possible to obtain a liquid crystal alignment film with excellent seal adhesion.
[0091] -OE 1 In the group represented by the formula: 1 The monovalent leaving group represented by the following formula is preferably a group which is released by heat or light and is replaced with a hydrogen atom. 1 Specific examples of the leaving group represented by the formula (I) include ether-based leaving groups such as alkyl groups having 7 or less carbon atoms, benzyl groups, and p-methoxybenzyl groups; acetal-based leaving groups such as methoxymethyl groups, ethoxyethyl groups, and 2-tetrahydropyranyl groups; acyl-based leaving groups such as acetyl groups and benzoyl groups; allyl-based leaving groups such as allyl groups and methallyl groups; and silyl ether-based leaving groups such as trimethylsilyl groups, triethylsilyl groups, and tert-butyldimethylsilyl groups. From the viewpoint of achieving both ease of removal and storage stability, E 1Of these, the leaving group represented by the formula (I) is preferably an ether-based leaving group, an acetal-based leaving group, or an acetyl group, more preferably an alkyl group having 4 to 7 carbon atoms, a 2-tetrahydropyranyl group, a methoxymethyl group, a 1-ethoxyethyl, or an acetyl group, and still more preferably a 2-tetrahydropyranyl group, a methoxymethyl group, a 1-ethoxyethyl, or an acetyl group.
[0092] E 1 From the viewpoint of improving the seal adhesion, among the above, a hydrogen atom, an alkyl group having 7 or less carbon atoms, an acetyl group, a 2-tetrahydropyranyl group, a methoxymethyl group, or a 1-ethoxyethyl group is particularly preferred. In addition, -OE is particularly preferred because it has a high reactivity with the polymer (P) (particularly the fluorene ring site in the partial structure (a1)). 1 The group represented by the following formula (I) is preferably bonded to a carbon atom, more preferably bonded to an alkanediyl group, and even more preferably is a group constituting a part of a methylol group or a hydroxyalkylamide group.
[0093] In the protected amino group, the leaving group bonded to the nitrogen atom is, for example, Y 1 In the case where E is a thermally detachable group, specific examples and preferred examples thereof include the same groups as those in the case where E is a thermally detachable group. In the case of a protected mercapto group, examples of the detachable group bonded to a sulfur atom include E 1 Examples of the groups include the same groups as those exemplified as the groups.
[0094] When the crosslinkable group F1 of the compound (A) is an amino group or a protected amino group, the compound (A) is preferably a chain compound. When the compound (A) has a group in which a primary amino group is protected as a protected amino group, the protected amino group may be a group in which only one of the two hydrogen atoms in the primary amino group is replaced with a leaving group, or may be a group in which both of the two hydrogen atoms are replaced with a leaving group. In other words, when at least one of the two hydrogen atoms in the primary amino group is replaced with a leaving group, the group corresponds to a "protected primary amino group".
[0095] -Si(OR 11 ) r (R 12 ) 3-r For the group represented by R 11 or R 12 Examples of the monovalent hydrocarbon group having 1 to 10 carbon atoms represented by the formula (I) include a monovalent chain hydrocarbon group having 1 to 10 carbon atoms, a monovalent alicyclic hydrocarbon group having 3 to 10 carbon atoms, and a monovalent aromatic hydrocarbon group having 6 to 10 carbon atoms. 11 R is preferably an alkyl group having 1 to 10 carbon atoms, more preferably an alkyl group having 1 to 3 carbon atoms, and further preferably a methyl group or an ethyl group. 12 is preferably an alkyl group having 1 to 10 carbon atoms or a substituted or unsubstituted phenyl group, and more preferably a methyl group, an ethyl group or a phenyl group. From the viewpoint of increasing the crosslinking reactivity, r is preferably 2 or 3, and more preferably 3.
[0096] When compound (A) has a polymerizable carbon-carbon double bond group, the polymerizable carbon-carbon double bond group preferably constitutes a part of a group represented by any one of the following formulae (g1-1) to (g1-10), in that a liquid crystal alignment film having high crosslinking reactivity and excellent electrical properties and seal adhesion can be obtained. [ka] (In formulas (g1-1) to (g1-10), "*" represents a bond.)
[0097] When compound (A) has a polymerizable carbon-carbon double bond group, compound (A) preferably has a group represented by any one of the above formulas (g1-1) to (g1-7), and from the standpoints of high crosslinking reactivity and ease of introduction of a functional group, it is more preferable that compound (A) has a group represented by any one of the above formulas (g1-1) to (g1-4).
[0098] The number of crosslinkable groups F1 in the compound (A) is not particularly limited. From the viewpoint of increasing the crosslinking reactivity between the polymer (P1) and the compound (A) and obtaining a liquid crystal alignment film with higher film density, the number of crosslinkable groups in one molecule of the compound (A) is preferably 2 or more, more preferably 2 to 10. The compound (A) is preferably a compound different from a polymer (i.e., a low molecular weight compound). The molecular weight of the compound (A) is, for example, 1,200 or less, preferably 1,000 or less, more preferably 800 or less.
[0099] Specific examples of the compound (A) include -OE 1 Examples of the compound having a group represented by the formula (5A-1) to (5A-36) include compounds represented by the formula (5A-1) to (5A-36) below: As the compound having a mercapto group or a protected mercapto group, the compounds represented by each of the following formulae (5B-1) to (5B-6) are mentioned; As the compound having an amino group or a protected amino group, the compounds represented by each of the following formulae (5C-1) to (5C-13) and the like are included: Examples of compounds having an oxiranyl group or an oxetanyl group include ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, tripropylene glycol diglycidyl ether, triglycidyl isocyanurate, 1,6-hexanediol diglycidyl ether, trimethylolpropane triglycidyl ether, 2,2-dibromoneopentyl glycol diglycidyl ether, N,N,N',N'-tetraglycidyl-m-xylylenediamine, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, N,N,N',N'-tetraglycidyl-4,4'-diaminodiphenylmethane, N,N-diglycidyl-benzylamine, N,N-diglycidyl-aminomethylcyclohexane, N,N-diglycidyl-cyclohexylamine, and epoxidation products of pentaerythritol tetraallyl ether with hydrogen peroxide; -Si(OR 11 ) r (R 12 ) 3-rExamples of compounds having a group represented by the formula (I) include 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, 3-(meth)acryloxypropylmethyldiethoxysilane, and vinyltriethoxysilane; Examples of the compound having a polymerizable carbon-carbon double bond group include ethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, pentaerythritol tri(meth)acrylate, and compounds represented by the following formulas (5D-1) to (5D-7). [ka] [ka] [ka] [ka] [ka] [ka]
[0100] From the viewpoint of crosslinking reactivity with the polymer (P1), the compound (A) is preferably -OE 1 and at least one selected from the group consisting of a compound having a group represented by the formula: 1 More preferred is at least one selected from the group consisting of a compound having a group represented by the following formula:
[0101] When the first liquid crystal alignment agent contains the compound (A), the content is preferably 0.5 parts by mass or more relative to 100 parts by mass of the total amount of the polymer components contained in the liquid crystal alignment agent (i.e., the total amount of the polymer (P1) and the polymer (Q)) from the viewpoint of increasing the film density of the liquid crystal alignment film. The content of the compound (A) is more preferably 1 part by mass or more, and even more preferably 5 parts by mass or more, relative to 100 parts by mass of the total amount of the polymer components. In addition, from the viewpoint of obtaining a liquid crystal element having good liquid crystal alignment properties and electrical properties, and from the viewpoint of improving the storage stability of the liquid crystal alignment agent, the content of the compound (A) is preferably 30 parts by mass or less, and more preferably 20 parts by mass or less, relative to 100 parts by mass of the total amount of the polymer components.
[0102] The first liquid crystal alignment agent may contain a crosslinking agent different from the compound (A). In addition to the above, other components than the solvent to be contained in the first liquid crystal alignment agent include, for example, antioxidants, metal chelate compounds, curing accelerators, surfactants, fillers, dispersants, photosensitizers, acid generators, base generators, and radical generators. The mixing ratio of these can be appropriately selected according to each compound within a range that does not impair the effects of the present disclosure.
[0103] ·solvent The first liquid crystal aligning agent is prepared as a liquid composition in which the polymer (P1) and components used as necessary are dispersed or dissolved preferably in a suitable solvent.
[0104] Examples of the organic solvent to be used include N-methyl-2-pyrrolidone, γ-butyrolactone, γ-butyrolactam, N,N-dimethylformamide, N,N-dimethylacetamide, 4-hydroxy-4-methyl-2-pentanone, ethylene glycol monomethyl ether, butyl lactate, butyl acetate, methyl methoxypropionate, ethyl ethoxypropionate, ethylene glycol methyl ether, ethylene glycol ethyl ether, ethylene glycol-n-propyl ether, ethylene glycol-i-propyl ether, and ethylene glycol-n-butyl ether ( butyl cellosolve), ethylene glycol dimethyl ether, ethylene glycol ethyl ether acetate, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diisobutyl ketone, isoamyl propionate, isoamyl isobutyrate, diisopentyl ether, ethylene carbonate, propylene carbonate, etc. These can be used alone or in combination of two or more.
[0105] The solid content concentration in the liquid crystal alignment agent (the ratio of the total mass of the components other than the solvent of the liquid crystal alignment agent to the total mass of the liquid crystal alignment agent) is appropriately selected in consideration of viscosity, volatility, etc., and is preferably in the range of 1 to 10 mass %. That is, the liquid crystal alignment agent is applied to the surface of a substrate as described below, and preferably heated to form a coating film that is a liquid crystal alignment film or a coating film that will become a liquid crystal alignment film. In this case, when the solid content concentration is 1 mass % or more, the thickness of the coating film can be sufficiently ensured, and a good liquid crystal alignment film tends to be easily obtained. When the solid content concentration is 10 mass % or less, the thickness of the coating film does not become too large, and an increase in the viscosity of the liquid crystal alignment agent can be suppressed, and the coating property tends to be good.
[0106] A particularly preferred range of solid content varies depending on the application of the liquid crystal alignment agent and the method used for applying the liquid crystal alignment agent to a substrate. For example, when applying a liquid crystal alignment agent for a liquid crystal display element to a substrate by a spinner method, it is particularly preferred that the solid content (the ratio of the total mass of all components other than the solvent in the liquid crystal alignment agent to the total mass of the liquid crystal alignment agent) is in the range of 1.5 to 4.5 mass%. When applying by a printing method, it is particularly preferred that the solid content is in the range of 3 to 9 mass%, thereby making the solution viscosity in the range of 12 to 50 mPa·s. When applying by an inkjet method, it is particularly preferred that the solid content is in the range of 1 to 5 mass%, thereby making the solution viscosity in the range of 3 to 15 mPa·s. The temperature when preparing the liquid crystal alignment agent is preferably 10 to 50°C, more preferably 20 to 30°C. In addition, with regard to the liquid crystal alignment agent for the retardation film, from the viewpoint of the applicability of the liquid crystal alignment agent and the thickness of the coating film to be formed being appropriate, the solid content concentration of the liquid crystal alignment agent is preferably in the range of 0.2 to 10 mass %, and more preferably in the range of 3 to 10 mass %.
[0107] [Second Liquid Crystal Alignment Agent] Next, the second liquid crystal alignment agent will be described. Note that the description of the second liquid crystal alignment agent that has the same configuration as the first liquid crystal alignment agent will be omitted. The second liquid crystal alignment agent contains a polymer (P2) and a compound (A1).
[0108] <Polymer (P2)> The polymer (P2) is a polymer having the partial structure (a1) represented by the above formula (1). That is, the polymer (P2) corresponds to the second polymer (P12) that may be contained in the first liquid crystal alignment agent. The explanation of the polymer (P1) can be cited for specific examples and preferred examples of the partial structure (a1) contained in the polymer (P2), the content ratio in the polymer, other structural units that the polymer (P2) may have, and synthesis methods.
[0109] <Compound (A1)> Compound (A1) is -OE 1 (wherein E 1is a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a monovalent leaving group.), a mercapto group, a protected mercapto group, an amino group, a protected amino group, an oxetanyl group, -Si(OR 11 ) r (R 12 ) 3-r and polymerizable carbon-carbon double bond groups (hereinafter also referred to as "crosslinkable group F2"). 1 a protected mercapto group, a protected amino group, -Si(OR 11 ) r (R 12 ) 3-r For specific examples and preferred examples of the group represented by the following formula (I) and the polymerizable carbon-carbon double bond group, the explanation of the crosslinkable group F1 contained in the compound (A) can be cited.
[0110] The number of crosslinkable groups F2 in the compound (A1) is 2 or more, more preferably 2 to 10, from the viewpoint of increasing the crosslinking reactivity between the polymer (P2) and the compound (A1) and obtaining a liquid crystal alignment film with higher film density. The compound (A1) is preferably a compound different from a polymer (i.e., a low molecular weight compound). The molecular weight of the compound (A1) is, for example, 1,200 or less, preferably 1,000 or less, more preferably 800 or less.
[0111] Specific examples of the compound (A1) include compounds having a corresponding crosslinkable group among the compounds shown as the compounds (A) that may be blended in the first liquid crystal alignment agent.
[0112] From the viewpoint of crosslinking reactivity with the polymer (P2), the compound (A1) is preferably -OE 1 and at least one selected from the group consisting of a compound having a group represented by the formula: 1 More preferred is at least one selected from the group consisting of a compound having a group represented by the following formula:
[0113] The content ratio of the compound (A1) in the second liquid crystal alignment agent is preferably 0.5 parts by mass or more relative to 100 parts by mass of the total amount of the polymer components contained in the liquid crystal alignment agent (i.e., the total amount of the polymer (P2) and the polymer (Q) that is optionally blended) from the viewpoint of increasing the film density of the liquid crystal alignment film. The content ratio of the compound (A1) is more preferably 1 part by mass or more, and even more preferably 5 parts by mass or more, relative to 100 parts by mass of the total amount of the polymer components. In addition, from the viewpoint of obtaining a liquid crystal element having good liquid crystal alignment properties and electrical properties, and from the viewpoint of improving the storage stability of the liquid crystal alignment agent, the content ratio of the compound (A1) is preferably 30 parts by mass or less, and more preferably 20 parts by mass or less, relative to 100 parts by mass of the total amount of the polymer components.
[0114] The second liquid crystal aligning agent may further contain a component different from the polymer (P2) and the compound (A1). Other components that may be blended in the second liquid crystal aligning agent include the same components as those exemplified as other components in the description of the first liquid crystal aligning agent. In addition, the description of the first liquid crystal aligning agent is used for the preparation method, viscosity, etc. of the second liquid crystal aligning agent.
[0115] <Liquid crystal alignment film and liquid crystal element> The liquid crystal alignment film of the present disclosure is formed by the liquid crystal alignment agent prepared as described above. The liquid crystal element of the present disclosure includes a liquid crystal alignment film formed by using the liquid crystal alignment agent described above. The operation mode of the liquid crystal in the liquid crystal element is not particularly limited, and can be applied to various modes such as TN (Twisted Nematic) type, STN (Super Twisted Nematic) type, VA (Vertical Alignment) type (including VA-MVA type, VA-PVA type, etc.), IPS (In-Plane Switching) type, FFS (Fringe Field Switching) type, OCB (Optically Compensated Bend) type, and PSA (Polymer Sustained Alignment) type. The liquid crystal element can be manufactured by a method including, for example, the following steps 1 to 3. In step 1, the substrate used differs depending on the desired operation mode. Steps 2 and 3 are common to each operation mode.
[0116] (Step 1: Formation of coating film) First, a liquid crystal alignment agent is applied onto a substrate, and the applied surface is preferably heated to form a coating film on the substrate. As the substrate, for example, a transparent substrate made of glass such as float glass or soda glass, or plastic such as polyethylene terephthalate, polybutylene terephthalate, polyethersulfone, polycarbonate, or poly(alicyclic olefin) can be used. The transparent conductive film provided on one side of the substrate may be a NESA film (registered trademark of PPG, USA) made of tin oxide (SnO2), an ITO film made of indium oxide-tin oxide (In2O3-SnO2), or the like. When manufacturing a TN-type, STN-type, VA-type, or PSA-type liquid crystal element, two substrates each having a patterned transparent conductive film are used. On the other hand, when manufacturing an IPS-type or FFS-type liquid crystal element, a substrate having an electrode made of a transparent conductive film or metal film patterned into a comb shape and an opposing substrate having no electrode are used. The metal film may be, for example, a film made of a metal such as chromium. The liquid crystal alignment agent is preferably applied to the substrate on the electrode-forming surface by offset printing, spin coating, roll coating, or inkjet printing.
[0117] After the liquid crystal alignment agent is applied, preheating (prebaking) is preferably performed for the purpose of preventing dripping of the applied liquid crystal alignment agent. The prebaking temperature is preferably 30 to 200°C, and the prebaking time is preferably 0.25 to 10 minutes. Thereafter, if necessary, a baking (postbaking) step is performed for the purpose of completely removing the solvent or thermally imidizing the amic acid structure present in the polymer. The baking temperature (postbaking temperature) at this time is preferably 80 to 300°C, and the postbaking time is preferably 5 to 200 minutes. The film thickness of the film thus formed is preferably 0.001 to 1 μm. After the liquid crystal alignment agent is applied on the substrate, the organic solvent is removed to form a liquid crystal alignment film or a coating film that will become a liquid crystal alignment film.
[0118] (Step 2: Orientation Treatment) When a TN-type, STN-type, IPS-type or FFS-type liquid crystal element is manufactured, a treatment (alignment treatment) is carried out to impart liquid crystal alignment ability to the coating film formed in step 1. This imparts the alignment ability of liquid crystal molecules to the coating film, forming a liquid crystal alignment film. Examples of the alignment treatment include a rubbing treatment in which the surface of the coating film formed on the substrate is rubbed with cotton or the like, and a photo-alignment treatment in which the coating film is irradiated with light to impart liquid crystal alignment ability. On the other hand, when a vertical alignment type (VA type) liquid crystal element is manufactured, the coating film formed in step 1 can be used as it is as a liquid crystal alignment film, but the coating film may also be subjected to an alignment treatment. A liquid crystal alignment film suitable for a vertical alignment type liquid crystal element can also be preferably used for a PSA type liquid crystal element.
[0119] The light irradiation in the photo-alignment treatment can be performed by a method of irradiating the coating film after the post-bake step, a method of irradiating the coating film after the pre-bake step but before the post-bake step, or a method of irradiating the coating film during heating in at least one of the pre-bake step and the post-bake step. In the photo-alignment treatment, the radiation to be irradiated to the coating film can be, for example, ultraviolet light and visible light containing light with a wavelength of 150 to 800 nm. Preferably, ultraviolet light containing light with a wavelength of 200 to 400 nm. When the radiation is polarized, it may be linearly polarized or partially polarized. In addition, when the radiation used is linearly polarized or partially polarized, the radiation may be performed from a direction perpendicular to the substrate surface, from an oblique direction, or a combination of these. When non-polarized radiation is irradiated, the direction of irradiation is an oblique direction.
[0120] The light source used may be, for example, a low pressure mercury lamp, a high pressure mercury lamp, a deuterium lamp, or a meta Examples of the radiation that can be used include an argon resonance lamp, a xenon lamp, and an excimer laser. The radiation dose is preferably 400 to 20,000 J / m 2 and more preferably 1,000 to 5,000 J / m 2 The coating film may be irradiated with light while being heated in order to enhance the reactivity.
[0121] In producing a liquid crystal alignment film, the coating film that has been subjected to light irradiation treatment may be heated within a temperature range of 120°C to 280°C to further improve the liquid crystal alignment (thermal realignment). This heating may be post-baking, or may be a heat treatment that is performed after the post-baking separately from the post-baking. In the heat treatment of the coating film that has been subjected to light irradiation treatment, the heating temperature is preferably 140°C or higher, more preferably 150°C to 250°C, from the viewpoint of promoting the realignment of molecular chains by heating. The heating time is preferably 5 to 200 minutes, more preferably 10 to 60 minutes.
[0122] The production of the liquid crystal alignment film may further include a step of contacting the coating film that has been subjected to the light irradiation treatment with water, a water-soluble organic solvent, or a mixed solvent of water and a water-soluble organic solvent. Examples of the water-soluble organic solvent include methanol, ethanol, 1-propanol, isopropanol, 1-methoxy-2-propanol acetate, butyl cellosolve, ethyl lactate, acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclopentanone. Of these, the solvent used in this step is preferably water, isopropanol, or a mixture thereof. Examples of the method of contacting the coating film with the solvent include, but are not limited to, a spraying (spray) treatment, a shower treatment, a dipping treatment, and a puddle treatment. The contact time between the coating film and the solvent is not particularly limited, but is, for example, 5 seconds to 15 minutes. After contact with the solvent, the coating film may be subjected to a heat treatment.
[0123] (Step 3: Construction of liquid crystal cell) Two substrates on which a liquid crystal alignment film is formed are prepared as described above, and a liquid crystal is placed between the two substrates arranged opposite to each other to manufacture a liquid crystal cell. For example, the liquid crystal cell can be manufactured by (1) arranging two substrates opposite to each other with a gap (spacer) between them so that the liquid crystal alignment films face each other, bonding the peripheries of the two substrates with a sealant, injecting liquid crystal into the substrate surfaces and the cell gap partitioned by the sealant, and then sealing the injection hole, or (2) applying a sealant to a predetermined location on one substrate on which a liquid crystal alignment film is formed, dropping liquid crystal at a few predetermined locations on the liquid crystal alignment film surface, bonding the other substrate so that the liquid crystal alignment film faces each other, and spreading the liquid crystal over the entire surface of the substrate (ODF method). It is preferable to further heat the manufactured liquid crystal cell to a temperature at which the liquid crystal used has an isotropic phase, and then slowly cool it to room temperature to remove the flow alignment during liquid crystal filling.
[0124] As the sealing agent, for example, an epoxy resin containing a hardener and aluminum oxide spheres as a spacer can be used. As the spacer, a photospacer, a bead spacer, etc. can be used. As the liquid crystal, nematic liquid crystal and smectic liquid crystal can be mentioned. Among these, nematic liquid crystal is preferable, and for example, Schiff base liquid crystal, azoxy liquid crystal, biphenyl liquid crystal, phenylcyclohexane liquid crystal, ester liquid crystal, terphenyl liquid crystal, biphenylcyclohexane liquid crystal, pyrimidine liquid crystal, dioxane liquid crystal, bicyclooctane liquid crystal, cubane liquid crystal, etc. can be used. In addition, cholesteric liquid crystal, chiral agent, ferroelectric liquid crystal, etc. may be added to these liquid crystals.
[0125] In manufacturing a PSA mode liquid crystal element, a photopolymerizable compound is filled into the cell gap together with liquid crystal, a liquid crystal cell is constructed, and then a process of irradiating the liquid crystal cell with light is performed while a voltage is applied between the conductive films of a pair of substrates. That is, it is preferable to manufacture a liquid crystal element by a method including the following steps. [1] A step of forming a coating film using a liquid crystal alignment agent on each of the conductive films of a pair of substrates having a conductive film (corresponding to step 1 above) [2] A step of constructing a liquid crystal cell by disposing a pair of substrates on which a coating film has been formed so that the coating films face each other via a liquid crystal layer containing a photopolymerizable compound (corresponding to step 3 above). [3] A process of irradiating the liquid crystal cell with light while applying a voltage between the conductive films.
[0126] As the photopolymerizable compound, a polyfunctional compound having two or more radically polymerizable functional groups such as an acryloyl group, a (meth)acryloyl group, a vinyl group, etc. can be preferably used. From the viewpoint of reactivity, the photopolymerizable compound is preferably a polyfunctional (meth)acrylic compound having two or more (meth)acryloyl groups. In addition, from the viewpoint of stably maintaining the alignment of liquid crystal molecules, a compound having a total of two or more rings of at least one of a cyclohexane ring and a benzene ring as a liquid crystal skeleton can be preferably used as the photopolymerizable compound. Note that, as such a photopolymerizable compound, a conventionally known compound can be used. In manufacturing a PSA type liquid crystal element, the proportion of the photopolymerizable compound used is, for example, 0.01 to 3 parts by mass, preferably 0.05 to 1 part by mass, relative to 100 parts by mass of the liquid crystal in total.
[0127] The voltage applied can be, for example, 5 to 50 V DC or AC. As the light to be irradiated, for example, ultraviolet light and visible light containing light with a wavelength of 150 to 800 nm can be used, and ultraviolet light containing light with a wavelength of 300 to 400 nm is preferred. As the light source for the irradiation light, for example, a low pressure mercury lamp, a high pressure mercury lamp, a deuterium lamp, a metal halide lamp, an argon resonance lamp, a xenon lamp, an excimer laser, etc. can be used. The light irradiation dose is preferably 1,000 J / m 2 More than 200,000J / m 2 or less, more preferably 1,000 to 100,000 J / m 2 It is.
[0128] Next, a polarizing plate is attached to the outer surface of the liquid crystal cell as needed. Examples of polarizing plates include a polarizing film called an "H film" made by absorbing iodine while stretching and aligning polyvinyl alcohol, sandwiched between cellulose acetate protective films, or a polarizing plate made of the H film itself. This produces a liquid crystal element.
[0129] The liquid crystal element of the present disclosure can be effectively applied to various applications, for example, it can be used in various display devices such as watches, portable game machines, word processors, notebook computers, car navigation systems, camcorders, PDAs, digital cameras, mobile phones, smartphones, various monitors, liquid crystal televisions, and information displays, as well as light control films, etc. In addition, the liquid crystal element formed using the liquid crystal alignment agent of the present disclosure can also be applied to retardation films.
[0130] According to the present disclosure described above, the following means are provided. [Means 1] A liquid crystal aligning agent comprising a polymer (P1) having a partial structure (a1) represented by the above formula (1) and a partial structure (a2) shown below in the same molecule or in different molecules. Partial structure (a2): at least one selected from the group consisting of a nitrogen-containing heterocyclic structure, a partial structure represented by the above formula (2), and a partial structure represented by the above formula (3). [Means 2] Furthermore, -OE 1 (wherein E 1 is a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a monovalent leaving group.), a mercapto group, a protected mercapto group, an amino group, a protected amino group, an oxiranyl group, an oxetanyl group, -Si(OR 11 ) r (R 12 ) 3-r (wherein R 11 and R 12 are each independently a monovalent hydrocarbon group having 1 to 10 carbon atoms, r is an integer of 1 to 3, and when r is 2 or 3, multiple R 11 are the same or different, and when r is 1, multiple R 12are the same or different.) and a compound (A) having at least one selected from the group consisting of a polymerizable carbon-carbon double bond group. [Means 3] The liquid crystal aligning agent according to [Means 1] or [Means 2], wherein the polymer (P1) has, as a partial structure including the partial structure (a1), at least one selected from the group consisting of the partial structure represented by the above formula (1-1) and the partial structure represented by the above formula (1-2). [Means 4] The liquid crystal aligning agent according to any one of [Means 1] to [Means 3], wherein the polymer (P1) is at least one selected from the group consisting of polyamic acid, polyamic acid ester, and polyimide. [Measure 5] The liquid crystal aligning agent according to any one of [Means 1] to [Means 4], wherein the polymer (P1) contains a structural unit derived from at least one selected from the group consisting of a tetracarboxylic acid derivative having the partial structure (a1) and a diamine having the partial structure (a1), and a structural unit derived from a diamine having the partial structure (a2) in the same molecule or in different molecules. [Means 6] The liquid crystal aligning agent according to any one of [Means 1] to [Means 5], further comprising a polymer having neither the partial structure (a1) nor the partial structure (a2). [Means 7] A polymer (P2) having a partial structure (a1) represented by the above formula (1) and -OE 1 (wherein E 1 is a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a monovalent leaving group.), a mercapto group, a protected mercapto group, an amino group, a protected amino group, an oxetanyl group, -Si(OR 11 ) r (R 12 ) 3-r (wherein R 11 and R 12 are each independently a monovalent hydrocarbon group having 1 to 10 carbon atoms, r is an integer of 1 to 3, and when r is 2 or 3, multiple R 11 are the same or different, and when r is 1, multiple R 12are the same or different, and a compound having in one molecule a total of two or more of at least one type selected from the group consisting of polymerizable carbon-carbon double bond groups. [Means 8] The liquid crystal aligning agent according to [Means 7], wherein the polymer (P2) has at least one selected from the group consisting of the partial structure represented by the above formula (1-1) and the partial structure represented by the above formula (1-2) as a partial structure including the partial structure (a1). [Measure 9] The liquid crystal aligning agent according to [Measure 7] or [Measure 8], wherein the polymer (P2) is at least one selected from the group consisting of polyamic acid, polyamic acid ester, and polyimide. [Measure 10] The liquid crystal aligning agent according to any one of [Means 7] to [Means 9], wherein the polymer (P2) has a structural unit derived from at least one selected from the group consisting of a tetracarboxylic acid derivative having the partial structure (a1) and a diamine having the partial structure (a1). [Measure 11] The liquid crystal aligning agent according to any one of [Measure 7] to [Measure 10], further comprising a polymer not having the partial structure (a1). [Means 12] A liquid crystal alignment film formed by using the liquid crystal aligning agent according to any one of [Means 1] to [Means 11]. [Means 13] A liquid crystal element comprising the liquid crystal alignment film according to [Means 12]. [Means 14] A method for producing a liquid crystal alignment film, comprising: forming a coating film using the liquid crystal aligning agent according to any one of [Means 1] to [Means 11]; and irradiating the coating film with light to impart liquid crystal alignment ability. [Means 15] A method for producing a liquid crystal element, comprising: forming a coating film on each conductive film of a pair of substrates having a conductive film by using the liquid crystal aligning agent according to any one of [Means 1] to [Means 11]; constructing a liquid crystal cell by disposing the pair of substrates on which the coating films are formed so that the coating films face each other via a liquid crystal layer containing a photopolymerizable compound; and irradiating the liquid crystal cell with light while a voltage is applied between the conductive films. EXAMPLES
[0131] The present invention will be described in more detail below with reference to examples. However, the present invention should not be construed as being limited to the following examples.
[0132] In the following example, the imidization rate of polyimide in the polymer solution and the weight average molecular weight (M w ), number average molecular weight (M n ) and epoxy equivalent were measured by the following method. [Imidization rate of polyimide] The polyimide solution was poured into pure water, and the resulting precipitate was thoroughly dried under reduced pressure at room temperature. It was then dissolved in deuterated dimethyl sulfoxide and measured at room temperature using tetramethylsilane as a standard substance. 1 H-NMR measurement was performed. 1 The imidization rate [%] was calculated from the H-NMR spectrum using the following formula (1). Imidization rate [%] = (1-(A 1 / (A 2 ×α)))×100 …(1) (In formula (1), A 1 is the peak area due to the proton of the NH group that appears at a chemical shift of around 10 ppm. 2 is the peak area due to other protons. α is the ratio of the number of other protons to one proton of the NH group in the polymer precursor (polyamic acid).
[0133] [Weight average molecular weight of polymer (M w ) and number average molecular weight (M n )] By gel permeation chromatography (GPC), M w and M n The molecular weight distribution (M w / M n ) is the obtained M w and M n Calculated from. Equipment: Showa Denko Co., Ltd. "GPC-101" GPC column: Shimadzu GLC's "GPC-KF-801", "GPC-KF-802", "GPC-KF-803" and "GPC-KF-804" combined Mobile phase: Tetrahydrofuran (THF) Column temperature: 40℃ Flow rate: 1.0mL / min Sample concentration: 1.0% by mass Sample injection volume: 100 μL Detector: Differential refractometer Standard material: Monodisperse polystyrene
[0134] [Epoxy equivalent] The measurement was performed by the hydrochloric acid-methyl ethyl ketone method described in JIS C 2105.
[0135] The necessary amounts of the raw material compounds and polymers used in the following examples were ensured by repeating the synthesis on a synthesis scale as necessary, as shown in the following synthesis examples. In the examples and comparative examples, "parts" and "%" are by mass unless otherwise specified.
[0136] The abbreviations of the compounds are as follows: In the following, the compound represented by formula (X) may be simply referred to as "compound (X)". (Tetracarboxylic acid dianhydride) [ka] [ka]
[0137] (Diamine compounds) [ka] [ka] [ka]
[0138] (Other compounds) [ka] [ka] [ka]
[0139] <Polymer synthesis> 1. Synthesis of polyamic acid [Synthesis Example 1] Tetracarboxylic dianhydrides, 10 molar parts of compound (CA-2) and 90 molar parts of compound (CA-3), as well as diamine compounds, 10 molar parts of compound (DA-1), 20 molar parts of compound (DB-2), 10 molar parts of compound (DC-15), 35 molar parts of compound (DC-2), and 25 molar parts of compound (DC-17), were dissolved in N-methyl-2-pyrrolidone (NMP) and reacted at 60° C. for 6 hours to obtain a solution containing 20 mass% of polyamic acid (referred to as polymer (PAA-1)).
[0140] [Synthesis Examples 2-20] Polyamic acids (polymer (PAA-2) to polymer (PAA-20)) were obtained by the same procedure as in Synthesis Example 1, except that the types and amounts of the tetracarboxylic dianhydrides and diamine compounds used were changed as shown in Table 1. In Table 1, the values of the tetracarboxylic dianhydrides (acid dianhydride 1 to acid dianhydride 3) represent the ratio (molar ratio) of each compound to 100 parts by mole of the total amount of the tetracarboxylic dianhydrides used in the synthesis of the polyamic acid. The values of the diamine compounds (diamine 1 to diamine 6) represent the ratio (molar ratio) of each compound to 100 parts by mole of the total amount of the diamine compounds used in the synthesis of the polyamic acid.
[0141] 2. Synthesis of Polyimide [Synthesis Example 21] As tetracarboxylic dianhydrides, 80 mol parts of compound (CB-3) and 20 mol parts of compound (CB-4), as well as 20 mol parts of compound (DA-1), 20 mol parts of compound (DB-1), 10 mol parts of compound (DC-14), 25 mol parts of compound (DC-11), and 25 mol parts of compound (DC-18) were dissolved in NMP and reacted at 60 ° C for 6 hours to obtain a solution containing 20 mass% of polyamic acid. Next, NMP was added to the obtained polyamic acid solution to obtain a solution with a polyamic acid concentration of 10 mass%, and pyridine and acetic anhydride were added to perform a dehydration ring-closing reaction at 80 ° C for 4 hours. After the dehydration ring-closing reaction, the solvent in the system was replaced with new NMP to obtain a solution containing 15 mass% of polyimide (this is polymer (PI-1)) with an imidization rate of about 69%.
[0142] [Synthesis Examples 22-33] Polyimides (polymers (PI-2) to (PI-13)) were obtained by the same procedure as in Synthesis Example 21, except that the types and amounts of the tetracarboxylic dianhydrides and diamine compounds used were changed as shown in Table 1. In Table 1, the values of the tetracarboxylic dianhydrides (acid dianhydride 1, acid anhydride 2) represent the ratio (molar ratio) of each compound to 100 parts by mole of the total amount of the tetracarboxylic dianhydrides used in the synthesis of the polyimide. The values of the diamine compounds (diamine 1 to diamine 6) represent the ratio (molar ratio) of each compound to 100 parts by mole of the total amount of the diamine compounds used in the synthesis of the polyimide.
[0143] [Table 1]
[0144] 3. Synthesis of polyorganosiloxane [Synthesis Example 34] In a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel and a reflux condenser, 100.0 g of 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane (a compound represented by the above formula (S-1)), 500 g of methyl isobutyl ketone and 10.0 g of triethylamine were charged and mixed at room temperature. Next, 100 g of deionized water was dropped from the dropping funnel over 30 minutes, and the reaction was carried out at 80 ° C. for 6 hours while stirring under reflux. After the reaction was completed, the organic layer was taken out and washed with a 0.2 mass% aqueous ammonium nitrate solution until the water after washing became neutral, and then the solvent and water were distilled off under reduced pressure to obtain a polyorganosiloxane (ESSQ-1) containing epoxy groups as a viscous transparent liquid. The weight average molecular weight Mw of the obtained polyorganosiloxane (ESSQ-1) was 3,500 and the epoxy equivalent was 180 g / mol. In a 200mL three-neck flask, 10.0g of polyorganosiloxane (ESSQ-1), 30.28g of methyl isobutyl ketone as a solvent, compound (S-2) and compound (S-3) as modified components (carboxylic acids) were charged in amounts equivalent to 20 mol% and 10 mol% respectively relative to the total amount of epoxy groups possessed by polyorganosiloxane (ESSQ-1), and 0.10g of UCAT 18X (trade name, manufactured by San-Apro Co., Ltd.) as a catalyst were charged, and the reaction was carried out under stirring at 100 ° C for 48 hours. After the reaction was completed, ethyl acetate was added to the reaction mixture, and the resulting solution was washed with water three times, the organic layer was dried using magnesium sulfate, and the solvent was distilled off to obtain polyorganosiloxane (PSQ-1) having a liquid crystal alignment group. The weight average molecular weight (Mw) of the obtained polymer was 8000.
[0145] 4.Synthesis of styrene-maleimide copolymer [Synthesis Example 35] In a 100 mL two-neck flask under nitrogen, 18.7 mmol of compound (MA-2), 18.7 mmol of compound (MA-4), 10.6 mmol of compound (MA-6), and 5.3 mmol of compound (MA-7) were added as polymerization monomers, 0.98 g of 2,2'-azobis(2,4-dimethylvaleronitrile) as a radical polymerization initiator, and 50 mL of N-methyl-2-pyrrolidone (NMP) as a solvent, and polymerization was carried out at 70°C for 6 hours. After reprecipitation in methanol, the precipitate was filtered and dried in vacuum at room temperature for 8 hours to obtain an addition polymer (referred to as polymer (MI-1)). The weight average molecular weight (Mw) measured in terms of polystyrene by GPC was 35,000, and the molecular weight distribution (Mw / Mn) was 2.
[0146] [Synthesis Example 36] An addition polymer (polymer (MI-2)) was obtained in the same manner as in Synthesis Example 35, except that the types and amounts of the polymerization monomers used were changed as shown in Table 2.
[0147] [Table 2]
[0148] <Preparation and Evaluation of Liquid Crystal Alignment Agent> [Example 1: PSA type liquid crystal display element] 1. Preparation of Liquid Crystal Alignment Agent The solution containing the polymer (PAA-1) obtained in Synthesis Example 1 was diluted with NMP and BC to obtain a solution with a solvent composition of NMP / BC=80 / 20 (mass ratio) and a solid content concentration of 3.5 mass%. This solution was filtered through a filter with a pore size of 0.2 μm to prepare a liquid crystal alignment agent (AL-1).
[0149] 2. Preparation of Liquid Crystal Composition 5% by mass of a liquid crystal compound represented by the following formula (L1-1) and 0.3% by mass of a photopolymerizable compound represented by the following formula (L2-1) were added to 10 g of nematic liquid crystal (MLC-6608, manufactured by Merck) and mixed to obtain liquid crystal composition LC1. [ka]
[0150] 3. Preparation of insulating film forming composition In a flask equipped with a cooling tube and a stirrer, 7 parts by mass of 2,2'-azobis(2,4-dimethylvaleronitrile), 200 parts by mass of propylene glycol monomethyl ether acetate, 15 parts by mass of methacrylic acid, 30 parts by mass of glycidyl methacrylate, 20 parts by mass of styrene, 5 parts by mass of 2-hydroxyethyl acrylate, and 30 parts by mass of isobornyl acrylate were charged, and after nitrogen replacement, gentle stirring was started. After the reaction solution was raised to 62°C, this temperature was maintained for 5 hours to obtain a polymer solution containing an acrylic copolymer (R-1). The obtained polymer solution was dropped into 900 parts by mass of hexane to precipitate the acrylic copolymer (R-1). The precipitated acrylic copolymer (R-1) was separated, and 150 parts by mass of propylene glycol monomethyl ethyl acetate was added, heated to 40°C, and distilled under reduced pressure to obtain a polymer solution containing an acrylic copolymer (R-1). The solid concentration of the obtained polymer solution containing the acrylic copolymer (R-1) was 30 mass %, and as a result of GPC analysis, the area of unreacted monomer and polymerization initiator was 2.3%, and the weight average molecular weight (Mw) was 12,800. For an amount equivalent to 100 parts by mass (solid content) of the acrylic copolymer (R-1), 25 parts by mass of a condensation product of 4,4'-[1-[4-[1-[4-hydroxyphenyl]-1-methylethyl]phenyl]ethylidene]bisphenol (1.0 mol) and 1,2-naphthoquinone diazide-5-sulfonic acid chloride (2.0 mol) were used as a photosensitizer, and a mixture of dipentaerythritol hexaacrylate and dipentaerythritol pentaacrylate ("KAYARAD" manufactured by Nippon Kayaku Co., Ltd.) was used as a polymerizable compound. A mixture of 5 parts by mass of 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate (Kyowa Hakko Kirin's "Kyowanol M") as a film-forming aid, 10 parts by mass of SH28PA (Dow Corning Toray) as a leveling agent, and diethylene glycol ethyl methyl ether was added to the mixture to give a solids concentration of 18% by mass. The mixture was then filtered through a membrane filter having a pore size of 0.2 μm to prepare a composition for forming an insulating film (RD-1).
[0151] 4. Preparation of a substrate with an insulating film The insulating film forming composition (RD-1) was applied onto a glass substrate using a spin coater, and then prebaked on a hot plate at 90°C for 2 minutes. Then, a proximity exposure machine (Canon's "MA-1200" (mixed ghi line)) was used to expose the substrate to 300 mJ / cm2. 2 After irradiating the entire surface of the substrate with light, the substrate was cured by heating (post-baking) at 230° C. for 30 minutes in an oven to form an insulating film with a thickness of 3 μm on the glass substrate.
[0152] 5. Fabrication of liquid crystal cells for evaluating impurity tolerance A liquid crystal alignment agent (AL-1) was applied by a spinner to the electrode formation surface of the substrate having an ITO electrode patterned into a comb shape, and to the insulating film formation surface of the substrate having an insulating film, and pre-baked for 1 minute on a hot plate at 80°C. After that, the substrate was heated at 230°C for 1 hour in an oven with the interior replaced with nitrogen, to produce a pair (2 substrates) of substrates having a liquid crystal alignment film with a thickness of 0.1 μm. An epoxy resin adhesive containing aluminum oxide spheres having a diameter of 3.5 μm was applied by screen printing to the outer circumference of the surface having the liquid crystal alignment film of the substrate having an insulating film, and then the liquid crystal alignment film surfaces of a pair of substrates were opposed to each other and pressed together, and the adhesive was thermally cured at 150° C. for 1 hour. Next, the liquid crystal composition LC1 was filled into the gap between the substrates through the liquid crystal injection port, and the liquid crystal injection port was sealed with an epoxy adhesive. Furthermore, in order to remove the flow alignment during liquid crystal injection, the liquid crystal cell was manufactured by heating it at 130° C. and then slowly cooling it to room temperature. Note that, since the substrate can be easily manufactured, the liquid crystal cell for evaluating the impurity resistance was manufactured using an electrode substrate for an IPS type liquid crystal cell.
[0153] 6. Fabrication of Liquid Crystal Cells for Cell Transmittance Evaluation The liquid crystal alignment agent (AL-1) prepared above was applied to the transparent electrode surface of a glass substrate with a transparent electrode made of an ITO film using a spinner, and pre-baked for 1 minute on a hot plate at 80°C. After that, the substrate was heated for 1 hour at 230°C in an oven substituted with nitrogen to remove the solvent, forming a coating film (liquid crystal alignment film) with a thickness of 0.1 μm. This coating film was subjected to rubbing treatment using a rubbing machine having a roll wrapped with rayon cloth at a roll rotation speed of 400 rpm, a stage movement speed of 3 cm / sec, and a pile indentation length of 0.1 mm. After that, ultrasonic cleaning was performed in ultrapure water for 1 minute, and then drying was performed for 10 minutes in a clean oven at 100°C to obtain a substrate having a liquid crystal alignment film. This operation was repeated to obtain a pair (2 sheets) of substrates having a liquid crystal alignment film. This rubbing treatment was a weak rubbing treatment performed for the purpose of controlling the collapse of the liquid crystal and performing alignment division in a simple manner. An epoxy resin adhesive containing aluminum oxide spheres with a diameter of 3.5 μm was applied by screen printing to the outer periphery of the surface having the liquid crystal alignment film of one of the above substrates, and then the liquid crystal alignment film surfaces of the pair of substrates were placed opposite each other, overlapped and pressed together, and the adhesive was thermally cured by heating at 150° C. for 1 hour. Next, liquid crystal composition LC1 was filled into the gap between the substrates through the liquid crystal injection port, and the liquid crystal injection port was sealed with an epoxy adhesive. In order to eliminate flow alignment during liquid crystal injection, the resultant was heated at 150° C. for 10 minutes and then slowly cooled to room temperature. Next, an AC voltage of 10 V with a frequency of 60 Hz was applied between the electrodes of the obtained liquid crystal cell, and while the liquid crystal was in a driven state, ultraviolet rays of 50,000 J / m were irradiated using an ultraviolet irradiation device that used a metal halide lamp as a light source. 2 The irradiation amount was measured using an actinometer that measures at a wavelength of 365 nm as a standard. In this manner, a PSA type liquid crystal cell was manufactured.
[0154] 7. Evaluation (1) Evaluation of impurity tolerance The liquid crystal cell manufactured in 5. above was placed in a 60°C oven, and then the voltage holding ratio (VHR) was measured under conditions of 1V and 1670 milliseconds using a VHR measuring device "VHR-1" manufactured by Toyo Corporation. If the VHR was higher than 60%, it was rated "good (○)", if it was 60% or less and 45% or more, it was rated "fair (△)", and if it was less than 45%, it was rated "poor (×)". As a result, the electrical characteristics of this example were rated "good (○)".
[0155] (2) Evaluation of seal adhesion A liquid crystal alignment agent (AL-1) was applied onto a glass substrate using a spinner, prebaked on a hot plate at 80°C for 2 minutes, and then heated (post-baked) for 30 minutes in an oven at 230°C with the interior replaced with nitrogen, forming a coating film (liquid crystal alignment film) with an average thickness of 0.10 μm. By repeating the same operation, two glass substrates with coating films were produced. An ODF sealant (S-WB42, manufactured by Sekisui Chemical Co., Ltd.) was applied to the coating film of one of the glass substrates with the coating film formed thereon to a width of 0.5 mm, and the other glass substrate was laminated so that the coating film and the ODF sealant were in contact with each other. Then, a metal halide lamp was used to illuminate the substrate at 30,000 J / m. 2 After irradiating the specimen with light (converted to 365 nm), the specimen was heated in an oven at 120° C. for 1 hour. The adhesion strength was then measured using a tensile / compression tester (model number: SDWS-0201-100SL) manufactured by Imada Seisakusho to evaluate the seal adhesion. The evaluation is adhesion strength of 180N / cm 2 If it is more than 170N / cm, it is "particularly good (◎)". 2 More than 180N / cm 2 If it was less than 150N / cm, it was rated as "Good (○)". 2 More than 170N / cm 2 If it is less than 150N / cm, it is "Fair (△)". 2 If the measured value was less than 100%, it was rated as "poor (x)". As a result, the seal adhesion of this example was rated as "good (◯)".
[0156] (3) Measurement of cell transmittance The liquid crystal cell manufactured in 6. above was subjected to measurement of the absorption spectrum in the ultraviolet-visible region using an ultraviolet-visible near-infrared spectrophotometer (manufactured by JASCO Corporation, product name "V-670"). The angle of incidence to the liquid crystal cell was set to 0°. When the average transmittance in the wavelength range of 380-800 nm was 87% or more, it was rated as "good (○)", when it was 85% or more and less than 87%, it was rated as "fair (△)", and when it was less than 85%, it was rated as "poor (×)". As a result, the cell transmittance of this example was rated as "good (○)".
[0157] [Examples 2 to 19 and Comparative Examples 1 to 5] Liquid crystal alignment agents (AL-2) to (AL-19) and (AR-1) to (AR-5) were prepared by the same operation as in Example 1, except that the composition of the liquid crystal alignment agent was changed as shown in Table 3. In addition, liquid crystal cells were produced using the obtained liquid crystal alignment agents in the same manner as in Example 1, and various evaluations were performed. The results are shown in Table 3. In Table 3, the numerical values in the mass ratio column indicate the blending ratio (parts by mass) of the solid content of each compound (polymer, additive) relative to 100 parts by mass of the total amount of the polymer components used in the preparation of the liquid crystal alignment agent.
[0158] [Example 20: Optical FFS type liquid crystal display element] 1. Preparation of liquid crystal alignment agent and evaluation of impurity resistance and seal adhesion A liquid crystal alignment agent (AL-20) was prepared by the same operation as in Example 1, except that the composition of the liquid crystal alignment agent was changed as shown in Table 3. In addition, a liquid crystal cell for evaluating impurity resistance was produced in the same manner as in Example 1, except that the obtained liquid crystal alignment agent (AL-20) was used and a negative liquid crystal (MLC-6608, manufactured by Merck) was used as the liquid crystal composition, and the impurity resistance was evaluated, and the seal adhesion was evaluated using the liquid crystal alignment agent (AL-20). The results are shown in Table 3.
[0159] 2. Cell Permeability Measurement The liquid crystal alignment agent (AL-20) prepared above was applied using a spinner onto the transparent electrode surface of a glass substrate with a transparent electrode made of an ITO film, and pre-baked on a hot plate at 80°C for 1 minute. The substrate was then heated at 200°C for 1 hour in an oven substituted with nitrogen to remove the solvent, forming a coating film (liquid crystal alignment film) with a thickness of 0.1 μm. This operation was repeated to obtain a pair (2 sheets) of substrates with liquid crystal alignment films. The resulting coating film was irradiated with 1,000 J / m2 of linearly polarized ultraviolet light containing a 254 nm emission line using an Hg-Xe lamp. 2 The coating film was irradiated with light from the normal direction of the substrate to perform a photo-alignment treatment. The amount of irradiation was measured using an actinometer that measures at a wavelength of 254 nm. Next, the coating film that had been subjected to the photo-alignment treatment was heated in a clean oven at 200°C for 30 minutes to perform a heat treatment, thereby forming a liquid crystal alignment film. An epoxy resin adhesive containing aluminum oxide spheres with a diameter of 3.5 μm was applied by screen printing to the outer periphery of the surface having the liquid crystal alignment film of one of the above substrates, and then the liquid crystal alignment film surfaces of the pair of substrates were placed facing each other, overlapped and pressed together, and the adhesive was thermally cured by heating at 150° C. for 1 hour. Next, negative liquid crystal (MLC-6608, manufactured by Merck) was filled into the gap between the substrates through the liquid crystal injection port, the liquid crystal injection port was sealed with an epoxy adhesive, and in order to eliminate flow alignment during liquid crystal injection, it was heated at 150° C. for 10 minutes and then slowly cooled to room temperature. The absorption spectrum of the prepared liquid crystal cell in the ultraviolet-visible region was measured using an ultraviolet-visible-near infrared spectrophotometer (manufactured by JASCO Corporation, product name "V-670"). The evaluation results are shown in Table 3.
[0160] [Example 21] A liquid crystal alignment agent (AL-21) was prepared by the same operation as in Example 1, except that the composition of the liquid crystal alignment agent was changed as shown in Table 3. In addition, various evaluations were performed in the same manner as in Example 20 using the obtained liquid crystal alignment agent (AL-21). The results are shown in Table 3.
[0161] [Example 22: Rubbed FFS type liquid crystal display element] 1. Preparation of liquid crystal alignment agent and evaluation of impurity resistance and seal adhesion A liquid crystal alignment agent (AL-22) was prepared by the same operation as in Example 1, except that the composition of the liquid crystal alignment agent was changed as shown in Table 3. In addition, a liquid crystal cell for evaluating impurity resistance was produced using the obtained liquid crystal alignment agent (AL-22) in the same manner as in Example 1, except that a negative liquid crystal (MLC-6608, manufactured by Merck) was used as the liquid crystal composition, and the impurity resistance was evaluated. The seal adhesion was also evaluated using the liquid crystal alignment agent (AL-22). The results are shown in Table 3.
[0162] 2. Cell Permeability Measurement The liquid crystal alignment agent (AL-22) prepared above was applied to the transparent electrode surface of a glass substrate with a transparent electrode made of an ITO film using a spinner, and pre-baked for 1 minute on a hot plate at 80°C. After that, the substrate was heated for 1 hour at 200°C in an oven substituted with nitrogen to remove the solvent, forming a coating film (liquid crystal alignment film) with a thickness of 0.1 μm. Next, the coating film surface was subjected to rubbing treatment using a rubbing machine having a roll wrapped with rayon cloth at a roll rotation speed of 1000 rpm, a stage movement speed of 3 cm / sec, and a pile indentation length of 0.3 mm. Then, ultrasonic cleaning was performed in ultrapure water for 1 minute, and then the substrate was dried for 10 minutes in a clean oven at 100°C. This operation was repeated to obtain a pair (2 sheets) of substrates with liquid crystal alignment films. An epoxy resin adhesive containing aluminum oxide spheres with a diameter of 3.5 μm was applied by screen printing to the outer periphery of the surface having the liquid crystal alignment film of one of the above substrates, and then the liquid crystal alignment film surfaces of the pair of substrates were placed facing each other, overlapped and pressed together, and the adhesive was thermally cured by heating at 150° C. for 1 hour. Next, negative liquid crystal (MLC-6608, manufactured by Merck) was filled into the gap between the substrates through the liquid crystal injection port, the liquid crystal injection port was sealed with an epoxy adhesive, and in order to eliminate flow alignment during liquid crystal injection, it was heated at 150° C. for 10 minutes and then slowly cooled to room temperature. The absorption spectrum of the prepared liquid crystal cell in the ultraviolet-visible region was measured using an ultraviolet-visible-near infrared spectrophotometer (manufactured by JASCO Corporation, product name "V-670"). The evaluation results are shown in Table 3.
[0163] [Example 23] A liquid crystal alignment agent (AL-23) was prepared by the same operation as in Example 1, except that the composition of the liquid crystal alignment agent was changed as shown in Table 3. In addition, the obtained liquid crystal alignment agent (AL-23) was used to carry out various evaluations in the same manner as in Example 22. The results are shown in Table 3.
[0164] [Example 24: Optical VA type liquid crystal display element] 1. Preparation of liquid crystal alignment agent and evaluation of impurity resistance and seal adhesion A liquid crystal alignment agent (AL-24) was prepared by the same operation as in Example 1, except that the composition of the liquid crystal alignment agent was changed as shown in Table 3. In addition, a liquid crystal cell for evaluating impurity resistance was produced in the same manner as in Example 1, except that the obtained liquid crystal alignment agent (AL-24) was used and a negative liquid crystal (MLC-6608, manufactured by Merck) was used as the liquid crystal composition, and the impurity resistance was evaluated, and the seal adhesion was evaluated using the liquid crystal alignment agent (AL-24). The results are shown in Table 3.
[0165] 2. Cell Permeability Measurement The liquid crystal alignment agent (AL-24) prepared above was applied to the transparent electrode surface of a glass substrate with a transparent electrode made of an ITO film using a spinner, and pre-baked on a hot plate at 80°C for 1 minute, and then heated at 200°C for 1 hour in an oven substituted with nitrogen to remove the solvent, forming a coating film (liquid crystal alignment film) with a thickness of 0.1 μm. Next, the surface of this coating film was irradiated with 1,000 J / m of polarized ultraviolet light containing a 313 nm emission line using a Hg-Xe lamp and a Glan-Taylor prism. 2 The substrate was irradiated with the light from a direction inclined by 40° from the normal line of the substrate to impart liquid crystal alignment ability. This operation was repeated to obtain a pair (two sheets) of substrates having a liquid crystal alignment film. An epoxy resin adhesive containing aluminum oxide spheres with a diameter of 3.5 μm was applied by screen printing to the outer periphery of the surface having the liquid crystal alignment film of one of the above substrates, and then the liquid crystal alignment film surfaces of the pair of substrates were placed facing each other, overlapped and pressed together, and the adhesive was thermally cured by heating at 150° C. for 1 hour. Next, negative liquid crystal (MLC-6608, manufactured by Merck) was filled into the gap between the substrates through the liquid crystal injection port, the liquid crystal injection port was sealed with an epoxy adhesive, and in order to eliminate flow alignment during liquid crystal injection, it was heated at 150° C. for 10 minutes and then slowly cooled to room temperature. The absorption spectrum of the prepared liquid crystal cell in the ultraviolet-visible region was measured using an ultraviolet-visible-near infrared spectrophotometer (manufactured by JASCO Corporation, product name "V-670"). The evaluation results are shown in Table 3.
[0166] [Example 25] A liquid crystal alignment agent (AL-25) was prepared by the same operation as in Example 1, except that the composition of the liquid crystal alignment agent was changed as shown in Table 3. In addition, various evaluations were performed in the same manner as in Example 24 using the obtained liquid crystal alignment agent (AL-25). The results are shown in Table 3.
[0167] [Table 3]
[0168] As shown in Table 3, impurity resistance, seal adhesion, and cell transmittance were all rated as "particularly good (◎)", "good (○)", or "fair (△)" for Examples 1 to 25, and the balance of various properties was good. Among these, Examples 1 to 13, 17 to 20, and 22 to 25, which contained compound (A) or compound (A1), were particularly excellent in that the seal adhesion was rated as "particularly good (◎)" or "good (○)". In contrast, Comparative Examples 1 to 5 were rated as "poor (x)" in at least one of impurity resistance, seal adhesion, and cell transmittance, and were inferior to Examples 1 to 25.
Claims
1. The following formula (1) 【Chemistry 1】 (In formula (1), R 1 and R 2 are each independently a monovalent substituent. n1 and n2 are each independently 0 or 1. m1 is an integer from 0 to (n1×2+4). m2 is an integer from 0 to (n2×2+4). R 1 When there are multiple R 1 are the same or different, R 2 When there are multiple R 2 are the same or different. "*" represents a bond to a carbon atom.) and a partial structure (a2) shown below in the same molecule or in different molecules. Partial structure (a2): at least one selected from the group consisting of a nitrogen-containing heterocyclic structure, a partial structure represented by the following formula (2), and a partial structure represented by the following formula (3): 【Chemistry 2】 (In formula (2), Y 1 is a hydrogen atom or a monovalent group which is eliminated by heating and is replaced with a hydrogen atom. 1 A is an alkanediyl group, a substituted or unsubstituted divalent alicyclic group, or a substituted or unsubstituted divalent aromatic ring group. 2 is an alkanediyl group. "*" represents a bond.) 【Chemistry 3】 (In formula (3), Y 2 is a monovalent group which is eliminated by heating and is replaced by a hydrogen atom. X 3 R is a single bond or an alkanediyl group. 4 and R 5 are each independently a hydrogen atom or a monovalent hydrocarbon group. "*" represents a bond.)
2. Furthermore, -OE 1 (wherein E 1 is a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a monovalent leaving group; mercapto group, a protected mercapto group, an amino group, a protected amino group, an oxiranyl group, an oxetanyl group, —Si(OR 11 ) r (R 12 ) 3-r (wherein R 11 and R 12 are each independently a monovalent hydrocarbon group having 1 to 10 carbon atoms, r is an integer from 1 to 3, and when r is 2 or 3, multiple R 11 are the same or different, and when r is 1, a plurality of R 12 are the same or different, and a compound (A) having at least one selected from the group consisting of a polymerizable carbon-carbon double bond group.
3. The following formula (1) 【Chemistry 4】 (In formula (1), R 1 and R 2 are each independently a monovalent substituent. n1 and n2 are each independently 0 or 1. m1 is an integer from 0 to (n1×2+4). m2 is an integer from 0 to (n2×2+4). R 1 When there are multiple R 1 are the same or different, R 2 When there are multiple R 2 are the same or different. "*" represents a bond.) A polymer having a partial structure (a1) represented by the following formula: -OE 1 (wherein E 1 is a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a monovalent leaving group; mercapto group, a protected mercapto group, an amino group, a protected amino group, an oxetanyl group, —Si(OR 11 ) r (R 12 ) 3-r (wherein R 11 and R 12 are each independently a monovalent hydrocarbon group having 1 to 10 carbon atoms, r is an integer from 1 to 3, and when r is 2 or 3, multiple R 11 are the same or different, and when r is 1, a plurality of R 12 are the same or different; and a compound having, in one molecule, a total of two or more of at least one type selected from the group consisting of a polymerizable carbon-carbon double bond group, A liquid crystal aligning agent comprising:
4. The polymer (P1) has at least one selected from the group consisting of a partial structure represented by the following formula (1-1) and a partial structure represented by the following formula (1-2) as a partial structure including the partial structure (a1). The liquid crystal aligning agent according to claim 1. 【Chemistry 5】 (In formula (1-1) and formula (1-2), Ar 1 and Ar 2 are each independently a divalent aromatic ring group. 1 and X 2 are each independently a single bond, —O—, —S—, —CO—, or —NR 8 -, -COO-, -CONR 8 --, --NR 8 C.O.N.R. 9 -, -SO 2 -, -SO 2 -O-, an alkanediyl group having 1 to 10 carbon atoms, or any methylene group in an alkanediyl group having 2 to 10 carbon atoms is -O-, -S-, -CO-, -NR 8 -, -COO-, -OCO-, -CONR 8 --, --NR 8 CO- or -NR 8 C.O.N.R. 9 -substituted group. 8 and R 9 are each independently a hydrogen atom or a monovalent organic group. 3 and Ar 4 are each independently a trivalent aromatic ring group. 1 , R 2 , n1, n2, m1 and m2 are defined as in formula (1). "*" represents a bond.)
5. The liquid crystal aligning agent according to claim 1, wherein the polymer (P1) is at least one selected from the group consisting of polyamic acid, polyamic acid ester, and polyimide.
6. The polymer (P1) contains a structural unit derived from at least one selected from the group consisting of a tetracarboxylic acid derivative having the partial structure (a1) and a diamine having the partial structure (a1), and a structural unit derived from a diamine having the partial structure (a2) in the same molecule or in different molecules. The liquid crystal aligning agent according to claim 1.
7. The liquid crystal aligning agent according to claim 1 , further comprising a polymer having neither the partial structure (a1) nor the partial structure (a2).
8. A liquid crystal alignment film formed by using the liquid crystal aligning agent according to any one of claims 1 to 7.
9. A liquid crystal element comprising the liquid crystal alignment film according to claim 8 .
10. A step of forming a coating film using the liquid crystal aligning agent according to any one of claims 1 to 7; a step of irradiating the coating film with light to impart liquid crystal alignment ability; A method for producing a liquid crystal alignment film comprising the steps of:
11. A step of forming a coating film using the liquid crystal aligning agent according to any one of claims 1 to 7 on each of the conductive films of a pair of substrates having a conductive film; a step of constructing a liquid crystal cell by disposing a pair of substrates on which the coating film is formed such that the coating film faces each other via a liquid crystal layer containing a photopolymerizable compound; applying a voltage between the conductive films to the liquid crystal cell; A method for manufacturing a liquid crystal element comprising the steps of:
Citation Information
Patent Citations
Liquid aligning agent
JP1999212097A
Liquid crystal alignment agent, liquid crystal alignment film, liquid crystal display element, manufacturing method of liquid crystal display element, polymer, and compound
JP2015197611A
Liquid crystal display element and manufacturing method for the same, and liquid crystal alignment agent
JP2016173544A
Polyamic acid, polyimide, and element formed therefrom
JP2022164544A
Liquid crystal alignment agent, liquid crystal alignment film and liquid crystal display element having thereof
US20150232665A1
Cited By
Liquid crystal alignment agent, liquid crystal alignment film, and liquid crystal display element
WO2026216543A1